A thermally conductive composite substrate and its preparation method

By designing a thermally conductive composite substrate, and utilizing a combination of a base layer, a barrier layer, and a thermal interface plastic layer, the problems of high interfacial thermal resistance and easy drying of thermal interface materials in existing technologies are solved, achieving efficient and reliable heat dissipation, and making it suitable for long-term use with high heat flux density.

CN123124801APending Publication Date: 2026-11-17ZHEJIANG ZHENGHANYUAN SEMICONDUCTOR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611304399.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing thermally conductive substrates and thermal interface materials suffer from problems such as high interfacial thermal resistance, easy drying of thermal interface materials, low thermal conductivity, and high cost, which limit heat dissipation efficiency.

Method used

The material employs a thermally conductive composite substrate, comprising a base layer, a barrier layer, and a thermal interface plastic layer. The base layer is made of a highly thermally conductive material, the barrier layer is made of metal or a metal alloy, and the thermal interface plastic layer contains indium. A metal bonding interface is formed through electroplating or physical vapor deposition processes to eliminate nanoscale voids at the interface and enhance adhesion strength.

Benefits of technology

It effectively reduces interface thermal resistance, improves heat dissipation stability and reliability, meets the long-term heat dissipation requirements of high heat flux density, eliminates the need for separate thermal interface materials, and reduces installation difficulty and failure probability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124801A_ABST
    Figure CN123124801A_ABST
Patent Text Reader

Abstract

This invention discloses a thermally conductive composite substrate and its preparation method, comprising a base layer, a barrier layer, and a thermal interface plastic layer. The base layer is a thermally conductive material, and the barrier layer is located between the base layer and the thermal interface plastic layer. The barrier layer is one or more of a metal, a metal alloy, or a metal compound, and the thermal interface plastic layer contains indium. The surface of the base layer facing the thermal interface plastic layer is the first surface of the base layer, and the heating element is in contact with the thermal interface plastic layer. The barrier layer includes a target area and a non-target area, and the target area is in contact with the thermal interface plastic layer. The thermally conductive composite substrate can fully conform to the microscopic uneven heat dissipation interface of the heating element, effectively eliminating interfacial contact thermal resistance, exhibiting excellent thermal conductivity, excellent heat dissipation stability, and long-term service reliability. It can meet the long-term heat dissipation requirements of high heat flux density heating elements and improves subsequent installation efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of thermally conductive composite substrate technology, and specifically to a thermally conductive composite substrate technology and preparation method. Background Technology

[0002] To effectively dissipate heat from power devices and other heat sources and reduce their temperature, existing power devices are generally mounted on thermally conductive bases, i.e., thermally conductive substrates. Some thermally conductive bases are also integrated into active or passive cooling devices such as air cooling, water cooling, and phase change cooling. Existing thermally conductive substrates are generally made of pure metal or adhesive composite materials, which have the following drawbacks: 1. High interfacial thermal resistance due to hard contact: The substrate and the heat source are in hard contact. Due to the influence of machining flatness and device packaging tolerance, there will inevitably be micron-level gaps at the bonding interface, which greatly increases the interfacial thermal resistance.

[0003] 2. Additional thermal resistance introduced by independent thermal interface materials: To reduce the gap, an independent thermal interface material needs to be filled between the heat source and the thermally conductive substrate. Mechanical contact is formed between the thermal interface material and the substrate, but nanoscale voids still exist at the interface. In this case, the total thermal resistance of the thermal interface material consists of three parts: the interfacial thermal resistance between the heat source and the thermal interface material, the bulk thermal resistance of the thermal interface material, and the interfacial thermal resistance between the thermal interface material and the thermally conductive substrate.

[0004] 3. Inherent defects of existing thermal interface materials: Existing thermal interface materials generally use thermally conductive silicon, silicone, liquid metal, etc. Thermally conductive silicone grease is prone to drying, oiling, and migration, and is not suitable for high heat flux density and long life requirements; silicone pads are thick, have low thermal conductivity, and fast compression rebound decay, resulting in a continuous increase in thermal resistance over long-term operation; liquid metal is expensive and prone to short circuits.

