Mixed powder
By using a mixed powder containing iron-based soft magnetic powder, an insulating layer, and a specific lubricant in the pressed magnetic core, the problem of balancing demolding and compressibility was solved, achieving high density and efficient molding.
Patent Information
- Application Number
- CN202580026376.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-24
- Filing Date
- 2025-03-27
- Publication Date
- 2026-11-17
AI Technical Summary
Existing pressed powder magnetic cores have the problem of difficulty in achieving both demolding and compressibility during molding, especially after adding lubricant which reduces density and affects core performance.
The mixture of powders, including iron-based soft magnetic powder, insulating layer and lubricant, is used. The insulating layer is composed of condensed aluminum phosphate and organosilicon resin. The lubricant includes organic lubricant and inorganic layered compound, such as hexagonal boron nitride. The release properties and compressibility are improved by controlling the content and density of the lubricant.
This achieves improved demolding performance while maintaining high density, ensuring the molding quality and efficiency of pressed magnetic cores, reducing friction, and enhancing compressibility and demolding performance during molding.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to mixed powders. Background Technology
[0002] For a long time, the magnetic cores used in motors, transformers and other devices have been made of laminated electromagnetic steel plates, but in recent years, pressed powder magnetic cores have attracted attention.
[0003] When using electromagnetic steel sheets as the material, the magnetic core is formed by stacking, thus limiting the degree of freedom in shape. On the other hand, pressed powder magnetic cores are obtained by pressing soft magnetic particles with insulating layers, and their shape can be changed by altering the mold, thus achieving a degree of shape freedom that surpasses that of electromagnetic steel sheets. Furthermore, when using electromagnetic steel sheets as the material, the target shape is mainly obtained through methods such as punching, while pressed powder magnetic cores can be obtained through pressing, thus improving the yield. In addition, by using insulating layers to insulate the particles constituting the soft magnetic powder from each other in the pressed powder magnetic core, eddy current losses can be suppressed compared to magnetic cores manufactured by stacking electromagnetic steel sheets, enabling higher efficiency in motors, transformers, and the like.
[0004] In the manufacture of pressed powder magnetic cores, soft magnetic powder is mixed with a lubricant as needed. The lubricant acts as a lubricant when the mixed powder (pressed powder) obtained by pressing in a mold is removed from the mold (demolding). Typically, the pressed powder is demolded by a punch, but this generates significant frictional resistance due to friction between the pressed powder and the mold surface. However, by adding a lubricant, the friction between the pressed powder and the mold surface is reduced, allowing the pressed powder to be demolded with less demolding energy. Here, the lubricant typically has a lower density than the soft magnetic powder, so when a lubricant is added to obtain the necessary demolding properties, there is a tendency for the density of the resulting pressed powder (pressed powder density) to decrease. However, to obtain the desired performance as a magnetic core, it is necessary to achieve high density in the pressed powder core. Against this background, research has been conducted on a mixed powder containing soft magnetic powder and lubricant to simultaneously achieve demolding and compressibility.
[0005] In Patent Document 1, in addition to organic lubricants, a bismuth-based microparticle compound with a Mohs hardness of less than 3.5 was added as a soft inorganic substance in microparticle form.
[0006] Existing technical documents Patent documents Patent Document 1: Japanese Patent Publication No. 2013-505563 Summary of the Invention
[0007] The problem that the invention aims to solve According to the technology proposed in Patent Document 1, the compressibility and demolding properties are improved to some extent, but further performance improvement is required.
[0008] The present invention was made in view of the above-mentioned actual situation, and its purpose is to provide a mixed powder that has both excellent compressibility and release properties during molding.
[0009] Methods for solving problems This invention was made to solve the above-mentioned problems, and its main purpose is as follows.
[0010] 1. A mixed powder comprising: Iron-based soft magnetic powder; An insulating layer is formed on the surface of the particles constituting the aforementioned iron-based soft magnetic powder; and Lubricant The aforementioned lubricant includes organic lubricants and inorganic layered compounds.
[0011] 2. The mixed powder as described in 1 above, wherein S, as defined by the following formula (1), is greater than 0 and less than 0.50.
[0012] [Mathematical Expression 1] Where n is the number of the aforementioned lubricants, a i The content of each of the aforementioned lubricants is expressed in parts by mass relative to a total of 100 parts by mass of the aforementioned iron-based soft magnetic powder and the aforementioned insulating layer, ρ i It is based on g / cm 3 The density of each of the aforementioned lubricants is indicated.
[0013] 3. The mixed powder as described in 1 or 2 above, wherein the aforementioned insulating layer has, in sequence from the surface of the aforementioned particles toward the outside, a first coating layer comprising condensed aluminum phosphate and a second coating layer comprising silicone resin.
[0014] 4. The mixed powder as described in any one of 1 to 3 above, wherein the aforementioned inorganic layered compound is at least one selected from the group consisting of tungsten disulfide, molybdenum disulfide, hexagonal boron nitride, talc, mica and graphite.
