COMPOUNDER, DESICATOR, SEALING STRUCTURE AND ORGANIC EL ELEMENT

A desiccant compound with a specific formula, containing aluminum, titanium, or boron atoms and fluorine, addresses moisture penetration in organic EL elements, enhancing durability by preventing dark spot formation and maintaining element integrity.

DE102015209342B4Inactive Publication Date: 2024-10-24FUTABA CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
DE102015209342
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2014-05-22
Filing Date
2015-05-21
Publication Date
2024-10-24
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional organic EL elements face issues with durability due to moisture and oxygen penetration, leading to the formation of non-light-emitting dark spots, which can cause device failure.

Method used

A compound with a specific formula (1) is used as a desiccant in a sealing structure, containing aluminum, titanium, or boron atoms, with fluorine atoms in a predetermined proportion, to suppress moisture penetration into the organic layer while maintaining transparency and avoiding cloudiness.

Benefits of technology

The compound effectively inhibits moisture penetration, maintaining the integrity of the organic layer and preventing dark spot formation, thus enhancing the durability of organic EL elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Connection represented by formula (1): where M represents an aluminum atom, a titanium atom, a silicon atom, or a boron atom; m represents 1 or 2; n represents a positive integer from 1 to 100; R 1 , R 2 and R 3 each independently represents a C1-16 alkyl group, optionally substituted with one or more fluorine atoms, or a C2-17 acyl group, optionally substituted with one or more fluorine atoms, and if several R 3 are present, which include several R 3 They may be the same or different from each other; wherein some of the carbon atoms forming the C1-16 alkyl group, which is optionally substituted with one or more fluorine atoms, may be replaced by one or more oxygen atoms, and wherein some of the carbon atoms forming the C2-17 acyl group, which is optionally substituted with one or more fluorine atoms, may be replaced by one or more oxygen atoms; and wherein the proportion of the total number of fluorine atoms in R 1 , R 2 and R 3 15% or more, relative to the total number of fluorine and hydrogen atoms in R 1 , R 2 and R 3 , and in the case where at least one of R 1 , R 2 and R 3 an acyl group substituted with one or more fluorine atoms, at least one other of R 1 , R 2 and R 3 an alkyl group that is substituted with one or more fluorine atoms.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a compound as well as a desiccant, a sealing structure and an organic EL element using them. STATE OF THE ART

[0002] In recent years, active research and development has been conducted on organic EL displays or organic EL lights, which are light-emitting devices using an organic electroluminescence (EL) element. The organic EL element has a structure in which an organic layer, which is a thin film containing an organic light-emitting material, is sandwiched between a pair of electrodes. The organic EL element is a self-light-emitting element that utilizes light emission (fluorescence or phosphorescence) at the time of deactivation of excitons generated by the recombination of holes and electrons introduced into the thin film.

[0003] The biggest challenge for organic EL elements is improving durability. Specifically, preventing the appearance and growth of non-light-emitting areas, called dark spots, in the organic layer. When the diameter of a dark spot grows to a few tens of micrometers, non-light-emitting areas become visually observable. As the fundamental cause of dark spots, the influence of moisture and oxygen is significant, and it is known that moisture, even in extremely small amounts, exerts a particularly significant influence.

[0004] For this reason, various studies have been conducted on methods for preventing moisture and oxygen penetration into organic EL elements. For example, Patent Literature 1 proposes a method involving the provision of a sealing layer around the periphery of an organic EL element, which consists of an inert liquid containing an adsorbent in which an organic layer is laminated.

[0005] Alternatively, for the purpose of physically protecting the organic layer, improving heat dissipation properties, and the like, a filled sealing structure has been proposed in which an airtight container of the organic EL element is filled with a filler. In addition, a filled sealing structure containing a desiccant as a filler has also been proposed. For example, Patent Literature 2 proposes a method involving the use of an organic metal compound, which is a desiccant and has a predetermined structure, together with a viscous substitute material such as silicone as a filler. LITERATURE LISTPATENT LITERATURE [Patent Literature 1] JP H09-035868 A [Patent Literature 2] JP 2013-176751 A SUMMARY

[0006] Incidentally, a conventional organic metal compound used as a desiccant of the filled sealing structure for organic EL elements and the like has the property of dissolving organic layers in the organic EL elements. In organic EL elements of the filled sealing structure, it is rare for a desiccant to come into direct contact with an organic layer because the electrode formed of aluminum and the like comes into contact with the desiccant. However, in the case where the desiccant comes into contact with the organic layer, there is a possibility that the desiccant will penetrate the organic layer and cause dissolution of the organic layer.Because the dissolution of the organic layer becomes a cause of the formation of dark spots and leads to loss failure in the device, it is desired to use an agent as a desiccant which can suppress its penetration into the organic layer.

