Ceramic core structure for casting

By designing a structure with fixed and free ends and waxed layers on the ceramic core, the fracture problem caused by inconsistent expansion coefficient in silicon sol precision casting is solved, and the fracture rate during baking and pouring is significantly reduced and production is achieved. Reduced costs.

CN222058757UActive Publication Date: 2024-11-26HUIDONG COUNTY JIBANG HARDWARE PROD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202323507622.7
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-21
Publication Date
2024-11-26
Estimated Expiration
2033-12-21

AI Technical Summary

Technical Problem

During the precision casting of silicon sols, the ceramic core fractures due to tensile stress caused by inconsistent expansion coefficients during high-temperature roasting and casting, which affects the accuracy of product structure and size and increases production costs.

Method used

Design a ceramic core structure for casting, which includes several ends, one of which is set as a fixed end, and the rest is a free end. The outer surface of the free end is coated with a wax layer of 0.4mm-0.6mm thick, by reducing the dewaxing after The number of fixed ends and the formation of voids to offset internal stress changes and reduce the risk of fracture.

Benefits of technology

It effectively reduces the fracture of the ceramic core during the baking and pouring process, and the fracture ratio is reduced by 80%, ensuring the accuracy of product structure and size and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222058757U_ABST
    Figure CN222058757U_ABST
Patent Text Reader

Abstract

The utility model discloses a ceramic core structure for casting. The ceramic core structure comprises a plurality of end heads, one of the plurality of end heads is provided with a fixed end, and the other end heads are free ends; a wax layer is arranged on the outer surface of the free end. The ceramic core is reasonable in structural design, and has the following beneficial effects that the fixed end is arranged in the end of the ceramic core, and the other ends are the free ends, so that the position of the ceramic core is fixed during shell making, the relative position and the size of the ceramic core of a product are ensured, and after dewaxing, the free ends are wrapped with wax liquid, so that the ceramic core is not damaged. A gap is formed between the shell mold and the ceramic core, so that only one fixed end which is not soaked in wax liquid is reserved in the whole ceramic core in the shell mold, the other free ends have relative degrees of freedom after dewaxing, and the phenomenon that the ceramic core is damaged due to inconsistent expansion coefficients in the roasting and pouring process is effectively avoided. And the ceramic core is broken due to the generated tensile stress.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of precision casting, in particular to a ceramic core structure for casting. Background Art

[0002] In silica sol precision casting, the contour size structure of the casting is realized through the silica sol precision casting process. The casting realization process is: product wax part mold manufacturing---injection of product wax parts---wax part shell mold making---dewaxing---baking shell mold---pouring metal---casting parts; the realization of deep holes, small narrow grooves and special anisotropic structures in the product part structure has always been a difficult problem in the precision casting industry; deep holes, small narrow grooves and special anisotropic structures are not easy to be directly realized through conventional shell making processes in the actual production process. Usually, the subsequent process is to solve the process defects of existing wax parts that are difficult to make shells or low strength of shell molds in corresponding positions by pre-embedded fired ceramic cores.

[0003] Although the ceramic core solves the problem of deep holes, small narrow grooves, and special heterogeneous structures in the current silica sol shell making process, the shell mold and the ceramic core will undergo physical expansion due to the influence of high temperature when the shell mold undergoes 1100° high-temperature roasting and 1600° pouring stages. Due to the different chemical material compositions of the two, the thermal expansion coefficients of the two are different after high-temperature heating. Since the thermal expansion coefficient of the shell mold is much larger than the expansion coefficient of the ceramic core, tensile stress will be generated between the two. When the tensile stress exceeds the yield strength of the ceramic core, deformation or even fracture will occur at the weak position of the ceramic core, eventually causing the position of the ceramic core inside the product to change, resulting in poor product structure and size. If the casting after pouring does not meet the requirements of the product part drawing or cannot meet the use requirements, it can only be scrapped, increasing production costs. Utility Model Content

[0004] The utility model aims to provide a ceramic core structure for casting, which can effectively reduce the occurrence of fracture of the ceramic core during the roasting and pouring process.

[0005] In order to achieve the above-mentioned purpose, the technical solution of the utility model provides a ceramic core structure for casting, which includes a plurality of end heads; a fixed end is provided among the plurality of end heads, and the rest are free ends; a wax layer is provided on the outer surface of the free end.

