Porous catalyst gas diffusion electrode

By using a porous catalyst gas diffusion electrode structure during the electrolytic hydrogen production process, and using electrochemical deposition and pore formation treatment technology, the problems of easy shedding of the anode catalyst and degradation of the proton exchange membrane are solved, and the catalyst stability and electrode life are improved.

CN222119406UActive Publication Date: 2024-12-06BEIJING SINOHYTEC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202322836162.6
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-10-20
Publication Date
2024-12-06
Estimated Expiration
2033-10-20

AI Technical Summary

Technical Problem

During the existing process of electrolyzing hydrogen production, the anode catalyst is easily disturbed and falls off by gas, and changes in microstructure lead to a decrease in catalytic function. The proton exchange membrane also gradually degrades over time, resulting in a decrease in membrane electrode activity and shortening service life.

Method used

Using a porous catalyst gas diffusion electrode structure, in which the anode diffusion layer is prepared by an electrochemical deposition method, comprising a mixture of the first element (such as iridium) and the second element (such as aluminum, manganese, iron, cobalt), and pore formation by alternating current deposition and pore formation The treatment forms a porous structure, enhancing the stability of the catalyst.

Benefits of technology

The stability of the catalyst and the service life of the electrolytic water-based hydrogen production electrode are improved, and the catalyst is prevented from falling off the proton exchange membrane, extending the activity life of the membrane electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222119406U_ABST
    Figure CN222119406U_ABST
Patent Text Reader

Abstract

The utility model provides a porous catalyst gas diffusion electrode, which belongs to the technical field of water electrolysis, and is characterized in that a porous anode catalyst is combined with an anode diffusion layer to form the gas diffusion electrode. The gas diffusion electrode is recombined with other assemblies to form a complete water electrolysis hydrogen production electrode, and the specific combination mode comprises a proton exchange membrane and a cathode catalyst layer located on the first side of the proton exchange membrane; the cathode diffusion layer is positioned on the cathode catalyst layer; and one side of the anode gas diffusion electrode, which is provided with the anode catalyst layer, is attached to the second side of the proton exchange membrane. Wherein the anode diffusion electrode is prepared by adopting an electrochemical deposition method, and the catalyst is not easy to fall off from the proton exchange membrane, so that the stability of the catalyst is improved, and the service life of the membrane electrode is further prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water electrolysis, and in particular relates to a porous catalyst gas diffusion electrode. Background Art

[0002] In the electrolysis of water to produce hydrogen, the electrolytic stack is the place where the electrochemical reaction occurs. In the electrolytic stack, the water at the anode is catalytically oxidized on the catalyst surface to generate oxygen and is discharged by the water flow, and the protons pass through the proton exchange membrane to reach the cathode catalyst, where they obtain electrons under the catalytic action of the catalyst to generate hydrogen. Under the same conditions (such as bipolar plates, diffusion layers, proton exchange membranes, etc.), the DC efficiency and service life of the electrolytic stack are mainly subject to the activity and stability of the anode catalyst.

[0003] In existing electrolytic stacks, the cathode catalyst and the anode catalyst are usually coated on both sides of the proton exchange membrane, and then combined with the cathode diffusion layer and the anode diffusion layer to form a "five-in-one" membrane electrode assembly (MEA). During the electrolysis of water, water is oxidized on the anode catalyst layer to generate oxygen, while protons are transferred to the cathode catalyst layer through the proton exchange membrane under the action of the electric field and further reduced to hydrogen. Through the gas diffusion layer, oxygen and hydrogen are respectively exported to the flow channel and then discharged from the electrolytic stack, completing the process of electrolytic hydrogen and oxygen production.