[0005] 4. Thermal resistance bottleneck restricts heat dissipation efficiency: After the independent thermal interface material is filled, the interface thermal resistance between the heat source and the thermal interface material, as well as between the thermal interface material and the substrate, is too high due to insufficient contact. This becomes a key factor restricting the efficient heat dissipation of various heat sources.

[0006] Therefore, how to efficiently dissipate heat from heating components is an urgent problem to be solved. Summary of the Invention

[0007] To address the above problems, the main objective of this invention is to provide a thermally conductive composite substrate and its preparation method, which has good thermal conductivity and high reliability, and is beneficial for mass production and subsequent packaging.

[0008] One aspect of the present invention provides a thermally conductive composite substrate, comprising a base layer, a barrier layer, and a thermal interface plastic layer. The base layer is a thermally conductive material, and the barrier layer is located between the base layer and the thermal interface plastic layer. The barrier layer is one or more of a metal, a metal alloy, or a metal compound, and the thermal interface plastic layer contains indium. The surface of the base layer facing the thermal interface plastic layer is a first surface of the base layer, a heating element is in contact with the thermal interface plastic layer, and the barrier layer includes a target area and a non-target area, the target area being in contact with the thermal interface plastic layer.

[0009] In one embodiment, the projection of the thermal interface plastic layer onto the first surface of the base layer along a direction perpendicular to the thickness of the base layer is a designated area of ​​the base layer, and other areas of the first surface of the base layer are non-designated areas of the base layer. The designated area of ​​the base layer is in contact with the barrier layer.

[0010] In one embodiment, the non-designated area of ​​the base layer may or may not be in contact with the barrier layer.

[0011] In one embodiment, the base layer is one or more of metal, ceramic, carbon-based composite material, and metal-based composite material.

[0012] In one embodiment, the substrate is one or more of copper, aluminum, molybdenum, tungsten, and aluminum silicon carbide.

[0013] In one embodiment, the thermal conductivity of the base layer is greater than 100 W / (m·K), and preferably, the thermal conductivity of the base layer is greater than 150 W / (m·K).

[0014] In one embodiment, the roughness of the first surface of the base layer is less than 5 micrometers, preferably, the roughness of the first surface of the base layer is less than or equal to 4 micrometers.

[0015] In one embodiment, the barrier layer is one or more of nickel, titanium, platinum, chromium, tungsten, tantalum, molybdenum, and zirconium.

[0016] In one embodiment, the thickness of the barrier layer is 0.2 μm to 5 μm, preferably 2 μm to 3 μm.

[0017] In one embodiment, the barrier layer is used to isolate the thermal interface plastic layer from the base layer and to enhance the adhesion strength between the thermal interface plastic layer and the base layer.

[0018] In one embodiment, the thermal conductivity of the barrier layer is greater than 50 W / (m·K).

[0019] In one embodiment, the barrier layer further includes an adhesive layer located near the substrate. The adhesive layer is any one of titanium, zirconium, tungsten, and tantalum, and is used to enhance the surface adhesion between the barrier layer and the substrate.

[0020] In one embodiment, the thickness of the thermal interface plastic layer is 2μm to 50μm, preferably, the thickness of the thermal interface plastic layer is 2μm to 30μm.

[0021] In one embodiment, the thermal conductivity of the thermal interface plastic layer is greater than 70 W / (m·K).

[0022] In one embodiment, the Mohs hardness of the thermal interface plastic layer is less than 2.

[0023] In one embodiment, the thermal interface plastic layer is an indium-silver alloy, wherein the indium content is greater than 90% by mass, preferably greater than or equal to 95% by mass.

[0024] In one embodiment, a metal-bonded metallurgical interface is formed between the base layer and the barrier layer, and between the barrier layer and the thermal interface plastic layer.

