Fabrication method of ultrasonic transducer based on multi-frequency piezoelectric materials and 3D printed microrings

By using photolithography and 3D printing technology to prepare multi-frequency piezoelectric materials and micro-ring arrays, the problem of balancing accuracy and performance of piezoelectric arrays in small sizes was solved, and a high-precision and high-performance ultrasonic transducer was realized.

CN123124656APending Publication Date: 2026-11-17SOUTH CHINA NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611620628.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

When the size and spacing of existing piezoelectric ultrasonic arrays decrease, the processing accuracy decreases, and it is difficult to balance high driving capability and high receiving sensitivity. Traditional piezoelectric array elements have performance contradictions when they simultaneously undertake transmission and reception.

Method used

An ultrasonic transducer fabrication method using multi-frequency piezoelectric materials and 3D-printed microrings was developed. A multi-frequency piezoelectric array was fabricated by forming an etching mask through photolithography and performing physical ion beam etching. A microring array was then directly 3D printed on the array, with transmission and reception functions configured respectively.

Benefits of technology

The processing precision of complex piezoelectric array elements has been improved, and the differentiated design of multi-frequency piezoelectric arrays has been realized. This has alleviated the problem of balancing high driving capability and high receiving sensitivity, and improved the performance of ultrasonic transducers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124656A_ABST
    Figure CN123124656A_ABST
Patent Text Reader

Abstract

This invention discloses a method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings, belonging to the fields of ultrasonic transducers, piezoelectric micromachining, 3D micro / nano manufacturing, and array-type ultrasonic detection technology. The fabrication method includes determining the array design layout; pre-treating the piezoelectric material and preparing a backing layer, electrode layer, and photoresist layer; preparing an etched mask and then fabricating the piezoelectric material array; performing PDMS filling followed by surface planarization; determining the microring receiving array layout and then 3D printing the microring array; finally, immersion treatment and natural air drying to obtain an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings. This method improves the processing accuracy of complex piezoelectric elements, enables patterned etching on the same piezoelectric material wafer to obtain a multi-frequency piezoelectric array, and alleviates the difficulty of simultaneously achieving high driving capability and high receiving sensitivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of ultrasonic transducers, piezoelectric micromachining, 3D micro / nano manufacturing, and array-type ultrasonic testing technology, specifically to a method for fabricating ultrasonic transducers based on multi-frequency piezoelectric materials and 3D-printed microrings. Background Technology

[0002] Ultrasonic transducers are core components in systems such as medical ultrasound imaging, industrial non-destructive testing, acoustic sensing, and microfluidic manipulation, used to convert electrical energy, mechanical vibration energy, and acoustic energy. Among them, piezoelectric material ultrasonic arrays can independently constitute ultrasonic transducers, and can achieve sound beam focusing, scanning imaging, and spatial sound field manipulation through multi-channel phased excitation and multi-point echo reception. Micro-ring arrays can be used as optical ultrasonic receiving arrays or ultrasonic sensing units in ultrasonic transducers.

[0003] Existing piezoelectric ultrasonic arrays mostly use mechanical cutting or dicing to form the array element structure. That is, grooves are machined on the piezoelectric ceramic sheet by diamond blades or grinding wheels, and then filled with polymer material to achieve array element isolation. However, when the array element size and array element spacing are further reduced, factors such as cutting blade width, tool vibration, edge chipping, and microcracks will reduce the array resolution and array element consistency, thereby reducing the processing accuracy of complex piezoelectric array elements. In addition, traditional piezoelectric array elements usually perform both transmitting and receiving functions. However, the transmitting stage requires high electromechanical conversion efficiency, large driving displacement, and strong voltage withstand capability; while the receiving stage requires low noise, high compliance, and high sensitivity. Therefore, there is a problem that it is difficult to balance high driving capability and high receiving sensitivity. It is usually necessary to add transceiver isolation switches, amplifiers, and filters to the hardware circuit system to process weak ultrasonic echo signals.

[0004] Based on this, the present invention designs an ultrasonic transducer fabrication method based on multi-frequency piezoelectric materials and 3D printed microrings to solve the above problems. Summary of the Invention

[0005] To address the aforementioned shortcomings of existing technologies, this invention provides a method for fabricating ultrasonic transducers based on multi-frequency piezoelectric materials and 3D-printed microrings.

[0006] To achieve the above objectives, the present invention provides the following technical solution: The method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings includes the following steps: Step 1: Etching the multi-frequency piezoelectric material wafer array 1.1 Design the array layout; 1.2. Prepare a backing layer on the back of the piezoelectric material; 1.3. A common electrode is deposited on the back side of the piezoelectric material, and a patterned electrode layer is deposited on the front side of the piezoelectric material; then a photoresist layer for etching is prepared on the patterned electrode layer. 1.4. Based on the array design layout and using the patterned electrode layer as a reference, fabricate an exposure mask; using the exposure mask as a reference, sequentially expose, develop, rinse and dry the photoresist layer used for etching to obtain a piezoelectric material with an etching mask. 1.5. Place the piezoelectric material with the etching mask in an ion beam etching device and perform physical ion beam etching on the piezoelectric material to obtain a piezoelectric material array; 1.6. The piezoelectric material array is filled with a filling liquid and then cured to obtain a piezoelectric material array with a filling layer; then the surface is planarized to obtain a matching layer, and after encapsulation, a multi-frequency piezoelectric material array is obtained. Step 2: Fabrication of an integrated micro-ring array structure ultrasonic transducer 2.1 Design the micro-ring receiving array layout based on the array element arrangement of the multi-frequency piezoelectric material array, obtain the designed pattern file, and import it into the 3D printer; 2.2 First, a photoresist layer for printing is prepared on the matching layer of the multi-frequency piezoelectric material array. Then, micro-rings and straight waveguides are formed on the photoresist layer for printing using a 3D printer to obtain the processing substrate. 2.3 The substrate is sequentially developed, terminated, replaced, and dried to obtain an ultrasonic transducer of multi-frequency piezoelectric material and 3D printed microring.

