Plated steel wire, rope, and rope manufacturing method
By using bridge steel wires with specific chemical composition and microstructure, combined with Zn-based coatings and hot stretching treatment, the problems of hydrogen embrittlement and corrosion of bridge steel wires in hydrogen-intrusion environments have been solved, achieving high strength, resistance to hydrogen intrusion, and torsional properties.
Patent Information
- Application Number
- CN202580027843.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-18
- Filing Date
- 2025-04-18
- Publication Date
- 2026-11-17
AI Technical Summary
Bridge steel wires are prone to hydrogen embrittlement and corrosion in hydrogen-infiltrated environments, leading to delayed fracture. Furthermore, the increase in strength reduces the delayed fracture characteristics, and the corrosion progression during plating peeling leads to a decrease in corrosion resistance.
It is composed of steel wire with specific chemical composition, including C, Si, Mn, Cu, etc., forming a mixed structure of ferrite and cementite phases, and covered with a Zn-based coating on the surface. Through a combination of hot stretching and plating treatment, hydrogen intrusion is suppressed and torsional characteristics are improved.
This study achieves hydrogen intrusion resistance and torsion characteristics of high-strength steel wire in a hydrogen-intrusion environment, reduces the possibility of delayed fracture, and improves the corrosion resistance of coated steel wire.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This disclosure relates to plated steel wire, rope, and a method for manufacturing the rope. Background Technology
[0002] Steel wires used for bridge cables and ropes are typically made by drawing high-carbon steel wire after lead quenching to create a pearlitic structure.
[0003] In recent years, high-strength steel wire has been required to reduce construction costs and make structures lighter.
[0004] However, if high-strength steel wire is used in hydrogen-infiltrated or corrosive environments, the likelihood of breakage due to hydrogen embrittlement or corrosion increases. Therefore, excellent resistance to hydrogen embrittlement and corrosion is desired for high-strength steel wire.
[0005] High-strength plated steel bars and plated steel wires with high strength and excellent resistance to hydrogen embrittlement have been proposed (for example, see Patent Documents 1 and 2).
[0006] Patent Document 1: Japanese Patent Application Publication No. 2003-328077
[0007] Patent Document 2: Japanese Patent Application Publication No. 2021-183709 Summary of the Invention
[0008] The technical problem that the invention aims to solve
[0009] Steel wires used in bridges are coated to ensure corrosion resistance, but corrosion progresses as the coating peels off over long-term use.
[0010] Recently, progress has been made in increasing the strength of steel wires used in bridges, which increases the possibility of delayed fracture during plating peeling.
[0011] It is believed that drawing steel wire introduces a large number of dislocations during the drawing process, thus increasing the amount of hydrogen intrusion. High levels of hydrogen intrusion may lead to delayed fracture, therefore it is necessary to suppress hydrogen intrusion.
[0012] Furthermore, increasing strength reduces the delayed fracture characteristics. In particular, the likelihood of delayed fracture increases when the tensile strength is above 1900 MPa. Regarding delayed fracture, suppressing hydrogen intrusion is one solution.
[0013] In addition, for galvanized steel wires such as those used in bridges, torsional properties are required as a ductility requirement.
[0014] In view of the above, the purpose of this disclosure is to provide a plated steel wire, rope, and a method for manufacturing the rope that has high strength and excellent torsional properties and resistance to hydrogen intrusion.
[0015] Technical solutions for solving technical problems
[0016] The means used to solve the above problems include the following methods.
[0017] <1> A galvanized steel wire has the following steel composition: the steel portion contains, by mass%, C: 0.80~1.10%, Si: 0.10~1.50%, Mn: 0.10~1.00%, P: less than 0.050%, S: less than 0.050%, N: less than 0.0120%, O: less than 0.0100%, Al: 0.005~0.070%, Cu: 0.04~0.80%, Mo: 0~0.20%, Cr: 0~1.00%, V: 0~0.15%, Sn: 0~0.50%, Ni: 0~0.80%, Ti: 0~0.050%, Nb: 0~0.050%, B: 0~0. The steel portion comprises 0.040%, REM: 0~0.030%, Bi: 0~0.020%, Mg: 0~0.0040%, Ca: 0~0.0040%, Zr: 0.030%, W: 0~0.10%, Te: 0~0.030%, Sb: 0~0.030%, and the remainder is Fe and impurities. In the central portion of a section parallel to the length direction and passing through the central axis, within 1.0 mm of the central axis, the area fraction of a mixed microstructure consisting of ferrite and cementite phases is 95.0% or more. The diameter of the steel portion is 5.0 mm or more, and the surface of the steel portion is covered with a Zn-based coating with Zn as the main component at a depth of 100 g / m². 2 The above conditions apply: the tensile strength TS is 1900 MPa or more and 2250 MPa or less, and the yield strength YS, i.e., the ratio of 0.2% endurance to the tensile strength TS, is 0.87 or more.
[0018] <2> according to <1> The plated steel wire, wherein the steel portion contains, by mass percentage, one or more elements selected from groups A to C below.
[0019] (Group A)
[0020] Select one or more from the group consisting of Mo: less than 0.20%, Cr: less than 1.00%, and V: less than 0.15%.
[0021] (Group B)
[0022] Choose one or both of the following groups: Sn: less than 0.50% and Ni: less than 0.80%.
[0023] (Group C)
[0024] Select one or more from the group consisting of Ti: less than 0.050%, Nb: less than 0.050%, B: less than 0.0040%, REM: less than 0.030%, Bi: less than 0.020%, Mg: less than 0.0040%, Ca: less than 0.0040%, Zr: less than 0.030%, W: less than 0.10%, Te: less than 0.030%, and Sb: less than 0.030%.
[0025] <3> according to <2> The plated steel wire, wherein the steel composition includes group A.
[0026] <4> according to <2> or <3> The plated steel wire, wherein the steel composition includes group B.
[0027] <5> according to <2> ~ <4> The plated steel wire according to any one of the following methods, wherein the steel composition comprises the C group.
[0028] <6> A rope in which multiple strands are bound together. <1> ~ <5> The plated steel wire as described in any one of the above.