[0025] Another aspect of the present invention provides a method for preparing a thermally conductive composite substrate, comprising the following steps: S1: Pre-treat the substrate, the pre-treatment including ultrasonic degreasing and plasma activation treatment of the substrate surface to obtain the pre-treated substrate; S2: A barrier layer is deposited on the surface of the pretreated substrate using electroplating or physical vapor deposition. S3: Apply a thermal interface plastic layer to the target area of ​​the barrier layer using electroplating or physical vapor deposition.

[0026] In one embodiment, the physical vapor deposition method in step S2 employs PVD magnetron sputtering to deposit a barrier layer of metal stack structure on the first surface of the pretreated substrate.

[0027] In one embodiment, step S3 employs a vacuum evaporation process to deposit a thermal interface plastic layer in the target area of ​​the barrier layer.

[0028] In one embodiment, step S3 employs a dual-source vacuum evaporation process to deposit an indium-silver alloy in the target region of the barrier layer.

[0029] The beneficial effects of this invention are as follows: 1. The present invention utilizes the high thermal conductivity, high plasticity, and excellent plastic deformation capability of the thermal interface plastic layer to fully conform to the microscopic concave and convex heat dissipation interface of the heating element, effectively eliminating the interface contact thermal resistance.

[0030] 2. The base layer has excellent thermal conductivity. Combined with the anti-oxidation and anti-diffusion function of the barrier layer, the composite substrate has excellent heat dissipation stability and long-term service reliability, which can meet the long-term heat dissipation requirements of high heat flux density heating elements.

[0031] 3. In later processing and use, there is no need to install thermal interface material separately, which reduces the difficulty of installation and the probability of failure, and improves installation efficiency. Attached Figure Description

[0032] Figure 1 This is a schematic diagram of the structure of Example 1; Figure 2 This is a schematic diagram of the structure of Example 2.

[0033] Figure label: 1. Base layer; 11. Designated area of ​​base layer; 12. Undesignated area of ​​base layer; 2. Barrier layer; 21. Target area; 22. Non-target area; 3. Thermal interface plastic layer. Detailed Implementation

[0034] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions in the embodiments will be clearly and completely described below with reference to the accompanying drawings. However, the specific implementation methods and embodiments described below are for illustrative purposes only and are not intended to limit the scope of protection of this invention.

[0035] Example 1 like Figure 1 As shown, this embodiment provides a thermally conductive composite substrate with a thickness of 50 μm. A 6101 aluminum alloy plate is used as the base layer 1, with a flatness of less than or equal to 3 μm. The thermal interface plastic layer 3 is an indium-silver alloy, where the mass ratio of indium to silver is 98:2. The indium-silver alloy has a thickness of 5 μm and a Mohs hardness of less than 2. A barrier layer 2 is formed between the 6101 aluminum alloy plate (base layer 1) and the indium-silver alloy (thermal interface plastic layer 3). The barrier layer 2 is made of nickel and has a thickness of 2 μm. The heating element is disposed on the surface of the thermal interface plastic layer away from the barrier layer. The surface of the base layer 1 facing the thermal interface plastic layer 3 and the barrier layer 2 is the first surface of the base layer. The first surface of the base layer includes a designated area 11 and a non-designated area 12. The projection of the contact surface between the heating element and the thermal interface plastic layer 3 along a direction perpendicular to the thickness of the base layer onto the first surface of the base layer is the designated area 11. The other areas of the first surface of the base layer are the non-designated areas 12. In this embodiment, no barrier layer is coated on the unspecified area 12 of the substrate, meaning that the unspecified area 12 of the substrate is not in contact with the barrier layer 2. The roughness of the specified area 11 of the substrate is less than or equal to 1 μm, and the roughness of the unspecified area 12 of the substrate is less than 3 μm.

[0036] Metallic bonds are formed between the nickel layer and the aluminum alloy plate, and between the nickel layer and the indium alloy layer. These strong bonds eliminate nanoscale voids in mechanical contact, significantly reducing interfacial thermal resistance. Simultaneously, an indium-silver alloy is used as the thermal interface plastic layer. Its soft texture and tendency to deform under pressure allow it to fill microscopic irregularities at the interface, further reducing the interfacial thermal resistance between the thermal interface plastic layer and the heating element. The total thermal resistance of the thermally conductive composite substrate provided in this embodiment is 0.032℃. cm 2 / W, at a chip heat flux density of 100W / cm² 2 Under these conditions, the temperature rise is approximately 3.2 degrees Celsius, and there is no degradation even after long-term use.

