Sintered body and sputtering target and method for manufacturing sintered body

By controlling the composition and sintering conditions of IGZO sintered bodies, sintered bodies with IGZO homologous crystalline phases as the main phase were prepared, solving the cracking problem and realizing sputtering targets with high stability and low resistance, which are suitable for the manufacture of large-area sputtering targets.

CN123125364APending Publication Date: 2026-11-17JX NIPPON MINING & METALS CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202480091018.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-17
Filing Date
2024-12-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Layered homologous crystalline phases are easily formed in IGZO sintered bodies, leading to grain growth and crack formation, which affects sputtering stability and target reliability.

Method used

By controlling the sintering conditions and composition ratio, a sintered body with IGZO homologous crystalline phase as the main phase was prepared, the crack length was limited to less than 1 μm2, the volume resistivity was less than 10 mΩ·cm, and grain growth was suppressed by hot pressing sintering under vacuum or inert atmosphere.

Benefits of technology

It effectively suppressed the formation of cracks, improved the bending strength and resistivity stability of the sputtering target, and ensured the stability of sputtering and high-power operation capability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125364A_ABST
    Figure CN123125364A_ABST
Patent Text Reader

Abstract

The technical problem of this disclosure is to provide a sintered body and a method for manufacturing the same, wherein the sintered body contains indium, gallium, zinc, and oxygen, and the sintered body is dominated by an IGZO homologous crystalline phase, thereby suppressing crack initiation. A sintered body containing indium, gallium, zinc, and oxygen, wherein the sintered body is dominated by an IGZO homologous crystalline phase, and the total crack length is less than 1 μm. 2 Its thickness is below 0.1 μm and its volume resistivity is below 10 mΩ·cm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to sintered bodies and sputtering targets, as well as methods for manufacturing sintered bodies. Background Technology

[0002] Oxide films (also known as IGZO) composed of indium (In), gallium (Ga), zinc (Zn), and oxygen (O) have attracted attention as transparent conductive films and oxide semiconductors. IGZO films have the advantage of higher mobility than a-Si (amorphous silicon), and therefore their business is gradually expanding as driving elements for displays (TFTs) (Patent Documents 1-3). A higher In content tends to result in higher mobility, therefore research on regions with high In content (high In) is actively being conducted (Patent Document 4). A higher Zn content tends to result in increased crystallinity (Patent Document 5).

[0003] IGZO thin films are typically formed using sputtering targets composed of IGZO sintered bodies. In IGZO sintered bodies, layered homologous crystalline phases are generated, which easily leads to grain growth. Therefore, microwave sintering has been proposed to suppress grain growth (Patent Document 6). Patent Document 7 describes how forming sintered bodies with two or more homologous crystalline phases can reduce particle size.

[0004] Existing technical documents Patent documents Patent Document 1: Japanese Patent Application Publication No. 2008-163441 Patent Document 2: Japanese Patent Application Publication No. 2008-163442 Patent Document 3: International Publication No. 2009 / 142289 Patent Document 4: Japanese Patent Application Publication No. 2011-106003 Patent Document 5: Japanese Patent Application Publication No. 2017-145510 Patent Document 6: Japanese Patent Application Publication No. 2014-040348 Patent Document 7: International Publication No. 2009 / 142289 Summary of the Invention

[0005] The problem that the invention aims to solve In sintered bodies containing indium, gallium, zinc, and oxygen, homologous crystalline phases are easily formed, and these homologous crystalline phases have a layered structure. Therefore, they generate shear forces and are prone to cracking within the grains.

[0006] In view of the above problems, the technical problem of this disclosure is to provide a sintered body and a method for manufacturing the same, wherein the sintered body contains indium, gallium, zinc and oxygen, and the sintered body is dominated by a homologous crystalline phase, thereby suppressing the generation of cracks.

[0007] Solution for solving the problem In order to solve the above-mentioned technical problems, the inventors conducted in-depth research and obtained the following insights: by designing manufacturing methods, it is possible to obtain a sintered body with homologous crystalline phase as the main phase and the generation of cracks suppressed.

[0008] That is, the main point of this disclosure is as follows.

[0009] [1] A sintered body containing indium, gallium, zinc and oxygen, wherein the sintered body is dominated by an IGZO homologous crystalline phase and the total length of cracks is less than 1 μm. 2 Its thickness is below 0.05 μm and its volume resistivity is below 10 mΩ·cm.

[0010] [2] The sintered body according to [1], wherein the average grain size is less than 3 μm.

[0011] [3] The sintered body according to [1] or [2], wherein the volume resistivity is less than 5 mΩ·cm.

[0012] [4] The sintered body according to any one of [1] to [3], wherein the coefficient of variation of the volume resistivity is less than 10%.

[0013] [5] The sintered body according to any one of [1] to [4], wherein the intensity of the largest XRD diffraction peak among the normalized XRD diffraction peak intensities of the IGZO homologous phase is set as P. max The intensity of the largest diffraction peak in the normalized XRD diffraction peaks of other crystalline phases excluding IGZO homologues is set as Q. max At that time, the XRD diffraction peak intensity ratio (P) max / Q max () is 3 or above.

[0014] [6] The sintered body according to any one of [1] to [5], wherein the relative density is 95% or more.

