Sealing system, in particular for insert hoses, insert hose and method for manufacturing an insert hose, as well as method for lining a pipe with an insert hose and use of a sealing tape for manufacturing an insert hose.
The sealing system for resin-impregnated carrier systems in trenchless sewer renovation uses a sealing tape with a resin-absorbing first layer and thermally activated polymer second layer to form a seal during resin curing, addressing complexity and cost issues, achieving high tightness and stability with minimal resin leakage.
Patent Information
- Application Number
- DE102016120225
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2016-10-24
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2036-10-24
AI Technical Summary
Existing sealing systems for resin-impregnated carrier systems in trenchless sewer renovation are complex, costly, and prone to resin and solvent leakage, with high demands for tightness and stability, especially during high-pressure cleaning, and existing solutions fail to effectively prevent resin and solvent leakage while maintaining ease of handling and cost-effectiveness.
A sealing system comprising a hose with a resin/support system and a sealing tape having a first outer layer that absorbs resin and a second outer layer with a thermally activated polymer, which bonds to the first layer during resin curing, forming a seal against gases, liquids, and resin, without significant resin involvement at overlapping winding areas.
The system achieves pressure drops of less than 5 mbar, meeting DIN EN 1610 standards, ensuring high tightness and stability with reduced complexity and cost, and preventing resin and solvent leakage, while maintaining ease of handling and production cleanliness.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The present invention relates to a sealing system for resin-impregnated, curable support systems, i.e., resin / support systems. After the resin / support system has cured, the penetration of liquids, gases, and other substances in particular should be prevented. The system should therefore be leak-tight. Such a sealing system is typically part of an insert hose (also called a lining hose or pipe liner) in trenchless sewer rehabilitation. Furthermore, the invention relates to an insert hose with such a sealing system and a method for producing an insert hose.
[0002] Such sealing systems and methods for producing such sealing systems are known, inter alia, from WO 00 / 73692 A1 and DE 10 2014 111 427 A1.
[0003] In the glass fiber hose liner system with UV or steam curing, such an insert hose typically comprises an outer hose (outer hose film) constructed as a tubular film and an inner hose (inner hose film) constructed as a tubular film, between which a carrier material, such as glass fibers, is inserted, which is impregnated with reactive plastic resin. Examples of reactive plastic resins used include commercially available UP resins (polyester or unsaturated polyester resins), VE resins (vinyl ester resins), or EP resins (epoxy resins). In this context, such a combination of carrier material and resin is referred to as a resin / carrier system. The curing of the resins, for example, occurs with the aid of photoinitiators in the case of UP or VE resins. However, curing can also occur thermally.The insert tube is inflated from the inside of the pipe by compressed air directed against the mechanically stable inner tube film until the outer tube film rests against the inner pipe wall or the sliding film. The resin is then cured – for example, using UV light from a UV light source slowly drawn through the interior of the inflated insert tube. Finally, the inner tube film of the insert tube is peeled off and removed. Alternatively, the inner tube film remains in the duct.
[0004] WO 95 / 04646 A1 describes the production of such an insert tube. A film strip is wound helically around a winding mandrel, forming an inner film tube that serves as a protective film. At least one resin-impregnated fiber tape is wound diagonally or helically onto this, and a second film strip is wound onto this, forming an outer tube film. Instead of a wound inner tube film, a pre-extruded inner tube film can also be used, onto which the resin-impregnated fiber tapes are then wound helically.
[0005] EP 1180225 A1 describes corresponding insert hoses with improved strength, in which the hose outer film has a reinforcement in the form of a nonwoven layer on the side facing the resin-impregnated fiber bands.
[0006] In general, the rehabilitation of fluid-carrying systems with in-line hoses is intended to prevent resin or solvents contained in the resin from escaping from the inside of the in-line hose, as these would then contaminate the flowing media. For the same environmental reasons, the leakage of resin and solvents from the pipe walls should be prevented. It also goes without saying that the media flowing within the pipe itself must not escape into the environment. Therefore, in-line hoses are subject to particularly stringent requirements in terms of tightness and stability (even during high-pressure cleaning of the pipe).
[0007] DE 10 2013 111 094 A1 discloses an insert hose in which a film having reinforcement on both sides is provided between the at least one inner film hose and the at least one resin-impregnated fiber tape. The reinforcement on the side facing the resin-impregnated fiber tape allows the resin to be absorbed by the reinforcement and to bond with the reinforcement as the resin hardens. In this way, the insert hose is sealed against, for example, resin penetration or liquids and gases reaching the pipe interior (i.e. coming from the outside) or the sewer wall or the soil (i.e. coming from the internal medium running through the interior of the rehabilitated sewer). The second reinforcement on the side facing away from the resin-impregnated fiber tape (and facing the inner film of the hose) is also used to seal against the medium flowing in the rehabilitated pipe.For this purpose, this second reinforcement can also be impregnated with resin, for example, allowing the resin to bond with the inner tube film if the latter is to remain in the duct. Furthermore, impregnating both sides of the reinforced film (e.g., in the form of a film laminated with nonwoven fabric on both sides) with resin during wrapping can create a seal, as the resins rest on each other in the overlapping areas and can bond together during curing.
[0008] Overall, according to DE 10 2013 111 094 A1, the tightness of the insert tube should be improved against the penetration of resin, liquids, gases, or other substances. However, this insert tube has a relatively complex design. In particular, the double-sided reinforcement with resin impregnation on both sides (similar to a plaster cast, where the plaster is previously treated with water) is very complex and costly. Handling is also cumbersome and leads to considerable soiling of the production facility because the resin drips onto the floor. Since both sides of the double-sided reinforced film are impregnated with resin, a significant amount of excess resin is squeezed out of the overlapping areas during wrapping, which is very disadvantageous because it can lead to resin contamination.
[0009] The object of the present invention is to further improve the tightness of a sealing system against resin penetration and against gases and liquids or other substances while at the same time being low cost and easy to handle.
[0010] The object is achieved by a sealing system according to claims 1 to 13, an insert tube according to claims 14 to 16, a method for producing an insert tube according to claims 17 and 18, a method for lining a pipe with an insert tube according to claim 19 and use of a sealing tape for producing an insert tube according to claim 20.
[0011] The sealing system according to the invention comprises at least one tubular resin / carrier system and at least one helically wound sealing tape with overlapping regions, which seals against the resin / carrier system. The sealing tape comprises a first outer layer capable of absorbing resin, and a second outer layer comprising at least one thermally activatable polymer. The second outer layer bonds to the first outer layer in overlapping winding regions through thermal activation of the at least one polymer in the range of 60° to 120°C, forming a seal against gases, liquids, and resin. In other words, in contrast to DE 10 2013 111 094 A1, the sealing in the present invention is achieved in such a way that no resin is involved to any significant extent at the sealing points in the overlapping winding regions (at most at the edges of the overlapping winding regions).