[0037] Under the same conditions, the substrate solution using thermal grease on a 6101 aluminum alloy plate has a total thermal resistance of 0.08 cm. 2 / W, at a chip heat flux density of 100W / cm² 2 Under certain conditions, the thermal grease will experience a temperature rise of approximately 8 degrees Celsius. It will degrade due to drying out over long-term use. Using a 6101 aluminum alloy plate directly as the heat dissipation substrate results in a total thermal resistance of 0.05℃. cm 2 / W, at a chip heat flux density of 100W / cm² 2 Under these conditions, the temperature rise is approximately 5 degrees Celsius.

[0038] Example 2 like Figure 2 As shown, this embodiment provides a thermally conductive composite substrate with a thickness of 50 μm. A 6063 aluminum alloy plate is used as the base layer 1, with a flatness of less than or equal to 3 μm. The thermal interface plastic layer 3 is indium, with a thickness of 20 μm and a Mohs hardness of less than 2. The barrier layer 2 between the 6063 aluminum alloy plate (base layer) and the indium (thermal interface plastic layer) is made of nickel, with a thickness of 2 μm. The heating element is disposed on the surface of the thermal interface plastic layer 3 away from the barrier layer 2. The surface of the base layer 1 facing the thermal interface plastic layer 3 and the barrier layer 2 is the first surface of the base layer, with a roughness of less than 1 μm. The first surface of the base layer is coated with the barrier layer 2. The barrier layer 2 is disposed on the entire first surface of the base layer, including a designated area and a non-designated area. A metallographic bonding interface is formed between the base layer 1 and the barrier layer 2, and between the barrier layer 2 and the thermal interface plastic layer 3, resulting in strong bonding and no significant cross-sectional thermal resistance. The surface of the barrier layer 2 includes a target area 21 and a non-target area 22. When no heating element is installed on the substrate, the surface of the target area 21 has a thermal interface plastic layer 3, and the surface of the non-target area 22 does not contact the thermal interface plastic layer 3. When the heating element is installed on the thermal interface plastic layer 3, the thermal interface plastic layer 3 will deform, causing indium to fill the entire non-target area.

[0039] The barrier layer effectively isolates the indium in the thermal interface plastic layer from the aluminum alloy of the substrate, preventing chemical reactions that could lead to performance degradation. It also strengthens the adhesion between the thermal interface plastic layer and the substrate, preventing detachment. After the heating element is mounted onto the substrate, the indium metal in the thermal interface plastic layer fills the gap between the heating element and the barrier layer, further improving thermal conductivity and reducing interfacial thermal resistance.

[0040] The thermally conductive composite substrate provided in this embodiment uses indium as the thermal interface plastic layer. Indium is soft and easily undergoes plastic deformation under pressure, filling the micro-unevenness of the interface. Strong metallic bonds are formed between the nickel layer and the aluminum alloy plate layer, and between the nickel layer and the indium layer, eliminating nanoscale voids in mechanical contact and significantly reducing interfacial thermal resistance. The total thermal resistance of the thermally conductive composite substrate provided in this embodiment is 0.035℃. cm 2 / W, at a chip heat flux density of 100W / cm² 2 Under these conditions, the temperature rise is approximately 3.5 degrees Celsius, and there is no degradation even after long-term use.

[0041] Compared to a substrate solution using 6063 aluminum alloy plate with thermal grease under the same conditions, its total thermal resistance is 0.08 cm⁻¹. 2 / W. At a chip heat flux density of 100W / cm² 2 Under these conditions, the temperature rise is approximately 8 degrees Celsius, and it will degrade due to drying out after long-term use.