[0029] <7> A method for manufacturing a rope, comprising: bonding multiple ropes... <1> ~ <5> The process of binding galvanized steel wire into rope as described in any one of the above.
[0030] Invention Effects
[0031] According to this disclosure, there are high-strength coated steel wires, ropes, and methods for manufacturing ropes that also possess excellent torsional properties and resistance to hydrogen intrusion. Attached Figure Description
[0032] Figure 1A This is an example of a SEM image of a longitudinal section of a steel wire containing a mixed microstructure of ferrite and cementite phases as well as an unmixed microstructure.
[0033] Figure 1B It is Figure 1A An enlarged image of the portion containing non-mixed tissue.
[0034] Figure 2A This is another example of a SEM image of a longitudinal section of a steel wire containing a mixed microstructure of ferrite and cementite phases as well as an unmixed microstructure.
[0035] Figure 2B It is Figure 2A An enlarged image of the portion containing non-mixed tissue. Detailed Implementation
[0036] An example implementation of this disclosure will be described.
[0037] It should be noted that, in this disclosure, the numerical range represented by "~" refers to the range of values recorded before and after "~" that are included as lower and upper limits. Where the values before and after "~" are marked "exceeding" or "less than", the numerical range refers to the range of values not included as lower or upper limits.
[0038] The amount of elements in a chemical composition is sometimes indicated by labeling the element symbol with "amount" (e.g., C amount, Si amount, etc.).
[0039] Regarding the content of elements in a chemical composition, "%" refers to "mass %".
[0040] When the content of an element in a chemical composition is recorded as "0~", it means that the element may not be included.
[0041] The term "process" is not only used to refer to an independent process, but also to any process that can achieve its intended purpose, even if it cannot be clearly distinguished from other processes.
[0042] The "surface" of a steel wire refers to its "outer circumference".
[0043] The "central axis" of a steel wire refers to an imaginary line that passes through the center point of a cross-section perpendicular to the length of the wire and extends along the length direction (axial direction).
[0044] The inventors conducted repeated experiments and research, and obtained the following insights.
[0045] (a) The coated steel wire has many dislocations, resulting in a large amount of hydrogen intrusion. In the case of coating peeling, a large amount of hydrogen intrusion into the steel wire (steel base) may lead to delayed fracture.
[0046] (b) Adding Cu is effective in suppressing the amount of hydrogen intrusion.
[0047] (c) When plating is performed after wire drawing, carbon is fixed to the dislocation core when heated to around 450°C for several tens of seconds, which prevents hydrogen from fixing around the dislocation and reduces the amount of diffusible hydrogen that delays fracture. However, large amounts of diffusible hydrogen still penetrate when the plating is peeled off.
[0048] (d) Furthermore, heating to above 450°C is effective in reducing the amount of diffusible hydrogen, but the plating will dissolve again at temperatures above 450°C, so it cannot be applied.
[0049] (e) Therefore, by simultaneously aging and constant load (thermal stretching) after plating, carbon can be effectively fixed to the dislocation core, and the amount of diffusible hydrogen is further reduced (as a material property, improving durability by 0.2%).
[0050] (f) By combining the addition of Cu with hot stretching after plating, hydrogen intrusion can be effectively suppressed even in the case of plating peeling, and plating wire with reduced possibility of delayed fracture can be obtained.
[0051] (g) It should be noted that without plating, the recovery and recrystallization of a large number of dislocations introduced into the layered ferrite cannot be carried out during the wire drawing process, thus reducing the torsional characteristics and failing to take into account the delayed fracture characteristics.
[0052] (h) When multiple galvanized steel wires are bundled together to manufacture ropes for bridge applications, if the diameter of the galvanized steel wires is too small, the rigidity of the structure becomes insufficient. Therefore, the diameter (wire diameter) of the steel wires before galvanizing for ropes used in bridges, etc., generally needs to be 5.0 mm or more. On the other hand, if the diameter of the steel wire is increased by reducing the reduction of area during wire drawing, the tensile strength is insufficient. Therefore, the diameter of the high-strength steel wire used for manufacturing galvanized steel wires for bridge applications, etc., is preferably 7.5 mm or less.
[0053] The galvanized steel wire, rope, and rope manufacturing method disclosed herein are based on these insights.
[0054] [Glazed Steel Wire]
[0055] The plated steel wire of the present invention has the following steel composition, by mass%, containing C: 0.80~1.10%, Si: 0.10~1.50%, Mn: 0.10~1.00%, P: less than 0.050%, S: less than 0.050%, N: less than 0.0120%, O: less than 0.0100%, Al: 0.005~0.070%, and Cu: 0.04~0.80%, with the remainder being Fe and impurities, or Fe, any element and impurities.
[0056] Furthermore, in the steel portion of the plated steel wire of the present invention, in the central part of the cross section parallel to the length direction and within 1.0 mm from the central axis, the area fraction of the mixed structure composed of ferrite phase and cementite phase (sometimes referred to in this disclosure as "mixed structure of ferrite phase and cementite phase" or simply "mixed structure") is 95.0% or more.
[0057] Furthermore, in the plated steel wire disclosed herein, the diameter of the steel portion (i.e., the wire portion) is 5.0 mm or more, and the surface is covered with a Zn-based coating with Zn as the main component, at a density of 100 g / m. 2 above.
[0058] Furthermore, the tensile strength of the plated steel wire of the present invention is 1900 MPa or more and 2250 MPa or less, and the ratio of yield strength (0.2% endurance) YS to tensile strength TS, YS / TS, is 0.87 or more.
[0059] (Steel composition)
[0060] The steel composition refers to the chemical composition of the portion of the steel wire covered by the Zn-based coating in the plated steel wire of the present invention. The contents of each component of the steel composition will be explained below.
[0061] C: 0.80~1.10%
[0062] C is a component required to improve the tensile strength of steel wire.
[0063] If the C content is less than 0.80%, the tensile strength is insufficient.
[0064] On the other hand, if the carbon content in the steel wire is too high, the wire will harden, reducing its delayed fracture characteristics. If the carbon content exceeds 1.10%, it will be difficult to suppress the formation of proeutectoid cementite, reducing its torsional properties. Therefore, the carbon content should be between 0.80% and 1.10%.
