Composite aluminum foil, electrode and battery

By introducing an aluminum-carbon transition layer into the composite aluminum foil, the adhesion between the carbon layer and the aluminum layer is improved, the problem of poor adhesion of the existing composite aluminum foil carbon layer is solved, and the conductivity and cycling performance of the battery are improved.

CN222029115UActive Publication Date: 2024-11-19BYD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323577168.2
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2024-11-19
Estimated Expiration
2033-12-26

AI Technical Summary

Technical Problem

The carbon layer of the existing composite aluminum foil has poor adhesion and is easy to peel off, which affects the conductivity and cycling performance of lithium-ion batteries.

Method used

A composite aluminum foil structure consisting of a first aluminum layer, a base layer, a second aluminum layer and a second carbon layer are adopted, wherein a first aluminum carbon transition layer is arranged between the first aluminum layer and the first carbon layer, and a second aluminum layer is A second aluminum-carbon transition layer is provided between the second carbon layer, and the adhesion between the carbon layer and the aluminum layer is improved by adjusting the carbon content and thickness of the transition layer.

Benefits of technology

It effectively improves the adhesion between the carbon layer and the aluminum layer, prevents the carbon layer from falling off during use, and improves the conductivity of the composite aluminum foil and the cycling performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222029115U_ABST
    Figure CN222029115U_ABST
Patent Text Reader

Abstract

The composite aluminum foil comprises a first carbon layer, a first aluminum layer, a base material layer, a second aluminum layer and a second carbon layer which are sequentially stacked, a first aluminum-carbon transition layer is arranged between the first carbon layer and the first aluminum layer, and a second aluminum-carbon transition layer is arranged between the second aluminum layer and the second carbon layer. In the technical scheme, the first aluminum-carbon transition layer and the second aluminum-carbon transition layer comprise aluminum atoms and carbon atoms, the average atomic diameter of the first aluminum-carbon transition layer is between the average atomic diameter of the first aluminum layer and the average atomic diameter of the second aluminum layer, and the average atomic diameter of the second aluminum-carbon transition layer is between the average atomic diameter of the second aluminum layer and the average atomic diameter of the second carbon layer. Therefore, the first aluminum-carbon transition layer is smaller in average molecular diameter difference and higher in adhesive force for the first aluminum layer and the second aluminum layer, and the second aluminum-carbon transition layer is smaller in average atomic diameter difference and higher in adhesive force for the second aluminum layer and the second aluminum layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of aluminum foil, and in particular to a composite aluminum foil, an electrode and a battery. Background Art

[0002] The conductivity of the plate in lithium-ion batteries is an important factor affecting the performance of the plate. Good conductivity can reduce the internal resistance of the battery and improve the cycle performance. At present, the current collector of lithium-ion batteries is generally aluminum foil. However, since aluminum easily reacts with oxygen in the air, an oxide film is formed on the surface of the aluminum foil after the reaction, which will greatly hinder the transfer of electrons in the aluminum foil, thereby reducing the conductivity of the aluminum foil.

[0003] Therefore, in order to solve the above problems, a conductive carbon layer is usually coated on the surface of the aluminum foil to protect the aluminum foil from oxidation. However, due to the difference between the atomic structure of the aluminum foil and the atomic structure of the carbon layer, it is not easy for carbon atoms to adhere to the surface of the aluminum foil. Therefore, the composite aluminum foil in the related art has the problem of poor adhesion of the carbon layer and easy peeling. Utility Model Content

[0004] The purpose of the present application is to provide a composite aluminum foil, an electrode and a battery, aiming to solve the problem that the carbon layer of the existing composite aluminum foil has poor adhesion and is easy to fall off.

[0005] To achieve the purpose of the present application, in a first aspect, the present application provides a composite aluminum foil, comprising a first carbon layer, a first aluminum layer, a substrate layer, a second aluminum layer, and a second carbon layer stacked in sequence;

[0006] Wherein, a first aluminum-carbon transition layer is arranged between the first carbon layer and the first aluminum layer, and a second aluminum-carbon transition layer is arranged between the second aluminum layer and the second carbon layer.

