Pulsed current assisted laser-arc welding of narrow gap of ferromagnetic materials and apparatus

By arranging conductive contacts on both sides of the narrow gap bevel to form a closed current loop, and utilizing the pulsed current to excite a self-induced magnetic field and the Joule heating effect, the problems of arc deflection and sidewall incomplete fusion in the welding of ferromagnetic materials are solved, achieving uniform heating and high-quality fusion of the welded joint.

CN123149581APending Publication Date: 2026-11-24SOUTHWEST JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611622895.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing technologies for welding ferromagnetic materials, the electric arc is prone to deflection and the energy is difficult to diffuse to the sidewalls, resulting in sidewall incomplete fusion defects. The effects of external magnetic fields or welding torch oscillation control methods are limited.

Method used

The pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials forms a closed current loop by arranging conductive contacts on both sides of the narrow-gap groove. The pulsed current excites a self-induced magnetic field to drive the arc deflection, and the Joule heating effect and Lorentz force promote the flow of the molten pool, thereby achieving directional heating and fusion of the sidewalls.

Benefits of technology

This method achieves uniform heating and full fusion of the sidewalls of the welded joint, improving welding quality and mechanical properties, eliminating sidewall incomplete fusion defects, and enhancing the metallurgical bonding quality and stability of the welded joint.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149581A_ABST
    Figure CN123149581A_ABST
Patent Text Reader

Abstract

This invention discloses a pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials. The method includes: positioning the laser head and welding torch above a narrow-gap groove; symmetrically arranging conductive contacts on both sides of the base material and connecting them to a pulsed power supply to form a closed current loop through the base material and the molten pool; outputting a pulsed current during the welding process, using an in-situ excited self-induced magnetic field to drive the arc to periodically and alternately deflect along the groove width direction; based on the Joule heating effect and the transverse Lorentz force generated by the coupling of the pulsed current and the self-induced magnetic field, driving the molten metal in the molten pool to flow towards the sidewalls of the groove on both sides; and completing the filler welding through the synergistic effect of directional arc heating, additional heat input, and preheating by molten metal flushing. This method avoids the shielding effect of the external magnetic field, solves the problem of incomplete fusion caused by uncontrollable arc deflection and insufficient heat input to the sidewalls in ferromagnetic materials, and significantly improves the weld formation quality and process stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of welding technology, and more specifically, to a pulsed current-assisted narrow-gap laser-arc welding method and equipment for ferromagnetic materials. Background Technology

[0002] Key components of high-end energy equipment such as large steam turbines commonly use extra-thick-walled ferromagnetic heat-resistant steel. Welding, as a core manufacturing process, directly determines service performance through joint quality. Currently, a highly promising welding method is narrow-gap laser-arc hybrid welding technology, which relies on the laser keyhole effect and arc wetting to complete filling welding within ultra-narrow gaps. However, conventional laser-arc hybrid narrow-gap welding suffers from significant technical drawbacks when applied to ferromagnetic materials: due to the uneven magnetic properties of the ferromagnetic base material or the shielding effect of the applied magnetic field, the arc is prone to uncontrollable deflection; simultaneously, the arc energy is naturally concentrated in the molten pool region at the center of the bevel, attenuating along the depth direction and failing to effectively diffuse to the sidewalls, resulting in insufficient heat input and incomplete melting of the bevel sidewalls, thus inducing severe sidewall incomplete fusion defects. Existing control methods such as applied alternating magnetic fields or mechanical oscillation of the welding torch are limited by narrow-gap spatial interference, weak magnetic field penetration, or the inability to overcome the magnetic bypass effect of ferromagnetic materials, making it difficult to effectively solve these problems. Summary of the Invention

[0003] The purpose of this invention is to provide a pulsed current-assisted narrow-gap laser-arc welding method and equipment for ferromagnetic materials, which addresses the shortcomings of existing technologies and solves the problems mentioned in the background.

[0004] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: A pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials includes: Position the laser head and welding torch above the narrow gap bevel of the ferromagnetic base material to be welded, and establish the laser-arc composite heat source arrangement relationship; Conductive contacts are symmetrically arranged on the base material surfaces on both sides of the narrow gap bevel, and the conductive contacts are connected to a pulse power supply to form a closed current loop through the base material and the molten pool in the narrow gap bevel. As the composite heat source travels along the welding direction, the pulse power supply is controlled to output pulse current to the current closed loop. Based on the self-induced magnetic field generated in situ by the pulse current in the current closed loop, the arc in the composite heat source is driven to periodically deflect alternately along the width direction of the narrow gap bevel. At the same time, based on the Joule heating effect generated by the pulse current flowing through the molten pool and the bevel sidewall region, and the transverse Lorentz force generated by the coupling of the pulse current and the self-induced magnetic field, the liquid metal in the molten pool is driven to flow to the bevel sidewalls on both sides. Under the combined effects of the directional heating of the sidewalls of the bevel by the periodic alternating deflection of the electric arc, the additional heat input of the Joule heating effect, and the scouring and preheating of the sidewalls by the transverse flow of liquid metal, the filling welding of the narrow gap bevel is completed, resulting in a welded joint with fused sidewalls.