[0007] The present invention has been made in view of the problems described above, and has an object to provide a compound which has sufficient water-occluding properties and, when used as a desiccant, can suppress its penetration into an organic layer, as well as to provide a desiccant, a sealing structure and an organic EL element using this compound.

[0008] The present invention provides a compound represented by formula (1): wherein M represents an aluminum atom, a titanium atom, a silicon atom or a boron atom; m represents 1 or 2; n represents a positive integer of 1 to 100; R 1 , R 2 and R 3 each independently represents a C1-16 alkyl group optionally substituted by one or more fluorine atoms, or a C2-17 acyl group optionally substituted by one or more fluorine atoms, and when multiple R 3 exist that correspond to several R 3 may be the same or different from each other; wherein a part of the carbon atoms constituting the C1-16 alkyl group optionally substituted with one or more fluorine atoms may be replaced by one or more oxygen atoms, and a part of the carbon atoms constituting the C2-17 acyl group optionally substituted with one or more fluorine atoms may be replaced by one or more oxygen atoms; and the proportion of the total number of fluorine atoms in R 1 , R 2 and R 3 15% or more, relative to the total number of fluorine atoms and hydrogen atoms in R 1 , R 2 and R 3 , and if at least one of R 1 , R 2 and R 3 is an acyl group substituted by one or more fluorine atoms, at least another one from R 1 , R 2 and R 3 is an alkyl group substituted by one or more fluorine atoms.

[0009] The amount of water trapped per unit volume of the compound represented by formula (1) is high, and the compound exhibits excellent water-trap properties. In addition, because the compound contains fluorine atoms in a predetermined proportion, whose compatibility with an organic layer is low, it becomes possible to suppress their penetration into the organic layer when used as a desiccant. Furthermore, because the compound represented by formula (1) exhibits excellent light transmittance and does not crack or cloud after water trap, the compound can be suitably applied to top-emission type organic EL elements that extract light from a sealing substrate side, as described below.

[0010] The present invention also provides a desiccant containing a compound represented by formula (1). It is preferred that the desiccant further contains a viscosity modifier.

[0011] The present invention provides a sealing structure wherein a pair of substrates are sealed with a sealing agent, and wherein the sealing structure comprises the desiccant therein.

[0012] The present invention also provides an organic EL element comprising an element substrate, a sealing substrate disposed opposite to the element substrate, a laminate disposed on the element substrate and comprising an organic layer sandwiched between a pair of electrodes, and a sealing agent sealing the outer peripheral parts of the element substrate and the sealing substrate, wherein a sealed space of the organic EL element is filled with the desiccant.

[0013] According to the present invention, there can be provided a compound which is excellent in water occlusion properties and which can suppress its penetration into an organic layer when used as a desiccant, as well as a desiccant, a sealing structure and an organic EL element in which this compound is used. BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1 is a schematic cross-sectional view illustrating the structure of an organic EL element according to an embodiment of the present invention; Fig. 2 is a schematic cross-sectional view illustrating a method for manufacturing the organic EL element according to an embodiment of the present invention; and Fig. Figure 3 is a graph showing the relationship between the elapsed time and the dissolution distance of the organic layer in a storage test in an environment of 85°C. DETAILED DESCRIPTION

[0014] An embodiment of the present invention will be described below, but the present invention should not be limited thereto. [Connection]

[0015] The compound according to the present embodiment is a compound represented by formula (1).

[0016] In the formula (1), M represents an aluminum atom, a titanium atom, a silicon atom or a boron atom, and it is preferable that M is an aluminum atom.

[0017] In formula (1) m represents the number of OR 3 -groups in M ​​and denotes 1 or 2. When M is an aluminum atom or a boron atom, m is 1, and when M is a titanium atom or a silicon atom, m is 2.

[0018] In the formula (1), n ​​represents the number of M in a molecule and denotes a positive integer from 1 to 100. It is preferable that n is from 1 to 10, and it is particularly preferable that n is 1.