[0015] 5. The mixed powder as described in 4 above, wherein the aforementioned inorganic layered compound is hexagonal boron nitride.
[0016] 6. The mixed powder as described in any one of 1 to 4 above, wherein the volume resistivity of the aforementioned inorganic layered compound is 1.0 × 10⁻⁶. 6 Ω·cm or higher.
[0017] The effects of the invention According to the present invention, a mixed powder that has both excellent compressibility and release properties during molding can be provided. Detailed Implementation
[0018] The method for implementing the present invention will be described in detail below. It should be noted that the following description represents examples of preferred embodiments of the present invention, and the present invention is not limited thereto. Furthermore, in the following description, iron-based powder refers to powder containing 50% by mass or more Fe.
[0019] [Mixed Powder] The mixed powder of the present invention comprises iron-based soft magnetic powder, an insulating layer formed on the surface of the particles constituting the aforementioned iron-based soft magnetic powder, and a lubricant. The aforementioned mixed powder is suitable for use as a pressed magnetic core. The aforementioned mixed powder can be an iron-based mixed powder or a soft magnetic mixed powder. The aforementioned mixed powder can be a mixed powder formed from iron-based soft magnetic powder, an insulating layer formed on the surface of the particles constituting the aforementioned iron-based soft magnetic powder, and a lubricant.
[0020] (Iron-based soft magnetic powder) As the aforementioned iron-based soft magnetic powder, iron powder or iron-based alloy powder can be used, for example. Iron powder is preferred from the perspective of good compressibility during pressure molding and ease of achieving high density. Here, "iron powder" refers to powder formed from Fe and unavoidable impurities, and is generally referred to as "pure iron powder" in this technical field. Furthermore, "iron-based alloy powder" refers to alloy powder containing 50% by mass or more of Fe.
[0021] The aforementioned iron-based soft magnetic powder is preferably an atomized powder. Powders obtained by oxide reduction and electrolytic extraction have low apparent density, and even with additional processing such as pulverization to improve apparent density, sufficient apparent density cannot be obtained. Therefore, from the viewpoint of improving powder density, the aforementioned iron-based soft magnetic powder is preferably a powder manufactured using an atomization method (atomized powder). An atomization method is a method of pulverizing and cooling molten metal, and any of water atomization, gas atomization, or centrifugal atomization can be used. Water atomization is a method of blowing water onto molten metal to pulverize it, while gas atomization is a method of blowing gas to pulverize it. Both water and gas can also be blown to pulverize it. Centrifugal atomization is a method of pulverizing molten metal using centrifugal force based on rotation. Powders obtained using two or more of these methods can be combined. That is, the aforementioned iron-based soft magnetic powder can be at least one selected from the group consisting of gas atomized powder, water atomized powder, and centrifugal atomized powder. When using water atomization, the particle surface has numerous unevennesses, making particle entanglement more likely. This, when molded into pressed powder magnetic cores, improves the strength of the cores. Furthermore, water atomization is inexpensive. Therefore, from the viewpoint of strength and cost of the resulting pressed powder magnetic cores, water-atomized powder is preferred. Water-atomized iron powder is even more preferred. In contrast, gas atomization allows for mass production; therefore, from the viewpoint of mass production, gas-atomized powder is preferred.
[0022] The apparent density of the aforementioned iron-based soft magnetic powder is not limited, but from the viewpoint of easily manufacturing high-density pressed powder magnetic cores, 2.8 Mg / m³ is preferred. 3 That's all. There's no specific upper limit for apparent density; typically, it can be set to 5.0 Mg / m³. 3 the following.
[0023] The average particle size of the aforementioned iron-based soft magnetic powder is not particularly limited, but from the viewpoint of improving flowability and facilitating filling into the mold during the manufacture of pressed magnetic cores, it is preferably 10 μm or more, and more preferably 60 μm or more. On the other hand, for the same reason, the aforementioned average particle size is preferably 200 μm or less. Here, the aforementioned average particle size uses the median particle size D based on volume, determined by laser diffraction. 50 .
[0024] (Insulation layer) The mixed powder of the present invention has an insulating layer formed on the surface of the particles constituting the aforementioned iron-based soft magnetic powder. By having the aforementioned insulating layer, insulation between particles can be ensured, and short circuits between particles can be suppressed.
[0025] As the aforementioned insulating layer, any coating film can be used. The aforementioned insulating layer can be a single-layer coating film or a multilayer coating film containing two or more layers. The aforementioned multilayer coating film can be a multilayer coating film formed from the same type of coating film or a multilayer coating film formed from different types of coating films.
[0026] As the aforementioned insulating layer, for example, one or both of inorganic and organic insulating layers can be used.
[0027] The aforementioned inorganic insulating layer may use one or both of amorphous and crystalline materials as the inorganic insulating material. Examples of amorphous materials include metal phosphate salts and metal borate salts. The metal phosphate salts are not particularly limited, but condensed aluminum phosphate is preferred from the viewpoint of more easily ensuring interparticle insulation. Examples of crystalline materials include metal oxides and SiO2. Examples of metal oxides include MgO, forsterite, talc, and Al2O3. The aforementioned inorganic insulating layer is a layer containing the aforementioned inorganic insulating material, and is preferably formed from the aforementioned inorganic insulating material.