[0005] Furthermore, conductive contacts are symmetrically arranged on the base material surfaces on both sides of the narrow gap bevel, including: Conductive contacts are symmetrically arranged on the upper surface of the base material on both sides of the narrow gap bevel, and the downward pressure of the conductive contacts is adjusted so that the end face of the conductive contacts is pressed tightly against the surface of the base material. During the welding process, the conductive contacts are controlled to move synchronously with the welding head along the welding direction to maintain the continuous conduction of the current closed loop.

[0006] Furthermore, controlling the pulse power supply to output pulse current to the current closed loop includes: The control pulse power supply outputs AC pulse current, causing the electric arc to oscillate periodically along the width direction of the narrow gap bevel. The waveform of an alternating pulse current is a rectangular wave or a sine wave.

[0007] Furthermore, the parameters of the alternating pulse current satisfy the following conditions: The pulse current intensity is 400A~2000A, the pulse current pulse width is 2ms~20ms, and the pulse current frequency is 5Hz~50Hz.

[0008] Furthermore, the arrangement relationship of the laser-arc composite heat source is established, including: The laser head is positioned with a laser leader and arc follower, tilted forward along the welding direction at an angle α of 3°. ~10 ; The welding torch is tilted to the side of the laser head, with a tilt angle β of 60°. ~70 ; The filament spacing b is defined as the horizontal distance between the tip of the welding wire and the central axis of the laser beam, and the filament spacing b is set to 3mm~4mm.

[0009] Furthermore, the process of controlling the pulse power supply to output pulse current to the current closed loop also includes: Get the current welding travel speed; The frequency of the pulse current output by the pulse power supply is dynamically adjusted based on the welding travel speed, so that the single-cycle deflection coverage of the arc matches the welding travel speed.

[0010] Furthermore, the frequency of the pulse current output by the pulse power supply is dynamically adjusted based on the welding travel speed, including: When the welding travel speed decreases, the pulse current frequency should be adjusted to a lower level; when the welding travel speed increases, the pulse current frequency should be adjusted to a higher level. During the welding process, the real-time amplitude and waveform of the pulse current are monitored online using a Hall sensor and an oscilloscope.

[0011] Furthermore, before positioning the laser head and welding torch above the narrow-gap bevel of the ferromagnetic base material to be welded, the process also includes: The welding torch tip is equipped with a conductive tip, and high-temperature resistant insulating cloth is evenly wrapped around the outer wall of the conductive tip for insulation, thereby blocking the conductive path between the conductive tip and the narrow gap bevel sidewall. The conductive tip is a narrow-gap conductive tip with a reduced diameter to fit the width of the narrow-gap bevel.

[0012] Furthermore, before positioning the laser head and welding torch above the narrow-gap bevel of the ferromagnetic base material to be welded, the process also includes: The inner wall and both end faces of the narrow gap bevel are polished to remove oxide scale, and surface impurities are removed by wiping with solvent. The ferromagnetic base material to be welded is clamped and fixed, and the misalignment of the ferromagnetic base material to be welded is controlled within 0.3mm; Preheat the ferromagnetic base material to be welded to 200℃ before welding. 300℃, and preset 1 according to the workpiece structure ~5 The amount of inverse deformation; After completing the filler welding of the narrow gap bevel, the following is also included: The shielding gas delivered coaxially by the welding torch is controlled to shut off after a delay of 5 to 10 seconds. The shielding gas is high-purity argon, and the flow rate of the shielding gas during the welding process is 30 L / min to 40 L / min.

[0013] A welding apparatus, the above method, comprising: The welding machine body includes a laser head, welding torch, conductive contacts, and pulse power supply. The laser head is vertically positioned above the narrow gap bevel of the ferromagnetic base material to be welded; The welding torch is tilted to the side of the laser head, and a conductive tip is fitted to the end of the welding torch. Two conductive contacts are symmetrically arranged on both sides of the laser head. The end faces of the conductive contacts are used to press against the upper surface of the base material on both sides of the narrow gap bevel. The pulse power supply is connected to two conductive contacts via a cable and is used to output pulse current to a closed current loop consisting of the conductive contacts, the base material, and the molten pool. The pulse power supply is configured to output AC pulse current, which causes the self-induced magnetic field generated in the current closed loop to drive the electric arc to deflect periodically and alternately along the width direction of the narrow gap bevel.