[0015] [7] The sintered body according to any one of [1] to [6], wherein the bending strength is 200 MPa or more.

[0016] [8] The sintered body according to any one of [1] to [7], wherein the composition is within the following range in terms of atomic ratio.

[0017] 0.11≤In / (In+Ga+Zn)≤0.40 (1) 0.11≤Ga / (In+Ga+Zn)≤0.40 (2) 0.20≤Zn / (In+Ga+Zn)≤0.78 (3) [9] A sputtering target, which is composed of a sintered body as described in any one of [1] to [8].

[0018]

[10] According to the sputtering target described in [9], the area of ​​the sputtered surface is 176 cm². 2 The diameter of the surface being sputtered is 150 mm or more.

[0019]

[11] A method for manufacturing a sintered body, which is the method for manufacturing a sintered body as described in any one of [1] to [8], wherein In2O3 powder, Ga2O3 powder, and ZnO powder are mixed, and the resulting mixed powder is subjected to a maximum sintering temperature of 1000-1150°C and a pressing pressure of 150 kgf / cm² under vacuum or inert gas atmosphere. 2 Hot pressing is performed under the above conditions.

[0020]

[12] According to the method for manufacturing the sintered body described in

[11] , the pressing pressure is set to 125 kgf / cm² in the temperature range from 900°C to the highest sintering temperature. 2 above.

[0021] Invention Effects According to this disclosure, a sintered body and a sputtering target can be provided, the sintered body containing indium, gallium, zinc and oxygen, wherein the sintered body is dominated by a homologous crystalline phase, and the generation of cracks is suppressed. Attached Figure Description

[0022] Figure 1 This is an image analysis diagram used when analyzing cracks (for reference only).

[0023] Figure 2 This is a binarized image of a sintered body (single phase) (reference). Detailed Implementation

[0024] The following specific embodiments are provided to illustrate this disclosure. However, each component and combination thereof in each embodiment is only an example. Appropriate additions, omissions, substitutions and other changes to the components may be made without departing from the spirit of this disclosure.

[0025] The sintered body of the embodiments disclosed herein contains indium, gallium, zinc, and oxygen. A sintered body having such a composition is sometimes referred to as an IGZO sintered body. IGZO is an abbreviation derived from the first letters of each of the constituent elements: indium (In), gallium (Ga), zinc (Zn), and oxygen (O). IGZO thin films are used as transparent conductive films and oxide semiconductors, and in particular, they possess superior properties such as higher mobility than a-Si. Therefore, they are used as driving elements for displays (TFT: Thin Film Transistor).

[0026] IGZO thin films can typically be formed using sputtering. A sputtering target (sometimes called an IGZO sputtering target) made of IGZO sintered material is placed in a vacuum chamber, and argon ions generated by glow discharge collide with the sputtering target at high speed, causing the ejected atoms to deposit on an opposing glass substrate, thereby forming a thin film with a composition approximately the same as that of the sputtering target.

[0027] IGZO sputtering targets are fabricated from sintered raw material powders. During sintering, the oxides containing In, Ga, and Zn, which are the raw materials, react to form homologous crystalline phases. These homologous crystalline phases are stable, but they also have a layered structure, making them prone to shear stress and cracking. Cracks can cause arcing during sputtering and, in high-power sputtering, can lead to target breakage; therefore, minimizing these cracks is desirable.

[0028] The IGZO sintered body of this embodiment is dominated by the IGZO homologous phase. The IGZO homologous phase consists of (In,Ga)₂O₃(ZnO). m The homologous crystalline phases represented (m = 0.5 or an integer from 1 to 20), especially those consisting of (In,Ga)₂O₃ (ZnO). m The homologous crystalline phases are indicated by m = 1, 2, 3, 4. Besides the IGZO homologous phase, IGZO sintered bodies can also contain ZnGa₂O₄, In₂O₃, β-GaInO₃, and In₂Zn₇O phases. 10 Equal crystalline phases.

[0029] XRD (X-ray diffraction) was used to analyze the sintered IGZO body, and each crystal phase was identified using ICSD (Crystal Structure Database). The maximum XRD diffraction peak intensity among the normalized XRD diffraction peak intensities of the IGZO homologous phases was set as P. max The largest XRD diffraction peak intensity among the normalized XRD diffraction peak intensities of other crystalline phases excluding IGZO homologues is set as Q. max When the XRD diffraction peak intensity ratio (P) is... max / Q max If the value is at least 1, then it is determined that the IGZO homologous crystal phase is the main phase.

[0030] The standardized XRD diffraction peak intensity refers to the XRD diffraction peak intensity obtained by subtracting the "background intensity" from the XRD diffraction peak intensity of each crystal phase (crystal plane) when the average intensity of the XRD diffraction angle 2θ = 40° to 41° is set as the "background intensity". It should be noted that when peaks originating from the crystal phase exist within the above angle range, a range of Δ2θ = 1° without peaks originating from the crystal phase is selected within the range of 2θ = 20° to 50°, and its average intensity is set as the background. When the standardized XRD diffraction peak intensity is below 0, the diffraction peak intensity is considered zero.