[0019] In formula (1), R 1 , R 2 and R 3each independently represents a C1-16 alkyl group optionally substituted by one or more fluorine atoms, or a C2-17 acyl group optionally substituted by one or more fluorine atoms, with a linear or branched C1-12 alkyl group substituted by one or more fluorine atoms or a linear or branched C2-13 acyl group substituted by one or more fluorine atoms being preferred, and a linear or branched C2-8 alkyl group substituted by one or more fluorine atoms being more preferred. When multiple R 3 present, the multiple R 3 be the same or different from each other.

[0020] Examples of the C1-16 alkyl group include linear, branched, or cyclic alkyl groups, and specifically, they include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a sec-pentyl group, a neopentyl group, an n-hexyl group, a cyclohexyl group, an n-heptyl group, an n-octyl group, a nonyl group, a decanyl group, a dodecanyl group, a tetradecanyl group, and a hexadecanyl group.

[0021] The C1-16 alkyl group optionally substituted with one or more fluorine atoms refers to a C1-16 alkyl group and a C1-16 alkyl group in which any hydrogen atom is replaced by one or more fluorine atoms. In the C1-16 alkyl group substituted with one or more fluorine atoms, all of the hydrogen atoms may be replaced by fluorine atoms, and only a portion of the hydrogen atoms may be replaced by fluorine atoms. When only a portion of the hydrogen atoms are replaced by fluorine atoms, it is preferable that the hydrogen atoms at the terminal carbon atom in the alkyl group are all replaced by fluorine atoms.

[0022] Examples of the C1-16 alkyl group substituted with one or more fluorine atoms include a difluoromethyl group, a trifluoromethyl group, a 2,2-difluoroethyl group, a 2,2,2-trifluoroethyl group, a 3,3,3-trifluoropropyl group, a heptafluoropropyl group, a 3,3,4,4,5,5,6,6,6-nonafluorohexyl group, and a 2,2,3,3,4,4,5,5,6,6,7,7,7-tridecafluoroheptyl group. The proportion of fluorine atoms in the alkyl group substituted with one or more fluorine atoms is not particularly limited, but is preferably 40% or more, more preferably 50% or more, and further preferably 60% or more, relative to the total number of fluorine atoms and hydrogen atoms in the alkyl group substituted with one or more fluorine atoms.

[0023] The C2-17 acyl group, optionally substituted with one or more fluorine atoms, denotes a group represented by R 4 -CO-represented group. Herein, R denotes 4a C1-16 alkyl group optionally substituted with one or more fluorine atoms. Examples of the C1-16 alkyl group optionally substituted with one or more fluorine atoms in R 4 include those similar to the C1-16 alkyl group optionally substituted with one or more fluorine atoms in R 1 , R 2 and R 3 .

[0024] A portion of the carbon atoms constituting the C1-16 alkyl group, optionally substituted with one or more fluorine atoms, may be replaced by one or more oxygen atoms. Examples of the alkyl group optionally substituted with such an oxygen group include a trifluoromethoxymethyl (CF3OCH2) group, a CF3OCF2CF2OCF2CH2 group, a CF3O(CF2CF2O)2CF2CH2 group, a CF3CF2CF2CF2OCF2CF2OCF2CH2 group, and a CF3CF2CF2CF2O(CF2CF2O)2CF2CH2 group. Alternatively, a portion of the carbon atoms constituting the C2-17 acyl group, optionally substituted with one or more fluorine atoms, may be replaced by one or more oxygen atoms. Examples of the acyl group optionally substituted with one or more oxygen atoms include that having a group similar to an alkyl group optionally substituted with one or more oxygen atoms as R 4The number of carbon atoms to be replaced by one or more oxygen atoms can be, for example, from 0 to 5, preferably 0 or 1. If a plurality of the carbon atoms are replaced by one or more oxygen atoms, it is preferred that the oxygen atoms are not adjacent to one another.

[0025] In formula (1), the proportion of the total number of fluorine atoms in R 1 , R 2 and R 3 15% or more, relative to the total number of fluorine atoms and hydrogen atoms in R 1 , R 2 and R 3 . The proportion of the total number of fluorine atoms in R 1 , R 2 and R 3 is preferably 30% or more, more preferably 40% or more, and further preferably 50% or more, relative to the total number of fluorine atoms and hydrogen atoms in R 1 , R 2 and R 3. Note that the hydrogen atoms in the alkyl group or the acyl group in R 1 , R 2 and R 3 all of which can be replaced by one or more fluorine atoms.