[0004] The existing membrane electrode is to directly apply the cathode and anode catalyst layers on both sides of the proton exchange membrane. In order to ensure the activity of the membrane electrode, a high-load catalyst is often required to be applied on the anode side. In the process of water electrolysis to generate bubbles, the catalyst layer is easily disturbed by the gas and falls off; even under high voltage, the microstructure of the anode catalyst changes, thereby losing its catalytic function and reducing the activity of the membrane electrode. Moreover, with long-term reaction, the proton exchange membrane will gradually degrade from the outside to the inside, and the catalyst will also fall off the proton exchange membrane and lose its catalytic effect, causing the membrane electrode to be more easily deactivated. Summary of the invention

[0005] The present invention provides a porous catalyst gas diffusion electrode, which can solve the problem that in the process of water electrolysis to generate bubbles, the catalyst layer is easily disturbed by gas and falls off; even under high voltage, the microstructure of the anode catalyst changes, thereby losing the catalytic function and reducing the activity of the membrane electrode. Moreover, with long-term reaction, the proton exchange membrane will gradually degrade from the outside to the inside, and the catalyst will also fall off the proton exchange membrane and lose its catalytic effect, resulting in the technical problem that the membrane electrode is relatively easy to deactivate.

[0006] The technical solution provided by the present invention is as follows:

[0007] A porous catalyst gas diffusion electrode is provided, wherein the electrode is prepared by any of the above methods, and the electrode comprises:

[0008] Proton exchange membrane,

[0009] a cathode catalyst layer, located on a first side of the proton exchange membrane;

[0010] A cathode diffusion layer, located on the cathode catalyst layer;

[0011] an anode diffusion layer, wherein one side of the anode diffusion layer has an anode catalyst layer;

[0012] The anode diffusion layer has a side with an anode catalyst layer located on the second side of the proton exchange membrane, wherein the anode catalyst layer is prepared by an electrochemical deposition method.

[0013] In an optional embodiment, the anode diffusion layer includes a first element and a second element.

[0014] In an optional embodiment, the second element includes at least one or more of aluminum, manganese, iron, nickel, and cobalt.

[0015] In an optional embodiment, the first element is iridium.

[0016] In an optional embodiment, the molar ratio of the first element to the second element is 1:10-15. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The above and other objects, features and advantages of the present disclosure will become more apparent through a more detailed description of exemplary embodiments of the present disclosure in conjunction with the accompanying drawings, wherein like reference numerals generally represent like components throughout the exemplary embodiments of the present disclosure.

[0018] Figure 1 A schematic diagram of the structure of a porous catalyst gas diffusion electrode is shown.

[0019] Wherein, the accompanying drawings are marked as follows:

[0020] 1-proton exchange membrane, 2-cathode catalyst layer, 3-anode catalyst layer, 4-cathode diffusion layer, 5-anode diffusion layer. DETAILED DESCRIPTION

[0021] Embodiments of the present disclosure will be described in more detail below with reference to the accompanying drawings. Although embodiments of the present disclosure are shown in the accompanying drawings, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present disclosure more thorough and complete, and to fully convey the scope of the present disclosure to those skilled in the art.

[0022] As used herein, the term "including" and its variations mean open inclusion, i.e., "including but not limited to". Unless otherwise stated, the term "or" means "and / or". The term "based on" means "based at least in part on". The terms "an example embodiment" and "an embodiment" mean "at least one example embodiment". The term "another embodiment" means "at least one additional embodiment". The terms "first", "second", etc. may refer to different or the same objects. Other explicit and implicit definitions may also be included below.

[0023] See also Figure 1 , provides a porous catalyst gas diffusion electrode, the electrode comprising:

[0024] Proton exchange membrane 1,

[0025] A cathode catalyst layer 2, located on a first side of the proton exchange membrane 1;

[0026] A cathode diffusion layer 4 is located on the cathode catalyst layer 2;

[0027] an anode catalyst layer 3, located on one side of the anode diffusion layer 5;

[0028] The anode diffusion layer 5 is combined with the anode catalyst layer to form an anode electrode, wherein the anode electrode is prepared by an electrochemical deposition method.