[0028] Examples of condensed aluminum phosphates include aluminum tripolyphosphate, aluminum metaphosphate, and mixtures thereof, all of which can be obtained by heating aluminum dihydrogen phosphate to induce a dehydration reaction. Among these, aluminum tripolyphosphate is preferred from the viewpoint of forming a highly adhesive insulating layer due to its high reactivity with iron. The aqueous state of aluminum tripolyphosphate is not limited; for example, it can be a dihydrate (AlH₂P₃O₄). 10 (·2H2O). It should be noted that in this specification, aluminum dihydrogen tripolyphosphate is sometimes referred to as aluminum tripolyphosphate.
[0029] The aforementioned organic insulating layer is a layer containing an organic resin, preferably formed from an organic resin. As the aforementioned organic resin, silicone resin is preferred. Silicone resin forms Si-O bonds with excellent heat resistance through heat treatment, thus maintaining excellent insulation properties even when the molded body undergoes strain-relief heat treatment at high temperatures (e.g., 600°C) during the fabrication of the powder core.
[0030] Examples of silicone resins include resin-based silicone resins, such as silicone resins with a T-unit (trifunctional siloxane unit) of 60 mol% or more. Among these, silicone resins with methyl groups of 50 mol% or more on the Si side are preferred. Examples include methylphenyl silicone resins (Shin-Etsu Chemical Industry Co., Ltd., KR-255, KR-311, KR-300, etc.), methyl silicone resins (Shin-Etsu Chemical Industry Co., Ltd., KR-251, KR-400, KR-220L, KR-220LP, KR-242A, KR-240, KR-500, KC-89, SILRES (registered trademark) MKPOWDER, etc., manufactured by Wacker Asahikasei Silicone Co., Ltd.). Additionally, SR2400 and Trefil R-910 manufactured by Toray Dow Corning Co., Ltd. can also be used. Furthermore, the aforementioned silicone resin is not particularly limited, and silicone resins in powder or flake form, or both, can be used. Preferably, the aforementioned silicone resin is a resin that softens upon heating.
[0031] From the viewpoint of further ensuring insulation, the content of the insulating layer is preferably set to 0.20 parts by mass or more, relative to the total 100 parts by mass of the aforementioned iron-based soft magnetic powder and the aforementioned insulating layer. On the other hand, if the coating amount is too large, there is a possibility that the magnetic flux density will decrease, thereby impairing the function of the iron core, and there is also a possibility that the density of the iron core will decrease. Therefore, the content of the insulating layer is preferably set to 2.00 parts by mass or less, more preferably 1.00 parts by mass or less, relative to the total 100 parts by mass of the aforementioned iron-based soft magnetic powder and the aforementioned insulating layer.
[0032] In a preferred embodiment of the present invention, the aforementioned insulating layer comprises, from the surface of the aforementioned particles toward the outside, a first coating layer comprising condensed aluminum phosphate and a second coating layer comprising silicone resin. That is, the powder on which the aforementioned insulating layer is formed preferably comprises, from the inside out, the aforementioned iron-based soft magnetic powder, the aforementioned first coating layer, and the aforementioned second coating layer. More preferably, the aforementioned insulating layer is formed from the aforementioned first coating layer and the aforementioned second coating layer.
[0033] The first coating layer is less likely to be damaged during the pressure molding of the mixed powder, thus ensuring interparticle insulation is more easily achieved by having the aforementioned first coating layer. The content of the first coating layer is preferably 0.10 parts by mass or more, more preferably 0.15 parts by mass or more, relative to a total of 100 parts by mass of the aforementioned iron-based soft magnetic powder and the aforementioned insulating layer. On the other hand, in order to further improve the specific resistivity of the manufactured pressed powder core, the content of the first coating layer is preferably 0.50 parts by mass or less, more preferably 0.30 parts by mass or less, relative to a total of 100 parts by mass of the aforementioned iron-based soft magnetic powder and the aforementioned insulating layer.
[0034] The content of condensed aluminum phosphate in the aforementioned first coating layer is not limited, and can be, for example, 50% by mass or more. However, the aforementioned content is preferably 99% by mass or more, and more preferably the aforementioned first coating layer is formed from condensed aluminum phosphate. The aforementioned first coating layer is preferably a coating layer using condensed aluminum phosphate.
[0035] By having a second coating layer, the flexibility of the insulating layer is improved, making it less prone to damage caused by particle deformation during press molding. To further improve the flexibility of the insulating layer, the content of the second coating layer is preferably 0.10 parts by mass or more, relative to 100 parts by mass of the aforementioned iron-based soft magnetic powder and the aforementioned insulating layer. On the other hand, to further improve the specific resistivity of the manufactured pressed powder core, the content of the second coating layer is preferably 1.50 parts by mass or less, more preferably 0.60 parts by mass or less, and even more preferably 0.30 parts by mass or less, relative to 100 parts by mass of the aforementioned iron-based soft magnetic powder and the aforementioned insulating layer.
