Composite loose nanofiltration membrane
By using a composite structure of a non-woven fabric layer, aramid-based film and sulfonated polyphenylsulfone layer in the nanofiltration membrane, and preparing by phase transformation process, the existing nanofiltration membrane is solved when separating dyes and inorganic salts in the printing and dyeing wastewater. The performance reduction problem achieves efficient separation effect and maintains long-term stability.
Patent Information
- Application Number
- CN202420595107.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2034-03-26
AI Technical Summary
The existing nanofiltration membranes cannot effectively separate dyes and inorganic salts in the printing and dyeing wastewater, and their performance is significantly reduced after acid-base cleaning.
A composite loose nanofiltration membrane structure, including a nonwoven fabric layer, aramid-based membrane and sulfonated polyphenylsulfone layer, is prepared by a phase transformation process to form a membrane structure with moderate pore size to achieve efficient separation of dyes and inorganic salts.
The dye retention rate is as high as 99%, the sodium sulfate retention rate is as low as 20%, and the performance remains good after acid-base cleaning, making it suitable for industrial applications.
Smart Images

Figure CN222056972U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of nanofiltration membranes, in particular to the structural improvement of a composite loose nanofiltration membrane. Background Art
[0002] The textile industry is one of the pillar industries that my country focuses on developing. In the printing and dyeing process, 100 to 200 tons of water are consumed for processing 1 ton of textiles, of which 80% to 90% will be discharged as wastewater, which will cause serious damage to my country's ecological environment. How to treat printing and dyeing wastewater to meet the discharge standards or reuse has become a current research hotspot. However, the content of inorganic salts in printing and dyeing wastewater is high, and excessive osmotic pressure will cause various strains to dehydrate and die, greatly reducing the effect of biochemical treatment.
[0003] Nanofiltration (NF) is a pressure-driven membrane separation technology between ultrafiltration and reverse osmosis. Its typical membrane pore size is about 1 nm, and the molecular weight cutoff (MWCO) is 200-2000 Da. It is favored for its easy operation, low energy consumption, pollution-free and high efficiency, and is widely used in water treatment, food and medicine. However, the current mainstream nanofiltration membrane products cannot be used for the separation of inorganic salts and dyes. This is mainly because these products are prepared by interfacial polymerization and have small separation pores, which intercept inorganic salts while intercepting dyes. Some scholars have prepared loose nanofiltration membranes by controlling the interfacial polymerization process or using post-treatment methods. Although this type of product has a good separation effect on dyes and inorganic salts in the short term, this type of membrane is obtained by sacrificing the low cross-linking degree of polypiperazineamide. The performance is severely degraded after acid and alkali cleaning during actual use. Utility Model Content
[0004] In view of the above problems, the utility model provides a composite loose nanofiltration membrane for separating dyes and inorganic salts in printing and dyeing wastewater, with a dye retention rate of up to 99% and a sodium sulfate retention rate as low as 20%, thus having a good separation effect.
[0005] The technical solution of the utility model is:
[0006] The composite loose nanofiltration membrane comprises:
[0007] The non-woven fabric layer serves as the support material for the nanofiltration membrane and blocks the passage of fine particles;
[0008] Aramid-based membrane, with a pore size of 10-40 nm, is used as the base membrane for nanofiltration membranes;
[0009] The sulfonated polyphenylsulfone layer, with a pore size of 2~5nm, serves as the separation layer of the nanofiltration membrane.
[0010] Specifically, the aramid content in the middle position of the aramid base film is 6-25%.
[0011] Specifically, the sulfonation degree of the sulfonated polyphenylene sulfone layer is 10-80%.
[0012] Specifically, the pore size of the non-woven fabric layer is 100-300 nm.
[0013] Specifically, the thickness of the non-woven fabric layer is 70-150 um.
[0014] Specifically, the thickness of the aramid base film is 5-50 um.
[0015] Specifically, the thickness of the sulfonated polyphenylene sulfone layer is 1-20 um.
[0016] Specifically, the thickness of the non-woven fabric layer is greater than the thickness of the aramid-based film and the thickness of the sulfonated polyphenylene sulfone layer.
[0017] The utility model first prepares an aramid ultrafiltration base membrane (or composite nanofiltration membrane support layer A) with a pore size of about 10-40nm; then a sulfonated polysulfone casting liquid is coated on its surface, and a porous cortex (or primary composite nanofiltration membrane B) is generated through a phase transition process with a pore size range of 2-5nm. Combined with the ultrafine pore size of the cortex and the charged repulsive effect of the sulfonic acid group, the interception scale of the composite membrane is at the nanofiltration level, and it has a looser structure than the commercial polypiperazineamide system nanofiltration membrane, and can be used for the separation of dyes and inorganic salts. The composite loose nanofiltration membrane prepared by the two phase transition methods has a good separation effect on dyes / inorganic salts, and the preparation process is simple, which is suitable for industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the process flow chart of the utility model membrane
[0019] Figure 2 This is a cross-sectional structure diagram of a composite loose nanofiltration membrane. DETAILED DESCRIPTION
[0020] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0021] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0022] The present invention is described below with reference to Figures 1 and 2;
[0023] The composite loose nanofiltration membrane comprises:
[0024] The non-woven fabric layer serves as a supporting material for the nanofiltration membrane and prevents fine particles from passing through; the pore size of the non-woven fabric layer is 100-300nm; the thickness of the non-woven fabric layer is 70-150um.
