Semiconductor devices
By employing a high aspect ratio oxide semiconductor structure and conductor configuration in a semiconductor device, the problems of low mobility, slow speed, and poor reliability in the prior art are solved, realizing a semiconductor device with high mobility and fast operation, good electrical characteristics and low power consumption, and supporting miniaturization and high integration.
Patent Information
- Application Number
- CN202580029389.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-10
- Filing Date
- 2025-05-01
- Publication Date
- 2026-11-17
AI Technical Summary
Existing semiconductor devices suffer from problems such as low field-effect mobility, slow operating speed, poor reliability, non-uniform electrical characteristics, small on-state current, high power consumption, and low productivity, and are difficult to miniaturize and highly integrate.
A semiconductor device structure incorporating oxide semiconductors is employed. By setting an oxide semiconductor layer on an insulator and configuring the conductor and insulator in a specific manner, a high aspect ratio insulator structure is formed, ensuring consistent grain orientation. Nitride insulators are used to protect the conductors, and the channel width and length are optimized to reduce leakage current.
It improves field-effect mobility, enhances operating speed and reliability, reduces electrical characteristic inhomogeneity, increases on-state current, reduces power consumption, and enables miniaturization and high integration of semiconductor devices.
Smart Images

Figure CN123126049A_ABST
Abstract
Description
Technical Field
[0001] One aspect of the present invention relates to a semiconductor device, a memory device, and an electronic device using an oxide semiconductor layer. Furthermore, another aspect of the present invention relates to a method for manufacturing the aforementioned semiconductor device.
[0002] Note that one aspect of the present invention is not limited to the technical fields described above. Examples of technical fields encompassing one aspect of the present invention include semiconductor devices, display devices, light-emitting devices, energy storage devices, memory devices, electronic devices, lighting devices, input devices (e.g., touch sensors), input / output devices (e.g., touch panels), driving methods for the aforementioned devices, or manufacturing methods for the aforementioned devices.
[0003] Note that in this specification, etc., a semiconductor device refers to any device capable of operating by utilizing the properties of semiconductors. Besides semiconductor elements such as transistors, semiconductor circuits, arithmetic processing devices, and storage devices are also types of semiconductor devices. Sometimes it can be said that display devices (liquid crystal displays, light-emitting displays, etc.), projection devices, lighting devices, electro-optical devices, energy storage devices, storage devices, semiconductor circuits, imaging devices, electronic devices, etc., include semiconductor devices. Background Technology
[0004] In recent years, semiconductor devices have been developed, with LSI (Large Scale Integration), CPU (Central Processing Unit), and memory being the main components used in semiconductor devices. A CPU is an assembly of semiconductor integrated circuits (including at least transistors and memory) that are fabricated from semiconductor wafers into chips and have electrodes formed as connection terminals.
[0005] Semiconductor circuits (IC chips) such as LSI, CPU, and memory are mounted on circuit boards, such as printed circuit boards, and are used as components of various electronic devices.
[0006] Furthermore, the technique of constructing transistors using semiconductor thin films formed on substrates with insulating surfaces has attracted attention. These transistors are widely used in electronic devices such as integrated circuits (ICs) and image display devices (simply referred to as display devices). Silicon-based semiconductor materials are widely known as semiconductor thin films that can be used in transistors. Among other materials, oxide semiconductors have also garnered attention.
[0007] Furthermore, it is known that the leakage current of transistors using oxide semiconductors is extremely small in the non-conducting state. For example, Patent Document 1 discloses a low-power CPU that utilizes the characteristic of low leakage current of transistors using oxide semiconductors. Furthermore, for example, Patent Document 2 discloses a storage device that utilizes the characteristic of low leakage current of transistors using oxide semiconductors to achieve long-term retention of stored content.
[0008] Furthermore, examples of oxide semiconductors that can be used as active layers in transistors include indium oxide and indium gallium zinc oxide. Non-Patent Document 1 discloses a thin-film transistor using hydrogenated polycrystalline indium oxide, formed by low-temperature solid-state crystallization, as the active layer.
[0009] [Preliminary Technology Documents] [Patent Literature] [Patent Document 1] Japanese Patent Application Publication No. 2012-257187 [Patent Document 2] Japanese Patent Application Publication No. 2011-151383 [Non-patent literature] [Non-Patent Literature 1] Y. Magari et al., “High-mobility hydrogenated polycrystalline In2O3 (In2O3:H) thin-film transistors”, Nature COMMUNICATIONS, 13, 1078 (2022). [Non-Patent Literature 2] N. Preissler et al., “Electrical transport, electronothermal transport, and effective electron mass in single-crystalline In2O3 films”, Phys. Rev. B, 88, 085305 (2013). [Non-Patent Literature 3] Takashi Koida, “High Mobility Transparent Conductive Film”, National Institute of Advanced Industrial Science and Technology (AIST), Japan, AIST Solar Power Generation Research Results Presentation 2019, website:<URL:https: / / unit.aist.go.jp / rpd-envene / PV / ja / results / 2019 / oral / T13.pdf> . Summary of the Invention
[0010] The technical problem that the invention aims to solve One objective of this invention is to provide a semiconductor device with high field-effect mobility. Another objective of this invention is to provide a semiconductor device with high operating speed. Another objective of this invention is to provide a semiconductor device with high reliability. Another objective of this invention is to provide a semiconductor device that can be miniaturized or highly integrated. Another objective of this invention is to provide a semiconductor device with good electrical characteristics. Another objective of this invention is to provide a semiconductor device with less non-uniformity in the electrical characteristics of transistors. Another objective of this invention is to provide a semiconductor device with high on-state current. Another objective of this invention is to provide a semiconductor device with low power consumption. Another objective of this invention is to provide a novel semiconductor device. Another objective of this invention is to provide a method for manufacturing a semiconductor device with high productivity. Another objective of this invention is to provide a novel method for manufacturing a semiconductor device.
[0011] Furthermore, one objective of this invention is to provide a storage device that can be miniaturized or highly integrated. Another objective of this invention is to provide a storage device with a large storage capacity. Another objective of this invention is to provide a storage device with a high operating speed. Another objective of this invention is to provide a storage device with low power consumption. Finally, one objective of this invention is to provide a novel storage device.
[0012] Note that the description of these objectives does not preclude the existence of other objectives. One aspect of the invention does not necessarily require achieving all of the above objectives. Objectives other than those described above can be extracted from the description, drawings, and claims.
[0013] means of solving technical problems One aspect of the present invention is a semiconductor device comprising an oxide semiconductor, first to fourth insulators, and first to third conductors. A second insulator is disposed on the first insulator. The oxide semiconductor is disposed on the first insulator and covers the second insulator. The first and second conductors are disposed on the oxide semiconductor. A third insulator is disposed on the first and second conductors and has an opening overlapping the region between the first and second conductors. A fourth insulator is disposed within the opening, overlapping the oxide semiconductor. The third conductor is disposed on the fourth insulator within the opening. In a top view, the side surface of the first insulator is consistent with or substantially consistent with the side surface of the oxide semiconductor, the side surface of the first conductor, and the side surface of the second conductor. The thickness of the first insulator is greater than the thickness of the fourth insulator. In a cross-section along the channel width direction, the height of the second insulator is greater than its width. The oxide semiconductor comprises indium and has a cubic crystal structure. The oxide semiconductor has a first region contacting the side surface of the second insulator and a second region contacting the top surface of the second insulator. The crystal orientation of the grains contained in the first region is consistent with or substantially consistent with the crystal orientation of the grains contained in the second region.
[0014] In the above structure, the oxide semiconductor preferably contains one grain.
[0015] Furthermore, in the above structure, the crystal orientation of the grains contained in the first region and the crystal orientation of the grains contained in the second region are preferably... <111> .
[0016] Furthermore, in the above structure, it is preferable to include a fourth conductor on the first insulator, the fourth conductor being covered by the second insulator.
[0017] Furthermore, in the above structure, it is preferable that, when viewed from above, a portion of the side of the third insulator is consistent with or substantially consistent with the side of the first conductor and the side of the second conductor.
[0018] Furthermore, in the above structure, the bottom surface of the third conductor preferably has a portion located below the bottom surface of the oxide semiconductor.
[0019] Furthermore, in the above structure, it is preferable to further include a fifth insulator. Both the first conductor and the second conductor include a first conductive layer and a second conductive layer on the first conductive layer. The fifth insulator is disposed within the opening of the third insulator and contacts the top surface of the first conductive layer of the first conductor, the side surface of the second conductive layer of the first conductor, the top surface of the first conductive layer of the second conductor, and the side surface of the second conductive layer of the second conductor. The fifth insulator has an opening that overlaps with the area between the first conductive layer of the first conductor and the first conductive layer of the second conductor. The shortest distance between the first conductive layer of the first conductor and the first conductive layer of the second conductor is smaller than the shortest distance between the second conductive layer of the first conductor and the second conductive layer of the second conductor.
[0020] Furthermore, in the above structure, it is preferable that, when viewed from above, a portion of the side surface of the third insulator is consistent with or substantially consistent with the side surface of the second conductive layer of the first conductor and the side surface of the second conductive layer of the second conductor.
[0021] In addition, in the above structure, the fifth insulator preferably comprises silicon nitride.
[0022] Furthermore, in the above structure, the first conductive layer of the first conductor and the first conductive layer of the second conductor preferably comprise tantalum nitride.
[0023] Invention Effects According to one aspect of the present invention, a semiconductor device with high field-effect mobility can be provided. Additionally, according to one aspect of the present invention, a semiconductor device with high operating speed can be provided. Furthermore, according to one aspect of the present invention, a semiconductor device with high reliability can be provided. Furthermore, according to one aspect of the present invention, a semiconductor device capable of miniaturization or high integration can be provided. Furthermore, according to one aspect of the present invention, a semiconductor device with good electrical characteristics can be provided. Furthermore, according to one aspect of the present invention, a semiconductor device with less non-uniformity in the electrical characteristics of the transistor can be provided. Furthermore, according to one aspect of the present invention, a semiconductor device with high on-state current can be provided. Furthermore, according to one aspect of the present invention, a semiconductor device with low power consumption can be provided. Furthermore, according to one aspect of the present invention, a novel semiconductor device can be provided. Furthermore, according to one aspect of the present invention, a method for manufacturing a semiconductor device with high productivity can be provided. Furthermore, according to one aspect of the present invention, a novel method for manufacturing a semiconductor device can be provided.
[0024] Furthermore, according to one aspect of the present invention, a storage device capable of miniaturization or high integration can be provided. Additionally, according to one aspect of the present invention, a storage device with large storage capacity can be provided. Furthermore, according to one aspect of the present invention, a storage device with high operating speed can be provided. Furthermore, according to one aspect of the present invention, a storage device with low power consumption can be provided. Furthermore, according to one aspect of the present invention, a novel storage device can be provided.
[0025] Note that the description of these effects does not preclude the existence of other effects. One aspect of the invention does not necessarily require all of the aforementioned effects. Effects other than those described above can be extracted from the specification, drawings, and claims. Attached Figure Description
[0026] Figure 1A This is a plan view showing an example of a semiconductor device. Figures 1B to 1D This is a cross-sectional view showing an example of a semiconductor device.
[0027] Figure 2A and Figure 2B This is a cross-sectional view showing an example of a semiconductor device.
[0028] Figure 3A This is a cross-sectional view illustrating the indium oxide film. Figure 3B and Figure 3C This is a graph illustrating the carrier concentration for Hall mobility.
[0029] Figure 4 This is a graph illustrating the carrier concentration dependence of the indium oxide mobility disclosed in Non-Patent Document 2.
[0030] Figures 5A to 5C This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor device.
[0031] Figures 6A to 6E It is a diagram illustrating the crystal structure of metal oxides.
[0032] Figures 7A to 7C This is a three-dimensional schematic diagram illustrating an example of a method for manufacturing a semiconductor device.
[0033] Figure 8A and Figure 8B This is a cross-sectional view showing an example of a semiconductor device. Figure 8C This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor device.
[0034] Figure 9A and Figure 9B This is a cross-sectional view showing an example of a semiconductor device.
[0035] Figure 10Aand Figure 10B This is a cross-sectional view showing an example of a semiconductor device.
[0036] Figures 11A to 11C This is a cross-sectional view showing an example of a semiconductor device.
[0037] Figures 12A to 12C This is a cross-sectional view showing an example of a semiconductor device.
[0038] Figures 13A to 13C This is a cross-sectional view showing an example of a semiconductor device.
[0039] Figure 14A and Figure 14B This is a cross-sectional view showing an example of a semiconductor device.
[0040] Figure 15A This is a plan view showing an example of a semiconductor device. Figures 15B to 15D This is a cross-sectional view showing an example of a semiconductor device.
[0041] Figure 16A This is a plan view showing an example of a semiconductor device. Figures 16B to 16D This is a cross-sectional view showing an example of a semiconductor device.
[0042] Figure 17A This is a plan view showing an example of a semiconductor device. Figures 17B to 17D This is a cross-sectional view showing an example of a semiconductor device.
[0043] Figure 18A and Figure 18B This is a cross-sectional view showing an example of a semiconductor device.
[0044] Figures 19A to 19C This is a cross-sectional view showing an example of a semiconductor device.
[0045] Figure 20A and Figure 20B This is a cross-sectional view showing an example of a semiconductor device.
[0046] Figure 21A This is a plan view illustrating an example of a method for manufacturing a semiconductor device. Figures 21B to 21D This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor device.
[0047] Figure 22A This is a plan view illustrating an example of a method for manufacturing a semiconductor device. Figures 22B to 22D This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor device.
[0048] Figure 23A This is a plan view illustrating an example of a method for manufacturing a semiconductor device. Figures 23B to 23D This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor device.
[0049] Figure 24A This is a plan view illustrating an example of a method for manufacturing a semiconductor device. Figures 24B to 24D This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor device.
[0050] Figure 25A This is a plan view illustrating an example of a method for manufacturing a semiconductor device. Figures 25B to 25D This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor device.
[0051] Figure 26A This is a plan view illustrating an example of a method for manufacturing a semiconductor device. Figures 26B to 26D This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor device.
[0052] Figure 27A This is a plan view illustrating an example of a method for manufacturing a semiconductor device. Figures 27B to 27D This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor device.
[0053] Figure 28A This is a plan view illustrating an example of a method for manufacturing a semiconductor device. Figures 28B to 28D This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor device.
[0054] Figure 29A This is a plan view illustrating an example of a method for manufacturing a semiconductor device. Figures 29B to 29D This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor device.
[0055] Figure 30A This is a plan view illustrating an example of a method for manufacturing a semiconductor device. Figures 30B to 30D This is a cross-sectional view illustrating an example of a method for manufacturing a semiconductor device.
[0056] Figure 31 This is a block diagram illustrating an example of the structure of a semiconductor device.
[0057] Figures 32A to 32H This is a diagram illustrating an example of the circuit structure of a memory cell.
[0058] Figure 33A and Figure 33B This is a three-dimensional diagram illustrating an example of the structure of a semiconductor device.
[0059] Figure 34 This is a block diagram illustrating the CPU.
[0060] Figure 35A and Figure 35B It is a 3D diagram of a semiconductor device.
[0061] Figure 36A and Figure 36B It is a 3D diagram of a semiconductor device.
[0062] Figure 37 This is a schematic diagram illustrating the hierarchy of storage devices.
[0063] Figure 38A and Figure 38B This is a diagram illustrating an example of an electronic device. Figures 38C to 38E This is a diagram illustrating an example of a large computer.
[0064] Figure 39 This is a diagram illustrating an example of a space device.
[0065] Figure 40 This is a diagram illustrating an example of a storage system that can be used in a data center.
[0066] Figure 41A and Figure 41B This is an example of the structure of a display device.
[0067] Figure 42 This is an example of the structure of a display device.
[0068] Figure 43 This is an example of the structure of a display device.
[0069] Figure 44 This is an example of the structure of a display device.
[0070] Figures 45A to 45D This is an example of the structure of a display device.
[0071] Figure 46A and Figure 46B This is an example of the structure of a display device.
[0072] Figure 47A and Figure 47B This is a diagram illustrating an example of the structure of a display device.
[0073] Figures 48A to 48D This is a diagram illustrating an example of the structure of a display device.
[0074] Figures 49A to 49D This is a diagram illustrating an example of the structure of a display device.
[0075] Figure 50 This is a diagram illustrating an example of the structure of a display device.
[0076] Figures 51A to 51F This is an example of the structure of an electronic device.
[0077] Figures 52A to 52FThis is an example of the structure of an electronic device.
[0078] Figures 53A to 53G This is an example of the structure of an electronic device. Detailed Implementation
[0079] The embodiments will be described in detail with reference to the accompanying drawings. Note that the present invention is not limited to the following description, and those skilled in the art will readily understand that its methods and details can be varied in many ways without departing from the spirit and scope of the invention. Therefore, the present invention should not be construed as being limited only to the contents described in the embodiments shown below.
[0080] Note that in the structure of the invention described below, the same symbols are used in different figures to represent the same parts or parts with the same function, and repeated descriptions are omitted. Furthermore, when representing parts with the same function, the same shading lines are sometimes used without additional symbols.
[0081] Furthermore, for ease of understanding, the positions, sizes, and extents of the constituent elements shown in the accompanying drawings may not represent their actual positions, sizes, and extents. Therefore, the disclosed invention is not necessarily limited to the positions, sizes, and extents disclosed in the accompanying drawings.
[0082] Furthermore, especially in top views (also known as "plan views") or perspective views, descriptions of some constituent elements are sometimes omitted to facilitate understanding of the invention. Additionally, descriptions of some hidden lines are sometimes omitted.
[0083] Note that, for convenience, ordinal numbers such as "first" and "second" are used in this specification, etc., but these do not limit the number of constituent elements or the order of the constituent elements (e.g., process sequence or stacking sequence). Furthermore, the ordinal numbers used for constituent elements in one part of this specification may sometimes differ from those used for the same constituent element in other parts of this specification or in the claims.
[0084] Furthermore, depending on the circumstances, the "film" and "layer" can be interchanged. For example, a "conductive layer" can be replaced with a "conductive film." Or, for example, an "insulating film" can be replaced with an "insulating layer." Additionally, depending on the circumstances, a "conductor" can be replaced with a "conductive layer" or a "conductive film." Furthermore, depending on the circumstances, an "insulator" can be replaced with an "insulating layer" or an "insulating film."
[0085] Furthermore, in this specification, "parallel" refers to a state where the angle formed by two straight lines is between -10 degrees and 10 degrees. Therefore, it also includes a state where the angle is between -5 degrees and 5 degrees. Additionally, "approximately parallel" refers to a state where the angle formed by two straight lines is between -20 degrees and 20 degrees. Furthermore, "perpendicular" refers to a state where the angle formed by two straight lines is between 80 degrees and 100 degrees. Therefore, it also includes a state where the angle is between 85 degrees and 95 degrees. Additionally, "approximately perpendicular" refers to a state where the angle formed by two straight lines is between 70 degrees and 110 degrees.
[0086] Openings include, for example, grooves and slits. Furthermore, the area where an opening is formed is sometimes referred to as an opening portion.
[0087] Furthermore, the accompanying drawings used in this specification show the case where the sidewall of the insulator in the opening of the insulator is perpendicular or substantially perpendicular to the substrate surface or the surface to which it is formed, but the sidewall may also be tapered.
[0088] Note that in this specification, a conical shape refers to a shape in which at least a portion of the side surface of a constituent element is inclined relative to the substrate surface or the surface to be formed. For example, it is preferable to have a region where the angle (hereinafter sometimes referred to as the cone angle) formed by the inclined side surface and the substrate surface or the surface to be formed is less than 90°. Note that the side surface of the constituent element and the substrate surface do not necessarily have to be completely flat; they may also be approximately planar with slight curvature or approximately planar with slight irregularities.
[0089] Note that in this specification, "height consistent or substantially consistent" refers to a structure that is at the same height as a reference surface (e.g., a flat surface such as a substrate surface) when viewed in cross-section. For example, in the manufacturing process of memory devices, sometimes a planarization process (typically using chemical mechanical polishing (CMP)) exposes the surfaces of one or more layers. In this case, the CMP-treated surface has a structure at the same height as the reference surface. Note that depending on the processing apparatus, processing method, or material of the treated surface during CMP processing, the heights of multiple layers may differ. In this specification, "height consistent or substantially consistent" also includes this case. For example, in the case of layers with two heights relative to a reference surface (here, the first layer and the second layer), when the difference between the height of the top surface of the first layer and the height of the top surface of the second layer is less than 20 nm, it is also referred to as "height consistent or substantially consistent".
[0090] In this specification, "side-end consistency or substantially consistency" means that at least a portion of the contours of stacked layers overlap when viewed from above. For example, this includes cases where the upper and lower layers are processed using the same mask pattern or a portion thereof. However, there are actually cases where the contours do not overlap; sometimes the contour of the upper layer is inside the contour of the lower layer, or the contour of the upper layer is outside the contour of the lower layer. In such cases, it can also be said that the contours are "side-end consistency or substantially consistency".
[0091] In this specification, "consistent or substantially consistent planar shapes" means that at least a portion of the outlines of stacked layers overlap. For example, this means that the upper and lower layers are processed using the same mask pattern or a portion thereof. However, in reality, there are cases where the outlines do not overlap; sometimes the upper layer is positioned inside or outside the lower layer, and in these cases, it can also be said that the planar shapes are "consistent or substantially consistent." Furthermore, when planar shapes are consistent or substantially consistent, it can also be said that the ends are aligned or substantially aligned, or that the side ends are consistent or substantially consistent.
[0092] In this specification and other materials, the cubic crystal system is sometimes referred to as cubic crystal, cubic crystal structure, etc. The same applies to other crystal systems (hexagonal, trigonal, tetragonal, orthorhombic, monoclinic, triclinic).
[0093] (Implementation Method 1) In this embodiment, using Figures 1A to 30D The invention describes a semiconductor device including an oxide semiconductor layer and a method for manufacturing the semiconductor device.
[0094] <Examples of semiconductor device structures> use Figures 1A to 20B Illustrate the structure of a semiconductor device using examples. Figures 1A to 1D This is a top view and a cross-sectional view of a semiconductor device including transistor 200 on a substrate (not shown).
[0095] Figure 1A This is a top view of the aforementioned semiconductor device. Additionally, Figures 1B to 1D This is a cross-sectional view of the semiconductor device. Here, Figure 1B It is along Figure 1A The cross-sectional view of the section marked with dotted lines A1-A2 is also a cross-sectional view of the transistor 200 along the channel width direction. Furthermore, Figure 1C It is along Figure 1A The cross-sectional view of the section with dotted lines A3-A4 is also a cross-sectional view of the transistor 200 in the channel width direction. Figure 1D It is along Figure 1AThe cross-sectional view of the section marked with dotted lines A5-A6 is also a cross-sectional view along the channel length of transistor 200. Here, dotted lines A5-A6 are orthogonal to dotted lines A1-A2 and A3-A4, and dotted lines A1-A2 and A3-A4 are parallel to each other. Note that in Figure 1A In the top view, for clarity, some constituent elements are omitted and shown transparently. Additionally, Figure 2A Show Figure 1D A magnified view of the conductor around 260. Additionally, Figure 2B Show Figure 1B A magnified view of the area near oxide semiconductor 230. Additionally, Figure 13A Show Figure 1C An enlarged view of the area near oxide semiconductor 230. Note that in this specification, etc., the representation of a "cross section in the channel width direction" does not necessarily include the channel formation region of the transistor. The representation of a "cross section in the channel width direction" sometimes includes a cross section parallel to the cross section in the channel width direction that includes the channel formation region.
[0096] The semiconductor device according to this embodiment includes an insulator 216 on a substrate (not shown), an insulator 221 on the insulator 216, an insulator 222 on the insulator 221, an insulator 224 on the insulator 222, an insulator 225 on the insulator 224, an oxide semiconductor 230 on the insulator 224 and the insulator 225, conductors 242a (conductors 242a1 and 242a2) and conductors 242b (conductors 242b1 and 242b2) on the oxide semiconductor 230, an insulator 250 on the oxide semiconductor 230, and conductors 260 (conductors 260a and 260b) on the insulator 250. Furthermore, an insulator 255 is disposed between the insulator 222, conductors 242a1, 242b1, 242a2, 242b2, insulator 275, and insulator 280 and the insulator 250. Hereinafter, conductors 242a and 242b will sometimes be referred to as conductor 242.
[0097] An insulator 275 is provided on the conductor 242 and the insulator 222, and an insulator 280 is provided on the insulator 275. An opening 201 is provided in both the insulator 280 and the insulator 275. The side surfaces of the insulator 280 and the insulator 275 serve as sidewalls of the opening 201. Additionally, the side surfaces of the conductors 242a1, 242a2, 242b1, and 242b2 can also serve as sidewalls of the opening 201. Insulators 250 and 255, and conductor 260 are disposed inside the opening 201. Furthermore, insulators 224 and 225, and a portion of the oxide semiconductor 230 are also disposed inside the opening 201. Figure 1B As shown, opening 201 reaches oxide semiconductor 230 and insulator 222, and insulator 250 contacts oxide semiconductor 230 and insulator 222 in opening 201.
[0098] Here, an opening is formed on the bottom surface of the insulator 255, which overlaps with the area between the conductors 242a1 and 242b1. (See cross-sectional view in the channel width direction). Figure 1B The opening of the insulator 255 contains the insulator 224, the insulator 225, and the oxide semiconductor 230. The insulator 255 is disposed along the sidewall and bottom surface of the opening 201, so the insulator 255 can also be regarded as part of the sidewall and bottom surface of the opening 201.
[0099] An insulator 282 is provided on the insulator 280 and the conductor 260. Furthermore, an insulator 283 is provided on the insulator 282. Additionally, an insulator 215 is provided below the insulator 216.
[0100] An insulator 241a is provided in contact with the inner wall of an opening in an insulator 280, etc., and a conductor 240a is provided in contact with the side of the insulator 241a. The bottom surface of the conductor 240a is in contact with the top surface of the conductor 242a. An insulator 241b is provided in contact with the inner wall of an opening in an insulator 280, etc., and a conductor 240b is provided in contact with the side of the insulator 241b. The bottom surface of the conductor 240b is in contact with the top surface of the conductor 242b. Hereinafter, conductors 240a and 240b are sometimes referred to together as conductor 240. In addition, insulators 241a and 241b are sometimes referred to together as insulator 241.
[0101] The oxide semiconductor 230 has a region that serves as the channel formation region of the transistor 200. Additionally, the conductor 260 has a region that serves as the first gate electrode (upper gate electrode) of the transistor 200. The insulator 250 has a region that serves as the first gate insulator of the transistor 200.
[0102] Conductor 242a has a region that serves as one of the source and drain electrodes of transistor 200. Conductor 240a is used as a connector to conductor 242a. Conductor 242b has a region that serves as the other of the source and drain electrodes of transistor 200. Conductor 240b is used as a connector to conductor 242b.
[0103] Conductor 242a has a stacked structure of conductor 242a1 and conductor 242a2 on conductor 242a1, and conductor 242b has a stacked structure of conductor 242b1 and conductor 242b2 on conductor 242b1. Conductors 242a1 and 242b1 in contact with the oxide semiconductor 230 are preferably conductors that are not easily oxidized, such as metal nitrides. This prevents over-oxidation of conductors 242a and 242b due to oxygen in the oxide semiconductor 230. Furthermore, conductors 242a2 and 242b2 are preferably conductors such as metal layers having higher conductivity than conductors 242a1 and 242b1. This allows conductors 242a and 242b to be used as wiring or electrodes with high conductivity. Thus, a semiconductor device can be provided in which conductors 242a and 242b, which serve as wiring or electrodes, are disposed in contact with the top surface of an oxide semiconductor 230, which serves as an active layer.
[0104] like Figure 2A As shown, when viewed in cross-section along the channel length of transistor 200, the distance D1 between conductors 242a1 and 242b1 is less than the distance D2 between conductors 242a2 and 242b2. Here, distance D2 refers to the shortest distance between the opposing sides of conductors 242a2 and 242b2. Conversely, distance D1 refers to the shortest distance between the opposing sides of conductors 242a1 and 242b1. By employing this structure, the distance between the source and drain can be further shortened, and the channel length can be correspondingly reduced. Therefore, the frequency characteristics of transistor 200 can be improved. Thus, by reducing the channel length of the semiconductor device, a semiconductor device with high operating speed can be provided.
[0105] The opening 201 overlaps with the region between conductors 242a1 and 242b2. Alternatively, it can be viewed that a portion of conductors 242a1 and 242b1 is formed protruding into the opening 201. Furthermore, it can be said that a portion of conductors 242a1 and 242b1 is formed protruding from the outer edge of the opening 201 and overlapping with it. Therefore, the insulator 255 contacts the top surface of conductors 242a1, the top surface of conductors 242b1, the side surface of conductors 242a2, and the side surface of conductors 242b2 within the opening 201. Additionally, the insulator 250 contacts the top surface of insulator 222 and the top surface of oxide semiconductor 230 in the region between conductors 242a1 and 242b1.
[0106] The insulator 255 is preferably an insulator that is not easily oxidized, such as a nitride. The insulator 255 is formed in contact with the sides of the conductors 242a2 and 242b2, and functions to protect the conductors 242a2 and 242b2. Preferably, heat treatment is performed in an oxygen-containing atmosphere after the conductors 242a1 and 242b1 are separated and before the insulator 250 is deposited; details of this will be explained later. At this time, since the insulator 255 is formed in contact with the sides of the conductors 242a2 and 242b2, excessive oxidation of the conductors 242a2 and 242b2 can be prevented.
[0107] The oxide semiconductor 230 is formed by covering the insulator 225. For example... Figure 2B and Figure 13A As shown, the insulator 225 has a high aspect ratio when viewed in cross-section along the channel width direction. Therefore, the insulator 225 can also be described as having a fin-like shape. Here, the aspect ratio of the insulator 225 when viewed in cross-section along the channel width direction refers to the ratio of the length L of the insulator 225 in the A1-A2 direction (also referred to as the width L of the insulator 225) to the length H (also referred to as the height H of the insulator 225) in the direction perpendicular to the surface to which the insulator 225 is formed (e.g., insulator 224). The aspect ratio of the insulator 225 is preferably as large as possible within the range that the insulator 225 will not collapse during the manufacturing process of the transistor 200. The height H of the insulator 225 is preferably greater than the width L of the insulator 225.
[0108] An oxide semiconductor 230 and a conductor 242 are disposed such that they cover an insulator 225 with a high aspect ratio. Near the channel formation region of the transistor 200, such as... Figure 2BAs shown, the oxide semiconductor 230 is disposed in a folded state, sandwiching the insulator 225. Therefore, when viewed in cross-section along the channel width direction, the oxide semiconductor 230 and the conductor 260 are disposed opposite each other, separated by the insulator 250, on the upper part of the insulator 225, the side surface on the A1 side, the side surface on the A2 side, and near the insulator 224. In other words, the upper part of the oxide semiconductor 230, the side surface on the A1 side, the side surface on the A2 side, and the vicinity of the insulator 224 are all used as channel forming regions. Therefore, compared to a planar transistor without the insulator 225, the channel width of the transistor 200 exceeds the portion of the side surface on the A1 side and the side surface on the A2 side of the oxide semiconductor 230.
