Wafer debonding method
By using infrared laser scanning to vaporize and expand the wafer bonding material, the problem of damage and debris contamination to ultrathin wafers caused by mechanical debonding is solved, achieving efficient and stable wafer debonding, which is suitable for high-temperature processes and mass production of ultrathin wafers.
Patent Information
- Application Number
- CN202611236302.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing mechanical debonding methods are prone to mechanical stress damage to ultrathin wafers, require high operational precision, pose a high risk of debris contamination, and are difficult to adapt to high-temperature processes. Traditional ultraviolet laser methods are incompatible with silicon substrates.
Infrared lasers are used to scan the non-chip areas of wafer bonding pairs, causing the bonding material to vaporize and expand. Debonding is achieved with a small pulling force, avoiding mechanical contact and chip damage, and is suitable for high-temperature processes.
It achieves wafer debonding with no mechanical contact, no chip damage, low stress, and high capacity, which is suitable for mass production of ultra-thin wafers, broadens application scenarios, and reduces operational complexity and the risk of debris contamination.
Smart Images

Figure CN123124697A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of wafer processing technology and relates to a method for debonding wafers. Background Technology
[0002] In the fields of advanced semiconductor packaging, microelectromechanical systems (MEMS), and 3D integrated circuit (3D-IC) manufacturing, wafer temporary bonding and debonding technologies are key process steps for achieving wafer thinning and back-side processes (such as photolithography, etching, and deposition). A typical process flow is as follows: First, the device wafer is bonded to a rigid carrier (such as a silicon or glass carrier) using temporary bonding materials to form a wafer bonding pair; then, the device wafer undergoes back-side thinning and subsequent processes; finally, the thinned device wafer is separated from the carrier through a debonding process to obtain an ultra-thin chip.
[0003] Currently, the mainstream debonding methods include mechanical debonding, thermal slip debonding, and ultraviolet (UV) laser debonding. Among them, mechanical debonding is widely used due to its low cost and simple operation. In the mechanical debonding process, a crucial pre-step is "vacuum breaking", which means breaking the vacuum seal at the edge of the bond pair to facilitate the subsequent separation of the bond pair by the suction nozzle under mechanical force. Traditional vacuum breaking methods generally adopt blade insertion, which uses an extremely thin metal blade to physically insert from the edge gap of the wafer bond pair to break the vacuum state at the edge. However, this method has the following significant problems in practical applications: (1) Risk of mechanical stress damage: For ultra-thin device wafers with a thickness of only tens of micrometers after thinning, the local mechanical stress generated by blade insertion can easily cause microcracks, fragments, or even complete breakage at the edge of the wafer, seriously affecting the product yield. (2) High operational precision requirements: The depth and angle of blade insertion are difficult to control precisely. If it is too shallow, it cannot effectively break the vacuum, and if it is too deep, it may damage the chip area of the device. (3) Debris contamination: The physical contact process may generate tiny particles of debris. Once these debris enters the clean bonding interface, they will become a source of contamination for subsequent processes. (4) Poor adaptability to high-strength bonding interfaces: After high-temperature (e.g., above 300°C) processes, the bonding strength of some temporary bonding materials will be enhanced, resulting in an increased breakage rate.
[0004] To address the aforementioned issues, various improvement schemes have been attempted in existing technologies. For example, a 248-355nm ultraviolet laser is used to scan the bonding layer across the entire area, relying on photosensitive adhesive for photodecomposition and peeling. Even if the laser path is limited to scanning only along the dicing grid, high-energy ultraviolet light will still scatter and transmit to the active region of the die, ablate the passivation layer (PI layer) on the chip surface, and cause device failure. Furthermore, ultraviolet lasers are only compatible with transparent glass substrates and cannot be used with silicon substrates.
[0005] Therefore, developing a debonding method that is non-mechanically contactless, causes no damage to the chip surface, has low stress, high throughput, and is compatible with the mass production requirements of ultra-thin wafers is a technical problem that urgently needs to be solved. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide a wafer debonding method. The debonding method provided by this invention utilizes infrared laser to scan the non-chip regions of the wafer bonding pairs. After laser scanning, no mechanical debonding is required; wafer debonding can be achieved through simple lifting with minimal pulling force. This method offers good process repeatability, stable debonding results, no mechanical contact, no chip surface damage, low stress, and high throughput. It is more suitable for the mass production needs of panelized ultra-thin wafers, overcoming the limitations of traditional processes that are difficult to adapt to high-temperature wafer fabrication, and broadening its application scenarios.
[0007] To achieve this objective, the present invention adopts the following technical solution:
[0008] This invention provides a method for debonding wafers, the method comprising the following steps:
[0009] Provide wafer bonding pairs to be debonded, perform infrared laser scanning on the non-chip areas of the wafer bonding pairs to be debonded, causing the bonding material in the wafer bonding pairs to vaporize and expand the gas outward from the vaporization location as the center, to obtain wafer bonding pairs after preliminary treatment of the bonding surface;
[0010] After the bonding surface has been pre-processed, the carrier wafer of the wafer bonding pair is pulled up to complete the debonding of the wafer.