[0025] Aramid base membrane (or composite nanofiltration membrane support layer A) has a pore size of 10~40nm and is used as the base membrane of the nanofiltration membrane; the aramid content in the middle position of the aramid base membrane is 6~25%. The thickness of the aramid base membrane is 5-50um.
[0026] The sulfonated polyphenylsulfone layer (or primary composite nanofiltration membrane B) has a pore size of 2-5 nm and serves as the separation layer of the nanofiltration membrane.
[0027] The sulfonation degree of the sulfonated polyphenylene sulfone layer is 10-80%. The thickness of the sulfonated polyphenylene sulfone layer is 1-20 um.
[0028] In this case, the thickness of the nonwoven fabric layer is greater than the thickness of the aramid base film and the thickness of the sulfonated polyphenylene sulfone layer.
[0029] The following is an introduction to the preparation method of the composite loose nanofiltration membrane in this case:
[0030] The steps include:
[0031] Step 1: Preparation of composite nanofiltration membrane support layer A with ultrafiltration scale pore size structure
[0032] A meta-aramid casting liquid is prepared and degassed; the degassed meta-aramid casting liquid is scraped onto the surface of the non-woven fabric, and then put into a meta-aramid non-solvent system for phase transformation to prepare a meta-aramid ultrafiltration membrane; the ultrafiltration membrane is fully washed to obtain a composite nanofiltration membrane support layer A;
[0033] Specifically, the meta-aramid content in the meta-aramid casting solution is 6-25%, the phase transition additive is lithium chloride or calcium chloride, the content is 3%-15%, and the remaining components of the casting solution are aprotic solvents, mainly including one or more of DMAc, DMF, and DMSO;
[0034] Specifically, the non-solvent system includes the following combinations:
[0035] 1) Water, methanol, ethanol;
[0036] 2) A mixed solution of water and methanol or ethanol;
[0037] 3) Mixed solution of water and glycerol.
[0038] Specifically, the solution used to clean the ultrafiltration membrane is mainly pure water, and the main purpose is to remove the residual organic solvent and phase transition additive in the support layer;
[0039] In this case, aramid is used as the base membrane instead of the common polysulfone material, mainly to avoid the solvent in the mixed solution in step 2 from damaging the base membrane structure and to ensure the integrity of the base membrane.
[0040] Step 2: preparing a mixed solution of the sulfonated polysulfone material and the aprotic solvent, and performing degassing;
[0041] Take a quantitative aprotic solvent, add sulfonated polysulfone in proportion and stir; after stirring evenly, degas the solution, and after degassing, let it stand for use;
[0042] Specifically, the sulfonated polysulfone material includes one or more of sulfonated polysulfone, sulfonated polyethersulfone, and sulfonated polyphenylsulfone, with a sulfonation degree of 10-80% and a content of 1.0-10.0% in the mixed solution;
[0043] Specifically, the aprotic solvent includes one or more of DMAc, DMF, and DMSO.
[0044] Step 3, fully apply the mixed solution on the surface of the support layer and let it stand in dry air for a period of time;
[0045] Specifically, the amount of the mixed solution coated on the surface of the support layer is 3-100 g / m 2 .
[0046] Step 4, placing the support layer coated with the mixed solution into a non-solvent system for secondary phase transition to generate a primary composite nanofiltration membrane B;
[0047] Specifically, the non-solvent includes the following combinations:
[0048] water, methanol, and ethanol;
[0049] A mixed solution of water and methanol or ethanol;
[0050] A mixture of water and glycerol.
[0051] Step 5, placing the primary composite nanofiltration membrane B in hot water for swelling and washing, and finally obtaining the composite loose nanofiltration membrane C described in this case;
[0052] Specifically, the temperature of the hot water is 50-90° C., and the soaking and swelling time is 10-60 minutes.