[0109] Thus, by increasing the channel width, the on-state current, transconductance, and frequency characteristics of the transistor 200 can be improved. This provides a semiconductor device with a high operating speed. Furthermore, the operating speed of a memory device using this semiconductor device can be increased. Additionally, in the above structure, by providing the oxide semiconductor 230 in a manner that covers the insulator 225, the channel width can be increased without making the occupied area of the transistor 200 excessively large. This allows for miniaturization or high integration of the semiconductor device. Furthermore, the storage capacity of a memory device using this semiconductor device can be increased. Moreover, by adopting the above structure, the area of the opposing sides of the conductor 260 and the oxide semiconductor 230 is increased, thus allowing for threshold control to keep the transistor 200 in a normally off state.
[0110] Furthermore, such as Figure 2B As shown, the thickness t1 of the insulator 224 within the opening 201 is preferably greater than the thickness t2 of the insulator 250. By employing this structure, the bottom surface (also referred to as the lower end or lower end portion) of the conductor 260, located in the region within the opening 201 that does not overlap with the oxide semiconductor 230, is located below the bottom surface (also referred to as the lower end or lower end portion) of the oxide semiconductor 230. Therefore, a sufficient electric field can be applied from the conductor 260 to the upper end portion to the lower end portion of the oxide semiconductor 230. This reduces the leakage current between the source and drain electrodes at the lower end portion of the oxide semiconductor 230. Furthermore, it suppresses characteristic defects in the transistor caused by this leakage current, such as constant-on behavior. In other words, the electrical characteristics of the transistor 200 can be improved.
[0111] The oxide semiconductor 230 has a channel formation region. The oxide semiconductor 230 also has a source region and a drain region. The source and drain regions are n-type regions (low-resistance regions) with a higher carrier concentration than the channel formation region. The oxide semiconductor 230 can be a single-layer structure or a stacked structure of two or more layers.
[0112] Transistor 200 contains a metal oxide serving as a semiconductor within an oxide semiconductor 230, including a channel formation region. Hereinafter, a transistor like transistor 200, with its channel formed in an oxide semiconductor, is sometimes referred to as an OS transistor. In contrast, a transistor with a silicon channel formation region is sometimes described as a Si transistor. Furthermore, in this specification, since the oxide semiconductor 230 contains a metal oxide, it can be referred to as a metal oxide layer.
[0113] In an OS transistor, when oxygen vacancies (V0) exist in the channel formation region of the oxide semiconductor... O When oxygen vacancies and impurities are present, the electrical properties are prone to change, which may reduce reliability. Therefore, in the channel formation region of an oxide semiconductor, it is preferable to minimize oxygen vacancies and impurities. In other words, it is preferable that the carrier concentration in the channel formation region of the oxide semiconductor is reduced and intrinsically or substantially eigentyped.
[0114] Furthermore, when an excessive amount of oxygen is supplied to the oxide semiconductor 230, electron traps caused by the excess oxygen form in the insulator 250. Consequently, in the OS transistor, forward drift degradation during +GBT (Gate Bias-Temperature) stress testing is more likely to occur. In other words, the amount of forward drift degradation during +GBT stress testing increases.
[0115] Therefore, in one aspect of the semiconductor device of the present invention, the impurity concentration in the oxide semiconductor 230 is preferably low. Furthermore, it is preferable to supply an appropriate amount of oxygen to the oxide semiconductor 230. Additionally, it is preferable to reduce the amount of excess oxygen in the oxide semiconductor 230.
[0116] The oxide semiconductor 230 preferably uses indium oxide. In this case, the oxide semiconductor 230 contains indium and oxygen. For example, the oxide semiconductor 230 preferably includes an indium oxide film. In metal oxides, the higher the proportion of indium atoms in the total number of atoms of all metal elements, the higher the field-effect mobility of the transistor. Therefore, by using indium oxide in the oxide semiconductor 230, the transistor can achieve large on-state current and high frequency characteristics.
[0117] Furthermore, the indium oxide film preferably has crystallinity. For example, the indium oxide film preferably contains grains. Examples of films containing grains include monocrystalline films, polycrystalline films, and amorphous films containing grains. It can be considered that polycrystalline films are composed of two or more grains, while monocrystalline films are composed of one grain. Grain boundaries (also called grain boundaries) are observed in polycrystalline films, but not in monocrystalline films.
[0118] Note that, unlike polycrystalline films, grain boundaries are not observed in the channel formation region of monocrystalline films. Impurities that impede carrier flow (typically insulating impurities, insulating oxides, etc.) tend to segregate at grain boundaries. Therefore, the presence of grain boundaries in the channel formation region increases the inhomogeneity of transistor characteristics. On the other hand, in a monocrystalline film according to one embodiment of the present invention, grain boundaries are not observed in the channel formation region, thus exhibiting the excellent effect of suppressing inhomogeneities in transistor characteristics caused by these grain boundaries.
[0119] Furthermore, in this specification, a semiconductor layer in which no crystal boundary is observed in the channel formation region, a semiconductor layer in which the channel formation region is included in a single grain, or a semiconductor layer in which the crystal axis orientation is the same in at least two regions of the channel formation region, may be referred to as a single crystal film. Alternatively, a semiconductor layer in which at least one crystal orientation is oriented in the same direction in the channel formation region may be referred to as a single crystal film.
[0120] Note that the channel formation region refers to the region in the semiconductor layer that overlaps (or is opposite) to the gate electrode across the gate insulating layer, and specifically refers to the region located between the region contacting the source electrode and the region contacting the drain electrode. Note that the following semiconductor layers can also be referred to as single-crystal films: semiconductor layers in which no grains are observed in the region between the region contacting the source electrode and the region contacting the drain electrode; semiconductor layers in which the region between the region contacting the source electrode and the region contacting the drain electrode is contained within a single grain; or semiconductor layers in which at least two regions in the region between the region contacting the source electrode and the region contacting the drain electrode have the same crystal axis orientation. Alternatively, a semiconductor layer in which at least one crystal orientation in the region between the region contacting the source electrode and the region contacting the drain electrode is oriented in the same direction can be referred to as a single-crystal film.
[0121] Note that the current path in the channel formation region is the shortest distance between the source electrode and the drain electrode. Therefore, by observing the cross-section including the semiconductor layer, the source electrode, and the drain electrode, the grains, grain boundaries, grain axes, crystal orientations, etc., in the aforementioned channel formation region or the region between the source electrode and the drain electrode can be identified.
[0122] The crystallinity of oxide semiconductor 230 can be analyzed, for example, by X-ray diffraction (XRD), transmission electron microscopy (TEM), or electron diffraction (ED). Alternatively, a combination of the above methods can be used for analysis.
[0123] For example, grains can be observed in high-resolution transmission electron microscopy (TEM) images. Furthermore, grain boundaries can sometimes be observed in high-resolution TEM images, for example. That is, grains and grain boundaries can sometimes be observed in high-resolution TEM images of crystalline films. Note that the total magnification when obtaining the TEM image is preferably 2 million times or more, more preferably 4 million times or more.
[0124] Indium oxide films are more preferably single-crystal. Since single crystals lack grain boundaries, carrier scattering at grain boundaries can be suppressed, thereby enabling transistors with high field-effect mobility. Furthermore, transistors with high reliability can be achieved.
[0125] The indium oxide film can also be polycrystalline or amorphous, containing grains. In this case, it is preferable that no grain boundaries are observed or that the grain boundary content is low in the channel formation region. For example, by placing a single grain in the channel formation region, a structure in which no grain boundaries are observed in the channel formation region can be achieved. This structure can also perform the same function as a single-crystal indium oxide film.
[0126] Furthermore, two or more grains can be located in the channel forming region. For example, when the first grain and the second grain are located in the channel forming region, the crystal orientation of the first grain is preferably the same as or substantially the same as the crystal orientation of the second grain. When the crystal orientation of the first grain is the same as or substantially the same as the crystal orientation of the second grain, sometimes no grain boundary is observed at the boundary between the first grain and the second grain. By making the crystal orientation of the first grain the same as or substantially the same as the crystal orientation of the second grain, the formation of grain boundaries between the first grain and the second grain can be suppressed. Therefore, the same effect as the structure where the indium oxide film is a single crystal can be achieved in this structure. For example, sometimes the crystal orientation of the first grain is the same as or substantially the same as the crystal orientation of the second grain can be observed in high-resolution TEM images. Specifically, in high-resolution TEM images, the lattice fringes of the first grain and the second grain are continuously connected at the boundary between the first grain and the second grain.
[0127] Note that in this specification, a grain boundary refers, for example, to the boundary between adjacent grains with different crystal orientations. Therefore, in this specification, the boundary between adjacent grains with the same crystal orientation is not included in the term grain boundary. For example, even if the boundary between two grains is observed in a high-resolution TEM image, it is sometimes not referred to as a grain boundary when the crystal orientations of the two grains are consistent or substantially consistent.
[0128] Furthermore, crystal orientation can be evaluated using diffraction patterns observed by nanobeam electron diffraction (NBED). Alternatively, crystal orientation can also be evaluated using patterns obtained by performing a Fast Fourier Transform (FFT) on a TEM image (also known as FFT patterns). FFT patterns reflect the same reciprocal space information as the diffraction patterns described above.
[0129] For example, in each FFT pattern of the first grain and the second grain, when the angle difference between their FFT patterns is -5 degrees or more and 5 degrees or less, preferably -3 degrees or more and 3 degrees or less, and more preferably -2 degrees or more and 2 degrees or less, it can be said that the crystal orientation of the first grain and the crystal orientation of the second grain are consistent or approximately consistent. Note, for example, the angle of the FFT pattern in the orientation
[111] refers to the acute angle formed by the approximate straight line between the spot originating from the (222) plane and the spot originating from the (-2-2-2) plane and the center spot and the reference line (e.g., a straight line extending in the vertical direction).
[0130] The polycrystalline degree of indium oxide films can be evaluated based on the grain size. The grain size can be calculated, for example, by calculating the grain area, assuming a circle corresponding to that area, and using the diameter of that circle as the grain size. This diameter is sometimes referred to as the equivalent circular area diameter, etc.
[0131] Furthermore, the polycrystalline nature of indium oxide films can be evaluated based on the elongation length of grain boundaries. The elongation length of grain boundaries can be calculated, for example, by extracting a specific area of field of view from a TEM image of the film obtained at a total magnification sufficient to observe the grain boundaries, and using the sum of the lengths of the grain boundaries observed in that field of view as the elongation length. An indium oxide film with an elongation length of 0 nm can be considered a single crystal. This also implies that the longer the elongation length of the grain boundaries, the greater the grain boundary composition.
[0132] The elongation length of grain boundaries in the indium oxide film is preferably 0 nm or more and 1500 nm or less, more preferably 0 nm or more and 1000 nm or less, and even more preferably 0 nm or more and 800 nm or less. By using an indium oxide film with an elongation length of grain boundaries within the above-mentioned range in the oxide semiconductor 230, a structure in which no grain boundaries are observed or where the grain boundary composition is low can be achieved. Note that, unless otherwise specified in this specification, the field of view used for calculating the elongation length of grain boundaries is 90 nm squared.
[0133] The thickness of the oxide semiconductor 230 is preferably 2 nm or more and 50 nm or less, more preferably 2.5 nm or more and 30 nm or less, even more preferably 2.5 nm or more and 20 nm or less, even more preferably 5 nm or more and 20 nm or less, and even more preferably 5 nm or more and 10 nm or less. Furthermore, at least a portion of the oxide semiconductor 230 may have the aforementioned thickness. For example, a region with the aforementioned thickness in the channel formation region of the oxide semiconductor 230 may be sufficient. Increasing the thickness of the oxide semiconductor 230 can increase the on-state current of the transistor. On the other hand, when the thickness of the oxide semiconductor 230 is too large, the grain boundary elongation length increases, and the on-state current of the transistor may decrease due to the scattering of charge carriers at the grain boundaries. Conversely, decreasing the thickness of the oxide semiconductor 230 can suppress the decrease in threshold voltage, thereby enabling a normally-off transistor. On the other hand, when the thickness of the oxide semiconductor 230 is too small, the non-uniform crystallinity of the oxide semiconductor 230 within the substrate surface may lead to non-uniform electrical characteristics of the transistor. Therefore, by setting the thickness of the oxide semiconductor 230 within the aforementioned range, the crystallinity of the oxide semiconductor 230 can be improved. By improving the crystallinity of the oxide semiconductor 230, the oxide semiconductor 230 can contain grains.
[0134] Furthermore, when metal oxides contain indium and zinc, they sometimes exhibit a CAAC (c-axis aligned crystalline) structure. CAAC structures have fewer grain boundaries on the ab plane than polycrystalline structures. Examples of metal oxides containing indium and zinc include indium zinc oxide (also known as In-Zn oxide, IZO (registered trademark)) and indium gallium zinc oxide (also known as In-Ga-Zn oxide, IGZO).
[0135] In a crystalline oxide semiconductor layer, an indium oxide film, for example, is a film in which hydrogen and oxygen migrate more readily than an IGZO film. Therefore, an indium oxide film can be considered, for example, a film in which hydrogen and oxygen are more readily supplied and discharged than an IGZO film. Furthermore, an indium oxide film can be considered, for example, a film with higher permeability to hydrogen and oxygen than an IGZO film. In other words, an indium oxide film can be considered, for example, a film with lower barrier properties to hydrogen and oxygen than an IGZO film.
[0136] The indium oxide film preferably has the following properties: in a heat treatment at a heating temperature of 400°C and a treatment time of 8 hours, for example, 1×10 20 atoms / cm 3 Above and 2×10 21 atoms / cm 3 Oxygen permeability within the following range is preferably 2×1020 atoms / cm 3 Above and 1×10 21 atoms / cm 3 Oxygen permeability within the following range. Furthermore, the indium oxide film preferably possesses the following properties: [e.g., 1×10⁻⁶] [This refers to a specific heat treatment process, e.g., heat treatment at 400°C for 8 hours, resulting in a film with a permeability of 1×10⁻⁶]. 20 atoms / cm 3 Above and 2×10 21 atoms / cm 3 The following is preferred: 2×10 20 atoms / cm 3 Above and 1×10 21 atoms / cm 3 Oxygen diffuses within the grains within the following range.
[0137] By allowing oxygen in the indium oxide film to diffuse through grains and grain boundaries, the amount of V present in grains or grain boundaries can be reduced. O Therefore, the electrical characteristics and reliability of transistors can be improved.
[0138] Furthermore, the permeability of the membrane to oxygen and hydrogen can be evaluated, for example, using calculations based on the NEB (Nudged elastic band) method. Specifically, this can be evaluated by calculating the migration barriers of oxygen and hydrogen atoms using the NEB method. In other words, the smaller the migration barrier value, the easier it is for the atom to migrate (the easier it is to permeate).
[0139] Table 1 shows an example of the calculation results. The In₂O₃ shown in Table 1 is the crystal model of indium oxide, and the IGZO shown is the crystal model of In-Ga-Zn oxide. Note that the excess oxygen shown in Table 1 refers to oxygen not located at lattice positions or oxygen located between lattice points.
[0140] [Table 1] Table 1 shows that the migration barriers for oxygen, hydrogen, and excess oxygen are large in the In-Ga-Zn oxide crystal model but small in the indium oxide crystal model. This indicates that oxygen and hydrogen migrate more easily (permeate more readily) in indium oxide compared to In-Ga-Zn oxide. Furthermore, the permeability of the indium oxide film to oxygen and hydrogen atoms is higher than that of the In-Ga-Zn oxide film. Therefore, it can be inferred that the indium oxide film is a film where hydrogen and oxygen are easily supplied and expelled. Additionally, it is expected that oxygen can be used to fill the V generated during the +GBT test. O Based on its function, it can be inferred that it can achieve highly reliable transistors.
[0141] Thus, as Figure 3AAs shown, diffusion occurs into the indium oxide film (referred to as InO). X Oxygen (O) permeates through the indium oxide membrane and is released as oxygen molecules (O2). Additionally, it is sometimes released as water molecules (H2O) by reacting with hydrogen contained in the membrane. Furthermore, when oxygen vacancies (V) are present in the membrane... O When oxygen diffuses, it fills the oxygen vacancies. Because oxygen diffuses easily, indium oxide films can fill oxygen vacancies more readily than IGZO films. Therefore, indium oxide films are more likely to reduce oxygen vacancies compared to IGZO films. Thus, by using indium oxide films in transistors, transistors with extremely high reliability can be realized.
[0142] In addition, such as Figure 3A As shown, hydrogen diffuses through the indium oxide membrane. Hydrogen diffuses from the outside into the indium oxide membrane and is released as hydrogen molecules (H2) through the membrane. Alternatively, as described above, the hydrogen reacts with oxygen contained in the membrane and is released as water molecules.
[0143] The content of the first element in the oxide semiconductor 230 is preferably low. Furthermore, the concentration of the first element in the oxide semiconductor 230 is preferably low. In particular, the concentration of the first element in the channel forming region is preferably low. Here, the first element is at least one selected from boron, carbon, aluminum, silicon, zinc, and gallium. That is, in the oxide semiconductor 230, it is preferable that the concentration of any one of boron, carbon, aluminum, silicon, zinc, and gallium is low; more preferably, the concentration of two selected from boron, carbon, aluminum, silicon, zinc, and gallium is low; and even more preferably, the concentrations of each of boron, carbon, aluminum, silicon, zinc, and gallium are low. The concentration of the first element in the oxide semiconductor 230 is preferably, for example, 1 atomic% or less, more preferably 0.1 atomic% or less, and even more preferably 0.01 atomic% (100 ppm) or less. Furthermore, the preferred concentration of the first element in the oxide semiconductor 230 can also be considered the preferred concentration of the first element in the channel forming region.
[0144] Furthermore, as described below, by using a precursor that has undergone more than one distillation, the concentration of the first element in the oxide semiconductor 230 can be set to 0.01 atomic% (100 ppm) or less, 0.0001% (1 ppm) or less, 0.00001% (0.1 ppm or 100 ppb) or less, or 0.0000001% (0.001 ppm or 1 ppb) or less. In other words, the content (purity) of indium other than oxygen in the oxide semiconductor 230 can be set to 99.99 atomic% or more (4N), 99.9999 atomic% or more (6N), 99.99999 atomic% or more (7N), or 99.9999999 atomic% or more (9N), making it possible to form an oxide semiconductor 230 with a purity equivalent to that of silicon used for the semiconductor layer (10N).
[0145] The crystallinity of oxide semiconductor 230 can be improved by reducing the concentrations of boron, carbon, aluminum and silicon in it.
[0146] When the oxide semiconductor 230 contains gallium atoms, these gallium atoms bond with excess oxygen atoms to form a Ga-O structure. The Ga-O structure acts as an acceptor for trapped electrons. Therefore, in transistors containing oxide semiconductor 230 with both gallium atoms and excess oxygen atoms, the threshold voltage variation in PBTS (Positive Bias Temperature Stress) testing increases. Therefore, by reducing the gallium concentration in the oxide semiconductor 230, the threshold voltage variation in PBTS testing can be reduced. Thus, a transistor with high reliability when applying a positive bias voltage can be realized. Furthermore, when the oxide semiconductor 230 contains zinc atoms, the same situation may occur as when it contains gallium atoms.
[0147] Furthermore, aluminum, gallium, and zinc atoms have stronger bonding forces with oxygen atoms compared to indium atoms. Therefore, by reducing the concentration of aluminum, gallium, and zinc in the indium oxide film, the decrease in oxygen permeability can be suppressed.
[0148] Furthermore, impurities such as the first element contained in the indium oxide film can act as crystal nuclei. By minimizing impurities in the indium oxide film, the number of crystal nuclei can be reduced, which can promote larger crystal sizes as described below.
[0149] Furthermore, when the indium oxide film is a polycrystalline film, the first element segregates at the grain boundaries, forming an oxide containing the first element. Because this oxide has insulating properties, it can potentially cause a decrease in the transistor's on-state current or field-effect mobility. By minimizing the amount of the first element in the indium oxide film, the transistor's on-state current or field-effect mobility can be improved.
[0150] Furthermore, by reducing impurities in the indium oxide film, impurity scattering can be suppressed. This allows for the realization of transistors with high field-effect mobility. For example, by setting the concentration of the first element in the oxide semiconductor 230 within the aforementioned preferred range, the field-effect mobility of the transistor can be set to 100 cm⁻¹. 2 / (V·s) or more, preferably 150cm 2 / (V·s) or more, more preferably 200cm 2 / (V·s) or more, further preferably 250cm 2 / (V·s) above.
[0151] Furthermore, Non-Patent Literature 2 reports the following: Hall mobility is calculated under the assumption that the main cause of scattering in indium oxide is ionized impurities and polar optical phonons, with an upper limit of 270 cm⁻¹. 2 / (V·s)(reference) Figure 4 ).
[0152] Here, the carrier concentration dependence of Hall mobility for indium oxide, silicon, and IGZO is explained. Figure 3B It concerns silicon (Si) and indium oxide (InO). X A schematic diagram illustrating the carrier concentration dependence of Hall mobility. Figure 3C This is a schematic diagram showing the carrier concentration dependence of Hall mobility in IGZO.
[0153] First, such as Figure 3C As indicated by the arrows, IGZO tends to exhibit higher Hall mobility with higher carrier concentrations. On the other hand, as... Figure 3B As indicated by the arrows, indium oxide (INO) tends to exhibit higher Hall mobility with lower carrier concentrations (see Non-Patent Literature 3). This tendency is similar to that of silicon; the lower the concentration of dopants (impurities) in the material, the less impurity scattering occurs, and the higher the Hall mobility. In other words, the higher the purity and the more intrinsic the INO, the higher the Hall mobility. From this result, it can be concluded that, unlike IGZO, INO possesses properties close to those of silicon. Note that... Figure 3B The properties of indium oxide shown are based on the assumption of a single crystal. Therefore, when indium oxide is not a single crystal (e.g., polycrystalline), the properties may differ. Figure 3B The characteristics shown are different.
[0154] exist Figure 3B In this context, the range R1, characterized by low carrier concentration, corresponds to a range with extremely high Hall mobility. Therefore, it can be considered, for example, a suitable range of carrier concentrations for use in the channel formation region of a transistor. For instance, in indium oxide, the range R1 includes carrier concentrations of 1 × 10⁻⁶. 15 cm-3 The range, for example, is 1×10 14 cm -3 Above and 1×10 18 cm -3 The following range. By sufficiently reducing the carrier concentration, it is expected that the Hall mobility value can be increased to 270 cm⁻¹. 2 Approximately / (V·s).
[0155] Furthermore, in indium oxide, the region with a carrier concentration in the range R1 can contain elements that reduce the carrier concentration. Examples of elements that reduce carrier concentration include magnesium, calcium, zinc, cadmium, and copper. Replacing indium with these elements reduces the carrier concentration. Other examples of elements that reduce carrier concentration include nitrogen, phosphorus, arsenic, and antimony. For example, replacing oxygen with nitrogen, phosphorus, arsenic, or antimony reduces the carrier concentration.
[0156] On the other hand, the range of high carrier concentration R2 is the range of low resistance; for example, it can be said to be the range of carrier concentrations suitable for use in the source and drain regions of transistors, resistive bodies, or transparent conductive films. The range R2 includes carrier concentrations of 1 × 10⁻⁶. 20 cm -3 The range, for example, is 1×10 19 cm -3 Above and 1×10 22 cm -3 The following range. By significantly increasing the carrier concentration, it is expected that the resistivity can be reduced to 1 × 10⁻⁶. -4 Below Ω·cm.
[0157] Furthermore, in indium oxide, the region with a carrier concentration in the range R2 can contain elements that increase the carrier concentration. For example, it is preferable to include the same elements as the source and drain electrodes of the transistor. Examples of elements that increase the carrier concentration include titanium, tantalum, tungsten, molybdenum, tin, silicon, germanium, zirconium, hafnium, and boron. In particular, it is more preferable to use elements whose oxides have conductive or semiconductor properties.
[0158] Thus, in indium oxide, regions with low carrier concentration are used for the channel formation region of the transistor, while regions with high carrier concentration are used for the source and drain regions. In other words, indium oxide can also be considered an oxide capable of controlling valence electrons. Note that valence electron control in silicon transistors is generally known. On the other hand, valence electron control in indium oxide transistors is a novel technical concept that is not usually considered. Based on this technical concept, transistors with high mobility, low off-state current, and the ability to be normally off can be realized.
[0159] Furthermore, the concentration of the first element can be evaluated using methods such as inductively coupled plasma mass spectrometry (ICP-MS), X-ray photoelectron spectroscopy (XPS), secondary ion mass spectrometry (SIMS), time-of-flight secondary ion mass spectrometry (ToF-SIMS), Auger electron spectroscopy (AES), energy dispersive X-ray spectroscopy (EDX), or inductively coupled plasma atomic emission spectrometry (ICP-AES).
[0160] Hydrogen contained in oxide semiconductors reacts with oxygen bonded to metal atoms to form water, sometimes creating oxygen vacancies. This can cause electrical properties to fluctuate, leading to decreased reliability. On the other hand, hydrogen present at grain boundaries can sometimes terminate dangling bonds at grain boundaries, improving the electrical properties and reliability of transistors. Therefore, while it is preferable to reduce the hydrogen concentration in the indium oxide film, the hydrogen concentration can sometimes be higher than the concentration of the first element.
[0161] Indium oxide has a band gap of 2.5 eV or higher and 3.7 eV or lower. By using indium oxide, which has a larger band gap than silicon, in oxide semiconductor 230, the off-state current of transistors can be reduced, thus significantly reducing the power consumption of semiconductor devices.
[0162] OS transistors are accumulation transistors where electrons are the majority carriers. In other words, the carriers in an OS transistor are electrons. Assuming a constant relaxation time for the carriers, the smaller the effective mass of the electrons (carriers), the higher the electron mobility (carrier mobility). That is, by using metal oxides with small effective electron mass in the semiconductor layer of the transistor, the on-state current or field-effect mobility of the transistor can be improved.
[0163] Table 2 shows the effective masses of single-crystal indium oxide (In₂O₃ in this case) and single-crystal silicon (Si). The effective masses of electrons and holes shown in Table 2 are values calculated using first-principles electronic state calculations.
[0164] [Table 2] As shown in Table 2, indium oxide (IO) has a low effective electron mass. Therefore, by using IO, with its low effective electron mass, in oxide semiconductor 230, transistors with high on-state current, high field-effect mobility, and high frequency characteristics (also known as f-characteristics) can be realized. Furthermore, IO also has the characteristic that the effective electron mass is almost independent of crystal orientation. Moreover, the effective electron mass of IO is, for example, smaller than that of silicon. Therefore, from the viewpoint of effective electron mass, transistors using IO in the channel formation region exhibit higher f-characteristics than Si transistors.
[0165] As shown in Table 2, indium oxide (IO) has a large effective hole mass. Therefore, by using IO with its large effective hole mass in oxide semiconductor 230, transistors with extremely low off-state currents can be realized. Furthermore, the effective hole mass of IO is, for example, greater than that of silicon. Therefore, from the viewpoint of effective hole mass, the off-state current of transistors using IO in the channel formation region is significantly smaller than that of Si transistors.
[0166] In transistors using indium oxide as a semiconductor 230, the off-state current value per channel width of 1 μm at room temperature (25°C) can be set to 1 A (1 × 10⁻⁶). -18 A) or below or 1zA (1×10 -21 A) Below. Furthermore, the off-state current value per channel width of 1 μm at 85°C can be set to 1 × 10⁻⁶. -16 Below A / μm, preferably 1×10 -17 A / μm or less, more preferably 1×10 -18 Below A / μm. Furthermore, the off-state current at 125°C with a channel width of 1μm can be set to 1fA (1×10⁻⁶). -15 A) or below or 1aA (1×10 -18 A) The following.
[0167] Furthermore, miniaturizing the OS transistor can improve its high-frequency characteristics. For example, the transistor's cutoff frequency can be increased. Specifically, at room temperature (25°C), the transistor's cutoff frequency can be 50 GHz or higher, preferably 100 GHz or higher, and more preferably 150 GHz or higher.
[0168] Indium oxide films can contain one or more of the periodic elements with high period numbers in the periodic table, within a range that exhibits crystallinity. There is a tendency for greater overlap of the orbitals of metal elements in metal oxides to result in greater carrier conductivity. Therefore, by including periodic elements with high period numbers in the periodic table, the field-effect mobility of transistors can sometimes be improved. Examples of periodic elements with high period numbers in the periodic table include elements belonging to period 5 and period 6. Specifically, examples of such elements include yttrium, zirconium, silver, cadmium, tin, antimony, barium, lead, bismuth, and light rare earth elements (lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium).
[0169] Figures 1A to 1D Examples of oxide semiconductor 230 having a single-layer structure are shown. Furthermore, oxide semiconductor 230 can employ a stacked structure of two or more layers. For example, in the case where oxide semiconductor 230 has a two-layer structure of a first semiconductor layer and a second semiconductor layer on the first semiconductor layer, it is preferable to use a metal oxide (typically indium oxide) suitable for the aforementioned oxide semiconductor 230 as the first semiconductor layer, and a metal oxide with its conduction band bottom located closer to the vacuum level than the conduction band bottom of the first semiconductor layer as the second semiconductor layer. In this case, the first semiconductor layer can be primarily used as a current path (channel). That is, the surface of the first semiconductor layer on the side of the second semiconductor layer and its vicinity have a channel forming region.
[0170] By employing the above structure, the number of carriers trapped at and near the interface between the first and second semiconductor layers can be reduced. Furthermore, by positioning the channel away from the surface of the insulator 250, the effects of surface scattering can be reduced. This, in turn, improves the field-effect mobility of the transistor.
[0171] As metal oxides that can be used for the second semiconductor layer, examples include indium gallium oxide (In-Ga oxide), indium Zn oxide, indium tin oxide (In-Sn oxide, also denoted as ITO), indium titanium oxide (In-Ti oxide), indium aluminum zinc oxide (In-Al-Zn oxide, also denoted as IAZO), indium Ga-Zn oxide, indium tin zinc oxide (also denoted as In-Sn-Zn oxide), indium titanium zinc oxide (In-Ti-Zn oxide), and indium tin oxide containing silicon oxide (also denoted as ITSO). Alternatively, zinc oxide, aluminum zinc oxide (Al-Zn oxide, also denoted as AZO), and aluminum tin oxide (Al-Sn oxide) can be used.
[0172] Specifically, the In-Zn oxide used for the second semiconductor layer can have an In:Zn ratio of 1:1 or closer, an In:Zn ratio of 2:1 or closer, or an In:Zn ratio of 4:1 or closer. Similarly, the IGZO used for the second semiconductor layer can have an In:Ga:Zn ratio of 1:1:1 or closer, an In:Ga:Zn ratio of 1:3:2 or closer, or an In:Ga:Zn ratio of 1:3:4 or closer. Furthermore, the "closely related" composition includes a range of ±30% of the desired atomic ratio.
[0173] There are no particular restrictions on the crystallinity of the metal oxide contained in the second semiconductor layer. For example, the second semiconductor layer may sometimes contain one or more of the following: amorphous semiconductor (semiconductor with an amorphous structure), single-crystal semiconductor (semiconductor with a single-crystal structure), and semiconductor with crystallinity other than single crystal (microcrystalline semiconductor, polycrystalline semiconductor, or a portion thereof having a crystalline region).