[0036] The content of silicone resin in the aforementioned second coating layer is not limited, and can be, for example, 50% by mass or more. However, the aforementioned content is preferably 99% by mass or more, and the aforementioned second coating layer is more preferably formed from silicone resin. The aforementioned second coating layer is preferably a coating layer using silicone resin.
[0037] (Lubricant) To improve demolding properties during molding, the mixed powder of the present invention includes a lubricant. Hereinafter, the lubricant content (parts by mass) is expressed as 100 parts by mass, which is the total of the aforementioned iron-based soft magnetic powder and the aforementioned insulating layer. To more easily ensure lubricity, the aforementioned mixed powder preferably contains 0.10 parts by mass or more of the aforementioned lubricant, more preferably 0.15 parts by mass or more, and even more preferably 0.20 parts by mass or more. Furthermore, to further improve the powder density, the aforementioned mixed powder preferably contains 1.05 parts by mass or less of the aforementioned lubricant, more preferably 0.80 parts by mass or less. It should be noted that the insulating layer is formed in layers on the surface of the particles constituting the iron-based soft magnetic powder, while the lubricant typically exists in a free state.
[0038] Regarding the lubricant, S, as defined by the above formula (1), is preferably greater than 0 and less than 0.50. When S is less than 0.50, the content of low-density lubricant in the mixed powder is low, and therefore the theoretical density of the mixed powder is further increased. As a result, the compressibility of the mixed powder is further improved, and a similar powder density can be obtained when using a mold lubrication molding method. To further improve compressibility, S is more preferably less than 0.23. On the other hand, to further improve demolding properties, S is more preferably greater than 0.13.
[0039] The aforementioned lubricants include organic lubricants. As organic lubricants, one or more selected from the group consisting of fatty acid amides, metal soaps, fatty acids, liquid lubricants, and thermoplastic resins may be used. Examples of fatty acid amides include monoamides and diamides. It should be noted that a fatty acid amide with a total of one amide group and amide bond is called a monoamide, and a fatty acid amide with a total of two amide groups is called a diamide. Examples of monoamides include stearamide (SA) and erucamide. Examples of diamides include ethylene bis-stearamide (EBS). Examples of the aforementioned metal soaps include zinc stearate, manganese stearate, and lithium stearate. Examples of the aforementioned fatty acids include, for example, oleic acid and stearic acid. Examples of the aforementioned liquid lubricants include, for example, phosphate esters, polyol esters, mineral oils, and polyethylene glycol. Examples of the aforementioned thermoplastic resins include, for example, polyamides, polyethylene, and polyacetals.
[0040] To further improve mold release properties, the content of organic lubricant is preferably 0.07 parts by weight or more, more preferably 0.10 parts by weight or more. On the other hand, to further improve powder density, the content of organic lubricant is preferably 0.80 parts by weight or less, more preferably 0.50 parts by weight or less.
[0041] Furthermore, the aforementioned lubricant includes inorganic layered compounds. Inorganic layered compounds are those having a layered structure formed by stacking unit layers of atoms bonded by strong bonds such as covalent or ionic bonds using weak van der Waals forces. Compared to organic lubricants, inorganic layered compounds and other inorganic lubricants have higher densities, thus minimizing the decrease in powder density even when mixed. Moreover, their layered structure facilitates shearing under load, thereby reducing friction and improving mold release properties during molding. In particular, the reduction in kinetic friction is significant. Therefore, from the viewpoint of compressibility and mold release properties during molding, the aforementioned lubricant includes inorganic layered compounds.
[0042] The aforementioned layered structure can be, for example, a sandwich structure. A sandwich structure has a structure where easily sliding surfaces and non-slip surfaces are stacked. Therefore, if an inorganic layered compound with a sandwich structure is used, lower friction can be achieved, further improving mold release properties.
[0043] Examples of the aforementioned inorganic layered compounds include tungsten disulfide (WS2), molybdenum disulfide (MoS2), hexagonal boron nitride (BN), graphite, fluorinated graphite, and layered silicates. Examples of layered silicates include talc and mica. Two or more materials can be used as the inorganic layered compound. The aforementioned inorganic layered compound is preferably selected from at least one of the group consisting of tungsten disulfide, molybdenum disulfide, hexagonal boron nitride, talc, mica, and graphite. Furthermore, from the viewpoint of further reducing the coefficient of friction between the insulating layer and the mold and further improving the demolding performance during molding, the aforementioned inorganic layered compound is more preferably hexagonal boron nitride. Here, hexagonal boron nitride is particularly effective in reducing the coefficient of friction between the silicone resin and the mold. Therefore, from the viewpoint of further improving the demolding performance during molding, it is further preferred that the aforementioned inorganic layered compound is hexagonal boron nitride, and that the aforementioned insulating layer has a coating layer containing silicone resin.