[0014] This invention has at least the following advantages or beneficial effects: This invention provides a pulsed current-assisted narrow-gap laser-arc welding method and equipment for ferromagnetic materials. By symmetrically arranging conductive contacts on both sides of the narrow-gap groove to form a closed current loop through the base material and the molten pool, a self-induced magnetic field is generated in situ using the pulsed current. This magnetic field directly acts on the arc and molten pool regions. Based on this self-induced magnetic field, the Lorentz force generated by the pulsed current drives the arc to periodically deflect alternately along the groove width direction, breaking the inertial distribution of arc energy concentrated in the center and achieving directional heating of the groove sidewalls on both sides. Simultaneously, the pulsed current flowing through the high-resistivity molten pool and groove sidewall regions generates a significant Joule heating effect, providing an additional heat input source to compensate for the thermal energy attenuation of the laser-arc composite heat source in the deep sidewalls. Furthermore, the transverse Lorentz force generated by the coupling of the pulsed current and the self-induced magnetic field also drives the liquid metal in the molten pool to flow violently towards the groove sidewalls on both sides. This not only promotes the transfer of high-temperature metal to the low-temperature sidewalls but also effectively scours and preheats the sidewalls, further reducing the activation energy for sidewall melting. This invention ensures a uniform distribution of energy in the width and depth directions of the bevel, thereby effectively eliminating the sidewall incomplete fusion defects commonly found in narrow gap welding of ferromagnetic materials with a large depth-to-width ratio, and improving the metallurgical bonding quality and mechanical property stability of the welded joint. Attached Figure Description

[0015] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0016] Figure 1 A front view of the apparatus for a pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials provided in this application; Figure 2 A side view of an apparatus for a pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials provided in this application; Figure 3 A schematic diagram showing the filament spacing of the device provided in this application; Figure 4 A schematic diagram of the narrow gap bevel dimensions for the device provided in this application; Figure 5 A schematic diagram showing the dimensions of the narrow-gap dedicated conductive nozzle for the device provided in this application; Figure 6 A schematic diagram of the numerical simulation results of the current distribution field of the device provided in this application; Figure 7 A schematic diagram of the numerical simulation results of the magnetic field distribution of the device provided in this application; Figure 8 High-speed camera images of random deflection of an uncontrolled electric arc without pulsed current assistance; Figure 9 High-speed camera images showing the controlled oscillation of an electric arc under pulsed current assistance; Figure 10 A cross-sectional view of a narrow-gap laser-arc hybrid welding joint without pulsed current assistance; Figure 11 A cross-sectional view of a narrow-gap laser-arc hybrid welding joint under pulsed current assistance; Figure 12 The flowchart provided in this application illustrates a pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials.

[0017] Icons: 1. Laser head; 2. Welding gun; 21. Welding wire; 22. Conductive nozzle; 3. Base material; 41. First conductive contact; 42. Second conductive contact; 5. Pulse power supply. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The components of the embodiments of the present invention described and shown in the accompanying drawings can generally be arranged and designed in various different configurations.

[0019] Please refer to Figures 1 to 12 As shown, the welding equipment includes a laser head 1, a welding torch 2, a conductive nozzle 22, two conductive contacts (a first conductive contact 41 and a second conductive contact 42, respectively), and a pulse power supply 5. The laser head 1 is vertically positioned directly above the narrow-gap bevel of the ferromagnetic base material 3 to be welded. The welding torch 2 is tilted to the side of the laser head 1, and the conductive nozzle 22 is mounted at the end of the torch 2. The base material 3 has a pre-formed narrow-gap bevel located between two pieces of base material 3. The welding wire 21 is fed into the weld pool area within the narrow-gap bevel through the internal guide channel of the conductive nozzle 22. The first conductive contact 41 and the second conductive contact 42 are symmetrically arranged on both sides of the laser head 1, i.e., on both sides of the width direction of the narrow-gap bevel. The end faces of the conductive contacts are used to press against the upper surfaces of the base material 3 on both sides of the narrow-gap bevel. The pulse power supply 5 is connected to the two conductive contacts via cables and is used to output pulsed current to the closed current loop formed by the conductive contacts, the base material 3, and the weld pool.