[0029] The electrode provided by the embodiment of the present invention has at least the following beneficial effects:

[0030] In the electrode provided by the embodiment of the present invention, the catalyst will not fall off from the proton exchange membrane easily, thereby improving the stability of the catalyst and further increasing the life of the electrode for producing hydrogen by electrolyzing water.

[0031] In an optional embodiment, the first element is iridium.

[0032] In an optional embodiment, the second element includes at least one or more of aluminum, manganese, iron, nickel, and cobalt.

[0033] As an example, the second element may be a mixture of the above metal elements, or may be a single metal element.

[0034] In an optional embodiment, the molar ratio of the first element to the second element is 1:10-15.

[0035] It should be noted that the size of the pores in the porous catalyst gas diffusion electrode provided in the embodiment of the present invention is determined by the deposition amount of the first element and the second element. In this embodiment, the molar ratio of the first element to the second element includes 1:10 to 15. For example, it can be 1:10, 1:11, 1:12, 1:13, 1:14 or 1:15, etc.

[0036] The present invention provides a method for preparing a porous catalyst gas diffusion electrode, comprising:

[0037] S1, immersing the anode diffusion layer in a first solution, and performing current deposition at a first preset current density;

[0038] S2, immersing the anode diffusion layer in a second solution, and performing current deposition at a second preset current density;

[0039] S3, alternately performing current deposition on the anode diffusion layer in the first solution and the second solution;

[0040] S4, performing pore forming treatment on the deposited anode diffusion layer, calcining, and cooling to obtain a porous catalyst gas diffusion electrode;

[0041] The first solution contains a first element, and the second solution contains a second element.

[0042] A method for preparing a porous catalyst gas diffusion electrode can also be prepared by the following steps, including:

[0043] S5, immersing the anode diffusion layer in a mixture of the first solution, the second solution and the third solution, and performing current deposition at a third preset current density;

[0044] S6, performing pore forming treatment on the deposited anode diffusion layer, calcining, and cooling to obtain a porous catalyst gas diffusion electrode;

[0045] The first solution contains the first element, the second solution contains the second element, and the third solution contains the third element.

[0046] In an optional embodiment, the second solution includes at least one or more of nickel chloride, cobalt chloride, aluminum chloride, manganese chloride, iron chloride, and ruthenium chloride.

[0047] For example, the second solution can be a single nickel chloride, cobalt chloride, aluminum chloride, manganese chloride, iron chloride or ruthenium chloride solution, or a mixture of nickel chloride and cobalt chloride, the mixing ratio can be 1:1, or a mixture of nickel chloride, cobalt chloride and silicon chloride, the mixing ratio can be 1:1:1, or a mixture of aluminum chloride, manganese chloride, iron chloride and ruthenium chloride, the mixing ratio can be 1:1:1:1. The embodiment of the present invention is not limited to the type of the mixed solution of the first solution, and the proportion of the remaining solutions in the mixed solution is not limited to this.

[0048] In an optional embodiment, the first solution is chloroiridic acid.

[0049] By providing the first solution as chloroiridic acid, metal iridium can be electrochemically deposited on the anode diffusion layer. Since metal iridium is not corroded by acid and alkaline solutions, during the pore-forming process, the remaining metal deposited on the anode diffusion layer is corroded to form pores.

[0050] In an optional embodiment, the third solution is a mixture of polyvinyl pyrrolidone and one or both of sodium chloroplatinate or ruthenium chloride.

[0051] It should be noted that the electrode provided in the embodiment of the present invention can be prepared by two methods. One is to immerse the anode diffusion layer in a mixture of the first solution, the second solution and the third solution to perform current deposition. By providing the third solution, the catalytic performance of the gas diffusion electrode can be more directly regulated.

[0052] As an example, the third solution may be polyvinyl pyrrolidone or sodium chloroplatinate alone, or a mixture of the two. When the mixture is a mixture of the two, the molar ratio may be 15 to 30. The ratio of the third solution in the embodiment of the present invention when the mixture is a mixture is not limited thereto.