[0012] If the first outer layer is directed towards the resin of the resin / carrier system, it can also absorb resin from the resin / carrier system and bond inseparably with this system during resin curing (for example, using a UV light source or thermal heat source). In the overlapping winding areas, however, the first outer layer does not lie against the resin / carrier system, but directly above or on the second outer layer of the previous winding of the sealing tape. Through thermal activation - triggered, for example, by the aforementioned UV light source or thermal heat source and the resulting exothermic reaction of the resin curing - the at least one polymer of the second outer layer can bond with the first outer layer and create a seal against gases, liquids and the resin.The heat generated during resin curing is conducted in particular to the first outer layer of the sealing tape, which lies directly against the resin, on its second outer layer, where the at least one polymer is thermally activated, which can then fuse with the first outer layer of the overlapping winding of the sealing tape.
[0013] Thus, if the first outer layer is directed towards the resin / carrier system, which is a preferred embodiment, the first outer layer can bond firmly and tightly both to the resin and - in the overlapping winding areas - to the thermally activatable polymer of the second outer layer.
[0014] It has been found that pressure drops of less than 5 mbar according to DIN EN 1610 (1997), Chapter 13.3, method LD (pressure drop) can be achieved using the sealing system according to the invention.
[0015] The first outer layer of the sealing tape is preferably a fleece, felt, woven fabric, scrim, or knitted fabric, each of which is capable of absorbing resin or liquids. Fleeces, also known as nonwovens, consist of fibers arranged randomly within the nonwoven fabric. The fibers of felts are intertwined in a random manner. Woven fabrics are generally made of at least two fiber systems arranged at right angles to each other. The threads of scrims are not woven together, but rather laid one upon the other and embedded in a matrix. Knitted fabrics, on the other hand, are created by stitching.
[0016] The basis weight of the first outer layer is preferably in the range of 5 to 5000 g / m 2 , more preferably in the range of 10 to 1000 g / m 2 , particularly preferably in the range of 20 to 500 g / m 2 and most preferably in the range of 30 to 250 g / m 2 .
[0017] The peak melting point of the at least one polymer or, in the case of an amorphous polymer, its Vicat softening point according to VST / A50 is preferably below 120°C, more preferably below 110°C and most preferably below 100°C.
[0018] The melting point of the at least one polymer or, in the case of an amorphous polymer, its Vicat softening point according to VST / A50 is preferably above 30°C, more preferably above 40°C, particularly preferably above 50°C and most preferably above 60°C.
[0019] In other words, the at least one thermally activatable polymer melts even at relatively low temperatures. In this case, the thermal energy generated during resin curing is sufficient to thermally activate the second outer layer, causing the overlapping winding areas of the sealing tape to adhere to each other and form a seal against the resin or against liquids, gases, and all other substances.
[0020] Preferably, the at least one thermally activatable polymer is selected from the group: a) Polyolefin plastomers (POP); b) Thermoplastic elastomers (TPE), such as polyolefin elastomers (POE); c) Ethylene homo- or copolymers, such as ethylene-acrylic acid copolymers (EAA copolymers), LDPE (low density polyethylene), LLDPE (linear low density polyethylene), mLLDPE (metallocene linear low density polyethylene).
[0021] The thermoplastic elastomers (TPE) can be selected from the following group: - TPE-U or TPU, i.e. thermoplastic elastomers based on urethane; - TPE-O or TPO, i.e. olefin-based thermoplastic elastomers, such as polyolefin elastomers (POE); - TPE-V or TPV, i.e. cross-linked thermoplastic elastomers based on olefins, mainly PP / EPDM; - TPE-E or TPC, i.e. thermoplastic polyester elastomers / thermoplastic copolyesters; - TPE-S or TPS, i.e. styrene block copolymers (SBS, SEBS, SEPS, SEEPS and MBS); - TPE-A or TPA, i.e. thermoplastic copolyamides; - TPE silicone.
[0022] According to a preferred embodiment, the second outer layer is an outer layer of a film. It is further preferred that this film is a mono- or multi-layer film, in this case preferably a 3-layer film or a 5-layer film. In a monolayer film, this also simultaneously represents said second outer layer. In a multi-layer structure, said outer layer of the film, which serves as the second outer layer of the sealing tape, contains said at least one thermally activatable polymer, for example a POP, TPE or an ethylene homo- or copolymer. A preferred 3-layer film has the layer structure PE (polyethylene) / HV (adhesion promoter) / PA (polyamide), while a preferred 5-layer film has the layer structure PE / HV / PA / HV / PE or PE / HV / PE / HV / PA.In this case, the thermally activatable polymer in said outer layer is advantageously a PE, for example a thermally activatable LDPE, LLDPE or mLLDPE (see above) according to the invention.
[0023] The said film preferably has a thickness of 5 µm to 5000 µm, more preferably of 10 µm to 3200 µm, and particularly preferably of 20 µm to 2000 µm.
[0024] According to a preferred embodiment, the first outer layer is laminated to said outer layer of the film containing the at least one thermally activatable polymer, preferably using the extrusion lamination process. If the first outer layer is, for example, a nonwoven, this can be readily laminated to said film.
[0025] According to an alternative embodiment, the second outer layer is formed by a coating or covering with the at least one thermally activatable polymer. This coating or covering is preferably applied to the first outer layer. This results in a simple and relatively thin sealing tape.
[0026] According to an alternative, the coating (as a second outer layer) is applied to a film, wherein the film can preferably be laminated against the first outer layer.
[0027] The basis weight of the at least one thermally activatable polymer in a coating is preferably in the range of 0.5 to 1000 g / m 2 , more preferably in the range of 2 to 500 g / m 2 , particularly preferably in the range of 5 to 200 g / m 2 and most preferably in the range of 10 to 100 g / m 2 .
[0028] According to a likewise preferred embodiment, one or more further layers are arranged between the first and second outer layer, for example in the form of polymer layers or films.
[0029] The invention also relates to an insert tube with an inner tube film and an outer tube film, wherein at least one sealing system as described above is arranged between the inner tube film and the outer tube film. In this embodiment, the sealing system is located inside the insert tube, whereby the sealing system according to the invention ensures that the resin escapes through the sealing tape – just as a seal against gases, liquids, and other substances is achieved after the resin has cured. It is possible for additional films or layers to be arranged at various points on the insert tube, for example, between the sealing system and the outer tube film.
[0030] The inner tube film, which is preferably UV-permeable, and the outer tube film, which is preferably substantially impermeable to UV radiation, can preferably be constructed according to the prior art, in particular as described in WO 2013 / 026568 A1. Furthermore, inner tube films and outer tube films suitable for the tube lining process are also described in EP 2 379 625 B1.
[0031] The resin / carrier system of the sealing system can be located at various points along the insert tube. Possible arrangements include the following: a) between said sealing tape and the inner tube film, the first outer layer of said sealing tape being in contact with the resin / carrier system; b) between said sealing tape and the inner tube film, the second outer layer of said sealing tape being in contact with the resin / carrier system; c) between said sealing tape and the outer tube film, the first outer layer of said sealing tape being in contact with the resin / carrier system; d) between said sealing tape and the outer tube film, wherein the second outer layer of said sealing tape is in contact with the resin / carrier system.
[0032] In arrangements according to a) and b), the resin / carrier system is located between the sealing tape and the inner tube film. In arrangements according to c) and d), the resin / carrier system is located between the sealing tape and the outer tube film.