[0020] According to this embodiment, the core operation process of the welding method is as follows: The laser head 1 and welding torch 2 are positioned above the narrow gap groove of the ferromagnetic base material 3 to be welded, establishing a laser-arc composite heat source arrangement; conductive contacts are symmetrically arranged on the surface of the base material 3 on both sides of the narrow gap groove, and the conductive contacts are connected to the pulse power supply 5 to form a closed current loop through the base material 3 and the molten pool within the narrow gap groove; as the composite heat source travels along the welding direction, the pulse power supply 5 is controlled to output pulse current to the closed current loop; based on the self-induced magnetism excited in situ by the pulse current in the closed current loop... The electric arc in the composite heat source is driven to periodically and alternately deflect along the width of the narrow gap bevel. At the same time, based on the Joule heating effect generated by the pulsed current flowing through the molten pool and the bevel sidewall region, and the transverse Lorentz force generated by the coupling of the pulsed current and the self-induced magnetic field, the liquid metal in the molten pool is driven to flow towards the bevel sidewalls on both sides. Under the synergistic effect of the directional heating of the bevel sidewalls by the periodic alternating deflection of the electric arc, the additional heat input of the Joule heating effect, and the scouring and preheating of the sidewalls by the transverse flow of the liquid metal, the filling welding of the narrow gap bevel is completed, and a welded joint with sidewall fusion is obtained.

[0021] The following is an exemplary welding scenario illustrating the overall operation of the above method. In this scenario, the laser head 1 is tilted forward along the welding direction to output a laser beam. The laser beam is focused on the surface of the base material 3 at the bottom of the narrow-gap groove, forming a keyhole and melting the base metal. Simultaneously, the welding torch 2 feeds in the welding wire 21, which melts under the heat of the electric arc, forming molten droplets that transition into the molten pool and merge with the laser-melted base metal to form a eutectic pool. At this time, the pulse power supply 5 forms a complete conductive loop through the first conductive contact 41, one side of the base material 3, the molten pool, the other side of the base material 3, and the second conductive contact 42. The pulse power supply 5 outputs an alternating current pulse to this loop. When the pulse current flows through this closed loop, a self-induced magnetic field is generated in the space surrounding the loop. Since the self-induced magnetic field is located inside the groove, adjacent to the region of the electric arc and the molten pool, the charged particles in the electric arc are subjected to a Lorentz force in the magnetic field, causing the electric arc to deflect in the groove width direction. Because the pulsed current is an alternating waveform with periodically alternating directions, the direction of the self-induced magnetic field also periodically reverses, and the direction of the Lorentz force on the arc alternates synchronously, thus driving the arc to periodically reciprocate along the bevel width direction. Simultaneously, when the pulsed current flows through the molten pool and bevel sidewall region, significant Joule heating is generated due to the high current density and high resistance in this region. Furthermore, the pulsed current and the self-induced magnetic field couple, inducing a transverse Lorentz force in the liquid metal within the molten pool, driving the liquid metal to flow towards the bevel sidewalls on both sides. Upon reaching the sidewalls, the driven high-temperature liquid metal forcibly scours the sidewalls and transfers heat to them, serving a preheating function. Based on the above process, the filling welding of the narrow-gap bevel is completed, ultimately resulting in a welded joint where both bevel sidewalls are fully fused.

[0022] In one embodiment, conductive contacts are symmetrically arranged on the upper surface of the base material 3 on both sides of the narrow gap bevel, and the downward pressure of the conductive contacts is adjusted so that the end faces of the conductive contacts are pressed tightly against the surface of the base material 3. As a specific implementation, the conductive contacts are constructed as roller structures that can rotate around their own axis, with their outer circumferential end faces forming line contact or narrow band contact with the upper surface of the base material 3. By adjusting the downward stroke of the conductive contacts relative to the welding head, the end faces of the conductive contacts are pressed tightly against the surface of the base material 3 with a certain contact pressure, thereby ensuring good electrical contact and reliable conductivity between the two. During the welding process, the conductive contacts are controlled to move synchronously with the welding head along the welding direction to maintain the continuous conduction of the current closed loop. That is, as the laser head 1 and the welding torch 2 advance along the weld direction, the conductive contacts roll or slide synchronously on the surface of the base material 3, thereby always maintaining the continuous unobstructed flow of the closed loop formed at the current welding position. By using a combination of pressing and synchronous movement, the contact resistance between the conductive contact and the surface of the base material 3 is effectively reduced, avoiding circuit breakage or current fluctuations caused by poor contact, ensuring stable injection of pulse current, and providing a continuous and reliable current carrier for arc deflection and molten pool flow control.