[0006] Furthermore, the ceramic core structure includes a middle end and a plurality of connecting ends.

[0007] Furthermore, the middle end is fixedly connected to a plurality of connecting ends, and the connecting ends are fixedly connected to the end heads.

[0008] Furthermore, the number of the connecting ends is three, and correspondingly, the number of the end heads is three, among which there is one fixed end and two free ends; the middle end is fixedly connected to the three connecting ends, and the connecting ends are fixedly connected to the end heads.

[0009] Furthermore, the wax layer has a thickness of 0.4 mm to 0.6 mm.

[0010] Furthermore, the wax layer has a thickness of 0.5 mm.

[0011] Furthermore, the ceramic core is a high temperature resistant ceramic core.

[0012] Furthermore, the wax of the wax layer is casting wax.

[0013] To sum up, the device structure of the utility model is reasonably designed, and the use of the technical scheme of the utility model has the following beneficial effects: because a fixed end is provided in the end of the ceramic core, and the rest are free ends, the position of the ceramic core is fixed during shell making, thereby ensuring the relative position and size of the product ceramic core. However, after dewaxing, the free end is wrapped in wax liquid, and a gap is formed between the shell mold and the ceramic core, so that the entire ceramic core only retains a fixed end that is not soaked in wax liquid in the shell mold, and the remaining free ends obtain relative freedom after dewaxing, effectively avoiding the tensile stress caused by inconsistent expansion coefficients during the roasting and pouring process, which leads to the fracture of the ceramic core. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a structural schematic diagram of the ceramic core of the utility model when in use;

[0015] Figure 2 It is a structural schematic diagram of the ceramic core of the utility model;

[0016] Explanation of the reference numerals: 1-ceramic core, 101-fixed end, 102-free end, 103-wax layer, 104-connecting end, 105-middle end; 2-shell mold; 3-wax part of the casting product. DETAILED DESCRIPTION

[0017] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention, but this does not constitute a limitation on the protection scope of the present invention.

[0018] In the present invention, for a clearer description, the following explanation is made: the observer faces the attached Figure 1For observation, the left front side of the observer is set as the front, the right rear side of the observer is set as the rear, the left rear side of the observer is set as the left, the right front side of the observer is set as the right, the top of the observer is set as the top, and the bottom of the observer is set as the bottom. It should be pointed out that the terms "front end", "rear end", "left side", "right side", "middle", "top", "bottom" and the like in the text indicate the orientation or position relationship based on the orientation or position relationship set in the drawings, which is only for the convenience of clearly describing the utility model, and does not indicate or imply that the structure or component referred to must have a specific orientation or be constructed in a specific orientation, and therefore cannot be understood as a limitation on the utility model. In addition, the terms "first", "second", "third", and "fourth" are only used for the purpose of clarifying or simplifying the description, and cannot be understood as indicating or implying relative importance or quantity.

[0019] During normal shell making, the exposed ends of the ceramic core 1 are wrapped and fixed by the shell mold 2. At this time, the ceramic core 1 loses its freedom in the shell mold 2. After dewaxing, it is tightly wrapped by the shell mold 2 and cannot change its displacement. At this time, if it is heated and expands, it can only rely on the plastic deformation of the internal structure to resist the external tensile stress. When the external tensile stress exceeds its own yield strength, it will produce yield deformation until the ceramic core 1 breaks; therefore, the utility model reduces the number of fixed ends 101 of the ceramic core 1 after dewaxing, so that only one fixed end 101 is retained, and the other end positions obtain relative freedom during its thermal expansion process, thereby offsetting the internal stress changes of the ceramic core 1 and reducing its plastic deformation, thereby solving the probability of the ceramic core breaking during the roasting and pouring process. Experiments have found that the fracture ratio of the ceramic core 1 structure using the utility model is reduced by 80% during the roasting and pouring process.

[0020] See also Figure 1 The utility model provides a ceramic core 1 structure for casting, which includes a plurality of end heads; a fixed end 101 is provided among the plurality of end heads, and the rest are free ends 102; a wax layer 103 is provided on the outer surface of the free end 102.