[0174] Next, the crystal structure of oxide semiconductor 230 will be explained. For example... Figure 1A As shown, the oxide semiconductor 230 and the insulator 224 are formed as islands in the transistor 200. Before the oxide semiconductor 230 and the insulator 224 are patterned into islands, as... Figure 5C As shown, a film deposited to form an oxide semiconductor 230 (hereinafter referred to as oxide semiconductor film 230f) and a film deposited to form an insulator 224 (hereinafter referred to as insulating film 224f) are shown. Figure 5C In the middle, an island-shaped layer 235 and an insulator 225 are provided in contact with the top surface of the insulating film 224f, and an oxide semiconductor film 230f is provided in the manner of covering the layer 235 and the insulator 225.
[0175] Layer 235 contains crystals. When a process is performed to improve the crystallinity of the oxide semiconductor film 230f, layer 235 is used as a seed or nucleus. In other words, layer 235 is used as a seed or nucleus during the crystal growth of the oxide semiconductor film 230f. In this specification, layer 235 or the crystals contained in layer 235 may be referred to as seed crystals or nuclei. Furthermore, since layer 235 contains crystals, layer 235 may be referred to as a crystalline portion.
[0176] Indium oxide has a cubic crystal structure (manganese permanganate type). When indium oxide is used in the oxide semiconductor film 230f, layer 235 preferably contains, for example, a hexagonal or trigonal crystal structure. In this case, the crystal orientation of layer 235 relative to the surface of layer 235 or the surface to which it is formed is... <001> The crystallization can form crystals with a crystal orientation of <111> A crystalline oxide semiconductor film 230f. The crystal orientation of the crystals contained in layer 235 relative to the surface of layer 235 or the surface in which they are formed is... <001> At this time, the c-axis of the crystal is perpendicular or substantially perpendicular to the surface of layer 235 or the surface in which it is formed. Note that hexagonal or trigonal crystals can sometimes be referred to as crystals with layered structures, so the above structure can be considered as a structure in which an oxide semiconductor film 230f containing cubic crystals is formed on a layer 235 containing crystals with layered structures. In other words, it can also be considered as a stacked structure manufactured using heteroepitaxial growth technology or a technique such as heteroepitaxial growth.
[0177] like Figure 5C As shown, in the oxide semiconductor film 230f, the crystal orientation of the grains is preferably uniform or substantially uniform at any location. For example, as Figure 5C As shown, preferably, in the oxide semiconductor film 230f, the crystal orientation of the grains contained in the region between layer 235 and insulator 225, the region in contact with the side surface of insulator 225, the region in contact with the top surface of insulator 225, and the region between insulators 225 are all [missing information]. <111> .
[0178] Figure 2B The oxide semiconductor 230 of the transistor 200 shown is similar; the crystal orientation of the grains in the regions of the oxide semiconductor 230 that contact the side surface of the insulator 225 and the regions that contact the top surface of the insulator 225 is preferably the same or substantially the same. Furthermore, the crystal orientation of the grains in the regions of the oxide semiconductor 230 that contact the side surface of the insulator 225 and the regions that contact the top surface of the insulator 225 is preferably... <111> Here, the crystal orientation of the oxide semiconductor 230 is... <111> The surface of the substrate (or the surface of the insulator 224) is perpendicular or substantially perpendicular to it at any location. Alternatively, the crystal orientation of the oxide semiconductor 230 can also be described as... <111> Parallel or substantially parallel to the side surface of insulator 225, and perpendicular or substantially perpendicular to the top surface of insulator 225.
[0179] As described above, the oxide semiconductor 230 is used as a channel formation region near both the top and side surfaces of the insulator 225. Therefore, by making the crystal structure of the regions near the top and side surfaces of the insulator 225 of the oxide semiconductor 230 uniform, the electrical characteristics of the transistor 200 can be stabilized. This improves the on-state current, field-effect mobility, frequency characteristics, etc., of the transistor 200.
[0180] In this specification, space groups are represented using the shortnotation of the International Notation (or Hermann-Mauguin notation). Additionally, Miller indices are used to represent crystal planes and crystal orientations. In crystallography, a superscript is added to numbers to indicate space groups, crystal planes, and crystal orientations. However, in this specification, due to the notation limitations in the patent application, a - (negative number symbol) is sometimes added before numbers to indicate space groups, crystal planes, and crystal orientations instead of a superscript. Furthermore, "[ ]" indicates an individual orientation within the crystal, "<>" indicates a set of orientations of all equivalent orientations, "()" indicates an individual crystal plane, and "{}" indicates a set of planes with equivalent symmetry.
[0181] In this specification and the like, the crystal orientation of crystallization refers to its orientation relative to the surface of the substrate. Therefore, for example, the crystal orientation is... <100> The crystallization can be described as the (100) plane being parallel to the substrate surface. However, it is not limited to this; the crystal orientation of the crystallization can also be described as the orientation relative to the surface of layer 235 or the surface of layer 235 that is formed.
[0182] Specifically, zinc oxide, In-Ga oxide, gallium zinc oxide (Ga-Zn oxide, also denoted as GZO), aluminum zinc oxide (Al-Zn oxide, also denoted as AZO), In-Al-Zn oxide, In-Ga-Zn oxide, or In-Sn-Zn oxide can be used as layer 235. In-Ga-Zn oxide is preferred as layer 235. In this case, layer 235 contains indium, gallium, zinc, and oxygen. Furthermore, its composition is preferably In:Ga:Zn = 1:1:1 [atomic ratio] or close to it, or In:Ga:Zn = 1:3:2 [atomic ratio] or close to it. Since the metal oxides with the above compositions readily form layered structures, they are suitable for use as layer 235.
[0183] In-Ga-Zn oxides and In-Sn-Zn oxides readily possess a CAAC structure. When an oxide with a CAAC structure is used as layer 235, the c-axis of the crystals contained in layer 235 is perpendicular or substantially perpendicular to the surface of layer 235 or the surface to which it is formed. In other words, the crystal orientation of the crystals contained in layer 235 relative to the surface of layer 235 or the surface to which it is formed is... <001> Therefore, by using oxides that readily possess CAAC structures for layer 235, the controllability of the crystal orientation of the crystal nuclei can be improved.
[0184] Here, Figures 6A to 6E The crystal structure of the metal oxide is shown. Figure 6A This is a diagram of the crystal structure of an In-Ga-Zn oxide with an In:Ga:Zn ratio of 1:1:1 [atomic number ratio], viewed from a direction perpendicular to the c-axis. Figure 6B Looking along the c-axis Figure 6A The diagram shows the surface indicated by the dashed lines. Figure 6C Looking along the c-axis Figure 6A The diagram showing the surface indicated by the dashed lines in the image. Figure 6D Looking along the c-axis Figure 6A The diagram shows the surface indicated by the double-dotted line. Figure 6A , Figure 6C and Figure 6D The Mx recorded therein refers to Ga or Zn atoms. Additionally, in Figure 6A In Chinese, surfaces shown by dashed lines, dashed lines, and double dashed lines are sometimes collectively referred to as surface c. Additionally, Figure 6E This is a diagram of the crystal structure of indium oxide viewed from the direction perpendicular to the (111) plane.
[0185] The interatomic distance of metal atoms in the c-plane ( Figures 6B to 6D Each of the arrows shown is 0.330 nm. Additionally, the In-In distance in the (111) plane ( Figure 6E The arrows shown represent 0.334 nm and 0.385 nm. In other words, the configuration of metal atoms on the c-plane of the CAAC structure is similar to that on the (111)-plane of indium oxide. Therefore, an oxide that readily has a CAAC structure can be used as layer 235.
[0186] When an oxide that readily possesses a CAAC structure is used for layer 235, a layer containing crystal orientations can be formed. <111> 230f of crystalline oxide semiconductor film.
[0187] Layer 235 can also be an oxide with a cubic crystal structure. By giving layer 235 the same crystal structure as the oxide semiconductor film 230f, the oxide semiconductor film 230f can be epitaxially grown using layer 235 as a seed or nucleus, thereby improving the crystallinity of the oxide semiconductor film 230f. Oxides containing elements from Group 3 of the periodic table tend to have a cubic crystal structure. Furthermore, the Group 3 elements in this crystal mainly exist as trivalent cations. Therefore, layer 235 preferably contains at least one element that can be a trivalent cation. The element that can be a trivalent cation contained in layer 235 is preferably scandium, yttrium, cerium, gadolinium, erbium, or ytterbium.
[0188] As layer 235, for example, an oxide containing one or both of yttrium and zirconium, erbium oxide, etc., can be used. Examples of oxides containing one or both of yttrium and zirconium include yttrium oxide, zirconium oxide, and yttrium zirconium oxide.
[0189] Furthermore, the difference between the lattice constant or the length of a unit lattice vector of the crystal nucleus and the lattice constant or the length of a unit lattice vector of the crystal contained in the oxide semiconductor film 230f (also known as lattice mismatch) is preferably small. By using an oxide with a small lattice mismatch for layer 235, the crystallinity of the oxide semiconductor film 230f can be improved.
[0190] One method for evaluating the degree of lattice mismatch is to use the lattice mismatch value shown below. The lattice mismatch Δa[%] of the crystals contained in the formed film (in this case, an indium oxide film) relative to the crystals contained in the film being formed is calculated according to the following formula (1). Hereinafter, the lattice mismatch Δa of the crystals contained in the formed film relative to the crystals contained in the film being formed is sometimes simply referred to as the lattice mismatch Δa of the formed film relative to the film being formed.
[0191] [Equation 1] In formula (1), L1 represents the lattice constant or the length of the unit lattice vector of the crystal contained in the above-formed film, and L2 represents the lattice constant or the length of the unit lattice vector of the crystal contained in the above-formed film.
[0192] The lattice mismatch Δa of the grains contained in the oxide semiconductor film 230f relative to the crystal nucleus is preferably -10% or more and 10% or less, more preferably -5% or more and 5% or less, and even more preferably -3% or more and 3% or less. By using a material with a small lattice mismatch relative to the oxide semiconductor film 230f in layer 235, the crystallinity of the oxide semiconductor film 230f can be improved.
[0193] For example, the lattice constant of indium oxide crystal (argentite type) is 1.01194 nm. Additionally, the lattice constant of yttrium oxide crystal (argentite type) is considered to be 1.05976 nm. Therefore, the lattice mismatch of indium oxide crystal relative to yttrium oxide crystal is -4.5%. Therefore, when indium oxide is used in oxide semiconductor film 230f, yttrium oxide can be used in layer 235.
[0194] For example, the lattice constant of erbium oxide crystal (argentite-manganese type) is considered to be 1.0582 nm. Therefore, the lattice mismatch of indium oxide crystal relative to erbium oxide crystal is -4.4%. Therefore, when indium oxide is used in oxide semiconductor film 230f, erbium oxide can be used in layer 235.
[0195] For example, Zr, as an example of yttrium zirconium oxide 0.9 Y 0.1 O 1.95 The lattice constant of the crystal (fluorite type) is 0.51481 nm (refer to ICSD coll.code.248790). Therefore, the lattice constant of indium oxide crystal relative to Zr... 0.9 Y 0.1 O 1.95 The lattice mismatch of the crystal is -1.7%. Therefore, when indium oxide is used for the oxide semiconductor film 230f, yttrium zirconium oxide can be used for layer 235. Note that yttrium zirconium oxide contains yttrium, zirconium, and oxygen.
[0196] By adding yttrium or yttrium oxide to zirconium oxide, that is, by ensuring that the yttrium content of yttrium zirconium oxide is greater than 0 atomic%, the crystal structure of zirconium oxide can be stabilized. Note that as this content increases, the crystal structure of yttrium zirconium oxide sometimes changes from a cubic crystal system to other crystal systems; therefore, this content is preferably not too high. Thus, for example, the yttrium content of yttrium zirconium oxide is preferably 2 atomic% or more and 15 atomic% or less, more preferably 5 atomic% or more and 10 atomic% or less.
[0197] Furthermore, indium oxide can also be used as layer 235. By using indium oxide as layer 235, the oxide semiconductor film 230f can be homoepitaxially grown using layer 235 as a seed or nucleus, thereby improving the crystallinity of the oxide semiconductor film 230f. In this case, the crystal orientation of the crystals contained in layer 235 is consistent with or substantially consistent with the crystal orientation of the crystals contained in the oxide semiconductor film 230f. For example, by using the method described later, a crystal orientation identical to that of the oxide semiconductor film 230f can be formed. <111> Indium oxide is deposited and patterned to form layer 235. This allows for crystal orientation. <111> Layer 235 serves as the core, causing the crystal orientation to be... <111> Homoenomic growth of 230f oxide semiconductor film was performed.
[0198] There are no particular restrictions on the materials that can be used for layer 235. Layer 235 can be made of insulating, semiconductor, or conductive materials. When a semiconductor material is used for layer 235, layer 235 can also be considered as part of oxide semiconductor film 230f.
[0199] Additionally, layer 235 can appear as an island when viewed from above. When layer 235 is formed as an island, it can be a shape that is approximately circular or elliptical, triangular, quadrilateral (including rectangles, rhombuses, and squares), pentagonal, or star-shaped polygon when viewed from above, or the corners of these polygons can be rounded. Furthermore, when sputtered particles are used as layer 235, layer 235 may sometimes appear as a triangle or hexagon when viewed from above.
[0200] Alternatively, layer 235 can also be strip-shaped when viewed from above. For example, similar to insulator 225, it can be formed in a manner that extends along the length of the channel (A5-A6 direction).
[0201] Alternatively, layer 235 can also be tapered in cross-section. For example, the angle formed between the top surface of insulating film 224f and the side surface of layer 235 can be less than 90°, preferably 30° or more and less than 90°. By making layer 235 tapered, the coverage of oxide semiconductor film 230f can be improved, thereby reducing defects such as voids. In addition, it can promote the crystal growth of oxide semiconductor film 230f.
[0202] in addition, Figure 5C An example is shown where layer 235 is disposed in contact with the top surface of insulating film 224f, but the present invention is not limited thereto. For example, layer 235 may also be disposed in a recess provided in insulating film 224f. This allows the top surface of insulating film 224f to be flat, which can improve the crystallinity of oxide semiconductor film 230f. Furthermore, the aforementioned recess may also be an opening penetrating insulating film 224f.
[0203] The thickness of layer 235 is preferably small. For example, the thickness of layer 235 is preferably smaller than the thickness of oxide semiconductor film 230f. Specifically, layer 235 preferably has a region with a thickness of 0.1 nm or more and less than 2 nm, and more preferably has a region with a thickness of 0.5 nm or more and less than 2 nm. By reducing the thickness of layer 235, the step between layer 235 and insulating film 224f is reduced. As a result, the coverage of oxide semiconductor film 230f is improved, and defects such as voids can be reduced. In addition, the crystal growth of oxide semiconductor film 230f can be promoted. Note that layer 235 can be layered or granular.
[0204] The insulating film 224f preferably has the function of supplying oxygen to the oxide semiconductor film 230f. For example, the insulating film 224f preferably has a region containing oxygen that has been removed by heating (hereinafter sometimes referred to as excess oxygen). Furthermore, the insulator 250 preferably has the function of trapping or fixing oxygen. By employing this structure, oxygen can be forced into the oxide semiconductor film 230f from the insulating film 224f side to reduce the amount of oxygen vacancies in the oxide semiconductor film 230f, and excess oxygen in the oxide semiconductor film 230f can be pulled out from the insulator 250 side to reduce excessive oxygen in the oxide semiconductor film 230f. Thus, a semiconductor device with high reliability can be provided.
[0205] Alternatively, an insulating film 224f can be used that traps or fixes oxygen, and an insulator 250 can supply oxygen to the oxide semiconductor film 230f. By employing this structure, oxygen can be forced into the oxide semiconductor film 230f from the insulator 250 side to reduce the amount of oxygen vacancies in the oxide semiconductor film 230f, and excess oxygen can be pulled out from the insulating film 224f side to reduce excessive oxygen in the oxide semiconductor film 230f. Thus, a semiconductor device with high reliability can be provided.
[0206] Furthermore, the insulating film 224f preferably uses a material with a smaller coefficient of thermal expansion than the metal oxide used for the oxide semiconductor film 230f. For example, a material with a smaller coefficient of thermal expansion than indium oxide can be used as the insulating film 224f. Specifically, the coefficient of thermal expansion of the insulating film 224f is preferably 0.01 × 10⁻⁶. -6 K -1 Above and 5.5×10 -6 K -1 Hereinafter, 0.01×10 is more preferred. -6 K -1 Above and 5.0×10 -6 K -1 Hereinafter, 0.01×10 is further preferred. -6 K -1 Above and 3.0×10 -6 K -1 The following is a further preferred value of 0.01×10 -6 K -1 Above and 1.0×10 -6 K -1The following describes a structure where, by bringing an indium oxide-containing oxide semiconductor film 230f into contact with or near an insulating film 224f with a low coefficient of thermal expansion, tensile stress is applied to the indium oxide upon cooling, making it energy-unstable. As a result, the indium oxide becomes an energy-more stable cubic crystal. Furthermore, crystal growth can be promoted to form large-grained cubic crystals. Silicon oxide has a lower coefficient of thermal expansion than indium oxide, making it suitable for use in the insulating film 224f.
[0207] Table 3 shows the coefficients of thermal expansion for oxide semiconductors and insulators. In Table 3, the coefficients of thermal expansion for IGZO and indium oxide (In₂O₃ in this case) are shown as oxide semiconductors, and the coefficients of thermal expansion for silicon oxide (SiO₂), silicon nitride (Si₃N₄), and yttrium-stabilized zirconium oxide (YSZ) are shown as insulators. As can be seen from Table 3, silicon nitride is also suitable for use in insulating film 224f.
[0208] [Table 3] Figure 5C An example of a single-layer structure is shown for the insulating film 224f. Furthermore, the insulating film 224f can have a stacked structure of two or more layers. When the insulating film 224f has a stacked structure of two or more layers, the layer in contact with the oxide semiconductor film 230f among the two or more layers included in the insulating film 224f is preferably an insulating material suitable for the aforementioned insulating film 224f (typically silicon oxide). By employing this structure, the crystallinity of the oxide semiconductor film 230f can be improved.
[0209] The following is for reference Figures 5A to 5C An example illustrating the manufacturing method of oxide semiconductor film 230f. Figures 5A to 5C It corresponds to Figure 1B and Figure 2B Cross-sectional view. Note that in Figures 5A to 5C The diagram shows a plurality of insulators 225 corresponding to a plurality of transistors 200.
[0210] The layers constituting a semiconductor device (insulating film 224f, layer 235, oxide semiconductor film 230f, etc.) can be formed using sputtering, chemical vapor deposition (CVD), vacuum evaporation, pulsed laser deposition (PLD), or atomic layer deposition (ALD).
[0211] Unlike deposition methods that deposit particles released from a target or similar material, the ALD (Alternating Layer Deposition) method forms a film through a reaction on the surface of the workpiece. Therefore, this method is less affected by the shape of the workpiece and exhibits high step coverage. In particular, the ALD method has excellent step coverage and thickness uniformity, making it suitable for covering surfaces with high aspect ratios, such as openings or grooves.
[0212] Precursors used in ALD sometimes contain elements such as carbon or chlorine. Therefore, films prepared using ALD sometimes contain more carbon or chlorine than films prepared using other deposition methods. Furthermore, the quantification of these elements can be performed using XPS or SIMS. Note that by employing one or both of the following methods during ALD—high substrate temperature during deposition and impurity removal—the amount of carbon and chlorine contained in the film can sometimes be reduced compared to using ALD without these methods.
[0213] Examples of ALD methods include thermal ALD (thermal ALD) which uses only thermal energy to react precursors and reactants, and plasma ALD (PEALD) which uses reactants excited by plasma.
[0214] In a deposition apparatus utilizing the ALD method, a first source gas (sometimes referred to as a precursor, precursor, or metal precursor) and a second source gas (sometimes referred to as a reactant, reactant, oxidant, or nonmetal precursor) are alternately introduced into the chamber, and this introduction of source gases is repeated to achieve deposition. Note that, for example, the introduced source gas can be switched by switching various on / off valves (sometimes referred to as high-speed valves). Furthermore, inert gases such as nitrogen (N2), argon (Ar), or helium (He) can be used as carrier gases when introducing the source gas, and they are introduced into the chamber along with the source gas. By using a carrier gas, even if the source gas has low volatility or vapor pressure, adsorption of the source gas into the pipes and valves can be suppressed, thereby allowing the source gas to be introduced into the chamber. Furthermore, the uniformity of the formed film is improved, making this method preferred.
[0215] When using the ALD method, films of arbitrary composition can be deposited by simultaneously introducing multiple different precursors. Alternatively, by controlling the number of cycles for each precursor while introducing multiple different precursors, films of arbitrary composition can be deposited.
[0216] First, a substrate (not shown) is prepared, and an insulating film 224f is formed on the substrate. Then, an insulator 225 is formed on the insulating film 224f. The method for forming the insulator 225 will be described in detail later. The top surface of the insulating film 224f is preferably flat. By making the top surface of the insulating film 224f flat, the crystallinity of the oxide semiconductor film 230f to be formed later can be improved. For example, lateral growth of the crystals contained in the oxide semiconductor film 230f in the first heat treatment, which will be described later, can be promoted.
[0217] The insulating film 224f can be formed, for example, by sputtering in an oxygen-containing atmosphere. By using a sputtering method that does not require the use of hydrogen-containing molecules as a deposition gas, the hydrogen concentration in the insulating film 224f can be reduced. Furthermore, by forming the insulating film 224f by sputtering in an oxygen-containing atmosphere, oxygen can be added to the insulating film 224f. Since the heat applied after the formation of the oxide semiconductor film 230f can supply oxygen from the insulating film 224f to the oxide semiconductor film 230f, oxygen vacancies can be reduced.
[0218] Before forming layer 235, it is preferable to perform a heat treatment. As a heat treatment, for example, it can be performed at a temperature of 250°C or higher and 650°C or lower, preferably at 300°C or higher and 500°C or lower, and more preferably at 320°C or higher and 450°C or lower.
[0219] The heating treatment is performed in an atmosphere of nitrogen or an inert gas, or in an atmosphere containing 10 ppm (0.001%) or more, 1% or more, or 10% or more of an oxidizing gas. For example, when the heating treatment is performed in a mixed atmosphere of nitrogen and oxygen gas, the ratio of oxygen gas is preferably set to about 20%. The heating treatment can also be performed under reduced pressure. Alternatively, the heating treatment can be performed in a nitrogen or inert gas atmosphere, and then, in order to replenish the detached oxygen, the heating treatment is performed in an atmosphere containing 10 ppm or more, 1% or more, or 10% or more of an oxidizing gas. By performing the above-described heating treatment, impurities such as hydrogen or water contained in the insulating film 224f, insulator 225, etc., can be reduced before depositing the oxide semiconductor film 230f.
[0220] Furthermore, the gas used in the above-described heat treatment is preferably of high purity. For example, the water content in the gas used in the above-described heat treatment is preferably 1 ppb (1 × 10⁻⁶). -3 ppm or less, more preferably 0.1 ppb (1×10⁻⁶ ppm). -4 ppm or less, more preferably 0.05 ppb (5 × 10⁻⁶ ppm), -5 (ppm) or less. By using a highly purified gas for heating treatment, the absorption of moisture and other substances by the insulating film 224f can be prevented as much as possible.
[0221] There are no particular restrictions on the heating device used for heat treatment; devices that utilize heat conduction or thermal radiation generated by heating elements such as resistance heating elements can also be used to heat the workpiece. For example, electric furnaces or RTA (Rapid Thermal Anneal) devices such as LRTA (Lamp Rapid Thermal Anneal) devices and GRTA (Gas Rapid Thermal Anneal) devices can be used. LRTA devices heat the workpiece using radiation of light (electromagnetic waves) emitted from lamps such as halogen lamps, metal halide lamps, xenon arc lamps, carbon arc lamps, high-pressure sodium lamps, or high-pressure mercury lamps. GRTA devices use high-temperature gases for heat treatment.
[0222] Furthermore, it is preferable to perform the oxygen supply process before forming layer 235. This allows oxygen to be supplied to the insulating film 224f, and oxygen can also be supplied from the insulating film 224f to the oxide-oxide-semiconductor film 230f by heat or the like applied after the formation of the oxide-oxide-semiconductor film 230f.
[0223] Examples of oxygen supply methods include heating in an oxygen-containing atmosphere or plasma treatment in an oxygen-containing atmosphere. Note that plasma treatment in this specification includes microwave plasma treatment, which will be described later. Alternatively, oxygen can be supplied to the insulating film 224f by depositing an oxide film (preferably a metal oxide film) in an oxygen-containing atmosphere using a sputtering method. The deposited oxide film can be removed immediately or left as a residue. When the deposited oxide film is left as a residue, it can be used as part of the oxide semiconductor film 230f. Furthermore, the oxygen-containing atmosphere includes, in addition to oxygen gas (O2), an atmosphere containing oxygen-containing compounds such as ozone (O3) or nitrous oxide (N2O). Furthermore, the substrate temperature in the plasma treatment is above room temperature (25°C) and below 450°C.
[0224] Next, layer 235 is formed on insulating film 224f (refer to...) Figure 5A Layer 235 serves as the nucleus for the crystallization and growth of the oxide semiconductor film 230f. Therefore, layer 235 can be referred to as a seed layer, seed crystal, etc.
[0225] There are no particular limitations on the method for forming layer 235. For example, layer 235 can be formed by forming a film that becomes layer 235 and processing the film. The film can be formed using methods such as sputtering, CVD, vacuum evaporation, PLD, or ALD.
[0226] Layer 235 can be formed using sputtering. By forming layer 235 using sputtering, the crystallinity of layer 235 can be improved. Furthermore, by forming layer 235 using sputtering in an oxygen-containing atmosphere, oxygen can be added to the insulating film 224f.
[0227] When a sputtering target has multiple grains with a layered structure and easily cleavable interfaces exist within the grains, ions can collide with the sputtering target, sometimes causing the grains to cleave and resulting in plate-shaped or granular sputtered particles. Plate-shaped or granular sputtered particles deposited on the insulating film 224f can also be used as layer 235.
[0228] Alternatively, a recess can be formed in the insulating film 224f, and the film to be layer 235 can be embedded in the recess. The film can be polished by CMP or the like until the surface of the insulating film 224f is exposed, thereby forming layer 235 embedded in the insulating film 224f. This makes the surface of the oxide semiconductor film 230f flat.
[0229] As described above, by forming layer 235 before forming oxide semiconductor film 230f, the effect of heat on oxide semiconductor film 230f can be reduced, thereby suppressing the miniaturization of crystals contained in oxide semiconductor film 230f and the increase of grain boundaries.
[0230] Next, an oxide semiconductor film 230f is formed in the manner of a capping layer 235 and an insulator 225 (see reference). Figure 5A The oxide semiconductor film 230f is deposited along the insulator 225, and therefore preferably has good coverage. Thus, the oxide semiconductor film 230f is preferably deposited using a method such as ALD, which provides good coverage. Furthermore, the aspect ratio of the oxide semiconductor 230 is preferably high, so the thickness of the oxide semiconductor film 230f is preferably small. Therefore, it is preferable to deposit the oxide semiconductor film 230f using an ALD method that allows for smaller thickness adjustments. By depositing the oxide semiconductor film 230f in this way, the oxide semiconductor film 230f is formed in contact with the top and side surfaces of the insulator 225.
[0231] When depositing an oxide semiconductor film 230f using the ALD method, a first precursor and a first oxidant can be used. The first precursor preferably contains indium. At this time, an indium oxide film is formed as the oxide semiconductor film 230f. In other words, an oxide film containing a single element other than oxygen is deposited. Note that when the first precursor contains indium, a thermal ALD method can be used as the ALD method.
[0232] As precursors containing indium, for example, trimethylindium, triethylindium, ethyl dimethylindium, tris(1-methylethyl)indium, tris(2,2,6,6-tetramethyl-3,5-heptanoic acid)indium, cyclopentadienylindium, indium(III)acetylacetone, (3-(dimethylamino)propyl)dimethylindium, (diethylphosphine)dimethylindium, dimethylchloroindium, dimethylbromoindium, dimethyl(2-propanol)indium, etc.
[0233] In addition, inorganic precursors that do not contain hydrocarbons can also be used as indium-containing precursors. Halogenated indium compounds such as indium trifluoroethylene (indium(III) fluoride), indium trichloride (indium(III) chloride), indium tribromide (indium(III) bromide), and indium triiodide (indium(III) iodide) can be used as indium-containing inorganic precursors. The decomposition temperature of indium trichloride is approximately 500°C to 700°C. Therefore, by using indium trichloride, deposition can be performed using the ALD method while heating the substrate at a temperature of 400°C to 600°C, for example, 500°C.
[0234] In the method for forming the oxide semiconductor film 230f, it is preferable to use a precursor with low impurity concentration, i.e., high purity. For example, by using a precursor with a purity of 3N (99.9%) or higher, preferably 4N (99.99%) or higher, more preferably 5N (99.999%) or higher, and even more preferably 6N (99.9999%) or higher, impurities in the oxide semiconductor film 230f can be reduced.
[0235] The gallium and aluminum content of the indium-containing precursor is preferably 1000 ppm or less, more preferably 500 ppm or less, even more preferably 100 ppm or less, further preferably 50 ppm or less, even more preferably 10 ppm or less, and even more preferably 1 ppm or less. By using a precursor with low gallium content, the gallium concentration in the oxide semiconductor film 230f can be reduced, thereby improving the reliability of the transistor. By using a precursor with low aluminum content, the aluminum concentration in the oxide semiconductor film 230f can be reduced, thereby improving the crystallinity of the oxide semiconductor film 230f.
[0236] Furthermore, as the precursor used in this embodiment, it is preferable to use a precursor purified by performing two or more distillations (also known as rectification or precision distillation). Using the aforementioned precursor allows for the easy deposition of metal oxides with few impurities, which is therefore preferred. Multiple distillations further suppress the residue of impurities from the starting materials used in the precursor's production, which is also preferred. Note that the invention is not limited to the above structure; a precursor purified by a single distillation may also be used. Using single distillation reduces manufacturing costs, which is therefore preferred.
[0237] By performing one or more distillations, the aluminum content of the indium-containing precursor can be set to below 100 ppm, below 1 ppm, or below 1 ppb (0.001 ppm). Using this indium-containing precursor, it may be possible to form an indium oxide film with a purity equivalent to that of silicon (10N) used for semiconductor layers.
[0238] Ozone (O3), oxygen (O2), water (H2O), hydrogen peroxide (H2O2), etc., can be used as the first oxidant. Preferably, the first oxidant contains at least one of ozone and oxygen. By using ozone, oxygen, etc., which do not contain hydrogen, as the first oxidant, the amount of hydrogen mixed into the insulating film 224f can be reduced. Furthermore, the first oxidant can contain at least one of water and hydrogen peroxide. Thus, an oxide semiconductor film 230f with low crystallinity can be formed.