[0031] Thin films composed mainly of IGZO homologous crystalline phases exhibit excellent characteristics as channel layers for TFTs, such as high mobility and low carrier concentration. In this embodiment, the XRD diffraction peak intensity ratio (P... max / Q max More preferably, the ratio is 3 or more, further preferably 5 or more, and particularly preferably 10 or more. Furthermore, if the XRD diffraction peak intensity ratio (P...) is... max / Q max If the value is at least 1, then In, Ga, and Zn can be replaced with other elements as needed.

[0032] Cracks can cause arcing during sputtering and may also lead to breakage and fissures in the sputtering target; therefore, minimizing them is desirable. In this embodiment, the total crack length in the IGZO sintered body is less than 1 μm. 2 The crack length is below 0.05 μm. This suppresses the adverse effects of cracks during sputtering, target breakage, and fissures. Preferably, the total crack length is less than 1 μm per 1 μm. 2 The crack length is 0.03 μm or less, more preferably 0.02 μm or less. The lower limit of the total crack length does not need to be specifically limited; it can be within the range of 1 μm. 2 It is above 0.000μm.

[0033] In this embodiment, the average grain size of the sintered body is preferably 3 μm or less. IGZO homologous phases readily grow grains, and when the grains become coarse, cracks are easily generated. Furthermore, as mentioned above, when the layered IGZO homologous phase is the dominant phase, cracks are easily generated due to shear forces, but crack generation can be suppressed by reducing the grain size. Moreover, grain growth is also related to a decrease in flexural strength; therefore, a fine grain size is preferred. Preferably, the average grain size is 2 μm or less.

[0034] The volume resistivity of the sintered body in this embodiment is 10 mΩ·cm or less. The lower the volume resistivity of the sputtering target made of the IGZO sintered body, the more stable the sputtering can be. In the case of an IGZO homologous crystalline phase, grain growth is easy; therefore, the use of "microwave sintering" to suppress grain growth has been studied. However, this sintering method has difficulty obtaining sintered bodies with low resistivity. According to this disclosure, a sintered body with suppressed grain growth and low resistivity can be obtained. The volume resistivity is more preferably 5 mΩ·cm or less, and even more preferably 1 mΩ·cm or less.

[0035] The in-plane coefficient of variation of the volume resistivity of the sintered body in this embodiment is preferably 10% or less. In a sputtering target composed of an IGZO sintered body, the smaller the coefficient of variation of the volume resistivity, the more stable the sputtering can be. As described above, the IGZO homologue has the property of easy grain growth, but in conventional manufacturing methods, when grain growth is suppressed, the volume resistivity and its deviation will change. According to this disclosure, grain growth can be suppressed, and the coefficient of variation of the volume resistivity can be kept small. More preferably, it is 5% or less.

[0036] The coefficient of variation of volume resistivity is calculated according to the following formula.

[0037] Coefficient of variation (CV) [%] = (Standard deviation) / (Arithmetic mean) × 100 For the measurement sites and number of measurement points for volume resistivity, the area of ​​the sintered body is set as Scm. 2 When the length of the outer perimeter is set to Lcm, the interval between the measuring points is set to (L... 1 / 2 For a resistivity of 1.5 cm or more, set the number of measurement points to the smallest positive number calculated based on 3 × S / L, measure the volume resistivity at each measurement point, and calculate its arithmetic mean and standard deviation. It should be noted that if the number of measurement points cannot be obtained as specified in the above formula, determine the maximum number of points that can be measured.

[0038] The relative density of the sintered body in this embodiment is preferably 95% or higher. The higher the relative density of the sputtering target composed of the IGZO sintered body, the better it suppresses the generation of particles during sputtering. In the case of a homologous IGZO phase, grain growth is easy; therefore, efforts have been made to lower the sintering temperature to suppress grain growth. However, it is difficult to obtain a high-density sintered body in this low-temperature sintering. According to this disclosure, a sintered body with suppressed grain growth and high density can be obtained. A relative density of 97% or higher is more preferred, and 98% or higher is even more preferred.

[0039] The flexural strength of the sintered body in this embodiment is preferably 200 MPa or higher. In particular, when the sintered body has an IGZO homologous crystalline phase, there is a problem that cracks can easily form due to grain growth, leading to a decrease in flexural strength. According to this disclosure, grain growth can be suppressed, thus suppressing crack formation and preventing a decrease in flexural strength. More preferably, it is 230 MPa or higher. In particular, by increasing the strength of the sintered body, cracks during sputtering can be suppressed, enabling high-power sputtering.

[0040] The sintered body of this embodiment contains indium, gallium, and zinc, and the content of each is not particularly limited. However, in order to set the IGZO homologue as the main phase, the content ratio of indium, gallium, and zinc preferably satisfies the following formulas (1) to (3). In the following formulas, In, Ga, and Zn represent the atomic ratio of each element contained in the sintered body. In addition, other elements may be added or replaced as needed.

[0041] 0.11≤In / (In+Ga+Zn)≤0.40 (1) 0.11≤Ga / (In+Ga+Zn)≤0.40 (2) 0.20≤Zn / (In+Ga+Zn)≤0.78 (3) More preferably, it satisfies the following equations (4) to (6).

