Fibrous oil crystals and their manufacturing method
By controlling the structure and manufacturing conditions of triglycerides, fibrous oil crystals of a specific shape are formed, solving the problem of insufficient dispersibility of oils in food and cosmetics, achieving efficient dispersion and gelation capabilities, and improving the processing performance and health benefits of oils.
Patent Information
- Application Number
- CN202580029185.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-03-28
- Filing Date
- 2025-04-25
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to form highly functional fibrous crystals in oils and fats, and existing oil and fat crystal materials exhibit insufficient dispersibility in food and cosmetics, affecting their processing performance and health benefits.
By controlling the structure and manufacturing conditions of triglycerides, fibrous lipid crystals with specific shapes and aspect ratios are formed, including combinations of ABA-type and AAB-type triglycerides. The solution is prepared and the crystal growth is controlled using a polarizing microscope.
It achieves efficient dispersibility and gelation in hydrophobic solvents, making it suitable for the development of gel-like and low-saturation products, and improving the processing performance and health of oils.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention relates to a type of oil crystal made from oils and fats. Background Technology
[0002] Fibers are long, slender materials that combine softness and rigidity. They are made from a wide variety of materials, ranging from natural sources like cotton or silk to those derived from petroleum, carbon, and glass, and are used in a wide range of fields, including the textile industry, chemical industry, and regenerative medicine. Furthermore, nanofibers, with diameters on the nanometer scale, exhibit optical properties resulting from their high specific surface area and nanoscale effects, and are being utilized as high-value-added functional materials.
[0003] Due to its characteristic morphology, it is effective even in the food industry. Cellulose nanofibers made from woody materials are used in food applications, and by adding them to food, they can impart texture modification, thickening, and water retention effects.
[0004] However, although cellulose nanofibers are suitable for aquatic food, their low dispersibility in oils and fats remains a concern. Furthermore, even for materials whose lipophilicity is improved through cellulose derivatization, there is still a problem of insufficient dispersibility in oils and fats for food applications. Additionally, there is the issue of the need to specify additives.
[0005] Against this backdrop, there is a need for a highly functional fibrous material that can be safely used in food and cosmetic applications and is dispersible in hydrophobic solvents.
[0006] It is known that the functionality of processed fats is closely related to fat crystals. Without fat crystals, processed fats cannot exhibit their various functions, such as the softness of being ready to use immediately after being taken out of the refrigerator, the heat resistance of not dissolving even in high summer temperatures, the ability to stretch along with the dough when kneaded into pie dough, the melt-in-your-mouth texture of whipped cream, and the bubble stability of buttercream. Therefore, controlling fat crystals is an important topic in the development of processed fats. Throughout the long history of fats, crystallization behavior has been systematically studied. The crystallization of fats begins with the formation of a layered structure (lamellar structure) of parallel hydrocarbon chains of fatty acids. The lamellar structure is characterized by five structural elements: chain length, sublattice structure (hydrocarbon chain stacking), arrangement of terminal methyl groups, configuration of double bonds, and conformation of glycerol. Lamellar structures can form crystalline nanoplatelets through stacking, and can further aggregate to form a single crystal. By further condensing clusters of crystals several micrometers in size, a three-dimensional crystalline network is formed. Fats and oils are mixtures of triglyceride molecules bonded together with various fatty acids. In butter and margarine, which are solid at room temperature, fat crystals composed of high-melting-point fats form a solid fat network, thus creating a structure that encloses the liquid oil composed of low-melting-point fats.
[0007] When processed oils were first developed, natural solid fats, primarily tallow, were used as raw materials. In this context, Germany developed a hydrogenation reaction in 1902 to convert liquid oils into solid fats. Hydrogenation involves adding hydrogen to oils in the presence of catalysts such as nickel, saturating unsaturated bonds. Unsaturated fatty acids become saturated fatty acids, raising the melting point of the oil. Consequently, partially hydrogenated oils from soybean oil and fish oil were widely used as solid fats in margarine. However, in addition to the saturation of unsaturated fatty acids, various side reactions occur during hydrogenation. From the 1990s to the 2000s, the health risks of trans fats, primarily their impact on ischemic heart disease, attracted significant attention. Interventional studies in humans reported increases in low-density lipoprotein cholesterol (LDL) and decreases in high-density lipoprotein cholesterol (HDL) caused by trans fatty acids, potentially increasing the risk of heart disease. Furthermore, studies showing that trans fatty acids increase the risk of arteriosclerosis have spurred efforts to reduce trans fatty acid intake, primarily in Europe and the United States. Due to the health effects of trans fatty acids, the use of partially hydrogenated oils has become difficult. Therefore, transesterified oils and fractionated oils are widely used in processed oils. Currently, palm oil, a natural oil that is solid at room temperature, and its fractionated and transesterified forms are widely used as raw materials for processed oils. However, in recent years, reports have linked saturated fatty acids in oils to cardiovascular disease, raising concerns about their health effects. Trans fatty acids and saturated fatty acids are the main components of high-melting-point oils that form crystals in processed oils. If the levels of saturated and trans fatty acids in processed oils are made to meet WHO standards, the crystallinity of the product will decrease significantly, resulting in properties similar to liquid oils. This would prevent the characteristic functions of processed oils, such as plasticity, ductility, and crispness that provides a fresh, crunchy texture, from being realized. Therefore, in recent years, research has been conducted worldwide on how to suppress saturated and trans fatty acids while reproducing the properties of solid processed oils.
[0008] The most attention has been focused on the exploration and utilization technologies of materials capable of gelling liquid oils, serving as alternatives to high-melting-point fats. While oleogels are primarily used in non-food applications such as as a hardener in lipsticks and tempura oils, they have gained attention in recent years as a potential alternative to edible solid fats, with the number of academic papers on oleogels increasing dramatically since around 2012. Oleogels are formed by adding a small amount, typically less than 10%, of a gelling agent to liquid oil. The gel formation mechanism can be broadly categorized into mechanisms involving the formation of solid particle networks and the formation of molecular polymer networks. Despite extensive research on oleogels over the past 20 years, challenges remain regarding their performance and industrial applications, and oleogels have not yet reached the level of industrial utilization.
[0009] In Patent Document 1, the inventors studied the relationship between the triglyceride composition and gelling ability of high-melting-point oils derived from palm oil processing, and disclosed that highly hydrogenated oils such as Hard Palm Oil Intermediate Extract (HMF) exhibit high gelling ability.
[0010] While gelling ability was confirmed in Patent Document 1, crystal shape was not. Although the amount of crystals can be controlled by the triglyceride composition, controlling the crystal shape is complex, and the relationship between gelling ability and crystal shape is not clear. The structure of triglycerides suitable for forming novel oil crystal shapes and the temperature profiles during the manufacturing process have also not been determined.
[0011] Existing technical documents
[0012] Patent documents
[0013] Patent document 1: Japanese Patent Application Publication No. 2022-180968. Summary of the Invention
[0014] Furthermore, in advancing research focusing on gelation capabilities, crystals in the solvent were investigated. As the structure and manufacturing conditions of triglycerides were continuously explored, and microscopic observation methods such as polarizing microscopy and dark-field microscopy were improved, crystals exhibited various shapes, sometimes appearing as fine granules or short needles with low aspect ratios. However, in some oils where the structure and manufacturing conditions of triglycerides were altered, under unpredictable specific manufacturing conditions, fibrous crystals resembling nanofibers were confirmed to form. These high aspect ratio fibrous crystals are single crystals with a particularly whisker-like morphology. Previously, the formation of fibrous crystals in oils was unknown; this discovery is the first confirmation within the scope of the present invention's knowledge.