[0239] In this specification and the like, unless otherwise specified, when ozone, oxygen, and water are used as oxidants, they also include plasma states, free radical states, or ionic states, and are not limited to gaseous states or molecular states.
[0240] The pulse duration for introducing the first oxidant is preferably 0.1 seconds or more and 30 seconds or less, more preferably 0.3 seconds or more and 15 seconds or less, and even more preferably 0.3 seconds or more and 10 seconds or less. By shortening the pulse duration for introducing the first oxidant, the amount of the first oxidant introduced is reduced, and more hydrogen contained in the first precursor remains in the membrane. By allowing more hydrogen to remain in the membrane, the formation of crystal nuclei can be suppressed while eliminating some of the crystal nuclei in the membrane, thus reducing the number of crystal nuclei in the membrane.
[0241] Here, the substrate heating temperature when the first precursor is introduced into the reaction chamber is preferably a temperature corresponding to the decomposition temperature of the first precursor. In the thermal ALD method using triethylindium as the indium-containing precursor, the substrate heating temperature can be, for example, 100°C or higher and 350°C or lower, preferably 150°C or higher and 300°C or lower. When layer 235 is provided, the substrate heating temperature can be room temperature (25°C) or higher and 300°C or lower, preferably room temperature or higher and 200°C or lower, more preferably room temperature or higher and 150°C or lower. By lowering the substrate heating temperature, the crystallinity of the oxide semiconductor film 230f during deposition can be reduced.
[0242] Alternatively, the oxide semiconductor film 230f can also be formed by sputtering, for example. As the sputtering gas, a rare gas (typically argon) or a single gas of oxygen, or a mixture of a rare gas and oxygen, can be used. The proportion of the rare gas (typically argon) in the total sputtering gas is, for example, 50% or more and 100% or less, preferably 70% or more and 100% or less, more preferably 90% or more and 100% or less. By increasing the proportion of the rare gas (typically argon) in the total sputtering gas, an oxide semiconductor film 230f with low crystallinity can be formed. Furthermore, an oxide semiconductor film 230f with many dangling bonds can be formed. Therefore, the etching rate of the oxide semiconductor film 230f can be increased. Thus, the processing of the oxide semiconductor film 230f becomes easier, thereby increasing the productivity of semiconductor devices. Note that the oxide semiconductor film 230f with low crystallinity has, for example, an amorphous structure.
[0243] Note that the sputtering gas may also contain hydrogen (H2). By introducing hydrogen during the formation of the oxide semiconductor film 230f using sputtering, an oxide semiconductor film 230f with low crystallinity can be formed. Furthermore, the formation of crystal nuclei can be suppressed or the disappearance of crystal nuclei can be promoted during the formation of the oxide semiconductor film 230f. Moreover, when there are many crystal nuclei, the growing crystals collide with each other, thereby suppressing large-size crystals. In other words, small-size crystals are formed. However, by further reducing the number of crystal nuclei by eliminating some of the crystal nuclei in the film while suppressing the formation of crystal nuclei, and performing the first heat treatment described later, crystal growth can be promoted with fewer crystal nuclei, thereby increasing the grain size in the oxide semiconductor film 230f.
[0244] The oxide semiconductor film 230f can also be formed by sputtering in an oxygen-containing atmosphere. In this case, by using a sputtering method that does not require the use of hydrogen-containing molecules as the deposition gas, the hydrogen concentration in the oxide semiconductor film 230f can be reduced. For example, oxygen or a mixture of oxygen and rare gases can be used as the sputtering gas.
[0245] When the oxide semiconductor film 230f has a stacked structure, it can be formed, for example, by sputtering or ALD. For instance, when the oxide semiconductor film 230f has a two-layer structure with a first semiconductor layer and a second semiconductor layer on the first semiconductor layer, the first semiconductor layer can be deposited using ALD and the second semiconductor layer can be deposited using sputtering. Because the coverage of ALD is superior to that of sputtering, the coverage of the oxide semiconductor film 230f can be improved by depositing the first semiconductor layer using ALD. Furthermore, damage to the substrate (in this case, the insulating film 224f) can be reduced, and the formation of a mixed layer at the interface between the substrate and the oxide semiconductor film 230f can be suppressed, thereby further improving crystallinity. Moreover, productivity can be improved by depositing the second semiconductor layer using sputtering.
[0246] Alternatively, a first semiconductor layer can be deposited using sputtering, and a second semiconductor layer can be deposited using ALD. Even if pinholes or breaks are formed in the first semiconductor layer deposited using sputtering, the overlapping portions with the aforementioned pinholes or breaks can be filled using a second semiconductor layer deposited using the well-covering ALD method.
[0247] Next, a first heat treatment is performed. The first heat treatment is preferably performed, for example, in an atmosphere containing at least one of hydrogen (H2) and nitrogen (N2), more preferably in an atmosphere containing both hydrogen (H2) and nitrogen (N2). At this time, the hydrogen flow rate is preferably 3% or more and 15% or less, more preferably 5% or more and 10% or less. Furthermore, the temperature of the first heat treatment is preferably 120°C or more and 300°C or less, more preferably 120°C or more and 250°C or less, and even more preferably 120°C or more and 200°C or less. Furthermore, the duration of the first heat treatment is preferably 1 hour or more and 8 hours or less.
[0248] By performing a first heat treatment, with layer 235 as the core, the epitaxial growth and lateral grain growth of the oxide semiconductor film 230f can be improved, thereby enhancing the crystallinity of the oxide semiconductor film 230f (refer to...). Figure 5B In particular, by using a material with a low coefficient of thermal expansion for the insulating film 224f, crystal growth can be promoted. For example, grains are formed in the oxide semiconductor film 230f in the portion overlapping with layer 235, and these grains grow laterally, thereby allowing the oxide semiconductor film 230f to crystallize along the surface of the substrate. That is, as Figure 5B As shown, with layer 235 as the core, crystals grow laterally, and region 231c expands. Region 231c has a higher crystallinity than region 231a. As the processing time progresses, region 231c further expands along the surface of the substrate.
[0249] The aforementioned crystal growth also occurs near the insulator 225, which has a high aspect ratio. In other words, in the oxide semiconductor film 230f in the region contacting the side surface of the insulator 225, the grains also grow laterally. Therefore, similar to the region contacting the top surface of the insulator 225 and the region between the insulator 225 and layer 235, a highly crystalline region 231c is also formed in the region contacting the side surface of the insulator 225. Thus, the crystal orientation of the grains contained in the regions of the oxide semiconductor film 230f that contact the side surface of the insulator 225 and those that contact the top surface of the insulator 225 is consistent or substantially consistent. Furthermore, the crystal orientation of the grains contained in the regions of the oxide semiconductor film 230f that contact the side surface of the insulator 225 and those that contact the top surface of the insulator 225 is... <111> .
[0250] At the end of the first heat treatment, region 231c extends to the entire oxide semiconductor film 230f (refer to...). Figure 5C This improves the overall crystallinity of the oxide semiconductor film 230f, including the area near the insulator 225. Thus, indium oxide whose crystallinity is improved by growing crystals laterally from the crystal nucleus is called Lateral Growth Indium Oxide (LGIO).
[0251] Furthermore, by using silicon oxide with a small coefficient of thermal expansion for the insulating film 224f and applying tensile stress from the top surface of the insulating film 224f to indium oxide during cooling, the crystal growth of the oxide semiconductor film 230f can be promoted.
[0252] Next, a second heat treatment is performed. The second heat treatment is preferably performed in an atmosphere containing nitrogen and oxygen (typically, a nitrogen:oxygen volume ratio of 4:1). The temperature of the second heat treatment is preferably higher than that of the first heat treatment. For example, it is preferably 300°C or higher and 400°C or lower, more preferably 300°C or higher and 350°C or lower. Furthermore, the duration of the second heat treatment is preferably 1 hour or more and 4 hours or less.
[0253] The gas used for the second heat treatment is preferably highly purified. By using a highly purified gas for heat treatment, the absorption of moisture and other substances by the oxide semiconductor film 230f can be minimized.
[0254] There are no particular restrictions on the heating treatment used for the second heating treatment; for example, an electric furnace or an RTA device can be used.
[0255] By performing the first heat treatment at a temperature lower than that of the second heat treatment, the generation of crystal nuclei can be suppressed, and the crystals can be made larger in size. Furthermore, since the first heat treatment is performed in a reducing atmosphere, the amount of oxygen vacancies contained in the oxide semiconductor film 230f increases. Therefore, by performing the second heat treatment, oxygen can be supplied to the oxide semiconductor film 230f, and the supplied oxygen can fill the oxygen vacancies (making them null). Moreover, by performing the first heat treatment at a temperature lower than that of the second heat treatment, impurities sometimes remain in the oxide semiconductor film 230f. Therefore, by performing the second heat treatment at a temperature higher than that of the first heat treatment, the impurity concentration in the oxide semiconductor film 230f can be reduced. Additionally, the hydrogen concentration in the oxide semiconductor film 230f can be reduced.
[0256] As described above, by sequentially performing the first heating treatment and the second heating treatment, the amount of oxygen vacancies and impurities in the oxide semiconductor film 230f can be reduced while the oxide semiconductor film 230f is crystallized and grown.
[0257] Alternatively, microwave plasma treatment can be performed after depositing the oxide semiconductor film 230f. This microwave plasma treatment can reduce the concentration of impurities such as hydrogen or water contained in the oxide semiconductor film 230f. Furthermore, sometimes crystalline regions of the oxide semiconductor film 230f are grown.
[0258] In this specification and the like, microwaves refer to electromagnetic waves with frequencies of 300 MHz or higher and 300 GHz or lower. Microwave plasma treatment, for example, refers to a process using a device that includes a power source for generating high-density plasma using microwaves. Microwave plasma treatment may also be referred to as microwave-excited high-density plasma treatment.
[0259] By performing microwave plasma treatment in an oxygen-containing atmosphere, the impurity concentration in the oxide semiconductor film 230f can be reduced. Carbon is an example of an impurity. Note that the above describes a structure in which the oxide semiconductor film 230f is subjected to microwave plasma treatment in an oxygen-containing atmosphere, but the method is not limited thereto. For example, an insulating film disposed near the oxide semiconductor film 230f, more specifically, a silicon oxide film, can also be subjected to microwave plasma treatment in an oxygen-containing atmosphere. Furthermore, due to the heat generated during microwave plasma treatment, the crystallinity of the oxide semiconductor film 230f is sometimes improved.
[0260] Microwave plasma treatment is preferably carried out under reduced pressure, preferably 10 Pa or more and 1000 Pa or less, more preferably 50 Pa or more and 700 Pa or less, and even more preferably 100 Pa or more and 400 Pa or less. Furthermore, the treatment temperature is preferably room temperature (25°C) or more and 750°C or less, more preferably 300°C or more and 500°C or less, and can be 400°C or more and 450°C or less.
[0261] During microwave plasma treatment, the substrate can also be heated. The heating temperature of the substrate is preferably above room temperature (e.g., 25°C), above 100°C, above 200°C, above 300°C, or above 400°C and below 500°C, or below 450°C. For example, the heating temperature of the substrate is preferably above room temperature and below 500°C, more preferably above 100°C and below 450°C, even more preferably above 200°C and below 450°C, even more preferably above 300°C and below 450°C, and still even more preferably above 400°C and below 450°C.
[0262] For example, microwave plasma treatment can be performed using oxygen and argon gases. In microwave plasma treatment using oxygen and argon gases, the main oxygen free radicals can be triplet oxygen (O(...)). 3 P j Singlet oxygen (O( 1 D2) and oxygen ions (O2) + The three states of the oxide film are as follows. Furthermore, oxygen ions play an effective role in reducing the hydrogen concentration in the oxide film through microwave plasma treatment. Moreover, the amount of oxygen free radicals in each state varies depending on the oxygen flow rate ratio or pressure during microwave plasma treatment. For example, under conditions of low oxygen flow rate ratio and low pressure, there is a tendency for the amount of oxygen ions to increase. On the other hand, when the oxygen flow rate ratio or pressure is too low, there are concerns such as: unstable control of the oxygen flow rate makes it difficult to stabilize the discharge; and etching of the oxide film, etc. Therefore, for example, the oxygen flow rate ratio (O2 / (O2+Ar)) during microwave plasma treatment is preferably greater than 0% and less than 10%, more preferably more than 0.5% and less than 5%, further preferably more than 0.5% and less than 3%, and typically preferably 1%.
[0263] The shorter the processing time of microwave plasma treatment, the higher the productivity. Therefore, for example, the processing time of microwave plasma treatment is preferably more than 1 minute and less than 60 minutes, more preferably more than 1 minute and less than 30 minutes, and even more preferably more than 1 minute and less than 10 minutes.
[0264] By performing microwave plasma treatment in an oxygen-containing atmosphere, oxygen gas can be plasmaized using microwaves or high frequencies such as RF, and the oxygen free radicals generated by this plasmaization can act on the oxide semiconductor layer. Due to the effects of plasma, microwaves, and oxygen free radicals, hydrogen can be removed from the oxide semiconductor layer. This reduces the hydrogen concentration in the oxide semiconductor layer. Sometimes, carbon bonded to oxygen or hydrogen can also be removed. Thus, microwave plasma treatment reduces impurities. Furthermore, by supplying oxygen free radicals to oxygen vacancies formed in the oxide semiconductor layer, the number of oxygen vacancies in the oxide semiconductor layer can be further reduced.
[0265] Furthermore, when some oxygen in the oxide semiconductor present before microwave plasma treatment reacts with hydrogen in the oxide semiconductor, i.e., when the reaction "2H + O → H₂O↑" occurs, this hydrogen can be removed as H₂O (also known as dehydration or dehydrogenation). Since H₂O is one of the main factors hindering the improvement of crystallinity, it is preferable to remove H₂O from the oxide semiconductor. Removing hydrogen from the oxide semiconductor as H₂O reduces the hydrogen concentration in the oxide semiconductor, thereby promoting improved crystallinity. Furthermore, by increasing the temperature in the microwave plasma treatment, the hydrogen concentration in the oxide semiconductor can be further reduced.
[0266] Alternatively, heating treatment can be performed continuously after microwave plasma treatment without exposure to the atmosphere. The heating temperature is preferably 100°C or higher and 750°C or lower, more preferably 300°C or higher and 500°C or lower, and even more preferably 400°C or higher and 450°C or lower.
[0267] Note that plasma treatment containing oxygen gas can also be used instead of microwave plasma treatment to improve crystallinity.
[0268] The oxygen supplied to the oxide semiconductor film 230f can take various forms, such as oxygen atoms, oxygen molecules, oxygen ions (charged oxygen atoms or oxygen molecules), and oxygen free radicals (oxygen atoms, oxygen molecules, or oxygen ions containing unpaired electrons). Furthermore, the oxygen implanted into the oxide semiconductor layer is preferably one or more of the above-mentioned forms, and particularly preferably oxygen free radicals.
[0269] Alternatively, hydrogen can be supplied to the oxide semiconductor film 230f (also known as hydrogenation). By supplying hydrogen to the oxide semiconductor film 230f, dangling bonds present at grain boundaries or the like can sometimes be terminated, thereby improving the electrical characteristics and reliability of the transistor. Furthermore, examples of hydrogen supply processes include heating in a hydrogen-containing atmosphere or plasma treatment.
[0270] Through the above steps, it is possible to manufacture Figure 5CThe oxide semiconductor film is shown. Then, by processing the oxide semiconductor film 230f and the insulating film 224f into island shapes, the oxide semiconductor 230 and the insulator 224 can be formed. At this time, layer 235 can be removed.
[0271] Note that when forming the oxide semiconductor film 230f using the ALD method, it is sometimes possible to form a crystalline oxide semiconductor film 230f using layer 235 as a nucleus during the formation of the oxide semiconductor film 230f. For example, by setting the substrate heating temperature during ALD deposition to a range of 100°C or higher and 300°C or 150°C or higher and 250°C, a crystalline oxide semiconductor film 230f can be formed during deposition. In this case, the heat treatment required for crystallizing the oxide semiconductor film 230f may not be necessary.
[0272] Furthermore, when a crystalline oxide semiconductor film 230f can be formed during the formation of the oxide semiconductor film 230f, at least one of the above-mentioned first heat treatment, second heat treatment, microwave plasma treatment, and hydrogenation treatment can also be performed. This can sometimes further improve the crystallinity of the semi-oxide semiconductor film 230f.
[0273] By using the above-described method for forming the oxide semiconductor film 230f, a large-area oxide semiconductor film 230f can be formed. Therefore, transistors using the oxide semiconductor film 230f and semiconductor chips using these transistors can be mass-produced with high yield. See below for reference. Figures 7A to 7C This describes the manufacturing method of semiconductor chip 238.
[0274] Figure 7A A three-dimensional schematic diagram of substrate 236 is shown. Figure 7A As shown, a layer 235 is formed near the outer periphery of the substrate 236, and then an oxide semiconductor film 230f is formed on the entire surface of the substrate 236 as a cover layer 235. Thus, as... Figure 7B As shown, layer 235 can be used as a seed crystal for crystal growth, thereby forming a single-crystal or polycrystalline oxide semiconductor film 230f with a uniform crystal orientation across the entire surface of substrate 236. More specifically, the crystal orientation of layer 235 is... <001> In this case, crystal orientation can be formed. <111> A crystalline oxide semiconductor film 230f perpendicular to the top surface of the substrate 236. Figure 7B In the diagram, the dividing line 237 is shown as a dashed line. Layer 235 is preferably positioned at a location overlapping the dividing line 237.
[0275] Silicon wafers can typically be used as substrate 236. In addition, insulating substrates such as glass substrates, quartz substrates, sapphire substrates, and yttrium-stabilized zirconia substrates (yttrium-stabilized zirconia substrates), as well as semiconductor substrates such as germanium substrates, silicon carbide substrates, silicon-germanium substrates, gallium arsenide substrates, indium phosphide substrates, zinc oxide substrates, and gallium oxide substrates can be used. Substrate 236 can, for example, be 3-inch, 5-inch, 8-inch, or 12-inch in diameter. In particular, even when using large substrates such as 12-inch substrates, oxide semiconductor films 230f with good crystallinity can be obtained, thereby improving productivity.
[0276] Then, by forming transistors with oxide semiconductor films 230f, wiring, electrodes, etc., multiple semiconductor chips 238 can be formed. Note that for the method of forming transistors, etc., please refer to the following description. Next, as... Figure 7C As shown, multiple semiconductor chips 238 can be separated by dividing the substrate 236 on which semiconductor chips 238 are formed along the dividing line 237. At this time, by placing the layer 235 at a position overlapping with the dividing line 237, a structure in which layer 235 does not remain within the semiconductor chip 238 can be achieved.
[0277] Furthermore, layer 235 can also be disposed outside the dividing line 237. Moreover, layer 235 is not limited to one; two or more layers can be disposed. For example, multiple layers 235 can be disposed at equal intervals and configured to overlap with the dividing line 237 respectively.
[0278] In transistors using oxide semiconductors, if impurities, oxygen vacancies, or V are present in the region where the oxide semiconductor forms the channel, O H, etc., electrical properties are prone to variation, sometimes reducing reliability. In contrast, by performing heat treatment with an insulator containing excess oxygen near the oxide semiconductor, oxygen can be supplied to the oxide semiconductor from the insulator, reducing oxygen vacancies and V. O H. Note that supplying excessive oxygen to the source or drain regions may cause a decrease in the on-state current or field-effect mobility of the transistor 200. Furthermore, if the amount of oxygen supplied to the source or drain regions is uneven within the substrate surface, the characteristics of the semiconductor device, including the transistor, will become uneven. In addition, when oxygen supplied from the insulator to the oxide semiconductor diffuses to the conductors such as the gate, source, and drain electrodes, these conductors may sometimes be oxidized, leading to a loss of conductivity and thus negatively impacting the electrical characteristics and reliability of the transistor.
[0279] Preferably, in the transistor, excessive hydrogen is suppressed in the channel formation region, oxidation of conductors 242a, 242b and 260 is suppressed, and hydrogen concentration reduction in the source and drain regions is suppressed.
[0280] The insulator 250 in contact with the channel formation region in the oxide semiconductor 230 preferably has the function of trapping or fixing hydrogen. This reduces the hydrogen concentration in the channel formation region of the oxide semiconductor 230. Therefore, the Vg in the channel formation region can be reduced. O H is used to make the channel forming region i-shaped or substantially i-shaped.
[0281] Here, as Figure 2A As shown, the insulator 250 preferably has a stacked structure of an insulator 250a in contact with the oxide semiconductor 230, an insulator 250b on the insulator 250a, an insulator 250c on the insulator 250b, and an insulator 250d on the insulator 250c. In this case, the insulators 250a and 250c preferably have the function of capturing or fixing hydrogen.
[0282] Metal oxides with amorphous structures can be cited as insulators capable of trapping or fixing hydrogen. For example, magnesium oxide or oxides containing one or both of aluminum and hafnium are preferred as insulators 250a and 250c. These metal oxides with amorphous structures sometimes possess the property that oxygen atoms have dangling bonds, which trap or fix hydrogen. In other words, metal oxides with amorphous structures have a high ability to trap or fix hydrogen.
[0283] Insulators 250a and 250c are preferably made of high-k materials. Furthermore, an example of a high-k material is an oxide comprising one or both of aluminum and hafnium. When a high-k material is used as insulators 250a and 250c, the gate potential applied during transistor operation can be reduced while maintaining the physical thickness of the gate insulator. Additionally, the equivalent oxide thickness (EOT) of the insulator used as the gate insulator can be reduced.
[0284] As insulators 250a and 250c, it is preferable to use an oxide containing one or both of aluminum and hafnium, and more preferably an oxide having an amorphous structure and containing one or both of aluminum and hafnium.
[0285] In this embodiment, an alumina film is used as the insulator 250a. Furthermore, this alumina preferably has an amorphous structure. Here, by providing the insulator 250a in contact with the oxide semiconductor 230, hydrogen contained in the oxide semiconductor 230 and the like can be more effectively captured and immobilized.
[0286] In this embodiment, hafnium oxide is used as the insulator 250c. Here, by providing the insulator 250c between the insulator 250b and the insulator 250d, hydrogen contained in the insulator 250b and the like can be captured and fixed more effectively.
[0287] Next, silicon oxide or silicon oxynitride, which are thermally stable insulators, are preferably used as insulator 250b. Note that in this specification, oxynitride refers to a material in which the oxygen content is greater than the nitrogen content, while oxynitride refers to a material in which the nitrogen content is greater than the oxygen content. For example, when described as silicon oxynitride, it refers to a material in which the oxygen content is greater than the nitrogen content, while when described as silicon oxynitride, it refers to a material in which the nitrogen content is greater than the oxygen content.
[0288] The silicon oxide film used as the insulator 250b is preferably formed using the PEALD method.
[0289] To suppress oxidation of conductors 242a, 242b, and 260, it is preferable to provide an oxygen-barrier insulator near each of conductors 242a, 242b, and 260. In the semiconductor device described in this embodiment, such insulators are, for example, insulators 250a, 250d, 250c, and 275.
[0290] Note that in this specification, etc., a barrier insulator refers to an insulator that has barrier properties. In this specification, "barrier property" means having the property of hindering the transmission of the corresponding substance (also called low permeability). For example, a barrier insulator has the property that the corresponding substance does not easily diffuse into the interior of the insulator. For example, a barrier insulator has the function of trapping or fixing (also called gettering) the corresponding substance inside the insulator.
[0291] Examples of oxygen barrier insulators include oxides containing one or both of aluminum and hafnium, magnesium oxide, gallium oxide, silicon nitride, and silicon oxynitride. Examples of oxides containing one or both of aluminum and hafnium include aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium (hafnium aluminate), and oxides containing hafnium and silicon (hafnium silicate). For example, insulators 250a, 250c, 250d, and 275 preferably employ a single-layer or multilayer structure of the aforementioned oxygen barrier insulators.
[0292] Insulator 250a preferably has oxygen-barrier properties. Insulator 250a is preferably at least less permeable to oxygen than insulator 280. Insulator 250a has regions that contact the sides of conductor 242a and the sides of conductor 242b. When insulator 250a has oxygen-barrier properties, oxidation of the sides of conductors 242a and 242b, resulting in the formation of an oxide film on those sides, can be suppressed. Therefore, a decrease in the on-state current or field-effect mobility of transistor 200 can be suppressed.
[0293] Furthermore, the insulator 250a is provided in contact with the top and side surfaces of the oxide semiconductor 230 and the top surface of the insulator 222. When the insulator 250a has oxygen-barrier properties, oxygen can be suppressed from escaping from the channel formation region of the oxide semiconductor 230 during heat treatment or similar processes. As a result, oxygen vacancies formed in the oxide semiconductor 230 can be reduced.
[0294] Furthermore, by providing insulator 250a, excessive oxygen supply from insulator 280 to oxide semiconductor 230 is suppressed, while an appropriate amount of oxygen can be supplied to oxide semiconductor 230. Therefore, the decrease in on-state current or field-effect mobility of transistor 200 due to excessive oxidation of the source and drain regions can be suppressed.
[0295] Because oxides containing one or both of aluminum and hafnium have oxygen-blocking properties, they can be suitably used as insulators 250a.
[0296] The insulator 250d preferably also has oxygen-barrier properties. The insulator 250d is disposed between the channel formation region of the oxide semiconductor 230 and the conductor 260, and between the insulator 280 and the conductor 260. By employing this structure, oxygen diffusion from the channel formation region of the oxide semiconductor 230 to the conductor 260, thus preventing the formation of oxygen vacancies in the channel formation region of the oxide semiconductor 230, can be suppressed. Furthermore, the diffusion of oxygen from the oxide semiconductor 230 and the insulator 280 to the conductor 260, thus preventing oxidation of the conductor 260, can be suppressed. The insulator 250d is preferably at least less permeable to oxygen than the insulator 280. For example, a silicon nitride film is preferably used as the insulator 250d. In this case, the insulator 250d is an insulator containing at least nitrogen and silicon.
[0297] Furthermore, the insulator 250d preferably has hydrogen-blocking properties. This prevents impurities such as hydrogen contained in the conductor 260 from diffusing into the oxide semiconductor 230.
[0298] The insulator 275 preferably also has oxygen-barrier properties. The insulator 275 is disposed between the insulator 280 and the conductor 242a, and between the insulator 280 and the conductor 242b. The insulator 275 is disposed in contact with the side surface of the conductor 242, the side surface of the oxide semiconductor 230, and the top surface of the insulator 222. By employing this structure, the diffusion of oxygen contained in the insulator 280 to the conductor 242 can be suppressed. Therefore, the increase in resistivity caused by oxidation of the conductor 242 due to oxygen contained in the insulator 280 can be suppressed. The insulator 275 is preferably at least less permeable to oxygen than the insulator 280. For example, silicon nitride is preferably used as the insulator 275. In this case, the insulator 275 becomes an insulator containing at least nitrogen and silicon.
[0299] To suppress the decrease in hydrogen concentration in the source and drain regions of the oxide semiconductor 230, it is preferable to provide hydrogen barrier insulators near the source and drain regions. In the semiconductor device described in this embodiment, the hydrogen barrier insulator is, for example, insulator 275.
[0300] Examples of hydrogen barrier insulators include oxides such as aluminum oxide, hafnium oxide, and tantalum oxide, as well as nitrides such as silicon nitride. For example, the insulator 275 preferably employs a single-layer structure or a multilayer structure of the aforementioned hydrogen barrier insulators.
[0301] Furthermore, since the sidewalls of the insulator 275 are the sidewalls of the opening 201, the regions of the source and drain regions of the oxide semiconductor 230 that overlap with the opening 201 (or, in other words, the regions of the source and drain regions of the oxide semiconductor 230 that overlap with conductors 242a1 and 242b1 but not with conductors 242a2 and 242b2) are exposed from the insulator 275. Therefore, the insulator 255 covering this region of the oxide semiconductor 230 is preferably a hydrogen barrier insulator (e.g., silicon nitride). Thus, the insulator 255, which serves as a hydrogen barrier insulator, can also cover the regions of the source and drain regions of the oxide semiconductor 230 that are not covered by the insulator 275.
[0302] By setting the aforementioned insulators 275 and 255, hydrogen diffusion from the source and drain regions to the outside can be suppressed, thus preventing the decrease in hydrogen concentration in the source and drain regions. Therefore, the source and drain regions can be n-type.
[0303] By adopting the above structure, the channel forming region can be made i-type or substantially i-type, and the source and drain regions can be made n-type, thereby providing a semiconductor device with excellent electrical characteristics. By adopting the above structure, even when the semiconductor device is miniaturized or highly integrated, it can still possess excellent electrical characteristics. Furthermore, miniaturizing the transistor 200 can improve frequency characteristics. Specifically, the cutoff frequency can be increased.
[0304] Insulators 250a to 250d are used as part of the gate insulator. Insulators 250a to 250d are disposed together with conductor 260 in an opening formed in insulator 280. To achieve miniaturization of transistor 200, the thickness of insulators 250a to 250d is preferably small. The thickness of insulators 250a to 250d is preferably 0.1 nm or more and 10 nm or less, more preferably 0.1 nm or more and 5.0 nm or less, further preferably 0.5 nm or more and 5.0 nm or less, even more preferably 1.0 nm or more and less than 5.0 nm, and even more preferably 1.0 nm or more and 3.0 nm or less. Furthermore, at least a portion of insulators 250a to 250d may have regions with the thicknesses described above.
[0305] Furthermore, the thickness of the silicon oxide film used as insulator 250b is preferably 0.7 nm or more and 3 nm or less.
[0306] To reduce the thickness of insulators 250a to 250d as described above, deposition using the ALD method is preferred. Furthermore, to provide insulators 250a to 250d within openings in insulators 280, etc., deposition using the ALD method is also preferred. ALD methods include thermal ALD and PEALD. In the PEALD method, deposition can be performed at lower temperatures by utilizing plasma, and therefore it is sometimes preferred.
[0307] ALD (Alternating Layer Deposition) can deposit atoms layer by layer, thus offering advantages such as the ability to deposit extremely thin layers, deposit structures with high aspect ratios, deposit with few defects such as pinholes, achieve high coverage, and deposit at low temperatures. Therefore, a thin insulator 250 can be deposited with high coverage on the sides of openings formed in the insulator 280 and on the side ends of conductors 242a and 242b.
[0308] Note that the precursors used in the ALD method sometimes contain carbon and other impurities. Therefore, films prepared using the ALD method sometimes contain more carbon and other impurities compared to films prepared using other deposition methods. Furthermore, the quantification of impurities can be performed using SIMS, XPS, or Auger Electron Spectroscopy (AES).
[0309] Note that in the above description, insulator 250 has a four-layer structure of insulators 250a to 250d, but the present invention is not limited thereto. Insulator 250 may have a structure including at least one of insulators 250a to 250d. By having insulator 250 composed of one, two, or three layers of insulators 250a to 250d, the manufacturing process of semiconductor devices can be simplified, thereby improving productivity.