[0026] If at least one of R 1 , R 2 and R 3 in formula (1) is an acyl group substituted by one or more fluorine atoms, at least one other of R 1 , R 2 and R 3 an alkyl group substituted by one or more fluorine atoms.

[0027] The compound represented by formula (1) can form an association compound of the compounds represented by formula (1).

[0028] Suitable specific examples of the compound represented by formula (1) include compounds represented by formulas (1A), (1B), (1C), (1D) and (1E) shown below. wherein R arepresents a 2,2,3,3,4,4,5,5,6,6,7,7,7-tridecafluoroheptyl group, R b represents a 2,2,2-trifluoroethyl group, R c represents a heptafluorobutanoyl group, R d represents a sec-butyl group and R e represents an isopropyl group.

[0029] Note that the proportions of the total number of fluorine atoms in the compounds represented by formulas (1A), (1B), (1C), (1D) and (1E) are 87%, 60%, 28%, 16% and 87%, respectively, relative to the total number of fluorine atoms and hydrogen atoms.

[0030] According to the compounds represented by formula (1), it is possible that the amount of enclosed water per unit volume is, for example, more than 70 mg / cm 3 is preferably 80 mg / cm 3 or more. [Method for making the connection]

[0031] It is possible to obtain the compound represented by formula (1) by allowing, for example, a compound having M, or a simple substance of M, to react with an alcohol having R 1 , R 2 or R 3 or with a carboxylic acid which R 4 Herein, the alcohol and the carboxylic acid correspond to the C1-16 alkyl group optionally substituted with one or more fluorine atoms and the C2-17 acyl group optionally substituted with one or more fluorine atoms, respectively, in the formula (1).

[0032] When M is an aluminum atom, examples of the compound having M include aluminum tri-n-butoxide, aluminum tri-sec-butoxide, aluminum tri-tert-butoxide, aluminum tri-n-octoxide, aluminum tri-sec-octoxide, aluminum tri-n-dodecoxide, aluminum tri-sec-dodecoxide, aluminum trihydride, and lithium aluminum tetrahydride. When M is a titanium atom, examples of the compound having M include titanium tetra-n-butoxide, titanium tetra-sec-butoxide, titanium tetra-tert-butoxide, titanium tetra-n-octoxide, titanium tetra-sec-octoxide, titanium tetra-n-dodecoxide, titanium tetra-sec-dodecoxide, and titanium tetrahydride. When M is silicon, examples of the compound having M include tetra-n-butoxysilane, tetra-sec-butoxysilane, tetra-tert-butoxysilane, tetra-n-octoxysilane, tetra-sec-octoxysilane, tetra-n-dodecoxysilane, tetra-sec-dodecoxysilane, and silane.When M is a boron atom, examples of the compound having M include tri-n-butylborate, tri-sec-butylborate, tri-tert-butylborate, tri-n-octoxide borate, tri-sec-octoxide borate, tri-n-dodecoxide borate, tri-sec-dodecoxide borate, sodium tetrahydroborate, and diborane.

[0033] Examples of alcohol, R 1 , R 2 or R 3 specifically include methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, sec-butyl alcohol, tert-butyl alcohol, n-pentyl alcohol, isopentyl alcohol, sec-pentyl alcohol, neopentyl alcohol, n-hexyl alcohol, cyclohexanol, n-heptyl alcohol, n-octyl alcohol, nonyl alcohol, decanyl alcohol, tetradecanyl alcohol, hexadecanyl alcohol, difluoromethanol, trifluoromethanol, 2,2-difluoro-1-ethanol, 2,2,2-trifluoro-1-ethanol, 3,3,3-trifluoro-1-propanol, 3,3,4,4,5,5,6,6,6-nonafluoro-1-hexanol and 2,2,3,3,4,4,5,5,6,6,7,7,7-tridecafluoro-1-heptanol.

[0034] The carboxylic acid, the R 4is a function defined by R 4 COOH represented carboxylic acid. Examples of carboxylic acids that R 4 include those obtained by replacing a hydroxyl group in an alcohol identified above as the alcohol having R 1 , R 2 or R 3 is mentioned as an example, are formed by a carboxyl group.

[0035] Compounds containing M or simple compounds of M, alcohols with R 1 , R 2 or R 3 or carboxylic acids with R 4 can be used individually, or can be used in combination of two or more, but it is preferable to use them individually.