[0053] In an optional embodiment, the second preset current density is 2 mA / cm 2 -5mA / cm 2 The constant current deposition was carried out for 5-10 min at a current density of 1.50 Å.

[0054] The anode diffusion layer was immersed in the second dissolving solution at 2 mA / cm 2 -5mA / cm 2 For example, the second preset current density may be 2 mA / cm 2 , 2.1mA / cm 2 , 2.2mA / cm 2 , 2.3mA / cm 2 , 2.5mA / cm 2 , 2.8mA / cm 2 , 3mA / cm 2 , 3.1mA / cm 2 , 2, 3.2mA / cm2, 3.5mA / cm 2 , 3.6mA / cm 2 、3.9mA / cm 2 , 4.0mA / cm 2 , 4.1mA / cm 2 , 4.2mA / cm 2 , 4.5mA / cm 2 , 4.6mA / cm 2 , 4.9mA / cm 2 , 5.0mA / cm 2 .

[0055] The constant current deposition time at the second preset current density can be 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, or 10 minutes.

[0056] In an optional embodiment, the first solution is chloroiridic acid (H2IrCl6·6H2O).

[0057] In an optional embodiment, the first preset current density is 2 mA / cm 2 -5mA / cm 2 The anode diffusion layer was immersed in the second solution at 2 mA / cm 2 -5mA / cm 2 Current deposition, the first preset current density can be 2mA / cm 2 , 2.1mA / cm 2 , 2.2mA / cm 2 , 2.3mA / cm 2 , 2.5mA / cm 2 , 2.8mA / cm 2 , 3mA / cm 2 , 3.1mA / cm 2 , 2, 3.2mA / cm2, 3.5mA / cm 2 , 3.6mA / cm 2 、3.9mA / cm 2 , 4.0mA / cm 2 , 4.1mA / cm 2 , 4.2mA / cm 2 , 4.5mA / cm 2 , 4.6mA / cm 2 , 4.9mA / cm 2 , 5.0mA / cm 2 wait.

[0058] Furthermore, in the embodiment of the present invention, the first preset current is the same as the second preset current.

[0059] In an optional embodiment, the current deposition is performed alternately with the first preset current density and the second preset current density 30-50 times.

[0060] The number of times of alternating current deposition is 20 times, 23 times, 24 times, 25 times, 27 times, 28 times, 30 times, 33 times, 34 times, 36 times, 39 times, 40 times, 41 times, 43 times, 44 times, 47 times, 48 ​​times, 49 times, 50 times, etc.

[0061] In an optional embodiment, the third preset current density is 2 mA / cm 2-5mA / cm 2 The constant current deposition was carried out for 150-200 min at a current density of 1.50 Å.

[0062] The anode diffusion layer was immersed in the second dissolving solution at 2 mA / cm 2 -5mA / cm 2 Current deposition, the second preset current density can be 2 mA / cm 2 , 2.1mA / cm 2 , 2.2mA / cm 2 , 2.3mA / cm 2 , 2.5mA / cm 2 , 2.8mA / cm 2 , 3mA / cm 2 , 3.1mA / cm 2 , 2, 3.2mA / cm2, 3.5mA / cm 2 , 3.6mA / cm 2 、3.9mA / cm 2 , 4.0mA / cm 2 , 4.1mA / cm 2 , 4.2mA / cm 2 , 4.5mA / cm 2 , 4.6mA / cm 2 , 4.9mA / cm 2 , 5.0mA / cm 2 wait.

[0063] The constant current deposition time at the third preset current density can be 150 minutes, 153 minutes, 167 minutes, 170 minutes, 178 minutes, 180 minutes, 183 minutes, 190 minutes, 196 minutes, 200 minutes, etc.