[0007] In a possible implementation, along the direction from the first aluminum layer to the first carbon layer, the carbon content of the first aluminum-carbon transition layer varies between a first preset value and a second preset value;

[0008] Along the direction from the second aluminum layer to the second carbon layer, the carbon content of the second aluminum-carbon transition layer varies between a first preset value and a second preset value;

[0009] The first preset value is smaller than the second preset value.

[0010] In a possible implementation manner, the first preset value is less than 50%, and the second preset value is greater than 50%.

[0011] In a possible implementation manner, the first preset value is 10-30%, and the second preset value is 70-90%.

[0012] In a possible implementation, the carbon content of the first aluminum-carbon transition layer gradually increases from the first preset value to the second preset value;

[0013] The carbon content of the second aluminum-carbon transition layer gradually increases from the first preset value to the second preset value.

[0014] In a possible implementation, the thickness of the first aluminum-carbon transition layer and the second aluminum-carbon transition layer are each independently A, 0.01 μm≤A≤0.2 μm.

[0015] In a possible implementation manner, the substrate layer is made of a polymer material or aluminum.

[0016] In a possible implementation, the substrate layer is made of aluminum, and the thickness of the first aluminum layer and the second aluminum layer along the direction from the first carbon layer to the second carbon layer are each independently B, and 0.01 μm≤B≤1 μm.

[0017] In a possible implementation, the substrate layer is made of a polymer material, and the thickness of the first aluminum layer and the second aluminum layer along the direction from the first carbon layer to the second carbon layer are each independently C, and 0.5 μm≤C≤6 μm.

[0018] In a possible implementation manner, the thickness of the first carbon layer and the second carbon layer along a direction from the first carbon layer to the second carbon layer are each independently D, and 0.01 μm≤D≤0.2 μm.

[0019] In a second aspect, the present application further provides an electrode, the electrode comprising the composite aluminum foil, the composite aluminum foil comprising a first carbon layer, a first aluminum layer, a substrate layer, a second aluminum layer, and a second carbon layer stacked in sequence;

[0020] Wherein, a first aluminum-carbon transition layer is arranged between the first carbon layer and the first aluminum layer, and a second aluminum-carbon transition layer is arranged between the second aluminum layer and the second carbon layer.

[0021] In a third aspect, the present application further provides a battery, the battery comprising the electrode, the electrode comprising the composite aluminum foil, the composite aluminum foil comprising a first carbon layer, a first aluminum layer, a substrate layer, a second aluminum layer, and a second carbon layer stacked in sequence;

[0022] Wherein, a first aluminum-carbon transition layer is arranged between the first carbon layer and the first aluminum layer, and a second aluminum-carbon transition layer is arranged between the second aluminum layer and the second carbon layer.

[0023] In the technical solution of the present application, a first aluminum-carbon transition layer is provided between the first aluminum layer and the first carbon layer, and a second aluminum-carbon transition layer is provided between the second aluminum layer and the second carbon layer. The first aluminum-carbon transition layer and the second aluminum-carbon transition layer include aluminum atoms and carbon atoms. The average atomic diameter of the first aluminum-carbon transition layer is between the average atomic diameters of the first carbon layer and the first aluminum layer, and the average atomic diameter of the second aluminum-carbon transition layer is between the second aluminum layer and the second carbon layer. Therefore, compared with the direct combination of the first aluminum layer and the first carbon layer, and the second aluminum layer and the second carbon layer, the first aluminum-carbon transition layer has a smaller difference in average molecular diameters between the first carbon layer and the first aluminum layer, and has a stronger adhesion. The second aluminum-carbon transition layer has a smaller difference in average atomic diameters between the second carbon layer and the second aluminum layer, and has a stronger adhesion. The first aluminum-carbon transition layer is used as the transition layer between the first aluminum layer and the first carbon layer, and the second aluminum-carbon transition layer is used as the transition layer between the second carbon layer and the second aluminum layer, which can effectively improve the adhesion of the first aluminum layer to the first carbon layer and the second aluminum layer to the second carbon layer, and prevent the carbon layer from falling off from the surface of the composite aluminum foil during use. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0025] Figure 1 This is a schematic structural diagram of an embodiment of the composite aluminum foil provided in this application.