[0036] The relationship when a compound having M or a simple substance of M with an alcohol having R 1 , R 2 or R 3 or with a carboxylic acid which R 4reacts, may contain at least 3 mol or more of the alcohol containing R 1 , R 2 or R 3 or the carboxylic acid which R 4 with respect to 1 mol of the compound having M or the simple substance of M, however, it is preferably possible to make it the alcohol having R 1 , R 2 or R 3 or the carboxylic acid which R 4 to be present in an amount of 3 to 9 mol.

[0037] Apart from the compounds that have M, the simple substance of M, the alcohols that have R 1 , R 2 or R 3 or the carboxylic acids, which R 4 a diol or dicarboxylic acid can be mixed in an arbitrary ratio to allow them to react as one component.

[0038] Examples of the diol herein include those obtained by replacing one of the hydrogen atoms on the carbon atoms of the alcohol, R 1 , R 2 or R 3 by a hydroxyl group. Examples of dicarboxylic acids include those formed by replacing two hydroxyl groups in a diol with carboxyl groups.

[0039] The reaction conditions can be selected as appropriate depending on the starting materials used, but it is preferable to conduct heating and stirring in the absence or presence of a solvent at 40 to 150°C for 0.5 to 48 hours. Additionally, it is possible to distill off the volatile components under reduced pressure after the reaction is completed. [desiccant]

[0040] The desiccant of the present embodiment contains a compound represented by formula (1).

[0041] It is preferable that the desiccant of the present embodiment further contains a viscosity modifier. By allowing the viscosity modifier to be included, the viscosity of the desiccant can be modified, thereby facilitating the filling of the desiccant into the sealing structure.

[0042] Examples of the viscosity modifier include, as silicones, dimethyl silicones, methylphenyl silicones, alkyl-modified silicones, polyether-modified silicones, and fluorosilicones. It is preferable to use a fluorosilicone. Alternatively, a perfluoropolyether can be used as the viscosity modifier.

[0043] The proportion of the viscosity modifier contained can be, for example, from 0.05 to 20 times, based on the mass of the compound represented by formula (1).

[0044] The desiccant of the present embodiment may contain components other than the compound represented by formula (1) and the viscosity modifier, as long as the effects according to the present application are not impaired. Examples of other components include conventionally known desiccants, for example, chemical adsorbents such as calcium oxide and physical adsorbents such as zeolites and silica gel.

[0045] It is possible to introduce the desiccant of the present embodiment to the target by a dispense application method, a one-drop-fill (ODF) method, a screen printing method, a spraying method, a hot-melt method, and the like. When a dispense application method is employed, the viscosity of the desiccant is preferably from 1 to 5,000 Pa·s, more preferably from 1 to 1,000 Pa·s, and more preferably from 1 to 300 Pa·s. Alternatively, in the case of employing an ODF method, the viscosity of the desiccant is preferably from 0.1 to 1 Pa·s.

[0046] Since the desiccant of the present embodiment comprises the compound represented by formula (1) containing fluorine atoms in a predetermined proportion whose compatibility with an organic layer is low, it becomes possible to suppress its penetration into the organic layer. [Sealing structure]

[0047] The sealing structure of the present embodiment is a sealing structure in which a pair of substrates are sealed with a sealing agent, and the sealing structure includes the desiccant in the sealing structure. The desiccant can be applied to a part of a sealed space, for example, only to a predetermined area on the substrates, or can fill the sealed space.

[0048] The sealing structure of the present embodiment can be particularly suitably used when sealing a moisture-sensitive device. Examples of such a device include organic electronic devices such as organic EL elements, organic semiconductors, and organic solar cells. [Organic EL element]

[0049] With reference to Fig. 1, an embodiment of the organic EL element according to the present invention will be described below.

[0050] An organic EL element (1) of the present embodiment is an organic EL element of a filled sealing structure composed of an element substrate (2), a sealing substrate (3) disposed opposite to the element substrate (2), a laminate disposed on the element substrate (2) and including an organic layer (4) sandwiched between a pair of electrodes (5) and (6), a sealing agent (8) that seals outer peripheral parts of the element substrate (2) and the sealing substrate (3), and a filler (7) that fills the sealed space. The filler (7) is the desiccant of the present embodiment described above.

[0051] In the organic EL element (1), conventionally known components can be used as components other than the filler (7), and an example thereof will be briefly described below.