[0065] From the viewpoint of tensile strength, a carbon content of 0.85% or more is preferred, and particularly 0.90% or more exhibits better properties. On the other hand, from the viewpoint of also considering torsional properties, a carbon content of 1.05% or less is preferred, and particularly 1.00% or less exhibits better properties.
[0066] Si: 0.10~1.50%
[0067] Si is an effective component for improving the tensile strength of steel wire.
[0068] When the Si content of the steel wire is less than 0.10%, the full effect brought by the presence of Si cannot be obtained.
[0069] On the other hand, if the Si content of the steel wire exceeds 1.50%, it is difficult to suppress the formation of martensite as a hard layer, and the wire drawing processability is reduced.
[0070] Therefore, the Si content is 0.10~1.50%, preferably 0.50~1.40%, and more preferably 0.70~1.30%.
[0071] Mn: 0.10~1.00%
[0072] Mn is an effective component for improving the tensile strength of steel wire. Additionally, Mn has the function of fixing sulfur (S) in steel into the form of MnS, thereby suppressing hot brittleness.
[0073] When the Mn content in the steel wire is less than 0.10%, the full benefits of having Mn cannot be obtained.
[0074] On the other hand, if the steel wire contains more than 1.00% Mn, it is difficult to suppress the formation of martensite as a hard layer, and the wire drawing processability is reduced.
[0075] Therefore, the Mn content is 0.10~1.00%, preferably 0.25~0.80%.
[0076] P: below 0.050%
[0077] P is an element that reduces the delayed fracture characteristics of steel wire due to grain boundary segregation.
[0078] If the phosphorus content of the steel wire is below 0.050%, the reduction in delayed fracture characteristics is suppressed, and other requirements are also met, thus obtaining the target delayed fracture characteristics.
[0079] The upper limit of P content is preferably 0.030%, more preferably 0.020% or less. It should be noted that there is no limit to the lower limit of P content, which can be 0% (i.e., none), or, from the perspective of reducing the cost of P removal, it can be more than 0% or more than 0.001%.
[0080] S: Below 0.050%
[0081] S is an element that reduces delayed fracture characteristics.
[0082] If the sulfur content of the steel wire is below 0.050%, then by also satisfying other requirements, the target delayed fracture characteristics can be obtained.
[0083] The preferred upper limit for sulfur content is 0.030%. It should be noted that there is no lower limit for sulfur content; from the perspective of reducing the cost of sulfur removal, it can exceed 0% or be above 0.001%.
[0084] N: below 0.0120%
[0085] N is an element that reduces torsional properties.
[0086] If the N content of the steel wire is below 0.0120%, then by also satisfying other requirements, the target delayed fracture characteristics can be obtained.
[0087] The preferred upper limit for nitrogen content is 0.0100%, and the more preferred upper limit is 0.0070%. It should be noted that there is no lower limit for nitrogen content; from the perspective of reducing refining costs, it can exceed 0% or be above 0.0001%.
[0088] O: Below 0.0100%
[0089] O is an element that easily forms oxide inclusions in steel wire.
[0090] If the oxygen content of the steel wire is below 0.0100%, it can suppress the coarsening of oxide inclusions and the reduction of torsional properties and delayed fracture properties.
[0091] The preferred upper limit for O content is 0.0070%, and the more preferred upper limit is 0.0050%. It should be noted that there is no lower limit for O content; from the perspective of reducing refining costs, it can exceed 0% or be above 0.0001%.
[0092] Al: 0.005~0.070%
[0093] Al is an element with deoxidizing properties, which is necessary to reduce the oxygen content in steel wire.
[0094] When the Al content of steel wire is less than 0.005%, it is difficult to obtain the effects brought about by the presence of Al.
[0095] On the other hand, Al is an element that easily forms hard oxide inclusions. If the Al content of the steel wire is higher than 0.070%, large oxide inclusions are easily formed, and the reduction in wire drawing processability becomes significant.
[0096] Therefore, the Al content is 0.005~0.070%, preferably 0.010~0.050%, and more preferably 0.020~0.040%.
[0097] Cu: 0.04~0.80%
[0098] Cu has the effect of inhibiting hydrogen intrusion, which is necessary to improve delayed fracture characteristics. When the Cu content of steel wire is less than 0.04%, the effect of Cu content cannot be fully obtained.
[0099] On the other hand, if the steel wire contains more than 0.80% Cu, it is difficult to suppress the formation of martensite as a hard layer, and the wire drawing processability is reduced.
[0100] Therefore, the Cu content is 0.04~0.80%, preferably 0.10~0.60%.
[0101] The plated steel wire of the present invention may also contain elements other than those described above (any elements) within a range that does not impair the delayed fracture characteristics. Hereinafter, the arbitrary elements that may be included in the steel portion (steel wire) of the plated steel wire of the present invention will be described. From the viewpoint of effect, the arbitrary elements that may be included in the steel portion of the plated steel wire of the present invention are divided into groups A to C as follows.
[0102] (Group A)
[0103] Select one or more from the group consisting of Mo: less than 0.20%, Cr: less than 1.00%, and V: less than 0.15%.
[0104] (Group B)
[0105] Choose one or both of the following groups: Sn: less than 0.50% and Ni: less than 0.80%.
[0106] (Group C)
[0107] Select one or more from the group consisting of Ti: less than 0.050%, Nb: less than 0.050%, B: less than 0.0040%, REM: less than 0.030%, Bi: less than 0.020%, Mg: less than 0.0040%, Ca: less than 0.0040%, Zr: less than 0.030%, W: less than 0.10%, Te: less than 0.030%, and Sb: less than 0.030%.
[0108] The following is an explanation of each arbitrary element.
[0109] Mo: 0~0.20%
[0110] The presence of Mo is arbitrary.
[0111] Mo has the effect of increasing the tensile strength of steel wire. To obtain this effect stably, a Mo content of 0.01% or more is preferred.
[0112] On the other hand, even if the Mo content of the steel wire exceeds 0.20%, its effect is saturated.
[0113] Therefore, when Mo is actively present in the steel wire, the Mo content is preferably in the range of 0.01 to 0.20%. More preferably, it is 0.02 to 0.10%.