[0053] Embodiment 1:
[0054] S1 is prepared with a casting solution containing 15%, 5% and 80% of meta-aramid, lithium chloride and DMAc respectively, which is degassed and then scraped onto the surface of the non-woven fabric, and then placed in pure water for phase transition. After the membrane is formed, it is fully washed to obtain an ultrafiltration membrane A1;
[0055] S2 Take 100 ml of DMF solvent, add 2.0% sulfonated polyphenylsulfone with a sulfonation degree of 35% and stir, degas the solution after stirring evenly, and let it stand for use after degassing;
[0056] S3 Fully coat and soak the surface of the support layer with 10g / m 2 The solution was mixed and allowed to stand in dry air for 2 min;
[0057] S4: placing the support layer coated with the mixed solution into pure water for secondary phase inversion to form a primary composite membrane B1;
[0058] S5. Put the primary composite nanofiltration membrane B1 into 60° C. hot water for swelling and washing for 20 min, and finally obtain the composite loose nanofiltration membrane C1 described in this case;
[0059] S6 Test the separation of magnesium sulfate and Congo red in C1, Congo red content 1000mg / L, magnesium sulfate content 2000mg / L, test pressure 0.5bar
[0060] The test results are: magnesium sulfate retention 17.7%, Congo red retention 99.1%
[0061] Comparative Example 1:
[0062] S1 prepares a casting solution with polysulfone, lithium chloride and DMAc contents of 15%, 5% and 80% respectively, degasses it and then applies it to the surface of the non-woven fabric, then puts it into pure water for phase transition, and washes it thoroughly after the membrane is formed to obtain the ultrafiltration membrane A2;
[0063] S2 Take 100 ml of DMF solvent, add 2.0% sulfonated polyphenylsulfone with a sulfonation degree of 35% and stir, degas the solution after stirring evenly, and let it stand for use after degassing;
[0064] S3 Fully apply 10g / m2 mixed solution on the surface of the support layer and let it stand in dry air for 2 minutes;
[0065] Experimental results: After the mixed solution was poured onto the surface of the polysulfone base membrane, the base membrane dissolved
[0066] Comparative Example 2:
[0067] S1 is prepared with a casting solution containing 15%, 5% and 80% of meta-aramid, lithium chloride and DMAc respectively, which is degassed and then scraped onto the surface of the non-woven fabric, and then placed in pure water for phase transition. After the membrane is formed, it is fully washed to obtain an ultrafiltration membrane A3;
[0068] S2 Take 100 ml of DMF solvent, add 2.0% sulfonated polyethersulfone with a sulfonation degree of 35% and stir, degas the solution after stirring evenly, and let it stand for use after degassing;
[0069] S3 Fully apply 10g / m2 mixed solution on the surface of the support layer and let it stand in dry air for 2 minutes;
[0070] S4: placing the support layer coated with the mixed solution into pure water for secondary phase inversion to form a primary composite membrane B3;
[0071] S5 The primary composite nanofiltration membrane B1 is placed in 60° C. hot water for swelling and washing for 20 min, and finally the composite loose nanofiltration membrane C3 described in this case is obtained;
[0072] S6 Test the separation of magnesium sulfate and Congo red in C3, Congo red content 1000mg / L, magnesium sulfate content 2000mg / L, test pressure 0.5bar
[0073] The test results are: magnesium sulfate retention 19.5%, Congo red retention 99.4%
[0074] Comparative Example 3:
[0075] S1 is a casting solution containing 15%, 5% and 80% of meta-aramid, lithium chloride and DMAc respectively, which is degassed and then scraped onto the surface of the non-woven fabric, and then placed in pure water for phase transition. After the membrane is formed, it is fully washed to obtain an ultrafiltration membrane A4;
[0076] S2 Take 100 ml of DMF solvent, add 2.0% sulfonated polyphenylsulfone with a sulfonation degree of 35% and stir, degas the solution after stirring evenly, and let it stand for use after degassing;
[0077] S3 Fully apply and soak 20g / m2 mixed solution on the surface of the support layer and let it stand in dry air for 2 minutes;
[0078] S4: placing the support layer coated with the mixed solution into pure water for secondary phase inversion to form a primary composite membrane B4;
[0079] S5 The primary composite nanofiltration membrane B1 is placed in 60° C. hot water for swelling and washing for 20 minutes, and finally the composite loose nanofiltration membrane C4 described in this case is obtained;
[0080] S6 C4 was tested for separation of magnesium sulfate and Congo red, Congo red content was 1000mg / L, magnesium sulfate content was 2000mg / L, and the test pressure was 0.5bar
[0081] The test results are: magnesium sulfate retention 58.7%, Congo red retention 99.9%
[0082] Comparative Example 4:
[0083] S1 is a casting solution containing 15%, 5% and 80% of meta-aramid, lithium chloride and DMAc respectively, which is degassed and then scraped onto the surface of the non-woven fabric, and then placed in pure water for phase transition. After the membrane is formed, it is fully washed to obtain an ultrafiltration membrane A5;
[0084] S2 Take 100 ml of DMF solvent, add 2.0% sulfonated polyphenylsulfone with a sulfonation degree of 35% and stir, degas the solution after stirring evenly, and let it stand for use after degassing;