[0044] To further improve the powder density, the density of the aforementioned inorganic layered compound is preferably 2.0 g / cm³. 3 That's all. Additionally, the density of the aforementioned inorganic layered compounds can be less than 4.0 g / cm³. 3 It can also be 4.0 g / cm³. 3 That's all. Here, when using two or more inorganic layered compounds, the average density is set to the density of the aforementioned inorganic layered compound. For example, the density ρ of 70 parts by mass in 100 parts by mass of the aforementioned inorganic layered compound is... A The density ρ of 30 parts by mass of inorganic layered compound A B In the case of inorganic layered compound B, the average density ρ is calculated as follows. AB The density of the aforementioned inorganic layered compound.
[0045] ρ AB =1 / {(0.7 / ρ)} A ) + (0.3 / ρ B ) It should be noted that, as a substance with a density of 4.0 g / cm³ 3 Examples of the above-mentioned inorganic layered compounds include molybdenum disulfide and tungsten disulfide. Additionally, a compound with a density of 2.0 g / cm³... 3 Above and below 4.0 g / cm³ 3Inorganic layered compounds, for example, include graphite, hexagonal boron nitride, talc, and mica. That is, the aforementioned inorganic layered compounds can be at least one selected from the group consisting of hexagonal boron nitride, talc, mica, and graphite.
[0046] The volume resistivity of the aforementioned inorganic layered compound is not particularly limited. However, the aforementioned inorganic layered compound preferably has high insulating properties. Unlike organic lubricants, inorganic lubricants do not decompose during heat treatment and therefore remain in the molded body after heat treatment. Therefore, there is a possibility that the insulating film may be impaired due to the different substances involved. On the other hand, if the aforementioned inorganic layered compound has insulating properties, it is expected to have an effect that assists the insulating film. Therefore, the volume resistivity of the aforementioned inorganic layered compound is preferably 1.0 × 10⁻⁶. 6 Ω·cm or more, more preferably 1.0×10 9 Above Ω·cm. It should be noted that there is no specific upper limit to the volume resistivity of the aforementioned inorganic layered compounds; for example, it can be 1.0 × 10⁻⁶ Ω·cm. 18 Below Ω·cm. Here, regarding the aforementioned volume resistivity, it is assumed that the resistance value of the inorganic layered compound under load is measured using a universal testing machine. Specifically, the measurement is performed using the method described in the examples.
[0047] To further improve the release properties during molding, the content of the inorganic layered compound is preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass or more. Furthermore, to further improve the release properties during molding, the density of the inorganic layered compound is 4.0 g / cm³. 3 In the above cases, the content is more preferably 0.15 parts by mass or more, and even more preferably 0.25 parts by mass or more. On the other hand, in order to further improve compressibility while ensuring mold release properties, the density of the inorganic layered compound is less than 4.0 g / cm³. 3 In the case of [specific content], the content is preferably 0.25 parts by weight or less, and more preferably 0.15 parts by weight or less.
[0048] The aforementioned lubricant can be formed from organic lubricants and inorganic layered compounds. However, in addition to organic lubricants and inorganic layered compounds, one or more other inorganic lubricants may be used as the aforementioned lubricant. Examples of inorganic lubricants other than inorganic layered compounds include zinc oxide (ZnO), bismuth oxide (Bi2O3), iron sulfide (FeS), and bismuth sulfide (Bi2S3). However, it is preferable that the mixture does not contain inorganic lubricants other than inorganic layered compounds. In other words, the inorganic lubricant contained in the aforementioned mixed powder is preferably formed from inorganic layered compounds.
[0049] [Method for manufacturing mixed powder] Next, a method for manufacturing the above-described mixed powder according to one embodiment of the present invention will be described. It should be noted that the following description represents only one example of the manufacturing method, and the present invention is not limited to the following description.
[0050] The aforementioned mixed powder can be manufactured by further mixing a lubricant after forming an insulating layer on the surface of the particles constituting the aforementioned iron-based soft magnetic powder.
[0051] Regarding the aforementioned insulating layer, there are no particular limitations; it can be formed using methods such as wet or dry methods. The wet method involves mixing the material used in the insulating layer with the aforementioned iron-based soft magnetic powder using a solvent such as water or an organic solvent. On the other hand, the dry method involves mixing the material used in the insulating layer with the aforementioned iron-based soft magnetic powder without using a solvent. Mixing can be performed using a mixer, such as a rotary blade type. The rotary blades can be, for example, stirring blades located at the bottom of the mixing container. Examples of rotary blade type mixers include the FM mixer series (manufactured by Nippon Coke & Engineering Co., Ltd.) and the high-speed mixer series (manufactured by EarthTechnica Co., Ltd.).
[0052] The following is a detailed description of the case where the aforementioned insulating layer has a first coating layer formed from condensed aluminum phosphate and a second coating layer formed from silicone resin in sequence from the surface of the aforementioned particles outward.