[0023] The arrangement of the laser-arc composite heat source is established, including: adopting a laser-leading, arc-following arrangement, with the laser head 1 tilted forward along the welding direction at an angle α of 3°~10°; the welding torch 2 tilted to the side of the laser head 1 at an angle β of 60°~70°; and the filament spacing b defined as the horizontal distance between the tip of the welding wire 21 and the central axis of the laser beam, with a spacing of 3mm~4mm. Specifically, as the composite heat source travels along the welding direction, the laser beam first acts on the area to be welded, forming a keyhole and preheating and deeply melting the base material 3; the arc heats and wets the formed molten pool and bevel sidewalls behind and to the side of the laser beam. The laser head 1 is tilted forward along the welding direction at an angle α, which aims to direct the incident direction of the laser beam towards the welding front, preventing the laser beam from reflecting back from the surface of the formed weld to the optical components of the laser head 1 and causing damage, while also facilitating arc guidance and molten pool stabilization. Within the tilt angle α range of 3° to 10°, reflected light can be effectively avoided without the laser beam forming an excessively large elliptical spot on the surface of the base material 3 due to an excessively large forward tilt angle, thus reducing the laser power density. The tilt angle β of the welding torch 2 is set to 60° to 70°. Within this angle range, the contact tip 22 and the welding wire 21 can smoothly extend into the narrow space of the narrow gap groove, ensuring that the end of the welding wire 21 is positioned appropriately behind the laser keyhole, so that the molten droplet transition of the welding wire 21 forms an effective coupling with the molten pool area of ​​the laser keyhole. The wire spacing b is 3mm to 4mm. If this distance is too small, the end of the welding wire 21 may be too close to the laser beam, causing the welding wire 21 to be prematurely melted by the laser beam or to stick to the end of the contact tip 22; if this distance is too large, the synergistic coupling effect between the laser and the arc is weakened, the formation conditions of the eutectic pool deteriorate, and the stability of the composite welding is reduced.

[0024] Before positioning the laser head 1 and welding torch 2 above the narrow gap bevel of the ferromagnetic base material 3 to be welded, the welding torch 2 is equipped with a conductive nozzle 22 at its end. The outer wall of the conductive nozzle 22 is uniformly wrapped with high-temperature resistant insulating cloth for insulation and isolation treatment, so as to block the conductive path between the conductive nozzle 22 and the side wall of the narrow gap bevel. The conductive nozzle 22 is a narrow gap-specific conductive nozzle with a reduced diameter to adapt to the width of the narrow gap bevel.

[0025] Before positioning the laser head 1 and welding torch 2 above the narrow gap bevel of the ferromagnetic base material 3 to be welded, the process includes: grinding the inner wall and both end faces of the narrow gap bevel to remove oxide scale, and wiping away surface impurities with solvent; clamping and fixing the ferromagnetic base material 3 to be welded, controlling the misalignment of the ferromagnetic base material 3 to be welded to within 0.3mm; preheating the ferromagnetic base material 3 to be welded before welding, with a preheating temperature of 200℃~300℃, and presetting a reverse deformation amount of 1°~5° according to the workpiece structure.

[0026] Controlling the pulse power supply 5 to output pulse current into the closed-loop current circuit includes: controlling the pulse power supply 5 to output AC pulse current, causing the arc to periodically oscillate back and forth along the width direction of the narrow gap bevel. The waveform of the AC pulse current is a rectangular wave or a sine wave. Specifically, when the pulse current is in the positive half-cycle, the current flows through the closed loop in a certain direction, and the arc is deflected to one side of the bevel width direction by the Lorentz force in the self-induced magnetic field in that direction; when the pulse current enters the negative half-cycle, the current direction reverses, and the direction of the Lorentz force on the arc also reverses, driving the arc to deflect to the other side of the bevel width direction. Thus, the arc forms a periodic reciprocating oscillation in the bevel width direction corresponding to the frequency of the AC pulse current. Both rectangular waves and sine waves can be directly output from a standard pulse power supply without the need for additional waveform transformation. Compared to rectangular waves, sine waves have a slower rate of change during current commutation, and the change in the self-induced magnetic field is also relatively gentle. Therefore, the commutation process of the arc swing is more gentle and has less disturbance and impact on the molten pool. On the other hand, rectangular waves commutate rapidly, and the self-induced magnetic field is generated and established faster, which is conducive to realizing the state switching of the arc on both sides and the arc dwelling position is more clearly defined.