[0033] In the arrangements according to a) and c), which are preferred in many cases over the arrangements according to b) and d), the first outer layer of the sealing tape rests against the resin / carrier system and can thus absorb resin from this resin / carrier system or become impregnated with resin. The second outer layer, containing the at least one thermally activatable polymer, bonds to the first outer layer of the sealing tape through the thermal activation of this polymer during the exothermic reaction of the resin curing in the overlapping winding areas, thus ensuring the desired seal according to the invention.
[0034] In the arrangements according to b) and d), the second outer layer of the sealing tape rests against the resin / carrier system. While the bond between the resin and the second outer layer and the at least one thermally activated polymer is not necessarily as good in this case as with the first outer layer formed as a nonwoven or similar material, it can certainly be achieved with the appropriate choice of material. Irrespective of this, the thermal activation of the at least one polymer during the exothermic reaction of the resin curing bonds the first and second outer layers of the sealing tape in the overlapping winding areas, ensuring the desired seal.
[0035] Particularly preferably, the at least one resin / carrier system is wound helically around the inner film of the tube, and the at least one sealing tape is wound helically around the resin / carrier system. Known winding techniques, in particular using a winding mandrel, can be used for this purpose.
[0036] The invention further relates to a method for producing an insert tube, in particular an insert tube as described above, comprising the following steps in this order: (a) providing a tubular inner film which is either wound, extruded in a tubular form or a flat film sealed into a tube; b) covering the inner film of the tube with a resin / carrier system impregnated with resin; c) helically and overlappingly wrapping the resin / carrier system with a sealing tape, said sealing tape comprising at least a first outer layer capable of absorbing or being impregnated with a portion of the resin of the resin / carrier system, and a second, thermally activatable outer layer, said second outer layer capable of sealingly bonding to the first outer layer (which then does not come into contact with the resin) in overlapping winding areas by thermal activation in the range of 60° to 120°C; and d) wrapping said inner tube film and said resin / carrier system as well as said sealing tape with a tube outer film, for example by means of helical and overlapping wrapping or in the form of a tube film consisting of one or more flat films joined together by sealing.
[0037] According to an alternative, the sealing tape is first wound helically onto the inner film of the hose and then the resin / carrier system.
[0038] The invention also relates to a method for lining a pipe, in particular in trenchless sewer rehabilitation, with an insert hose as described above, comprising the following steps in this order: a) the insert hose is pulled into the pipe, b) the insert hose is then widened so that it comes into contact with the inner wall of the pipe, and c) finally, the resin layer(s) is / are cured by means of a UV source moved through the pipe, whereby thermal energy is released, by means of which the second outer layer of the sealing system is thermally activated or melted in such a way that areas of this second outer layer bond with the overlapping areas of the first outer layer directly adjacent to them, created by the helical winding, so that a seal is obtained between these areas, which preferably complies with DIN EN 1610 (1997), Chapter 13.3, Method LD (pressure drop).
[0039] It should be noted that in this case the term “pipe” refers to all fluid-carrying systems with a closed cross-section, including channels and, in particular, channels or sewer pipes buried in the ground.
[0040] Accordingly, the invention also relates to a use of a sealing tape as described above with a first and a second outer layer for the production of an insert hose as described above or for the lining of a pipe as described above.
[0041] Further advantages of the invention are described in the following exemplary embodiments. They show: Fig. 1 a cross-section through an insert hose according to the invention, drawn into a sewer pipe, with a sealing system according to the invention; Fig. 2 a side view of a sealing system according to the invention with overlapping areas; Fig. 3 a section of a cross-section of the Fig. 1 shows the first embodiment of an insert hose according to the invention (with overlapping winding areas); Fig.4 shows a section of a cross section of a second embodiment of an insert tube according to the invention (with overlapping winding areas); Fig. 5 shows a section of a cross section of a third embodiment of an insert tube according to the invention (with overlapping winding areas); Fig. 6 shows a section of a cross section of a fourth embodiment of an insert tube according to the invention (with overlapping winding areas);
[0042] The Fig.1 shows a cross-section of a sewer pipe K to be renovated, into which a tubular preliner 20 made of sturdy plastic, known from the prior art, is inserted, which is in contact with the wall of the sewer pipe K. The preliner 20 provides mechanical protection for an insert hose 1, and on the other hand, the insert hose 1 can slide along the wall of the preliner 20 facing the inside of the pipe when being inserted into the sewer pipe K, which facilitates the insertion process. Fig.1, the preliner 20 surrounds the insert tube 1 (also called a tube liner or lining tube), which in this case comprises a - preferably substantially UV- and light-permeable - inner tube film 2, a resin / carrier system 11 containing resin 11b and, for example, glass fibers 11a as a carrier, and a preferably substantially UV- and light-tight outer tube film 3. The inner tube film 2, the resin / carrier system 11, and the outer tube film are known from the prior art and need not be explained in detail.
[0043] According to the invention, a sealing system 10 is provided with a sealing tape 12 and a resin / carrier system 11, wherein the sealing tape 12 according to the embodiment of the Fig. 1 is wound helically around the resin support system 11. In the Fig.2 shows a side view of the sealing system 10, wherein the flow direction of the liquid or gaseous medium carried by the pipe K is designated by f1. Fig. 2 shows that the sealing tape 12 is wound with an overlap, i.e., a straight layer is wound onto the previously wound layer with an overlap of approximately 50%. The invisible edges of the lower layers are shown in dashed lines for clarity. In this example, two layers of the sealing tape 12 are overlapped at each point.
[0044] Such an overlapping area 15 is also shown in the sectional view of the Fig. 1. Furthermore, it can be seen that the sealing strip 12 has a first outer layer 13 and a second outer layer 14. One or more inner layers can be provided between these two outer layers 13, 14, but this is by no means mandatory.
[0045] The first outer layer 13 is designed to absorb resin or liquids or to be impregnated with resin or liquids. For this purpose, the first outer layer 13 is designed, for example, as a nonwoven, felt, woven, scrim, or knitted fabric, each of which is capable of absorbing resin or liquids.
[0046] The basis weight of the first outer layer is preferably in the range of 5 to 5000 g / m², more preferably in the range of 10 to 1000 g / m², particularly preferably in the range of 20 to 500 g / m² and most preferably in the range of 30 to 250 g / m².
[0047] The second outer layer 14 contains at least one thermally activatable polymer. This polymer is capable of sealing the first outer layer 13 in the overlapping winding areas 15 through thermal activation in the range of 60°C to 120°C. The sealed overlapping winding areas 15 particularly preferably comply with DIN EN 1610 (1997), Chapter 13.3, Method LD (pressure drop). Experiments (see below) have shown that this can be easily achieved using the invention.
[0048] According to an advantageous embodiment, the second outer layer 14 represents a covering or coating of the first outer layer 13. According to a further advantageous embodiment, the second outer layer 14 is the outer layer of a film onto which the first outer layer 13 is laminated. The film thickness is, for example, in the range from 5 µm to 5000 µm, preferably in the range from 20 µm to 3200 µm.