[0042] Example 3 This embodiment provides a method for preparing a thermally conductive composite substrate, including the following steps: Step S1: Pre-treatment of the substrate A metal with high thermal conductivity is selected as the base material, such as aluminum, aluminum alloy, or copper; aluminum is used as an example in this embodiment. First, the first surface of the base material is pre-processed to a set roughness; in this embodiment, a roughness of 1 μm is used to ensure the subsequent coating adhesion accuracy. For other surface areas of the base material, i.e., those not in direct contact with the barrier layer and those indirectly separated from the thermal interface plastic layer on the barrier layer surface, a roughness of less than 4 μm is sufficient. Then, the base material undergoes sequential dust removal and impurity removal, ultrasonic degreasing cleaning, rinsing and drying, and vacuum plasma activation treatment to obtain a high-cleanliness, high-surface-activity coating substrate. Specifically, this includes: S11. Surface shaping: The coating working surface of the base layer is precision milled or ground to control the surface roughness to less than 4μm, so as to ensure that the subsequent coating layer has a flat and uniform foundation.

[0043] S12. Ultrasonic Degreasing Treatment: Using a water-based or alcohol-based degreasing agent, ultrasonically clean the surface-shaped substrate for 5-20 minutes at 30kHz-40kHz and 40℃-60℃ to remove oil, dust, particulate impurities, and other contaminants. After cleaning, rinse with deionized water in multiple stages to remove residual cleaning agent, followed by dust-free hot air drying to prevent water stains and residual liquid from contaminating the surface.

[0044] S13. Plasma activation treatment of the first surface of the substrate: Using vacuum plasma cleaning equipment, the first surface of the substrate is activated by plasma bombardment in an inert gas atmosphere. This activates the functional groups on the substrate surface, increases the surface energy of the substrate surface, and effectively enhances the interfacial bonding strength between the subsequent metal barrier layer and the substrate, completing the overall pretreatment process of the substrate. Since aluminum is easily oxidized, zinc immersion replacement treatment can be performed first to eliminate the instantaneous regenerated oxide film on the surface.

[0045] Step S2: Prepare a barrier layer on the first surface of the pretreated substrate. In this embodiment, a 2μm thick nickel layer is deposited on the substrate surface by electroplating as a barrier layer. This can be achieved by electroplating or PVD magnetron sputtering. In this embodiment, an electroplating process is used to deposit a metallic nickel barrier layer on the aluminum plate surface.

[0046] The nickel plating solution used is a conventional Watt-type nickel plating solution, and the plating current density is controlled at 2~3 A / dm³. 2 The electroplating temperature is 50~55℃, and the electroplating time is matched with the coating thickness to obtain a 2μm thick nickel barrier layer. After electroplating, the workpiece is removed, rinsed with deionized water, and dried. This process can block element interdiffusion between the aluminum alloy substrate and the subsequent indium silver alloy film, suppress the formation of brittle intermetallic compounds under high-temperature cycling conditions, and improve the temperature cycling reliability of the multilayer film interface.

[0047] Alternatively, the barrier layer can also be a structure with different metal layers. For example, in another embodiment, a combination of titanium and nickel is used as a barrier layer. Here, an adhesion layer, a titanium layer, is first formed by sputtering, with a thickness controlled in the range of 0.05 μm to 0.1 μm. Then, the sputtering source is changed, and a nickel layer is deposited by magnetron sputtering, with a thickness controlled in the range of 1 μm to 3 μm. This dual-layer structure can improve the bonding strength between the barrier layer and the substrate.

[0048] After sputtering, vacuum furnace cooling is performed to obtain a barrier layer with dense film, strong adhesion, and no obvious pinhole defects, which balances low added thin film thermal resistance and high diffusion barrier capability.