[0007] Furthermore, the piezoelectric material is PZT piezoelectric wafer; the conductive silver paste is E-solder 3022 conductive silver paste; the electrode material used for both the common electrode and the patterned electrode layer is Cu; the photoresist is AZ9260 thick film positive photoresist; and the developer is AZ400K developer.

[0008] Furthermore, step 1.2 specifically involves cleaning, drying, and planarizing the piezoelectric material, polishing and bonding conductive silver paste to the back of the piezoelectric material, and then performing a curing operation to obtain a backing layer.

[0009] Furthermore, step 1.3 specifically involves: depositing a common electrode on the back side of the piezoelectric material using ion beam sputtering; depositing a patterned electrode layer on the front side of the piezoelectric material using photolithography and ion beam sputtering; subsequently spin-coating photoresist onto the patterned electrode layer on the front side of the piezoelectric material, and obtaining a photoresist layer for etching after soft baking.

[0010] Furthermore, in step 1.3, the spin coating adopts a combination of low-speed photoresist spreading and high-speed photoresist homogenization. The specific steps are as follows: first, spin coating at 500~800 rpm for 5~10 seconds to spread the photoresist evenly, and then spin coating at 2000~3000 rpm for 30~60 seconds.

[0011] Furthermore, in step 1.4, the exposure dose is preferably 150~300 mJ / cm². 2 .

[0012] Furthermore, in step 1.5, the physical ion beam etching uses an ion energy of 500-800 eV and a current of 0.5-0.8 mA / cm². 2 The beam current density was set, and the Ar working pressure was set to 0.05~0.15Pa. At the same time, the etching time and etching depth were calibrated by using actual piezoelectric material test pieces to obtain the relationship curve between etching time and etching depth. Then, the etching time at the isolation groove on the piezoelectric material was determined according to the etching depth required for the isolation groove between adjacent array elements.

[0013] Furthermore, in step 1.6, the specific filling method is as follows: under vacuum conditions, the PDMS filling liquid is fully introduced into the isolation tank of the piezoelectric material array for filling, and after filling is completed, the pressure is restored to normal.

[0014] Furthermore, in step 2.1, the specific method for designing the micro-ring receiving array layout based on the array element arrangement of the multi-frequency piezoelectric material array is as follows: each micro-ring in the micro-ring array is spatially positioned corresponding to the array element of the corresponding multi-frequency piezoelectric material array.

[0015] Furthermore, in step 2.2, the specific steps for forming micro-rings and straight waveguides on the photoresist layer used for printing using a two-photon 3D printer are as follows: using the 100× oil immersion objective of the two-photon 3D printer, an ultrashort pulse laser with a wavelength of 1025~1035nm and a pulse repetition frequency of 0.8~1.2MHz is focused onto the photoresist layer used for printing. The rated output power of the laser is set to 1W, the processing power is set to 6~10% of the rated output power, and the processing rate is set to 4000~6000 points / s. The photoresist layer used for printing on the matching layer is cured, thereby forming micro-rings and straight waveguides on the photoresist layer used for printing.

[0016] Compared with the prior art, the beneficial effects of this invention are as follows: 1. This invention can improve the processing accuracy of complex piezoelectric array elements: by using photolithography to form an etching mask, and by obtaining the relationship curve between etching time and etching depth through experimental calibration, the etching time of physical ion beam etching on piezoelectric material is controlled according to the depth of specific isolation trenches to form isolation trenches of corresponding depth, thereby achieving the effect of improving the processing accuracy of complex piezoelectric array elements. 2. This invention can realize a multi-frequency piezoelectric array by patterning etching on the same piezoelectric material wafer: by differentiating the shape, size, spacing, isolation structure and bonding structure of the array elements in different regions on the same piezoelectric material wafer, the array elements in different regions generate different resonant frequencies, thereby realizing a multi-frequency piezoelectric array; 3. This invention can alleviate the problem of balancing high driving capability and high receiving sensitivity: a multi-frequency piezoelectric material array formed by differential ion beam etching is used as a substrate, and a micro-ring array is directly 3D printed on its planarized surface. This results in an ultrasonic transducer that integrates transmission and reception, with the multi-frequency piezoelectric array handling ultrasonic transmission and the 3D-printed micro-ring array handling optical reception. By configuring the transmission and reception functions separately, the problem of balancing high driving capability and high receiving sensitivity when traditional piezoelectric array elements simultaneously handle both transmission and reception is alleviated. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without any creative effort.

[0018] Figure 1 This is a schematic diagram of the multi-frequency piezoelectric material array of the present invention; Figure 2 This is a schematic diagram of the fabrication process of the ultrasonic transducer using the multi-frequency piezoelectric material and 3D-printed microrings of the present invention. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0020] Example 1: As Figures 1-2 As shown, the method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings specifically includes the following steps: Step 1: Etching the multi-frequency piezoelectric material wafer array 1.1 Array Design Layout A piezoelectric material with a thickness of 0.28 mm was selected as the substrate of the piezoelectric array. The array structure was designed according to the target ultrasonic working frequency and the array arrangement to form a multi-frequency piezoelectric array. The array design layout was determined based on the multi-frequency piezoelectric array. The piezoelectric material used is a PZT piezoelectric wafer.

[0021] The array arrangement includes adjacent arrangement, alternating arrangement, partitioned arrangement, chessboard arrangement, and row and column arrangement.

[0022] The array structure is formed by combining array elements with different resonant frequencies.

[0023] 1.2 Pretreatment of piezoelectric materials and formation of backing layer After cleaning, drying and planarizing the piezoelectric material, the back of the piezoelectric material is polished and E-solder 3022 conductive silver paste is bonded on it. It is cured at 25°C for 24 hours and then ground to obtain a backing layer with a thickness of 0.5 mm.

[0024] The E-solder 3022 conductive silver paste is obtained by thoroughly mixing silver epoxy resin and a hardener at a mass ratio of 100:7.

[0025] Furthermore, the hardener used is Hardener No. 18.