[0015] In industrial applications, if the relationship between the formation of fibrous crystals and the structure and manufacturing conditions of triglycerides can be more specifically elucidated, it can be applied to the development of gel-like and low-saturation products, or to the control of the physical properties of processed oils. Based on this, further adjustments to the structure and manufacturing conditions of triglycerides were made, thus completing this invention.
[0016] That is, this disclosure provides the following invention: (1) A fibrous oil crystal.
[0017] (2) The fibrous oil crystals according to (1), wherein, The oil contains triglycerides that constitute fatty acids with 12 to 22 carbon atoms.
[0018] (3) The fibrous oil crystals according to (1) or (2), wherein, The oil contains a triglyceride whose carbon chain length differs from that of at least one of the three constitutive fatty acids.
[0019] (4) The fibrous oil crystals according to any one of (1) to (3), wherein, Two of the three constituent fatty acids of the triglyceride have the same carbon chain length.
[0020] (5) The fibrous oil crystals according to any one of (1) to (4), wherein, The oil contains triglycerides of the ABA or AAB type.
[0021] (6) The fibrous oil crystals according to any one of (1) to (5), wherein, The oil contains carbon atoms of type C. n-6 C n C n-6 C n-4 C n C n-4 C n-2 C n C n-2 C n+2 C n C n+2 C n+4 C n C n+4 C n+6 C n C n+6 Any of the triglycerides in the formula.
[0022] (7) The fibrous oil crystals according to any one of (1) to (6), wherein, The oil contains carbon atoms of type C. n-6 C n-6 C n C n-4 C n-4 C n C n-2 C n-2 C n C n+2 C n+2 C n C n+4 C n+4 C n C n+6 C n+6 C n Any of the triglycerides in the formula.
[0023] (8) The fibrous oil crystals according to any one of (1) to (7), wherein, The fibrous oil crystals are β'-type crystals.
[0024] (9) The fibrous oil crystals according to any one of (1) to (8), wherein, The length of the fiber is any one of the following: 10 μm or more, 30 μm or more, 50 μm or more, 70 μm or more, 90 μm or more, 110 μm or more, less than 1000 μm, less than 900 μm, less than 800 μm, less than 700 μm, less than 600 μm, 10 μm or more and less than 1000 μm, 30 μm or more and less than 900 μm, 50 μm or more and less than 800 μm, 70 μm or more and less than 700 μm, 90 μm or more and less than 600 μm, and 110 μm or more and less than 600 μm.
[0025] (10) Fiber-like oil crystals according to any one of (1) to (9), wherein, The width of the fiber is any one of the following: 1 nm or more, 10 nm or more, 50 nm or more, 100 nm or more, 200 nm or more, 300 nm or more, less than 2000 nm, less than 1800 nm, less than 1600 nm, less than 1400 nm, less than 1200 nm, less than 1000 μm, 1 nm or more and less than 2000 nm, 10 nm or more and less than 1800 nm, 50 nm or more and less than 1600 nm, 100 nm or more and less than 1400 nm, 200 nm or more and less than 1200 nm, and 300 nm or more and less than 1000 μm.
[0026] (11) The fibrous oil crystals according to any one of (1) to (10), wherein, The aspect ratio of the fiber is any one of the following: 2 or more, 5 or more, 10 or more, 20 or more, 30 or more, 40 or more, 50 or more, less than 1,000,000, less than 100,000, less than 10,000, less than 5,000, less than 2,000, 2 or more and less than 1,000,000, 5 or more and less than 100,000, 10 or more and less than 10,000, 20 or more and less than 5,000, 30 or more and less than 2,000, 40 or more and less than 2,000, and 50 or more and less than 2,000.
[0027] (12) Fiber-like oil crystals according to any one of (1) to (11), wherein, The curvature of the fiber is any one of the following: greater than 1, greater than 1.5, greater than 2, greater than 5, less than 10000, less than 1000, less than 100, less than 50, greater than 1 and less than 10000, greater than 1 and less than 1.5 and less than 1000, greater than 2 and less than 100, and greater than 5 and less than 50.
[0028] (13) An oil and fat composition, wherein, The oil composition contains fibrous oil crystals as described in any one of (1) to (12).
[0029] (14) The oil composition according to (13), wherein, It contains fibrous oil crystals in any one of the following proportions: 5% or more by mass, 10% or more by mass, 20% or more by mass, 30% or more by mass, 40% or more by mass, 50% or more by mass, 60% or more by mass, 70% or more by mass, 80% or more by mass, 90% or more by mass, or 95% or more by mass.
[0030] (15) A food or chemical product comprising or containing fibrous oil crystals, wherein, The fibrous oil crystals are any one of (1) to (12).
[0031] (16) A food or chemical product according to (15) comprising or containing fibrous oil crystals, wherein, The fibrous oil crystals or the oil composition containing the fibrous oil crystals are crystals or oil compositions formulated as either a composition containing fibrous oil crystals or an aggregate of fibrous oil crystals, wherein the fibrous oil crystals are present in a proportion of 0.1% by mass or more, 0.5% by mass or more, 1% by mass or more, 2% by mass or more, 5% by mass or more, 10% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more.
[0032] The method for manufacturing fibrous oil crystals according to any one of (17) (1) to (12), wherein, The method for manufacturing the fibrous oil crystals includes the following steps: The process of preparing a solution involves mixing an oil, which is used as a raw material for fibrous oil crystals, with a lipophilic solvent and dissolving the oil in the lipophilic solvent under heating. The process of cooling the solution to promote crystal nucleation; and The process of heating and storing the cooled solution to promote the growth of the fibrous oil crystals.
[0033] (18) A method for promoting the formation of fibrous oil crystals, wherein, The oil raw material uses triglycerides from which the carbon chain length of one of the three constituent fatty acids of triglycerides is different from the carbon chain length of at least one of the other constituent fatty acids.
[0034] (19) According to the method described in (18), wherein, Two of the three constituent fatty acids of the triglyceride have the same carbon chain length.
[0035] (20) A method for promoting the formation of fibrous oil crystals, wherein, When oils used as raw materials are dissolved in a lipophilic solvent under heating and then cooled, and then heated and stored to generate fibrous oil crystals, the fibrous oil crystals grown through the storage are made into β'-type crystals.
[0036] (21) Fibrous oil crystals according to any one of (1) to (12), wherein, The oil contains triglycerides whose three constituent fatty acids are a combination of ABA and AAA, ABA and BBB, AAB and AAA, or AAB and BBB.
[0037] (22) The fibrous oil crystals according to (21), wherein, The mass ratio of the triglycerides is 50:50 to 90:10.
[0038] (23) A method for controlling the shape of fibrous oil crystals, wherein, Oil raw materials containing triglycerides are those with a combination of ABA and AAA, ABA and BBB, AAB and AAA, or AAB and BBB.
[0039] (24) The method for controlling the shape of fibrous oil crystals according to (23), wherein, The mass ratio of the triglycerides is 50:50 to 90:10.
[0040] (25) A method for promoting the formation of fibrous oil crystals or controlling the shape of fibrous oil crystals, wherein, When manufacturing fibrous oil crystals from oils that serve as raw materials for fibrous oil crystals, oils and emulsifiers are used as the raw materials.