[0011] The non-chip region includes the edge region and dicing region of the wafer bond pair to be debonded; the raw materials of the bonding material of the wafer bond pair to be debonded include thermally decomposable resin and photosensitive resin.
[0012] In one embodiment of the present invention, the expansion width of the gas expansion from the vaporization position to the expansion edge of the gas expansion is 5mm to 20mm.
[0013] In one embodiment of the present invention, the gas between adjacent cutting channel regions expands to the point where the gas is interconnected.
[0014] In one embodiment of the present invention, the pulling force is ≤8N.
[0015] In one embodiment of the present invention, during the laser scanning process, the bonding edges of the wafer bonding pairs to be debonded are subjected to auxiliary air blowing treatment and / or the pressure in the laser scanning environment is reduced.
[0016] In one embodiment of the present invention, the mass ratio of the thermally decomposable resin to the photosensitive resin is (1~3):(3~1).
[0017] In one embodiment of the present invention, the thermally decomposable resin includes any one or a combination of at least two of the following: silicone resin, polyimide resin, polycarbonate resin, or polymethyl methacrylate.
[0018] In one embodiment of the present invention, the raw materials of the bonding material further include a diluent and an antioxidant.
[0019] In one embodiment of the present invention, the wavelength of the laser used for infrared laser scanning is 0.2μm~11μm.
[0020] In one embodiment of the present invention, the power of the infrared laser scanning is 20W to 2000W.
[0021] In one embodiment of the present invention, the scanning speed of the infrared laser scanning is 20 mm / s to 20000 mm / s.
[0022] In one embodiment of the present invention, the number of infrared laser scans is 1 to 100.
[0023] In one embodiment of the present invention, the wafer bonding pairs to be debonded include wafer bonding pairs of device wafers and carrier wafers.
[0024] In one embodiment of the present invention, the width of the edge region of the wafer bonding pair to be debonded is 2mm to 5mm.
[0025] In one embodiment of the present invention, the bonding strength of the wafer bonding pairs to be debonded is 0.2 MPa to 1 MPa.
[0026] In one embodiment of the present invention, the device wafer includes an ultrathin wafer.
[0027] In one embodiment of the present invention, the laser scanning scans the non-chip region of the carrier wafer.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] This invention uses infrared laser scanning on the non-chip areas of wafer bonding pairs to be debonded, without direct contact with the wafer. Instead, the laser is selectively absorbed by the thermally decomposable resin and photosensitive resin in the bonding material, inducing the resin (especially the thermally decomposable resin) to thermally decompose and vaporize, generating small molecule gases (such as methane, ethane, siloxane gases, etc.). These gases expand outwards from the vaporization point, not only breaking the vacuum at the edge of the wafer bonding pair but also separating the bonding interface in the dicing area. This separation effect allows for one-step wafer debonding under low tension, eliminating the need for additional mechanical debonding operations. The process has good repeatability, stable debonding effect, no mechanical contact, no chip surface damage, low stress, and high throughput, making it more suitable for the mass production needs of panelized ultra-thin wafers. It solves the limitation of traditional processes being difficult to adapt to high-temperature wafer processes and broadens the application scenarios. Attached Figure Description
[0030] Figure 1 This is a process flow diagram of the wafer bonding and debonding process provided in Embodiment 1 of the present invention. Detailed Implementation
[0031] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0032] The "range" disclosed in this invention can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of the specific range. This type of range definition can include or exclude endpoints; any endpoint can be independently included or excluded, and they can be arbitrarily combined, meaning any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60~120 and 80~110 are listed for specific parameters, it is understood that ranges of 60~110 and 80~120 are also expected. Furthermore, if minimum range values 1 and 2 are listed, and maximum range values 3, 4, and 5 are also listed, then the following ranges are all expected: 1~3, 1~4, 1~5, 2~3, 2~4, and 2~5. In this invention, unless otherwise stated, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0" and "5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is described as an integer ≥2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For instance, when a parameter is described as an integer selected from "2~10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.
[0033] In this invention, "a combination of at least two" refers to a quantity greater than or equal to two, unless otherwise specified. For example, "any combination of one or at least two" means one or more or more items. It can be understood that when referring to "a combination of at least two," it refers to any suitable combination of multiple items, that is, a combination of "at least two" items carried out in a manner that does not conflict with and enables the implementation of this invention.
[0034] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions.
[0035] The term "embodiment" as used in this invention means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a mutually exclusive, independent, or alternative embodiment. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described in this invention can be combined with other embodiments.