[0026] Description of reference numerals:

[0027] 10 composite aluminum foil; 1 first carbon layer; 2 first aluminum-carbon transition layer; 3 first aluminum layer; 4 substrate layer; 5 second aluminum layer; 6 second aluminum-carbon transition layer; 7 second carbon layer. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0029] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there can be a central component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there can be a central component at the same time.

[0030] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in this application and in the specification are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more of the related listed items.

[0031] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0032] The existing composite aluminum foil has poor adhesion to the carbon layer. To solve the above problem, please refer to Figure 1 , the present application proposes a battery, the battery comprising an electrode.

[0033] The electrode includes a composite aluminum foil 10 and an active material attached to the composite aluminum foil 10, wherein the composite aluminum foil 10 includes a first carbon layer 1, a first aluminum layer 3, a substrate layer 4, a second aluminum layer 5, and a second carbon layer 7 stacked in sequence, a first aluminum-carbon transition layer 2 is arranged between the first carbon layer 1 and the first aluminum layer 3, and a second aluminum-carbon transition layer 6 is arranged between the second aluminum layer 5 and the second carbon layer 7.

[0034] In the technical solution of the present application, a first aluminum-carbon transition layer 2 is provided between the first aluminum layer 3 and the first carbon layer 1, and a second aluminum-carbon transition layer 6 is provided between the second aluminum layer 5 and the second carbon layer 7. The first aluminum-carbon transition layer 2 and the second aluminum-carbon transition layer 6 include aluminum atoms and carbon atoms. The average atomic diameter of the first aluminum-carbon transition layer 2 is between the average atomic diameters of the first aluminum layer 3 and the first carbon layer 1, and the average atomic diameter of the second aluminum-carbon transition layer 6 is between the second aluminum layer 5 and the second carbon layer 7. Therefore, compared with the direct combination of the first aluminum layer 3 and the first carbon layer 1, the second aluminum layer 5 and the second carbon layer 7, the first aluminum-carbon transition layer 2 has a smaller difference in average molecular diameters with respect to the first aluminum layer 3 and the first carbon layer 1, and has a stronger adhesion, and the second aluminum-carbon transition layer 6 has a smaller difference in average atomic diameters with respect to the second aluminum layer 5 and the second carbon layer 7, and has a stronger adhesion. Using the first aluminum-carbon transition layer 2 as the transition layer between the first aluminum layer 3 and the first carbon layer 1, and using the second aluminum-carbon transition layer 6 as the transition layer between the second carbon layer 7 and the second aluminum layer 5 can effectively improve the adhesion of the first aluminum layer 3 to the first carbon layer 1 and the second aluminum layer 5 to the second carbon layer 7, and prevent the first carbon layer 1 and the second carbon layer 7 from falling off from the surface of the composite aluminum foil 10 during use.

[0035] The aluminum-carbon content in the first aluminum-carbon transition layer 2 and the second aluminum-carbon transition layer 6 can be fixed or can change with the change of thickness, and the present application does not impose any restrictions on this. It can be understood that for the first aluminum-carbon transition layer 2 and the second aluminum-carbon transition layer 6, the higher the carbon content of the first aluminum-carbon transition layer 2 and the second aluminum-carbon transition layer 6, the smaller the difference in atomic diameter between the first aluminum-carbon transition layer 2 and the first carbon layer 1, the second aluminum-carbon transition layer 6 and the second carbon layer 7, and the stronger the adhesion of the first aluminum-carbon transition layer 2 to the first carbon layer 1 and the second aluminum-carbon transition layer 6 to the second carbon layer 7, and the lower the carbon content of the first aluminum-carbon transition layer 2 and the second aluminum-carbon transition layer 6, the smaller the difference in diameter between the first aluminum-carbon transition layer 2 and the first aluminum layer 3, the second aluminum-carbon transition layer 6 and the second aluminum layer 5, and the stronger the adhesion to the aluminum layer.