[0041] The method for manufacturing fibrous oil crystals according to any one of (26) (1) to (12), wherein, The method for manufacturing the fibrous oil crystals includes the following steps: The process of preparing a solution involves mixing an oil, which is used as a raw material for fibrous oil crystals, with a lipophilic solvent, and dissolving the oil in the lipophilic solvent under heating; and The process of forming fibrous oil crystals by adding seed crystals made of oil as raw material for fibrous oil crystals to the solution.
[0042] Compared to liquid oils, high-melting-point oils are among the materials exhibiting gelling ability. High-melting-point oils can be easily dissolved into liquid oils simply by heating, making them easy to handle and, due to their low cost, suitable for industrial use as oil gelling agents. However, in recent years, when using high-melting-point oils containing saturated fatty acids as gelling agents as described above, it has been desirable to effectively initiate gelation with the smallest possible amount of addition. The fibrous oil crystals of the present invention can efficiently gellelate solvents even in small quantities.
[0043] According to the present invention, it can be safely used in the development of gel-like products and low-saturation products, or for the physical property control of processed oils, for use in food and beverage and chemical products, and has dispersibility in hydrophobic solvents, and has industrial potential for use in highly functional fibrous materials. Attached Figure Description
[0044] Figure 1 This is a dark-field micrograph of the oil crystals in Example 3.
[0045] Figure 2 This is a dark-field micrograph of the oil crystals in Example 6.
[0046] Figure 3 This is a dark-field micrograph of the oil crystals in Example 7.
[0047] Figure 4 This is a dark-field micrograph of the oil crystals in Example 8.
[0048] Figure 5 Dark-field micrograph of the oil crystals in Comparative Example 1.
[0049] Figure 6 Dark-field micrograph of the oil crystals in Comparative Example 2.
[0050] Figure 7 Dark-field micrograph of the oil crystals in Comparative Example 3.
[0051] Figure 8 This is a dark-field micrograph of the oil crystals in Example 9.
[0052] Figure 9 This is a dark-field micrograph of the oil crystals from Example 10.
[0053] Figure 10 This is a dark-field micrograph of the oil crystals from Example 11.
[0054] Figure 11 This is a dark-field micrograph of the oil crystals from Example 12.
[0055] Figure 12 This is a dark-field micrograph of the oil crystals in Example 13.
[0056] Figure 13 This is a dark-field micrograph of the oil crystals in Example 14.
[0057] Figure 14 This is a dark-field micrograph of the oil crystals in Example 15.
[0058] Figure 15 This is a dark-field micrograph of the oil crystals in Example 16.
[0059] Figure 16 This is a dark-field micrograph of the oil crystals in Example 17.
[0060] Figure 17This is a dark-field micrograph of the oil crystals in Example 18.
[0061] Figure 18 This is a dark-field micrograph of the oil crystals in Example 19.
[0062] Figure 19 This is a dark-field micrograph of the oil crystals from Example 20.
[0063] Figure 20 This is a dark-field micrograph of the oil crystals from Example 21.
[0064] Figure 21 This is a dark-field micrograph of the oil crystals in Example 22.
[0065] Figure 22 This is a dark-field micrograph of the oil crystals in Example 23.
[0066] Figure 23 This is a dark-field micrograph of the oil crystals in Example 27.
[0067] Figure 24 This is a dark-field micrograph of the oil crystals in Example 28.
[0068] Figure 25 This is a dark-field micrograph of the oil crystals in Example 29. Detailed Implementation
[0069] The following is a detailed description of the methods used to implement the present invention.
[0070] (Fibrous oil crystals)
[0071] In this invention, fibrous oil crystals refer to oil crystals having a fibrous shape. The fibrous oil crystals of this invention can use oils and triglycerides, which are their main components. The fibrous oil crystals of this invention can also be called fibrous triglyceride crystals. The constitutive fatty acids of triglycerides, as fatty acids derived from oils, can be understood by referring to the technical knowledge available at the time of this application regarding the types and number of carbon atoms of their long-chain fatty acids.
[0072] The fibrous shape referred to here is a long, continuous, and winding rope-like shape, unlike the needle-like and granular shapes previously known as crystals of oils. Whiskers are an example of this.
[0073] The fiber length is not particularly limited, and can be, for example, 10 μm or more, 30 μm or more, 50 μm or more, 70 μm or more, 90 μm or more, or 110 μm or more. These lower limits are preferably in descending order to further distinguish it from linear needle-like crystals. Additionally, the fiber length can be less than 1000 μm, 900 μm or less, 800 μm or less, 700 μm or less, or 600 μm or less. However, the upper limits shown here are illustrative examples, and the fiber length can also be longer than these.
[0074] The width of the fibers is not particularly limited; for example, it can be 1 nm or more, 10 nm or more, 50 nm or more, 100 nm or more, 200 nm or more, or 300 nm or more. Alternatively, it can be less than 2000 nm, less than 1800 nm, less than 1600 nm, less than 1400 nm, less than 1200 nm, or less than 1000 μm. Since the crystals emit light in the microscope, they may appear thicker than the actual fibers. Furthermore, in samples stored at lower temperatures than when manufacturing fibrous oil crystals, the coarsening of the crystals is suppressed, resulting in a tendency for finer fibers to increase, making measurement in the microscope difficult. However, these factors are also taken into account here, and examples are described. Furthermore, in the case of high concentrations of fibrous crystals, measurement becomes difficult due to the overlap between the crystals; these factors are also taken into account here, and examples are described.
[0075] The aspect ratio of the fiber, i.e., the ratio of the fiber's length to its width, is not particularly limited and can be, for example, 2 or more, 5 or more, 10 or more, 20 or more, 30 or more, 40 or more, or 50 or more. As for the aspect ratios of fibers that are characteristic of the fibrous oil crystals of the present invention, exhibiting elongated continuity and reflecting a more curved, rope-like shape, their lower limit values are preferably in descending order. Furthermore, the aspect ratio of the fiber can be 1,000,000 or less, 100,000 or less, 10,000 or less, 5,000 or less, or 2,000 or less. However, the upper limit value shown here is exemplified, and the fiber length may also be longer than that.
[0076] The fiber curvature, which is the ratio of fiber length to the straight-line distance from the start to the end of the fiber, is not particularly limited and can be, for example, greater than 1, greater than 1.5, greater than 2, or greater than 5. Additionally, the fiber curvature can be less than 10,000, less than 1,000, less than 100, or less than 50. Curved fibers form rigid gels, while straight fibers form gels with high shear resistance. However, the upper limit shown here is for illustrative purposes; the fiber curvature may also be higher.
[0077] The length, width, aspect ratio, and curvature of the fibers in the aforementioned fibrous oil crystals can be measured for a single fiber, or they can be the average value of 20 individual fibers measured from an optional sample of individual fibers observed in a microscope photograph.
[0078] The fact that oil crystals are fibrous can be confirmed by observing various microscopic methods, such as polarized light, bright field, dark field, and phase difference observation, and by visual inspection.