[0049] In the case of a film, this can be a mono- or multi-layer film. In a monolayer film, this also simultaneously serves as said second outer layer 14. In a multi-layer structure, said outer layer of the film, which represents the second outer layer 14 of the sealing tape 12, contains said at least one thermally activatable polymer, for example a POP, TPE, or an ethylene homo- or copolymer. A multi-layer film is preferably a 3-layer film, preferably with the layer structure PE (polyethylene) / HV (adhesion promoter) / PA (polyamide), or a 5-layer film, preferably with the layer structure PE / HV / PA / HV / PE or PE / HV / PE / HV / PA. In these cases, the PE in an outer layer of the film, which serves as the second outer layer 14, can be said thermally activatable polymer, for example in the form of LDPE, LLDPE, or mLLDPE that can be thermally activated according to the invention.
[0050] The second outer layer 14 can of course also be a coating on a film, wherein this film is connected to the first outer layer, either directly (e.g. by lamination) or indirectly with the interposition of, for example, one or more further films.
[0051] The peak melting point of the at least one polymer or, in the case of an amorphous polymer, its Vicat softening point according to VST / A50, is on the one hand preferably below 120°C, more preferably below 110°C and most preferably below 100°C. On the other hand, the melting point of the at least one polymer or, in the case of an amorphous polymer, its Vicat softening point according to VST / A50, is preferably above 30°C, more preferably above 40°C, particularly preferably above 50°C and most preferably above 60°C.
[0052] The at least one polymer can be, in particular, a polyolefin plastomer (POP), a thermoplastic elastomer (TPE) such as a polyolefin elastomer (POE), or an ethylene homopolymer or copolymer, such as an ethylene-acrylic acid copolymer (EAA copolymer). The latter also include, for example, LDPE (low-density polyethylene), LLDPE (linear low-density polyethylene), and mLLDPE (metallocene linear low-density polyethylene).
[0053] The sealing system 10 according to the invention thus uses a sealing tape 12 with a first outer layer 13, which is designed, for example, as a nonwoven fabric, which allows for good bonding to resin when the resin is in contact with the resin / carrier system 11. Prior resin impregnation of the sealing tape 12 is not required. Rather, the resin / carrier material (referred to in DE 10 2013 111 094 A1 as a "resin-impregnated fiber tape") is wrapped around it. The first outer layer 13, for example the nonwoven fabric, contacts the resin 11b on the one hand, but also, in the overlapping winding areas 15, the second outer layer 14 of the sealing tape 12, which—according to an advantageous embodiment—represents a coating with a thermally easily activated material in the form of the aforementioned at least one polymer. On the side facing away from the resin / carrier system 11, only the polymer coating is present.At all overlapping winding areas 15, the first outer layer 13 comes into contact with the easily thermally activated polymer coating of the second outer layer 14. Upon exposure to heat (during exothermic resin curing), this causes the polymer of the second outer layer 14 to melt and then bond directly to the first outer layer 13, in this case the nonwoven. Furthermore, if the first outer layer is in contact with the resin / carrier system, the resin penetrates the nonwoven, if the first outer layer is designed as such, and, after the resin has cured, forms a sealing bond with it.
[0054] An insert tube according to the invention can be produced in particular according to the following method: A tubular inner film or inner tube film 2 is produced either by winding, by extrusion into a tubular shape, or by sealing one or more flat films to form a tube. The inner tube film 2 is then wrapped with a resin / carrier system 11, i.e., a carrier system that is or will be impregnated with resin. Subsequently, the resin / carrier system 11 is helically wrapped with a sealing tape 12 designed as described above, so that overlapping winding areas 15 are obtained. Finally, the inner tube film 2, the resin carrier system 11, and the said sealing tape 12 are coated with a tube outer film 3, for example, by helically and overlapping wrapping or in the form of one or more flat films sealed to form a tube.As previously noted, additional layers or films may be provided that are not described here.
[0055] According to an alternative, the sealing tape 12 is first wound helically onto the inner tube film 2 and then the resin / carrier system 11 is wound onto the sealing tape 12.
[0056] A pipe K to be renovated, or an underground and leaking or damaged sewer pipe, is lined as follows using an insert hose 1 according to the invention: First, if necessary, a preliner 20 or a sliding film (e.g. on the lower half-shell of the sewer) is placed against the inner wall of the pipe K. The insert hose 1 is then pulled into the pipe K and then expanded so that it rests against the inner pipe wall or the preliner 20 or the sliding film. A UV source is then moved through the pipe K to cure the resin layer(s). During this process, thermal energy is released, which thermally activates or melts the second outer layer 14 of the sealing tape 12 of the sealing system 10 in such a way that regions of this second outer layer 14 bond with overlap regions 15 of the first outer layer 13 that are directly adjacent to them and are created by the helical winding.The resulting seal preferably complies with DIN EN 1610 (1997), Chapter 13.3, method LD (pressure drop).
[0057] In the Fig. 3 to 6 show four different embodiments of an insert hose 1 according to the invention, wherein overlapping winding regions 15 of the sealing strip 12 are shown. In a winding according to Fig. 2, the overlapping winding areas 15 extend completely around the entire circumference of the inner tube film 2 along the central axis Z.
[0058] The resin / carrier system 11 according to the embodiments of the Fig. 3 and Fig. 4 is arranged between the inner tube film 2 and the sealing tape 12.
[0059] According to the Fig.3, the first outer layer 13, consisting for example of fleece, is directed towards the central axis Z of the insert tube 1, while the second outer layer 14 of the sealing tape 12 is directed outwards. During the exothermic reaction of the resin during its curing by means of an activation source (e.g. UV source) moved through the insert tube (in the inserted and expanded state in the sewer pipe K), according to the Fig. 3 in the overlapping winding areas 15 the first outer layer 13 of the outer wound layer of the sealing tape 12 with the second outer layer 14 of the inner layer of the sealing tape 12.
[0060] According to the Fig. 4, the second outer layer 14 is directed towards the central axis Z of the insert tube 1, while the first outer layer 13 of the sealing tape 12 is directed outwards. Fig.4, the second outer layer 14 of the outer wound layer of the sealing tape 12 bonds to the first outer layer 13 of the inner layer of the sealing tape 12 in overlapping winding areas 15 when the resin releases sufficient heat during its exothermic curing reaction.
[0061] In the Fig. 5 and Fig. 6, the resin / carrier system 11 is arranged between the sealing tape 12 and the outer tube film 3.
[0062] According to the Fig. 5, the second outer layer 14 is directed towards the central axis Z of the insert tube 1, while the first outer layer 13 of the sealing tape 12 is directed outwards. Fig. 5, the second outer layer 14 of the outer wound layer of the sealing tape 12 bonds to the first outer layer 13 of the inner layer of the sealing tape 12 in overlapping winding areas 15 when the resin releases sufficient heat during its exothermic curing reaction.
[0063] According to the Fig. 6, the first outer layer 13, for example made of nonwoven fabric, is directed towards the central axis Z of the insert tube 1, while the second outer layer 14 of the sealing tape 12 is directed outwards. Fig. 6, the first outer layer 13 of the outer wound layer of the sealing tape 12 bonds to the second outer layer 14 of the inner layer of the sealing tape 12 in overlapping winding areas 15 when the resin releases sufficient heat during its exothermic curing reaction.