[0052] The element substrate (2) is constructed of a rectangular glass substrate having insulating properties and light transmittance, and an anode (electrode) (5) made of indium tin oxide (ITO), a transparent, electrically conductive material, is formed on this element substrate (2). This anode (5) is formed by patterning an ITO film deposited on the element substrate (2) by a physical vapor deposition (PVD) method such as a vacuum deposition method and a sputtering method into a predetermined pattern shape by etching according to a photoresist method. A part of the anode (5) as an electrode is connected to a drive circuit (not shown) protruding from one end of the element substrate (2).

[0053] On the top surface of the anode (5), an organic layer (4), which is a thin film containing an organic light-emitting material, is laminated by a PVD method such as a vacuum deposition method and a resistance heating method. The organic layer (4) may be formed of a single layer or may be formed of a plurality of layers having different functions. The organic layer (4) in the present embodiment is a four-layer structure in which a hole-injection layer (4a), a hole-transport layer (4b), a light-emitting layer (4c), and an electron-transport layer (4d) are sequentially laminated from the anode (5) side. The hole-injection layer (4a) is formed, for example, of copper phthalocyanine (CuPc) with a film thickness of several tens of nanometers. The hole-transport layer (4b) is, for example,from bis[N-(1-naphthyl)-N-phenyl]benzidine (α-NPD) with a film thickness of several tens of nanometers. The light-emitting layer (4c) is formed, for example, from tris(8-quinolinato)aluminum (Alq3) with a film thickness of several tens of nanometers. The electron-transport layer (4d) is formed, for example, from lithium fluoride (LiF) with a film thickness of several nanometers. Then, a light-emitting region was formed from the laminate in which the anode (5), the organic layer (4), and the cathode (6), described below, were laminated in this order.

[0054] On the top surface of the organic layer (electron transport layer (4d)), a cathode (electrode) (6) is laminated, which is a thin metal film, by a PVD method such as a vacuum deposition method. Examples of the thin metal film include simple substances made of metals whose exit function is low, such as Al, Li, Mg, and In, and alloys whose exit function is small, such as Al-Li and Mg-Ag. The cathode (6) is formed with a film thickness of several tens of nanometers to several hundred nanometers (preferably from 50 nm to 200 nm). A part of the cathode (6) protrudes from one end of the element substrate (2) and is connected to the drive circuit (not shown).

[0055] The sealing substrate (3) is arranged in such a manner as to oppose the element substrate (2) with the organic layer (4) interposed therebetween, and the periphery of the element substrate (2) and the sealing substrate (3) are sealed with a sealant (8). A UV-curing resin can be used as the sealant. In addition, a filler (7), which is the desiccant of the present embodiment, is filled into the sealed space. This protects the organic layer (4) and the like.

[0056] Note that although the organic EL element is a bottom-emission type organic EL element that extracts light from the element substrate side, the organic EL element of the present invention may be a top-emission type organic EL element that extracts light from the sealing substrate side. Top-emission type organic EL elements can also be manufactured by conventionally known methods, but modifications are required, such as using a transparent electrode as the cathode (6) or exchanging the positions of the anode (5) and the cathode (6), in addition to using a substrate having translucent properties as the sealing substrate (3).Because the desiccant of the present embodiment has excellent light transmittance and does not crack or cloud after water is trapped, it can be particularly suitably used in organic EL elements of this top emission type. [Method for manufacturing the organic EL element]

[0057] Now, with reference to Fig. 2, a method for manufacturing the organic EL element, particularly a sealing process, is described below.

[0058] First, a laminate is provided in which an organic layer (4) and the like (electrodes are not shown) are laminated on an element substrate (2) ( Fig. 2(a)).

[0059] Subsequently, the desiccant of the present embodiment is applied to a separately provided sealing substrate (3) in a volume that can be filled into a space to be sealed, using a dosing device. Furthermore, a sealing agent (8) is applied using a dosing device to enclose the desiccant applied to the sealing substrate (3). Fig. 2(b)). It is preferable to perform these two operations in a nitrogen-purged glove box with a dew point of -76°C or less.

[0060] Subsequently, the element substrate (2) on which the organic layer (4) and the like are laminated and the sealing substrate (3) are bonded together ( Fig. 2(c)). An organic EL element of the present embodiment is manufactured by sealing the bonded substrates with UV irradiation and heating at about 80°C ( Fig. 2(d)). EXAMPLES

[0061] The present invention will now be described more specifically with reference to examples. However, the present invention should not be limited to these examples.