[0064] In an optional embodiment, the anode diffusion layer deposited alternately by the first solution and the second solution is immersed in an acid solution to form pores.

[0065] For example, the concentration of the acid solution may be 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L. The concentration of the alkali solution may be 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L, etc.

[0066] In an optional embodiment, the anode diffusion layer that has undergone pore formation treatment is washed with deionized water, calcined at a preset temperature for 5 to 8 hours, and cooled to obtain a porous catalyst gas diffusion electrode.

[0067] The pickled anode diffusion layer is cleaned with deionized water to remove the acid solution thereon, and is calcined at a high temperature of 500° C. to 800° C. in a nitrogen or vacuum furnace. For example, the calcination temperature may be 500° C., 510° C., 540° C., 590° C., 600° C., 620° C., 650° C., 680° C., 700° C., 730° C., 740° C., 750° C., 780° C., 790° C., 290° C., etc. The calcination time may be 5 hours, 6 hours, 7 hours, or 8 hours, etc.

[0068] In an optional embodiment, the anode diffusion layer deposited alternately by the first solution and the second solution is immersed in an acid solution to form pores, including performing pore forming treatment in a 3mol / L to 5mol / L acid solution or a 3mol / L to 5mol / L alkaline solution.

[0069] For example, the concentration of the acid solution may be 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, or 5 mol / L. The concentration of the alkaline solution may be 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, or 5 mol / L.

[0070] In an optional embodiment, the acid solution includes at least one of nitric acid, sulfuric acid or hydrochloric acid, and the alkaline solution is sodium hydroxide.

[0071] It should be noted that in the second preparation method, the embodiment of the present invention forms a porous structure 100 by subjecting the anode diffusion layer to pore formation, that is, by subjecting the anode diffusion layer on which the first element and the second element are deposited to constant current deposition and then corroding. The acid solution may be a mixture of one or more of nitric acid, sulfuric acid or hydrochloric acid. The embodiment of the present invention does not limit the type of the mixture of the acid solution.

[0072] The method provided by the embodiment of the present invention will be further explained and described below through specific examples.

[0073] Example 1

[0074] Anode electrode preparation: The anode diffusion layer was immersed in a 0.2 M chloroiridic acid (H2IrCl6·6H2O) solution at 2 mA / cm 2 The constant current deposition was carried out for two and a half minutes at a density of 1.50 m / s, and this step was recorded as ED1;

[0075] The anode diffusion layer was transferred to a 0.2 M nickel chloride (NiCl2) solution and charged at 2 mA / cm 2 The constant current deposition was carried out for five minutes at a density of 1000 nm. This step was recorded as ED2.

[0076] Repeat steps ED1 and ED2 thirty times. Transfer the anode diffusion layer into a 3M nitric acid (HNO3) solution, soak for one hour, take it out and wash it with deionized water.

[0077] The anode diffusion layer is placed in a nitrogen / vacuum furnace, calcined at 500°C for one hour, and cooled naturally to obtain a gas diffusion layer electrode (anode electrode) with a porous catalyst layer.

[0078] Platinum carbon is coated on one side of the proton exchange membrane by spraying or scraping to form a CCM (catalyst-coated membrane). The platinum-coated carbon side of the CCM is then bonded to the cathode diffusion layer, while the other side is directly bonded to the anode electrode, ultimately forming a complete water electrolysis membrane electrode.

[0079] Example 2

[0080] Anode electrode preparation: The anode diffusion layer was immersed in a solution containing 0.2 M nickel chloride (NiCl2), 0.12 M chloroiridic acid (H2IrCl6·6H2O) and 2 M polyvinyl pyrrolidone (PVP) and charged at 2 mA / cm 2 The constant current deposition was carried out for one hundred and fifty minutes.

[0081] The anode diffusion layer was transferred into a 3M nitric acid (HNO3) solution, soaked for one hour, taken out and washed with deionized water.