[0026] 1.3 Electrode layer fabrication and photoresist layer formation A common electrode is deposited on the back side of the piezoelectric material using ion beam sputtering to provide a common potential terminal for each piezoelectric element and to form a unified electric field reference in the thickness direction of the piezoelectric material. A patterned electrode layer is deposited on the front side of the piezoelectric material using photolithography and ion beam sputtering. The patterned electrode layer corresponds to the spatial position of each element and is used to electrically excite different elements independently or in groups, so that each element generates mechanical vibration and ultrasonic waves of corresponding frequencies under the action of an external electric field. The common electrode layer and the patterned electrode layer are conductive metal layers with a thickness of 200 nm.

[0027] Furthermore, the conductive metal layer is preferably made of Cu; an adhesion layer with a thickness of 20 nm can also be provided between Cu and the piezoelectric material, and an Au anti-oxidation protective layer with a thickness of 75 nm can also be provided on the outer surface of Cu.

[0028] Furthermore, the adhesive layer may be made of either Ti or Cr.

[0029] Subsequently, AZ9260 thick-film positive photoresist was spin-coated onto the patterned electrode layer on the front side of the piezoelectric material. After soft baking at 95°C for 5 minutes, a photoresist layer for etching was obtained. The spin coating process employs a combination of low-speed photoresist spreading and high-speed photoresist homogenization. The specific steps are as follows: first, spin coating at 500 rpm for 10 seconds to evenly spread the photoresist, then spin coating at 2000 rpm for 60 seconds. The thickness of the spin-coated photoresist is measured using a step meter to obtain a photoresist layer with a thickness of 6 μm for etching.

[0030] 1.4 Fabrication of piezoelectric array etching masks on piezoelectric materials Based on the array design layout obtained in step 1.1 and the patterned electrode layer in step 1.3 as a reference, an exposure mask is fabricated. The array elements with different resonant frequencies in the exposure mask are set with different array element patterns and sizes. The exposure mask also includes isolation groove patterns between adjacent array elements, connection area patterns for realizing array element connection, and spacing area patterns for limiting the array element spacing.

[0031] Using the exposure mask as a reference, an ultraviolet lithography machine is used to expose the photoresist layer on the piezoelectric material for etching. The preferred exposure dose is 150 mJ / cm. 2 The exposed photoresist layer is obtained; After exposure, the exposed photoresist layer was developed using AZ400K developer (the volume ratio of developer to deionized water was 1:3) for 45 seconds. The developed photoresist layer was then immediately rinsed with deionized water for 30 seconds and dried with nitrogen to obtain a piezoelectric array etching mask. The edge integrity, opening width, and residual photoresist on the etching mask were then inspected using an optical microscope to ensure that array elements of different sizes and shapes were accurately transferred to the etching mask layer, thus obtaining a piezoelectric material with the etching mask.

[0032] 1.5 Fabrication of piezoelectric material arrays A piezoelectric material with an etching mask is placed in an ion beam etching apparatus. High-purity Ar (purity 5N, i.e., purity ≥ 99.999%) is used as the working gas to perform physical ion beam etching on the piezoelectric material with the array design pattern. The physical ion beam etching uses an ion energy of 500 eV and a current of 0.5 mA / cm². 2 With the beam current density set to 0.05 Pa and the Ar working pressure set to 0.05 Pa, a piezoelectric material array was obtained. The etching time and etching depth can be calibrated by conducting etching time and etching depth calibration experiments on actual piezoelectric material specimens to obtain the relationship curve between etching time and etching depth. Then, the etching time for the isolation groove on the piezoelectric material can be determined according to the etching depth required for the isolation groove between adjacent array elements.

[0033] The isolation trench between adjacent array elements includes the following structures: a completely isolated structure, a partially connected structure, or a combined structure with a predetermined coupling region. Specifically, the completely isolated structure refers to an isolation trench that penetrates the piezoelectric material, separating adjacent array elements within the piezoelectric material layer; the partially connected structure refers to an isolation trench that does not penetrate the piezoelectric material, but retains a piezoelectric material connection layer of predetermined thickness at the bottom of the isolation trench; the combined structure with a predetermined coupling region refers to a structure where most of the area between adjacent array elements is separated by the isolation trench, while retaining a connecting bridge, connecting rib, or locally unetched area formed by piezoelectric material at a predetermined position to constitute the predetermined coupling region.

[0034] 1.6 Fabrication of piezoelectric material arrays with PDMS filling layers PDMS (polydimethylsiloxane) prepolymer and curing agent (Sylgard 184 curing agent) were thoroughly mixed at a mass ratio of 8:1 for 5 minutes and then placed in a vacuum drying oven with a vacuum degree of -0.08MPa for 20 minutes for degassing. Degassing was stopped when the number of bubbles inside the PDMS was significantly reduced and the liquid level returned to stability, resulting in PDMS filling liquid. Under vacuum, the PDMS filling liquid was dropped onto the surface of the piezoelectric material array, allowing the PDMS filling liquid to fully enter the isolation groove of the piezoelectric material array for filling. After filling, the pressure was restored to normal to obtain the filling intermediate. The filling intermediate was heat-cured at 60℃ for 4 hours. After curing, it was naturally cooled to room temperature to obtain the piezoelectric material array with PDMS filling layer.

[0035] 1.7. The PDMS filling layer of the piezoelectric material array is planarized to obtain the PDMS matching layer. If the PDMS filling layer is thick and the difference between the height of the PDMS filling layer and the height of the piezoelectric material array surface is greater than 20 μm, the PDMS filling layer that is significantly higher than the piezoelectric material array surface is removed by first scraping, and then the PDMS filling layer and the piezoelectric material array surface are basically coplanar by low-speed mechanical grinding to obtain a PDMS matching layer with a thickness of 50 μm. After encapsulation, a multi-frequency piezoelectric material array is obtained. If the PDMS filling layer thickness is small, and the difference between the height of the PDMS filling layer and the height of the piezoelectric material array surface is >5μm and ≤20μm, then a mechanical scraping method is used to obtain a PDMS matching layer with a thickness of 50μm. After encapsulation, a multi-frequency piezoelectric material array is obtained.