[0310] For example, such as Figure 11A As shown, the insulator 250 can also have a three-layer structure. In this case, the insulator 250 preferably has a stacked structure of insulator 250a, insulator 250b on insulator 250a, and insulator 250d on insulator 250b. In other words, it has a structure consisting of... Figure 2A The structure shown is the structure obtained by removing insulator 250c. However, it is not limited to this; for example, insulator 250 may also have a stacked structure of insulator 250b, insulator 250c on insulator 250b, and insulator 250d on insulator 250c. In other words, it has a structure from... Figure 2A The structure shown is the structure obtained by removing insulator 250a.
[0311] When forming the insulator 250, it is preferable to perform the ALD process twice or more. For example, it is preferable that the insulator 250 has a laminated structure composed of multiple insulating films, and that two or more of the multiple insulating films are formed using the ALD process. By forming at least two insulating films using the ALD process, the coverage and thickness uniformity of the insulator 250 can be improved. In addition, by continuously forming two or more different films, such as two or more insulating films, using the ALD process, productivity can be improved.
[0312] In addition to the structure described above, it is preferable to also have a structure that suppresses hydrogen ingress into the transistor 200, etc. For example, it is preferable to provide an insulator that has the function of suppressing hydrogen diffusion by covering one or both of the top and bottom of the transistor 200, etc. In the semiconductor device described in this embodiment, the insulator is, for example, insulator 283, insulator 282, insulator 222, and insulator 221, etc. In addition, the insulator 215 provided under the transistor 200 may also have the same structure as either or both of insulator 282 and insulator 283. In this case, the insulator 215 may have a stacked structure of insulator 282 and insulator 283, and may have a structure in which insulator 282 is below and insulator 283 is above, or may have insulator 282 above and insulator 283 below.
[0313] One or more of insulators 283, 282, 222, and 221 are preferably used as barrier insulators to suppress the diffusion of impurities such as water and hydrogen from the substrate side or above the transistor 200. Therefore, one or more of insulators 283, 282, 222, and 221 preferably comprise an insulating material that functions to suppress the diffusion of impurities such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules (N2O, NO, NO2, etc.), and copper atoms (making it difficult for the aforementioned impurities to permeate). Furthermore, it is preferable to include an insulating material that functions to suppress the diffusion of oxygen (e.g., at least one of oxygen atoms, oxygen molecules, etc.) (making it difficult for the aforementioned oxygen to permeate).
[0314] Insulators 283, 282, 222, and 221 preferably all include insulators that suppress the diffusion of impurities such as water and hydrogen, as well as oxygen. Examples of suitable materials include aluminum oxide, magnesium oxide, hafnium oxide, zirconium oxide, oxides containing aluminum and hafnium (hafnium aluminate), oxides containing hafnium and zirconium (hafnium zirconium oxide), gallium oxide, silicon nitride, or silicon oxynitride. For example, insulators 283 and 221 preferably use silicon nitride, which has higher hydrogen barrier properties. Furthermore, insulator 282 preferably uses aluminum oxide, which has a high ability to trap or fix hydrogen. Similarly, insulator 222 preferably uses hafnium oxide, which has a high ability to trap or fix hydrogen and is a high-k dielectric constant material.
[0315] Note that, as at least one of insulators 221 and 222, a multilayer structure of silicon oxide or silicon oxynitride may be used in addition to the materials described above. For example, a multilayer structure of silicon nitride and silicon oxide may also be used as insulator 221. Furthermore, for example, insulator 222 may have a multilayer structure of hafnium oxide and silicon oxide.
[0316] By employing this structure, the diffusion of impurities such as water and hydrogen from the interlayer insulating film disposed above insulator 283 to transistor 200 and the like can be suppressed. Furthermore, the diffusion of impurities such as water and hydrogen from the interlayer insulating film disposed below insulator 221 to transistor 200 and the like can be suppressed. Additionally, hydrogen in insulators 280 and 250 can be captured or fixed to insulator 282 or insulator 222. Furthermore, by providing insulators 282 and 283, the diffusion of oxygen from insulator 280 to the top of transistor 200 and the like can be suppressed. Furthermore, by providing insulators 222 and 221, the diffusion of oxygen from oxide semiconductor 230 to the bottom of transistor 200 and the like can be suppressed. Thus, by employing a structure in which insulators with the function of suppressing the diffusion of impurities such as water and hydrogen, as well as oxygen, surround the top and bottom of transistor 200, the diffusion of excess oxygen and hydrogen to oxide semiconductor can be suppressed. This results in improved electrical characteristics and reliability of the semiconductor device.
[0317] Furthermore, insulators 275 and 250d are preferably made of silicon nitride or the like, which have higher hydrogen barrier properties. Additionally, insulator 250a is preferably made of alumina or the like, which has a high ability to trap or fix hydrogen. Furthermore, insulator 250c is preferably made of hafnium oxide or the like, which has a high ability to trap or fix hydrogen.
[0318] Insulator 225 is formed in contact with the top surface of insulator 224. For example... Figure 2B and Figure 13A As shown, the insulator 225 has a high aspect ratio when viewed in cross-section along the channel width direction. The height H of the insulator 225 is preferably greater than the width L of the insulator 225. The height H of the insulator 225 can be more than 1 and less than 20 times the width L, preferably more than 1.3 and less than 15 times, more preferably more than 1.5 and less than 10 times. For example, the width L can be more than 5 nm and less than 100 nm, preferably more than 5 nm and less than 50 nm, more preferably more than 8 nm and less than 30 nm. Furthermore, for example, the height H can be more than 30 nm and less than 300 nm, preferably more than 50 nm and less than 150 nm.
[0319] In addition, such as Figure 2B As shown, when viewed in cross-section along the channel width direction, the angle θ formed by the side surface of the insulator 225 and the top surface of the insulator 224 is preferably perpendicular or substantially perpendicular. For example, the angle θ is preferably 80° or more and 100° or less, more preferably 85° or more and 95° or less.
[0320] In addition, the top of the insulator 225 may also have a curved shape. By having the above-mentioned curved shape, defects such as voids can be prevented from forming in the oxide semiconductor 230 and conductor 242 near the upper part of the insulator 225.
[0321] An oxide semiconductor 230 and a conductor 242 are disposed such that the high aspect ratio insulator 225 is covered. Near the channel formation region of the transistor 200, such as... Figure 2B As shown, an oxide semiconductor 230 is disposed in a folded state, sandwiching an insulator 225, and an insulator 250 and a conductor 260 are disposed to cover the oxide semiconductor 230. As a result, the channel width of the transistor 200 increases on the side of the insulator 225 on the A1 side and the side of the insulator 225 on the A2 side.
[0322] As described above, increasing the channel width can improve the on-state current, field-effect mobility, and frequency characteristics of the transistor 200. This provides a semiconductor device with a high operating speed. Furthermore, it can increase the operating speed of memory devices using this semiconductor device. In addition, in the above structure, by providing the insulator 225, the channel width can be increased without increasing the area occupied by the transistor 200. This allows for miniaturization or high integration of the semiconductor device. Furthermore, it can increase the storage capacity of memory devices using this semiconductor device.
[0323] The bottom surface of insulator 224 contacts insulator 222, and the top surface contacts insulator 225 and oxide semiconductor 230. The planar shape of insulator 224 is the same as that of oxide semiconductor 230, and in plan view, insulator 224 overlaps with oxide semiconductor 230. In other words, in plan view, the side surface of insulator 224 is aligned or substantially aligned with the side surface of oxide semiconductor 230. Furthermore, in plan view, at least a portion of insulator 224 overlaps with conductors 242a (conductors 242a1 and 242a2) and conductors 242b (conductors 242b1 and 242b2). In other words, in plan view, at least a portion of the side surface of insulator 224 is aligned or substantially aligned with the side surface of conductors 242a (conductors 242a1 and 242a2) and the side surface of conductors 242b (conductors 242b1 and 242b2).
[0324] like Figure 2B As shown, the thickness t1 of the insulator 224 within the opening 201 is preferably greater than the thickness t2 of the insulator 250. By adopting this structure, the bottom surface of the conductor 260 (conductor 260a) located within the opening 201 can be positioned below the bottom surface of the oxide semiconductor 230 by the difference between the thicknesses t1 and t2 (t1-t2).
[0325] By positioning the bottom surface of the conductor 260 below the bottom surface of the oxide semiconductor 230, a sufficient gate electric field can be applied to the upper and lower ends of the oxide semiconductor 230. In other words, the entire oxide semiconductor 230 can be electrically surrounded by the electric field of the conductor 260 within the opening of the insulator 280, etc., and used as a channel formation region. By employing this structure, the lower end of the oxide semiconductor 230 can be prevented from being used as a parasitic channel, thereby reducing the leakage current between the source and drain electrodes. Furthermore, characteristic defects such as always-on switching of the transistor caused by this parasitic channel can be suppressed. That is, the electrical characteristics of the transistor 200 can be improved.
[0326] As described above, by using the upper to lower ends of the oxide semiconductor 230 as the channel formation region, the channel width can be increased. This improves the on-state current, transconductance, frequency characteristics, etc., of the transistor 200.
[0327] Note that in this specification, the transistor structure described above, in which the electric field of the gate electrode forms a region around the channel, is referred to as a surrounded channel (S-channel) structure. In an S-channel structure, the gate electrode is arranged with at least two or more surfaces surrounding the channel (specifically, two, three, or four surfaces, etc.). By employing an S-channel structure, tolerance to short-channel effects can be improved; in other words, transistors that are less prone to short-channel effects can be realized.
[0328] Furthermore, the S-channel structure is a structure in which the electrical field forms a region around the channel, so it can be said that this structure is essentially the same as the GAA (Gate All Around) structure or the LGAA (Lateral Gate All Around) structure. By giving the transistor 200 an S-channel structure, a GAA structure, or an LGAA structure, the channel formation region formed at or near the interface between the oxide semiconductor 230 and the gate insulator can be located over the entire bulk. Therefore, the current density flowing through the transistor can be increased, and thus an increase in the transistor's on-state current or field-effect mobility can be expected.
[0329] As insulators 225 and 224, insulating materials suitable for insulators 222, 275, 280, and 250 can be used. As described above, silicon oxide or silicon nitride, which have a lower coefficient of thermal expansion than indium oxide used in oxide semiconductor 230, can be used as insulators 225 and 224. Furthermore, since insulators 225 and 224 are in contact with oxide semiconductor 230, as described above, insulating materials with low hydrogen release are preferred. Examples of such insulating materials with low hydrogen release include silicon nitride, silicon oxynitride, aluminum oxide, hafnium oxide, oxides containing aluminum and hafnium (hafnium aluminate), and oxides containing hafnium and silicon (hafnium silicate). This suppresses hydrogen incorporation into oxide semiconductor 230. In particular, when silicon nitride is used as at least one of insulators 225 and 224, the reliability of the transistor can be improved. Furthermore, insulators 225 and 224 are preferably used as hydrogen-barrier insulators, and preferably have the property that hydrogen does not easily diffuse into the interior of the insulator or the function of capturing or fixing hydrogen inside the insulator. Therefore, insulators 225 and 224 can also use the insulating materials described above for use as hydrogen-barrier insulators.
[0330] For example, silicon nitride can be used for insulators 225 and 224. Alternatively, silicon nitride can be used for insulator 225, and silicon oxide can be used for insulator 224. In these cases, the thickness of the region of insulator 224 that does not overlap with insulator 225 is sometimes smaller than the region of insulator 224 that overlaps with insulator 225. Furthermore, a structure can be adopted where hafnium silicate is used as insulator 225 and silicon nitride is provided as insulator 224. By adopting this structure, insulator 224 can suppress hydrogen diffusion from the lower side, and insulator 225 can trap or fix hydrogen in the region surrounded by insulator 224 and insulator 250. Thus, the hydrogen concentration in the region surrounded by insulator 224 and insulator 250 can be reduced.
[0331] Furthermore, even if the thickness of the oxide semiconductor 230 is reduced as described above, the oxide semiconductor 230 can be supported by the insulator 225 by providing the oxide semiconductor 230 in a manner that covers the insulator 225 with a high aspect ratio. Therefore, the oxide semiconductor 230 can be formed extending upward relative to the substrate without tilting. Thus, the channel width can be increased without increasing the occupied area.
[0332] Furthermore, the above example shows an insulator 224 disposed beneath insulator 225, but the present invention is not limited thereto. Figure 9AAs shown, a structure without insulator 224 can also be used. In this case, insulator 225 and oxide semiconductor 230 are formed in contact with the top surface of insulator 222. Furthermore, when oxide semiconductor 230 is processed into an island shape or an opening 201 is formed, sometimes a portion of the top surface of insulator 222 is removed. Thus, as... Figure 9A As shown, sometimes the top surface of the region of insulator 222 that overlaps with oxide semiconductor 230 is higher than the top surface of the region of insulator 222 that does not overlap with oxide semiconductor 230.
[0333] Furthermore, the above example shows an example where the side of insulator 225 is located inside the side of insulator 224, but the present invention is not limited thereto. Figure 9B As shown, the side surface of insulator 225 can also be formed in an aligned manner with the side surface of insulator 224. Here, the lower end of the side surface of insulator 225 can be aligned with or substantially aligned with the upper end of the side surface of insulator 224.
[0334] In addition, such as Figure 8A As shown, a conductor 205 can also be disposed inside the insulator 225. The conductor 205 is disposed on the insulator 224, and its top and side surfaces are covered by the insulator 225. The conductor 205 has a region serving as the second gate electrode (lower gate electrode) of the transistor 200. Additionally, the insulator 225 has a region serving as the second gate insulator of the transistor 200. Here, since... Figure 8A Corresponding to Figure 2B Therefore, for detailed structure information, please refer to the above description. Conductor 205 can use the same conductive material as conductor 260 described later. Furthermore, conductor 205 can have a single-layer structure or a multi-layer structure.
[0335] In addition, such as Figure 8B As shown, in a structure where the conductor 205 is disposed inside the insulator 225, the insulator 224 may not be provided. In this case, the conductor 205, the insulator 225, and the oxide semiconductor 230 are formed in contact with the top surface of the insulator 222. Furthermore, when the oxide semiconductor 230 is processed into an island shape or an opening 201 is formed, sometimes a portion of the top surface of the insulator 222 is removed. Therefore, as... Figure 8B As shown, sometimes the top surface of the region of insulator 222 that overlaps with oxide semiconductor 230 is higher than the top surface of the region of insulator 222 that does not overlap with oxide semiconductor 230.
[0336] In addition, such as Figure 8C As shown, when depositing the oxide semiconductor film 230f, the oxide semiconductor film 230f is deposited in such a way that it covers a pillar composed of a conductor 205 and an insulator 225 covering the conductor 205.
[0337] Alternatively, the conductor 205 can be extended and used as wiring. Furthermore, a plug can be provided on or below the conductor 205 to connect the conductor 205 to the wiring. Alternatively, the wiring can be embedded in the insulator 224 or both the insulator 224 and the insulator 225, and the conductor 205 can be provided in contact with the wiring.
[0338] Furthermore, the above example illustrates an oxide semiconductor 230 disposed in a manner covering the insulator 225, but the present invention is not limited thereto. Figure 10A As shown, the sidewall-shaped oxide semiconductor 230 is sometimes provided in contact with the side of the insulator 225. For example, when the conductor is divided into conductor 242a1 and conductor 242b1, sometimes the portion of oxide semiconductor 230 in contact with the top surface of the insulator 225 and the portion in contact with the top surface of the insulator 222 is removed, while the portion of oxide semiconductor 230 in contact with the side of the insulator 225 remains. Even if the oxide semiconductor 230 has the above structure, by increasing the height H of the insulator 225, the channel width of the transistor 200 can be made sufficiently large.
[0339] In addition, such as Figure 10B As shown, insulator 224 may have a structure including insulator 224a and insulator 224b on insulator 224a, and insulator 225 may have a structure including insulator 225a and insulator 225b on insulator 225a. Here, insulator 224a and insulator 225a may use insulating materials with low hydrogen release, such as silicon nitride.
[0340] As insulator 225b, the insulating material used as a hard mask in the etching process of insulator 225a can be used. For example, when silicon nitride is used for insulator 225a, aluminum oxide can be used for insulator 225b. In this case, the thickness of insulator 225b can also be smaller than that of insulator 225a.
[0341] As insulator 224b, an insulating material that is used as an etch stop layer in the etching process of insulator 225a can be used. For example, when silicon nitride is used for insulator 225a, aluminum oxide can be used for insulator 224b. In this case, the thickness of insulator 224b can also be smaller than that of insulator 224a.
[0342] Alternatively, silicon nitride with high hydrogen barrier properties can be used as insulator 224b. When insulator 224b can sufficiently suppress the diffusion of impurities such as hydrogen contained in insulator 224a, insulating materials such as silicon oxide that allow hydrogen to pass through can also be used as insulator 224a.
[0343] The conductors 242a, 242b, and 260 are preferably made of conductive materials that are not easily oxidized or have the function of inhibiting oxygen diffusion. Examples of such conductive materials include nitrogen-containing conductive materials and oxygen-containing conductive materials. This can suppress the decrease in conductivity of conductors 242a, 242b, and 260. When conductive materials containing metals and nitrogen are used as conductors 242a, 242b, and 260, conductors 242a, 242b, and 260 are conductors that contain at least metals and nitrogen.
[0344] Conductors 242a and 242b are disposed separately from each other through opening 201 and are arranged in contact with oxide semiconductor 230. For example... Figure 13A As shown, the conductor 242 is arranged to cover the insulator 225 with a high aspect ratio.
[0345] Here, near the source or drain of transistor 200, such as Figure 13A As shown, the oxide semiconductor 230 and the conductor 242a are arranged in a folded state, sandwiching the insulator 225. Therefore, when viewed in cross-section along the channel width direction, the conductor 242a contacts the oxide semiconductor 230 at the top of the insulator 225, on the side surface on the A3 side, on the side surface on the A4 side, and near the insulator 224. Consequently, the contact area between the conductor 242a and the oxide semiconductor 230 is larger than that without the insulator 225, particularly on the A3 and A4 sides of the insulator 225. Note that in... Figure 13A and Figure 1C The diagram shows the vicinity of conductor 242a, and the same applies to conductor 242b. In other words, similar to conductor 242a and oxide semiconductor 230, the contact area between conductor 242b and oxide semiconductor 230 is increased.
[0346] As described above, by increasing the contact area between the conductor 242 and the oxide semiconductor 230, the contact resistance between the conductor 242 and the oxide semiconductor 230 can be reduced without increasing the occupied area of the transistor 200. Therefore, the on-state current, frequency characteristics, etc., of the transistor 200 can be improved. This provides a semiconductor device with high operating speed. Furthermore, the operating speed of a memory device using this semiconductor device can be increased. Thus, miniaturization or high integration of the semiconductor device can be achieved. Additionally, the storage capacity of a memory device using this semiconductor device can be increased.
[0347] like Figure 1D and Figure 2AAs shown, conductors 242a and 242b preferably have a two-layer structure. Conductor 242a is a stacked film of conductor 242a1 and conductor 242a2 on conductor 242a1, and conductor 242b is a stacked film of conductor 242b1 and conductor 242b2 on conductor 242b1. In this case, as the layer (conductors 242a1 and conductor 242b1) in contact with the oxide semiconductor 230, it is preferable to use a conductive material that is not easily oxidized or a conductive material that has the function of inhibiting oxygen diffusion. This can suppress the decrease in conductivity of conductors 242a and 242b. Furthermore, it can suppress the formation of excessive oxygen vacancies due to oxygen extraction from the oxide semiconductor 230. Additionally, when a material that easily absorbs (extracts) hydrogen is used as the layer (conductors 242a1 and conductor 242b1) in contact with the oxide semiconductor 230, the hydrogen concentration of the oxide semiconductor 230 can be reduced, which is therefore preferred.
[0348] Metal nitrides are preferably used as conductors 242a1 and 242b1, such as nitrides containing tantalum, titanium, molybdenum, tungsten, tantalum and aluminum, and titanium and aluminum. In one aspect of the invention, tantalum-containing nitrides are particularly preferred. Furthermore, ruthenium, ruthenium oxide, ruthenium nitride, oxides containing strontium and ruthenium, and oxides containing lanthanum and nickel may also be used, for example. These materials are preferred because they are conductive materials that are not easily oxidized or maintain conductivity even when absorbing oxygen.
[0349] Note that sometimes hydrogen contained in the oxide semiconductor 230, etc., diffuses into the conductor 242a1 or conductor 242b1. In particular, by using a tantalum-containing nitride as conductor 242a1 and conductor 242b1, sometimes hydrogen contained in the oxide semiconductor 230, etc., readily diffuses into conductor 242a1 or conductor 242b1, and the diffused hydrogen bonds with the nitrogen contained in conductor 242a1 or conductor 242b1. That is, sometimes hydrogen contained in the oxide semiconductor 230, etc., is absorbed by conductor 242a1 or conductor 242b1.
[0350] The conductivity of conductors 242a2 and 242b2 is preferably higher than that of conductors 242a1 and 242b1. For example, the thickness of conductors 242a2 and 242b2 is preferably greater than that of conductors 242a1 and 242b1. Conductive materials with tungsten, copper, or aluminum as their main components can be used as conductors 242a2 and 242b2, for example. By adopting the above structure, the resistance of conductors 242a2 and 242b2 can be reduced. Therefore, the on-state current of transistor 200 can be increased, thereby improving the operating speed of the semiconductor device according to this embodiment.
[0351] For example, tantalum nitride or titanium nitride can be used as conductors 242a1 and 242b1, and tungsten can be used as conductors 242a2 and 242b2.
[0352] By employing the above structure, the top surface of the oxide semiconductor 230 is exposed in the region between the conductors 242a1 and 242b1, and the insulator 250 contacts this region. Here, as... Figure 11B As shown, sometimes the top surface of the oxide semiconductor 230 in this region is lower than that in other regions. That is, in the oxide semiconductor 230, the top surface of the region between conductors 242a1 and 242b1 is sometimes lower than the top surface of the region overlapping with conductors 242a1 or 242b1. In this case, sometimes the thickness of the portion of the oxide semiconductor 230 that contacts the top surface of the insulator 225 is smaller than the thickness of the portion of the oxide semiconductor 230 that contacts the side surface of the insulator 225. Furthermore, sometimes the portion of the oxide semiconductor 230 that contacts the top surface of the insulator 225, or a portion thereof, is removed, and a portion of the insulator 225 contacts the insulator 250.
[0353] Furthermore, to suppress the decrease in conductivity of conductors 242a and 242b, a crystalline oxide is preferably used as the oxide semiconductor 230. Additionally, a metal oxide comprising indium, zinc, and one or more metals selected from gallium, aluminum, and tin is preferably used. When a crystalline oxide is used, oxygen extraction from the oxide semiconductor 230 by conductors 242a or 242b can be suppressed. Furthermore, the decrease in conductivity of conductors 242a and 242b can be suppressed.
[0354] like Figure 1B and Figure 1D As shown, insulator 255 is disposed in opening 201 formed in insulator 280, etc., and is in contact with the side surface of insulator 280, side surface of insulator 275, side surface of conductor 242a2, side surface of conductor 242b2, top surface and side surface of conductor 242a1, top surface and side surface of conductor 242b1, and top surface of insulator 222. In other words, it can be said that an opening is formed in insulator 255 in such a way as to expose the island-shaped oxide semiconductor 230 within opening 201. Furthermore, in the region of insulator 255 where the opening is formed, insulator 250 is in contact with oxide semiconductor 230, insulator 224, and insulator 222. Note that in Figure 1BIn this invention, the insulator 255 has an opening only near the oxide semiconductor 230, but the invention is not limited thereto. The insulator 255 may have an opening at least in the region of the oxide semiconductor 230 sandwiched between the conductors 242a1 and 242b1. Therefore, for example, the insulator 255 may also be formed as a sidewall in the opening formed in the insulator 280 with almost no region in contact with the insulator 222.
[0355] The insulator 255 is formed in contact with the sides of the conductors 242a2 and 242b2, and serves as an inorganic insulator protecting the conductors 242a2 and 242b2. Because it is exposed to an oxidizing atmosphere, the insulator 255 is preferably an inorganic insulator that is not easily oxidized. Furthermore, since the insulator 255 is in contact with the conductors 242a2 and 242b2, it is preferably an inorganic insulator that does not easily oxidize the conductors 242a2 and 242b2. Therefore, the insulator 255 is preferably made of an insulating material suitable for use with the oxygen-barrier insulator 250d. For example, silicon nitride can be used as the insulator 255.
[0356] By using this insulator 255, even after heat treatment in an oxygen-containing atmosphere after the conductors are divided into conductors 242a1 and conductors 242b1 and before the insulator 250 is deposited, conductors 242a2 and conductors 242b2 will not be excessively oxidized. For example, the thickness of the oxide film on the side surface near the conductor 260 of conductors 242a2 and conductors 242b2 can be 0.5 nm or more and 5 nm or less, preferably 0.5 nm or more and 3 nm or less, and more preferably 0.5 nm or more and 2 nm or less.
[0357] Furthermore, the thickness of insulator 255 is preferably greater than that of any one of insulators 250a to 250d. The thickness of insulator 255 is preferably 1 nm or more and 20 nm or less, more preferably 1 nm or more and 15 nm or less, and even more preferably 3 nm or more and 10 nm or less; for example, it can be set to about 5 nm. When insulator 255 has the above-mentioned thickness, the distance between conductor 260 and conductor 242a or conductor 242b can be increased, thereby reducing parasitic capacitance. Note that insulator 255 only needs to have a region with the above-mentioned thickness in at least a portion thereof. Additionally, since insulator 255 is disposed in the opening formed in insulator 280, deposition using a method with good coverage, such as ALD, is preferable.
[0358] Furthermore, the insulator 255 may also have a multilayer structure with two or more layers using the aforementioned inorganic insulator that is not easily oxidized. When the insulator 255 has a multilayer structure with two or more layers, it is sufficient that at least one layer is the aforementioned inorganic insulator that is not easily oxidized. For example, the insulator 255 may have a two-layer structure of a silicon nitride film and a silicon oxide film on the silicon nitride film.
[0359] Additionally, the insulator 255 is used as part of a mask when dividing the conductor into conductor 242a1 and conductor 242b1. Therefore, as... Figure 2A As shown, when the transistor 200 is viewed in cross section, the side end of the insulator 255 is preferably the same as or substantially the same as the side end of the conductor 242a1 and the side end of the conductor 242b1.
[0360] Here, in conductor 242a1, the portion on the top surface where the insulator 255 is formed (hereinafter sometimes referred to as the protrusion of conductor 242a1) is formed in such a way that it protrudes towards conductor 260 compared to conductor 242a2. Similarly, in conductor 242b1, the portion on the top surface where the insulator 255 is formed (hereinafter sometimes referred to as the protrusion of conductor 242b1) is formed in such a way that it protrudes towards conductor 260 compared to conductor 242b2. Figure 2A As shown, when viewed in cross-section along the channel length of transistor 200, the distance D1 between conductor 242a1 and conductor 242b1 is less than the distance D2 between conductor 242a2 and conductor 242b2.
[0361] The distance D1 between conductors 242a1 and 242b1 reflects the channel length of transistor 200, and is therefore preferably small. For example, the distance D1 is preferably 60 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less and more than 1 nm or more, or more than 5 nm. For example, the distance D1 is more preferably 2 nm or more and about 20 nm or less. By adopting this structure, the distance between the source and drain can be further shortened, and the channel length can be correspondingly reduced. Therefore, the frequency characteristics of transistor 200 can be improved. Thus, by reducing the channel length of the semiconductor device, a semiconductor device with improved operating speed can be provided.
[0362] In addition, Figure 2A In the transistor 200 shown, the opposing sides of conductors 242a1 and 242b1 are substantially perpendicular to the top surface of the oxide semiconductor 230, but the invention is not limited thereto. For example, as Figure 12AAs shown, the opposing sides of conductors 242a1 and 242b1 can also be tapered. By adopting the above shape, the distance between conductor 260 and oxide semiconductor 230 is reduced near the side ends of conductors 242a1 and 242b1, so a gate electric field can be effectively applied to oxide semiconductor 230.
[0363] In addition, such as Figure 12B As shown, the opposing sides of conductors 242a1 and 242b1 can also be tapered, and the opposing sides of conductors 242a2 and 242b2 can also be tapered. Furthermore, as... Figure 12C As shown, a structure with a smaller cone angle than that of conductors 242a1 and 242b1 can also be adopted.
[0364] Note that the above description shows an example where conductors 242a and 242b have a two-layer stacked structure; however, the present invention is not limited thereto, and conductors 242a and 242b may also have a single-layer or three-layer stacked structure. For example, as... Figure 11C As shown, conductors 242a and 242b can also have a single-layer structure. In this case, conductive materials suitable for conductors 242a1 and 242b1 can be used as conductors 242a and 242b1. Furthermore, at this time, as... Figure 11C As shown, a structure can also be adopted in which the insulator 280 and the insulator 275 are in contact with the insulator 250 without the insulator 255.
[0365] like Figure 1B and Figure 1D As shown, the conductor 260 is disposed within an opening 201 formed in the insulator 280 and the insulator 275. The conductor 260 is disposed within the opening 201, separated by the insulator 250, in a manner that covers the top surface of the insulator 222, the side surface of the oxide semiconductor 230, and the top surface of the oxide semiconductor 230. Furthermore, as... Figure 2A As shown, a portion of conductor 260 overlaps with a portion of conductor 242a1 and a portion of conductor 242b1, separated by insulator 255. Furthermore, the top surface of conductor 260 is arranged such that its height is the same as or substantially the same as the height of the uppermost part of insulator 255, the uppermost part of insulator 250, and the top surface of insulator 280.
[0366] In the opening 201 where the conductor 260 and the insulator 250 are provided, the sidewall of the opening 201 may be perpendicular or substantially perpendicular to the top surface of the insulator 222, and may also have a conical shape. By making the sidewall conical, the coverage of the insulator 250 and the like provided in the opening of the insulator 280 is improved, thereby reducing defects such as voids.
[0367] Conductor 260 is used as the first gate electrode of transistor 200. Here, as... Figure 1A and Figure 1B As shown, the conductor 260 is preferably provided extending in the channel width direction. By adopting this structure, the conductor 260 is used as wiring when multiple transistors are arranged.
[0368] A portion of the conductor 260 is disposed in a folded state, with the insulator 225 in between. Thus, as... Figure 2B As shown, when viewed in cross-section along the channel width direction, the oxide semiconductor 230 and the conductor 260 are positioned opposite each other with the insulator 224 in the upper part of the oxide semiconductor 230, the side surface on the A1 side, the side surface on the A2 side, and near the insulator 224. In other words, the upper part of the oxide semiconductor 230, the side surface on the A1 side, the side surface on the A2 side, and the vicinity of the insulator 224 are all used as channel formation regions. Therefore, compared to the case where the insulator 225 is not provided, the channel width of the transistors 200 on the side surface on the A1 side and the side surface on the A2 side of the oxide semiconductor 230 is larger.
[0369] exist Figure 1D In this embodiment, the conductor 260 has a two-layer structure. Preferably, the conductor 260 includes a conductor 260a and a conductor 260b disposed on the conductor 260a. For example, it is preferable that the conductor 260a is disposed such that it surrounds the bottom and side surfaces of the conductor 260b. In this case, the conductor 260a is preferably made of a conductive material that is not easily oxidized or a conductive material that has the function of inhibiting oxygen diffusion.