[0042] 0.15≤In / (In+Ga+Zn)≤0.35 (4) 0.15≤Ga / (In+Ga+Zn)≤0.35 (5) 0.20≤Zn / (In+Ga+Zn)≤0.70 (6) The sintered body of this embodiment can be used as a material for PVD (physical vapor deposition), such as a sputtering target, vacuum evaporation material, ion plating material, etc. When used as a sputtering target, it can be formed into a circular plate, rectangular plate, or cylindrical shape, and can be bonded to a bonding material via a back plate. Furthermore, when used as a sputtering target, its thickness can be set to 20 mm or less, preferably 3.0 to 15 mm, more preferably 3.0 to 12 mm. Furthermore, it is preferable that the area of ​​the sputtered surface is 176 cm². 2 The diameter of the surface to be sputtered is 150 mm or more. It should be noted that achieving an area of ​​176 cm² is difficult in HIP (Hot Isostatic Pressing) and SPS (Spark Plasma Sintering). 2 Larger sizes, either 150mm or larger in diameter.

[0043] The manufacturing method of the sintered body, particularly the sputtering target, according to this embodiment will be described. However, it is obvious that the manufacturing conditions and other details described below are not limited to the scope disclosed, and some omissions and modifications may be made. It should be noted that, in order to avoid unnecessarily obscuring the disclosed manufacturing method, detailed descriptions of well-known manufacturing processes and handling operations are omitted.

[0044] (1. Raw material powder) Indium oxide (In₂O₃) powder, gallium oxide (Ga₂O₃) powder, and zinc oxide (ZnO) powder are prepared as raw material powders. The In₂O₃ powder preferably has a median particle size (D50) of 0.5–3.0 μm and a specific surface area of ​​4.0–10 m². 2 / g, the preferred Ga2O3 powder has a median particle size (D50) of 0.5–4.0 μm and a specific surface area of ​​6.0–30 m². 2 / g, ZnO powder preferably has a median particle size (D50) of 0.1–2.0 μm and a specific surface area of ​​2.0–20 m². 2 / g. Furthermore, the raw material powder preferably uses raw material powder with a purity of 99.9% by mass or higher. The raw material powder may also be pre-calcined.

[0045] (2. Mixing and grinding process) The raw material powders are weighed to achieve the desired composition ratio (content ratio of the sintered body) and then mixed and pulverized. Various pulverization methods are available depending on the required particle size and the material being pulverized; wet or dry ball mills, vibratory mills, bead mills, etc., can be used. To obtain uniform and fine grains, bead milling is preferred due to its high efficiency in breaking up aggregates in a short time and its good dispersion of additives. Preferred median particle size (D50) after pulverization: 0.1–1.0 μm, specific surface area: 10.0–30.0 m². 2 / g.

[0046] (3. Sintering process) Next, the mixed powder is sintered. Previously, sintering was carried out at around 1400–1600°C in an atmospheric or oxygen atmosphere. However, at higher sintering temperatures, problems such as grain growth and reduced flexural strength arise. Furthermore, the volume resistivity increases, leading to abnormal discharges and particles during sputtering, making stable sputtering difficult. Especially with the increasing size of the target and the desire for uniform film formation, sputtering stabilization is crucial.

[0047] In this disclosure, sintering is performed under a vacuum or an inert gas atmosphere (argon, nitrogen, etc.) from the viewpoint of creating oxygen deficiencies in the sintered body and reducing its volume resistivity. From the viewpoint of suppressing ZnO sublimation, sintering under an inert gas atmosphere is preferred over a vacuum. On the other hand, when sintering is performed without pressure (at atmospheric pressure) under an inert gas atmosphere, In₂O₃ and Ga₂O₃ will be reduced, hindering the increase of the density of the sintered body, and may also contaminate the interior of the apparatus. Therefore, pressure sintering, which can suppress reduction to a certain extent, is preferred, and hot-pressing sintering is particularly preferred from the viewpoint of productivity.

[0048] (3-1. Sintering temperature maintenance) The maximum sintering temperature in the sintering process is set to 1000℃~1150℃. Previously, sintering was performed at 1400~1600℃, but by setting it below 1150℃, grain growth can be suppressed, and flexural strength can be improved. If the maximum sintering temperature is set too high, there is a concern that In₂O₃ or Ga₂O₃ may react with the carbon in the sintering apparatus components and be reduced; therefore, it is set below 1150℃. On the other hand, if the maximum sintering temperature is set too low, the density of the sintered body will not increase; therefore, it is set above 1000℃.

[0049] (3-2. Suppressing pressure) The pressing pressure at the highest sintering temperature in pressure sintering is preferably set to 150 kgf / cm². 2 The above. When sintering is performed under a vacuum or inert gas atmosphere, In₂O₃ or Ga₂O₃ sometimes undergoes reduction, but this is mitigated by using a sintering rate of 150 kgf / cm². 2 Applying the above pressing pressure to hot pressing can suppress reduction. There is no particular upper limit to the pressing pressure, but considering the strength of the components used for hot pressing, it is preferably set to 400 kgf / cm². 2 the following.

[0050] (3-3. Sintering holding time) The holding time at the highest sintering temperature can be set from 2 hours to 50 hours. By controlling the holding time within this range, the density of the sintered body can be increased while maintaining productivity.