[0079] (triglycerides)
[0080] Triglycerides have a structure in which three fatty acid molecules are bonded to one molecule of glycerol. The first, second, and third sites of a triglyceride refer to the positions where fatty acids are bound. As triglycerides found in oils and fats, there are three types: trisaturated triglycerides (SSS) with all saturated fatty acid S molecules bonded to the first, second, and third sites; disaturated triglycerides (SUS, SSU, USS) with two saturated fatty acid S molecules and one unsaturated fatty acid U molecules bonded to one molecule of glycerol; diunsaturated triglycerides (SUU, UUS, USU) with two unsaturated fatty acid U molecules and one saturated fatty acid S molecules bonded to one molecule of glycerol; and triunsaturated triglycerides (UUU) with all unsaturated fatty acid U molecules bonded to the first, second, and third sites. Here, saturated fatty acid S refers to all saturated fatty acids contained in oils and fats. Saturated fatty acids (S) found in edible oils include butyric acid (4), hexanoic acid (6), caprylic acid (8), capric acid (10), lauric acid (12), myristic acid (14), palmitic acid (16), stearic acid (18), arachidic acid (20), docosanoic acid (22), and tetracosanoic acid (24). It should be noted that the values in parentheses for the above saturated fatty acids represent the number of carbon atoms in the fatty acid. Unsaturated fatty acids (U) found in edible oils include myristoleic acid (14:1), palmitoleic acid (16:1), hiragonic acid (16:3), oleic acid (18:1), linoleic acid (18:2), linolenic acid (18:3), eicosenoic acid (20:1), erucic acid (22:1), and squalane (24:1). It should be noted that the values in parentheses for the above unsaturated fatty acids represent the number of carbon atoms on the left and the number of double bonds on the right. The two or three saturated fatty acids S or unsaturated fatty acids U bonded to each triglyceride molecule are either the same fatty acid or different fatty acids. As for the oils and fats used in this invention, as with conventional edible oils and fats, a composition in which triglycerides constitute approximately all of the composition is preferred.
[0081] The triglycerides constituting the fibrous oil crystals of the present invention preferably have one or more saturated fatty acids ester-bonded to one molecule of glycerol, more preferably two or more saturated fatty acids, and even more preferably all three saturated fatty acids. Increasing the proportion of saturated fatty acids in the fatty acids constituting the triglycerides is beneficial for the formation of fibrous oil crystals. For example, since a higher proportion of saturated fatty acids results in lower solubility of the triglycerides used as raw materials for the fibrous oil crystals in the solvent during manufacturing, more fibrous oil crystals can be formed in the solvent.
[0082] Regarding the suitability for the formation of fibrous oil crystals, there is no particular limitation on the number of carbon atoms in the saturated fatty acid, but 12 to 22 is preferred. More specifically, it is 12, 14, 16, 18, 20, or 22. The saturated fatty acid can be linear or branched, but linear is preferred.
[0083] It can be considered that, in the formation of fibrous crystals, the important factor is not the type of fatty acid, but the combination of chain lengths. The triglycerides constituting the fibrous oil crystals of the present invention preferably have a difference in chain length between the fatty acids that are ester-bonded to one molecule of glycerol. If the triglycerides have a difference in chain length, it is suitable for the formation of fibrous oil crystals. The chain length difference of the triglycerides is preferably 2 or more. Specifically, 2, 4, and 6 are examples.
[0084] In other words, the fibrous oil crystals of the present invention are preferably triglycerides in which the carbon chain length of one of the three constitutive fatty acids is different from the carbon chain length of at least one other constitutive fatty acid. Preferably, the carbon chain lengths of two of the three constitutive fatty acids in the triglyceride are the same.
[0085] As triglycerides containing fatty acids with varying chain lengths, they exist in ABA and AAB forms. The ABA form is suitable for the formation of fibrous lipid crystals.
[0086] ABA type, using C as the number of carbon atoms n1 C n C n1 The expression is: n represents an integer, and n1 represents any integer among n-6, n-4, n-2, n+2, n+4, and n+6. Examples of n1 that are particularly suitable for the formation of fibrous fat crystals include n-2, n+4, and n-4.
[0087] AAB type, using C as the number of carbon atoms. n1 C n1 C n The expression is as follows. n and n1 are the same as above. As an example particularly suitable for the formation of fibrous oil crystals, n1 can be exemplified as n-4.
[0088] (A combination of triglycerides)
[0089] In the formation of fibrous crystals, the shape of the fibrous crystals can be controlled by optionally combining different triglycerides. This invention provides a method for controlling the shape of fibrous oil crystals by combining triglycerides. Specifically, considering the following factors, a method is provided to control the tortuosity of fibrous oil crystals, particularly to further reduce the tortuosity, by selecting a combination of triglycerides. Furthermore, a method for improving the dispersibility of fibrous oil crystals is also provided, particularly a method for suppressing the formation of spherical aggregates from fibrous oil crystal fibers. Here, improving the dispersibility of fibrous oil crystals includes improving the dispersibility of linear fibers. Suppressing the formation of spherical aggregates from fibers includes suppressing spherical aggregates containing fibers with higher tortuosity.
[0090] Examples of combinations particularly well-suited for shape control of such fibrous crystals include combinations of ABA and AAA types, combinations of ABA and BBB types, combinations of AAB and AAA types, and combinations of AAB and BBB types.
[0091] ABA type is used as the number of carbon atoms, represented by C. n1 C n C n1 The expression is as follows. n and n1 are the same as above. As examples particularly suitable for shape control of fibrous oil crystals, n1 can be exemplified as n-2 and n-4.
[0092] AAB type is used as the number of carbon atoms, represented by C. n1 C n1 C n The expression is as follows. n and n1 are the same as above. As an example particularly suitable for shape control of fibrous oil crystals, n1 can be exemplified as n-4.
[0093] In the temperature-controlled method, the curvature of the fibrous crystals is reduced, and the combination suitable for forming straight fibers is as follows.
[0094] C n-2 C n C n-2 (ABA) + C n C n C n (BBB)
[0095] C n-4 C n C n-4 (ABA) + C n-4 C n-4 C n-4 (AAA)
[0096] Cn-4 C n-4 C n (AAB) + C n-4 C n-4 C n-4 (AAA)
[0097] In the seed crystal method, the combination that makes the fibrous crystals more curved and suitable for forming curved fibers is as follows.
[0098] C n-2 C n C n-2 (ABA) + C n C n C n (BBB)
[0099] C n-4 C n C n-4 (ABA) + C n-4 C n-4 C n-4 (AAA)
[0100] C n-4 C n-4 C n (AAB) + C n-4 C n-4 C n-4 (AAA)
[0101] There are no particular restrictions on the mass ratio of ABA to AAA, ABA to BBB, AAB to AAA, and AAB to BBB types. Changing this mass ratio can also alter the curvature of the fibrous crystals. As an example, their mass ratios range from 50:50 to 90:10.
[0102] For fibrous oil crystals, the formation of fibrous oil crystals is applicable if the oil crystals are of the β' type. It is known that oils exhibit polymorphism during crystallization. Polymorphism is defined as the phenomenon where substances with the same chemical composition exhibit different crystal structures, displaying different crystal forms. Polymorphism manifests as differences in physical properties such as melting point, density, solubility, and stability. The temporal transformation of metastable polymorphs into more stable polymorphs, and the transformation from one polymorph to another, is called polymorphic transformation. The crystal systems visible in triglycerides are mainly hexagonal α-type, orthorhombic perpendicular β'-type, and triclinic parallel β-type. However, in the β'-type sublattice, all hydrocarbon chains have faces orthogonal to the formation faces of neighboring hydrocarbons, and the molecular axes of triglycerides are tilted relative to the perpendiculars of the lamellar planes. Adjacent hydrocarbon chains, i.e., the repeating units of hydrocarbon chains located at the corner and center positions of the sublattice, are oriented perpendicularly to each other. Saturated triglycerides form intermolecular compounds. Triglycerides containing unsaturated fatty acids (POP / OPO, etc.) improve the stacking (lateral) of fatty acid chains by forming intermolecular compounds. Saturated triglycerides suggest a smoothing of the methylation plateau (vertical). Based on this, the correlation between crystal polymorphism and fiber formation was investigated, revealing a clear correlation between the crystal shape and crystal polymorphism of high-melting-point oils in liquid oils. Intermolecular compounds are formed according to the combination of components, and the crystal polymorphism produced during recrystallization after dissolution in the solvent changes until the crystal shape also changes. It should be noted that crystal polymorphism can be confirmed by the diffraction pattern of diffraction peaks originating from the sublattice in X-ray crystal structure analysis.