[0114] Cr: 0~1.00%
[0115] The presence of Cr is arbitrary.
[0116] Cr has the effect of increasing the tensile strength of steel wire. To obtain this effect stably, it is preferable to set the Cr content to 0.03% or more.
[0117] If the Cr content exceeds 1.00%, it is difficult to suppress the formation of martensite as a hard layer, and the wire drawing processability is reduced.
[0118] Therefore, when Cr is actively contained in the steel wire, the Cr content is preferably in the range of 0.03% to 1.00%. Furthermore, the Cr content can preferably be 0.85% or less. More preferably, it is 0.10% to 0.70%.
[0119] V: 0~0.15%
[0120] The presence of V is arbitrary.
[0121] V has the effect of increasing the tensile strength of steel wire. To consistently achieve this effect, it is preferable to have a V content of 0.01% or more in the steel wire.
[0122] On the other hand, if the V content of the steel wire exceeds 0.15%, the wire drawing processability will decrease.
[0123] Therefore, the V content of the steel wire actively containing V is preferably 0.02 to 0.15%. More preferably, the V content is 0.03 to 0.13%, and even more preferably, it is 0.05 to 0.12%.
[0124] Sn: 0~0.50%
[0125] The presence of Sn is arbitrary.
[0126] Sn has the effect of improving the corrosion resistance of steel wire. To obtain this effect stably, the Sn content is preferably set to 0.005% or more.
[0127] On the other hand, even if the Sn content of the steel wire exceeds 0.50%, its effect is saturated.
[0128] Therefore, when the steel wire actively contains Sn, the Sn content is preferably in the range of 0.001 to 0.50%. More preferably, it is 0.005 to 0.40%.
[0129] Ni: 0~0.80%
[0130] The presence of Ni is arbitrary.
[0131] Ni improves the corrosion resistance of steel wire. To consistently achieve this effect, a Ni content of 0.01% or higher is preferred.
[0132] On the other hand, even if the Ni content of the steel wire exceeds 0.80%, its effect is saturated.
[0133] Therefore, when Ni is actively contained in the steel wire, the Ni content is preferably in the range of 0.01 to 0.80%. More preferably, it is 0.05 to 0.60%.
[0134] Ti: 0~0.050%
[0135] The presence of Ti is arbitrary.
[0136] Ti forms carbides or carbonitrides in steel wire, which improves the delayed fracture characteristics. To achieve this effect, it is preferable that the Ti content of the steel wire is 0.002% or more.
[0137] On the other hand, if the Ti content of the steel wire is higher than 0.050%, it is easy to form coarse carbides or carbonitrides, which reduces the wire drawing processability.
[0138] Therefore, when the steel wire actively contains Ti, the Ti content is preferably 0.002 to 0.050%. More preferably, it is 0.005 to 0.030%. The Ti content can be 0.025% or less.
[0139] Nb: 0~0.050%
[0140] The presence of Nb is arbitrary.
[0141] Nitrogen (Nb) forms carbides or carbonitrides in steel wire, which improves its delayed fracture characteristics. To achieve this effect, it is preferable that the Nb content of the steel wire is 0.002% or more.
[0142] On the other hand, if the Nb content of the steel wire is higher than 0.050%, it is easy to form coarse carbides or carbonitrides, which reduces the wire drawing processability.
[0143] Therefore, when the steel wire actively contains Nb, the Nb content is preferably 0.002 to 0.050%. More preferably, it is 0.005 to 0.030%. The Nb content can be 0.025% or less.
[0144] B: 0~0.0040%
[0145] The presence of B is arbitrary.
[0146] Boron (B) has the effect of inhibiting the formation of ferrite structure and improving delayed fracture characteristics. To achieve this effect, it is preferable that the B content of the steel wire is 0.0003% or more.
[0147] On the other hand, if the boron content of the steel wire exceeds 0.0040%, coarse carbides are easily formed, reducing the wire drawing processability.
[0148] Therefore, when the steel wire actively contains B, the B content is preferably 0.0003 to 0.0040%. More preferably, it is 0.0006 to 0.0030%.
[0149] REM: 0~0.030%
[0150] The inclusion of REM is arbitrary.
[0151] If REM is present, the high delayed fracture characteristics can be more stably maintained. To achieve this effect, it is preferable that the REM content of the steel wire is 0.002% or more.
[0152] On the other hand, if the REM content of the steel wire exceeds 0.030%, its effect will be saturated.
[0153] Therefore, when REM is actively present, the REM content of the steel wire is preferably 0.002~0.030%. The REM content can be less than 0.020%.
[0154] Furthermore, REM refers to a total of 17 elements, including Sc, Y, and the lanthanides. REM content refers to the content of a single REM element, and the total content of two or more REM elements.
[0155] Bi: 0~0.020%
[0156] The presence of Bi is arbitrary.
[0157] If Bi is present, the high delayed fracture characteristics can be more stably maintained. To achieve this effect, it is preferable that the Bi content of the steel wire is 0.001% or more.
[0158] On the other hand, if the Bi content of the steel wire exceeds 0.020%, its effect will be saturated.
[0159] Therefore, when the steel wire actively contains Bi, the Bi content is preferably 0.001 to 0.020%. The Bi content can be less than 0.015%.
[0160] Mg: 0~0.0040%
[0161] The presence of Mg is arbitrary.
[0162] If Mg is present, the high delayed fracture characteristics can be more stably maintained. To achieve this effect, it is preferable that the Mg content of the steel wire is 0.0002% or higher.
[0163] On the other hand, if the Mg content of the steel wire exceeds 0.0040%, its effect will be saturated.
[0164] Therefore, when steel wire actively contains Mg, the Mg content is preferably 0.0002~0.0040%. The Mg content can be less than 0.0030%.
[0165] Ca: 0~0.0040%
[0166] The presence of Ca is arbitrary.
[0167] If it contains Ca, it can more stably exhibit high delayed fracture characteristics. To achieve this effect, it is preferable to have a Ca content of 0.0002% or more in the steel wire.
[0168] On the other hand, if the Ca content of the steel wire exceeds 0.0040%, its effect will be saturated.
[0169] Therefore, when the steel wire actively contains Ca, the Ca content is preferably 0.0002~0.0040%. The Ca content can be less than 0.0030%.