[0036] Step 2: Fabrication of an integrated micro-ring array structure ultrasonic transducer The micro-ring receiving structure consists of an array of multiple micro-rings, which are connected sequentially by a straight waveguide to form a series optical transmission structure, thus constituting an arrayed optical ultrasonic receiving unit.

[0037] 2.1 Determine the layout of the micro-ring receiver array The micro-ring receiving array layout is designed based on the array element arrangement of the multi-frequency piezoelectric material array. Multiple micro-rings are arranged in a predetermined array pattern to obtain the designed pattern file, which is then imported into a two-photon 3D printer. The specific method for designing the micro-ring receiving array layout based on the array element arrangement of the multi-frequency piezoelectric material array is as follows: each micro-ring in the micro-ring array is spatially positioned corresponding to the array element of the corresponding multi-frequency piezoelectric material array, so that micro-rings at different positions receive the ultrasonic pressure signals propagating to the surface of the micro-ring receiving array from their corresponding regions.

[0038] 2.2 Two-photon 3D printing of micro-ring receiver array and straight waveguide A multi-frequency piezoelectric material array was fixed on the stage of a two-photon 3D printer. 0.8 ml of photoresist was dropped onto the PDMS matching layer of the array, and air bubbles were removed to form a photoresist layer for printing. Following a pre-designed pattern file, the three-dimensional structural model defined by the pattern file was sliced ​​in the printer's control software. The slice height was set to 145 nm, and the printing method was scan-fill. Subsequently, a 100× oil immersion objective lens from the two-photon 3D printer was used to print a sample with a wavelength of 1025 nm and a constant pulse repetition frequency of 0.8 MHz. The ultrashort pulse laser of z is focused onto the photoresist layer for printing on the PDMS matching layer. The rated output power of the laser is set to 1W, the processing power is set to 6% of the rated output power, and the processing rate is set to 4000 points / s. The photoresist layer for printing on the PDMS matching layer is cured, thereby forming a microring and a straight waveguide on the photoresist layer for printing. The microring serves as the sound pressure receiving unit, with a radius of 30μm and a cross-sectional width and height of 1.2μm. The straight waveguide serves as the connection unit between the light source input and output, with a cross-sectional width and height of 1.2μm. Furthermore, a coupling gap of 150 nm is provided between the microring and the straight waveguide.

[0039] 2.3 The processing substrate was sequentially immersed in PGMEA, isopropanol and n-hexanol to obtain an ultrasonic transducer of multi-frequency piezoelectric material and 3D printed microring; After curing, the entire processed substrate obtained in the previous step is removed and vertically immersed in PGMEA (propylene glycol methyl ether acetate) for 5 minutes for development to dissolve and remove uncured resin that has not undergone two-photon polymerization. Then, the processed substrate is removed and vertically immersed in isopropanol for 3 minutes to remove residual PGMEA and residual resin and reduce developer residue. After that, the processed substrate is removed and vertically immersed in n-hexanol for 2 minutes to remove isopropanol, resulting in the processed substrate after treatment. The processed substrate is then removed with tweezers and allowed to air dry naturally to evaporate any residual n-hexanol on the substrate. It is then placed in a clean container to obtain an ultrasonic transducer of multi-frequency piezoelectric material and 3D printed microrings.

[0040] Example 2: Figures 1-2 As shown, the method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings specifically includes the following steps: Step 1: Etching the multi-frequency piezoelectric material wafer array 1.1 Array Design Layout A piezoelectric material with a thickness of 0.32 mm was selected as the substrate of the piezoelectric array. The array structure was designed according to the target ultrasonic working frequency and the array arrangement to form a multi-frequency piezoelectric array. The array design layout was determined based on the multi-frequency piezoelectric array. The piezoelectric material used is a PZT piezoelectric wafer.

[0041] The array arrangement includes adjacent arrangement, alternating arrangement, partitioned arrangement, chessboard arrangement, and row and column arrangement.

[0042] The array structure is formed by combining array elements with different resonant frequencies.

[0043] 1.2 Pretreatment of piezoelectric materials and formation of backing layer After cleaning, drying and planarizing the piezoelectric material, the back of the piezoelectric material is polished and E-solder 3022 conductive silver paste is bonded and cured at 85°C for 1.5 hours. After grinding, a backing layer with a thickness of 2.0 mm is obtained.

[0044] The E-solder 3022 conductive silver paste is obtained by thoroughly mixing silver epoxy resin and a hardener at a mass ratio of 100:9.

[0045] Furthermore, the hardener used is Hardener No. 18, which is compatible with E-solder 3022 silver-filled epoxy resin compound.

[0046] 1.3 Electrode layer fabrication and photoresist layer formation A common electrode is deposited on the back side of the piezoelectric material using ion beam sputtering to provide a common potential terminal for each piezoelectric element and to form a unified electric field reference in the thickness direction of the piezoelectric material. A patterned electrode layer is deposited on the front side of the piezoelectric material using photolithography and ion beam sputtering. The patterned electrode layer corresponds to the spatial position of each element and is used to electrically excite different elements independently or in groups, so that each element generates mechanical vibration and ultrasonic waves of corresponding frequencies under the action of an external electric field. The common electrode layer and the patterned electrode layer are conductive metal layers with a thickness of 300 nm.

[0047] Furthermore, the conductive metal layer is preferably made of Cu; an adhesion layer with a thickness of 20 nm can also be provided between Cu and the piezoelectric material, and an Au anti-oxidation protective layer with a thickness of 75 nm can also be provided on the outer surface of Cu.

[0048] Furthermore, the adhesive layer may be made of either Ti or Cr.