[0036] In this invention, open-ended technical features or solutions described using terms such as "comprising" do not exclude additional members beyond those listed unless otherwise specified. They can be considered as providing both closed-ended features or solutions comprised of the listed members and open-ended features or solutions that include additional members beyond the listed members. For example, A includes a1, a2, and a3. Unless otherwise specified, it may also include other members or exclude additional members. This can be considered as providing both technical features or solutions where "A is composed of a1, a2, and a3" or "A is selected from a1, a2, and a3," and technical features or solutions where "A includes not only a1, a2, and a3, but also other members."
[0037] In this invention, unless otherwise specified, the features or solutions corresponding to "and / or" include any one of two or more of the related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" represents a group consisting of A, B, and "a combination of A and B". "Containing A and / or B" can mean "containing A, containing B, and containing A and B", or "containing A, containing B, or containing A and B", and can be appropriately understood according to the context.
[0038] In this invention, the terms "first aspect," "second aspect," "third aspect," "fourth aspect," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first," "second," "third," "fourth," etc., serve only as a non-exhaustive enumeration and should be understood not to constitute a closed limitation on the quantity.
[0039] In this invention, "room temperature" generally refers to 4℃~35℃, and can refer to 20℃±5℃. In some embodiments of this invention, room temperature refers to 20℃~30℃.
[0040] In one embodiment, the present invention provides a method for debonding wafers, the method comprising the following steps:
[0041] Provide wafer bonding pairs to be debonded, perform infrared laser scanning on the non-chip areas of the wafer bonding pairs to be debonded, causing the bonding material in the wafer bonding pairs to vaporize and expand the gas outward from the vaporization location as the center, to obtain wafer bonding pairs after preliminary treatment of the bonding surface;
[0042] After the bonding surface has been pre-processed, the carrier wafer of the wafer bonding pair is pulled up to complete the debonding of the wafer.
[0043] The non-chip region includes the edge region and dicing region of the wafer bond pair to be debonded; the raw materials of the bonding material of the wafer bond pair to be debonded include thermally decomposable resin and photosensitive resin.
[0044] This invention uses infrared laser scanning on the non-chip areas of wafer bonding pairs to be debonded, without direct contact with the wafer. Instead, the laser is selectively absorbed by the thermally decomposable resin and photosensitive resin in the bonding material, inducing the resin (especially the thermally decomposable resin) to thermally decompose and vaporize, generating small molecule gases (such as methane, ethane, siloxane gases, etc.). These gases expand outwards from the vaporization point, not only breaking the vacuum at the edge of the wafer bonding pair but also separating the bonding interface in the dicing area. This separation effect allows for one-step wafer debonding under low tension, eliminating the need for additional mechanical debonding operations. The process has good repeatability, stable debonding effect, no mechanical contact, no chip surface damage, low stress, and high throughput, making it more suitable for the mass production needs of panelized ultra-thin wafers. It solves the limitation of traditional processes being difficult to adapt to high-temperature wafer processes and broadens the application scenarios.
[0045] The debonding method provided by the present invention solves the following problems: (1) It solves the problem that traditional blade insertion process is prone to damaging wafers and generating debris, thus improving product yield; it uses infrared laser (especially mid-infrared laser MIR laser) to scan the edge area of wafer bonding pairs in non-chip areas in a non-contact manner. After the laser penetrates the wafer, it is only selectively absorbed by the temporary silicone bonding material and does not directly contact the wafer, thus avoiding scratches and chipping damage to the wafer edge caused by rigid blades; at the same time, scanning along the dicing path can greatly reduce the interface adhesion force through laser-induced gas expansion, thus achieving interface separation; especially for ultra-thin device wafers, non-contact vacuum breaking and gas-assisted separation control greatly reduce the risk of wafer breakage. (2) It solves the problems of cumbersome operation and low separation efficiency of traditional processes, and lowers the operation threshold. The laser scanning operation of the present invention can be precisely controlled by the equipment, without the need for operators to manually adjust the insertion depth and angle, making the operation simple. The laser scanning parameters can be flexibly adjusted, which can quickly meet the needs of different gas expansion distances. The vacuum breaking time of a single ring sweep of a 12-inch wafer bonding pair does not exceed 20 seconds. The laser scanning of the wafer dicing channel adopts an automatic mode and precise alignment logic. The entire debonding process takes significantly less time than the traditional process, and the skill requirements of the operators are greatly reduced, which is convenient for large-scale production applications. (3) It solves the problem of excessive debonding pull and high damage risk of wafer bonding pairs after high temperature treatment, and broadens the process adaptability range. For wafer bonding pairs treated at 300℃, the adhesion of the temporary bonding material will be slightly enhanced. This invention can effectively reduce the interface adhesion by using laser edge scanning and dicing scan. Compared with the traditional blade insertion method, this method greatly reduces the damage risk of ultra-thin device wafers. At the same time, MIR laser full-area scanning can achieve debris-free and precise debonding of the bonding interface of wafer bonding pairs, making this method adaptable to wafer bonding pairs after high temperature treatment. It solves the limitation of traditional processes that are difficult to adapt to high temperature process wafers and broadens the application scenarios of this method. (4) The overall process has the advantages of high safety and strong stability. Compared with the traditional blade insertion vacuum breaking process, the laser edge scanning and dicing scan method of this invention has no collision and friction of rigid parts, making the operation safer and effectively avoiding the risk of operators being scratched by blades. At the same time, the laser parameters can be precisely controlled, the process repeatability is good, and the debonding effect is stable.