[0170] Zr: 0~0.030%
[0171] The presence of Zr is arbitrary.
[0172] If Zr is present, the high delayed fracture characteristics can be more stably maintained. To achieve this effect, it is preferable to have a Zr content of 0.002% or more in the steel wire.
[0173] On the other hand, if the Zr content of the steel wire is higher than 0.030%, it is easy to form coarse carbides or carbonitrides, which reduces the wire drawing processability.
[0174] Therefore, when steel wire actively contains Zr, the Zr content is preferably 0.002~0.030%. The Zr content can be less than 0.025%.
[0175] W: 0~0.10%
[0176] The presence of W is arbitrary.
[0177] If it contains W, it can more stably exhibit high delayed fracture characteristics. To achieve this effect, it is preferable to make the W content of the steel wire 0.02% or more.
[0178] On the other hand, if the W content of the steel wire exceeds 0.10%, its effect will be saturated.
[0179] Therefore, when steel wire actively contains W, the W content is preferably 0.02~0.10%. The W content can be less than 0.08%.
[0180] Te: 0~0.030%,
[0181] The presence of Te is arbitrary.
[0182] If it contains Te, it can more stably exhibit high delayed fracture characteristics. To achieve this effect, it is preferable to have a Te content of 0.001% or more in the steel wire.
[0183] On the other hand, if the Te content of the steel wire exceeds 0.030%, its effect will be saturated.
[0184] Therefore, when the steel wire actively contains Te, the Te content is preferably 0.001 to 0.030%. The Te content can be less than 0.020%.
[0185] Sb: 0~0.030%
[0186] The presence of Sb is arbitrary.
[0187] If Sb is present, the high delayed fracture characteristics can be more stably maintained. To achieve this effect, it is preferable that the Sb content of the steel wire is 0.001% or more.
[0188] On the other hand, if the Sb content of the steel wire exceeds 0.030%, its effect will be saturated.
[0189] Therefore, when steel wire actively contains Sb, the Sb content is preferably 0.001~0.030%. The Sb content can be less than 0.020%.
[0190] (Metallic structure)
[0191] The steel portion (steel wire) of the galvanized steel wire disclosed herein has an area ratio of 95.0% or more of a mixed structure of ferrite phase and cementite phase in the center part of a cross section (longitudinal section) that is parallel to the length direction of the steel wire and passes through the central axis, within 1.0 mm of the central axis.
[0192] If the area fraction of the mixed ferrite and cementite phases in the central part of the longitudinal section (the section parallel to the length direction of the wire) of the steel wire is 95.0% or more, the drawn wire will exhibit good delayed fracture characteristics. If the area fraction of the mixed ferrite and cementite phases in the central part of the steel wire is 95.0% or more, then including the surface layer, the total area fraction of the remaining portion is low; therefore, the central part is used as a representative for measurement. The area fraction of the mixed ferrite and cementite phases in the central part of the steel wire cross-section can be 96.0% or more, or it can be 97.0%, 98.0%, 99.0%, or 100.0% or more.
[0193] -Determination of the area ratio of metallic structures-
[0194] Using a scanning electron microscope (SEM) at 3×10 -4 mm 2 Five images of the center section of the longitudinal cross-section of the wire were taken at 200 μm intervals (0.015 mm longitudinally and 0.02 mm transversely). Etching was performed using a picric acid-ethanol solution.
[0195] Figure 1A An example of a SEM image showing a longitudinal section of a steel wire containing a mixed microstructure of ferrite and cementite phases, as well as portions of the microstructure that are not a mixture of ferrite and cementite phases (sometimes referred to as "non-mixed microstructure" in this disclosure). The portion M indicated by the arrow represents the non-mixed microstructure. Figure 1B It is Figure 1A A magnified image of the portion containing the non-mixed tissue M. Additionally, Figure 2BThis is another example of SEM images of longitudinal sections of steel wires containing mixed and non-mixed microstructures of ferrite and cementite phases. Figure 2B It is Figure 2A An enlarged image of a portion containing non-mixed tissue M. Figure 1B and Figure 2B In the diagram, region M, enclosed by black dashed lines, represents a non-mixed tissue.
[0196] The mixed microstructure of ferrite and cementite phases is formed by drawing pearlite, bainite, etc., and the cementite phase is mixed in with the ferrite phase. The area fraction (%) in each SEM image was measured. Specifically, after printing each SEM image onto paper, a transparent sheet such as an OHP (Overhead Projector) was superimposed on the paper, and color was applied to the non-mixed microstructure. Then, the colored transparent sheet was analyzed by image resolution to determine the total area fraction of the non-mixed microstructure. The area of each field of view was set to 3 × 10⁻⁶. -4 mm 2 (0.015mm vertically, 0.02mm horizontally), image analysis software (e.g., LUZEX AP from NIRECO) is used for image analysis. The average (%) of the area ratio of the non-mixed microstructure is calculated from the 5 images, and the value obtained by subtracting the average from 100.0 is taken as the area ratio of the mixed microstructure of ferrite and cementite phases of the steel wire.
[0197] (Diameter of the steel part)
[0198] The diameter of the steel portion (steel wire) of the galvanized steel wire disclosed herein is 5.0 mm or more. The diameter of the steel portion can be 5.1 mm or more, 5.3 mm or more, 5.5 mm or more, or 6.0 mm or more. There is no particular upper limit to the diameter of the steel portion; however, if it is for bridge use, it can be 10.0 mm or less, 8.0 mm or less, or 7.0 mm or less.
[0199] (Tensile strength)
[0200] The tensile strength TS of the galvanized steel wire disclosed herein is above 1900 MPa and below 2250 MPa.
[0201] If the tensile strength of the coated steel wire is 1900 MPa or higher, the delayed fracture characteristics deteriorate. This is due to the increased hydrogen intrusion and the increased susceptibility to hydrogen-induced cracking. The coated steel wire of this disclosure can improve its delayed fracture characteristics even with a tensile strength of 1900 MPa by satisfying other requirements.
[0202] If the tensile strength of the steel wire exceeds 2250 MPa, its torsional properties deteriorate. Therefore, the upper limit of tensile strength is set at 2250 MPa.