[0085] S3 Fully apply 10g / m2 mixed solution on the surface of the support layer and let it stand in dry air for 2 minutes;
[0086] S4: The support layer coated with the mixed solution is placed in a 70°C oven and dried for 10 min to form a primary composite membrane B5;
[0087] S5. The primary composite nanofiltration membrane B1 is placed in 60° C. hot water for swelling and washing for 20 min, and finally the composite loose nanofiltration membrane C5 described in this case is obtained;
[0088] S6 Test the separation of magnesium sulfate and Congo red in C5, Congo red content 1000mg / L, magnesium sulfate content 2000mg / L, test pressure 0.5bar
[0089] The test result is: no water
[0090] Comparative Example 5:
[0091] S1 is a casting solution containing 15%, 5% and 80% of meta-aramid, lithium chloride and DMAc respectively, which is degassed and then scraped onto the surface of the non-woven fabric, and then placed in pure water for phase transition. After the membrane is formed, it is fully washed to obtain an ultrafiltration membrane A6;
[0092] S2 Take 100 ml of DMF solvent, add 2.0% sulfonated polyphenylsulfone with a sulfonation degree of 35% and stir, degas the solution after stirring evenly, and let it stand for use after degassing;
[0093] S3 Fully apply 10g / m2 mixed solution on the surface of the support layer and let it stand in dry air for 2 minutes;
[0094] S4: placing the support layer coated with the mixed solution into pure water for secondary phase inversion to form a primary composite membrane B6;
[0095] S5 Step 5, soaking the primary composite nanofiltration membrane B1 in 20° C. pure water, and finally obtaining the composite loose nanofiltration membrane C6 described in this case;
[0096] S6 C6 is tested for separation of magnesium sulfate and Congo red, Congo red content is 1000mg / L, magnesium sulfate content is 2000mg / L, test pressure is 0.5bar
[0097] The test results are: magnesium sulfate retention 18.1%, Congo red retention 99.5%
[0098] The summary results are as follows:
[0099]
[0100] It can be seen from the examples and comparative examples that the preparation process of the present invention mainly includes:
[0101] a. The base membrane is made of aramid ultrafiltration base membrane;
[0102] b. The coating layer mixed solution uses sulfonated polysulfone compounds such as sulfonated polyphenylsulfone and sulfonated polyethersulfone;
[0103] c. Fix a certain amount of coating mixture;
[0104] d. The coating is prepared by phase change process;
[0105] e. Hot water post-treatment swelling;
[0106] The above steps are the core technology for preparing composite loose nanofiltration membranes and are also necessary. The present invention prepares composite loose nanofiltration membrane sheets by a two-step method, which is commercially feasible and provides an important idea for the study of composite membrane structure and mechanism.
[0107] Regarding the contents disclosed in this case, there are a few points that need to be explained:
[0108] (1) The drawings of the embodiments disclosed in this case only involve the structures involved in the embodiments disclosed in this case. Other structures can refer to the general design;
[0109] (2) In the absence of conflict, the embodiments and features of the embodiments disclosed in this case may be combined with each other to obtain new embodiments;
[0110] The above are only specific implementation methods disclosed in this case, but the protection scope of the present disclosure is not limited thereto. The protection scope disclosed in this case should be based on the protection scope of the claims.
Claims
1. A composite loose nanofiltration membrane, characterized in that: Includes fixed connections in sequence: The non-woven fabric layer serves as the support material for the nanofiltration membrane and blocks the passage of fine particles; Aramid-based membrane, with a pore size of 10-40 nm, is used as the base membrane of the nanofiltration membrane; The sulfonated polyphenylsulfone layer, with a pore size of 2~5nm, serves as the separation layer of the nanofiltration membrane.
2. The composite loose nanofiltration membrane according to claim 1, characterized in that: The sulfonation degree of the sulfonated polyphenylene sulfone layer is between 10% and 80%.
3. The composite loose nanofiltration membrane according to claim 1, characterized in that: The pore size of the non-woven fabric layer is 100-300 nm.
4. The composite loose nanofiltration membrane according to claim 1 or 3, characterized in that: The thickness of the non-woven fabric layer is 70-150 um.
5. The composite loose nanofiltration membrane according to claim 1, characterized in that: The thickness of the aramid base film is 5-50um.
6. The composite loose nanofiltration membrane according to claim 1, characterized in that: The thickness of the sulfonated polyphenylene sulfone layer is 1-20 um.
7. The composite loose nanofiltration membrane according to claim 1, characterized in that: The thickness of the non-woven fabric layer is greater than the thickness of the aramid-based film and the thickness of the sulfonated polyphenylene sulfone layer.
Citation Information
Cited By
Composite loose nanofiltration membrane and preparation method thereof
CN118001950A