[0370] The conductor 260a preferably uses a conductive material that has the function of suppressing the diffusion of impurities such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules, and copper atoms. Furthermore, it is preferable to use a conductive material that has the function of suppressing the diffusion of oxygen (e.g., at least one of oxygen atoms, oxygen molecules, etc.).
[0371] Furthermore, when the conductor 260a has the function of suppressing oxygen diffusion, it can prevent oxygen contained in the insulator 280, etc., from oxidizing the conductor 260b and causing a decrease in conductivity. As a conductive material with the function of suppressing oxygen diffusion, titanium, titanium nitride, tantalum, tantalum nitride, ruthenium, ruthenium oxide, etc., are preferably used, for example.
[0372] Furthermore, the conductor 260b is preferably a conductor with high conductivity. For example, the conductor 260b can be a conductive material with tungsten, copper, or aluminum as the main component. In addition, the conductor 260b can have a laminated structure, for example, it can have a laminated structure of titanium or titanium nitride with the aforementioned conductive material.
[0373] Furthermore, in the transistor 200, the conductor 260 is formed in a self-aligned manner by filling the opening 201 formed in the insulator 280, etc. Here, the side surface of the insulator 280 in the opening 201 is aligned or substantially aligned with the side surface of the conductor 242a2 and the side surface of the conductor 242b2. Therefore, the conductor 260 can be arranged to overlap with the area between the conductor 242a2 and the conductor 242b2 without alignment.
[0374] The dielectric constants of insulators 216 and 280 are preferably lower than those of insulator 222. By using materials with low dielectric constants for the interlayer film, parasitic capacitances generated between wirings can be reduced.
[0375] For example, insulator 216 and insulator 280 preferably comprise one or more of silicon oxide, silicon oxynitride, fluorine-added silicon oxide, carbon-added silicon oxide, carbon and nitrogen-added silicon oxide, and porous silicon oxide.
[0376] In particular, silicon oxide and silicon oxynitride are preferred due to their thermal stability. Especially, materials such as silicon oxide, silicon oxynitride, and porous silicon oxide are preferred because they readily form regions containing oxygen that has been released upon heating.
[0377] In addition, the top surfaces of insulators 216 and 280 can also be planarized.
[0378] The concentration of impurities such as water and hydrogen in the insulator 280 is preferably reduced. For example, silicon oxides such as silicon oxynitride are preferably used as the insulator 280.
[0379] Conductors 240a and 240b are both formed within the openings of insulators 275, 280, 282, and 283. The bottom surface of conductor 240a contacts the top surface of conductor 242a, and the bottom surface of conductor 240b contacts the top surface of conductor 242b. Here, the height of the top surface of conductor 240a is approximately the same as the height of the top surface of insulator 283.
[0380] The conductor 240 is preferably made of a conductive material with tungsten, copper, or aluminum as its main components. Alternatively, the conductor 240 may also be a laminated structure in which a first conductor is disposed in contact with the side of the insulator 241 and a second conductor is disposed inside it. In this case, the aforementioned conductive material can be used as the second conductor. Here, the aforementioned first conductor corresponds to... Figure 13A The conductor 240a1 shown above corresponds to the second conductor mentioned above. Figure 13A The conductor shown is 240a2.
[0381] Furthermore, when a multilayer structure is adopted as the conductor 240, a conductive material with the function of suppressing the permeation of impurities such as water and hydrogen is preferably used as the first conductor disposed near insulators 283, 282, 280, and 275. For example, tantalum, tantalum nitride, titanium, titanium nitride, ruthenium, ruthenium oxide, etc. are preferred. Alternatively, a single layer or a multilayer of conductive material with the function of suppressing the permeation of impurities such as water and hydrogen can also be used. By adopting this structure, impurities such as water and hydrogen contained in the layer above insulator 283 can be suppressed from mixing into oxide semiconductor 230 through conductors 240a and 240b.
[0382] Both insulators 241a and 241b are formed in such a way that they contact the inner walls of the openings of insulators 275, 280, 282, and 283. The inner side of insulator 241a contacts conductor 240a, and the inner side of insulator 241b contacts conductor 240b.
[0383] As insulator 241, a barrier insulating film suitable for insulators such as 275 can be used. For example, silicon nitride, aluminum oxide, silicon oxynitride, etc., can be used as insulator 241. By providing insulator 241, impurities such as water and hydrogen contained in insulators such as 280 can be suppressed from entering oxide semiconductor 230 through conductors 240a and 240b. In particular, silicon nitride has high hydrogen barrier properties and is therefore preferred. Furthermore, oxygen contained in insulator 280 can be prevented from being absorbed by conductors 240a and 240b.
[0384] When the insulator 241 has a laminated structure, an oxygen-barrier insulating film and a hydrogen-barrier insulating film are preferably used in combination as a first insulator that contacts the inner wall of the opening of the insulator 280, etc., and a second insulator inside it.
[0385] For example, aluminum oxide deposited using the thermal ALD method can be used as the first insulator, and silicon nitride deposited using the PEALD method can be used as the second insulator. By adopting this structure, oxidation of the conductor 240 can be suppressed, and hydrogen ingress into the conductor 240 can be suppressed.
[0386] Note that although the above description shows an example of an insulator 241 having a two-layer stacked structure, the present invention is not limited thereto. For example, the insulator 241 may also have a single-layer structure or a stacked structure of three or more layers. Similarly, although the above description shows an example of a conductor 240 having a two-layer stacked structure, the present invention is not limited thereto. For example, the conductor 240 may also have a single-layer or a stacked structure of three or more layers.
[0387] Notice, Figure 13A The diagram shows a structure where conductor 240a primarily contacts the top surface of conductor 242a2, but the invention is not limited thereto. Conductor 240a may also cover the sides of conductor 242a2, conductor 242a1, oxide semiconductor 230, and insulator 224. By employing this structure, the contact area between conductor 240a and conductor 242a can be increased. Note that the above description of conductor 240a and conductor 240b is similar.
[0388] As described above, increasing the contact area between conductor 240 and conductor 242 reduces the contact resistance between them. Therefore, the on-state current and frequency characteristics of transistor 200 can be improved without increasing the occupied area of transistor 200. This provides a semiconductor device with high operating speed. Furthermore, the operating speed of memory devices using this semiconductor device can be increased. This enables miniaturization or high integration of semiconductor devices. Additionally, the storage capacity of memory devices using this semiconductor device can be increased.
[0389] Note that in the above structure, such as Figure 1A As shown, the opening for the conductor 240 and insulator 241 is square in shape when viewed from above, but it is not limited to this. For example, when viewed from above, the opening can also be a roughly circular shape, an ellipse, or a polygonal shape, such as a square, or a shape with rounded corners. Furthermore, as... Figure 1C As shown, the opening is formed in a manner that overlaps with the oxide semiconductor 230 and the insulator 225, but is not limited thereto; it may be formed in a manner that overlaps with at least the conductor 242a or the conductor 242b. For example, as Figure 13B As shown, a portion of the opening (also referred to as a portion of the conductor 240) can overlap with the insulator 225 without the other portion of the opening (also referred to as another portion of the conductor 240) overlapping with the insulator 225. Thus, by employing a structure where a portion of the conductor 240 overlaps with the insulator 225, the configuration options for the conductor 240 can be increased. Furthermore, for example, as... Figure 13C As shown, the opening and conductor 240 can also be provided in an area that does not overlap with the insulator 225.
[0390] In addition, Figure 1D , Figure 13B and Figure 13C In this embodiment, conductors 240a and 240b are arranged symmetrically around conductor 260, but the present invention is not limited thereto. For example, such as Figure 14A As shown, it can also be configured such that, when viewed in cross-section along the channel length direction, a portion of the conductor 240a overlaps with the insulator 225 and the conductor 240b does not overlap with the oxide semiconductor 230. Furthermore, for example, as... Figure 14B As shown, when viewed in cross-section along the channel length, the conductor 240a can be disposed entirely or substantially entirely at a position overlapping with the insulator 225, and the conductor 240b can be disposed at a position not overlapping with the oxide semiconductor 230.
[0391] exist Figures 1A to 1D In this invention, an insulator 224 is provided only in the region overlapping with the oxide semiconductor 230, but the invention is not limited thereto. For example, as... Figures 15A to 15D As shown, the insulator 224 can be disposed not only in the region overlapping with the oxide semiconductor 230, but also outside the opening 201. Here, Figures 15A to 15D Corresponding to Figures 1A to 1D Therefore, for details about the structure, please refer to the above description.
[0392] In one aspect of the semiconductor device of the present invention, the shape of the insulator 224 in plan view is identical or substantially identical to the shape of the oxide semiconductor 230 in plan view, at least within the opening 201. In other words, the opening 201 preferably reaches the oxide semiconductor 230 and the insulator 222 is reached in proximity to the oxide semiconductor 230. At this time, as... Figures 15B to 15D As shown, an insulator 224 is provided between insulator 222 and insulator 275.
[0393] In addition, Figures 1A to 1D In the transistor 200, one insulator 225 is provided, but the present invention is not limited to this, and multiple insulators 225 may also be provided. For example, as Figures 16A to 16D As shown, insulators 225_1 and 225_2 can also be arranged in the A1-A2 direction and the oxide semiconductor 230 can be disposed such that it covers insulators 225_1 and 225_2. Here, Figures 16A to 16D Corresponding to Figures 1A to 1D Therefore, for details about the structure, please refer to the above description.
[0394] like Figure 16BAs shown, by providing insulators 225_1 and 225_2, compared to the case where only one insulator 225 is provided, the area of the oxide semiconductor 230 and the conductor 260 facing each other across the insulator 250 can be increased. This increases the channel width per unit area. Furthermore, as... Figure 16C As shown, by providing insulators 225_1 and 225_2, the contact area between the oxide semiconductor 230 and the conductor 242a2 (conductor 242b2) can be increased compared to the case where only one insulator 225 is provided. Therefore, the contact resistance between the oxide semiconductor 230 and the conductor 242a2 (conductor 242b2) can be reduced.
[0395] Note that in the above structure, the insulator 225 (insulator 225_1 and insulator 225_2) is rectangular in shape extending in the A5-A6 direction, but the present invention is not limited thereto. For example, the planar shape of the insulator 225 can also be a ring shape with both ends being the same or substantially the same (also referred to as a frame shape, annular shape, or closed curve shape). For example, it can also be adopted... Figure 16A The shape of the connection between the two ends of insulator 225_1 and insulator 225_2 shown.
[0396] Figures 17A to 17D Corresponding to Figures 1A to 1D . Figures 17A to 17D The semiconductor device shown includes insulators 271a and 271b. Insulator 255 is configured as a sidewall relative to the sidewall of opening 201, and insulator 224 is not provided. This is consistent with... Figures 1A to 1D The semiconductor device shown is different. Note that it is different from the one illustrated. Figure 1C Unlike other methods, mark points and lines A3-A4 at positions that do not overlap with conductor 240a, so as to... Figure 17C This makes the structure of insulator 271a easier to understand.
[0397] Insulator 271a contacts the top surface of conductor 242a2, and is identical or substantially identical to conductor 242a2 when viewed from above. Similarly, insulator 271b contacts the top surface of conductor 242b2, and is identical or substantially identical to conductor 242b2 when viewed from above. The top surfaces of insulators 271a and 271b contact insulator 275. Insulator 271a also has an opening, in which its side surface contacts insulator 241a. Similarly, insulator 271b also has an opening, in which its side surface contacts insulator 241b. Furthermore, when viewed from above, the side ends of insulator 271a and 271b with openings 201 on one side contact insulator 255.
[0398] exist Figures 17A to 17DIn the example shown, insulators 271a and 271b can use insulating materials suitable for insulators 275 and 250, preferably insulating materials suitable for insulator 275. For example, silicon nitride can be used as insulators 271a and 271b. Note that in Figures 17A to 17D In the example shown, insulators 271a and 271b may also have a stacked structure with two or more layers. For example, when insulators 271a and 271b have a stacked structure with two layers, silicon nitride can be used as the lower layer and silicon oxide can be used as the upper layer.
[0399] exist Figures 17A to 17D In the manufacturing process of the semiconductor device shown, it is preferable to deposit conductive films as conductors 242a2 and 242b2, and then deposit insulating films as insulators 271a and 271b. By employing this structure, conductors 242a2 and 242b2 can be protected by insulators 271a and 271b during the manufacturing process of the semiconductor device. Therefore, the yield of the semiconductor device can be improved.
[0400] In addition, Figures 17A to 17D In the example shown, the insulator 255 is formed as a sidewall in contact with the sidewall of the opening 201. Therefore, as Figure 17B and Figure 17C As shown, the side surface of insulator 255 contacts the side surfaces of insulator 280, insulator 275, insulator 271a, insulator 271b, conductor 242a2, and conductor 242b2. Furthermore, the bottom surface of insulator 255 contacts the top surface of insulator 222, conductor 242a1, and conductor 242b1. With this structure, the thickness of insulator 255 is the same as or approximately the same as the length of the protrusions of conductor 242a1 and conductor 242b1.
[0401] After forming the opening 201, an insulating film is deposited to form an insulator 255, and the insulating film is anisotropically etched, thereby forming an insulator 255 with the above-described structure in a self-aligned manner. As a result, the insulator 255 can be formed inside the opening 201 without the need to form a separate mask, thus improving the productivity of semiconductor devices.
[0402] Note that in Figures 17A to 17D In the example shown, insulator 224 is not provided, so insulator 225 and oxide semiconductor 230 are in contact with the top surface of insulator 222. However, it is not limited to this, and insulator 224 can also be provided between insulator 225 and oxide semiconductor 230 and insulator 222.
[0403] In addition, such as Figure 18A As shown, the transistor 200, capacitor 460, and transistor 310 formed in the silicon substrate can be used as a 2T (transistor) 1C (capacitor) type memory cell. Figure 18A As shown, a layer including transistor 200 and capacitor 460 can be disposed on a layer including transistor 310. Additionally, Figure 19A This shows a cross-sectional view of transistor 200 along the channel width direction. Figure 19B A cross-sectional view of capacitor 460 in this direction is shown. Figure 19C A cross-sectional view of transistor 310 in the channel width direction is shown.
[0404] Transistor 310 is disposed on substrate 311 and includes a conductor 316 serving as a gate, an insulator 315 serving as a gate insulator, a semiconductor region 313 comprising a portion of substrate 311, and low-resistance regions 314a and 314b serving as source or drain regions. Transistor 310 can be a p-channel transistor or an n-channel transistor. Substrate 311 can be, for example, a single-crystal silicon substrate.
[0405] like Figure 19C As shown, in transistor 310, the semiconductor region 313 (a portion of substrate 311) forming the channel has a convex shape. Furthermore, a conductor 316 is provided such that it covers the sides and top surface of the semiconductor region 313 with an insulator 315 in between. The conductor 316 can also be made of a material with an adjustable work function. Since the transistor 310 utilizes the convex portion of the semiconductor substrate, it is also referred to as a finned transistor. Furthermore, an insulator for forming the convex portion can be provided such that it contacts the top of the convex portion. Although the case where the convex portion is formed by processing a portion of the semiconductor substrate is shown here, a semiconductor film with a convex shape can also be formed by processing an SOI (Silicon on Insulator) substrate.
[0406] Notice, Figure 18A The structure of transistor 310 shown is only an example and is not limited to the above structure. Appropriate transistors can be used depending on the circuit structure or driving method.
[0407] Wiring layers, including interlayer films, wiring, and plugs, can also be provided between the various structures. Furthermore, multiple wiring layers can be configured according to the design. Additionally, in this specification, wiring and plugs electrically connected to the wiring can also be considered components. That is, a portion of a conductor is sometimes used as wiring, and a portion of a conductor is sometimes used as a plug.
[0408] For example, insulators 320, 322, 324, and 326 are sequentially stacked as interlayer films on transistor 310. Furthermore, conductors such as 328 are embedded in insulators 320 and 322. Furthermore, conductors such as 330 are embedded in insulators 324 and 326. Moreover, conductors 328 and 330 are used as contact plugs or wiring.
[0409] Furthermore, the insulator used as an interlayer film can be used as a planarization film covering the uneven shape underneath. For example, in order to improve the flatness of the top surface of insulator 322, its top surface can also be planarized by using a planarization process such as CMP.
[0410] A transistor 200 and a capacitor 460 are disposed on an insulator 326. Here, the transistor 200 is used. Figure 1D The transistor 200 is shown. The structure of the transistor 200 and the layer on which the transistor 200 is formed is the same as the structure described above, and therefore it is shown with the same shading and symbols. For detailed structure, please refer to the above description. In addition, an insulator 285 is formed on the insulator 283, and a conductor 413 electrically connected to the conductor 240a is formed on the insulator 285. The insulator 285 can be made of an insulating material that can be used for the insulator 216. In addition, the conductor 413 can be made of a conductive material that can be used for the conductor 242.
[0411] The capacitor 460 includes an insulator 425 on an insulator 224, an oxide semiconductor 230 covering the insulator 425, a conductor 242b1 on the oxide semiconductor 230, an insulator 455 on the conductor 242b1, an insulator 454 on the insulator 455, and a conductor 456 on the insulator 454. The insulator 455, insulator 454, and conductor 456 are disposed in openings 202 formed in insulators 280, insulator 275, etc. Figure 18A , Figure 19A and Figure 19B As shown, capacitor 460 and transistor 200 share oxide semiconductor 230 and conductor 242b1. Opening 202 can be formed using the same process as opening 201. Insulator 425 can have the same structure as insulator 225 and be formed using the same process. Insulator 455 can have the same structure as insulator 255 and be formed using the same process. Insulator 454 has the same structure as insulator 250 and can be formed using the same process. Conductor 456 has the same structure as conductor 260 and can be formed using the same process. Furthermore, as described above, conductor 260 can be extended and used as wiring. Conductor 456 can also be extended and used as wiring in the same way.
[0412] Here, capacitor 460 includes a conductor 242b1 serving as a first electrode, a conductor 456 serving as a second electrode, and an insulator 455 and an insulator 454 serving as dielectrics. That is, capacitor 460 constitutes a MIM (Metal-Insulator-Metal) capacitor.
[0413] Capacitor 460 has a structure similar to transistor 200 and can be fabricated in parallel on the same layers as transistor 200. However, it differs from transistor 200 in that conductor 242b1 and insulator 455 overlap with conductor 456 and insulator 454. For example, as Figure 19A As shown, in opening 201, an opening is formed in a portion of the insulator 255, which overlaps with a portion of the oxide semiconductor 230. Furthermore, in the region where the opening of the insulator 255 overlaps with the oxide semiconductor 230, a conductor 242b1 is not formed on the oxide semiconductor 230. On the other hand, as... Figure 19B As shown, in opening 202, no opening is formed in insulator 455, and oxide semiconductor 230 is covered by insulator 455. Additionally, in opening 202, conductor 242b1 is in contact with the top surface of oxide semiconductor 230, and insulator 455 is in contact with the top surface of conductor 242b1.
[0414] like Figure 19B As shown, the insulator 425 of capacitor 460, like insulator 225, has a high aspect ratio. Therefore, the relative areas of the conductors 242b1, 455, 454, and 456 arranged along the top and side surfaces of insulator 425 can be increased. In this way, the electrostatic capacitance can be increased without increasing the area occupied by capacitor 460.
[0415] Furthermore, it is preferable to provide the conductor 458 in the openings formed in insulators 215, 216, 221, 222, and 224. The conductor 458 may, for example, have the same structure as the conductor 240. The top surface of the conductor 458 contacts the bottom surface of the oxide semiconductor 230 and can be electrically connected to the conductor 330. Note that in Figure 18AIn this diagram, only one conductor 458 is shown, but it is not limited to this; two or more conductors may be used to electrically connect conductor 242b1 and conductor 330. Furthermore, conductor 242b1 and a portion of oxide semiconductor 230 may be embedded in openings formed in insulators 215, 216, 221, 222, and 224. Moreover, it is not necessary for the top surface of conductor 458 to contact the bottom surface of oxide semiconductor 230. For example, a structure may be adopted in which the top surface of conductor 458 is exposed from the top surface of insulator 285, and a conductor identical to conductor 240 is provided in contact with the top surface of conductor 242b2, and this conductor is electrically connected to conductor 458 via wiring.
[0416] By employing the above structure, one of the source and drain terminals of transistor 200, one electrode of capacitor 460, and the gate of transistor 310 are electrically connected, thereby forming a 2T1C type memory cell. Alternatively, by employing a structure without transistor 310, a 1T1C type memory cell can be formed. Furthermore, by employing a structure without capacitor 460, a 2T0C type memory cell can be formed.
[0417] Here, transistor 310 is preferably arranged to overlap with at least one of transistor 200 and capacitor 460. For example, transistor 310 may overlap with transistor 200. By adopting this structure, the occupied area of the memory cell can be reduced.
[0418] In addition, Figure 18A In the illustrated structure, transistor 200 includes insulator 225, and capacitor 460 includes insulator 425; however, the invention is not limited thereto. For example, as... Figure 18B As shown, insulator 250, conductor 260, insulator 455, insulator 454, and conductor 456 can also be formed on insulator 225 and oxide semiconductor 230 without insulator 425. In other words, transistor 200 and capacitor 460 can share insulator 225. Therefore, it is not necessary to form insulator 225 patterns separately for transistor 200 and capacitor 460, so the occupied area of transistor 200 and capacitor 460 can be reduced.
[0419] In addition, although Figure 18A The illustrated structure shows a transistor 310 formed on a silicon substrate, but the invention is not limited thereto. For example, as Figure 20AAs shown, two transistors (hereinafter referred to as transistor 200a and transistor 200b) with the same structure as transistor 200 described above can also be provided. Here, transistor 200a and transistor 200b are formed in the same layer and are arranged to intersect each other in their respective channel length directions. Note that since transistor 200a and transistor 200b have the same structure as transistor 200, the constituent elements are shown with the same shading lines and symbols. For detailed structure information, please refer to the above description.
[0420] In addition, Figure 20A In the structure shown, a capacitor 400 is disposed on an insulator 285. The capacitor 400 includes a conductor 410 on the insulator 285, an insulator 430 on the conductor 410, and a conductor 420 on the insulator 430. Conductors 240b, insulator 241b, conductor 240c, and insulator 241c are disposed in contact with the bottom surface of conductor 410. Here, conductor 240c and insulator 241c are formed by being embedded in the openings of insulators 282, 283, and 285, and have the same structure as conductors 240b and 241c. The bottom surface of conductor 240c is in contact with the top surface of conductor 260 of transistor 200b. By employing this structure, one of the source and drain electrodes of transistor 200a, one electrode of capacitor 400, and the gate of transistor 200b are electrically connected.
[0421] The capacitor 400 includes a conductor 410 serving as a first electrode, a conductor 420 serving as a second electrode, and an insulator 430 serving as a dielectric. In other words, the capacitor 400 constitutes a MIM capacitor.
[0422] Conductors 410 and 420 can be made of conductive materials suitable for conductor 260. For example, tungsten can be used for conductors 410 and 420. Here, by adopting a structure where conductor 420 covers conductor 410, the side of conductor 410 can be used as capacitor 400. This increases the electrostatic capacitance of capacitor 400. In addition, conductor 413 can be formed simultaneously with conductor 410.
[0423] Conductors 410, 413, and 420 have a single-layer structure, but are not limited to this structure; they may also have a stacked structure of two or more layers. For example, a stacked structure of a barrier conductor and a highly conductive conductor may be used. For example, a stacked structure of titanium nitride and tungsten on titanium nitride may be used.
[0424] The insulator 430 included in the capacitor 400 is preferably made of a material with a high relative permittivity (high-k). Examples of high-k materials include gallium oxide, hafnium oxide, zirconium oxide, oxides containing aluminum and hafnium, oxynitrides containing aluminum and hafnium, oxides containing silicon and hafnium, oxynitrides containing silicon and hafnium, or nitrides containing silicon and hafnium. By using such a high-k material, the thickness of the insulator 430 can be set to a level that suppresses leakage current, and the electrostatic capacitance of the capacitor 400 can be sufficiently ensured. Furthermore, since the insulator 430 is formed to cover the conductor 410, it is preferable to deposit it using a deposition method with high coverage, such as ALD or CVD.
[0425] Furthermore, the insulator 430 may also have a laminated structure. Preferably, a laminated structure is used, consisting of a material with a high relative permittivity (high-k) and a material with a dielectric strength greater than that high-k relative permittivity. Materials with high dielectric strength (materials with low relative permittivity) include silicon oxide, silicon oxynitride, silicon oxynitride, silicon nitride, fluorine-added silicon oxide, carbon-added silicon oxide, and silicon oxide with both carbon and nitrogen. The insulator 430 may also have a laminated structure consisting of alumina, a material with a high relative permittivity (high-k), and silicon oxide with high dielectric strength on the alumina.
[0426] Furthermore, for example, as insulator 430, an insulator consisting of zirconium oxide, aluminum oxide, and zirconium oxide stacked sequentially can be used. Alternatively, for example, an insulator consisting of zirconium oxide, aluminum oxide, zirconium oxide, and aluminum oxide stacked sequentially can be used. Furthermore, for example, an insulator consisting of hafnium zirconium oxide, aluminum oxide, hafnium zirconium oxide, and aluminum oxide stacked sequentially can be used. By using an insulator with high dielectric strength, such as aluminum oxide, the dielectric strength is increased, thereby suppressing electrostatic discharge damage to the capacitor 400.
[0427] Furthermore, the insulator 430 can also be made of a material that is ferroelectric. Examples of ferroelectric materials include hafnium oxide, zirconium oxide, and HfZrO. XMetal oxides such as (X is a real number greater than 0). Furthermore, materials that can exhibit ferroelectric properties include hafnium oxide with the addition of element J1 (here, element J1 is selected from one or more of zirconium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.). Here, the ratio of the number of hafnium atoms to the number of element J1 atoms can be appropriately set; for example, the ratio can be set to 1:1 or close to 1. Furthermore, materials that can exhibit ferroelectric properties include zirconium oxide with the addition of element J2 (here, element J2 is selected from one or more of hafnium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.). Furthermore, the ratio of the number of zirconium atoms to the number of element J2 atoms can be appropriately set; for example, the ratio can be set to 1:1 or close to 1. Additionally, lead titanate (PbTiO2) can also be used as a material that can exhibit ferroelectric properties. X Piezoelectric ceramics with perovskite structure include barium strontium titanate (BST), strontium titanate, lead zirconate titanate (PZT), strontium bismuth tantalate (SBT), bismuth ferrite (BFO), and barium titanate.
[0428] Furthermore, metal nitrides containing elements M1, M2, and nitrogen can be cited as materials that can exhibit ferroelectric properties. Here, element M1 is selected from one or more of aluminum, gallium, indium, etc. Furthermore, element M2 is selected from one or more of boron, scandium, yttrium, lanthanum, cerium, neodymium, europium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, etc. Furthermore, the ratio of the number of atoms of element M1 to the number of atoms of element M2 can be appropriately set. Furthermore, metal oxides containing elements M1 and nitrogen sometimes exhibit ferroelectric properties even without element M2. Furthermore, materials that can exhibit ferroelectric properties include those to which element M3 is added. Note that element M3 is selected from one or more of magnesium, calcium, strontium, zinc, cadmium, etc. Here, the ratio of the number of atoms of element M1, the number of atoms of element M2, and the number of atoms of element M3 can be appropriately set.
[0429] In addition, perovskite-type oxynitrides such as SrTaO2N and BaTaO2N, and κ-type alumina such as GaFeO3 can be cited as materials that can exhibit ferroelectric properties.
[0430] Note that while examples of metal oxides and metal nitrides are shown in the above description, the invention is not limited to these. For example, metal oxynitrides with nitrogen added to the aforementioned metal oxides or metal oxynitrides with oxygen added to the aforementioned metal nitrides may also be used.
[0431] Furthermore, as a material that can exhibit ferroelectricity, for example, a mixture or compound composed of multiple materials selected from the above-mentioned materials can be used. Alternatively, the insulator 430 can have a multilayer structure composed of multiple materials selected from the above-mentioned materials. Note that the crystal structure (properties) of the materials listed above may vary not only depending on the deposition conditions but also depending on various processes, etc. Therefore, in this specification, materials exhibiting ferroelectricity are referred not only to ferroelectric materials but also to materials that can exhibit ferroelectricity.
[0432] Note that in Figure 20A The storage device shown uses a planar shape for the capacitor 400, but the storage device shown in this embodiment is not limited to this. For example, the capacitor 400 may also be cylindrical or columnar.
[0433] An insulator 487 is provided to cover the capacitor 400, and an insulator 488 is provided to cover the insulator 487. As the insulator 487, an insulator with the function of trapping or fixing hydrogen is preferably used. For example, aluminum oxide can be used as the insulator 487. As the insulator 488, an insulator with the function of inhibiting hydrogen diffusion is preferably used. For example, silicon nitride, which has higher hydrogen barrier properties, can be used as the insulator 488.
[0434] In addition, Figure 20A In the structure shown, transistors 200a and 200b are disposed in the same layer, but the present invention is not limited thereto. For example, as Figure 20B As shown, a layer 401a including transistor 200a can also be stacked on a layer 401b including transistor 200b. Note that layers 401a and 401b have the same characteristics as... Figure 20A The layers of insulators 215 to 285 shown have the same structure.
[0435] like Figure 20B As shown, conductors 240c and 241c can also be formed in the openings of insulators 282 to 285 in layer 401b and insulators 215 to 285 in layer 401a. With this structure, conductor 410 of capacitor 400 can be electrically connected to conductor 260 of transistor 200b. Note that it is not necessary to electrically connect conductor 410 to conductor 260 of transistor 200b using only conductor 240c. Furthermore, two or more conductors can be used to electrically connect conductor 410 to conductor 260 of transistor 200b.
[0436] Here, transistor 200b is preferably arranged to overlap with at least one of transistor 200a and capacitor 400. For example, the oxide semiconductor 230 of transistor 200b is preferably arranged to overlap with at least one of the oxide semiconductor 230 of transistor 200a and conductor 410 of capacitor 400. By adopting this structure, the occupied area of the memory cell can be reduced.
[0437] Materials Constituting Semiconductor Devices The following description pertains to the materials used in the construction of semiconductor devices. Note that the layers constituting a semiconductor device can have a single-layer structure or a stacked structure.
[0438] <<Substrate>> Substrates for forming transistors can be, for example, insulating substrates, semiconductor substrates, or conductive substrates. Examples of insulating substrates include glass substrates, quartz substrates, sapphire substrates, stabilized zirconia substrates (yttrium-stabilized zirconia substrates, etc.), and resin substrates. Examples of semiconductor substrates include semiconductor substrates made of silicon or germanium, and compound semiconductor substrates made of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, or gallium oxide. Furthermore, semiconductor substrates having insulating regions within the aforementioned semiconductor substrates, such as SOI substrates, can also be used. Examples of conductive substrates include graphite substrates, metal substrates, alloy substrates, and conductive resin substrates. Additionally, examples of substrates include substrates containing metal nitrides, substrates containing metal oxides, insulating substrates with conductors or semiconductors, semiconductor substrates with conductors or insulators, and conductive substrates with semiconductors or insulators. Alternatively, substrates on which one or more elements are disposed can also be used. Examples of elements disposed on the substrate include capacitors, resistors, switching elements, light-emitting elements, and memory elements.