[0049] Subsequently, AZ9260 thick-film positive photoresist was spin-coated onto the patterned electrode layer on the front side of the piezoelectric material and soft-baked at 110°C for 2 minutes to obtain the photoresist layer for etching. The spin coating process employs a combination of low-speed photoresist spreading and high-speed photoresist homogenization. The specific steps are as follows: First, spin coating at 800 rpm for 5 seconds to evenly spread the photoresist, then spin coating at 3000 rpm for 30 seconds. The thickness of the spin-coated photoresist is measured using a step meter to obtain a 10 μm thick photoresist layer for etching.

[0050] 1.4 Fabrication of piezoelectric array etching masks on piezoelectric materials Based on the array design layout obtained in step 1.1 and the patterned electrode layer in step 1.3 as a reference, an exposure mask is fabricated. The array elements with different resonant frequencies in the exposure mask are set with different array element patterns and sizes. The exposure mask also includes isolation groove patterns between adjacent array elements, connection area patterns for realizing array element connection, and spacing area patterns for limiting the array element spacing.

[0051] Using the exposure mask as a reference, an ultraviolet lithography machine is used to expose the photoresist layer on the piezoelectric material for etching. The preferred exposure dose is 300 mJ / cm. 2 The exposed photoresist layer is obtained; After exposure, the exposed photoresist layer was developed using AZ400K developer (developer to deionized water volume ratio of 1:4) for 90 seconds to obtain the developed photoresist layer. Immediately after development, the photoresist layer was rinsed with deionized water for 60 seconds and dried with nitrogen to obtain a piezoelectric array etching mask. Then, the edge integrity, opening width, and residual photoresist on the etching mask were inspected using an optical microscope to ensure that array element patterns of different sizes and shapes were accurately transferred to the etching mask layer, thus obtaining a piezoelectric material with the etching mask. 1.5 Fabrication of piezoelectric material arrays A piezoelectric material with an etching mask is placed in an ion beam etching apparatus. High-purity Ar (purity 5N, i.e., purity ≥ 99.999%) is used as the working gas to perform physical ion beam etching on the piezoelectric material with the etching mask. The physical ion beam etching employs an ion energy of 800 eV and a current of 0.8 mA / cm². 2 With the beam current density set to 0.15 Pa and the Ar working pressure set to 0.15 Pa, a piezoelectric material array was obtained. The etching time and etching depth can be calibrated by conducting etching time and etching depth calibration experiments on actual piezoelectric material specimens to obtain the relationship curve between etching time and etching depth. Then, the etching time for the isolation groove on the piezoelectric material can be determined according to the etching depth required for the isolation groove between adjacent array elements.

[0052] The isolation trench between adjacent array elements includes the following structures: a completely isolated structure, a partially connected structure, or a combined structure with a predetermined coupling region. Specifically, the completely isolated structure refers to an isolation trench that penetrates the piezoelectric material, separating adjacent array elements within the piezoelectric material layer; the partially connected structure refers to an isolation trench that does not penetrate the piezoelectric material, but retains a piezoelectric material connection layer of predetermined thickness at the bottom of the isolation trench; the combined structure with a predetermined coupling region refers to a structure where most of the area between adjacent array elements is separated by the isolation trench, while retaining a connecting bridge, connecting rib, or locally unetched area formed by piezoelectric material at a predetermined position to constitute the predetermined coupling region.

[0053] 1.6 Fabrication of piezoelectric material arrays with PDMS filling layers PDMS (polydimethylsiloxane) prepolymer and curing agent (Sylgard 184 curing agent) were thoroughly mixed at a mass ratio of 12:1 for 10 min and then placed in a vacuum drying oven with a vacuum degree of -0.095 MPa for degassing treatment for 40 min. Degassing was stopped when the number of bubbles inside the PDMS was significantly reduced and the liquid level returned to stability, resulting in PDMS filling liquid. Under vacuum, the PDMS filling liquid was scraped onto the surface of the piezoelectric material array, allowing the PDMS filling liquid to fully enter the isolation groove of the piezoelectric material array for filling. After filling, the pressure was restored to normal to obtain the filling intermediate. The filling intermediate was thermo-cured at 80℃ for 2 h. After curing, it was naturally cooled to room temperature to obtain the piezoelectric material array with PDMS filling layer.

[0054] 1.7. The PDMS filling layer of the piezoelectric material array is planarized to obtain the PDMS matching layer. If the PDMS filling layer is thick and the difference between the height of the PDMS filling layer and the height of the piezoelectric material array surface is greater than 20 μm, the PDMS filling layer that is significantly higher than the piezoelectric material array surface is removed by spin coating first, and then precision polishing is used to make the PDMS filling layer and the piezoelectric material array surface basically coplanar to obtain a PDMS matching layer with a thickness of 60 μm. After encapsulation, a multi-frequency piezoelectric material array is obtained. If the PDMS filling layer thickness is small, and the difference between the height of the PDMS filling layer and the height of the piezoelectric material array surface is >5μm and ≤20μm, then a soft mold flattening method is used to obtain a PDMS matching layer with a thickness of 60μm. After encapsulation, a multi-frequency piezoelectric material array is obtained.

[0055] Step 2: Fabrication of an integrated micro-ring array structure ultrasonic transducer The micro-ring receiving structure consists of an array of multiple micro-rings, which are connected sequentially by a straight waveguide to form a series optical transmission structure, thus constituting an arrayed optical ultrasonic receiving unit.

[0056] 2.1 Determine the layout of the micro-ring receiver array The micro-ring receiving array layout is designed based on the array element arrangement of the multi-frequency piezoelectric material array. Multiple micro-rings are arranged in a predetermined array pattern to obtain the designed pattern file, which is then imported into a two-photon 3D printer. The specific method for designing the micro-ring receiving array layout based on the array element arrangement of the multi-frequency piezoelectric material array is as follows: each micro-ring in the micro-ring array is spatially positioned corresponding to the array element of the corresponding multi-frequency piezoelectric material array, so that micro-rings at different positions receive the ultrasonic pressure signals propagating to the surface of the micro-ring receiving array from their corresponding regions.