[0062] Note that in the examples, the viscosity, water entrapment capacity, and the amount of water entrapped per unit volume were measured according to the following methods. (Viscosity)

[0063] A HBDV-E type digital viscometer manufactured by Brookfield Inc. was used to measure the viscosity at 25°C. (Water containment capacity and amount of water contained per unit volume)

[0064] A sample was added to hydrous ethanol, whose water content was 5% by mass, so that the sample concentration was 10% by mass. After stirring for 1 minute, centrifugation was performed under conditions of 2,000 rpm for 10 minutes. Using a moisture meter based on the Karl Fischer method (CA-100, VA-100: evaporation method), the change in the water content of the ethanol after centrifugation was calculated as the amount of entrained water, and the water entrainment capacity and the amount of water entrained per unit volume were calculated according to the following formulas. Water inclusion capacity [wt.%] = enclosed amount of water [mg] / amount of sample [mg] × 100 Amount of enclosed water per unit volume [mg / cm3] = Amount of enclosed water [mg] / Sample volume [cm3] Sample volume[cm3]=sample quantity[g] / sample density[g / cm3] [Establishment of the connection](Example 1-1)

[0065] To an egg-shaped flask, 31.4 g (0.127 mol) of aluminum tri-sec-butoxide and 147.4 g (0.421 mol) of 1H,1H-tridecafluoro-1-heptanol-(2,2,3,3,4,4,5,5,6,6,7,7,7-tridecafluoro-1-heptanol) were added and stirred while heating at 100°C for one hour. By distilling off the volatile components under reduced pressure at 150°C and 500 Pa, 116 g of a liquid compound were obtained. The viscosity of the obtained compound was 15 Pa s and the water inclusion capacity was 5 wt.%. In addition, the density of the obtained compound was 1.8 g / cm . 3 , and the amount of water enclosed per unit volume was 90 mg / cm 3 . (Example 1-2)

[0066] 12.1 g (0.05 mol) of aluminum tri-sec-butoxide and 10.5 g (0.05 mol) of heptafluorobutyrate were added to an egg-shaped flask and stirred while heating at 100°C for one hour. Distilling off the volatile components under reduced pressure at 150°C and 300 Pa yielded 16.1 g of a white solid compound. (Example 1-3)

[0067] To an egg-shaped flask, 52.9 g (0.21 mol) of aluminum tri-sec-butoxide, 247 g (0.711 mol) of 1H,1H, tridecafluoro-1-heptanol-(2,2,3,3,4,4,5,5,6,6,7,7,7-tridecafluoro-1-heptanol), and 1.53 g (0.09 mol) of water were added and stirred while heating at 100°C for one hour. By distilling off the volatile components under reduced pressure at 150°C and 280 Pa, 159 g of a liquid compound were obtained.

[0651] [Preparation of the desiccant] (Comparative Example 1)

[0068] A 48% solution of alumina octylate oligomer, an organic aluminum compound (product name: Olipe AOO, manufactured by Hope Chemical Co., Ltd.), and silicone (dimethylsilicone, product name: TSF451-100, manufactured by Momentive Performance Materials Japan LLC) was used. These were weighed so that the amount of organic aluminum compound was 85% by mass and the amount of silicone was 15% by mass, and they were mixed and stirred in an egg-shaped flask. A desiccant was obtained by distilling off the volatile components under reduced pressure. The density of the desiccant was 1.0 g / cm³. 3 , the water inclusion capacity was 7 wt.%, and the amount of water enclosed per unit volume was 70 mg / cm 3 . [Storage test at an environment of 85°C](Example 2)

[0069] First, an anode made of Ito as an electrically conductive material having transparency was deposited on an element substrate in a film thickness of 140 nm by a sputtering method and further patterned into a predetermined pattern shape by etching according to a photoresist method to thereby form an anode.

[0070] Subsequently, copper phthalocyanine (CuPc) was formed as a hole-injection layer with a film thickness of 70 nm on the top surface of the anode by a resistance heating method. Bis[N-(1-naphthyl)-N-phenyl]benzidine (α-NPD) was deposited as a hole-transport layer with a film thickness of 30 nm on the top surface of the hole-injection layer. Tris(8-quinolinato)aluminum (Alq3) was deposited as a light-emitting layer with a film thickness of 50 nm on the top surface of the hole-transport layer. Furthermore, lithium fluoride (LiF) was deposited as an electron-transport layer with a film thickness of 7 nm on the top surface of the light-emitting layer. Furthermore, aluminum was physically vapor-deposited as a cathode with a film thickness of 150 nm.