[0203] (Yield Ratio)
[0204] The ratio of the yield strength (0.2% endurance) YS to the tensile strength TS (yield ratio: YS / TS) of the galvanized steel wire disclosed herein is 0.87 or higher.
[0205] When the ratio of the yield strength YS to the tensile strength TS of the steel wire (YS / TS) is 0.87 or higher, carbon is fixed in the dislocation core, and hydrogen fixation around the dislocation is suppressed, thus it is presumed that hydrogen intrusion is suppressed. More preferably, the yield ratio (YS / TS) of the steel wire is 0.90 or higher, and even more preferably 0.93 or higher.
[0206] -Determination of tensile strength and yield strength-
[0207] The plated steel wire used for tensile testing can be straightened to achieve a straight line. Furthermore, if the straightening process is strictly performed, the YS (yellow-sharpness) will change, allowing for multi-point bending straightening even when the wire is bent and cannot be clamped.
[0208] The length of the galvanized steel wire was set to 340 mm, the distance between the chucks was set to 200 mm, and a tensile test was conducted at a stroke speed of 10 mm / min.
[0209] The diameter D of the coated steel wire is measured at the center of the wire's length using vernier calipers in two orthogonal directions, and the average value is recorded. The tensile strength is calculated from the cross-sectional area (mm²) calculated as "maximum load (N) during the tensile test / diameter of the coated steel wire". 2 ).
[0210] Yield strength is calculated using the linear relationship between stress and strain at 0.2% of tensile strength (0.2% endurance) at 0.2% plastic deformation.
[0211] (Zn-based coating)
[0212] In the plated steel wire of the present invention, the surface of the steel wire (steel base, i.e., steel part) is coated with a Zn-based coating with Zn as the main component at a concentration of 100 g / m. 2 Covering. Zn-based coatings, with Zn as the main component, refer to coatings in which Zn content (mass%) is the highest. They can be coatings composed solely of Zn, or coatings composed of alloys of Zn and other elements. Elements other than Zn that can be included in Zn-based coatings include, for example, one or more elements selected from the group consisting of Al, Cu, Sn, Mg, and Si.
[0213] Zn-based coatings are applied at 100 g / m 2 The above-mentioned surface covering the steel wire (steel base) can effectively inhibit the intrusion of hydrogen.
[0214] Here, the methods for measuring torsion characteristics, plating adhesion amount, and diffusible hydrogen content in the embodiments described later will be explained.
[0215] (Torsion characteristics)
[0216] The evaluation was based on the number of times the plated steel wire broke, with 5 wires tested for each method, and the minimum value was evaluated.
[0217] The distance between the chucks is 100 × wire diameter D. The rotation speed is 20 rpm.
[0218] It should be noted that the fracture of the coated steel wire includes not only the case of complete fracture but also the case of localized cracking. That is, in the case of localized cracking of the coated steel wire during the test, the evaluation is based on the number of torsion cycles at that moment. Cracks occurring during rotation can be determined by a sudden drop in torque.
[0219] (Platinum adhesion amount)
[0220] The coating adhesion amount is calculated from the weight difference and the peeling area when the coating is peeled off. The coated steel wire is cut into 100mm pieces and immersed in a solution containing an inhibitor in hydrochloric acid to chemically peel off the coating. The coating adhesion amount is calculated by dividing the weight difference before and after peeling by the surface area calculated from the wire diameter and length after peeling.
[0221] (Diffusive hydrogen content)
[0222] According to JASO M610-92 (Test Method for Corrosion of Automotive Components), for steel wires with removed plating, a brine spray based on a 5% sodium chloride aqueous solution was performed at 35°C for 2 hours, followed by drying at 60°C and 30% RH for 4 hours, and then wetting at 50°C and 95% RH for 2 hours, which was considered a cycle. After 168 cycles, the samples were recovered, and after rust removal by sandblasting, hydrogen analysis was performed using gas chromatography. The hydrogen released below 200°C was measured using two samples, and the average value was taken as the amount of diffusible hydrogen (HE) adsorbed in the service environment.
[0223] [Manufacturing method of plated steel wire]
[0224] The method for manufacturing the plated steel wire disclosed herein is not particularly limited. Hereinafter, an example of a preferred manufacturing method will be described.
[0225] (Wire manufacturing)
[0226] Use wire with the above-mentioned chemical composition (steel composition). In order to adjust the structure to be suitable for wire drawing, the wire is preferably heated to 950~1100°C and then immersed in a molten salt or lead bath at 550~650°C to form a pearlitic structure.
[0227] (Wire drawing process)
[0228] Steel wire is made by drawing wire.
[0229] The wire drawing strain ε caused by the wire drawing process is expressed by the following formula.
[0230] ε = Ln(D0 / D) 2
[0231] D0 is the diameter before wire drawing, and D is the diameter after wire drawing. The wire drawing strain ε is preferably between 1.00 and 2.50. When the wire drawing strain ε is below 1.00, it is difficult to exhibit strength; when it is above 2.50, the strength becomes excessive, and the torsional characteristics decrease. It should be noted that surface lubrication treatment such as zinc phosphate coating or borax coating is preferably performed before wire drawing.
[0232] It should be noted that the diameter D of the steel wire is 5.0 mm or more, as mentioned above. There is no specific upper limit to the diameter D of the steel wire, but if it exceeds 7.5 mm, it is difficult to obtain the target strength. Therefore, the diameter of the steel wire is limited to a range of 5.0 mm to 7.5 mm.
[0233] (Fused zinc plating)
[0234] After wire drawing and degreasing, the steel is galvanized or alloyed with zinc as the main component. The molten zinc temperature is preferably within the range of 400–530°C. Below 400°C, the steel hardens due to age hardening, and its torsional properties decrease. On the other hand, above 530°C, softening due to factors such as spheroidization of cementite becomes significant, resulting in insufficient strength. Therefore, it is preferable to perform the plating treatment within the molten zinc temperature range of 400–530°C.