[0049] Step S3: Prepare a thermal interface plastic layer in the target area of ​​the barrier layer. After completing step S2, a thermal interface plastic layer is deposited on the barrier layer using physical vapor deposition (PVD). In this embodiment, an indium silver alloy layer is selected as the thermal interface plastic layer. The indium silver alloy layer is precisely fabricated in the target area of ​​the nickel barrier layer using a combination of photolithography and vacuum evaporation. The specific process is as follows: (1) Mask preparation: A photolithographic mask lift-off process is used to mask the surface of the nickel-plated substrate. Two methods can be used: liquid photoresist spin coating or photosensitive dry film lamination. In this embodiment, liquid photoresist is used, and the photoresist is uniformly spin-coated onto the substrate surface before pre-baking and curing. In another embodiment, a dry film process can be used, where the photosensitive dry film is hot-pressed onto the entire surface of the substrate. Subsequently, a photolithography machine is used for precise exposure and development, retaining the mask layer in the non-coated areas of the substrate while fully exposing the nickel barrier layer surface in the preset coating target area, thus achieving selective masking of the designated area.

[0050] (2) Vacuum evaporation of indium-silver alloy: The substrate that has undergone mask treatment is placed inside the cavity of the vacuum evaporation equipment, and the cavity is evacuated to a vacuum degree of 8×10~2×10 Pa. A dual-source vacuum co-evaporation process is adopted, with high-purity indium ingot and high-purity silver ingot as independent evaporation targets. The evaporation temperature of the indium source and the silver source are adjusted separately, and the proportion of gas phase components is precisely controlled so that indium and silver atoms are synchronously and uniformly precipitated in the gas phase and co-deposited on the surface of the exposed nickel barrier layer target area. The deposition continues until the thickness of the indium-silver alloy layer reaches the preset process requirements.

[0051] (3) Mask stripping and post-processing: After the coating is completed, the substrate is removed and immersed in a special organic solvent at a constant temperature to fully swell and strip the residual photoresist / dry film mask layer in area B. At the same time, the excess indium silver alloy film attached to the mask surface is removed, leaving only the indium silver alloy thermal interface plastic layer on the surface of the nickel barrier layer in area A. Finally, the substrate is cleaned with deionized water and dried at low temperature to thoroughly remove residual solvents and impurities, completing the preparation of the thermally conductive composite substrate.

[0052] The thermally conductive composite substrate prepared in this embodiment allows for the direct mounting of heating elements onto the thermal interface plastic layer. A certain pressure is then applied to fix the heating element in place. Under pressure, the thermal interface plastic layer deforms, filling the gaps between the heating element and the substrate. When the heating element operates, it generates a large amount of heat, which is conducted to the substrate layer through the thermal interface plastic layer, and then dissipated by the substrate. This significantly reduces interfacial thermal resistance, effectively minimizing heat accumulation and lowering the temperature. Furthermore, the elimination of the need for separate thermal interface material reduces installation difficulty and the probability of failure, thus improving installation efficiency.

[0053] The thermally conductive composite substrate prepared in this embodiment uses 6101 aluminum alloy as the base layer, a nickel layer as the barrier layer, and an indium silver alloy layer in the target area as the thermal interface plastic layer, resulting in a stable overall structure. The indium silver alloy layer possesses excellent plastic deformation capability, high thermal conductivity, and oxidation resistance, allowing it to fully conform to the microscopic uneven heat dissipation interface of the chip, effectively eliminating interfacial contact thermal resistance and replacing traditional thermally conductive grease that is prone to drying and degradation. Testing showed that the thermally conductive composite substrate prepared in this embodiment, with a base layer thickness of 50 μm, a barrier layer thickness of 2 μm, and a local thermal interface plastic layer thickness of 15 μm, has a total thermal resistance of 0.035 °C·cm. 2 / W, at a chip heat flux density of 100W / cm² 2 Under operating conditions, the interface temperature rise is only 3.5℃. Compared with the traditional aluminum plate + thermal grease solution, the heat dissipation temperature rise is significantly reduced, and there are no issues with thermal grease drying out or aging and failure. The stability and heat dissipation reliability of long-term high-temperature operation are greatly improved.

[0054] Examples 1 and 2 provide thermally conductive composite substrates suitable for various heat dissipation technologies using independent heat sinks, such as the load-bearing thermally conductive and heat dissipation base structure for medium and high power devices like IGBT modules, MOS power transistors, energy storage PCS, photovoltaic inverters, and vehicle electronic control modules.