[0051] (3-4. Heating rate) Within the temperature range from 700°C to the maximum sintering temperature, the heating rate is preferably set to 0.1–5.0°C / min, more preferably 0.3–3.0°C / min. Within the aforementioned temperature range, a heating rate exceeding 5.0°C / min is not preferred from the viewpoint of process stability during mass production, and a rate less than 0.1°C / min is not preferred from the viewpoint of reduced productivity. However, the heating rate outside the aforementioned temperature range is not limited, and any heating rate can be used.

[0052] (3-5. Restoration measures) In temperature ranges above 900℃, the ideal pressing pressure is 125 kgf / cm² during heating, temperature holding, and cooling. 2 The above applies. When the pressing pressure is 125 kgf / cm² in a temperature range above 900°C. 2 Under the following conditions, In2O3 and Ga2O3 react with the carbon in the sintered structural components and are reduced, sometimes causing a decrease in density, a shift in composition, and damage to the components.

[0053] (3-6. Cooling rate) Within the temperature range from the highest sintering temperature to 600°C, it is preferable to set the cooling rate to 10°C / min or less. By setting the cooling rate to 10°C / min or less, cracking of the sintered body due to thermal stress can be suppressed. Here, the temperature range where the cooling rate is set to 10°C / min or less is set to 600°C or higher because the thermal stress of the sintered body tends to increase during cooling above 600°C. However, there are no particular limitations on the cooling rate outside the aforementioned temperature range, and any cooling rate can be used.

[0054] Furthermore, when continuous pressing pressure is applied in a temperature range below 600°C, internal stress accumulates, leading to cracking of the sintered body. Therefore, during cooling, a pressing pressure of 50 kgf / cm² is preferred below 600°C. 2 In the following, it is particularly preferred not to apply pressure.

[0055] (4. Regarding finishing) The sintered body obtained through the above sintering process can be machined into the desired shape using surface grinders, cylindrical grinders, machining, or other processing machines. The shape of the sputtering target is not particularly limited; it can be made into a flat disc, rectangular shape, cylindrical shape, etc. Furthermore, the sputtering target can be joined with a backing plate as needed.

[0056] Example The following description is based on embodiments and comparative examples. It should be noted that this embodiment is merely an example and is not intended to limit the invention in any way. That is, the invention is limited only by the claims and includes various modifications other than those included in this disclosure.

[0057] The evaluation methods used in the examples and comparative examples are described below. It should be noted that the sputtering target is processed by grinding, polishing, etc., of the sintered body; therefore, the surface of the polished sintered body is in a state substantially the same as the sputtering surface of the sputtering target. Furthermore, various evaluations are performed on representative portions (samples) of the sintered body. If the various physical properties of the representative sample are included within the scope of this disclosure, the sintered body is included in this invention. That is, even if the measurement of a sample that is not specific, exceptional, or localized like the sintered body and thus falls outside the scope of this disclosure, if the various physical properties of the representative sample are included within the scope of this disclosure, the sintered body is included in this invention as long as it achieves the effects of this invention.

[0058] (Regarding composition analysis) The composition of the sintered body was analyzed using the following apparatus.

[0059] Device: SII SPS3500DD Method: ICP-OES (Inductively Coupled Plasma Emission Spectroscopy).

[0060] (Analysis of crystal phase) The following apparatus was used for the analysis of the crystalline phase.

[0061] Principle: X-ray diffraction method Device: Rigaku Ultima IV Tube: Cu-Kα rays Tube voltage: 40kV Tube current: 30mA Measurement method: 2θ-θ reflection method Measurement range (2θ): 20–90° Scanning speed: 8° / min Sampling interval: 0.02° Diverging slit: 1° Longitudinal diverging slit: 10mm Scattering slit: 8mm Light-receiving slit: Open state Goniometer: Horizontal type Sample measurement site: Sputtering surface side.

[0062] (Regarding the cracks) The cross-sections (parallel to the sputtering surface) of the center and end of the sintered body (within 3 cm from the outer perimeter) were observed using backscattered electron images (magnification: 2000x) from a FE-EPMA (field emission electron probe microanalyzer), and any number of images were taken.

[0063] Device used: JXA-8500 (JEOL) Accelerating voltage: 15.0kV Beam current: 2.0 × 10 -8 .

[0064] The captured images were analyzed using ImageJ (an image processing software). The ImageJ analysis reference diagram is shown below. Figure 1 (Left image: Tissue photograph based on SEM; Right image: Image analysis based on ImageJ). For example... Figure 1 As shown, in ImageJ-based analysis, the frequencies (vertical axis) within the brightness (horizontal axis): n (range = 0 to 255) of the captured image can be counted. It should be noted that, for backscattered electron images, heavier elements are displayed in brighter colors, and lighter elements are displayed in darker colors.

[0065] Regarding the organization of a single phase, select three images as follows: the brightness (n) with the highest frequency. max ) is 160≤n max ≤180, and frequency n max The darkest brightness (n) among brightness values ​​that are more than 1 / 10 of the frequency. 1 / 10 ) is n max -20≤n 1 / 10 ≤n max -15. And, let n be... 1 / 10 -n def =5 of n def So that n def The following are black, above n def Binarization is performed by converting the brightness of a color to white (see reference). Figure 2 To distinguish them from pores, structures in the black area with a long side / short side ratio of 3 or more were considered cracks, and their lengths were measured. The total length of these cracks was divided by the field of view area to obtain the value per 1 μm. 2 The crack length, each of the three sheets at 1μm 2 The average crack length is taken as the total crack length.