[0064] The examples of the Fig. 3 and Fig. 5 are preferred, since the respective first outer layer 13, which can be designed in particular as a fleece, can absorb resin from the resin / carrier system 11 and in this way a connection of the sealing tape 12 to the resin / carrier system can be realized. Experimental Results I. Polymers Used a) Queo™ 8201: A polyolefin plastomer (POP) with a melt flow rate (2.16 kg / 190°C) of 1.1 dg / min according to ISO 1133; a DSC peak melting point of 73°C according to ISO 11357, a Vicat softening temperature (at 10N) of 50°C according to ISO 306 and a cold brittleness temperature of < -90°C according to ASTM D746. b) Queo™ 8210: A polyolefin plastomer (POP) with a melt flow rate (2.16 kg / 190°C) of 10 dg / min according to ISO 1133; with a DSC peak melting point of 75°C according to ISO 11357, a Vicat softening temperature (at 10N) of 45°C according to ISO 306 and a low temperature brittleness temperature of < -76°C according to ASTM D746. c) Queo™ 8207: A polyolefin plastomer (POP) with a melt flow rate (2.16 kg / 190°C) of 6.6 dg / min according to ISO 1133; with a DSC peak melting point of 76°C according to ISO 11357, a Vicat softening temperature (at 10N) of 47°C according to ISO 306 and a cold brittleness temperature of < -76°C according to ASTM D746. d) Escor™ 5100: An ethylene-acrylic acid copolymer resin (EAA copolymer) with a melt index (2.16 kg / 190°C) of 8.5 g / 10 min according to ASTM D1238 and a peak melting point of 95°C. However, when applied as a coating, the measured peak melting point was 76°C. e) Vistamaxx 3980FL: A polyolefin elastomer (POE) with a melt flow index (2.16 kg / 190°C) of 3.7 g / 10 min according to ASTM D1238 and a Vicat softening temperature of 76.7°C. However, when applied as a coating, the measured peak melting point was 75°C. f) Exact ® 0201: a polyolefin plastomer (POP) from Borealis Plastomers vof, specifically an ethylene-based octene plastomer produced in a solution polymerization process using a metallocene catalyst. Its density is 0.902 g / cm 3according to ISO 1183 (at 23 °C). DSC peak melting point is 95 °C according to ASTM D3418, and the Vicat softening temperature (at 10 N) is 87 °C according to ISO 306. g) Lupolen 2420 F: A low density polyethylene (LDPE) with a DSC peak melting point of 111°C. h) Lupolen 3010D: A low density polyethylene (LDPE) with a DSC peak melting point of 114°C. II. Fleeces used a) Sandler Sawabond 4313 with 40 g / m 2 . Fiber Polyethylene (PE) / Polypropylene (PP) Bico with melting points of PE = 130°C (= HDPE) and PP = 164°C; hereinafter "Sandler fleece 40 g / m 2 “. Manufacturer: Sandler AG, 95126 Schwarzenbach / Saale b) Sandler Sawabond 4313 with 80 g / m 2 . Fiber Polyethylene (PE) / Polypropylene (PP) Bico with melting points of PE = 130°C (= HDPE) and PP = 164°C; hereinafter "Sandler fleece 80 g / m 2". Manufacturer: Sandler AG, Schwarzenbach / Saale. c) Fiberweb Berotex LLDPE with 40 g / m 2 ; hereinafter referred to as “Fiberweb fleece 40 g / m 2 “.Manufacturer: Fiberweb Berlin GmbH, Berlin. 111. Other materials used
[0065] Durethan C38 F from Lanxess is a medium viscosity copolyamide.
[0066] Admer NF498E from Mitsui Chemicals is a maleic anhydride-modified LDPE, has strong adhesion to PET, EVOH and PA, is very easy to process and has thermal stability equivalent to conventional PE. IV. Examples and comparative examples a) Example B1: Sandler fleece 40 g / m 2 and then coating with 40 g / m 2 Escor 5100. b) Example B2: Sandler fleece 40 g / m 2 and then coating with 40 g / m 2 Vistamaxx 3980FL. c) Example B3: Fiberweb fleece 40 g / m 2 and then coating with 40 g / m 2 Escor 5100. d) Example B4: Fiberweb fleece 40 g / m 2 and then coating with 40 g / m 2 Vistamaxx 3980FL. e) Example B5: Sandler fleece 40 g / m 2 and then coating with 10 g / m 2 Escor 5100. f) Example B6: Sandler fleece 40 g / m 2 and then coating with 20 g / m 2 Escor 5100. g) Example B7: Sandler fleece 40 g / m 2 and then coating with 30 g / m 2 Escor 5100. h) Example B8: Sandler fleece 40 g / m 2 and then coating with 60 g / m 2 Escor 5100. i) Example B9: Sandler fleece 40 g / m 2 and then coating with 90 g / m 2 Escor 5100. j) Example B10: 100 µm thick flat film b10 (according to the following table) extrusion laminated against Sandler fleece 40 g / m 2 using 15 g / m 2 LLDPE polymer with MFI 8 (Melt Flow Index). Flat film b10: Shift number composition Share in shift in % Thickness in µm 1 (second outer layer) • Lupolen 3010D • 100 30 2 • Admer NF498E • 100 10 3 • Durethan C38 F • 100 20 4 • Admer NF498E • 100 10 5 (this side is laminated with fleece; fleece is the first outer layer) • Lupolen 3010D • 100 30 Total: 100 µm k) Example B11: 100 µm thick flat film b11 (according to the following table) extrusion laminated against Sandler fleece 40 g / m 2 using 15 g / m 2 LLDPE polymer with MFI 8. Flat film b11: Shift number composition Share in shift in % Thickness in µm 1 (second outer layer) • Lupolen 2420 F • 20 30 • Exactly 0201 • 80 2 • Admer NF498E • 100 10 3 • Durethan C38 F • 100 20 4 • Admer NF498E • 100 10 5 (this side is laminated with fleece; fleece is the first outer layer) • Lupolen 2420 F • 100 30 Total: 100 µm I) Example B12: 100 µm thick flat film b12 (according to the following table) extrusion laminated against Sandler fleece 40 g / m 2 using 15 g / m 2 LLDPE polymer with MFI 8. Flat film b12: Shift number composition Share in shift in % Thickness in µm 1 (second outer layer) • Exactly 0201 • 100 30 2 • Admer NF498E • 100 10 3 • Durethan C38 F • 100 20 4 • Admer NF498E • 100 10 5 (this side is laminated with fleece; fleece is the first outer layer) • Lupolen 2420 F • 100 30 Total: 100 µm m) Example B13: Sandler fleece 80 g / m 2 and then coating with 40 g / m 2 Escor 5100. n) Example B14: Sandler fleece 40 g / m2 and then coating with 40 g / m 2 Queue 8201. o) Example B15: Sandler fleece 40 g / m 2 and then coating with 40 g / m 2 Queue 8210. p) Example B16: Sandler fleece 40 g / m 2 and then coating with 40 g / m 2 Queue 8207. q) Comparative example 1: Polypropylene (PP) nonwoven fabric with a basis weight of 50 g / m 2 and a PP film laminated to it with a basis weight of 25 g / m 2 (Total weight per unit area: 75 g / m 2 ); total thickness: 0.35 mm; peak melting point of 167°C. r) Comparison example V2: Film b10 (like example B10, but without fleece). s) Comparison example V3: An insert tube without a (wound) sealing tape between the outer film and the resin / carrier system. Measurements and measurement results for tightness
[0067] The leak test was conducted according to DIN EN 1610 (1997), Chapter 13.3, Method LD. For a state-of-the-art insert hose, a pressure drop of no more than 15 mbar must be detectable at a pressure of 200 mbar and a test time of 1.5 to 7 minutes, depending on the diameter or thickness. This (maximum) pressure drop corresponds to a tightness of the insert hoses that is sufficient for many applications. The insert hoses according to the invention significantly undercut this value, as explained below.