[0082] The anode diffusion layer is placed in a vacuum furnace, calcined at 500°C for one hour, and cooled naturally to obtain a gas diffusion layer electrode with a porous catalyst layer.

[0083] Platinum carbon is coated on one side of the proton exchange membrane by spraying or scraping to form a CCM. The platinum carbon coated side of the CCM is then bonded to the cathode diffusion layer, while the other side is directly bonded to the anode electrode, ultimately forming a complete water electrolysis membrane electrode.

[0084] Example 3

[0085] Anode electrode preparation: The anode diffusion layer was immersed in a solution containing 0.2 M nickel chloride (NiCl2), 0.12 M chloroiridic acid (H2IrCl6), 0.036 M ruthenium chloride (RuCl3) and 2 M polyvinyl pyrrolidone (PVP) and charged at 2 mA / cm 2 The constant current deposition was carried out for one hundred and fifty minutes.

[0086] The anode diffusion layer was transferred into a 3M nitric acid (HNO3) solution, soaked for one hour, taken out and washed with deionized water.

[0087] The anode diffusion layer is placed in a vacuum furnace, calcined at 500°C for one hour, and cooled naturally to obtain a gas diffusion layer electrode (anode electrode) with a porous catalyst layer.

[0088] Platinum carbon is coated on one side of the proton exchange membrane by spraying or scraping to form a CCM. The platinum carbon coated side of the CCM is then bonded to the cathode diffusion layer, while the other side is directly bonded to the anode electrode, ultimately forming a complete water electrolysis membrane electrode.

[0089] Example 4

[0090] Anode electrode preparation: The anode diffusion layer was immersed in a solution containing 0.2 M nickel chloride (NiCl2), 0.12 M chloroiridic acid (H2IrCl6), 0.036 M sodium chloroplatinate (Na2PtCl6·6H2O) and 2 M polyvinylpyrrolidone (PVP) and charged at 2 mA / cm 2 The constant current deposition was carried out for one hundred and fifty minutes.

[0091] The anode diffusion layer was transferred into a 3M nitric acid (HNO3) solution, soaked for one hour, taken out and washed with deionized water.

[0092] The anode diffusion layer is placed in a vacuum furnace, calcined at 500°C for one hour, and cooled naturally to obtain a gas diffusion layer electrode (anode electrode) with a porous catalyst layer.

[0093] Platinum carbon is coated on one side of the proton exchange membrane by spraying or scraping to form a CCM. The platinum carbon coated side of the CCM is then bonded to the cathode diffusion layer, while the other side is directly bonded to the anode electrode, ultimately forming a complete water electrolysis membrane electrode.

[0094] Example 5

[0095] Anode electrode preparation: The anode diffusion layer was immersed in a 0.2 M chloroiridic acid (H2IrCl6·6H2O) solution at 2 mA / cm 2 The constant current deposition was carried out for two and a half minutes at a density of 1.50 m / s, and this step was recorded as ED1;

[0096] The anode diffusion layer was transferred to a 0.2 M cobalt chloride (CoCl2) solution and charged at 2 mA / cm 2 The constant current deposition was carried out for five minutes, and this step was recorded as ED1.

[0097] Repeat steps ED1 and ED2 thirty times. Transfer the anode diffusion layer into a 3M nitric acid (HNO3) solution, soak for one hour, take it out and wash it with deionized water.

[0098] The anode diffusion layer is placed in a nitrogen / vacuum furnace, calcined at 500°C for one hour, and cooled naturally to obtain a gas diffusion layer electrode (anode electrode) with a porous catalyst layer.

[0099] Platinum carbon is coated on one side of the proton exchange membrane by spraying or scraping to form a CCM. The platinum carbon coated side of the CCM is then bonded to the cathode diffusion layer, while the other side is directly bonded to the anode electrode, ultimately forming a complete water electrolysis membrane electrode.