[0103] (grease)
[0104] Edible oils are typically used as the oils used in this invention. Examples of such oils include vegetable oils, animal oils, synthetic oils, and processed oils. They can be used alone or in combination of two or more as a blended oil.
[0105] Examples of vegetable oils include rapeseed oil, coconut oil, palm oil, sunflower oil, soybean oil, corn oil, sesame oil, perilla oil, flaxseed oil, peanut oil, safflower seed oil, high-oleic safflower seed oil, high-oleic sunflower oil, cottonseed oil, grapeseed oil, macadamia nut oil, hazelnut oil, pumpkin seed oil, walnut oil, camellia oil, tea seed oil, perilla seed oil, borage oil, olive oil, rice bran oil, rice germ oil, wheat germ oil, cocoa butter, palm kernel oil, and algae oil.
[0106] Examples of animal fats include fish oil (derived from the oil of tuna, mackerel, sardines, bonito, herring, etc.), lard, beef tallow, milk fat, mutton fat, and chicken fat.
[0107] Examples of synthetic fats include medium-chain fatty acid oils, diacylglycerols, and monoacylglycerols.
[0108] As a processed oil, it can also be an oil that has undergone the desired treatment. Examples of such treatments include fractionation based on its melting point, hydrogenation, and transesterification. One or more of the above treatments can also be performed on the oil.
[0109] To facilitate the formation of fibrous oil crystals, the combination of chain lengths and bond positions of the fatty acids constituting the triglycerides can be adjusted. Examples of methods for adjustment include extreme hydrogenation, fractional distillation based on melting point, and transesterification. High-melting-point oils obtained through these methods can be appropriately used. The raw material oil can be a mixture of different types of triglycerides, but since the fibrous oil crystals reflect the characteristics of the triglycerides used as the raw material and thus the main component of the high-melting-point oil, it is preferable to use triglycerides suitable for the formation of fibrous oil crystals as the main component. Alternatively, high-purity triglycerides prepared in a manner that standardizes the composition of triglycerides can also be used.
[0110] (A composition containing fibrous oil crystals, or an aggregate of fibrous oil crystals)
[0111] The fibrous oil crystals of the present invention can be prepared as a composition containing fibrous oil crystals and / or an aggregate of fibrous oil crystals.
[0112] The composition containing fibrous oil crystals is not particularly limited, and includes the oil compositions described below. Other components in the composition containing fibrous oil crystals are not particularly limited, and examples include solvents and emulsifiers.
[0113] The fibrous lipid crystal aggregate is not particularly limited in that it is an aggregate of fibrous lipid crystals, and may also be an aggregate of fibrous lipid crystals containing other components. As such an aggregate, the main object is an aggregate in which the fibrous lipid crystals are aggregated to the extent that the fibers overlap with each other when observed under a microscope, and includes compositions containing fibrous lipid crystals.
[0114] From the viewpoint of containing fibrous oil crystals in compositions and aggregates of fibrous oil crystals, it is preferable that the fibrous oil crystals are present in an amount specified in a predetermined proportion or higher relative to the total amount of oil crystals. This proportion, expressed in preferred order, is 5% by mass or more, 10% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, and 95% by mass or more.
[0115] The content of fibrous oil crystals in compositions containing fibrous oil crystals and aggregates of fibrous oil crystals is not particularly limited, but examples include 0.1% by mass or more, 0.5% by mass or more, 1% by mass or more, 2% by mass or more, 5% by mass or more, 10% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, and 90% by mass or more.
[0116] The absolute content of fibrous oil crystals in compositions containing fibrous oil crystals and aggregates of fibrous oil crystals is not particularly limited, but examples include 0.1g or more, 1g or more, 10g or more, 100g or more, 1kg or more, and 10kg or more.
[0117] (Oil and fat composition)
[0118] As an example of an oil composition containing fibrous oil crystals, oil composition A, which is a liquid oil used as a lipophilic solvent in the manufacture of fibrous oil crystals, can be cited. However, it is not limited to this. Other oil compositions containing fibrous oil crystals include margarine, fat spreads, shortening, and other plastic oil compositions, frying oil, edible oils, flavored edible oils, oil-in-water emulsions (concentrated milk, whipped cream, mayonnaise, etc.), and powdered oils. These can also be prepared using oil composition A as a raw material.
[0119] (Method for manufacturing fibrous oil crystals)
[0120] The method for manufacturing the fibrous oil crystals of the present invention is not particularly limited. For example, the temperature adjustment method and the seeding method can be cited.
[0121] [Temperature Adjustment Method]
[0122] (Step-1-1) The oil, which is used as the raw material for fibrous oil crystals, is mixed with a lipophilic solvent and other components, including an emulsifier, if added. The oil is then dissolved in the lipophilic solvent under heating to prepare a solution.
[0123] (Step-1-2) The solution is cooled to promote the formation of crystal nuclei.
[0124] (Step-1-3) The cooled solution is heated and stored to promote the growth of the fibrous oil crystals.
[0125] It can be considered that the preferred method of dissolution under high-temperature storage in step-1-1 and recrystallization in steps-1-2 and-1-3 facilitates changes in physical properties, allowing crystal growth under low supercooling conditions after the formation of mostly deformed, or in other words, mostly incomplete crystal nuclei with many lattice defects. Even with the same composition, the crystal shape will differ depending on the storage temperature.
[0126] (Process-1-1)
[0127] As the lipophilic solvent for mixing with the aforementioned oils, there are no particular limitations on any solvent that can uniformly dissolve the oils in step-1-1. Examples include edible oils, ester oils, squalene, ethanol, and hexane. Edible oils are preferred, and oils that are liquid at 20°C are particularly preferred. By heating the oils to above their melting point, the oils are dissolved in the lipophilic solvent. However, if the dissolution refers to uniform mixing of the oils, then dispersion is also included in a broader sense.
[0128] (Process 1-2)
[0129] There are no particular limitations on the method for cooling the above solution; examples include rapid cooling and slow cooling. Rapid cooling is particularly preferred in terms of forming fibrous oil crystals. Examples of rapid cooling methods include cooling with ice water, combined cooling mixers, perfect cooling mixers, votators, nexus integrated cooling mixers, polaron cooling mixers, and ronotor cooling mixers.
[0130] As for the quenching rate, if it can generate crystal nuclei for forming fibrous oil crystals, there is no particular limitation on it. If expressed in a more preferred order, it is 2°C / min or more, 3°C / min or more, and 4°C / min or more.
[0131] The temperature of the cooled solution needs to be below the temperature at which crystal nuclei can form, i.e., below the crystallization temperature. Since the sample becomes opaque after crystal formation, the crystallization temperature can be confirmed visually or by measuring the cooling temperature using a differential scanning calorimeter (DSC) and estimating the extrapolated onset temperature of the crystallization peak. From this perspective, the temperature of the cooled solution is preferably 1°C or less, more preferably 3°C or less, and even more preferably 5°C or less, lower than its extrapolated onset temperature.