[0021] As a preferred embodiment of the present invention, Figure 1 , Figure 2 As shown, the ceramic core 1 includes a middle end 105 and three connecting ends 104, the middle end 105 is fixedly connected to the three connecting ends 104, and the connecting ends 104 are fixedly connected to the end heads. There are three connecting ends 104, and correspondingly, there are three end heads, including a fixed end 101 and two free ends 102. The wax layer 103 on the outer surface of the free end 102 has a thickness of 0.5 mm, and the parts other than the end heads of the ceramic core 1 are all wrapped by the wax part 3 of the casting product, and the structure after the ceramic core 1 and the wax part 3 of the casting product are combined is then wrapped by the shell mold 2.

[0022] Specifically, the ceramic core 1 is a high temperature resistant ceramic core 1, and the wax of the wax layer 103 is casting wax.

[0023] Shell making sequence: fix ceramic core - injection casting product wax part - wax part shell mold - dewaxing - baking shell mold - pouring metal - vibrating shell - cleaning sand

[0024] Implementation steps:

[0025] 1. When the ceramic core is injection-casting the wax part of the product, one of the exposed ends is exposed;

[0026] 2. Apply a layer of wax liquid with a thickness of about 0.5mm on the remaining exposed ends, and then make the shell in the conventional process;

[0027] 3. Dewaxing. After dewaxing, except for the fixed end that is not soaked in wax, it is completely wrapped with the shell mold. During dewaxing, the wax layer of the other fixed ends wrapped with wax layer also melts and flows out, and a gap of about 0.5mm is naturally formed between the shell and the ceramic core.

[0028] 4. Calcination, pouring, shell vibration, sand cleaning, shell vibration or sand cleaning and removal of ceramic core at the same time to obtain castings that meet the requirements.

[0029] When the exposed ends of the ceramic core 1 are not treated by soaking in wax liquid, they will be wrapped and fixed by the shell mold 2 during shell making. In this way, the ceramic core 1 loses its freedom in the shell mold 2. If subjected to external force, it can only rely on internal tissue to undergo plastic deformation. When its yield strength is exceeded, yield deformation will occur until the ceramic core 1 breaks. If one of the exposed ends of the ceramic core 1 is exposed during shell making, a layer of wax liquid with a thickness of about 0.5 mm is soaked in the remaining exposed ends, and then normal shell making is performed. In this way, during shell making, the position of the ceramic core 1 can be fixed to ensure the relative position and size of the product ceramic core 1, and after dewaxing, the position of the wax liquid is wrapped, and a gap of about 0.5 mm is formed between the shell mold 2 and the ceramic core 1. In this way, the entire ceramic core 1 only retains a fixed end 101 that is not soaked in wax liquid in the shell mold 2, and the remaining free space 102 obtains relative freedom after dewaxing, effectively avoiding the tensile stress caused by inconsistent expansion coefficients during the roasting and pouring process, which leads to the tensile fracture of the ceramic core 1.

[0030] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the protection scope of the present invention.

Claims

1. A ceramic core structure for casting, characterized in that: The ceramic core structure comprises a plurality of end heads; one fixed end is arranged among the plurality of end heads, and the rest are free ends; and a wax layer is arranged on the outer surface of the free end.

2. A ceramic core structure for casting according to claim 1, characterized in that: The ceramic core structure includes a middle end and a plurality of connecting ends.

3. A ceramic core structure for casting according to claim 2, characterized in that: The middle end is fixedly connected to a plurality of connecting ends, and the connecting ends are fixedly connected to the end heads.

4. A ceramic core structure for casting according to claim 3, characterized in that: The number of the connecting ends is three, and correspondingly, the number of the end heads is three, among which there is one fixed end and two free ends; the middle end is fixedly connected to the three connecting ends, and the connecting ends are fixedly connected to the end heads.

5. The ceramic core structure for casting according to claim 1, characterized in that: The wax layer has a thickness of 0.4 mm to 0.6 mm.

6. A ceramic core structure for casting according to claim 5, characterized in that: The wax layer has a thickness of 0.5 mm.

7. A ceramic core structure for casting according to claim 1, characterized in that: The ceramic core is a high temperature resistant ceramic core.

8. A ceramic core structure for casting according to claim 1, 5 or 6, characterized in that: The wax of the wax layer is casting wax.

Citation Information

Cited By

  • Annular narrow channel casting forming method

    CN119657838A