[0053] (First covering layer) First, a first coating layer formed from condensed aluminum phosphate is formed on the aforementioned iron-based soft magnetic powder. This first coating layer can be formed, for example, using a dry method. Specifically, it can be formed by mixing the iron-based soft magnetic powder with the condensed aluminum phosphate powder, preferably by heating. By using a dry method, the oxidation problem of the iron-based soft magnetic powder can be avoided, eliminating the need for solvent dissolution and solvent drying processes, thus providing advantages in terms of equipment and operability. Furthermore, heating and mixing achieves excellent adhesion between the first coating layer and the surface of the iron-based soft magnetic powder. This is presumably because a reaction occurs at the interface between the condensed aluminum phosphate film and the iron-based soft magnetic powder.
[0054] The average particle size of the aforementioned condensed aluminum phosphate powder is not limited. Setting the average particle size to 1 μm or more and 10 μm or less ensures sufficient flowability, improving operability. Furthermore, it allows for easy and uniform formation of the first coating layer into a continuous film. The average particle size can be 1 μm or more, preferably 1.5 μm or more. On the other hand, a smaller average particle size results in a larger specific surface area, thus increasing the coating efficiency. Therefore, the average particle size is preferably 10 μm or less, more preferably 7.5 μm or less, and even more preferably 5 μm or less. It should be noted that the aforementioned average particle size is the median particle size D based on volume, measured using laser diffraction. 50 .
[0055] In the aforementioned mixing process, the aforementioned mixer can be used. The rotational speed of the mixer is not particularly limited, but for efficient formation of the first coating layer and to produce a continuous film, a speed of 100 rpm or more is preferred, and more preferably 200 rpm or more. On the other hand, excessive high-speed stirring can cause plastic deformation of the iron-based soft magnetic powder, potentially leading to a decrease in compressibility and an increase in hysteresis loss during pressure molding. Therefore, the aforementioned rotational speed is preferably 1000 rpm or less, and more preferably 800 rpm or less.
[0056] In the aforementioned mixing process, the maximum temperature reached during mixing is not particularly limited. However, in order to facilitate the formation of the aforementioned first coating layer and improve the adhesion of the first coating layer, the aforementioned maximum temperature reached is preferably 130°C or higher, more preferably 150°C or higher. On the other hand, there is a possibility that the condensed aluminum phosphate may deteriorate and its crystallinity may decrease due to high temperatures. In addition, there is a possibility that the density of the pressed magnetic core may decrease due to the oxidation of the iron-based soft magnetic powder. Therefore, the aforementioned maximum temperature reached is preferably 200°C or lower. It should be noted that the temperature referred to here refers to the temperature of the powder during mixing. In the case of using a rotary blade mixer, it is the temperature displayed by a thermocouple protruding from the wall of the mixing tank to a degree that does not contact the rotating blades. The thermocouple can be embedded in the powder layer that is stationary in the mixing tank when the mixer is stationary. In addition, the maximum temperature reached during mixing refers to the highest temperature of the powder during mixing, which can be set as the highest temperature of the powder containing the iron-based soft magnetic powder and the condensed aluminum phosphate powder measured by the aforementioned thermocouple. The temperature during mixing can be controlled by heating or cooling. For example, a heating and cooling jacket can be installed in the mixing tank of the mixer to heat or cool the powder inside the mixing tank from outside the mixer, thereby controlling the temperature during mixing. For the heating, one or both of steam and warm water can be used; for the cooling, a refrigerant such as cold water can be used. Alternatively, the heat generated during mixing (heat of mixing) can also be used to control the temperature during mixing. From the perspective of suppressing the oxidation of iron-based soft magnetic powder, the aforementioned mixing is preferably carried out in a non-reactive gas atmosphere, for example, preferably in a nitrogen atmosphere.
[0057] After the aforementioned mixing, from the perspective of oxidation inhibition and subsequent operations, the powder having the first coating layer is preferably cooled to below 80°C. There is no particular limitation on the lower limit of the temperature of the cooled powder; for example, it can be set to above room temperature, above 0°C, or above 30°C.
[0058] (Second covering layer) Next, a second coating layer formed from silicone resin is formed on the powder obtained by the above method. The formation of the second coating layer can be carried out, for example, by a wet method using organic solvents or a dry method without solvents. The dry method is preferred because it is advantageous in terms of cost, equipment, and operability because there is no need to take safety measures associated with the use of organic solvents.
[0059] In the wet method, the silicone resin can be adhered by mixing a solution obtained by dissolving the silicone resin in an organic solvent with the powder obtained by the above method, followed by drying. Examples of the aforementioned organic solvent include petroleum-based organic solvents such as alcohols, xylene, and toluene. The concentration of the solid component of the silicone resin in the aforementioned solution can be set to 1-10% by mass. Drying can be carried out in the atmosphere. The drying temperature can be set to the evaporation temperature of the organic solvent used, and lower than the curing temperature of the silicone resin. The type and mixing ratio of the silicone resin being mixed are as described above. In the wet method, it is preferable to use at least one of the following silicone resins: SR2400 manufactured by Toray Dow Corning Co., Ltd., KR-311 manufactured by Shin-Etsu Chemical Industry Co., Ltd., and LR-220L.