[0071] Subsequently, in a nitrogen-purged glove box with a dew point of -76°C or less, the compound of Example 1-1 was applied as a desiccant to the sealing substrate using a dispensing device in a pre-measured volume that could be filled into a container. A sealing agent composed of a UV-curing resin was then applied using a dispensing device to enclose the desiccant filled into the sealing substrate.

[0072] Then, the element substrate on which the anode, the organic layer, and the cathode were laminated and the sealing substrate were bonded, and then sealed by UV irradiation and heating at 80°C, thereby obtaining an organic EL element with a filled sealing structure in which an airtight container was filled with the desiccant (the compound of Example 1-1). A hole was formed on the cathode of the organic EL element with a laser, which was left under conditions of 85°C, and the dissolution distance of the organic layer was observed with an optical microscope. Note that the dissolution distance represents a distance from the center of the hole to the end of a part where dissolution of the organic layer occurred. (Comparison example 2)

[0073] An organic EL element was obtained in the same manner as in Example 2, except that the desiccant of Comparative Example 1 was used instead of the compound of Example 1-1. A hole was formed on the cathode of the organic EL element with a laser, which was left under conditions of 85°C, and the dissolution distance of the organic layer was observed with an optical microscope.

[0074] The relationship between the elapsed time and the dissolution distance of the organic layer in the storage test in an environment of 85°C is shown in Fig. 3. The white circle indicates the dissolution distance when the compound of Example 1-1 was used as the desiccant. The black square indicates the dissolution distance when the desiccant of Comparative Example was used. Fig.3, it was found that the dissolution distance was smaller and thus the penetration into the organic layer was more suppressed when the compound of Example 1-1 was used than in the case where the desiccant of Comparative Example 1 was used. LIST OF REFERENCE SYMBOLS

[0075] 1 - organic EL element, 2 - element substrate, 3 - sealing substrate, 4 - organic layer, 4a - hole injection layer, 4b - hole transport layer, 4c - light emitting layer, 4d - electron transport layer, 5 - anode, 6 - cathode, 7 - filler, 8 - sealant.

Claims

[1] Compound represented by the formula (1): wherein M represents an aluminum atom, a titanium atom, a silicon atom or a boron atom; m represents 1 or 2; n represents a positive integer from 1 to 100; R 1 , R 2 and R 3 each independently represents a C1-16 alkyl group optionally substituted by one or more fluorine atoms, or a C2-17 acyl group optionally substituted by one or more fluorine atoms, and when multiple R 3 exist that correspond to several R 3 may be the same or different from each other; wherein a part of the carbon atoms constituting the C1-16 alkyl group optionally substituted with one or more fluorine atoms may be replaced by one or more oxygen atoms, and wherein a part of the carbon atoms constituting the C2-17 acyl group optionally substituted with one or more fluorine atoms may be replaced by one or more oxygen atoms; and where the proportion of the total number of fluorine atoms in R 1 , R 2 and R 3 15% or more, relative to the total number of fluorine atoms and hydrogen atoms in R 1 , R 2 and R 3 , and wherein in the case wherein at least one of R 1 , R 2 and R 3 is an acyl group substituted by one or more fluorine atoms, at least one other of R 1 , R 2 and R 3 is an alkyl group substituted by one or more fluorine atoms. [2] A compound according to claim 1, wherein m is an aluminum atom. [3] A compound according to claim 1 or 2, wherein R 1 , R 2 and R 3 a C2-8 alkyl group substituted by one or more fluorine atoms. [4] A desiccant comprising the compound according to any one of claims 1 to 3. [5] Desiccant according to claim 4, further comprising a viscosity modifier. [6] Sealing structure, wherein two substrates (2, 3) are sealed with a sealing agent (8), and wherein the sealing structure comprises the desiccant according to claim 4 or 5 herein. [7] Organic EL element (1) comprising: an element substrate (2); a sealing substrate (3) arranged opposite the element substrate (2); a laminate disposed on the element substrate (2) and comprising an organic layer sandwiched between a pair of electrodes (5, 6); and a sealing means (8) which seals the outer peripheral parts of the element substrate (2) and the sealing substrate (3); wherein a sealed space is filled with the desiccant (8) according to claim 4 or 5.

Citation Information

Patent Citations

  • Sealing method for organic el element and organic el element

    JP1997035868A

  • Desiccant and organic el element using the same

    JP2013176751A

  • Desiccant and electroluminescent element using the desiccant

    DE102013100956A1