[0235] (Thermal stretching)
[0236] To improve the ratio of yield strength YS to tensile strength TS (YS / TS), it is preferable to apply a load of approximately 0.35 to 0.55 times the tensile strength TS of the coated steel wire at 300 to 400°C for approximately 10 to 45 seconds after the aforementioned hot-drawing. If the temperature during such hot drawing is below 300°C, the strength of the coated steel wire increases, but the torsional characteristics decrease. On the other hand, at temperatures above 400°C, an improvement in durability cannot be expected, and the delayed fracture characteristics are not improved. Furthermore, at temperatures above 420°C, the coating may remelt. Therefore, hot drawing is preferably performed at 300 to 400°C.
[0237] The above processes enable the manufacture of the plated steel wire of this disclosure. It should be noted that the above method is an example of a preferred method for manufacturing the plated steel wire of this disclosure, and the manufacturing method of the plated steel wire of this disclosure is not limited to the above method.
[0238] (use)
[0239] The applications of the galvanized steel wire disclosed herein are not particularly limited, and it is suitable for applications requiring high strength, delayed fracture characteristics, and torsional properties, such as steel wire for bridge cables and various ropes. For example, ropes (strands) obtained by bundling multiple galvanized steel wires disclosed herein can be used for bridge cables.
[0240] Example
[0241] The following examples illustrate the plated steel wire of this disclosure in more detail. However, these examples do not limit the plated steel wire, rope, or method of manufacturing the rope disclosed herein.
[0242] <Example 1>
[0243] Steel (steel1) with the chemical composition shown in Table 1 (unit: mass%) was produced. Wire was manufactured using the methods (conditions) shown in Table 2, followed by wire drawing, hot-dip galvanizing, and hot stretching to produce coated steel wire. It should be noted that the "-" in Table 1 indicates that the content of that element is at the impurity level, meaning it is substantially absent. The same applies to the "-" in Table 4 (described later). Furthermore, the remaining components of the chemical compositions in Tables 1 and 4 are Fe and impurities. Additionally, in Table 2, the "-" indicates that no coating was performed.
[0244] In addition, underlines in the tables indicate items outside the scope of this disclosure.
[0245] [Table 1]
[0246]
[0247] [Table 2]
[0248]
[0249] For the coated steel wire manufactured by the above method, the area ratio, tensile strength, yield strength (0.2% endurance) YS, coating adhesion, torsional value, and diffusible hydrogen content HE of the mixed ferrite and cementite phase in the central part of the longitudinal section of the steel wire portion (steel base) were measured using the above methods. Furthermore, the non-mixed ferrite and cementite phase structure is mainly composed of ferrite and martensite.
[0250] The following situations are rated as good.
[0251] • Torsion value: 10 or higher
[0252] • Diffusible hydrogen content (HE): below 0.100 ppm
[0253] The measurement results are shown in Table 3. Cases where the torsion value or diffusive hydrogen content (HE) does not meet the above "good" standard are marked with an underline.
[0254] It should be noted that Comparative Example 9 was not plated and the measurement value is that of the steel wire after the wire drawing process.
[0255] [Table 3]
[0256]
[0257] The plated steel wires of Examples 1 to 4 have high strength of 1900 MPa or more and 2250 MPa or less, and have good torsional properties and resistance to hydrogen intrusion.
[0258] In Comparative Example 1, the high heating temperature during wire manufacturing resulted in coarse grains. During molten salt impregnation, the pearlite phase transformation was incomplete, leading to the formation of martensite, which reduced processability and caused cracks during wire drawing.
[0259] Comparative Example 2 has high wire drawing strain and excessive strength, resulting in insufficient torsional characteristics.
[0260] In Comparative Example 3, the strength becomes too high due to the low heating temperature during hot stretching, resulting in insufficient torsional properties.
[0261] Comparative Examples 4-8 all had insufficient endurance ratios and high levels of diffusible hydrogen (HE).
[0262] Comparative Example 9 exhibits insufficient torsional properties. This is believed to be because, without the heat input during plating, the ductility decreases due to thermal stretching.
[0263] <Example 2>
[0264] Prepare steel (steel 2~25) with the chemical composition shown in Table 4 (unit: mass%), and manufacture coated steel wire under the conditions of method A shown in Table 2.
[0265] [Table 4]
[0266]
[0267] For the manufactured coated steel wire, the total area ratio of ferrite and martensite, tensile strength, yield strength (0.2% endurance) YS, coating adhesion, torsion value, and diffusible hydrogen content HE were determined using the methods described above. It should be noted that, apart from the mixed structure composed of ferrite and cementite, the main structures are ferrite and martensite.
[0268] The measurement results are shown in Table 5.
[0269] [Table 5]
[0270]
[0271] The plated steel wires of Examples 11 to 24 have high strength of 1900 MPa or more and 2250 MPa or less, and have good torsional properties and resistance to hydrogen intrusion.
[0272] In Comparative Example 11, the amount of carbon was insufficient, resulting in insufficient strength, less than 1900 MPa.
[0273] Comparative Example 12 has too much carbon, resulting in excessive strength and insufficient torsional properties.
[0274] In Comparative Example 13, the amount of Si was too high, resulting in the formation of martensite and reduced machinability.
[0275] The excessive amount of Mn in Comparative Example 14 resulted in the formation of martensite, which reduced its processability.
[0276] The amount of N in Comparative Example 15 is too high, resulting in insufficient torsional characteristics.
[0277] The amount of Al in Comparative Example 16 was too high, resulting in reduced processability.
[0278] In Comparative Example 17, the excessive amount of Cu resulted in the formation of martensite, which reduced processability.
[0279] Comparative Example 18 has a Cu content below the lower limit and a high amount of diffusible hydrogen (HE).
[0280] The excessive amount of Mo in Comparative Example 19 resulted in the formation of martensite, which reduced processability.
[0281] Comparative Example 20 had too much Cr, which reduced its machinability.
[0282] The plated steel wire and the like of the present invention have been described above, but the plated steel wire and the like of the present invention are not limited to the embodiments and examples described above. For example, the method for manufacturing the plated steel wire of the present invention can also be to impregnate the wire with molten salt after winding the wire to produce a wire with a desired metallic structure, to draw the wire to produce steel wire, and to manufacture plated steel wire by galvanizing and hot drawing. In addition, the case of bundling the plated steel wire to manufacture ropes (cables) is also included within the scope of this disclosure.