[0132] The crystallization temperature varies depending on the triglyceride composition of the oil that forms fibrous oil crystals or the amount added, i.e. the concentration in the lipophilic solvent. Therefore, it cannot be generalized. For example, it may be below 35°C, below 25°C, or below 10°C.
[0133] (Process 1-3)
[0134] Storage temperature has an effect on crystal shape and crystal polymorphism. Regarding crystal polymorphism, for example, at storage temperature, a transfer can occur from α crystals formed by rapid cooling to the metastable polymorphism β' crystals.
[0135] The storage temperature for the cooled solution is not particularly limited, but from the viewpoint that fibrous oil crystals are more likely to form, it should be expressed in a more preferred order: 15°C or higher, 20°C or higher, 25°C or higher, 30°C or higher, and 35°C or higher. Regarding the upper limit of the storage temperature, since the fibrous oil crystals will disappear if the solution completely melts, it must be stored below the melting temperature of the fibrous oil crystals. The melting temperature can be confirmed by extrapolating the onset temperature of the melting peak obtained using differential scanning calorimetry (DSC), or by visual inspection since the solution becomes transparent after the crystals disappear.
[0136] The storage period after cooling is not particularly limited, but from the viewpoint that fibrous oil crystals are easily formed, if expressed in a more preferred order, it is 2 hours or more, 3 hours or more, 12 hours or more, 1 day or more, 3 days or more, and 6 days or more.
[0137] The storage temperature and storage period for step-3 have been shown as examples summarized above, but in terms of forming fibrous oil crystals, there are conditions corresponding to the triglycerides of the oils selected as raw materials. All disclosures, including the examples in this specification, are provided to those skilled in the art for reference to the technical common sense at the time of application regarding conditions that enable the formation of fibrous oil crystals.
[0138] [Seed Crystal Method]
[0139] (Step-2-1) The oil, which is used as the raw material for fibrous oil crystals, is mixed with a lipophilic solvent and other components, including an emulsifier, if added. The oil is then dissolved in the lipophilic solvent under heating to prepare a solution.
[0140] (Step-2-2) By adding seed crystals made of oil as raw material for fibrous oil crystals to the solution, fibrous oil crystals are formed.
[0141] If the melting process in step-2-1 is carried out under high temperature storage, then adding seed crystals in step-2-2 will help to change the physical properties. The added seed crystals will become templates in the crystallization process, thereby forming fibrous oil crystals.
[0142] (Process 2-1)
[0143] As the lipophilic solvent to be mixed with the oil, there are no particular limitations on any lipophilic solvent that can uniformly dissolve the oil in step-2-1. Examples include edible oils, ester oils, squalene, ethanol, and hexane. Edible oils and ester oils are preferred, and oils that are liquid at 20°C are particularly preferred. By heating the oil above its melting point, the oil dissolves in the lipophilic solvent. Dissolution, if referring to uniform mixing of the oil, also broadly includes dispersion.
[0144] (Process 2-2)
[0145] The added seed crystal is not particularly limited and can be any oil that becomes a raw material for fibrous oil crystals, preferably meaning that it forms fibrous oil crystals. More preferably, the seed crystal is in a fibrous form.
[0146] The crystal polymorph of the seed crystal is not particularly limited and can be a crystal containing a polymorph of oil that is the same as the raw material for fibrous oil crystals, preferably meaning that it forms fibrous oil crystals.
[0147] As a seed crystal, any one of the following can be used: powder obtained by crushing oil, seed crystal that crystallizes oil in a solvent, or seed crystal that only extracts crystals after crystallizing oil in a solvent. However, from the viewpoint of being able to form fine and dispersed fibers, a seed crystal that crystallizes oil in a solvent is more preferred.
[0148] There is no particular lower limit to the addition ratio of seed crystals of oil as raw materials for fibrous oil crystals in the solution, but from the viewpoint of easily forming fibrous oil crystals, it is preferably expressed in the following more preferred order: 0.1% by mass or more, 0.5% by mass or more, 1% by mass or more, 5% by mass or more, and 10% by mass or more. Furthermore, regarding the upper limit of the addition ratio, from the viewpoint of not hindering the formation of fibrous oil crystals, it is preferably expressed in the following more preferred order: less than 1000% by mass, less than 500% by mass, and less than 100% by mass.
[0149] As for the temperature at which the seed crystal is added, since the effect of adding the seed crystal cannot be obtained if the seed crystal completely melts, it needs to be added at a temperature lower than the melting temperature of the seed crystal. The melting temperature can be confirmed by extrapolating the onset temperature of the melting peak obtained by temperature measurement using a differential scanning calorimeter (DSC), or by visual inspection as the crystal becomes transparent upon disappearance.
[0150] When manufacturing fibrous oil crystals from oils used as raw materials, by incorporating an emulsifier into the triglycerides of the oil, the formation of fibrous oil crystals can be promoted or the shape of the fibrous oil crystals can be controlled. This invention provides a method for promoting the formation of fibrous oil crystals or controlling the shape of fibrous oil crystals by using oils and emulsifiers as raw materials. In particular, a method for controlling the tortuosity of fibrous oil crystals is provided, including a method for reducing the tortuosity, and a method for promoting the formation of such low-torsional ... Figure 11 Compared to, the addition of emulsifiers Figures 19-22 Microscopic images show the promotion of fibrous oil crystal formation or control of the shape of fibrous oil crystals as described above. In particular, a tendency to reduce spherical aggregation caused by curved fibers and promote the dispersion of straight fibers can be observed.
[0151] There are no particular limitations on emulsifiers, and examples include glycerol fatty acid esters, glycerol organic acid fatty acid esters, polyglycerol esters (polyglycerol fatty acid esters, polyglycerol condensed ricinoleate (PGPR)), sorbitan fatty acid esters, sucrose fatty acid esters, propylene glycol fatty acid esters, polyoxyethylene sorbitan fatty acid esters, lecithin (soybean lecithin, egg yolk lecithin, sunflower lecithin)), enzymatically hydrolyzed lecithin (soybean lysophosphatidylcholine, egg yolk lysophosphatidylcholine), saponins, calcium stearoyl lactylate (CSL), sodium stearoyl lactylate, sphingolipids, plant sterols, bile powder, and tomato glycolipids. When all the constituent fatty acids of the emulsifier are set to 100%, an emulsifier with a fatty acid ratio X+Y of 20% or more is preferred. Here, X is the proportion of unsaturated fatty acids in the fatty acids constituting the emulsifier. Y represents the proportion of fatty acids that are the same as the fatty acids that make up more than 10% of the fatty acids in the emulsifier when all the fatty acids constituting the fibrous oil crystals are set to 100%.
[0152] The amount of emulsifier added is not particularly limited. From the viewpoint of controlling the shape of fibrous oil crystals, it is, for example, 0.1% by mass or more, 0.5% by mass or more, 1% by mass or more, or 3% by mass or more, relative to the oil used as the raw material for fibrous oil crystals. Alternatively, it is, for example, 20% by mass or less, 12% by mass or less, or 8% by mass or less.