[0439] <<Insulators>> As an insulator that can be used in at least one of insulators 215, 216, 221, 222, 224, 225, 241, 250, 255, 271a, 271b, 275, 280, 282, 283, 285, 315, 320, 322, 324, 326, 425, 430, 454, 455, 487, and 488, examples of insulating oxides, nitrides, oxynitrides, nitrogen oxides, metal oxides, metal oxynitrides, and metal nitrogen oxides can be cited.
[0440] For example, when miniaturizing and highly integrating transistors, problems such as leakage current sometimes occur due to the thinning of the gate insulator. By using a high-k material as the insulator used as the gate insulator, low voltage can be achieved during transistor operation while maintaining the physical thickness. On the other hand, by using a material with a low relative permittivity as the insulator used as the interlayer film, parasitic capacitance generated between wirings can be reduced. Therefore, it is preferable to select materials based on the function of the insulator.
[0441] Examples of insulators with relatively high permittivity include gallium oxide, hafnium oxide, zirconium oxide, oxides containing aluminum and hafnium, oxynitrides containing aluminum and hafnium, oxides containing silicon and hafnium, oxynitrides containing silicon and hafnium, and nitrides containing silicon and hafnium.
[0442] Examples of insulators with relatively low permittivity include silicon oxide, silicon oxynitride, silicon oxynitride, silicon nitride, silicon oxide with added fluorine, silicon oxide with added carbon, silicon oxide with added carbon and nitrogen, porous silicon oxide, and resins.
[0443] Furthermore, by surrounding a transistor using a metal oxide with an insulator that suppresses the permeation of impurities such as hydrogen and oxygen, the electrical characteristics of the transistor can be stabilized. Examples of insulators that suppress the permeation of impurities such as hydrogen and oxygen include single layers or stacks of one or more of boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium, and tantalum. Specifically, examples of insulators that suppress the permeation of impurities such as hydrogen and oxygen include oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide, as well as nitrides such as aluminum nitride, silicon oxynitride, and silicon nitride.
[0444] Furthermore, the insulator used as the gate insulator is preferably an insulator having a region containing oxygen that has been removed by heating. For example, when a structure is used in which silicon oxide or silicon oxynitride having a region containing oxygen that has been removed by heating is contacted with the oxide semiconductor 230, the oxygen vacancies contained in the oxide semiconductor 230 can be filled.
[0445] <<Conductors>> As a conductor that can be used in at least one of conductors 205, 240, 242, 260, 316, 328, 330, 410, 413, 420, 456, and 458, it is preferable to use a metallic element selected from aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel, cobalt, titanium, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, iridium, strontium, and lanthanum, an alloy composed of the above-mentioned metallic elements, or an alloy combining the above-mentioned metallic elements. Examples of conductors include tantalum nitride, titanium nitride, nitrides containing titanium and aluminum, nitrides containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, oxides containing strontium and ruthenium, and oxides containing lanthanum and nickel. Furthermore, tantalum nitride, titanium nitride, nitrides containing titanium and aluminum, nitrides containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, oxides containing strontium and ruthenium, and oxides containing lanthanum and nickel are preferred materials as they are conductive materials that are not easily oxidized or maintain conductivity even after absorbing oxygen. Additionally, semiconductors with high conductivity, such as polycrystalline silicon containing impurity elements like phosphorus, or silicides such as nickel silicides can also be used.
[0446] When using a conductor with a multilayer structure, for example, a multilayer structure combining a material containing the aforementioned metal element and a conductive material containing oxygen, a multilayer structure combining a material containing the aforementioned metal element and a conductive material containing nitrogen, or a multilayer structure combining a material containing the aforementioned metal element, a conductive material containing oxygen, and a conductive material containing nitrogen may also be used.
[0447] Furthermore, when using oxides in the channel formation region of a transistor, a stacked structure combining a material containing the aforementioned metallic elements and an oxygen-containing conductive material is preferably used as the conductor serving as the gate electrode. In this case, it is preferable to provide the oxygen-containing conductive material on one side of the channel formation region. By providing the oxygen-containing conductive material on one side of the channel formation region, oxygen detached from this conductive material can be easily supplied to the channel formation region.
[0448] In particular, as the conductor used as the gate electrode, a conductive material containing a metal element and oxygen contained in the metal oxide forming the channel is preferably used. Alternatively, a conductive material containing the aforementioned metal element and nitrogen can also be used. For example, nitrogen-containing conductive materials such as titanium nitride and tantalum nitride can be used. Furthermore, one or more of the following can be used: indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide with added silicon. Additionally, indium gallium zinc oxide containing nitrogen can also be used. By using the above materials, hydrogen contained in the metal oxide forming the channel can sometimes be trapped. Alternatively, hydrogen mixed in from external insulators or the like can sometimes be trapped.
[0449] <Examples of Semiconductor Device Manufacturing Methods> Reference Figures 21A to 30D An example of a method for manufacturing a semiconductor device according to one aspect of the present invention will be described. Here, manufacturing... Figures 1A to 1D The case of the semiconductor device shown will be used as an example for explanation.
[0450] In each of the accompanying figures, (A) is a plan view. Furthermore, (B) of each of the accompanying figures is a cross-sectional view along the dashed lines A1-A2 in (A), which is also a cross-sectional view along the channel width direction of transistor 200. Furthermore, (C) of each of the accompanying figures is a cross-sectional view along the dashed lines A3-A4 in (A), which is also a cross-sectional view along the channel width direction of transistor 200. Furthermore, (D) of each of the accompanying figures is a cross-sectional view along the dashed lines A5-A6 in (A), which is also a cross-sectional view along the channel length direction of transistor 200. Note that, for clarity, some constituent elements are omitted in the plan view of each of the accompanying figures (A).
[0451] The insulating materials used to form insulators, the conductive materials used to form conductors, or the semiconductor materials used to form semiconductors can be deposited using methods such as sputtering, CVD, MBE, PLD, and ALD.
[0452] As sputtering methods, there are RF sputtering, which uses a high-frequency power supply for sputtering; DC sputtering, which uses a DC power supply; and pulsed DC sputtering, which changes the voltage applied to the electrodes in a pulsed manner. RF sputtering is preferred when using an insulating target for deposition. DC sputtering is mainly used when using a conductive target for deposition. Furthermore, conductive films can be formed using DC sputtering, and insulating films can be formed when performing reactive sputtering using pulsed DC sputtering. Specifically, pulsed DC sputtering can be used when depositing compounds such as oxides, nitrides, and carbides using reactive sputtering.
[0453] Note that CVD methods can be categorized into plasma CVD (PECVD), thermal CVD (TCVD), and photo CVD. Furthermore, they can be classified based on the source gas used, such as metal CVD (MCVD) and MOCVD.
[0454] By utilizing plasma CVD, high-quality films can be obtained at relatively low temperatures. Furthermore, because it does not use plasma, thermal CVD is a deposition method that reduces plasma damage to the workpiece. For example, wiring, electrodes, and components (transistors, capacitors, etc.) in semiconductor devices sometimes accumulate charge due to receiving charge from plasma. This accumulated charge can sometimes damage these components. On the other hand, thermal CVD, which does not use plasma, avoids this plasma damage, thus improving the yield of semiconductor devices. Moreover, since thermal CVD does not generate plasma damage during deposition, films with fewer defects can be obtained.
[0455] As ALD methods, there are thermal ALD methods that use only thermal energy to react the precursors and reactants, and PEALD methods that use reactants excited by plasma.
[0456] CVD and ALD methods differ from sputtering methods that deposit particles released from a target or similar material. Therefore, CVD and ALD are deposition methods that are less affected by the shape of the workpiece and offer high step coverage. In particular, ALD exhibits excellent step coverage and thickness uniformity, making it suitable for forming films covering surfaces with high aspect ratio openings. However, ALD has a relatively slow deposition rate, so it is sometimes preferred to combine it with other deposition methods, such as CVD, which has a faster deposition rate.
[0457] Furthermore, when using CVD, films of arbitrary composition can be deposited by adjusting the source gas flow rate ratio. For example, when using CVD, films with continuously varying compositions can be deposited by changing the source gas flow rate ratio during deposition. When deposition is performed while changing the source gas flow rate ratio, the deposition time can be shortened compared to using multiple deposition chambers because the time required for transfer or pressure adjustment is eliminated. Therefore, this can sometimes improve the productivity of semiconductor devices.
[0458] First, prepare a substrate (not shown), and deposit an insulator 215 (see reference) on the substrate. Figures 21A to 21D As described above, insulator 215 can be the same insulator as any one or more of the laminated films of insulators 282 and 283. For example, insulator 215 can be deposited by sputtering, CVD, MBE, PLD, or ALD. Using sputtering, which does not require the use of hydrogen-containing molecules as the deposition gas, reduces the hydrogen concentration in insulator 215, and is therefore preferred.
[0459] Next, insulator 216 is deposited on insulator 215. Insulator 216 is preferably deposited using a sputtering method. By utilizing sputtering, which does not require the use of hydrogen-containing molecules as the deposition gas, the hydrogen concentration in insulator 216 can be reduced. Note that the deposition method for insulator 216 is not limited to sputtering; for example, CVD, MBE, PLD, or ALD methods can also be appropriately used. In this embodiment, silicon oxide is deposited using a sputtering method as insulator 216.
[0460] Insulators 215 and 216 are preferably deposited continuously without exposure to the atmosphere. For example, a multi-chamber deposition apparatus can be used. This reduces the amount of hydrogen in the film during deposition of insulators 215 and 216, and also reduces hydrogen ingress into the film between deposition steps.
[0461] Next, insulator 221 is deposited on insulator 216 (see reference). Figures 21A to 21D ).
[0462] The insulator 221 can be any insulator that blocks oxygen, hydrogen, and water as described above. The insulator 221 can be deposited using methods such as sputtering, CVD, MBE, PLD, or ALD. In this embodiment, silicon nitride is deposited using the PEALD method as the insulator 221.
[0463] Next, insulator 222 is deposited on insulator 221 (see reference). Figures 21A to 21D ).
[0464] The insulator 222 is preferably deposited with an oxide containing one or both of aluminum and hafnium. For example, aluminum oxide, hafnium oxide, and oxides containing aluminum and hafnium (hafnium aluminate) are preferred as the insulator. Alternatively, hafnium zirconium oxide is preferred. The insulator containing one or both of aluminum and hafnium provides a barrier against oxygen, hydrogen, and water. When the insulator 222 provides a barrier against hydrogen and water, the diffusion of hydrogen and water contained in the surrounding structure of the transistor through the insulator 222 to the inside of the transistor can be suppressed, thereby suppressing the generation of oxygen vacancies in the oxide semiconductor 230.
[0465] The insulator 222 can be deposited using methods such as sputtering, CVD, MBE, PLD, or ALD. In this embodiment, hafnium oxide is deposited as the insulator 222 using thermal ALD.
[0466] In this embodiment, silicon nitride is deposited as insulator 221 using the PEALD method, and hafnium oxide is deposited as insulator 222 using the thermal ALD method. Thus, by using silicon nitride, which has the function of suppressing hydrogen diffusion, as insulator 221, hydrogen diffusion from the lower layer of transistor 200 can be suppressed. Furthermore, by using hafnium oxide, which has the function of trapping or fixing hydrogen, as insulator 222, hydrogen in oxide semiconductor 230 can be trapped or fixed by insulator 222. This reduces the hydrogen concentration in and around oxide semiconductor 230.
[0467] Next, an insulating film 224f is deposited on the insulator 222 (refer to...). Figures 21A to 21D The insulating film 224f is the insulating film that becomes the insulator 224 in subsequent processes. Therefore, the insulating material described above that can be used for the insulator 224 can be used. The insulating film 224f can be deposited, for example, by sputtering, CVD, MBE, PLD, or ALD. For example, silicon oxide can be deposited as the insulating film 224f by sputtering.
[0468] Next, an insulating film is deposited on the insulating film 224f, and the insulating film is etched to form the insulator 225 (see reference). Figures 21A to 21D As insulator 225, an insulating material that releases very little hydrogen, as described above, can be used for insulator 225. For example, an insulating film that becomes insulator 225 can be deposited using sputtering, CVD, MBE, PLD, or ALD methods. For example, silicon nitride can be deposited using sputtering as the insulating film that becomes insulator 225.
[0469] Insulator 225 can be fabricated into island shapes using photolithography. This fabrication can be performed using either dry etching or wet etching. Dry etching is suitable for microfabrication.
[0470] Note that in lithography, the photoresist is first exposed through a mask. Next, a developer is used to remove or leave the exposed areas, forming a photoresist mask. Then, etching is performed through this photoresist mask to process conductors, semiconductors, or insulators into the desired shape. For example, a KrF stimulated excimer laser, an ArF stimulated excimer laser, or EUV (Extreme Ultraviolet) light can be used to expose the photoresist mask. Alternatively, immersion lithography can be used, where exposure is performed with a liquid (e.g., water) filling the space between the substrate and the projection lens. Electron beams or ion beams can also be used instead of the aforementioned light. Furthermore, when using electron beams or ion beams, a photomask may sometimes be omitted.
[0471] Unwanted resist masks after processing can be removed by dry etching (sometimes referred to as oxygen plasma treatment) or wet etching, dry etching followed by wet etching, or wet etching followed by dry etching.
[0472] Furthermore, a hard mask made of an insulator or conductor can also be used under a photoresist mask. For example, in the above structure, an aluminum oxide film on a silicon nitride film is used as a hard mask. When using a hard mask, an insulating or conductive film can be formed as the hard mask material, and a photoresist mask can be formed on it. Then, the hard mask material is etched to form a hard mask of the desired shape. The etching of the silicon nitride film can be performed either after removing the photoresist mask or without removing it. In the latter case, the photoresist mask may sometimes disappear during etching. After the etching of the silicon nitride film, the hard mask can also be removed by etching. On the other hand, if the hard mask material does not affect subsequent processes or can be used in subsequent processes, it is not necessarily necessary to remove the hard mask.
[0473] In addition, SOC (Spin On Carbon) films and SOG (Spin On Glass) films can be deposited between the workpiece and the resist mask. Using SOC and SOG films as masks can improve the durability of the mask pattern. For example, lithography can be used to sequentially deposit SOC, SOG, and resist masks on the workpiece.
[0474] As the etching gas for dry etching, halogen-containing etching gases can be used; specifically, etching gases containing one or more of fluorine, chlorine, and bromine can be used. Examples of etching gases include one or more mixtures of C4F6, C5F6, C4F8, CF4, SF6, CHF3, CH2F2, Cl2, BCl3, SiCl4, and BBr3. Furthermore, oxygen, carbon dioxide, nitrogen, helium, argon, hydrogen, or hydrocarbon gases can be appropriately added to the above etching gases. Additionally, depending on the material being dry-etched, gases containing hydrocarbons or hydrogen but not halogens can also be used as etching gases. Hydrocarbons used as etching gases include methane (CH4), ethane (C2H6), propane (C3H8), and butane (C4H4H6). 10 One or more of the following: ethylene (C2H4), propylene (C3H6), acetylene (C2H2), and propyne (C3H4). Etching conditions can be appropriately set according to the object being etched.
[0475] Furthermore, as a dry etching apparatus, a capacitively coupled plasma (CCP) etching apparatus including parallel planar electrodes can be used. The capacitively coupled plasma etching apparatus including parallel planar electrodes can also employ a structure that applies a high-frequency voltage to one of the parallel planar electrodes. Alternatively, it can employ a structure that applies a high-frequency voltage of the same frequency to each of the parallel planar electrodes. Furthermore, it can employ a structure that applies multiple different high-frequency voltages to the parallel planar electrodes. This type of CCP etching apparatus is called a dual-frequency capacitively coupled plasma (DF-CCP) etching apparatus. The DF-CCP etching apparatus can employ a structure that applies high-frequency voltages of different frequencies to each of the parallel planar electrodes. Alternatively, it can employ a structure that applies multiple different high-frequency voltages to one of the parallel planar electrodes. Alternatively, a dry etching apparatus with a high-density plasma source can be used. For example, as a dry etching apparatus with a high-density plasma source, an inductively coupled plasma (ICP) etching apparatus can be used. The etching apparatus can be appropriately configured according to the object to be etched. Note that in the aforementioned dry etching apparatus, reactive ion etching can be performed by generating a self-biased potential by applying a high-frequency voltage to an electrode on one side of the substrate. In reactive ion etching, etching is performed by accelerating ions in the plasma to collide with the workpiece, thus enabling highly anisotropic etching processes.
[0476] Furthermore, by using a difficult-to-etch material such as alumina as the upper layer of the insulating film 224f, the insulating film 224f can be used as an etching stop layer in the etching process of the insulator 225.
[0477] Note that the above diagram shows a structure with one insulator 225 in the transistor 200, but the invention is not limited to this. Two or more insulators 225 can also be provided separately. For example, by providing insulators 225_1 and 225_2, a structure with... Figures 16A to 16D The transistor 200 shown has the following structure.
[0478] Next, an oxide semiconductor film 230f is deposited as an oxide semiconductor 230 in a manner that covers the insulator 225 (see reference). Figures 22A to 22D The oxide semiconductor film 230f is a metal oxide film that becomes oxide semiconductor 230 in subsequent processes, and the aforementioned metal oxide film can be used. The oxide semiconductor film 230f can be deposited using sputtering, CVD, MBE, PLD, or ALD methods.
[0479] The deposition of the oxide semiconductor film 230f can be referred to the above. Figures 5A to 5C The record states that the oxide semiconductor film 230f can be indium oxide (also known as indium oxide) with a single crystal structure or highly crystalline indium oxide. By employing this structure, a semiconductor device with high field-effect mobility can be provided. Furthermore, a semiconductor device with good electrical characteristics, frequency characteristics, and reliability can be provided.
[0480] Alternatively, at least one of the above-described first heat treatment, second heat treatment, microwave plasma treatment, and hydrogenation treatment can be performed after depositing the oxide semiconductor film 230f. This can sometimes further improve the crystallinity of the oxide semiconductor film 230f.
[0481] Next, a conductive film 242_1f is deposited on the oxide semiconductor film 230f, and a conductive film 242_2f is deposited on the conductive film 242_1f (refer to...). Figures 22A to 22D Conductive film 242_1f is a conductive film that serves as conductor 242a1 and conductor 242b1, and conductive film 242_2f is a conductive film that serves as conductor 242a2 and conductor 242b2. Conductive film 242_1f can use conductive materials that can be used for conductor 242a1 and conductor 242b1, and conductive film 242_2f can use conductive materials that can be used for conductor 242a2 and conductor 242b2. Hereinafter, conductive film 242_1f and conductive film 242_2f are sometimes collectively referred to as conductive film 242f.
[0482] Conductive films 242_1f and 242_2f can be deposited using methods such as sputtering, CVD, MBE, PLD, or ALD. For example, tantalum nitride can be deposited by sputtering as conductive film 242_1f. Tungsten can be deposited by sputtering as conductive film 242_2f. By depositing conductive film 242f in a manner that covers oxide semiconductor film 230f, the contact area between oxide semiconductor film 230f and conductors 242a and 242b can be increased without increasing the occupied area. This improves the on-state current and frequency characteristics of transistor 200.
[0483] Furthermore, insulating films that serve as insulators 271a and 271b can also be deposited on the conductive film 242_2f. For example, silicon nitride can be deposited by sputtering and silicon oxide can be deposited thereon by sputtering as the insulating film. By providing such an insulating film, a system can be formed. Figures 17A to 17D The transistor 200 shown.
[0484] Next, using photolithography, the insulating film 224f, the oxide semiconductor film 230f, the conductive film 242_1f, and the conductive film 242_2f are processed into islands to form insulator 224, oxide semiconductor 230, conductor 242_1, and conductor 242_2 (see reference). Figures 23A to 23D At this point, in the region that does not overlap with conductors 242_1 and 242_2, insulator 222 is exposed.
[0485] The above processing can be performed using either dry etching or wet etching. Dry etching is suitable for microfabrication. For details regarding the conditions and apparatus for dry etching, please refer to previous descriptions. Furthermore, the insulating film 224f, oxide semiconductor film 230f, conductive film 242_1f, and conductive film 242_2f can be processed under different conditions. Additionally, a hard mask can be applied to the conductive film 242_2f during the above processing.
[0486] Furthermore, in the process of processing the insulating film 224f, the oxide semiconductor film 230f, the conductive film 242_1f, and the conductive film 242_2f into island shapes, it is possible to remove Figure 5C Layer 235 is shown.
[0487] Here, it is preferable to process the insulator 224, oxide semiconductor 230, conductor 242_1, and conductor 242_2 into an island shape in one step. In this case, the side ends of conductor 242_1 and conductor 242_2 preferably coincide with or substantially coincide with the side ends of oxide semiconductor 230. Furthermore, the side ends of insulator 224 preferably coincide with or substantially coincide with the side ends of oxide semiconductor 230. By adopting the above structure, the number of steps in the semiconductor device according to one aspect of the present invention can be reduced. Thus, a method for manufacturing a semiconductor device with high productivity can be provided.
[0488] By processing the insulator 224 into an island shape as described above, the bottom surface of the conductor 260 can be positioned below the bottom surface of the oxide semiconductor 230 in the transistor 200. This allows a sufficient electric field to be applied to the oxide semiconductor 230 as a whole from the conductor 260. Therefore, the electrical characteristics of the transistor 200 can be improved.
[0489] The sides of insulator 224, oxide semiconductor 230, conductor 242_1, and conductor 242_2 can also be perpendicular to or substantially perpendicular to the top surface of insulator 222. By adopting this structure, a smaller area and higher density can be achieved when multiple transistors are arranged.
[0490] However, this is not a limitation; the sides of insulator 224, oxide semiconductor 230, conductor 242_1, and conductor 242_2 can also be tapered. The tapered angle of the sides of insulator 224, oxide semiconductor 230, conductor 242_1, and conductor 242_2 can, for example, be 60° or more and less than 90°. Thus, when the sides have a tapered shape, the coverage of insulator 275, etc., is improved in subsequent processes, and defects such as voids can be reduced.
[0491] In addition, such as Figure 9A As shown, a structure without insulator 224 can also be used. In this case, when the oxide semiconductor 230 is processed into an island shape, sometimes a portion of the top surface of insulator 222 is removed. Thus, as... Figure 9A As shown, sometimes the top surface of the region of insulator 222 that overlaps with oxide semiconductor 230 is higher than the top surface of the region of insulator 222 that does not overlap with oxide semiconductor 230.
[0492] Next, an insulator 275 is deposited in a manner that covers insulator 224, oxide semiconductor 230, conductor 242_1, and conductor 242_2, and an insulator 280 is deposited on insulator 275 (see reference). Figures 24A to 24D The above-mentioned insulators can be used as insulators 275 and 280.
[0493] Here, insulator 275 is preferably in contact with the top surface of insulator 222.
[0494] As the insulator 280, it is preferable to form an insulating film that serves as the insulator 280 and to perform CMP treatment on the insulating film to form an insulator with a flat top surface. Alternatively, silicon nitride may be deposited on the insulator 280, for example, by sputtering, and the silicon nitride may be CMP treated until it reaches the insulator 280.
[0495] Insulators 275 and 280 can each be deposited, for example, by sputtering, CVD, MBE, PLD or ALD.
[0496] The insulator 275 is preferably an insulator that inhibits oxygen permeation. For example, silicon nitride is preferably deposited using the PEALD method as the insulator 275. Furthermore, aluminum oxide is preferably deposited using sputtering, and silicon nitride is deposited thereon using the PEALD method. When the insulator 275 has the above-described structure, the function of inhibiting the diffusion of impurities such as water and hydrogen, as well as oxygen, can be improved.
[0497] Thus, the oxide semiconductor 230, conductor 242_1, and conductor 242_2 can be covered by an insulator 275 that has the function of suppressing oxygen diffusion. As a result, oxygen can be prevented from diffusing directly from the insulator 280, etc., into the oxide semiconductor 230, conductor 242_1, and conductor 242_2 in subsequent processes.
[0498] Furthermore, silicon oxide is preferably deposited using sputtering as the insulator 280. By depositing an insulating film as the insulator 280 using sputtering under an oxygen-containing atmosphere, an insulator 280 containing excess oxygen can be formed. By using a sputtering method that does not require the use of hydrogen-containing molecules as the deposition gas, the hydrogen concentration in the insulator 280 can be reduced. Additionally, a heat treatment can be performed before depositing the insulating film. This heat treatment can also be performed under reduced pressure, and the insulating film can be deposited continuously without exposure to the atmosphere. By performing this treatment, moisture and hydrogen adsorbed on the surface of the insulator 275 can be removed, and the moisture and hydrogen concentrations in the oxide semiconductor 230 can be reduced. The heat treatment can be performed under the conditions described above.
[0499] Next, photolithography is used to process conductor 242_2, insulator 275, and insulator 280 to form openings 201 reaching conductor 242_1 and insulator 222 (see reference). Figures 25A to 25D Here, conductor 242_2 is divided to form conductor 242a2 and conductor 242b2. Opening 201 is formed such that at least a portion of it overlaps with oxide semiconductor 230. When viewed in cross-section along the channel length of transistor 200, the width of opening 201 is D2, which corresponds to the distance D2 between conductor 242a2 and conductor 242b2. That is, the width D2 of opening 201 is greater than the distance D1 between conductor 242a1 and conductor 242b1.
[0500] The above-described method can be appropriately utilized in lithography. In order to finely process the opening of the insulator 280, lithography using short wavelength light such as EUV light or electron beams is preferred.
[0501] The above processing is preferably performed using a dry etching method. Dry etching is capable of anisotropic etching, making it suitable for forming openings 201 with high aspect ratios. For details regarding the conditions and apparatus for dry etching, please refer to the previous description.
[0502] Additionally, the above shows that, according to Figures 23A to 23D The process of forming insulator 224 is carried out in the process of forming the insulator, but it can also be done according to the process of forming the insulator 224. Figures 25A to 25DIn the process of etching, insulating film 224f is processed to form insulator 224. At this time, insulating film 224f can be etched after insulator 275 is etched. This removes the area of insulator 224 that does not overlap with oxide semiconductor 230 within opening 201, forming an opening reaching insulator 222. By employing this structure, a structure with… Figures 15A to 15D The transistor 200 shown has the following structure.
[0503] Next, an insulating film 255A is deposited in a manner that covers insulator 280, conductor 242_1, and insulator 222 (see reference). Figures 26A to 26D The insulating film 255A is the insulating film that becomes insulator 255 in subsequent processes, and the aforementioned insulator can be used. The insulating film 255A can be deposited, for example, by sputtering, CVD, MBE, PLD, or ALD.
[0504] The insulating film 255A is deposited along the opening 201, so it preferably has good coverage. Therefore, the insulating film 255A is preferably deposited using a high-coverage ALD method or the like. For example, silicon nitride is preferably deposited using the PEALD method as the insulating film 255A.
[0505] Next, photolithography is used to process the conductor 242_1 and the insulating film 255A within the opening 201 to form an opening reaching the oxide semiconductor 230 (see reference). Figures 27A to 27D Here, an insulator 255 with an opening is formed from the insulating film 255A, and the conductor 242_1 is disconnected, thereby forming conductors 242a1 and 242b1. When viewed in cross-section along the channel length of the transistor 200, the width of this opening is D1, which corresponds to the distance D1 between the conductors 242a1 and 242b1. This opening is formed inside the opening formed in the insulator 280, therefore the distance D1 between the conductors 242a1 and 242b1 is less than the distance D2 between the conductors 242a2 and 242b2.
[0506] The above-described method can be appropriately utilized in lithography. In order to perform micro-machining on the opening of the insulator 255, lithography using short-wavelength light such as EUV light or electron beams is preferred.
[0507] Note that, as Figure 27A and Figure 27DAs shown, in the above-mentioned opening, the insulator 255 is formed in such a way that the island-shaped oxide semiconductor 230 is exposed; however, the present invention is not limited to this. In this process, the conductors 242a1 and 242b1 are separated by a distance D1 between them. Therefore, for example, an opening may be formed in the insulator 255, which is substantially the same as the opening 201 except for the portion that contacts the top surfaces of the conductors 242a1 and 242b1. Note that in this case, the insulator 255 is sometimes formed as a sidewall in such a way that it contacts the sidewall of the opening 201.
[0508] The above processing is preferably performed using a dry etching method. Dry etching is capable of anisotropic etching, making it suitable for fine processing such as the openings in the insulator 255 within the opening 201. For information on the conditions and apparatus for dry etching, please refer to the previous description.
[0509] Furthermore, the above examples illustrate the use of lithography in the fabrication of insulator 255, but the present invention is not limited thereto. For example, anisotropic etching of insulator 255 can also be performed without using a mask. Thus, as Figures 17A to 17D As shown, the insulator 255 can be formed into a sidewall shape in a manner that contacts the sidewall of the opening 201.
[0510] Furthermore, during the processing of the conductor 242_1, sometimes a portion of the oxide semiconductor 230 is removed. For example, as Figure 10A As shown, sometimes the portion of the oxide semiconductor 230 that contacts the upper part of the insulator 225 is removed, while the portion of the oxide semiconductor 230 that contacts the side of the insulator 225 remains, thus forming a sidewall-shaped oxide semiconductor 230.
[0511] Through the above steps, conductors 242a2 and 242b2 with a distance of D2 between them, and conductors 242a1 and 242b1 with a distance of D1 between them, can be formed. By adopting this structure, the distance between the source and drain of transistor 200 can be shortened, thus improving the frequency characteristics of transistor 200 and increasing the operating speed of semiconductor device.
[0512] Furthermore, when conductor 242a1 and conductor 242b1 are formed as described above, they can be manufactured simultaneously. Figure 18A and Figure 18BThe transistor 200 and capacitor 460 are shown. In this case, the following structure can be adopted: when forming the conductors 242a1 and 242b1 of the transistor 200, the etching process is not performed in the capacitor 460, and the oxide semiconductor 230 is covered by the conductors 242b1 in the region where the capacitor 460 is formed. Thus, the capacitor 460, including the conductors 242b1, the insulator 454, and the conductors 456, can be manufactured in parallel with the transistor 200.
[0513] Furthermore, an ashing treatment using oxygen plasma can be performed after the processing of conductor 242_1 and conductor 242_2. By performing such oxygen plasma treatment, impurities generated during the etching process and diffused into the oxide semiconductor 230 can be removed. Examples of such impurities include impurities originating from components in the workpiece subjected to the etching process and impurities originating from components in the gas used in the etching process. Examples include chlorine, fluorine, tantalum, silicon, and hafnium. When chlorine gas is used in the etching process, the oxide semiconductor 230 is exposed to an atmosphere containing chlorine gas; therefore, it is preferable to remove chlorine adhering to the oxide semiconductor 230. By removing impurities adhering to the oxide semiconductor 230 in this way, the electrical characteristics and reliability of the transistor can be improved.
[0514] In addition, a washing process can be performed to remove impurities and other contaminants that adhere to the surface of the oxide semiconductor 230 during the etching process described above. Washing methods include wet washing (also known as wet etching) using a washing solution, plasma treatment using plasma, and washing using heat treatment; combinations of these methods are also possible. Note that this washing process can sometimes deepen the etching tank.