[0036] Based on this, in one possible implementation of the present application, the carbon content in the first aluminum-carbon transition layer 2 and the second aluminum-carbon transition layer 6 can vary with thickness. Specifically, along the direction from the first aluminum layer 3 to the first carbon layer 1, the carbon content of the first aluminum-carbon transition layer 2 varies between a first preset value and a second preset value; along the direction from the second aluminum layer 5 to the second carbon layer 7, the carbon content of the second aluminum-carbon transition layer 6 varies between a first preset value and a second preset value, and the first preset value is less than the second preset value.

[0037] It should be explained that in the present embodiment, the carbon content in the first aluminum-carbon transition layer 2 refers to the percentage of the mass of carbon atoms in the unit thickness of the first aluminum-carbon transition layer 2 to the total atomic mass of the first aluminum-carbon transition layer 2 of the unit thickness. The unit thickness can be one-tenth of the total thickness of the first aluminum-carbon transition layer 2, or one-twentieth of the total thickness of the first aluminum-carbon transition layer 2, and the present application does not impose any restrictions on this. The carbon content of the second aluminum-carbon transition layer 6 refers to the percentage of the total atomic mass of the second aluminum-carbon transition layer 6 in the unit thickness of the second aluminum-carbon transition layer 6. The unit thickness can be one-tenth of the total thickness of the second aluminum-carbon transition layer 6, or one-twentieth of the total thickness of the second aluminum-carbon transition layer 6, and the present application does not impose any restrictions on this. With such a configuration, the carbon content of the first aluminum-carbon transition layer 2 close to the first carbon layer 1 can be higher than the carbon content close to the first aluminum layer 3, thereby improving the adhesion of the first aluminum-carbon transition layer 2 to the first aluminum layer 3 and the first carbon layer 1. Similarly, in this way, the carbon content of the second aluminum-carbon transition layer 6 on the side close to the second carbon layer 7 can be higher than the carbon content of the second aluminum-carbon transition layer 6 on the side close to the second aluminum layer 5, thereby improving the adhesion of the second aluminum-carbon transition layer 6 to the second aluminum layer 5 and the second carbon layer 7.

[0038] In another possible implementation of the present application, the first preset value is less than 50%, so that the aluminum content of the first aluminum-carbon transition layer 2 close to the first aluminum layer 3 can be ensured to be greater than the carbon content, so as to further reduce the difference in atomic diameter between the first aluminum-carbon transition layer 2 and the first aluminum layer 3, and improve the bonding ability between the first aluminum-carbon transition layer 2 and the first aluminum layer 3. The second preset value is greater than 50%, so that the carbon content of the first aluminum-carbon transition layer 2 close to the first carbon layer 1 is greater than the aluminum content, thereby further reducing the difference in atomic diameter between the first aluminum-carbon transition layer 2 and the first carbon layer 1, and improving the bonding ability between the first aluminum-carbon transition layer 2 and the first carbon layer 1. The same is true for the second aluminum-carbon transition layer 6. The first preset value is less than 50%, so that the aluminum content of the second aluminum-carbon transition layer 6 close to the second aluminum layer 5 is greater than the carbon content, thereby reducing the difference in average atomic diameter between the second aluminum-carbon transition layer 6 and the second aluminum layer 5, and improving the bonding ability between the second aluminum-carbon transition layer 6 and the second aluminum layer 5. The second preset value is greater than 50%, which can ensure that the carbon content of the second aluminum-carbon transition layer 6 close to the second carbon layer 7 is greater than the aluminum content, reduce the difference in atomic diameter between the second aluminum-carbon transition layer 6 and the second carbon layer 7, and improve the bonding ability of the second aluminum-carbon transition layer 6 and the second carbon layer 7. Further, when the first preset value is between 10% and 30% and the second preset value is between 70% and 90%, the first aluminum-carbon transition layer 2 has a better adhesion effect on the first aluminum layer 3 and the first carbon layer 1, and the second aluminum-carbon transition layer 6 has a better adhesion effect on the second aluminum layer 5 and the second carbon layer 7.