[0027] Furthermore, the parameters of the AC pulse current meet the following conditions: pulse current intensity of 400A~2000A, pulse current pulse width of 2ms~20ms, and pulse current frequency of 5Hz~50Hz. These parameter ranges were determined based on extensive process experiments, specifically for typical bevel widths and filler welding conditions of ferromagnetic heat-resistant steel with large aspect ratios and narrow gaps. When the pulse current intensity is below 400A, the unit current density is low, and the generated self-induced magnetic field strength is insufficient to drive the arc to produce a significant deflection. The arc remains mainly concentrated in the center region of the bevel, and the directional heating effect on the sidewalls is not significant. Conversely, when the current intensity is above 2000A, the current density in the molten pool is too high, and the Joule heat input exceeds the process requirements, easily causing adverse problems such as molten pool overheating and weld coarsening. When the pulse current width is less than 2ms, the continuous conduction time of the current in one direction is too short, and the arc deflection and residence time in that direction is insufficient, making it difficult to effectively heat the sidewall. When the pulse width is greater than 20ms, the arc residence time on one side is too long, which can easily cause local overheating of the sidewall and reduce the frequency response capability of alternating deflection on both sides. When the pulse current frequency is less than 5Hz, the arc oscillation period is too long, and the matching with the welding travel speed becomes poor, which can easily lead to periodic omissions in sidewall heating in the welding travel direction. When the frequency is greater than 50Hz, the effective following ability of the arc deflection decreases due to the limitations of arc plasma inertia and molten pool response speed, and the stability and uniformity of sidewall heating actually deteriorate.

[0028] In some embodiments, the process of controlling the pulse power supply 5 to output pulse current to the current closed loop further includes: acquiring the current welding travel speed; dynamically adjusting the frequency of the pulse current output by the pulse power supply 5 based on the welding travel speed, so that the single-cycle deflection coverage of the arc matches the welding travel speed. Further, dynamically adjusting the frequency of the pulse current output by the pulse power supply 5 based on the welding travel speed includes: correspondingly lowering the pulse current frequency when the welding travel speed decreases; correspondingly increasing the pulse current frequency when the welding travel speed increases; and monitoring the real-time amplitude and waveform of the pulse current online using a Hall sensor and an oscilloscope during the welding process. Specifically, the welding travel speed determines the forward speed of the composite heat source along the weld direction, while the time required for the arc to complete one full width-direction round-trip deflection in a single cycle is determined by the frequency of the pulse current. To ensure a continuous and uniform heat input distribution along the weld length, the deflection coverage of the arc in a single cycle should match the welding travel speed, i.e., the number of arc deflections per unit length in the welding travel direction should remain stable.

[0029] After completing the filling welding of the narrow gap groove, the process also includes: controlling the shielding gas delivered coaxially by the welding torch 2 to be turned off after a delay of 5s to 10s. The shielding gas is high-purity argon, and the flow rate of the shielding gas is 30L / min to 40L / min, in order to avoid oxidation of the high-temperature weld and the weld bead end.

[0030] This application also provides a welding device for implementing the above-described method. The welding device includes a welding machine body, which comprises a laser head 1, a welding torch 2, and conductive contacts. The laser head 1 is vertically arranged above the narrow gap bevel of the ferromagnetic base material 3 to be welded. The welding torch 2 is inclinedly arranged to the side of the laser head 1, and a conductive nozzle 22 is fitted to the end of the welding torch 2. Two conductive contacts are symmetrically arranged on both sides of the laser head 1, and the end faces of the conductive contacts are used to press against the upper surfaces of the base material 3 on both sides of the narrow gap bevel. A pulse power supply 5 is connected to the two conductive contacts via a cable and is used to output a pulse current to a closed current loop formed by the conductive contacts, the base material 3, and the molten pool. The pulse power supply 5 is configured to output an alternating current pulse, causing the self-induced magnetic field excited in the closed current loop to drive the arc to periodically and alternately deflect along the width direction of the narrow gap bevel. The structural composition of this welding device corresponds to the description of the device in the aforementioned method embodiments. The connection relationships, spatial relationships, and cooperative working methods between the components have been described in detail in the aforementioned method embodiments, and will not be repeated here. The welding equipment generates a self-induced magnetic field in the closed loop formed by the conductive contact, the base material 3, and the molten pool through the AC pulse current output by the pulse power supply 5. The self-induced magnetic field drives the arc to deflect periodically and alternately in the width direction of the narrow gap bevel. At the same time, the Joule heating effect and transverse Lorentz force generated by the pulse current in the molten pool and bevel sidewall area together ensure the full fusion of the bevel sidewall.