[0515] As a wet cleaning process, an aqueous solution prepared by diluting one or more of oxalic acid, phosphoric acid, and hydrofluoric acid with carbonated water or pure water can also be used. Alternatively, a wet cleaning solution prepared by diluting ammonia with carbonated water or pure water can also be used. Furthermore, wet cleaning can also be performed using pure water or carbonated water. Alternatively, ultrasonic cleaning can be performed using the aforementioned aqueous solutions, pure water, or carbonated water. Alternatively, a combination of the above-mentioned cleaning methods can be appropriately combined.
[0516] Note that in this specification, the aqueous solution of hydrofluoric acid diluted with pure water is sometimes referred to as dilute hydrofluoric acid, and the aqueous solution of ammonia diluted with pure water is sometimes referred to as dilute ammonia. Furthermore, the concentration, temperature, etc., of the aforementioned aqueous solutions are appropriately adjusted according to the impurities to be removed and the structure of the semiconductor device being cleaned. The ammonia concentration of the dilute ammonia is preferably 0.01% or more and 5% or less, more preferably 0.1% or more and 0.5% or less. Furthermore, the hydrogen fluoride concentration of the dilute hydrofluoric acid is preferably 0.01 ppm or more and 100 ppm or less, more preferably 0.1 ppm or more and 10 ppm or less.
[0517] Furthermore, for ultrasonic cleaning, a frequency of 200 kHz or higher is preferred, and a frequency of 900 kHz or higher is even more preferred. By using this frequency, damage to oxide semiconductors 230 and the like can be reduced.
[0518] Furthermore, the above washing process can be performed multiple times, or the washing solution can be changed for each washing process. For example, the first washing process can be performed using dilute hydrofluoric acid or dilute ammonia, and the second washing process can be performed using pure water or carbonated water.
[0519] In this embodiment, a wet wash is performed using dilute ammonia water as the washing process described above. This washing process removes impurities adhering to the surface of the oxide semiconductor 230 or diffused into its interior. Furthermore, it improves the crystallinity of the oxide semiconductor 230.
[0520] The heat treatment is preferably performed after the etching or washing described above. The heat treatment temperature is 100°C or higher and 650°C or lower, preferably 250°C or higher and 600°C or lower, more preferably 300°C or higher and 550°C or lower, and even more preferably 350°C or higher and 400°C or lower. The heat treatment is performed in an atmosphere of nitrogen or an inert gas, or in an atmosphere containing 10 ppm or higher, 1% or higher, or 10% or higher of an oxidizing gas. For example, it is preferable to perform the heat treatment in an oxygen-containing atmosphere, preferably at a nitrogen to oxygen gas flow ratio of 4:1 and at a temperature of 350°C for 1 hour. This supplies oxygen to the oxide semiconductor 230, thereby reducing oxygen vacancies. Furthermore, the crystallinity of the oxide semiconductor 230 can be improved by performing the above heat treatment. Moreover, when residual hydrogen in the oxide semiconductor 230 reacts with the supplied oxygen, the hydrogen can be removed in the form of H2O (dehydration). This suppresses the recombination of residual hydrogen and oxygen vacancies in the oxide semiconductor 230 to form V. O H. This improves the electrical characteristics of the transistor with the oxide semiconductor 230, thereby increasing its reliability. Furthermore, it suppresses the inhomogeneity of electrical characteristics among multiple transistors formed on the same substrate. Additionally, the above-described heat treatment can be performed under reduced pressure. Alternatively, it can be performed in an oxygen atmosphere, followed by continuous heat treatment in a nitrogen atmosphere without exposure to the atmosphere. Furthermore, the above-described heat treatment can also be used to heat the oxide semiconductor film 230f. Therefore, sometimes the crystalline region of the oxide semiconductor 230 is grown through the above-described heat treatment.
[0521] Note that when heat treatment is performed with conductors 242a and 242b in contact with the oxide semiconductor 230, the sheet resistance of the regions of the oxide semiconductor 230 overlapping with conductors 242a and 242b sometimes decreases. Furthermore, the carrier concentration sometimes increases. Therefore, it is possible to self-align and reduce the resistance of the regions of the oxide semiconductor 230 overlapping with conductors 242a and 242b.
[0522] Here, as described above, the insulator 255, which includes an inorganic insulator that is not easily oxidized, is provided in contact with the side surfaces of the conductors 242a2 and 242b2. Therefore, even if the conductors 242a2 and 242b2 are made of materials such as tungsten films that are more easily oxidized, excessive oxidation of the conductors 242a2 and 242b2 due to the aforementioned heat treatment can be prevented.
[0523] Note that due to the processing of the aforementioned conductor 242_1 or subsequent washing processes, sometimes a portion of the top surface of the oxide semiconductor 230 in the region between conductors 242a1 and 242b1 is removed. Thus, as... Figure 11B As shown, in the oxide semiconductor 230, the top surface of the region between conductors 242a1 and 242b1 is sometimes lower than the top surface of the region that overlaps with conductors 242a1 or 242b1.
[0524] Next, an insulating film 250A (see reference) is deposited along the side and bottom surfaces of the opening 201 formed in the insulator 280, etc., to form the insulator 250. Figures 28A to 28D Here, the insulating film 250A is in contact with the insulator 255, the conductor 242a, the conductor 242b, the insulator 222, and the oxide semiconductor 230.
[0525] The insulating film 250A can be deposited using sputtering, CVD, MBE, PLD, or ALD methods. For example, the insulating film 250A is preferably deposited using the ALD method. Similar to the insulator 250 described above, the insulating film 250A is preferably formed thin, and thickness non-uniformity needs to be minimized. For this purpose, the ALD method involves alternately introducing precursors and reactants (e.g., oxidants) for deposition. Since the film thickness can be adjusted according to the number of cycles, the thickness can be precisely controlled. Furthermore, the insulating film 250A needs to be deposited with high coverage on the bottom and sides of the opening. By using the ALD method, atomic layers can be deposited on the bottom and sides of the opening, thus forming the insulating film 250A with high coverage within the opening.
[0526] In addition, when depositing the insulating film 250A using the ALD method, ozone (O3), oxygen (O2), water (H2O), etc., can be used as oxidants. By using ozone (O3), oxygen (O2), etc., which do not contain hydrogen, as oxidants, the amount of hydrogen diffusing into the oxide semiconductor 230 can be reduced.
[0527] The insulator 250 can adopt a laminated structure as shown in Figure 2, etc. For example, as... Figure 2A As shown, the insulator 250 can adopt a multilayer structure of insulators 250a to 250d. In this case, alumina can be deposited using thermal ALD as insulator 250a, silicon oxide can be deposited using PEALD as insulator 250b, hafnium oxide can be deposited using thermal ALD as insulator 250c, and silicon nitride can be deposited using PEALD as insulator 250d. Furthermore, the insulator 250 is not limited to a four-layer multilayer structure. For example, as... Figure 11A As shown, a three-layer stacked structure consisting of insulator 250a, insulator 250b on insulator 250a, and insulator 250d on insulator 250b can also be used.
[0528] Furthermore, it is preferable to perform microwave plasma treatment in an oxygen-containing atmosphere after depositing the insulating film 250A or after depositing any insulator constituting the insulating film 250A. Here, microwave plasma treatment sometimes refers to treatment using a device including a power supply that generates high-density plasma using microwaves. In addition, in this specification and the like, microwaves refer to electromagnetic waves with a frequency of 300 MHz or higher and 300 GHz or lower.
[0529] Microwave plasma processing preferably uses a microwave plasma processing apparatus, for example, that includes a power supply for generating high-density plasma using microwaves. Here, the frequency of the microwave plasma processing apparatus is preferably set to 300 MHz or more and 300 GHz or less, more preferably 2.4 GHz or more and 2.5 GHz or less, for example, 2.45 GHz. By using high-density plasma, high-density oxygen radicals can be generated. Furthermore, the power of the power supply for applying microwaves to the microwave plasma processing apparatus is preferably 1000 W or more and 10000 W or less, more preferably 2000 W or more and 5000 W or less. Additionally, the microwave plasma processing apparatus may also include a power supply that applies RF to one side of the substrate. Furthermore, by applying RF to one side of the substrate, oxygen ions generated by the high-density plasma can be efficiently introduced into the oxide semiconductor 230.
[0530] Furthermore, the aforementioned microwave plasma treatment is preferably performed under reduced pressure, preferably between 10 Pa and 1000 Pa, more preferably between 300 Pa and 700 Pa. The treatment temperature is preferably below 750°C, more preferably below 500°C, for example, around 250°C. Alternatively, heating treatment can be performed continuously after oxygen plasma treatment without exposure to external air. The heating temperature is preferably between 100°C and 750°C, more preferably between 300°C and 500°C.
[0531] Furthermore, for example, the microwave plasma treatment described above can be performed using oxygen gas and argon gas. Here, the oxygen flow ratio (O2 / (O2+Ar)) is greater than 0% and less than 100%. Preferably, the oxygen flow ratio (O2 / (O2+Ar)) is greater than 0% and less than 50%. More preferably, the oxygen flow ratio (O2 / (O2+Ar)) is more than 10% and less than 40%. Even more preferably, the oxygen flow ratio (O2 / (O2+Ar)) is more than 10% and less than 30%. In this way, by performing microwave plasma treatment in an oxygen-containing atmosphere, the carrier concentration in the oxide semiconductor 230 can be reduced. In addition, by preventing the introduction of excessive oxygen into the chamber during microwave plasma treatment, an excessive decrease in the carrier concentration in the oxide semiconductor 230 can be prevented.
[0532] By performing microwave plasma treatment in an oxygen-containing atmosphere, oxygen gas can be plasmaized using microwaves or high frequencies such as RF, and this oxygen plasma can then act on the region between conductors 242a and 242b of the oxide semiconductor 230. Through the action of plasma, microwaves, etc., the V in this region can be increased. O H separates into oxygen vacancies and hydrogen, and hydrogen is removed from this region. Here, in the use of Figure 2A When using the structure shown, an insulating film (e.g., alumina) with the function of trapping or fixing hydrogen is preferably used as the insulator 250a. By employing this structure, hydrogen generated by microwave plasma treatment can be trapped or fixed to the insulating film 250A. This reduces the Vo contained in the channel forming region. O H. This can reduce oxygen vacancies and V in the channel formation region. O H reduces carrier concentration. Furthermore, by supplying oxygen free radicals generated by the aforementioned oxygen plasma to the oxygen vacancies formed in the channel formation region, the oxygen vacancies in the channel formation region can be further reduced, thereby reducing carrier concentration.
[0533] The oxygen injected into the channel formation region can be in various forms, including oxygen atoms, oxygen molecules, oxygen ions, and oxygen free radicals (also known as O free radicals, which are atoms, molecules, or ions containing unpaired electrons). Furthermore, the oxygen injected into the channel formation region can be one or more of the above-mentioned forms, with oxygen free radicals being particularly preferred. In addition, the reliability of the transistor is improved because the film quality of the insulator 250 can be enhanced.
[0534] Furthermore, impurities such as carbon in the oxide semiconductor 230 can also be removed by microwave plasma treatment. Removing carbon, which is an impurity in the oxide semiconductor 230, can improve the crystallinity of the oxide semiconductor 230. In particular, when the oxide semiconductor 230 is deposited using the ALD method, carbon contained in the precursor is sometimes introduced into the oxide semiconductor 230; therefore, removing carbon by microwave plasma treatment is preferable.
[0535] On the other hand, the oxide semiconductor 230 has a region that overlaps with either conductor 242a or conductor 242b. This region can be used as a source region or a drain region. Here, conductor 242a and conductor 242b are preferably used as shielding films to protect against the effects of microwaves, RF, or oxygen plasma during microwave plasma processing in an oxygen-containing atmosphere. Thus, conductor 242a and conductor 242b preferably have the function of shielding electromagnetic waves of 300 MHz or higher and 300 GHz or lower, for example, 2.4 GHz or higher and 2.5 GHz or lower.
[0536] Conductors 242a and 242b shield against the effects of high-frequency microwaves or RF, oxygen plasma, etc., and therefore do not act on the region of oxide semiconductor 230 that overlaps with either conductor 242a or conductor 242b. Thus, Vo does not occur in the source and drain regions by microwave plasma treatment. O The decrease in H and the excessive supply of oxygen can prevent the decrease in carrier concentration.
[0537] Here, an oxygen-barrier insulator 255 is provided in contact with the sides of conductors 242a2 and 242b2. This prevents the formation of an oxide film on the sides of conductors 242a2 and 242b2 due to microwave plasma treatment.
[0538] As described above, oxygen vacancies and V can be selectively removed in the channel formation region of an oxide semiconductor. OH makes the channel formation region type I or substantially type I. Furthermore, it can suppress the supply of excessive oxygen to the regions used as source or drain regions, maintaining the conductivity (low resistance region state) prior to microwave plasma treatment. Thus, it can suppress variations in the electrical characteristics of the transistor and suppress non-uniformity of the transistor's electrical characteristics within the substrate surface.
[0539] Furthermore, by altering the film quality of the insulator 250 through microwave plasma treatment, the diffusion of hydrogen, water, impurities, etc., can be suppressed. This prevents the diffusion of hydrogen, water, impurities, etc., through the insulator 250 into the oxide semiconductor 230 and the like due to subsequent processes such as deposition of the conductive film that becomes the conductor 260, or post-processing such as heat treatment. Thus, by improving the film quality of the insulator 250, the reliability of the transistor can be improved.
[0540] When the insulator 250 has a stacked structure of insulators 250a to 250d, it is preferable to perform microwave plasma treatment after depositing insulator 250b. Alternatively, microwave plasma treatment can be performed again after depositing insulator 250c. Thus, multiple (at least two) microwave plasma treatments in an oxygen-containing atmosphere can be performed. Furthermore, the aforementioned microwave plasma treatment can sometimes also serve as a heating treatment for the aforementioned oxide semiconductor film 230f. Therefore, sometimes the aforementioned microwave plasma treatment can be used to grow crystalline regions of the oxide semiconductor 230.
[0541] Alternatively, heat treatment can be performed while maintaining a reduced pressure after microwave plasma treatment. This treatment efficiently removes hydrogen from the oxide semiconductor 230 in the insulating film. Alternatively, the following steps can be repeated, wherein heat treatment is performed while maintaining a reduced pressure after microwave plasma treatment. Repeated heat treatment further efficiently removes hydrogen from the oxide semiconductor 230 in the insulating film. Note that the heat treatment temperature is preferably 300°C or higher and 500°C or lower. Furthermore, the above-described heat treatment can also be used as a heat treatment for the oxide semiconductor film 230f. Therefore, sometimes the crystalline region of the oxide semiconductor 230 is grown through the above-described heat treatment.
[0542] Next, a conductive film 260A, which becomes conductor 260a, and a conductive film 260B, which becomes conductor 260b, are sequentially deposited (see reference). Figures 29A to 29DConductive films 260A and 260B are deposited by embedding them into openings 201 formed in insulators 280, etc. Conductive films 260A and 260B can be deposited, for example, by sputtering, CVD, MBE, PLD, plating, or ALD. In this embodiment, titanium nitride is deposited as conductive film 260A using CVD, and tungsten is deposited as conductive film 260B using CVD. Note that conductive films 260A and 260B can also be deposited simultaneously with heating the substrate. Substrate heating can also serve as a heating treatment for the oxide semiconductor film 230f described above. Therefore, sometimes the crystalline region of the oxide semiconductor 230 grows through the aforementioned substrate heating.
[0543] Next, the insulator 255, insulating film 250A, conductive film 260A, and conductive film 260B are polished by CMP until the insulator 280 is exposed. That is, the portions of the insulator 255, insulating film 250A, conductive film 260A, and conductive film 260B exposed from the opening 201 are removed. Thus, the insulator 255, insulator 250, and conductor 260 (conductor 260a and conductor 260b) are formed in the opening 201 (see reference). Figures 30A to 30D ).
[0544] Thus, insulator 255 is disposed within opening 201 in contact with insulator 280, insulator 275, and insulator 222. Insulator 250 is disposed within opening 201 in contact with insulator 255, conductor 242a1, conductor 242b1, oxide semiconductor 230, insulator 224, and insulator 222. Furthermore, conductor 260 is disposed such that it is inserted into opening 201 with insulator 250 in between. Thus, transistor 200 is formed.
[0545] Next, an insulator 282 is formed on insulator 255, insulator 250, conductor 260 and insulator 280 (see reference). Figures 1A to 1D The insulator 282 can be deposited, for example, using sputtering, CVD, MBE, PLD, or ALD methods. Sputtering is preferred for depositing the insulator 282. Alternatively, during the deposition of the insulator 282, a first layer can be formed using ALD, and a second layer can be formed thereon using sputtering.
[0546] Furthermore, by depositing insulator 282 in an oxygen-containing atmosphere using sputtering, oxygen can be added to insulator 280 during deposition. This allows insulator 280 to contain excess oxygen. In this case, it is preferable to deposit insulator 282 while heating the substrate. By depositing insulator 282 in this way, an appropriate amount of oxygen can be supplied from insulator 280 to oxide semiconductor 230 via insulator 250. Additionally, by providing insulator 250a within insulator 250, excessive oxidation of the vicinity of insulator 250 of conductors 242a and 242b due to excessive oxygen supply to insulator 250 can be prevented.
[0547] Alumina is deposited using an aluminum target in an atmosphere containing oxygen gas. The amount of oxygen injected into the insulator 280 can be controlled by the magnitude of the bias power applied to the substrate via sputtering. For example, a lower bias power results in less oxygen injected into the insulator 280, and the oxygen is easily saturated even if the thickness of the insulator 282 is small. Conversely, a higher bias power results in more oxygen injected into the insulator 280. By reducing the bias power, the amount of oxygen injected into the insulator 280 can be suppressed. Note that when applying a substrate bias using an RF power supply, the RF frequency is preferably 10 MHz or higher. Typically, it is 13.56 MHz. The higher the RF frequency, the less damage to the substrate can be caused.
[0548] In addition, by depositing a second layer on the first layer formed by the ALD method using a sputtering method, the upper end of the insulator 250 and the top surface of the conductor 260 can be protected from the impact of ion collisions caused by sputtering deposition.
[0549] Furthermore, heat treatment can be performed before depositing the insulator 282. This heat treatment can also be performed under reduced pressure, wherein the insulator 282 is deposited continuously without exposure to the atmosphere. By performing this treatment, moisture and hydrogen adsorbed on the surface of the insulator 280 can be removed, and the moisture concentration and hydrogen concentration in the insulator 280 can be reduced. The heat treatment temperature is preferably 100°C or higher and 400°C or lower. In this embodiment, the heat treatment temperature is set to 250°C.
[0550] Next, insulator 283 is formed on insulator 282 (see reference). Figures 1A to 1D The insulator 283 can be deposited, for example, using sputtering, CVD, MBE, PLD, or ALD methods. Sputtering is preferred for depositing the insulator 283. By using sputtering, which does not require the use of hydrogen-containing molecules as the deposition gas, the hydrogen concentration in the insulator 283 can be reduced. In this embodiment, silicon nitride is deposited as the insulator 283 using sputtering.
[0551] Here, it is preferable to deposit insulators 282 and 283 continuously without exposure to the atmospheric environment. By depositing without exposure to the atmosphere, impurities or moisture from the atmospheric environment can be prevented from adhering to insulators 282 and 283, thus keeping the interface or vicinity of the interface between insulators 282 and 283 clean.
[0552] In this embodiment, silicon nitride is deposited as insulator 283, and aluminum oxide is deposited as insulator 282. Thus, by using silicon nitride, which has the function of suppressing hydrogen diffusion, as insulator 283, hydrogen diffusion from the upper layer of transistor 200 can be suppressed. Furthermore, by using aluminum oxide, which has the function of trapping or fixing hydrogen, as insulator 282, hydrogen contained in insulator 280 and the like can be trapped or fixed by insulator 282. Therefore, the hydrogen concentration in and around oxide semiconductor 230 can be reduced.
[0553] Next, openings leading to conductor 242a and conductor 242b are formed in insulators 275, 280, 282, and 283 (see reference). Figures 1A to 1D The opening can be formed using lithography. When forming the opening, dry etching is preferably used on the workpiece. Dry etching is capable of anisotropic etching, making it suitable for forming openings with high aspect ratios. When performing anisotropic etching, reactive ion etching is preferred, for example. For information on the conditions and apparatus for dry etching, please refer to the previous description. Note that in... Figure 1A The opening appears as a quadrilateral when viewed from above, but it is not limited to this. For example, when viewed from above, the opening can also appear as a circle, an ellipse, or a polygon, or a quadrilateral or other polygon with rounded corners.
[0554] Next, a heat treatment can be performed after the opening is formed. The heat treatment temperature can be 100°C or higher and 600°C or lower, preferably 250°C or higher and 550°C or lower, more preferably 350°C or higher and 450°C or lower. The heat treatment is preferably performed in a nitrogen or inert gas atmosphere. In addition, since the heat treatment is performed with the conductors 242a and 242b exposed, it is preferable to perform it in an atmosphere that does not contain oxidizing gases or oxygen gases. For example, it is preferable to perform the heat treatment at 400°C for 1 hour in a nitrogen atmosphere. Furthermore, the heat treatment can also be performed under reduced pressure. Through the heat treatment, oxygen contained in the insulator 280 can be supplied to the oxide semiconductor 230 through the insulator 250. As a result, oxygen vacancies in the channel formation region of the oxide semiconductor 230 can be reduced. Furthermore, the heat treatment can also be used as a heat treatment for the oxide semiconductor film 230f. Therefore, sometimes the crystalline region of the oxide semiconductor 230 is grown through the heat treatment.
[0555] Here, since the side of the insulator 280 is exposed in the aforementioned opening, the oxygen contained in the insulator 280 can be diffused outward by the aforementioned heat treatment, thereby controlling the amount of oxygen contained in the insulator 280. On the other hand, since the insulator 280 is provided with oxygen-barrier insulators 282 and 283, oxygen does not diffuse outward from the top surface of the insulator 280. Thus, excessive oxygen can be prevented from diffusing outward from the insulator 280 and forming oxygen vacancies in the insulator 280. Furthermore, the oxide semiconductor 230, conductors 242a and 242b are covered by the insulator 275. Thus, excessive oxygen can be prevented from directly diffusing from the insulator 280 to the oxide semiconductor 230, conductors 242a and 242b during the aforementioned heat treatment.
[0556] In this way, by adjusting the oxygen content in the insulator 280 to a more appropriate level, a suitable amount of oxygen can be supplied to the oxide semiconductor 230. This reduces oxygen vacancies in the oxide semiconductor 230 and prevents excessive oxygen supply. Therefore, the electrical characteristics and reliability of the transistor 200 can be improved. Furthermore, the process of exposing the side of the insulator 280 can also serve as the process of forming openings for embedding conductors 240a and 240b, thus simplifying the manufacturing process of the semiconductor device.
[0557] Next, an insulating film is deposited to form insulator 241, and the insulating film is anisotropically etched to form insulator 241a in the opening reaching conductor 242a and insulator 241b in the opening reaching conductor 242b (see reference). Figures 1A to 1DThe insulating film that forms the insulator 241 can be deposited using sputtering, CVD, MBE, PLD, or ALD methods. As the insulating film for insulator 241, an insulating film with oxygen-suppressing properties is preferred. For example, silicon nitride is preferably deposited using the PEALD method. Silicon nitride has high hydrogen barrier properties, so it is preferred.
[0558] Furthermore, during anisotropic etching of the insulating film that serves as insulator 241, a method such as dry etching can be employed. By providing insulator 241 on the sidewall of the opening, the permeation of oxygen from the outside can be suppressed, and oxidation of the conductors 240a and 240b to be formed subsequently can be prevented. Additionally, impurities such as water and hydrogen from insulator 280 can be prevented from diffusing into conductors 240a and 240b. Note that sometimes, due to this anisotropic etching, a recess is formed on a portion of the top surface of conductors 242a and 242b.
[0559] Next, conductive films 240a and 240b are deposited. The conductive films 240a and 240b preferably employ a multilayer structure comprising conductive materials that suppress the permeation of impurities such as water and hydrogen. For example, it can be a multilayer of tantalum nitride, titanium nitride, tungsten, molybdenum, copper, etc. The conductive films 240a and 240b can be deposited using methods such as sputtering, CVD, MBE, PLD, or ALD.
[0560] Next, a portion of the conductive film that forms conductors 240a and 240b is removed by CMP processing, exposing the top surface of insulator 283. As a result, the conductive film remains only at the opening, thereby forming conductors 240a and 240b with flat top surfaces (see reference). Figures 1A to 1D Note that sometimes a portion of the top surface of insulator 283 is removed during this CMP process.
[0561] As described above, by providing a conductor 240a that contacts conductor 242a, conductor 240a, which can be used as one of the source and drain terminals of transistor 200, can be electrically connected to wiring. Furthermore, by providing a conductor 240b that contacts conductor 242b, conductor 240b, which can be used as the other of the source and drain terminals of transistor 200, can be electrically connected to wiring.
[0562] Alternatively, conductive films for wiring or for plugs can be formed on conductors 240a and 240b.
[0563] The semiconductor device shown in Figure 1 can be manufactured through the above-described process.
[0564] The semiconductor device according to this embodiment includes an OS transistor. In this embodiment, by using indium oxide with a single-crystal structure or highly crystalline indium oxide as the oxide semiconductor layer of the OS transistor, a semiconductor device with high field-effect mobility can be provided. For example, the electrical characteristics, on-state current, S-value (subthreshold swing value), and frequency characteristics of the transistor can be improved. Furthermore, a semiconductor device with high reliability can be provided.
[0565] This embodiment can be appropriately combined with other embodiments. Furthermore, in this specification, where multiple structural examples are shown in one embodiment, these structural examples can be appropriately combined.
[0566] (Implementation Method 2) In this embodiment, a semiconductor device 900 according to one aspect of the present invention is described. The semiconductor device 900 can be used as a storage device.
[0567] Figure 31 A block diagram showing an example of the structure of a semiconductor device 900. Figure 31 The semiconductor device 900 shown includes a driving circuit 910 and a memory array 920. The memory array 920 includes one or more memory cells 950. Figure 31 An example of a memory array 920 including multiple memory cells 950 configured in a matrix is shown.
[0568] The transistor shown in Embodiment 1 can be used in the memory cell 950. By using the transistor described above, the operating speed of the memory device can be improved. Furthermore, miniaturization and high integration of the memory device can be achieved. In addition, the capacity per unit area of the memory device can be increased.
[0569] The drive circuit 910 includes a PSW 931 (power switch), a PSW 932, and peripheral circuit 915. The peripheral circuit 915 includes peripheral circuit 911, a control circuit 912, and a voltage generation circuit 928.
[0570] In the semiconductor device 900, circuits, signals, and voltages can be appropriately selected or omitted as needed. Alternatively, other circuits or signals can be added. Signals BW, CE, GW, CLK, WAKE, ADDR, WDA, PON1, and PON2 are signals input from the outside, while signal RDA is a signal output to the outside. Signal CLK is the clock signal.
[0571] In addition, signals BW, CE, and GW are control signals. Signal CE is the chip enable signal, signal GW is the global write enable signal, and signal BW is the byte write enable signal. Signal ADDR is the address signal. Signal WDA is for writing data, and signal RDA is for reading data. Signals PON1 and PON2 are power gating control signals. Furthermore, signals PON1 and PON2 can also be generated in the control circuit 912.
[0572] The control circuit 912 is a logic circuit that controls the overall operation of the semiconductor device 900. For example, the control circuit 912 performs logical operations on signals CE, GW, and BW to determine the operating mode of the semiconductor device 900 (e.g., write operation, read operation). Alternatively, the control circuit 912 generates control signals for the peripheral circuit 911 to execute the aforementioned operating mode.
[0573] The voltage generation circuit 928 has the function of generating voltage. The signal WAKE has the function of controlling the input signal CLK to the voltage generation circuit 928. For example, when a signal of level H is applied as the signal WAKE, the signal CLK is input to the voltage generation circuit 928, and the voltage generation circuit 928 generates voltage.
[0574] The peripheral circuit 911 is used to write and read data ...
Claims
1. A semiconductor device, comprising: Oxide semiconductor; First to fourth insulators; as well as First to third conductors, The second insulator is disposed on the first insulator. The oxide semiconductor is disposed on the first insulator and covers the second insulator. The first conductor and the second conductor are disposed on the oxide semiconductor. The third insulator is disposed on the first conductor and the second conductor and has an opening that overlaps with the region between the first conductor and the second conductor. The fourth insulator is disposed within the opening in a manner that overlaps with the oxide semiconductor. The third conductor is disposed within the opening on the fourth insulator. When viewed from above, the side surface of the first insulator is the same as or substantially the same as the side surface of the oxide semiconductor, the side surface of the first conductor, and the side surface of the second conductor. The thickness of the first insulator is greater than the thickness of the fourth insulator. When viewed in cross-section along the width of the trench, the height of the second insulator is greater than the width of the second insulator. The oxide semiconductor comprises indium and has a cubic crystal structure. The oxide semiconductor has a first region that contacts the side surface of the second insulator and a second region that contacts the top surface of the second insulator. Furthermore, the crystal orientation of the grains contained in the first region is consistent with or substantially consistent with the crystal orientation of the grains contained in the second region.
2. The semiconductor device according to claim 1, The oxide semiconductor comprises one grain.
3. The semiconductor device according to claim 1, The crystal orientation of the grains contained in the first region is the same as the crystal orientation of the grains contained in the second region. <111> .
4. The semiconductor device according to claim 1, The first insulator includes a fourth conductor. Furthermore, the fourth conductor is covered by the second insulator.
5. The semiconductor device according to claim 1, When viewed from above, a portion of the side of the third insulator is consistent with or substantially consistent with the side of the first conductor and the side of the second conductor.
6. The semiconductor device according to claim 1, The bottom surface of the third conductor has a portion located below the bottom surface of the oxide semiconductor.
7. The semiconductor device according to any one of claims 1 to 6, further comprising: The fifth insulator, Both the first conductor and the second conductor include a first conductive layer and a second conductive layer on the first conductive layer. The fifth insulator is disposed within the opening of the third insulator and is in contact with the top surface of the first conductive layer of the first conductor, the side surface of the second conductive layer of the first conductor, the top surface of the first conductive layer of the second conductor, and the side surface of the second conductive layer of the second conductor. The fifth insulator has an opening that overlaps with the region between the first conductive layer of the first conductor and the first conductive layer of the second conductor. Furthermore, the shortest distance between the first conductive layer of the first conductor and the first conductive layer of the second conductor is smaller than the shortest distance between the second conductive layer of the first conductor and the second conductive layer of the second conductor.
8. The semiconductor device according to claim 7, When viewed from above, a portion of the side surface of the third insulator is consistent with or substantially consistent with the side surface of the second conductive layer of the first conductor and the side surface of the second conductive layer of the second conductor.
9. The semiconductor device according to claim 7, The fifth insulator comprises silicon nitride.
10. The semiconductor device according to claim 7, The first conductive layer of the first conductor and the first conductive layer of the second conductor contain tantalum nitride.
Citation Information
Patent Citations
Semiconductor device
JP2011151383A
Semiconductor integrated circuit
JP2012257187A