[0039] In the present application, in order to further improve the conductive effect and bonding strength of the composite aluminum foil 10, in one possible implementation mode of the present application, the thickness of the first aluminum-carbon transition layer 2 and the second aluminum-carbon transition layer 6 are each independently A, 0.01μm≤A≤0.2μm. In this way, while reducing the thickness of the composite aluminum foil 10 to improve the conductive effect, the adhesion ability of the first aluminum layer 3 and the first carbon layer 1, and the second aluminum-carbon transition layer 6 to the second aluminum layer 5 and the second carbon layer 7 is further improved.

[0040] The substrate layer 4 is the middle layer of the composite aluminum foil 10, and its function is to provide a carrier for the deposition of the first aluminum layer 3, the second aluminum layer 5, the first carbon layer 1 and the second carbon layer 7. The material of the substrate layer 4 can be a polymer material or aluminum. The present application does not limit this. In one embodiment of the present application, the material of the substrate layer 4 is a polymer material. Specifically, the substrate layer 4 is a resin. Compared with aluminum foil, the resin is lighter and has better toughness. In this way, the mass of the composite aluminum foil 10 after manufacture can be effectively reduced and the toughness of the composite aluminum foil 10 can be improved. When the material of the substrate layer 4 is a resin, polypropylene (PP) and polyethylene terephthalate plastics (PET) are preferred in the resin, which can effectively improve the toughness of the composite aluminum foil 10 after manufacture.

[0041] The first aluminum layer 3 and the second aluminum layer 5 are arranged on the substrate layer 4. The first aluminum layer 3 and the second aluminum layer 5 can be bonded to the substrate layer 4 by conductive paste, and can also be deposited on the substrate layer 4 by vacuum coating. The present application does not limit this. In one embodiment of the present application, the first aluminum layer 3 and the second aluminum layer 5 are deposited on the substrate layer 4 by vacuum coating. Vacuum coating can eliminate the need for conductive paste and effectively reduce the thickness of the composite aluminum foil 10 after forming.

[0042] The materials used for the substrate layer 4 are different, and the thicknesses of the first aluminum layer 3 and the second aluminum layer 5 are also different. When the substrate layer 4 is made of aluminum, the thicknesses of the first aluminum layer 3 and the second aluminum layer 5 along the direction from the first carbon layer 1 to the second carbon layer 7 are independently B, 0.01μm≤B≤1μm; when the substrate layer 4 is made of polymer material, the thicknesses of the first aluminum layer 3 and the second aluminum layer 5 along the direction from the first carbon layer 1 to the second carbon layer 7 are independently C, 0.5μm≤C≤6μm. When the thicknesses of the first aluminum layer 3 and the second aluminum layer 5 are within the above range, the adhesion of the first carbon layer 1 and the second carbon layer 7 to the active material can be further improved and the thickness of the composite aluminum foil 10 can be ensured not to be too thick.

[0043] The first carbon layer 1 is arranged on the side of the first aluminum layer 3 away from the substrate layer 4. The first carbon layer 1 can isolate the first aluminum layer 3 from the outside, prevent the first aluminum layer 3 from reacting with oxygen in the air or other chemical substances in the electrode, thereby achieving the purpose of protecting the first aluminum layer 3. At the same time, the first carbon layer 1 can also improve the adhesion of the current collector made of the composite aluminum foil 10 to the active material in the battery, thereby improving the conductivity of the composite aluminum foil 10. The second carbon layer 7 is arranged on the side of the second aluminum layer 5 away from the substrate layer 4. The second carbon layer 7 can isolate the second aluminum layer 5 from the outside, prevent the second aluminum layer 5 from reacting with oxygen in the air or other chemical substances in the electrode, thereby achieving the purpose of protecting the second aluminum layer 5. At the same time, the second carbon layer 7 can also improve the adhesion of the current collector made of the composite aluminum foil 10 to the active material in the battery, thereby improving the conductivity of the composite aluminum foil 10. When the thickness D of the first carbon layer 1 and the second carbon layer 7 along the direction from the first carbon layer 1 to the second carbon layer 7 is independently set between 0.01 μm≤D≤0.2 μm, it can ensure the adhesion ability of the first carbon layer 1 and the second carbon layer 7 to the active material and ensure that the thickness of the composite aluminum foil 10 is not too thick.