[0055] Example 4 This embodiment provides a method for preparing a thermally conductive composite substrate, using a copper plate as the base layer, and depositing a nickel barrier layer on the copper plate through an electroplating process.

[0056] S1. Pre-treatment of the base layer In this embodiment, a pure copper plate is selected as the heat dissipation base for the thermally conductive composite substrate. The copper plate substrate is precisely cut and finely ground to ensure that the overall flatness of the base plate is ≤3μm. The first surface of the substrate is finely polished to ensure that the surface roughness of the first surface of the substrate is ≤1μm. After the substrate is formed, ultrasonic degreasing and cleaning are performed. The copper plate is placed in a neutral degreasing cleaning solution for high-frequency ultrasonic cleaning to thoroughly remove oil, dust, particulate impurities, and processing residues from the substrate surface, avoiding foreign matter from affecting the adhesion of subsequent plating layers and the interfacial thermal conductivity. After ultrasonic cleaning, the copper plate is rinsed multiple times with deionized water, and then the entire surface of the copper plate is subjected to plasma activation treatment. Plasma bombardment is used to remove surface oxide impurities, increase surface energy and activity, and effectively enhance the adhesion of the subsequent nickel barrier layer plating. The treated surface is then ready for use.

[0057] S2. Prepare a barrier layer on the first surface of the pretreated substrate. A nickel barrier layer was prepared on the entire surface of a pretreated copper plate using an electroplating process. Using the copper plate as the cathode and a high-purity nickel plate as the anode, the plate was immersed in a conventional acidic nickel plating solution. Electroplating process parameters were precisely controlled to ensure stable current density and uniform plating time, ultimately forming a uniform, dense, pinhole-free, and crack-free nickel barrier layer with a thickness of 3 μm on the entire surface of the plate. After electroplating, the plate surface was thoroughly rinsed with deionized water to remove residual plating solution, and then dried at a low temperature to remove surface moisture and residual impurities. This dense nickel barrier layer effectively blocks the oxidation of the copper substrate under high-temperature conditions and inhibits the diffusion of copper elements to the surface metal film, preventing the formation of brittle compounds at the interface, increased thermal resistance, and structural failure. This significantly improves the high-temperature stability and service life of the composite substrate.

[0058] Step S3: Prepare a thermal interface plastic layer in the target area of ​​the barrier layer. In this embodiment, a highly ductile and thermally conductive indium thin film is used as a highly elastic thermally conductive functional layer at the thermal interface. A thick indium thin film is precisely fabricated in the heat source contact area (A region) of the nickel barrier layer using a combination of photolithography and electroplating, achieving precise zoned film deposition. The specific process is as follows: (1) Partition masking treatment: Selective masking is achieved by photolithography masking process, which can be achieved by either photolithography machine photoresist exposure and development or photosensitive dry film bonding exposure. Through the pre-coating baking, exposure and development or dry film bonding, exposure and development process, the non-target areas of the base copper plate, that is, the areas that do not need to be coated, are completely and tightly masked and protected by the mask layer, while the surface of the nickel barrier layer in the target area is fully exposed, ensuring that the indium film is deposited only in the functional area.

[0059] (2) Electroplating preparation of thick indium thin films: The substrate with a precise mask is placed in an indium plating bath, and an indium layer is deposited on the exposed nickel layer surface by electroplating. The electroplating process parameters are stably controlled, and deposition continues until the indium film thickness reaches the desired thickness. The indium film of this thickness has excellent microelasticity and plastic deformation ability, which can fully adapt to the micro-concave and convex morphology of the chip contact surface, completely fill the tiny gaps at the interface, and greatly reduce the interface contact thermal resistance.

[0060] (3) Mask stripping and post-processing: After electroplating, the substrate is immersed in a special organic solvent at a constant temperature to fully swell and strip the photoresist or dry film mask layer in non-target areas. Finally, the entire substrate is cleaned with deionized water and dried at low temperature to remove residual solvents and process impurities, thus completing the preparation of a high-precision and high-stability thermally conductive composite substrate.