[0057] 2.2 Two-photon 3D printing of micro-ring receiver array and straight waveguide A multi-frequency piezoelectric material array was fixed on the stage of a two-photon 3D printer. 1.2 ml of photoresist was dropped onto the PDMS matching layer of the array, and air bubbles were removed to form a photoresist layer for printing. Following a pre-designed pattern file, the three-dimensional structural model defined by the pattern file was sliced ​​in the printer's control software. The slice height was set to 155 nm, and the printing method was scan-fill. Subsequently, a 100× oil immersion objective lens from the two-photon 3D printer was used to print a sample with a wavelength of 1035 nm and a constant pulse repetition frequency of 1.2 MHz. The ultrashort pulse laser of z is focused onto the photoresist layer for printing on the PDMS matching layer. The rated output power of the laser is set to 1W, the processing power is set to 10% of the rated output power, and the processing rate is set to 6000 points / s. The photoresist layer for printing on the PDMS matching layer is cured, thereby forming a microring and a straight waveguide on the photoresist layer for printing. The microring serves as the sound pressure receiving unit, with a radius of 50μm and a cross-sectional width and height of 1.8μm. The straight waveguide serves as the connection unit between the light source input and output, with a cross-sectional width and height of 1.8μm. Furthermore, a 300nm coupling gap is provided between the microring and the straight waveguide.

[0058] 2.3 The processing substrate was sequentially immersed in PGMEA, isopropanol and n-hexanol to obtain an ultrasonic transducer of multi-frequency piezoelectric material and 3D printed microring; After curing, the entire processed substrate obtained in the previous step is removed and vertically immersed in PGMEA (propylene glycol methyl ether acetate) for 5 minutes for development to dissolve and remove uncured resin that has not undergone two-photon polymerization. Then, the processed substrate is removed and vertically immersed in isopropanol for 3 minutes to remove residual PGMEA and residual resin and reduce developer residue. After that, the processed substrate is removed and vertically immersed in n-hexanol for 2 minutes to remove isopropanol, resulting in the processed substrate after treatment. The processed substrate is then removed with tweezers and allowed to air dry naturally to evaporate any residual n-hexanol on the substrate. It is then placed in a clean container to obtain an ultrasonic transducer of multi-frequency piezoelectric material and 3D printed microrings.

[0059] Example 3: As Figures 1-2 As shown, the method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings specifically includes the following steps: Step 1: Etching the multi-frequency piezoelectric material wafer array 1.1 Array Design Layout A piezoelectric material with a thickness of 0.3 mm was selected as the substrate of the piezoelectric array. The array structure was designed according to the target ultrasonic working frequency and the array arrangement to form a multi-frequency piezoelectric array. The array design layout was determined based on the multi-frequency piezoelectric array. The piezoelectric material used is a PZT piezoelectric wafer.

[0060] The array arrangement includes adjacent arrangement, alternating arrangement, partitioned arrangement, chessboard arrangement, and row and column arrangement.

[0061] The array structure is formed by combining array elements with different resonant frequencies.

[0062] 1.2 Pretreatment of piezoelectric materials and formation of backing layer After cleaning, drying and planarizing the piezoelectric material, the back of the piezoelectric material is polished and E-solder 3022 conductive silver paste is bonded on it. It is cured at 65°C for 3 hours and then ground to obtain a backing layer with a thickness of 1.0 mm.

[0063] The E-solder 3022 conductive silver paste is obtained by thoroughly mixing silver epoxy resin and hardener at a mass ratio of 100:8.

[0064] Furthermore, the hardener used is Hardener No. 18, which is compatible with E-solder 3022 silver-filled epoxy resin compound.

[0065] 1.3 Electrode layer fabrication and photoresist layer formation A common electrode is deposited on the back side of the piezoelectric material using ion beam sputtering to provide a common potential terminal for each piezoelectric element and to form a unified electric field reference in the thickness direction of the piezoelectric material. A patterned electrode layer is deposited on the front side of the piezoelectric material using photolithography and ion beam sputtering. The patterned electrode layer corresponds to the spatial position of each element and is used to electrically excite different elements independently or in groups, so that each element generates mechanical vibration and ultrasonic waves of corresponding frequencies under the action of an external electric field. The common electrode layer and the patterned electrode layer are conductive metal layers with a thickness of 250 nm.

[0066] Furthermore, the conductive metal layer is preferably made of Cu; an adhesion layer with a thickness of 20 nm can also be provided between Cu and the piezoelectric material, and an Au anti-oxidation protective layer with a thickness of 75 nm can also be provided on the outer surface of Cu.

[0067] Furthermore, the adhesive layer may be made of either Ti or Cr.

[0068] Subsequently, AZ9260 thick-film positive photoresist was spin-coated onto the patterned electrode layer on the front side of the piezoelectric material, and after soft baking at 102°C for 3.5 min, a photoresist layer for etching was obtained. The spin coating process employs a combination of low-speed photoresist spreading and high-speed photoresist homogenization. The specific steps are as follows: First, spin coating is performed at 650 rpm for 8 seconds to spread the photoresist evenly. Then, spin coating is performed at 2500 rpm for 45 seconds. The thickness of the spin-coated photoresist is measured using a profilometer to obtain a photoresist layer with a thickness of 8 μm for etching.

[0069] 1.4 Fabrication of piezoelectric array etching masks on piezoelectric materials Based on the array design layout obtained in step 1.1 and the patterned electrode layer in step 1.3 as a reference, an exposure mask is fabricated. The array elements with different resonant frequencies in the exposure mask are set with different array element patterns and sizes. The exposure mask also includes isolation groove patterns between adjacent array elements, connection area patterns for realizing array element connection, and spacing area patterns for limiting the array element spacing.