[0066] In the case of an organization with multiple crystalline phases, arbitrarily select three images as follows: the frequency corresponding to the brightest crystalline phase (the phase with a high proportion of In₂O₃ phase) becomes the maximum brightness (n₁) with a frequency of 200 ≤ n₁ ≤ 220; the frequency corresponding to the darkest crystalline phase (the phase with a low proportion of In₂O₃ phase) becomes the maximum brightness (n₂) with a frequency of 115 ≤ n₂ ≤ 135. The darkest brightness among the brightness values ​​greater than 1 / 10 of the frequency that becomes n₂ is set as n. 1 / 10 Let n 1 / 10 -n def =5 of n def So that n defThe following are black, above n def The brightness is binarized to white. To distinguish it from pinholes, structures in the black area with a long side / short side ratio of 3 or more are considered cracks, and their lengths are measured. The total length of these lines is divided by the field of view area to obtain the value per 1 μm. 2 The crack length is calculated by taking the average crack length per unit area of ​​the three sheets as the total crack length.

[0067] (Regarding average grain size) An observation sample was cut from the sintered body, and the surface of the cut sample (equivalent to the sputtered surface) was mirror-polished. Five fields of view were photographed using a scanning electron microscope (SEM) at 5000x magnification. Next, three straight lines (hereinafter referred to as lines 1, 2, and 3) were drawn on the captured images, each line traversing at least 10 grains. The length of each line and the number of intersections with grain boundaries were determined. Grain boundaries at the starting and ending points of the lines were not included. Based on the measured line lengths and the number of intersections, the grain size in one field of view was calculated using the following formula.

[0068] Grain size in one field of view = (Length of line 1 / Number of intersections between line 1 and grain boundaries + Length of line 2 / Number of intersections between line 2 and grain boundaries + Length of line 3 / Number of intersections between line 3 and grain boundaries) ÷ 3 Furthermore, for each of the five fields of view, the grain size was calculated using the above formula, and the arithmetic mean of the five fields of view was taken as the average grain size. Where the number of particles traversed by each straight line within a field of view is not more than 10, a magnification of 2000x or 1000x was used. It should be noted that the apparatus and measurement conditions are as follows.

[0069] Device used: JXA-8500F (JEOL) Accelerating voltage: 15.0kV Beam current: 5.0 × 10 -8 A.

[0070] (Regarding volume resistivity) The surface of a sintered body with a diameter of 180 mm was polished. The volume resistivity was measured at 13 arbitrary points on the polished surface at intervals of more than 5.0 cm, and the arithmetic mean and standard deviation of these 13 points were calculated. The following apparatus was used for the measurement.

[0071] Apparatus: NPS resistivity meter Σ-5+ Method: Constant current application Method: DC four-probe method Measurement temperature: room temperature (20-25℃).

[0072] (Regarding relative density) The relative density is calculated using the following formula.

[0073] Relative density (%) = Archimedes density / calculated density × 100.

[0074] Archimedes density: The upper and lower surfaces of the sintered body are ground to a thickness of 1 mm, and the outer peripheral surface is ground to a thickness of 5 mm to prepare a sample for measurement. The Archimedes density is calculated using the Archimedes method.

[0075] Density calculation: Perform compositional analysis of the sintered body, convert the atomic ratio (at%) of each of the constituent elements In, Ga, and Zn relative to the total of 100 at% of In, Ga, and Zn, and calculate the oxide mass ratio (mass%). Use the theoretical densities of In2O3, Ga2O3, and ZnO shown below to calculate the calculated density.

[0076] Calculate density (g / cm³) 3 )=(W1+W2+W3) / (W1 / d1+W2 / d2+W3 / d3) W1: Mass ratio of In2O3 (mass%) The mass ratio of W2 to Ga2O3 (mass%) W3: Mass ratio of ZnO (mass%) Theoretical density: d1: 7.18 g / cm³ 3 (Theoretical density of In2O3) d2: 5.95 g / cm³ 3 (Theoretical density of Ga2O3) d3: 5.61 g / cm³ 3 (Theoretical density of ZnO).

[0077] (Regarding flexural strength) The sample is cut out from the sintered body, and the surface of the cut sample (equivalent to the sputtered surface) is polished. The flexural strength of the polished surface is determined according to JIS R 1601:2008.

[0078] Test method: Three-point bending test Distance between pivots: 30mm Sample size: 3×4×40mm Indenter speed: 0.5 mm / min Set the number of test pieces to 10 and calculate their average value.

[0079] (Example 1) Prepare In2O3 powder, Ga2O3 powder, and ZnO powder. Weigh and mix them in a manner that yields the desired composition, then pulverize them to obtain the median particle size D. 50 Micrometer: 0.64 μm, Specific surface area: 11.7 m² 2 / g of powder. Next, the mixed powder was filled into a carbon mold and sintered under an argon atmosphere at a maximum sintering temperature of 1150℃ and a pressing pressure of 250kgf / cm². 2 Holding time: Hot pressing sintering is carried out for 5 hours to produce a sintered body with a diameter of 180mm. It should be noted that the heating rate from 700℃ to the maximum sintering temperature is set to 3℃ / min, and the cooling rate from the maximum sintering temperature to 600℃ is set to 5℃ / min.