[0068] Test insert hoses were manufactured using the sealing tapes from examples B1 to B16 or comparative examples V1 and V2 with the following parameters: - Pipe with DN 300 (diameter: 300 mm); - Wall thickness of the tube: 3.7 mm - Resin: Standard UP resin, for example unsaturated polyester resins of type 1140 of Table 3 according to DIN 16 946-2 corresponding to group 3 in Table 1 according to DIN 18 820; - Support system for the resin: glass, for example corrosion-resistant ECR glass; - Test time: As determined from DIN EN 1610, method LD (“soaked concrete pipes and all other materials”), time: 2 min, pressure p0: 200 mbar; - the pressure drop Δp (delta p) is measured.
[0069] The structure of the test insert tubes from inside to outside was as follows: a) Inner tube film (installation aid), 120 µm thick (removed after resin curing); b) resin / glass fibre system to achieve a wall thickness of 3.7 mm; c) sealing tape according to the invention (e.g. fleece as first outer layer with thermally activated polymer side as second outer layer), wound helically, strip width 200 mm; d) Outer film, UV and light-tight, 230 µm thick, welded from a flat film to form a tube.
[0070] For the purpose of determining the tightness of the insert tube, the sealing tape c) according to the invention is wound up in such a way that the nonwoven side (first outer layer) is facing the resin. After the first strip width of 200 mm of the first layer (first layer of nonwoven as the first outer layer and first layer of polymer as the second outer layer) has been applied, the second layer (nonwoven as the first outer layer and polymer as the second outer layer) is wound up onto the first layer (nonwoven and polymer) so that it overlaps by 50%. With a width of 200 mm, it therefore overlaps 100 mm. It is therefore wound up in an "offset" or helical manner. After the first helical layer or first wrapping, i.e. at the beginning of the overlap and all further overlapping areas, the sealing tape according to the invention is in two layers.This means the following structure in cross-section: resin / carrier system - first layer of fleece (first outer layer of the sealing tape) - first layer of polymer (second outer layer of the sealing tape) - second layer of fleece (again first outer layer of the sealing tape) - second layer of polymer (again second outer layer of the sealing tape).
[0071] What is particularly important for the sealing according to the invention is that the thermally activatable polymer (second outer layer) of the first layer bonds very well with the fleece (first outer layer) of the second layer.
[0072] It goes without saying that the sealing tape according to the invention is wound around the resin / carrier layer (b) without bubbles or wrinkles.
[0073] It is of course possible to wind the sealing tape with less or more overlap, so that three or more layers of resin or fleece can be wound on top of each other.
[0074] Due to thermal energy which is generated during the exothermic resin curing, for example by a UV light source moved through the pipe, temperatures of up to 120°C, usually up to 100°C, act - depending on the speed of curing - locally on the sealing tape according to the invention consisting of the material of the first outer layer (e.g. fleece) which is absorbent for liquids and resin and the thermally activatable polymer of the second outer layer applied thereto, in particular in the present case as a coating (as in Examples B1 to B9 and B13 to 16) or as an outer layer (with a thermally activatable polymer) of a film (as in Examples B10 to B12).
[0075] According to the invention, this temperature increase leads to the polymer of the second outer layer, in the sealing system according to the invention, bonding firmly and tightly to the first outer layer, in this case the nonwoven. This guarantees the special tightness of the insert tube after its curing, e.g., with UV light. Various options for curing the insert tube are known from the prior art and need not be explained in detail here. After curing, the inner tube film is removed to test the tightness of the liner.
[0076] It should also be mentioned that the comparative example V3 represents an insert tube without a (wound) sealing tape between the outer film d) and the layer b) of the resin / carrier system.
[0077] The following table lists the most important information and parameters for examples B1 to B16 and for the comparative examples V1 to V3 as well as the measurement results for tightness (see last column). Example First outer layer: resin absorbent material Second outer layer: Thermally activated polymer (in B1-B16) Melting point of the polymer in °C Coating weight in g / m 2 or thickness (film) in µm / of which active layer in µm Insert hose, tightness according to DIN EN 1610 (1997), Chapter 13.3, Method LD Pressure drop in mbar. Δp B1 Sandler 40 g / m 2 Escor (EAA Copolymer) 76 40 g / m 2 2 B2 Sandler 40 g / m 2 Vistamaxx (POE) 75 40 g / m 2 4 B3 Fiberweb 40 g / m 2 Escor (EAA Copolymer) 76 40 g / m 2 2 B4 Fiberweb 40 g / m 2 Vistamaxx (POE) 75 40 g / m 2 4 B5 Sandler 40 g / m 2 Escor (EAA Copolymer) 76 10 g / m 2 11 B6 Sandler 40 g / m 2 Escor (EAA Copolymer) 76 20 g / m 2 7 B7 Sandler 40 g / m 2 Escor (EAA Copolymer) 76 30 g / m 2 0 B8 Sandler 40 g / m 2 Escor (EAA Copolymer) 76 60 g / m 2 2 B9 Sandler 40 g / m 2 Escor (EAA Copolymer) 76 90 g / m 2 1 B10 Sandler 40 g / m 2 Film b10 (PE) 114 100 µm / 30 µm 13 B11 Sandler 40 g / m 2 Film b11 (PE / POP 20 / 80) 111 / 95 100 µm / 30 µm 3 B12 Sandler 40 q / m 2 Slide b12 (POP 100%) 95 100 µm / 30 µm 4 B13 Sandler 80 g / m 2 Escor (EAA Copolymer) 76 40 g / m 2 2 B14 Sandler 40 g / m 2 Queue 8201 (POP) 73 40 g / m 2 0 B15 Sandler 40 g / m 2 Queue 8210 (POP) 75 40 g / m 2 2 B16 Sandler 40 g / m 2 Queue 8207 (POP) 76 40 g / m 2 2 V1 PP, 50 g / m 2 PP 167 25 g / m 2 22 V2 no PE 114 100 µm 19 V3 no no no no 27 Interpretation of the results
[0078] The sealing systems according to the invention from Examples B1 to B16 all meet the requirements for leak tightness according to DIN EN 1610 (1997), Chapter 13.3 Method L or Chapter 13.3 Method LD (Soaked Concrete Pipes and all other materials).
[0079] Example B1 shows that a 40 g / m 2 Nonwoven fabric based on PE / PP, which is coated with an EAA copolymer (40 g / m 2 ) with a peak melting point of 76°C, results in a pressure drop of only 2 mbar when wrapped around the insert tube after curing. A sewer renovated using the pipe lining process is excellently sealed with such an insert tube.