[0046] In this invention, if the entire wafer is scanned during laser scanning instead of targeted scanning of non-chip areas, continuous infrared irradiation will cause sustained heat buildup in the chip area, increasing the risk of photothermal damage to the ultrathin silicon device layer. Large-area scanning is time-consuming and has low throughput, and high-energy infrared radiation can easily damage the device passivation layer, making it only suitable for thick wafers and low-precision scenarios. On the other hand, if only the edge areas of the wafer bonding pairs in non-chip areas are scanned during laser scanning, only the edge adhesion is weakened, and the interface vacuum seal is not broken. Subsequent mechanical separation still requires high pulling force, and ultrathin wafers are prone to cracking due to tensile stress. Moreover, the process compatibility is insufficient. Edge lasers only decompose the surface adhesive, and there is no gas expansion through the adhesive layer. The bonding strength at the center of the wafer is still relatively high, and localized die adhesion and residual adhesive are prone to occur during separation, requiring additional wet cleaning, increasing the process steps and the risk of contamination. At the same time, the solution is only compatible with standard wafers of fixed size and cannot be compatible with multi-die panel irregularly shaped wafers, resulting in poor process compatibility.
[0047] In some embodiments, the expansion width of the gas expansion from the vaporization location to the expansion edge of the gas expansion is 5mm to 20mm, for example, 5mm, 6mm, 7mm, 8mm, 9mm, 10mm, 11mm, 12mm, 13mm, 14mm, 15mm, 16mm, 17mm, 18mm, 19mm or 20mm.
[0048] The gas expansion width range of 5mm to 20mm provided by this invention can not only break the vacuum at the edge, but also increase the expansion range to adapt to bonding interfaces with different bonding strengths, thereby facilitating the subsequent debonding of the wafer with minimal pulling force.
[0049] In some implementations, the gas extends between adjacent cutting channel regions to the point where the gas is interconnected.
[0050] The debonding method provided by this invention performs laser scanning in the cutting area (i.e., the cutting track) to allow the gas between adjacent cutting track areas to expand to interconnect, thereby ensuring non-destructive debonding of the bonding interface under low stress, especially for the debonding of ultrathin wafers.
[0051] In some embodiments, the pulling force is ≤8N, such as 1N, 2N, 3N, 4N, 5N, 6N, 7N or 8N.
[0052] The debonding method of the present invention can debond the wafer without excessive pulling force after the initial treatment of the bonding interface by laser scanning gas expansion. The pulling force range of ≤8N is less likely to damage the ultrathin wafer, while increasing the pulling force will further increase the risk of wafer damage.
[0053] In some embodiments, during the laser scanning process, the bonding edges of the wafer bonding pairs to be debonded are subjected to auxiliary air blowing and / or the pressure in the laser scanning environment is reduced.
[0054] During the laser scanning process of this invention, auxiliary air blowing treatment is performed on the bonding edges of the wafer bonding pairs to be debonded and / or the pressure in the laser scanning environment is reduced; through the above auxiliary means, the diffusion and discharge of gas can be promoted, and the gas expansion direction can be appropriately controlled to better achieve stress decomposition at the bonding interface.
[0055] As an example, a protective gas, such as nitrogen and / or an inert gas including argon or helium, may be blown in as an auxiliary gas.
[0056] As an example, the environmental pressure can be slightly reduced, for example, by placing the laser scanning process in a low-pressure chamber, where the low pressure includes 5 kPa to 10 kPa below the ambient atmospheric pressure, such as 5 kPa, 6 kPa, 7 kPa, 8 kPa, 9 kPa, or 10 kPa.
[0057] In some embodiments, the mass ratio of the thermally decomposable resin to the photosensitive resin is (1~3):(3~1), for example, 1:3, 1:2, 1:1, 2:3, 2:2, 2:1, 3:2 or 3:1, etc.
[0058] The present invention adjusts the mass ratio of thermally decomposable resin and photosensitive resin in the bonding material to (1~3):(3~1), which is more conducive to generating a large amount of gas during subsequent infrared laser scanning, increasing the width of gas expansion, and thus enhancing the debonding effect.