[0044] The manufacturing process of the composite aluminum foil with this structure is as follows:

[0045] S10, pre-treating the substrate layer.

[0046] The material of the substrate layer can be aluminum or resin, and the pretreatment includes ion cleaning, corona or irradiation treatment of the substrate layer, so as to clean the impurities on the surface of the substrate layer and improve the surface roughness of the substrate layer, thereby improving the bonding strength between the substrate layer and other deposited layers.

[0047] S20, depositing a first aluminum layer and a second aluminum layer on the substrate layer.

[0048] The first aluminum layer and the second aluminum layer are usually deposited on the surface of the substrate layer by vacuum coating or vapor deposition. The present application prefers vacuum coating. Specifically, when the first aluminum layer and the second aluminum layer are deposited by vacuum coating, the first aluminum layer and the second aluminum layer use Al targets, set the bias voltage to -200 to -400V, the duty cycle to 90%, and the Al target current to 20-30A. When the thickness of the plated film layer is 10-100nm, stop the coating and ion bombard for 5-10min, then set the DC mode (no bias), the Al target current to 5-10A, and continue coating to the target thickness.

[0049] S30, depositing a first aluminum-carbon transition layer on the first aluminum layer, and depositing a second aluminum-carbon transition layer on the second aluminum layer.

[0050] The first aluminum layer is coated on the first aluminum-carbon transition layer, and the second aluminum layer is coated on the second aluminum-carbon transition layer by vacuum coating. Specifically, the first aluminum-carbon transition layer and the second aluminum-carbon transition layer are coated together using an Al target and a C target. For example, the process parameters are set to a DC mode (no bias), the C target current is increased from 5A to 30A, and the Al target current is reduced from 20A to 5A. The total thickness of the aluminum-carbon transition layer is controlled by adjusting the current change time.

[0051] S40, depositing a first carbon layer on the first aluminum-carbon transition layer, and depositing a second carbon layer on the second aluminum-carbon transition layer.

[0052] The first carbon layer is coated on the first aluminum-carbon transition layer by vacuum coating, and the second carbon layer is coated on the second aluminum-carbon transition layer. The first carbon layer and the second carbon layer are coated by C target, and the DC mode (no bias) is set. The C target current is set to 30A. The target thickness of the carbon layer is obtained by controlling the coating time. After the coating is completed, the composite aluminum foil is rolled up.

[0053] The technical solution of the present application is described in detail below through specific embodiments.

[0054] Example 1

[0055] (1) Pretreatment of the substrate layer: The substrate layer is made of PET resin with a thickness of 4.5 μm. The vacuum is drawn to 1×10-3Pa, and the PET resin film is ion cleaned for 5 minutes;

[0056] (2) Deposition of the first aluminum layer and the second aluminum layer: using an Al target, bias voltage -200 V, duty cycle 90%, Al target current 25 A, when the film thickness of the first aluminum layer and the second aluminum layer on both sides of the substrate layer reaches 20 nm, stop the film coating and ion bombardment for 5-10 min; then set the DC mode (no bias), Al target current 10 A, and plate the first aluminum layer and the second aluminum layer to a thickness of 0.9 um;

[0057] (3) Deposition of the first aluminum-carbon transition layer and the second aluminum-carbon transition layer: Al target and C target are used to jointly plate the first aluminum-carbon transition layer and the second aluminum-carbon transition layer. Specifically, the DC mode (no bias) is set, the C target current is increased from 5A to 30A, and the Al target current is reduced from 20A to 5A. Correspondingly, the carbon content increases from 20% to 85%. A first aluminum-carbon transition layer with a thickness of 50nm is plated on one side of the first aluminum layer, and a second aluminum-carbon transition layer with a thickness of 50nm is plated on one side of the second aluminum layer, and the carbon content increases from 20% to 85%.