[0061] The thermally conductive composite substrate prepared in this embodiment uses a high thermal conductivity copper plate as the base layer, with a total thickness of 50 μm. A 3 μm thick nickel barrier layer and a 15 μm thick indium thin film as a thermal interface plastic layer are also included. Under standard assembly conditions, the total thermal resistance is 0.028 °C·cm.2 / W; at a chip heat flux density of 100W / cm² 2 Under these conditions, the interface temperature rise is only 2.8℃, which significantly improves heat dissipation performance compared to traditional thermal grease solutions. Furthermore, it avoids the aging and drying defects of organic media, exhibiting excellent long-term heat dissipation stability. This embodiment utilizes the high thermal conductivity and high plasticity of indium to achieve ultra-low interface thermal resistance, completely solving the problems of thermal resistance drift and heat dissipation attenuation associated with long-term high-temperature use of traditional thermal media. Simultaneously, the excellent thermal conductivity of the copper substrate, combined with precise flatness and roughness control, and the anti-oxidation and anti-diffusion properties of the nickel barrier layer, gives the composite substrate excellent heat dissipation stability and long-term service reliability, meeting the long-term heat dissipation requirements of high heat flux density chips.

[0062] While the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the invention. Any variations and modifications can be made by those skilled in the art without departing from the spirit and scope of the invention. Therefore, any modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention, without departing from the scope of the invention, fall within the protection scope defined by the claims of the present invention.

Claims

1. A thermally conductive composite substrate, characterized in that: The device includes a base layer, a barrier layer, and a thermal interface plastic layer. The base layer is a thermally conductive material, and the barrier layer is located between the base layer and the thermal interface plastic layer. The barrier layer is one or more of a metal, a metal alloy, or a metal compound, and the thermal interface plastic layer contains indium. The surface of the base layer facing the thermal interface plastic layer is the first surface of the base layer. The heating element is in contact with the thermal interface plastic layer. The barrier layer includes a target area and a non-target area, and the target area is in contact with the thermal interface plastic layer.

2. The thermally conductive composite substrate according to claim 1, characterized in that: The roughness of the first surface of the base layer is less than or equal to 4 μm.

3. The thermally conductive composite substrate according to claim 1, characterized in that: The thickness of the barrier layer is 0.2μm to 5μm.

4. The thermally conductive composite substrate according to claim 1, characterized in that: The barrier layer further includes an adhesive layer, which is located close to the base layer. The adhesive layer is any one of titanium, zirconium, tungsten, and tantalum, and is used to enhance the surface adhesion between the barrier layer and the base layer.

5. The thermally conductive composite substrate according to claim 1, characterized in that: The thickness of the thermal interface plastic layer is 2μm~30μm.

6. The thermally conductive composite substrate according to claim 1, characterized in that: A metal-bonded metallurgical interface is formed between the base layer and the barrier layer, and between the barrier layer and the thermal interface plastic layer.

7. The thermally conductive composite substrate according to claim 1, characterized in that: The thermal interface plastic layer is an indium-silver alloy, wherein the mass content of indium is greater than 90%.

8. A method for preparing a thermally conductive composite substrate, characterized in that, Includes the following steps: S1: Pre-treat the substrate, the pre-treatment including ultrasonic degreasing and plasma activation treatment of the substrate surface to obtain the pre-treated substrate; S2: A barrier layer is deposited on the surface of the pretreated substrate using electroplating or physical vapor deposition. S3: Apply a thermal interface plastic layer to the target area of ​​the barrier layer using electroplating or physical vapor deposition.

9. The method for preparing a thermally conductive composite substrate according to claim 8, characterized in that: In step S2, the physical vapor deposition method uses PVD magnetron sputtering to deposit a barrier layer of metal stack structure on the first surface of the pretreated substrate.

10. The method for preparing a thermally conductive composite substrate according to claim 8, characterized in that: In step S3, a thermal interface plastic layer is deposited in the target area of ​​the barrier layer using a vacuum evaporation process.