[0080] The physical properties of the sintered body obtained in Example 1 were measured, and the total crack length was found to be 0.002 μm / μm. 2 The results show good performance with an average grain size of 1.2 μm, a relative density of 98.6%, a volume resistivity of 0.6 mΩ·cm, a coefficient of variation of volume resistivity of 4.7%, and a flexural strength of 262.6 MPa. The sintered body is a sintered body with the InGaZnO4 homologue of IGZO as the main phase. The above results are shown in Table 1. (Example 2) Except for the different composition, the sintered body was prepared using the same manufacturing method and conditions as in Example 1. The physical properties of the sintered body obtained in Example 2 were measured, and the total crack length was found to be 0.019 μm / μm. 2 The sintered body exhibits favorable results, including an average grain size of 1.6 μm, a relative density of 99.1%, a volume resistivity of 0.6 mΩ·cm, a coefficient of variation of volume resistivity of 8.3%, and a flexural strength of 241.3 MPa. The sintered body is predominantly composed of the InGaZn2O5 IGZO homologue phase.

[0081] (Example 3) Except for the different composition, the sintered body was prepared using the same manufacturing method and conditions as in Example 1. The physical properties of the sintered body obtained in Example 3 were measured, and the crack length was found to be 0.010 μm / μm. 2 The sintered body exhibits favorable results, including an average grain size of 1.3 μm, a relative density of 98.7%, a volume resistivity of 0.8 mΩ·cm, a coefficient of variation of volume resistivity of 2.8%, and a flexural strength of 260.0 MPa. The sintered body is predominantly composed of the InGaZn4O7 IGZO homologue phase.

[0082] (Example 4) Except for the different composition, the sintered body was prepared using the same manufacturing method and conditions as in Example 1. The physical properties of the sintered body obtained in Example 3 were measured, and the total crack length was found to be 0.003 μm / μm. 2 The sintered body exhibits favorable results, including an average grain size of 0.7 μm, a relative density of 98.9%, a volume resistivity of 0.8 mΩ·cm, a coefficient of variation of volume resistivity of 4.6%, and a flexural strength of 279.9 MPa. The sintered body is dominated by the InGaZn3O6 IGZO homologue phase, with the presence of In2Zn7O. 10 Mutually.

[0083] (Comparative Example 1) Prepare In2O3 powder, Ga2O3 powder, and ZnO powder. Weigh and mix them to achieve the desired composition as shown in Table 1, then pulverize them to obtain the median particle size D. 50 Micrometer: 0.64 μm, Specific surface area: 11.7 m² 2 / g of powder. Next, the mixed powder is filled into a mold and pressed at a pressure of 785kfg / cm. 2 Hold for 1 minute for uniaxial forming, then press with a pressure of 1795 kgf / cm². 2 The sample was then subjected to CIP (Cold Isostatic Pressing) molding with a holding time of 1 minute. The resulting molded body was then sintered under atmospheric pressure in an oxygen atmosphere at a maximum sintering temperature of 1350°C and a holding time of 20 hours to produce a sintered body with a diameter of 180 mm. The physical properties of the sintered body obtained in Comparative Example 1 were measured, and the total crack length was found to be 0.111 μm / μm. 2 The average grain size was 8.3 μm, the volume resistivity was 70 mΩ·cm, and the flexural strength was 77.1 MPa, which were not the expected results. It should be noted that the sintered body is mainly composed of the InGaZnO4 IGZO homologue phase.

[0084] (Comparative Example 2) Prepare In2O3 powder, Ga2O3 powder, and ZnO powder. Weigh and mix them to achieve the desired composition as shown in Table 1, then pulverize them to obtain the median particle size D. 50 Micrometer: 0.24 μm, Specific surface area: 11.45 m² 2 / g of powder. Next, the mixed powder is filled into a mold and pressed at a pressure of 785kfg / cm. 2 Hold for 1 minute for uniaxial forming, then press with a pressure of 1795 kgf / cm². 2CIP molding was performed with a holding time of 1 minute. The resulting molded body was then subjected to atmospheric sintering at a maximum sintering temperature of 1400°C and a holding time of 20 hours to produce a sintered body with a diameter of 180 mm. The physical properties of the sintered body obtained in Comparative Example 2 were measured, and the total crack length was found to be 0.118 μm / μm. 2 The average grain size was 8.3 μm, the volume resistivity was 41.7 mΩ·cm, and the coefficient of variation of the volume resistivity was 13.29%, which did not yield the expected results. It should be noted that the sintered body is dominated by the InGaZn2O5 IGZO homologous crystalline phase.

[0085] (Comparative Example 3) Prepare In2O3 powder, Ga2O3 powder, and ZnO powder. Weigh and mix them to achieve the desired composition as shown in Table 1, then pulverize them to obtain the median particle size D. 50 Micrometer: 0.64 μm, Specific surface area: 11.7 m² 2 / g of powder. Next, the mixed powder is filled into a mold and pressed at a pressure of 785kfg / cm. 2 Hold for 1 minute for uniaxial forming, then press with a pressure of 1795 kgf / cm². 2 CIP molding was performed with a holding time of 1 minute. The resulting molded body was then microwave sintered under atmospheric conditions at a maximum sintering temperature of 1400°C and a holding time of 30 minutes to produce a sintered body with a diameter of 30 mm. In Comparative Example 3, the sintered body cracked. This is believed to be due to the application of high temperature to a portion of the sintered body during sintering, resulting in greater temperature unevenness within the sintered body.