[0058] (4) Deposition of the first carbon layer and the second carbon layer: A C target is selected to vacuum-coat the carbon layer. Specifically, a DC mode (no bias) is set, and the C target current is set to 30 A. A first carbon layer with a thickness of 20 nm is deposited on one side of the first aluminum-carbon transition layer, and a second carbon layer with a thickness of 20 nm is deposited on one side of the second aluminum-carbon transition layer, to finally form a composite aluminum foil.

[0059] Example 2

[0060] (1) Pretreatment of the substrate layer: The substrate layer is made of Al with a thickness of 8 μm. The Al foil is vacuumed to 1×10-3Pa and ion-cleaned for 5 min.

[0061] (2) Deposition of the first aluminum layer and the second aluminum layer: using an Al target, bias voltage -200 V, duty cycle 90%, Al target current 25 A, when the film thickness of the first aluminum layer and the second aluminum layer on both sides of the substrate layer reaches 20 nm, stop the film coating and ion bombardment for 5-10 min; then set the DC mode (no bias), Al target current 10 A, and plate the first aluminum layer and the second aluminum layer to a thickness of 0.9 um;

[0062] (3) Deposition of the first aluminum-carbon transition layer and the second aluminum-carbon transition layer: Al target and C target are used to jointly plate the first aluminum-carbon transition layer and the second aluminum-carbon transition layer. Specifically, the DC mode (no bias) is set, the C target current is increased from 5A to 30A, and the Al target current is reduced from 20A to 5A. Correspondingly, the carbon content increases from 20% to 85%. A first aluminum-carbon transition layer with a thickness of 50nm is plated on one side of the first aluminum layer, and a second aluminum-carbon transition layer with a thickness of 50nm is plated on one side of the second aluminum layer, and the carbon content increases from 20% to 85%.

[0063] (4) Deposition of the first carbon layer and the second carbon layer: A C target is selected to vacuum-coat the carbon layer. Specifically, a DC mode (no bias) is set, and the C target current is set to 30 A. A first carbon layer with a thickness of 20 nm is deposited on one side of the first aluminum-carbon transition layer, and a second carbon layer with a thickness of 20 nm is deposited on one side of the second aluminum-carbon transition layer, to finally form a composite aluminum foil.

[0064] Example 3

[0065] (1) Pretreatment of the substrate layer: The substrate layer is made of PET resin with a thickness of 4.5 μm. The vacuum is drawn to 1×10-3Pa, and the PET resin film is ion cleaned for 5 minutes;

[0066] (2) Deposition of the first aluminum layer and the second aluminum layer: using an Al target, bias voltage -200 V, duty cycle 90%, Al target current 25 A, when the film thickness of the first aluminum layer and the second aluminum layer on both sides of the substrate layer reaches 20 nm, stop the film coating and ion bombardment for 5-10 min; then set the DC mode (no bias), Al target current 10 A, and plate the first aluminum layer and the second aluminum layer to a thickness of 0.9 um;

[0067] (3) Deposition of the first aluminum-carbon transition layer and the second aluminum-carbon transition layer: Al target and C target are selected to jointly plate the first aluminum-carbon transition layer and the second aluminum-carbon transition layer. Specifically, the DC mode (no bias) is set, the C target current is increased from 10A to 20A, and the Al target current is reduced from 20A to 5A. Correspondingly, the carbon content increases from 30% to 80%. A first aluminum-carbon transition layer with a thickness of 50nm is plated on one side of the first aluminum layer, and a second aluminum-carbon transition layer with a thickness of 50nm is plated on one side of the second aluminum layer, and the carbon content increases from 30% to 80%.