[0153] Based on the results disclosed above and the embodiments described below, the present invention also provides a method for promoting the formation of fibrous oil crystals by using an oil ester raw material containing a triglyceride in which the carbon chain length of one of the three constituting fatty acids of the triglyceride is different from the carbon chain length of at least one other constituting fatty acid. In this method, it is preferable that two of the three constituting fatty acids of the triglyceride have the same carbon chain length. For details regarding the carbon chain lengths of other triglycerides and constituting fatty acids, please refer to the above description.
[0154] This disclosure further provides a method for promoting the formation of fibrous oil crystals, wherein when oil as a raw material is dissolved in a lipophilic solvent under heating and then cooled, and then heated and stored to form fibrous oil crystals, the oil crystals grown through the above storage are made into β' type crystals.
[0155] (use)
[0156] The fibrous oil crystals of the present invention are suitable for food and beverage or chemical products due to their lipophilic or hydrophobic solvent affinity and gelation ability.
[0157] No particular limitations are placed on the fibrous oil crystals contained in this invention, but examples include staple breads, rolls, sweet breads, filled breads, French breads, rye breads, whole wheat breads, Danish pastries, croissants, Stollen, Panettone, Koolhoff breads, brioche breads, pizzas, and other types of bread, as well as sponge cakes, butter cakes, and pound cakes. Cakes, Japanese hot cakes, donuts, biscuits, cookies, Bouchée, waffles, pies, snacks and other pastries; bases (curry base, stew base, etc.); fillings for ready-to-eat side dishes; chocolate, buttercream, takoyaki, okonomiyaki; frozen foods; soups; sauces; beverages; fried batter; snacks and cooked foods; seafood products; meat products; mixed powders; enteral nutrition agents; oil and fat compositions; jelly, yogurt, gelée, salad dressings, care foods and other gel-like foods; industrial pharmaceuticals, fertilizers, paper, pulp, rubber, synthetic fibers, synthetic resins, medicines, dyes, detergents, cosmetics and other chemical products.
[0158] Example
[0159] The present invention will be described in more detail below through embodiments, but the present invention is not limited to these embodiments.
[0160] <Preparation and Evaluation of Oil Crystals>
[0161] Oil crystals were prepared and evaluated using the following method. In addition to the oil names listed in the table, high-purity triglycerides prepared to standardize the triglyceride composition were also used. It should be noted that in Table 1, “Triglyceride Composition of Oils,” “La” represents lauric acid, “P” represents palmitic acid, “S” represents stearic acid, and “B” represents docosanoic acid.
[0162] (Preparation of fat crystals)
[0163] After mixing the oils and fats listed in Table 1 into a solvent, they were dissolved by heating. 3g of the solution was weighed into a test tube and rapidly cooled with ice water at a rate of 4.6°C / min to induce crystallization. Afterward, the solution was stored under the conditions listed in Table 1 and allowed to stand at room temperature. It should be noted that Comparative Example 4 was crystallized by slow cooling.
[0164] When using the oils and emulsifiers listed in Tables 2A, 2B, and 3, after mixing the emulsifier into the solvent, dissolve it by heating. Weigh 3g into a test tube and rapidly cool it with ice water at a rate of 4.6°C / min to crystallize it. Then, store it under the conditions listed in Tables 2A, 2B, and 3 and allow it to stand at room temperature. It should be noted that for the emulsifiers in Tables 2B and 3, when all constituent fatty acids are taken as 100%, it refers to emulsifiers where the ratio of the aforementioned constituent fatty acids X+Y is 20% or more.
[0165] When using the oils listed in Table 4, after mixing the base oils, dissolve them by heating, weigh 3g into a test tube, and cool to 40°C at room temperature. After visually confirming that no oil crystals have precipitated, add the oil containing seed crystals, homogenize it by stirring, and then allow it to crystallize naturally at room temperature of 20°C. It should be noted that the oil containing seed crystals is the oil that, after mixing, is dissolved by heating, then weighs 3g into a test tube, and is rapidly cooled with ice water at a rate of 4.6°C / min to crystallize it in rapeseed oil or ethylhexyl palmitate.
[0166] (Evaluation of oil crystals)
[0167] The oil crystals obtained above were evaluated by visual observation using a dark-field microscope (Keyence VHX 7000 (1000x)) according to the following criteria.
[0168] [Formation of fibrous lipid crystals]
[0169] ○: It forms fibrous oil crystals.
[0170] ×: No fibrous oil crystals formed.
[0171] [Linearity of fibrous lipid crystals]
[0172] ◎+: Contains straight fibers.
[0173] ◎: A mixture of spherical aggregates composed of straight and curved fibers.
[0174] ○: Curved fibers coalesce into a spherical shape.
[0175] [Gel-forming ability]
[0176] In the preparation of the above-mentioned oil crystals, the minimum concentration of solvent required for gelation was evaluated according to the following criteria. Regarding the presence or absence of gelation, a gel that does not flow when the test tube is placed completely horizontally is considered a gelled gel.
[0177] ◎: 1.0% or less.
[0178] ○: Greater than 1.0% and less than 2.0%.
[0179] ×: Greater than 2.0%.
[0180] The results of the above evaluations are presented in Tables 1, 2A, 2B, and 4. In Tables 1, Examples 1-10 and Comparative Examples 1-5 are as follows: Examples 1-10 are... Figures 1-4 , Figure 8 , Figure 9 As shown in the microscope photographs, fibrous oil crystals were formed. On the other hand, Comparative Examples 1-5, as... Figures 5-7 As shown in the microscope images, they are aggregated or needle-like in shape, as previously known. Examples 11-29 in Tables 2A, 2B, and 4 also formed as shown in the microscope images. Figures 10-25 The microscopic photograph shows fibrous oil crystals. This was formed in Example 12 without the addition of emulsifiers. Figure 11 Examples 20-23 with added emulsifiers Figures 19-22 A comparison of microscopic images shows that the addition of emulsifiers promotes the formation of fibrous oil crystals. In particular, it can be observed that the aggregation of spherical crystals caused by curved fibers is reduced, and the tendency to disperse straight fibers is promoted.
[0181] (Evaluation of gel properties)
[0182] The physical properties of the gel obtained by preparing the above-mentioned oil crystals were evaluated using a rheometer (Anton Paar Japan MCR-302). The composition of the oil, emulsifier, and solvent is shown in Table 3. The gel was placed on the sample stage of the rheometer, which was set to 20°C, and clamped with a parallel plate of 25 mm diameter with a 1 mm gap between the sample and the sample stage. Strain dispersion was measured at a frequency of 1 Hz. The strain added to the sample was increased in stages from 0.001% to 100%, and the storage modulus of the linear viscoelastic region (LVER) of the obtained curve at this point was taken as the initial storage modulus. The gel strength was used as an indicator, and the gel was evaluated according to the following criteria.
[0183] [Gel strength]
[0184] ◎: Above 25000Pa.
[0185] ○: Above 5000Pa and below 25000Pa.
[0186] △: Above 1000 Pa and below 5000 Pa.
[0187] ×: Below 1000 Pa.
[0188] Subsequently, the post-shear storage modulus after the strain was gradually reduced from 100% to 0.001% was used as an indicator of the gel's shear resistance, and it was evaluated according to the following criteria.
[0189] Shear tolerance
[0190] ○: Above 2500Pa.
[0191] △: Above 500Pa and below 2500Pa.
[0192] ×: Below 500 Pa.
[0193] A higher initial storage modulus indicates a harder gel (higher gelling force). A higher storage modulus after shearing indicates a higher storage modulus maintained after shearing. Moreover, the less the change in storage modulus before and after shearing, the more likely the gel is to be considered not hard and brittle, but rather a gel with high structural resilience (high thixotropy).