[0070] Using an exposure mask as a reference, an ultraviolet lithography machine is used to expose the photoresist layer on the piezoelectric material for etching. The preferred exposure dose is 220 mJ / cm². 2 The exposed photoresist layer is obtained; After exposure, the exposed photoresist layer was developed using AZ400K developer (developer to deionized water volume ratio of 1:3.5) for 75 seconds, resulting in a developed photoresist layer. Immediately after development, the photoresist layer was rinsed with deionized water for 45 seconds and dried with nitrogen to obtain a piezoelectric array etching mask. The edge integrity, opening width, and residual photoresist on the etching mask were then inspected using an optical microscope to ensure that array elements of different sizes and shapes were accurately transferred to the etching mask layer, resulting in a piezoelectric material with the etching mask. 1.5 Fabrication of piezoelectric material arrays A piezoelectric material with an etching mask is placed in an ion beam etching apparatus. High-purity Ar (purity 5N, i.e., purity ≥ 99.999%) is used as the working gas to perform physical ion beam etching on the piezoelectric material with the etching mask. The physical ion beam etching uses an ion energy of 650 eV and a current of 0.6 mA / cm². 2 With the beam current density set to 0.1 Pa and the Ar working pressure set to 0.1 Pa, a piezoelectric material array was obtained. The etching time and etching depth can be calibrated by conducting etching time and etching depth calibration experiments on actual piezoelectric material specimens to obtain the relationship curve between etching time and etching depth. Then, the etching time for the isolation groove on the piezoelectric material can be determined according to the etching depth required for the isolation groove between adjacent array elements.

[0071] The isolation trench between adjacent array elements includes the following structures: a completely isolated structure, a partially connected structure, or a combined structure with a predetermined coupling region. Specifically, the completely isolated structure refers to an isolation trench that penetrates the piezoelectric material, separating adjacent array elements within the piezoelectric material layer; the partially connected structure refers to an isolation trench that does not penetrate the piezoelectric material, but retains a piezoelectric material connection layer of predetermined thickness at the bottom of the isolation trench; the combined structure with a predetermined coupling region refers to a structure where most of the area between adjacent array elements is separated by the isolation trench, while retaining a connecting bridge, connecting rib, or locally unetched area formed by piezoelectric material at a predetermined position to constitute the predetermined coupling region.

[0072] 1.6 Fabrication of piezoelectric material arrays with PDMS filling layers PDMS prepolymer and curing agent (Sylgard 184 curing agent) were thoroughly mixed at a mass ratio of 10:1 for 7 minutes and then placed in a vacuum drying oven with a vacuum degree of -0.088MPa for degassing treatment for 30 minutes. Degassing was stopped when the number of bubbles inside the PDMS was significantly reduced and the liquid level returned to stability, resulting in PDMS filling liquid. Under vacuum, the PDMS filling liquid was dropped onto the surface of the piezoelectric material array, allowing the PDMS filling liquid to fully enter the isolation groove of the piezoelectric material array for filling. After filling, the pressure was restored to normal to obtain the filling intermediate. The filling intermediate was thermo-cured at 70℃ for 3 hours. After curing, it was naturally cooled to room temperature to obtain the piezoelectric material array with PDMS filling layer.

[0073] 1.7. The PDMS filling layer of the piezoelectric material array is planarized to obtain the PDMS matching layer. If the PDMS filling layer is thick and the difference between the height of the PDMS filling layer and the height of the piezoelectric material array surface is greater than 20 μm, the PDMS filling layer that is significantly higher than the piezoelectric material array surface is removed by first flattening, and then the PDMS filling layer and the piezoelectric material array surface are basically coplanar by low-speed mechanical grinding to obtain a PDMS matching layer with a thickness of 55 μm. After encapsulation, a multi-frequency piezoelectric material array is obtained. If the PDMS filling layer thickness is small, and the difference between the height of the PDMS filling layer and the height of the piezoelectric material array surface is >5μm and ≤20μm, then a mechanical scraping method is used to obtain a PDMS matching layer with a thickness of 55μm. After encapsulation, a multi-frequency piezoelectric material array is obtained.

[0074] Step 2: Fabrication of an integrated micro-ring array structure ultrasonic transducer The micro-ring receiving structure consists of an array of multiple micro-rings, which are connected sequentially by a straight waveguide to form a series optical transmission structure, thus constituting an arrayed optical ultrasonic receiving unit.

[0075] 2.1 Determine the layout of the micro-ring receiver array The micro-ring receiving array layout is designed based on the array element arrangement of the multi-frequency piezoelectric material array. Multiple micro-rings are arranged in a predetermined array pattern to obtain the designed pattern file, which is then imported into a two-photon 3D printer. The specific method for designing the micro-ring receiving array layout based on the array element arrangement of the multi-frequency piezoelectric material array is as follows: each micro-ring in the micro-ring array is spatially positioned corresponding to the array element of the corresponding multi-frequency piezoelectric material array, so that micro-rings at different positions receive the ultrasonic pressure signals propagating to the surface of the micro-ring receiving array from their corresponding regions.

[0076] 2.2 Two-photon 3D printing of micro-ring receiver array and straight waveguide A multi-frequency piezoelectric material array was fixed on the stage of a two-photon 3D printer. 1 ml of photoresist was dropped onto the PDMS matching layer of the array, and air bubbles were removed to form a photoresist layer for printing. Following a pre-designed pattern file, the three-dimensional structural model defined by the pattern file was sliced ​​in the printer's control software. The slice height was set to 150 nm, and the printing method was scan-fill. Subsequently, a 100× oil immersion objective lens of the two-photon 3D printer was used to print a sample with a wavelength of 1030 nm and a constant pulse repetition frequency of 1 MHz. An ultrashort pulse laser is focused onto a photoresist layer on a PDMS matching layer for printing. The laser's rated output power is set to 1W, the processing power is set to 8% of the rated output power, and the processing rate is set to 5000 points / s. This process cures the photoresist layer on the PDMS matching layer, thereby forming a microring and a straight waveguide on the photoresist layer. The microring serves as an acoustic pressure receiving unit with a radius of 40μm and a cross-sectional width and height of 1.5μm. The straight waveguide serves as the connection unit between the light source input and output, and its cross-sectional width and height are also 1.5μm. Furthermore, a 200nm coupling gap is provided between the microring and the straight waveguide.