[0100] Example 6

[0101] Anode electrode preparation: The anode diffusion layer was immersed in a solution containing 0.2 M cobalt chloride (CoCl2), 0.12 M chloroiridic acid (H2IrCl6·6H2O) and 2 M polyvinyl pyrrolidone (PVP) and charged at 2 mA / cm 2 The constant current deposition was carried out for one hundred and fifty minutes.

[0102] The anode diffusion layer was transferred into a 3M nitric acid (HNO3) solution, soaked for one hour, taken out and washed with deionized water.

[0103] The anode diffusion layer is placed in a vacuum furnace, calcined at 500°C for one hour, and cooled naturally to obtain a gas diffusion layer electrode (anode electrode) with a porous catalyst layer.

[0104] Platinum carbon is coated on one side of the proton exchange membrane by spraying or scraping to form a CCM. The platinum carbon coated side of the CCM is then bonded to the cathode diffusion layer, while the other side is directly bonded to the anode electrode, ultimately forming a complete water electrolysis membrane electrode.

[0105] Example 7

[0106] Anode electrode preparation: The anode diffusion layer was immersed in a solution containing 0.2 M cobalt chloride (CoCl2), 0.12 M chloroiridic acid (H2IrCl6), 0.036 M ruthenium chloride (RuCl3) and 2 M polyvinyl pyrrolidone (PVP) and charged at 2 mA / cm 2 The constant current deposition was carried out for one hundred and fifty minutes.

[0107] The anode diffusion layer was transferred into a 3M nitric acid (HNO3) solution, soaked for one hour, taken out and washed with deionized water.

[0108] The anode diffusion layer is placed in a vacuum furnace, calcined at 500°C for one hour, and cooled naturally to obtain a gas diffusion layer electrode with a porous catalyst layer.

[0109] Platinum carbon is coated on one side of the proton exchange membrane by spraying or scraping to form a CCM. The platinum carbon coated side of the CCM is then bonded to the cathode diffusion layer, while the other side is directly bonded to the anode electrode, ultimately forming a complete water electrolysis membrane electrode.

[0110] Example 8

[0111] Anode electrode preparation: The anode diffusion layer was immersed in a solution containing 0.2 M cobalt chloride (CoCl2), 0.12 M chloroiridic acid (H2IrCl6), 0.036 M sodium chloroplatinate (Na2PtCl6·6H2O) and 2 M polyvinylpyrrolidone (PVP) and charged at 2 mA / cm 2 The constant current deposition was carried out for one hundred and fifty minutes.

[0112] The anode diffusion layer was transferred into a 3M nitric acid (HNO3) solution, soaked for one hour, taken out and washed with deionized water.

[0113] The anode diffusion layer is placed in a vacuum furnace, calcined at 500°C for one hour, and cooled naturally to obtain a gas diffusion layer electrode (anode electrode) with a porous catalyst layer.

[0114] Platinum carbon is coated on one side of the proton exchange membrane by spraying or scraping to form a CCM. The platinum carbon coated side of the CCM is then bonded to the cathode diffusion layer, while the other side is directly bonded to the anode electrode, ultimately forming a complete water electrolysis membrane electrode.

[0115] The embodiments of the present disclosure have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A porous catalyst gas diffusion electrode, characterized in that: The electrode comprises: Proton exchange membrane, a cathode catalyst layer, located on a first side of the proton exchange membrane; A cathode diffusion layer, located on the cathode catalyst layer; an anode diffusion layer, wherein one side of the anode diffusion layer has an anode catalyst layer; The anode diffusion layer has a side with an anode catalyst layer located on the second side of the proton exchange membrane, wherein the anode catalyst layer is prepared by an electrochemical deposition method.

2. The electrode according to claim 1, characterized in that The anode catalyst layer includes a first element and a second element.

3. The electrode according to claim 2, characterized in that The first element is iridium.

4. The electrode according to claim 3, characterized in that The second element includes one of aluminum, manganese, iron, nickel and cobalt.