[0060] In the dry method, the silicone resin powder is mixed with the powder having the first coating layer obtained by the above method, thereby enabling the silicone resin to adhere. The aforementioned mixer can be used in the mixing process. Alternatively, the mixing can be continued using the same mixer used in the mixing process for forming the first coating layer. The mixing speed is not particularly limited, but for efficient formation of the second coating layer, 100 rpm or more is preferred, and more preferably 200 rpm or more. On the other hand, excessive high-speed stirring can cause plastic deformation of the iron-based soft magnetic powder, potentially leading to a decrease in compressibility and an increase in hysteresis loss during press molding. Therefore, the aforementioned speed is preferably 2000 rpm or less, and more preferably 1500 rpm or less. The mixing temperature is not particularly limited, but to soften the silicone resin and further improve the adhesion of the second coating layer, it is preferably set to 80°C or more. To increase the mixing temperature and utilize the heat storage of the powder layer to suppress manufacturing costs, the mixing with the silicone resin is preferably performed during cooling after the formation of the first coating layer. The type and mixing ratio of the silicone resin being mixed are as described above. In the case of the dry process, the silicone resin preferably used is at least one of the following: SILRES (registered trademark) MKPOWDER manufactured by WackerAsahikasei Silicone Co., Ltd., Trefil R-910 manufactured by Toray Dow Corning Co., Ltd., and KR-220LP manufactured by Shin-Etsu Chemical Industry Co., Ltd.
[0061] After the silicone resin is adhered using a wet or dry method, heat treatment can be performed to increase the hardness of the adhered silicone resin. The heat treatment temperature can be set, for example, between 150°C and 250°C. The heat treatment can be performed in the atmosphere or in a non-reactive gas atmosphere (such as a nitrogen atmosphere).
[0062] After forming the insulating layer as described above, a lubricant is further mixed. For example, a lubricant can be added to the iron-based soft magnetic powder on which the insulating layer has been formed using the above method, and then mixed. The mixer described above can be used for mixing. Alternatively, a mixer for forming the insulating layer can be used to continue the process without removing the powder. The type and amount of lubricant added are as described above.
[0063] [Powder-pressed magnetic core] Next, a method for manufacturing pressed powder magnetic cores using the mixed powder of the present invention will be described. It should be noted that the following description represents one example of the manufacturing method, and the present invention is not limited to the following description.
[0064] (Pressure molding) The aforementioned mixed powder is loaded into a mold and pressurized to achieve the desired size and shape. Furthermore, the pressurization method is not particularly limited; conventional molding methods such as room temperature molding and mold lubrication molding are applicable. Mold lubrication molding improves demolding properties by applying a lubricant to the mold wall and then pressing. Suitable lubricants for the mold wall include metal soaps such as lithium stearate, zinc stearate, and calcium stearate, as well as waxes such as fatty acid amides. It should be noted that while the molding pressure is appropriately determined according to the application, increasing the molding pressure increases the density of the resulting pressed powder core; therefore, 10 t / cm² is preferred. 2 The above is preferred, with 15t / cm being even better. 2 above.
[0065] (Strain-reducing heat treatment) Following the aforementioned pressure molding, a strain-reducing heat treatment is performed to reduce hysteresis loss and improve the strength of the molded body. The heat treatment temperature is not particularly limited. Furthermore, the holding time during heat treatment is not particularly limited, but is preferably set to 5–120 minutes. Additionally, a stage can be included in the heating or cooling process during heat treatment to maintain a constant temperature. The heat treatment atmosphere is not limited; for example, it can be in the atmosphere, an inactive atmosphere, a reducing atmosphere, or a vacuum. The dew point of the aforementioned atmosphere is not particularly limited and can be appropriately determined according to the application.
[0066] Example The present invention will now be described in detail based on specific embodiments.
[0067] (Experiment 1) As an iron-based soft magnetic powder, an apparent density of 3.0 Mg / m³ was used. 3The first step involved heating and mixing the aforementioned iron-based soft magnetic powder and aluminum dihydrogen phosphate dihydrate powder (Tayca Co., Ltd. K-FRESH #100P, average particle size approximately 5 μm) to form a coating layer from aluminum tripolyphosphate. 1.5 kg of the iron-based soft magnetic powder was used, and 0.2 parts by weight of the aluminum dihydrogen phosphate dihydrate powder were mixed relative to 100 parts by weight of the iron-based soft magnetic powder. The mixing was performed using a high-speed mixer (EarthTechnica Co., Ltd. (formerly Fukae Powtech) LFS-GS-2J type). The mixture was heated and mixed for 20 minutes under a nitrogen atmosphere and a rotating blade speed of 500 rpm. The maximum temperature reached by the powder during mixing was controlled at 170°C.