[0080] In example B2 the 40 g / m 2 Fleece (first outer layer) from example 1 with a POE (40 g / m 2 ) (second outer layer). Even with this material, the sealing system according to the invention achieved excellent tightness in the cured insert tube, as a pressure drop of only 4 mbar was observed.
[0081] Example B3 is like Example 1, but with a different nonwoven, namely an LLDPE nonwoven. The determined pressure drop value of 2 mbar shows, in comparison with Example B1, that the type of nonwoven or its material base has virtually no influence on the sealing effect. Example B3 also resulted in a pressure drop of only 2 mbar, just like Example B1.
[0082] The same applies when comparing example B4 (40 g / m 2 LLDPE fleece) compared to the otherwise identical example B2 (40 g / m 2PE / PP fleece). In both cases, a pressure drop of only 4 mbar was measured.
[0083] The chemical nature of the nonwoven therefore has no influence on the sealing properties of the inventive sealing system for insert tubes. Presumably, the sole determining factor is the nonwoven's absorbency for the thermally activatable polymer of the second outer layer. This allows the nonwoven to absorb the polymer melt of the thermally activatable polymer and bond firmly with it. Furthermore, the nonwoven side can bond very well and firmly with the resin, both in the uncured state (fixation) and, especially, in the cured state of the resin, in which a firm bond between the resin and the nonwoven side is realized.
[0084] In the series example B5 (coating of the fleece with 10 g / m 2 EAA copolymer), Example B6 (coating with 20 g / m 2 EAA copolymer), Example B7 (coating with 30 g / m2 EAA copolymer), the already known example B1 (coating with 40 g / m 2 EAA copolymer), Example B8 (coating with 60 g / m 2 EAA copolymer) and example B9 (coating with 90 g / m 2 EAA Copolymer), the amount of the thermally activated EAA copolymer with a peak melting point of 76°C was varied to determine the influence on the tightness of the insert tube. This resulted in a pressure drop of 11 mbar (Example B5), 7 mbar (Example B6), 0 mbar (Example B7), 2 mbar (Example B8), and 1 mbar (Example 9B). It can be seen that the tightness improves the more EAA polymer is used to coat the nonwoven (from 10 g / m 2 up to 30 g / m 2 ). From a quantity of approx. 30 g / m 2 However, within the limits of measurement accuracy, no further improvement in tightness is observed. From 30 g / m 2 Coating at an extremely low pressure drop in the range 0-2 mbar.
[0085] In Example B10, a film with a (free) LDPE-containing outer layer, 30 µm thick, with a peak melting point of 114°C, was laminated on the other side to the nonwoven fabric from Example B1. Here, too, a sealing effect of the composite was found at a pressure drop of 13 mbar. If a mixture of LDPE and POP = 20 / 80 with peak melting points of 111°C and 95°C is used as the outer (free) layer of the film, as shown in Example B11, the pressure drop is only 3 mbar. This value cannot be reduced further, even if 100% POP with a peak melting point of 95°C is used in the free outer layer of the film from Example 1 laminated to the nonwoven fabric, as shown in Example 12. A pressure drop of 4 mbar was found.
[0086] Thus, Examples B10 to B12 suggest that the peak melting point of the thermally activatable polymer (in the second outer layer of the sealing tape, which in Examples B10 to B12 is the same as the outer (free) layer of the film laminated to the nonwoven) plays a significant role in the sealing integrity of the insert tube in the sealing system according to the invention. Ideally, the melting point of the polymer (or its Vicat softening point if no melting point is present) is in the range of 40°C to 120°C, preferably between 60°C and 100°C.
[0087] In example B13, in comparison to example B1, the grammage of the fleece was 40 g / m 2 to 80 g / m 2 increased. Again, a pressure drop of 2 mbar occurred, so that it can be assumed that the grammage of the fleece from approximately 20 to 30 g / m 2plays no major role in the sealing values. The fleece serves, on the one hand, to fix and adhere to the resin, and, on the other, to absorb the thermally activated polymer of the second outer layer. After curing, it is firmly bonded to the resin and the thermally activated polymer. A certain minimum material thickness is required for this.
[0088] In examples B14 (40 g / m 2 POP with peak melting point 73°C), B15 (40 g / m 2 POP with peak melting point 75°C) and B16 (40 g / m 2 Other thermally low-melting polymers (e.g., POP with a peak melting point of 76°C) were coated onto the fleece from Example B1. Pressure drops in the range of 0 to 2 mbar were observed, meaning the cured insert tube is very dense and meets the DIN EN 1610 standard.
[0089] This shows that the sealing system according to the invention is ideally suited to almost completely seal cured insert tubes.
[0090] A look at the reference systems of Comparative Examples C1 to C3 illustrates the effectiveness of the sealing system according to the invention. As can be seen from Comparative Example C1, the use of conventional PP nonwovens with a PP coating leads to inadequate sealing, as a pressure drop of 22 mbar was measured. Thus, during resin curing, no sealing of the nonwoven with the polymer coated on the nonwoven occurs – the very high melting points (approx. 167°C) are likely far from being reached due to the temperature increase caused by the exothermic resin curing. In this case, the sealing system consisting of the nonwoven and the polymer coated on it cannot "bake" together.
[0091] If a film is used for sealing, as in Comparative Example V2, this also does not lead to complete sealing, as a pressure drop of 19 mbar was measured. This shows that the fleece - or generally a material that absorbs resin or liquids, or a material impregnated with resin or liquids - is necessary to create a tight system so that the fleece can bond with the molten, thermally activated polymer. Furthermore, the bond between the fleece and the resin contributes to the tightness of the sealing system. Furthermore, the use of the fleece side in the sealing system according to the invention also enables the sealing tape to be wrapped around the resin-impregnated glass fiber carrier system with absolutely no wrinkles. In particular, no channels are formed that would lead to leaks. This risk is far greater when using a bare film than when a fleece side is available.
[0092] Comparative example V3 shows that the cured insert hose, on which these examples and comparative examples are based, does not meet the tightness criteria of DIN EN 1610 without a sealing device. A pressure drop of 27 mbar was found to be much too high.
[0093] This shows how important it is to incorporate a functioning sealing system into insert hoses.