[0077] 2.3 The processing substrate was sequentially immersed in PGMEA, isopropanol and n-hexanol to obtain an ultrasonic transducer of multi-frequency piezoelectric material and 3D printed microring; After curing, the entire processed substrate obtained in the previous step is removed and vertically immersed in PGMEA (propylene glycol methyl ether acetate) for 5 minutes for development to dissolve and remove uncured resin that has not undergone two-photon polymerization. Then, the processed substrate is removed and vertically immersed in isopropanol for 3 minutes to remove residual PGMEA and residual resin and reduce developer residue. After that, the processed substrate is removed and vertically immersed in n-hexanol for 2 minutes to remove isopropanol, resulting in the processed substrate after treatment. The processed substrate is then removed with tweezers and allowed to air dry naturally to evaporate any residual n-hexanol on the substrate. It is then placed in a clean container to obtain an ultrasonic transducer of multi-frequency piezoelectric material and 3D printed microrings.

[0078] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings, characterized by comprising the following steps: Step 1: Etching the multi-frequency piezoelectric material wafer array 1.1 Design the array layout; 1.

2. Prepare a backing layer on the back of the piezoelectric material; 1.

3. A common electrode is deposited on the back side of the piezoelectric material, and a patterned electrode layer is deposited on the front side of the piezoelectric material. Subsequently, a photoresist layer for etching is fabricated on the patterned electrode layer; 1.

4. Based on the array design layout and using the patterned electrode layer as a reference, fabricate an exposure mask; using the exposure mask as a reference, sequentially expose, develop, rinse and dry the photoresist layer used for etching to obtain a piezoelectric material with an etching mask. 1.

5. Place the piezoelectric material with the etching mask in an ion beam etching device and perform physical ion beam etching on the piezoelectric material to obtain a piezoelectric material array; 1.

6. The piezoelectric material array is filled with a filling liquid and then cured to obtain a piezoelectric material array with a filling layer; then the surface is planarized to obtain a matching layer, and after encapsulation, a multi-frequency piezoelectric material array is obtained. Step 2: Fabrication of an integrated micro-ring array structure ultrasonic transducer 2.1 Design the micro-ring receiving array layout based on the array element arrangement of the multi-frequency piezoelectric material array, obtain the designed pattern file, and import it into the 3D printer; 2.2 First, a photoresist layer for printing is prepared on the matching layer of the multi-frequency piezoelectric material array. Then, micro-rings and straight waveguides are formed on the photoresist layer for printing using a 3D printer to obtain the processing substrate. 2.3 The substrate is sequentially developed, terminated, replaced, and dried to obtain an ultrasonic transducer of multi-frequency piezoelectric material and 3D printed microring.

2. The method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings according to claim 1, characterized in that the piezoelectric material is a PZT piezoelectric wafer; the conductive silver paste is an E-solder 3022 conductive silver paste; the electrode materials used for the common electrode and the patterned electrode layer are both Cu; the photoresist is an AZ9260 thick-film positive photoresist; and the developer is an AZ400K developer.

3. The method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings according to claim 1, characterized in that, Step 1.2 specifically involves cleaning, drying, and planarizing the piezoelectric material, then polishing and bonding conductive silver paste to the back of the piezoelectric material, followed by curing to obtain a backing layer.

4. The method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings according to claim 1, characterized in that, Step 1.3 specifically involves: depositing a common electrode on the back side of the piezoelectric material using ion beam sputtering; depositing a patterned electrode layer on the front side of the piezoelectric material using photolithography and ion beam sputtering; then spin-coating photoresist onto the patterned electrode layer on the front side of the piezoelectric material, and obtaining a photoresist layer for etching after soft baking.

5. The method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings according to claim 1, characterized in that, In step 1.3, the spin coating adopts a combination of low-speed photoresist spreading and high-speed photoresist homogenization. The specific steps are as follows: first, spin coating at 500~800 rpm for 5~10s to spread the photoresist evenly, and then spin coating at 2000~3000 rpm for 30~60s.

6. The method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings according to claim 1, characterized in that, In step 1.4, the exposure dose is 150~300 mJ / cm. 2 .

7. The method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings according to claim 1, characterized in that, In step 1.5, the physical ion beam etching uses an ion energy of 500-800 eV and a current of 0.5-0.8 mA / cm². 2 The beam current density was set, and the Ar working pressure was set to 0.05~0.15Pa. At the same time, the etching time and etching depth were calibrated by using actual piezoelectric material test pieces to obtain the relationship curve between etching time and etching depth. Then, the etching time at the isolation groove on the piezoelectric material was determined according to the etching depth required for the isolation groove between adjacent array elements.

8. The method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings according to claim 1, characterized in that, In step 1.6, the specific filling method is as follows: under vacuum environment, the PDMS filling liquid is fully introduced into the isolation tank of the piezoelectric material array for filling, and after filling is completed, the pressure is restored to normal.

9. The method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings according to claim 1, characterized in that, In step 2.1, the specific method for designing the micro-ring receiving array layout based on the array element arrangement of the multi-frequency piezoelectric material array is as follows: each micro-ring in the micro-ring array is spatially positioned corresponding to the array element of the corresponding multi-frequency piezoelectric material array.

10. The method for fabricating an ultrasonic transducer based on multi-frequency piezoelectric materials and 3D-printed microrings according to claim 1, characterized in that, In step 2.2, the specific steps for forming micro-rings and straight waveguides on the photoresist layer used for printing using a two-photon 3D printer are as follows: using the 100× oil immersion objective of the two-photon 3D printer, an ultrashort pulse laser with a wavelength of 1025~1035nm and a pulse repetition frequency of 0.8~1.2MHz is focused onto the photoresist layer used for printing. The rated output power of the laser is set to 1W, the processing power is set to 6~10% of the rated output power, and the processing rate is set to 4000~6000 points / s. The photoresist layer used for printing on the matching layer is cured, thereby forming micro-rings and straight waveguides on the photoresist layer used for printing.