[0283] (Postscript)
[0284] This disclosure includes the following methods.
[0285] <1> A type of plated steel wire has the following steel composition: the steel portion contains, by mass%, C: 0.80~1.10%, Si: 0.10~1.50%, Mn: 0.10~1.00%, P: less than 0.050%, S: less than 0.050%, N: less than 0.0120%, O: less than 0.0100%, Al: 0.005~0.070%, Cu: 0.04~0.80%, and the remainder is Fe and impurities. In the central part of a cross-section parallel to the length direction and passing through the central axis, the total area fraction of ferrite and martensite is less than 5.0%, and the remainder is a mixed structure composed of ferrite and cementite. The surface of the steel portion is covered with a Zn-based coating with Zn as the main component at a depth of 100 g / m. 2 The above conditions are met, the tensile strength TS is 1900 MPa or more and 2250 MPa or less, and the yield strength (0.2% endurance) YS is 0.87 or more relative to the tensile strength TS.
[0286] <2> A type of plated steel wire, wherein the steel portion contains, by mass percent, C: 0.80~1.10%, Si: 0.10~1.50%, Mn: 0.10~1.00%, P: less than 0.050%, S: less than 0.050%, N: less than 0.0120%, O: less than 0.0100%, Al: 0.005~0.070%, and Cu: 0.04~0.80%, and contains one or more elements selected from groups A to C below, the remainder being Fe and impurities.
[0287] (Group A)
[0288] Select one or more from the group consisting of Mo: less than 0.20%, Cr: less than 1.00%, and V: less than 0.15%.
[0289] (Group B)
[0290] Choose one or both of the following groups: Sn: less than 0.50% and Ni: less than 0.80%.
[0291] (Group C)
[0292] The steel portion is selected from one or more of the following groups: Ti: 0.050% or less, Nb: 0.050% or less, B: 0.0040% or less, REM: 0.030% or less, Bi: 0.020% or less, Mg: 0.0040% or less, Ca: 0.0040% or less, Zr: 0.030% or less, W: 0.10% or less, Te: 0.030% or less, and Sb: 0.030% or less. In a cross-section parallel to the length direction and passing through the central axis, within 1.0 mm of the center, the combined area fraction of ferrite and martensite is 5.0% or less, and the remaining portion is a mixed structure composed of ferrite and cementite. The surface of the steel portion is covered with a Zn-based coating with Zn as the main component, at a depth of 100 g / m². 2 The above conditions are met, the tensile strength TS is 1900 MPa or more and 2250 MPa or less, and the yield strength (0.2% endurance) YS is 0.87 or more relative to the tensile strength TS.
[0293] <3> according to <2> The plated steel wire, wherein the steel composition includes group A.
[0294] <4> according to <2> or <3> The plated steel wire, wherein the steel composition includes group B.
[0295] <5> according to <2> ~ <4> The plated steel wire according to any one of the following methods, wherein the steel composition comprises group C.
[0296] <6> A rope in which multiple strands are bound together. <1> ~ <5> The plated steel wire as described in any one of the above.
[0297] <7> A method for manufacturing a rope, comprising: bonding multiple ropes... <1> ~ <6> The process of binding galvanized steel wire into rope as described in any one of the above.
[0298] The publication of Japanese Patent Application No. 2024-067775, filed on April 18, 2024, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as the specific documents, patent applications, and technical standards described separately.
Claims
1. A type of plated steel wire, characterized in that, It has the following steel composition: The steel portion contains, by mass % C:0.80~1.10%、 Si: 0.10~1.50% Mn: 0.10~1.00% P: below 0.050% S: Below 0.050% N: below 0.0120% O: Below 0.0100% Al:0.005~0.070%、 Cu: 0.04~0.80%, Mo: 0~0.20%, Cr:0~1.00%、 V:0~0.15%、 Sn: 0~0.50% Ni: 0~0.80% Ti: 0~0.050%, Nb: 0~0.050%, B:0~0.0040%、 REM: 0~0.030%, Bi: 0~0.020% Mg: 0~0.0040% Ca: 0~0.0040% Zr:0.030%、 W:0~0.10%、 Te: 0~0.030%, Sb: 0~0.030%, The remainder consists of Fe and impurities. In the central portion of a section parallel to the length direction and passing through the central axis, within 1.0 mm of the central axis, the area fraction of a mixed microstructure composed of ferrite and cementite phases is 95.0% or more. The diameter of the steel portion is 5.0 mm or more. The surface of the steel portion is covered with a Zn-based coating with Zn as the main component, weighing 100 g / m². 2 above, Tensile strength TS is above 1900MPa and below 2250MPa The yield strength YS, i.e., 0.2% endurance, is greater than or equal to the tensile strength TS, and the ratio YS / TS is greater than or equal to 0.
87.
2. The plated steel wire according to claim 1, characterized in that, The steel portion contains, by mass percent, one or more elements selected from groups A to C below. (Group A) Select one or more from the group consisting of Mo: less than 0.20%, Cr: less than 1.00%, and V: less than 0.15%. (Group B) Choose one or both of the following groups: Sn: less than 0.50% and Ni: less than 0.80%. (Group C) Select one or more from the group consisting of Ti: less than 0.050%, Nb: less than 0.050%, B: less than 0.0040%, REM: less than 0.030%, Bi: less than 0.020%, Mg: less than 0.0040%, Ca: less than 0.0040%, Zr: less than 0.030%, W: less than 0.10%, Te: less than 0.030%, and Sb: less than 0.030%.
3. The plated steel wire according to claim 2, characterized in that, The steel composition includes group A.
4. The plated steel wire according to claim 2 or 3, characterized in that, The steel composition includes group B.
5. The plated steel wire according to any one of claims 2 to 4, characterized in that, The steel composition includes group C.
6. A rope, characterized in that, The bundle consists of multiple galvanized steel wires as described in any one of claims 1 to 5.
7. A method for manufacturing a rope, characterized in that, The process includes binding multiple galvanized steel wires as described in any one of claims 1 to 5 to form a rope.
Citation Information
Patent Citations
High-strength rolled and plated pc steel bar, and manufacturing method therefor
JP2003328077A
High-strength steel wire