[0031] The technical solution of this application will be further described below with reference to a specific embodiment. This embodiment takes the welding of 45mm thick 12Cr2MoR and 1Cr12Mo dissimilar heat-resistant steels as an example. Both 12Cr2MoR and 1Cr12Mo are ferromagnetic heat-resistant steels, which have a strong magnetic bypass and shielding effect on the applied magnetic field. Among them, 12Cr2MoR has stronger ferromagnetism, and under conventional welding conditions, the arc is prone to spontaneously deflecting to this side, resulting in poor controllability of arc deflection. In this embodiment, the narrow gap groove width is only 6mm, and the space is small, making it impossible to use mechanical oscillation of the welding torch or cable wire oscillation scheme. At the same time, due to the large groove depth, the laser beam focusing characteristics limit the use of beam oscillation technology. If the upper focal diameter of the beam is increased, it is very easy to interfere with the upper edge of the groove when deflected to both sides. The welding equipment in this embodiment forms a closed loop of "first conductive contact 41 - base material 3 - molten pool - base material 3 - second conductive contact 42", which can generate a self-induced magnetic field in situ inside the bevel without the need for an external magnetic field to penetrate the base material 3, thus avoiding the magnetic bypass shielding effect of ferromagnetic materials in principle. This embodiment uses Thermanit CG MTS 3 welding wire with a diameter of 1.2mm. The parameters for the root pass are: laser power 11000W, wire feed speed 8m / min, welding current 800A, welding speed 12mm / s, argon flow rate 30L / min, defocusing amount 0mm, wire spacing 3mm, laser head tilt angle α of 5°, and welding torch tilt angle β of 65°. The parameters for cover welding are as follows: laser power 1700W, wire feed speed 7m / min, welding current 285A, welding speed 5mm / s, argon flow rate 30L / min, defocusing amount 0mm, filament spacing 3mm, laser head tilt angle α is 5°, welding torch tilt angle β is 65°; AC auxiliary pulse current intensity 800A, pulse width 5ms, frequency 20Hz.

[0032] Numerical simulations were conducted on the conduction and distribution of the pulsed current under the aforementioned actual working parameters. The results show that an extremely high current density exists in the molten pool region, with a peak value reaching 500 A / mm², confirming that the pulsed current can form a complete closed loop. Simultaneously, the magnetic field distribution simulation results indicate that the closed loop of the pulsed current can generate an effective self-induced magnetic field in the arc and molten pool regions, providing sufficient Lorentz force to drive the arc deflection. During cap welding, without the application of AC pulsed current assistance, the arc exhibits a random and irregular deflection; after introducing AC pulsed current on both sides of the bevel, the arc exhibits periodic and regular reciprocating oscillations along the width of the bevel, demonstrating that the pulsed current has good controllability over the arc deflection behavior. Without auxiliary pulsed current, the random and uncontrollable deflection of the arc leads to insufficient heating of one or both sides of the bevel, causing severe sidewall incomplete fusion defects; simultaneously, the high residual stress level during weld solidification makes it prone to hot cracking. After applying an auxiliary pulsed current, the electric arc periodically and alternately heats the sidewalls of the bevel on both sides. Combined with the Joule heating of the pulsed current and the preheating effect of the molten pool's transverse flow driven by the Lorentz force, multiple mechanisms work together to ensure that both sidewalls are fully melted, forming a good metallurgical bond. Simultaneously, the electroplastic effect induced by the pulsed current can alleviate the shrinkage stress during weld solidification, effectively inhibiting the initiation of hot cracks. Using the process method of this embodiment, for deep, narrow-gap bevels of ferromagnetic heat-resistant steel, the magnetic bypass shielding effect of the external magnetic field can be avoided in principle. Through the synergistic effect of controllable arc oscillation, Joule heating, and molten pool transverse flow preheating, the sidewall incomplete fusion defects of each weld layer are eliminated, while the tendency for welding hot cracking is reduced. The weld joint quality meets the long-term service requirements of thick-walled high-end energy equipment.

[0033] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials, characterized in that, include: Position the laser head and welding torch above the narrow gap bevel of the ferromagnetic base material to be welded, and establish the laser-arc composite heat source arrangement relationship; Conductive contacts are symmetrically arranged on the base material surfaces on both sides of the narrow gap bevel, and the conductive contacts are connected to a pulse power supply to form a closed current loop through the base material and the molten pool in the narrow gap bevel. As the composite heat source travels along the welding direction, the control pulse power supply outputs pulse current to the current closed loop. Based on the self-induced magnetic field generated in situ by the pulsed current in the current closed loop, the electric arc in the composite heat source is driven to periodically and alternately deflect along the width direction of the narrow gap bevel; at the same time, based on the Joule heating effect generated by the pulsed current flowing through the molten pool and the bevel sidewall region, and the transverse Lorentz force generated by the coupling of the pulsed current and the self-induced magnetic field, the liquid metal in the molten pool is driven to flow to the bevel sidewalls on both sides. Under the combined effects of the directional heating of the sidewalls of the bevel by the periodic alternating deflection of the electric arc, the additional heat input of the Joule heating effect, and the scouring and preheating of the sidewalls by the transverse flow of liquid metal, the filling welding of the narrow gap bevel is completed, resulting in a welded joint with fused sidewalls.