[0059] In some embodiments, the pyrolytic resin includes any one or a combination of at least two of silicone resin, polyimide resin, polycarbonate resin, or polymethyl methacrylate.
[0060] In the selection of thermally decomposable resins in this invention, in addition to silicone resins which can selectively absorb laser energy with the assistance of photosensitive resins and undergo thermal decomposition to produce small molecule gases after absorbing laser energy, the other thermally decomposable resins that meet the following conditions also meet the requirements: a) stable at the required process temperature; b) strong absorption of MIR lasers; c) thermal decomposition to produce a large amount of gas; d) no harmful solid residues are produced.
[0061] In some embodiments, the raw materials for the bonding material also include diluents and antioxidants.
[0062] It is understood that, apart from thermally decomposable resin and photosensitive resin, the bonding materials selected in this invention are all conventional technical choices, which do not affect the realization of the technical concept of this invention.
[0063] As an example, the silicone resin includes polymethylsiloxane.
[0064] As an example, the photosensitive resin includes phenoxy resin.
[0065] As an example, the diluent includes xylene, and the added mass of the diluent is 15% to 25% of the total mass of the thermally decomposable resin and the photosensitive resin, such as 15%, 18%, 20%, 23%, or 25%.
[0066] As an example, the antioxidant includes 2,6-di-tert-butyl-p-cresol, and the added antioxidant is 0.1% to 1% of the mass of the thermally decomposable resin, such as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, or 1%.
[0067] In some embodiments, the wavelength of the laser used for infrared laser scanning is 0.2μm to 11μm, such as 0.2μm, 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm, 9.5μm, 10μm, 10.5μm, or 11μm.
[0068] This invention uses a mid-infrared laser band (MIR laser) during infrared laser scanning, which can avoid damage to the chip, and at the same time, it can pass through the wafer better and be absorbed by the bonding material and then vaporized without damaging the wafer.
[0069] More specifically, the wavelength of the laser used in the infrared laser scanning of this invention can be further limited according to different types of carrier wafers.
[0070] When the carrier wafer is a glass wafer, the wavelength of the laser used for infrared laser scanning is 0.2μm~8μm. If the wavelength is too high, it will be difficult for the laser to penetrate the wafer and irradiate the bonding material.
[0071] When the carrier wafer is a silicon wafer, the wavelength of the laser used for infrared laser scanning is 1.3μm~11μm. If the wavelength is too short, the laser will have difficulty penetrating the wafer.
[0072] In some embodiments, the power of the infrared laser scanning is 20W to 2000W, such as 20W, 50W, 100W, 200W, 300W, 400W, 500W, 600W, 700W, 800W, 900W, 1000W, 1100W, 1200W, 1300W, 1400W, 1500W, 1600W, 1700W, 1800W, 1900W, or 2000W.
[0073] In some embodiments, the scanning speed of the infrared laser scan is 20 mm / s to 20000 mm / s, such as 20 mm / s, 50 mm / s, 100 mm / s, 500 mm / s, 1000 mm / s, 1500 mm / s, 2000 mm / s, 3000 mm / s, 4000 mm / s, 5000 mm / s, 6000 mm / s, 7000 mm / s, 8000 mm / s, 9000 mm / s, 10000 mm / s, 11000 mm / s, 12000 mm / s, 13000 mm / s, 14000 mm / s, 15000 mm / s, 16000 mm / s, 17000 mm / s, 18000 mm / s, 19000 mm / s, or 20000 mm / s.
[0074] In some embodiments, the number of infrared laser scans is 1 to 100, such as 1, 3, 5, 8, 10, 20, 30, 40, 50, 60, 70, 80, 90 or 100 times.
[0075] In the infrared laser scanning process, the parameters of this invention can be precisely controlled. Based on the target gas expansion width range, the corresponding parameters of the infrared laser scanning can be adaptively selected and adjusted.
[0076] In some embodiments, the wafer bond pairs to be debonded include wafer bond pairs of device wafers and carrier wafers.
[0077] In some embodiments, the width of the edge region of the wafer bonding pair to be debonded is 2mm to 5mm, such as 2mm, 3mm, 4mm or 5mm.
[0078] In some embodiments, the bonding strength of the wafer bond pairs to be debonded is 0.2MPa to 1MPa, for example, 0.2MPa, 0.3MPa, 0.4MPa, 0.5MPa, 0.6MPa, 0.7MPa, 0.8MPa, 0.9MPa or 1MPa.
[0079] In some embodiments, the device wafer includes an ultrathin wafer.
[0080] The thickness of the ultrathin wafer is ≤50μm, such as 10μm, 20μm, 30μm, 40μm or 50μm.
[0081] In some embodiments, the laser scanning scans non-chip regions of the carrier wafer.