[0068] (4) Deposition of the first carbon layer and the second carbon layer: A C target is selected to vacuum-coat the carbon layer. Specifically, a DC mode (no bias) is set, and the C target current is set to 30 A. A first carbon layer with a thickness of 20 nm is deposited on one side of the first aluminum-carbon transition layer, and a second carbon layer with a thickness of 20 nm is deposited on one side of the second aluminum-carbon transition layer, to finally form a composite aluminum foil.

[0069] The carbon layer peeling force and the discharge specific capacity of the VDA structure ternary battery after being made of the composite aluminum foil prepared in Example 1, Example 2, and Example 3 and the homemade single-sided carbon-coated composite aluminum foil with a coating thickness of 0.5 μm were tested. The test method refers to: GB / T2792-2014 Test method for peeling strength of adhesive tape, and the test results are as follows:

[0070]

[0071] Discharge specific capacity test method: At room temperature (25°C), charge the battery to full capacity at 1C constant current, leave it in the test environment for 1 hour, discharge it to the cut-off voltage (3.2V) at 1C constant current, and record the released capacity. Repeat the test three times in a row to get the average value to improve accuracy. Divide the capacity by the weight of the positive electrode material to get the discharge specific capacity result.

[0072] It can be seen that the composite aluminum foil of the present application has better bonding between the carbon layer and the aluminum layer, and after being made into a battery, the electrical performance of the battery is better.

[0073] In the description of the embodiments of the present application, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" are based on the orientation or positional relationship described in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.

[0074] What is disclosed above is only a preferred embodiment of the present application, and it certainly cannot be used to limit the scope of rights of the present application. Ordinary technicians in this field can understand that all or part of the processes of implementing the above embodiment and equivalent changes made according to the claims of the present application are still within the scope covered by the present application.

Claims

1. A composite aluminum foil, characterized in that: It includes a first carbon layer, a first aluminum layer, a substrate layer, a second aluminum layer, and a second carbon layer stacked in sequence; Wherein, a first aluminum-carbon transition layer is arranged between the first carbon layer and the first aluminum layer, and a second aluminum-carbon transition layer is arranged between the second aluminum layer and the second carbon layer.

2. The composite aluminum foil according to claim 1, characterized in that Along the direction from the first aluminum layer to the first carbon layer, the carbon content of the first aluminum-carbon transition layer varies between a first preset value and a second preset value; Along the direction from the second aluminum layer to the second carbon layer, the carbon content of the second aluminum-carbon transition layer varies between a first preset value and a second preset value; The first preset value is smaller than the second preset value.

3. The composite aluminum foil according to claim 2, characterized in that: The first preset value is less than 50%, and the second preset value is greater than 50%.

4. The composite aluminum foil according to claim 2, characterized in that: The first preset value is 10-30%, and the second preset value is 70-90%.

5. The composite aluminum foil according to claim 2, characterized in that: The carbon content of the first aluminum-carbon transition layer gradually increases from the first preset value to the second preset value; The carbon content of the second aluminum-carbon transition layer gradually increases from the first preset value to the second preset value.

6. The composite aluminum foil according to claim 1, characterized in that: The thickness of the first aluminum-carbon transition layer and the second aluminum-carbon transition layer are each independently A, 0.01 μm≤A≤0.2 μm.

7. The composite aluminum foil according to claim 1, characterized in that: The substrate layer is made of a polymer material or aluminum.

8. The composite aluminum foil according to claim 7, characterized in that: The substrate layer is made of aluminum, and the thickness of the first aluminum layer and the second aluminum layer along the direction from the first carbon layer to the second carbon layer are each independently B, and 0.01 μm≤B≤1 μm.

9. The composite aluminum foil according to claim 7, characterized in that: The substrate layer is made of polymer material, and the thickness of the first aluminum layer and the second aluminum layer along the direction from the first carbon layer to the second carbon layer are independently C, 0.5μm≤C≤6μm.

10. The composite aluminum foil according to claim 1, characterized in that: The thickness of the first carbon layer and the second carbon layer along a direction from the first carbon layer to the second carbon layer is independently D, and 0.01 μm≤D≤0.2 μm.

11. An electrode, characterized in that: Comprising the composite aluminum foil as described in any one of claims 1 to 10.