[0086] It should be noted that the sintered body obtained in Comparative Example 3 did not yield a sample of sufficient size, therefore the coefficients of variation of XRD, flexural strength, and volume resistivity could not be determined. The volume resistivity showed significant inhomogeneity, reaching 11 mΩ·cm in the low-resistivity region but exceeding the upper limit of measurement in the high-resistivity region. Grain size measurements were taken in the low-resistivity region, resulting in an average grain size of 3.55 μm and a total crack length of 0.052 μm, which were not the expected results.

[0087] It is believed that the short sintering time of microwave sintering leads to greater temperature unevenness within the sintered body, resulting in uneven volume resistivity and particle size.

[0088] (Comparative Example 4) Except for the differences in composition and sintering temperature, sintered bodies were prepared using the same manufacturing method and conditions as in Example 1. The physical properties of the sintered body obtained in Comparative Example 4 were measured, and the results showed that in addition to the presence of the IGZO homologue phase of InGaZnO4, an In2O3 phase was also present, which was not the expected result.

[0089] According to this disclosure, it is expected that particles can be suppressed during sputtering, thus potentially improving product yield. Improved product yield contributes to a stable product supply and reduces the loss of metal raw materials, which are finite resources. Therefore, this disclosure may contribute to UN-led Sustainable Development Goals (SDGs) Goal 9, “Building resilient infrastructure, promoting inclusive and sustainable industrialization and pursuing expanded technological innovation,” and Goal 12, “Ensuring sustainable consumption and production patterns.” The sintered body and sputtering target of this disclosure are useful for forming IZO thin films as transparent conductive films and oxide semiconductor films.

[0090] Industrial availability According to this disclosure, a sintered body and a method for manufacturing the same are provided. The sintered body contains indium, gallium, zinc, and oxygen, and the sintered body is dominated by an IGZO homologous crystalline phase, thereby suppressing crack formation. The sintered body and sputtering target of this disclosure are useful for forming IGZO thin films as transparent conductive films and oxide semiconductor films.

Claims

1. A sintered body containing indium, gallium, zinc, and oxygen, wherein the sintered body is dominated by an IGZO homologous crystalline phase, and the total length of cracks is less than 1 μm per 1 μm. 2 Its thickness is below 0.05 μm and its volume resistivity is below 10 mΩ·cm.

2. The sintered body according to claim 1, wherein, The average grain size is less than 3 μm.

3. The sintered body according to claim 1, wherein, The volume resistivity is below 5 mΩ·cm.

4. The sintered body according to claim 1, wherein, The coefficient of variation of volume resistivity is less than 10%.

5. The sintered body according to claim 1, wherein, The maximum XRD diffraction peak intensity among the normalized XRD diffraction peak intensities of the IGZO homologues is defined as P. max The largest XRD diffraction peak intensity among the normalized XRD diffraction peak intensities of other crystalline phases excluding IGZO homologues is set as Q. max At that time, the XRD diffraction peak intensity was higher than that of P. max / Q max The value is 3 or higher.

6. The sintered body according to claim 1, wherein, The relative density is over 95%.

7. The sintered body according to claim 1, wherein, The flexural strength is above 200MPa.

8. The sintered body according to claim 1, wherein, The composition, based on atomic ratio, falls within the following range: 0.11 ≤ In / (In + Ga + Zn) ≤ 0.40 (1); 0.11≤Ga / (In+Ga+Zn)≤0.40 (2); 0.20≤Zn / (In+Ga+Zn)≤0.78 (3).

9. A sputtering target comprising a sintered body as described in any one of claims 1 to 8.

10. The sputtering target according to claim 9, wherein, The area of ​​the surface being sputtered is 176 cm². 2 The diameter of the surface being sputtered is 150 mm or more.

11. A method for manufacturing a sintered body, which is the method for manufacturing a sintered body according to any one of claims 1 to 8, wherein, In₂O₃ powder, Ga₂O₃ powder, and ZnO powder were mixed. The resulting mixed powder was then subjected to a vacuum or inert gas atmosphere at a maximum sintering temperature of 1000–1150 °C and a pressing pressure of 150 kgf / cm² at the maximum sintering temperature. 2 Hot pressing is performed under the above conditions.

12. The method for manufacturing a sintered body according to claim 11, wherein, Within the temperature range from 900℃ to the maximum sintering temperature, the pressing pressure is set to 125 kgf / cm². 2 above.

Citation Information

Patent Citations

  • Sputtering target and its manufacturing method

    JP2008163441A

  • Sputtering target and oxide semi-conductor film

    JP2008163442A

  • In-Ga-Zn-O BASED OXIDE SINTERED COMPACT SPUTTERING TARGET HAVING EXCELLENT STABILITY UPON LONG TERM FILM DEPOSITION

    JP2011106003A

  • IGZO sintered compact, method for producing the same, and sputtering target

    JP2014040348A

  • Method of manufacturing oxide film and method of manufacturing semiconductor device

    JP2017145510A