[0082] It should also be noted that the present invention does not impose specific limitations on the bonding and post-processing methods of the wafer bond pairs to be debonded. Without departing from the overall technical concept of the present invention, any conventional bonding and post-processing methods of wafer bond pairs are applicable to the present invention, that is, as long as the wafer bond pairs to be debonded are obtained.
[0083] As an example, the present invention provides a method for obtaining wafer bond pairs to be debonded, comprising:
[0084] Provide the target amount of temporary bonding material;
[0085] The carrier wafer and the device wafer are bonded using a temporary bonding material, and after curing, the bonding of the wafer bonding pairs is completed.
[0086] The device wafer is thinned to obtain wafer bonding pairs after thinning; optionally, it can be further subjected to high-temperature processing to obtain wafer bonding pairs to be debonded.
[0087] The numerical range described in this invention includes not only the point values listed above, but also any point values within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values included in the range.
[0088] In one specific embodiment, the present invention provides a method for obtaining wafer bond pairs to be debonded, comprising:
[0089] S1. Provide temporary bonding materials: silicone resin (polymethylsiloxane, CAS No.: 9006-08-2, degree of polymerization 1000~1200), photosensitive resin (phenoxy resin, CAS No.: 26402-79-9, purity 99%), diluent (xylene, CAS No.: 1330-20-7, purity 99.8%, the amount of diluent added is 20% of the total mass of silicone resin and photosensitive resin), antioxidant (2,6-di-tert-butyl-p-cresol, CAS No.: 128-37-0, the amount added is 0.5% of the mass of silicone resin); the mass ratio of silicone resin to photosensitive resin is (1~3):(3~1);
[0090] The mixture of the above formula was placed in a high-speed stirrer and stirred for 30 minutes at 25°C and 800 r / min. After mixing evenly, the mixture was degassed for 15 minutes (vacuum degree -0.095 MPa) to remove air bubbles from the mixture and obtain a temporary bonded material.
[0091] S2. Preparation of wafer bonding pairs: A 12-inch device wafer (300 μm thick, 3 mm wide non-die area at the edge) and a 12-inch carrier wafer (glass wafer or silicon carrier wafer, 500 μm thick) were selected. The prepared temporary bonding material was uniformly coated on the surface of the carrier wafer with a coating thickness of 50 μm. Then, the device wafer and the silicon carrier were bonded together using a bonding device and cured at 150 °C and 0.3 MPa for 20 min to obtain wafer bonding pairs.
[0092] S3. Backside process: The device wafer is thinned using a grinding machine to reduce its thickness to 50μm. After thinning, the grinding debris on the wafer surface is removed using a conventional cleaning process and then dried for later use. Optionally, the thinned wafer bonding pairs are subjected to an additional 300℃ high-temperature treatment for 30 minutes to simulate the working conditions after a high-temperature process. Finally, the wafer bonding pairs to be debonded are obtained.
[0093] The following examples and comparative examples all involve debonding the wafer bonding pairs to be debonded provided in the above specific embodiments.
[0094] Example 1
[0095] This embodiment provides a wafer debonding method, such as... Figure 1 As shown, the debonding method includes:
[0096] Provide wafer bonding pairs to be debonded: the mass ratio of organosilicon resin to photosensitive resin is 1:3, silicon carrier wafers, which are directly debonded after thinning;
[0097] The carrier wafer of the wafer bonding pair to be debonded is subjected to MIR laser scanning in the non-chip region, which includes the edge region and the dicing region. The specific parameters are: MIR laser wavelength 10.6μm, power 100W, scanning speed 1000mm / s, initial ring scan distance 2mm, and 3 scans.
[0098] The bonding material in the wafer bonding pair is vaporized and the gas expands outward from the vaporization point. The expansion width of the gas expansion is 12 mm from the vaporization point to the edge of the gas expansion. The gas expands to the point where the gas between adjacent dicing areas is interconnected, resulting in a wafer bonding pair after preliminary treatment of the bonding surface.
[0099] The laser-treated wafer bonding pairs are transferred to the separation station, and the carrier is gradually lifted by a vacuum nozzle with a lifting force of 3N to complete the debonding of the wafers.
[0100] Example 2
[0101] This embodiment provides a method for debonding wafers, the method comprising:
[0102] Provide wafer bonding pairs to be debonded: the mass ratio of organosilicon resin to photosensitive resin is 1:1, silicon carrier wafers, which are directly debonded after thinning;
[0103] The carrier wafer of the wafer bonding pair to be debonded is subjected to MIR laser scanning in the non-chip region, which includes the edge region and the dicing region. The specific parameters are: MIR laser wavelength 10.6μm, power 100W, scanning speed 1000mm / s, initial ring scan distance 2mm, and 3 scans.
[0104] The bonding material in the wafer bonding pair is vaporized and the gas expands outward from the vaporization point. The expansion width of the gas expansion is 9 mm from the vaporization point to the edge of the gas expansion. The gas expands to the point where the gas between adjacent dicing areas is interconnected, resulting in a wafer bonding pair after preliminary treatment of the bonding surface.