[0068] Next, silicone resin powder (Shin-Etsu Chemical Industry Co., Ltd. KR-220LP) was further added to and mixed with the powder in the mixing tank, thereby forming a silicone resin coating layer on the outside of the aforementioned aluminum tripolyphosphate coating layer. After the aforementioned heating and mixing, the addition was performed at a point when the powder temperature dropped to 150°C while maintaining the rotation speed of the rotating blade at 500 rpm. The addition amount was set to 0.2 parts by mass relative to 100 parts by mass of the aforementioned iron-based soft magnetic powder. Stirring continued until the powder temperature dropped to 60°C.
[0069] Next, organic and inorganic lubricants of the types and amounts shown in Table 1 were added to the powder in the mixing tank. The mixture was stirred for 5 minutes at a speed of 500 rpm, and then the powder was removed from the mixing tank. Here, the amounts added in Table 1 represent the parts by mass when the total mass of the iron-based soft magnetic powder and the insulating layer is set to 100 parts by mass. The densities of the various lubricants used are shown in Table 2.
[0070] Using the mixed powder obtained from the above steps, a pressed powder body was prepared. The density of the pressed powder body (pressed powder density) and the demolding energy when the pressed powder body was demolded from the mold were measured. For the aforementioned pressed powder body, 75g of the aforementioned mixed powder was filled into a mold with a diameter of 25mm, and pressure molding was performed at 80°C to produce a cylindrical pressed powder body. The pressure during the aforementioned pressure molding was set to 980MPa. The pressed powder density was calculated based on the dimensions and mass of the obtained pressed powder body. Furthermore, the demolding energy was calculated based on the integral value of the demolding load and the travel distance when the pressed powder body was demolded.
[0071] The evaluation results are shown in Table 1. The powder that meets the requirements of the present invention has high compaction density and low demolding energy. On the other hand, the mixed powders of Comparative Examples 1 to 7 do not contain inorganic layered compounds, and therefore have low compaction density or high demolding energy. It should be noted that in the above steps, no lubricant was added, and a powder formed from iron-based soft magnetic powder and an insulating layer was obtained. The powder was then formed using a mold lubrication molding method (lubricant: lithium stearate) to produce a compacted powder body, and the resulting compaction density was 7.60 g / cm³. 3 .
[0072] [Table 1] [Table 2] (Experiment 2) Using a mold lubrication molding method under a molding pressure of 980 MPa, the powders of Comparative Example 2 and Invention Examples 1-6 from Test 1 were molded to produce ring-shaped test pieces with an outer diameter of 38 mm, an inner diameter of 25 mm, and a height of 6 mm. The test pieces were then heat-treated in nitrogen at 600°C for 45 minutes. The specific resistivity and magnetic flux density of the resulting iron cores were measured using a four-terminal method. The results are shown in Table 3. Furthermore, the volume resistivity of each inorganic layered compound was measured according to the method for measuring electrical conductivity described in JIS K 1469, and the results are shown in Table 4. It should be noted that the volume resistivity was evaluated under a pressure of 250 N. All test pieces exhibited a specific resistivity of 100 μΩm or more, demonstrating sufficient insulation. Additionally, for the iron cores using a 1.0 × 10⁻⁶... 6 For the test pieces made from the powder of the inorganic layered compound with a volume resistivity of Ω·cm or higher in Examples 3 to 5 of the Invention, the resistivity is 1000 μΩm or higher, and the insulation properties are superior.
[0073] [Table 3] [Table 4]
Claims
1. A mixed powder comprising: Iron-based soft magnetic powder; An insulating layer formed on the surface of the particles constituting the iron-based soft magnetic powder; and Lubricant in, The lubricant comprises organic lubricants and inorganic layered compounds.
2. The mixed powder as described in claim 1, wherein, S, as defined by the following equation (1), is greater than 0 and less than 0.
50. [Mathematical Expression 1] Where n is the number of lubricants, a i The content of each of the lubricants is expressed in parts by mass relative to a total of 100 parts by mass of the iron-based soft magnetic powder and the insulating layer, ρ i It is based on g / cm 3 The density of each of the lubricants is indicated.
3. The mixed powder as described in claim 1 or 2, wherein, The insulating layer has a first coating layer comprising condensed aluminum phosphate and a second coating layer comprising silicone resin, which are sequentially arranged from the surface of the particle outwards.
4. The mixed powder according to any one of claims 1 to 3, wherein, The inorganic layered compound is selected from at least one of the group consisting of tungsten disulfide, molybdenum disulfide, hexagonal boron nitride, talc, mica, and graphite.
5. The mixed powder as described in claim 4, wherein, The inorganic layered compound is hexagonal boron nitride.
6. The mixed powder according to any one of claims 1 to 4, wherein, The volume resistivity of the inorganic layered compound is 1.0 × 10⁻⁶. 6 Ω·cm or higher.
Citation Information
Patent Citations
Ferromagnetic powder composition and method for producing the same
JP2013505563A