2. The pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials according to claim 1, characterized in that, Conductive contacts are symmetrically arranged on the base material surfaces on both sides of the narrow gap bevel, including: Conductive contacts are symmetrically arranged on the upper surface of the base material on both sides of the narrow gap bevel, and the downward pressure of the conductive contacts is adjusted so that the end face of the conductive contacts is pressed tightly against the surface of the base material. During the welding process, the conductive contacts are controlled to move synchronously with the welding head along the welding direction to maintain the continuous conduction of the current closed loop.

3. The pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials according to claim 1, characterized in that, Controlling the pulse power supply to output pulse current to the current closed loop includes: The control pulse power supply outputs AC pulse current, causing the electric arc to oscillate periodically along the width direction of the narrow gap bevel. The waveform of an alternating pulse current is a rectangular wave or a sine wave.

4. The pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials according to claim 3, characterized in that, The parameters of the alternating pulse current must satisfy the following conditions: The pulse current intensity is 400A~2000A, the pulse current pulse width is 2ms~20ms, and the pulse current frequency is 5Hz~50Hz.

5. The pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials according to claim 1, characterized in that, Establishing the arrangement relationship of laser-arc composite heat sources includes: The laser head is positioned with a laser leader and arc follower, tilted forward along the welding direction at an angle α of 3°. ~10 ; The welding torch is tilted to the side of the laser head, with a tilt angle β of 60°. ~70 ; The filament spacing b is defined as the horizontal distance between the tip of the welding wire and the central axis of the laser beam, and the filament spacing b is set to 3mm~4mm.

6. The pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials according to claim 1, characterized in that, The process of controlling the pulse power supply to output pulse current to the current closed loop also includes: Get the current welding travel speed; The frequency of the pulse current output by the pulse power supply is dynamically adjusted based on the welding travel speed, so that the single-cycle deflection coverage of the arc matches the welding travel speed.

7. The pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials according to claim 6, characterized in that, The frequency of the pulse current output by the pulse power supply is dynamically adjusted based on the welding travel speed, including: When the welding travel speed decreases, the pulse current frequency should be adjusted to a lower level; when the welding travel speed increases, the pulse current frequency should be adjusted to a higher level. During the welding process, the real-time amplitude and waveform of the pulse current are monitored online using a Hall sensor and an oscilloscope.

8. The pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials according to claim 1, characterized in that, Before positioning the laser head and welding torch above the narrow-gap bevel of the ferromagnetic base material to be welded, the process also includes: The welding torch tip is equipped with a conductive tip, and high-temperature resistant insulating cloth is evenly wrapped around the outer wall of the conductive tip for insulation, thereby blocking the conductive path between the conductive tip and the narrow gap bevel sidewall. The conductive tip is a narrow-gap conductive tip with a reduced diameter to fit the width of the narrow-gap bevel.

9. The pulsed current-assisted narrow-gap laser-arc welding method for ferromagnetic materials according to claim 1, characterized in that, Before positioning the laser head and welding torch above the narrow-gap bevel of the ferromagnetic base material to be welded, the process also includes: The inner wall and both end faces of the narrow gap bevel are polished to remove oxide scale, and surface impurities are removed by wiping with solvent. The ferromagnetic base material to be welded is clamped and fixed, and the misalignment of the ferromagnetic base material to be welded is controlled within 0.3mm; Preheat the ferromagnetic base material to be welded to 200℃ before welding. 300℃, and preset 1 according to the workpiece structure ~5 The amount of inverse deformation; After completing the filler welding of the narrow gap bevel, the following is also included: The shielding gas delivered coaxially by the welding torch is controlled to shut off after a delay of 5 to 10 seconds. The shielding gas is high-purity argon, and the flow rate of the shielding gas during the welding process is 30 L / min to 40 L / min.

10. A welding apparatus for implementing the method of claim 1, characterized in that, include: The welding machine body includes a laser head, welding torch conductive contacts, and a pulse power supply. The laser head is vertically positioned above the narrow gap bevel of the ferromagnetic base material to be welded; The welding torch is tilted to the side of the laser head, and a conductive tip is fitted to the end of the welding torch. Two conductive contacts are symmetrically arranged on both sides of the laser head. The end faces of the conductive contacts are used to press against the upper surface of the base material on both sides of the narrow gap bevel. The pulse power supply is connected to two conductive contacts via a cable and is used to output pulse current to a closed current loop consisting of the conductive contacts, the base material, and the molten pool. The pulse power supply is configured to output AC pulse current, which causes the self-induced magnetic field generated in the current closed loop to drive the electric arc to deflect periodically and alternately along the width direction of the narrow gap bevel.