[0105] The laser-treated wafer bonding pairs are transferred to the separation station, and the carrier is gradually lifted by a vacuum nozzle with a lifting force of 6N to complete the debonding of the wafers.
[0106] Example 3
[0107] This embodiment provides a method for debonding wafers, the method comprising:
[0108] Provide wafer bonding pairs to be debonded: the mass ratio of organosilicon resin to photosensitive resin is 3:1, silicon carrier wafers, which are directly debonded after thinning;
[0109] The carrier wafer of the wafer bonding pair to be debonded is subjected to MIR laser scanning in the non-chip region, which includes the edge region and the dicing region. The specific parameters are: MIR laser wavelength 10.6μm, power 100W, scanning speed 1000mm / s, initial ring scan distance 2mm, and 3 scans.
[0110] The bonding material in the wafer bonding pair is vaporized and the gas expands outward from the vaporization point. The expansion width of the gas expansion is 7 mm from the vaporization point to the edge of the gas expansion. The gas expands to the point where the adjacent dicing areas are interconnected, resulting in a wafer bonding pair after preliminary treatment of the bonding surface.
[0111] The laser-treated wafer bonding pairs are transferred to the separation station, and the carrier is gradually lifted by a vacuum nozzle with a lifting force of 8N to complete the debonding of the wafers.
[0112] Example 4
[0113] The difference between this embodiment and Embodiment 1 is that, in addition to the thinning process, the wafer bonding pairs to be debonded in this embodiment are further subjected to a high-temperature treatment of 300°C for 30 minutes to obtain wafer bonding pairs to be debonded under simulated high-temperature process conditions.
[0114] All other conditions remain the same as in Example 1.
[0115] Example 5
[0116] The difference between this embodiment and Embodiment 1 is that the carrier wafer in the wafer bonding pair to be debonded in this embodiment is a glass wafer, and the MIR laser wavelength is adjusted to 5μm.
[0117] All other conditions remain the same as in Example 1.
[0118] Example 6
[0119] The difference between this embodiment and Embodiment 1 is that the gas expansion width in this embodiment is 5mm and the adjustment power is 50W.
[0120] All other conditions remain the same as in Example 1.
[0121] Example 7
[0122] The difference between this embodiment and Embodiment 1 is that the gas expansion width in this embodiment is 20mm and the adjustment power is 200W.
[0123] All other conditions remain the same as in Example 1.
[0124] Example 8
[0125] The difference between this embodiment and Embodiment 1 is that the gas expansion width in this embodiment is 3mm and the adjustment power is 30W.
[0126] All other conditions remain the same as in Example 1.
[0127] Example 9
[0128] The difference between this embodiment and Embodiment 1 is that in the wafer bonding pairs of this embodiment, the mass ratio of silicone resin to photosensitive resin is 1:4.
[0129] All other conditions remain the same as in Example 1.
[0130] Example 10
[0131] The difference between this embodiment and Embodiment 1 is that in the wafer bonding pairs of this embodiment, the mass ratio of silicone resin to photosensitive resin is 4:1.
[0132] All other conditions remain the same as in Example 1.
[0133] Comparative Example 1
[0134] The difference between this comparative example and Example 1 is that in the MIR laser scanning of this comparative example, laser scanning processing of the cutting area is not performed, but only the edge area is laser scanned.
[0135] All other conditions remain the same as in Example 1.
[0136] Comparative Example 2
[0137] The difference between this comparative example and Example 1 is that in the MIR laser scanning of this comparative example, laser scanning processing of the edge area is not performed, but only laser scanning processing of the cutting track area is performed.
[0138] All other conditions remain the same as in Example 1.
[0139] Comparative Example 3
[0140] The difference between this comparative example and Example 4 is that in the MIR laser scanning of this comparative example, laser scanning processing of the cutting area is not performed, but only the edge area is laser scanned.
[0141] All other conditions remain the same as in Example 4.
[0142] Comparative Example 4
[0143] The difference between this comparative example and Example 4 is that in the MIR laser scanning of this comparative example, laser scanning processing of the edge area is not performed, but only laser scanning processing of the cutting track area is performed.
[0144] All other conditions remain the same as in Example 1.
[0145] The bonding strength of the wafer bond pairs to be debonded provided in the examples and comparative examples was tested using a universal tensile testing machine, according to the tensile strength test method in GB / T 14074-2008 "Test Methods for Adhesives and Resins for Wood Industry". The A / D interface bond strength of the wafer bond pairs was tested, with 3 samples tested in each group and the average value was taken.
[0146] The expansion width of gas expansion by laser scanning in the examples and comparative examples was tested. The test conditions were: the edge separation area was observed with an optical microscope, and the obvious gap distance extending inward from the wafer edge was measured.