[0194] The results of the above evaluations are shown in Table 3.
[0195] [Table 1]
[0196] [Table 2A]
[0197] [Table 2B]
[0198] [Table 3]
[0199] [Table 4]
Claims
1. A fibrous oil crystal.
2. The fibrous oil crystals according to claim 1, wherein, The oil contains triglycerides that constitute fatty acids with 12 to 22 carbon atoms.
3. The fibrous oil crystals according to claim 1, wherein, The oil contains a triglyceride whose carbon chain length differs from that of at least one of the three constitutive fatty acids.
4. The fibrous oil crystals according to claim 3, wherein, Two of the three constituent fatty acids of the triglyceride have the same carbon chain length.
5. The fibrous oil crystals according to claim 1, wherein, The oil contains triglycerides of the ABA or AAB type.
6. The fibrous oil crystals according to claim 1, wherein, The oil and fat contains a triglyceride of any one of C n-6 C n C n-6 , C n-4 C n C n-4 , C n-2 C n C n-2 , C n+2 C n C n+2 , C n+4 C n C n+4 , C n+ 6C n C n+6 6C 7. The fibrous oil crystals according to claim 1, wherein, The oil contains carbon atoms of type C. n-6 C n-6 C n C n-4 C n-4 C n C n-2 C n-2 C n C n+2 C n+2 C n C n+4 C n+4 C n C n+ 6C n+6 C n Any of the triglycerides in the formula.
8. The fibrous oil crystals according to claim 1, wherein, The fibrous oil crystals are β'-type crystals.
9. The fibrous oil crystals according to claim 1, wherein, The length of the fiber is any one of the following: 10 μm or more, 30 μm or more, 50 μm or more, 70 μm or more, 90 μm or more, 110 μm or more, less than 1000 μm, less than 900 μm, less than 800 μm, less than 700 μm, less than 600 μm, 10 μm or more and less than 1000 μm, 30 μm or more and less than 900 μm, 50 μm or more and less than 800 μm, 70 μm or more and less than 700 μm, 90 μm or more and less than 600 μm, and 110 μm or more and less than 600 μm.
10. The fibrous oil crystals according to claim 1, wherein, The width of the fiber is any one of the following: 1 nm or more, 10 nm or more, 50 nm or more, 100 nm or more, 200 nm or more, 300 nm or more, less than 2000 nm, less than 1800 nm, less than 1600 nm, less than 1400 nm, less than 1200 nm, less than 1000 μm, 1 nm or more and less than 2000 nm, 10 nm or more and less than 1800 nm, 50 nm or more and less than 1600 nm, 100 nm or more and less than 1400 nm, 200 nm or more and less than 1200 nm, and 300 nm or more and less than 1000 μm.
11. The fibrous oil crystals according to claim 1, wherein, The aspect ratio of the fiber is any one of the following: 2 or more, 5 or more, 10 or more, 20 or more, 30 or more, 40 or more, 50 or more, less than 1,000,000, less than 100,000, less than 10,000, less than 5,000, less than 2,000, 2 or more and less than 1,000,000, 5 or more and less than 100,000, 10 or more and less than 10,000, 20 or more and less than 5,000, 30 or more and less than 2,000, 40 or more and less than 2,000, and 50 or more and less than 2,000.
12. The fibrous oil crystals according to claim 1, wherein, The curvature of the fiber is any one of the following: greater than 1, greater than 1.5, greater than 2, greater than 5, less than 10000, less than 1000, less than 100, less than 50, greater than 1 and less than 10000, greater than 1 and less than 1.5 and less than 1000, greater than 2 and less than 100, and greater than 5 and less than 50.
13. An oil and fat composition, wherein, The oil composition contains fibrous oil crystals as described in any one of claims 1 to 12.
14. The oil and fat composition according to claim 13, wherein, It contains fibrous oil crystals in any one of the following proportions: 5% or more by mass, 10% or more by mass, 20% or more by mass, 30% or more by mass, 40% or more by mass, 50% or more by mass, 60% or more by mass, 70% or more by mass, 80% or more by mass, 90% or more by mass, or 95% or more by mass.
15. A food or chemical product comprising or containing fibrous oil crystals, wherein, The fibrous oil crystals are the fibrous oil crystals according to any one of claims 1 to 12.
16. The food or chemical product according to claim 15, comprising or containing fibrous oil crystals, wherein, The fibrous oil crystals or the oil composition containing the fibrous oil crystals are crystals or compositions formulated as either a composition containing fibrous oil crystals or an aggregate of fibrous oil crystals. The fibrous oil crystals are present in the composition containing the fibrous oil crystals and the fibrous oil crystal aggregate at any one of the following proportions: 0.1% by mass or more, 0.5% by mass or more, 1% by mass or more, 2% by mass or more, 5% by mass or more, 10% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, and 90% by mass or more.
17. A method for manufacturing fibrous oil crystals according to any one of claims 1 to 12, wherein, The method for manufacturing the fibrous oil crystals includes the following steps: The process of preparing a solution involves mixing an oil, which is used as a raw material for fibrous oil crystals, with a lipophilic solvent and dissolving the oil in the lipophilic solvent under heating. The process of cooling the solution to promote crystal nucleation; and The process of heating and storing the cooled solution to promote the growth of the fibrous oil crystals.
18. A method for promoting the formation of fibrous oil crystals, wherein, The oil raw material uses triglycerides from which the carbon chain length of one of the three constituent fatty acids of triglycerides is different from the carbon chain length of at least one of the other constituent fatty acids.
19. The method according to claim 18, wherein, Two of the three constituent fatty acids of the triglyceride have the same carbon chain length.
20. A method for promoting the formation of fibrous oil crystals, wherein, When oils used as raw materials are dissolved in a lipophilic solvent under heating and then cooled, and then heated and stored to generate fibrous oil crystals, the fibrous oil crystals grown through the storage are made into β'-type crystals.
21. The fibrous oil crystals according to claim 1, wherein, The oil contains triglycerides whose three constituent fatty acids are a combination of ABA and AAA, ABA and BBB, AAB and AAA, or AAB and BBB.
22. The fibrous oil crystals according to claim 21, wherein, The mass ratio of the triglycerides is 50:50 to 90:
10.
23. A method for controlling the shape of fibrous oil crystals, wherein, Oil raw materials containing triglycerides are those with a combination of ABA and AAA, ABA and BBB, AAB and AAA, or AAB and BBB.
24. The method for controlling the shape of fibrous oil crystals according to claim 23, wherein, The mass ratio of the triglycerides is 50:50 to 90:
10.
25. A method for promoting the formation of fibrous oil crystals or controlling the shape of fibrous oil crystals, wherein, When manufacturing fibrous oil crystals from oils that serve as raw materials for fibrous oil crystals, oils and emulsifiers are used as the raw materials.
26. The method for manufacturing fibrous oil crystals according to any one of claims 1 to 12, wherein, The method for manufacturing the fibrous oil crystals includes the following steps: The process of preparing a solution involves mixing an oil, which is used as a raw material for fibrous oil crystals, with a lipophilic solvent, and dissolving the oil in the lipophilic solvent under heating; and The process of forming fibrous oil crystals by adding seed crystals made of oil as raw material for fibrous oil crystals to the solution.
Citation Information
Patent Citations
Oil-and-fat composition
JP2022180968A