[0147] The tensile force in the examples and comparative examples was tested. The test conditions were as follows: a tensile sensor was used to monitor the maximum tensile force of a single nozzle in real time during the mechanical debonding process. Three samples were tested in each group, and the average value was taken.
[0148] The debonding effect of the device wafers after debonding in the examples and comparative examples was observed: the observation results included no wafer damage and no detachment, slight wafer detachment, slight wafer damage, severe wafer detachment, and severe wafer damage.
[0149] The results are shown in Table 1.
[0150] Table 1
[0151]
[0152]
[0153] From Table 1, we can obtain:
[0154] The debonding method provided by this invention utilizes infrared laser to perform laser scanning on the non-chip areas of the wafer bonding pairs. After laser scanning, no mechanical debonding is required. Wafer debonding can be achieved by simple lifting with a small pulling force. The process has good repeatability, stable debonding effect, no mechanical contact, no chip surface damage, low stress and high throughput. It is more suitable for the mass production needs of panelized ultra-thin wafers, solves the limitation of traditional processes that are difficult to adapt to high-temperature wafers, and broadens the application scenarios.
[0155] Data analysis of Examples 1, 4, and 5 shows that the debonding method provided by the present invention is applicable to wafer bonding pairs in different processes.
[0156] Data analysis of Examples 1 and 6-8 shows that the debonding method provided by the present invention, with a gas expansion width range of 5mm to 20mm, can both break the vacuum at the edge and increase the expansion range, adapting to bonding interfaces with different bonding strengths. This facilitates the subsequent debonding of the wafer with minimal pulling force.
[0157] Data analysis of Examples 1 and 9-10 shows that the present invention controls the mass ratio of thermally decomposable resin and photosensitive resin in the bonding material to (1~3):(3~1), resulting in excellent bonding effect without causing wafer thinning and is more conducive to generating a large amount of gas during subsequent infrared laser scanning, increasing the width of gas expansion, thereby enhancing the debonding effect.
[0158] Data analysis of Example 1 and Comparative Examples 1-2, Example 4 and Comparative Examples 3-4 shows that the debonding method provided by the present invention must simultaneously perform laser scanning on the edge and dicing areas in the non-chip region in order to achieve wafer debonding with no mechanical contact, no chip surface damage, low stress and high throughput.
[0159] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A method of debonding a wafer, the method comprising: The debonding method includes the following steps: Provide wafer bonding pairs to be debonded, perform infrared laser scanning on the non-chip areas of the wafer bonding pairs to be debonded, causing the bonding material in the wafer bonding pairs to vaporize and expand the gas outward from the vaporization location as the center, to obtain wafer bonding pairs after preliminary treatment of the bonding surface; After the bonding surface has been pre-processed, the carrier wafer of the wafer bonding pair is pulled up to complete the debonding of the wafer. The non-chip region includes the edge region and dicing region of the wafer bond pair to be debonded; the raw materials of the bonding material of the wafer bond pair to be debonded include thermally decomposable resin and photosensitive resin.
2. The debonding method of claim 1, wherein, From the vaporization location to the edge of the gas expansion, the expansion width of the gas expansion is 5mm to 20mm; And / or, gas expansion between adjacent cut channel regions to gas interconnection.
3. The debonding method according to claim 1 or 2, characterized in that, The pulling force is ≤8N.
4. The debonding method of claim 1, wherein, During the laser scanning process, the bonding edges of the wafer bonding pairs to be debonded are subjected to auxiliary air blowing treatment and / or the pressure in the laser scanning environment is reduced.
5. The debonding method of claim 1, wherein, The mass ratio of the thermally decomposable resin to the photosensitive resin is (1~3):(3~1). And / or, the thermally decomposable resin includes any one or a combination of at least two of silicone resin, polyimide resin, polycarbonate resin or polymethyl methacrylate.
6. The debonding method of claim 1, wherein, The raw materials for the bonding material also include diluents and antioxidants.
7. The debonding method of claim 1, wherein, The wavelength of the laser used in the infrared laser scanning is 0.2μm~11μm.
8. The debonding method according to claim 1, characterized in that, The power of the infrared laser scanning is 20W~2000W; And / or, the scanning speed of the infrared laser scan is 20 mm / s to 20000 mm / s; And / or, the number of scans of the infrared laser scan is 1 to 100.
9. The debonding method according to claim 1, characterized in that, The wafer bonding pairs to be debonded include wafer bonding pairs of device wafers and carrier wafers; And / or, the width of the edge region of the wafer bond pair to be debonded is 2mm~5mm; And / or, the bonding strength of the wafer bond pairs to be debonded is 0.2 MPa to 1 MPa.
10. The debonding method according to claim 9, characterized in that, The device wafer includes an ultrathin wafer; And / or, the laser scanning scans the non-chip regions of the carrier wafer.