[0094] The present invention is not limited to the illustrated and described embodiments. Modifications within the scope of the patent claims are possible, as are combinations of features, even if they are illustrated and described in different embodiments. List of reference symbols 1 insert tube 2 inner tube film 3 Tube outer film 10 Sealing system 11 Resin / carrier system 11a Glass fibers 11b Harz 12 sealing tape 13 First outer layer 14 Second outer layer 15 Overlapping changing areas 20 preliners K pipe f1 flow direction Z central axis
Claims
[1] Sealing system (10), in particular for insert hoses for trenchless sewer rehabilitation, with at least one hose-shaped resin / carrier system (11) and with at least one sealing tape (12) wound helically to form a hose with overlapping areas, which sealing tape rests against the resin / carrier system (11), wherein said sealing tape (12) comprises at least a first outer layer (13) which is capable of absorbing resin or liquids or of being impregnated with resin or liquids, and a second outer layer (14) with at least one thermally activatable polymer, wherein this second outer layer (14) is capable of sealingly bonding to the first outer layer (13) in overlapping winding areas (15) by thermal activation of the at least one polymer in the range from 60° to 120°C. [2] Sealing system according to claim 1, characterized bythat the first outer layer (13) is a fleece, a felt, a woven fabric, a scrim or a knitted fabric, each of which is capable of absorbing resin or liquids. [3] Sealing system according to at least one of the preceding claims, characterized by that the basis weight of the first outer layer (13) is in the range from 5 to 5000 g / m², preferably in the range from 10 to 1000 g / m², particularly preferably in the range from 20 to 500 g / m² and most preferably in the range from 30 to 250 g / m². [4] Sealing system according to at least one of the preceding claims, characterized by that the peak melting point of the at least one polymer or, in the case of an amorphous polymer, its Vicat softening point according to VST / A50 is below 120°C, preferably below 110°C and most preferably below 100°C. [5] Sealing system according to the preceding claim, characterized bythat the melting point of the at least one polymer or, in the case of an amorphous polymer, its Vicat softening point according to VST / A50 is above 30°C, preferably above 40°C, particularly preferably above 50°C and most preferably above 60°C. [6] Sealing system according to the preceding claim, characterized by that the at least one polymer is selected from the group: a) Polyolefin plastomers (POP); b) Thermoplastic elastomers (TPE), such as polyolefin elastomers (POE); c) Ethylene homo- or copolymers, such as ethylene-acrylic acid copolymers (EAA copolymers), LDPE (low density polyethylene), LLDPE (linear low density polyethylene), mLLDPE (metallocene linear low density polyethylene). [7] Sealing system according to at least one of the preceding claims, characterized by that the second outer layer (14) is the outer layer of a film. [8] Sealing system according to the preceding claim, characterized by that the film is a mono- or multi-layer film, preferably a 3-layer film or a 5-layer film, wherein in such a layer structure the said outer layer formed as a second outer layer (14) contains the said at least one thermally activatable polymer. [9] Sealing system according to the preceding claim, characterized by that the film has a thickness of 5 µm to 5000 µm, preferably 10 µm to 3200 µm, particularly preferably 20 µm to 2000 µm. [10] Sealing system according to at least one of the preceding claims, characterized by that the first outer layer (13) is laminated onto said outer layer of the film, which is designed as a second outer layer (14), preferably by extrusion lamination. [11] Sealing system according to at least one of the preceding claims, characterized bythat the second outer layer (14) is formed by a covering or coating, preferably by a covering or coating of the first outer layer (13), with the at least one thermally activatable polymer. [12] Sealing system according to the preceding claim, characterized by that the basis weight of the at least one thermally activatable polymer when coated is in the range from 0.5 to 1000 g / m², preferably in the range from 2 to 500 g / m², particularly preferably in the range from 5 to 200 g / m² and most preferably in the range from 10 to 100 g / m². [13] Sealing system according to at least one of the preceding claims, characterized by that one or more further layers are arranged between the first and second outer layer (13, 14), for example in the form of polymer layers or films. [14] Insert hose (1) with a hose inner film (2) and a hose outer film (3), wherein at least one sealing system (10) according to one or more of the preceding claims is arranged between the hose inner film (2) and the hose outer film (3). [15] Insert hose according to the preceding claim, characterized by that the arrangement of the resin / carrier system (11) of the sealing system (10) is selected from the following group: a) between said sealing tape (12) and the inner tube film (2), wherein the first outer layer (13) of said sealing tape (12) rests against the resin / carrier system (11); b) between said sealing tape (12) and the inner tube film (2), wherein the second outer layer (14) of said sealing tape (12) bears against the resin / carrier system (11); c) between said sealing tape (12) and the outer tube film (3), wherein the first outer layer (13) of said sealing tape (12) bears against the resin / carrier system (11); d) between said sealing tape (12) and the outer tube film (3), wherein the second outer layer (13) of said sealing tape (12) bears against the resin / carrier system (11). [16] Insert hose according to at least one of the two preceding claims, characterized by that the at least one resin / carrier system (11) is wound helically around the inner tube film (2) and the at least one sealing tape (12) is wound helically around the resin / carrier system (11). [17] Method for producing an insert hose, in particular an insert hose (1) according to one of the preceding claims, comprising the following steps in this order: a) providing a tubular inner film (2) which is either wound, extruded in a tubular shape or a flat film sealed into a tube; b) covering the inner film of the tube (2) with a carrier system (11) which is or will be impregnated with resin (resin / carrier system); c) helically and overlappingly wrapping the resin / carrier system (11) with a sealing tape (12), wherein said sealing tape (12) comprises at least a first outer layer (13) which is capable of absorbing or being impregnated with a portion of the resin of the resin / carrier system (11), and a second, thermally activatable outer layer (14), wherein said second outer layer (14) is capable of sealingly bonding to the first outer layer (13) in overlapping winding regions (15) by thermal activation in the range of 60° to 120°C; and d) wrapping said inner tube film (2) and said resin carrier system (11) as well as said sealing tape (12) with a tube outer film (3), for example by means of helical and overlapping wrapping or in the form of a tube film consisting of one or more flat films connected to one another by sealing. [18] Method for producing an insert hose, in particular an insert hose (1) according to one of the preceding claims, comprising the following steps in this order: a) providing a tubular inner film (2) which is either wound, extruded in a tubular shape or a flat film sealed into a tube; b) helically and overlappingly wrapping the inner tube film (2) with a sealing tape (12), said sealing tape (12) comprising at least a first outer layer (13) which is capable of absorbing or being impregnated with part of the resin of the resin / carrier system (11), and a second, thermally activatable outer layer (14), said second outer layer (14) being capable of sealingly bonding to the first outer layer (13) in overlapping winding regions (15) by thermal activation in the range from 60° to 120°C; c) covering the sealing strip (12) with a resin / carrier system (11) impregnated with resin; and d) wrapping said sealing tape (12) with a tubular outer film (3), for example by means of helical and overlapping wrapping or in the form of one or more flat films sealed to form a tube. [19] Method for lining a pipe (K), in particular a sewer pipe during trenchless sewer rehabilitation, with an insert hose (1) according to one of the preceding claims, comprising the following steps in this order: a) the insert hose (1) is pulled into the pipe (K) or inserted into the pipe (K) by inversion, b) then the insert hose (1) is widened so that it comes into contact with the inner wall of the pipe, and c) finally, the resin layer(s) is / are cured by means of a UV source moved through the pipe (K), thermal energy being released by which the second outer layer (14) of the sealing system (10) is thermally activated or melted in such a way that areas of this second outer layer (14) bond with overlapping areas (15) of the first outer layer (13) that are directly adjacent to them and are created by the helical winding, so that a seal is obtained between these areas, which preferably complies with DIN EN 1610 (1997), Chapter 13.3, Method LD (pressure drop). [20] Use of a sealing tape with a first and a second outer layer (13, 14) according to at least one of claims 1 to 13 for the production of an insert hose (1) according to at least one of claims 14 to 16 or for the lining of a pipe (K) according to one of the preceding claims.
Citation Information
Patent Citations
Lining hose for the rehabilitation of fluid-carrying pipe systems
DE102013111094A1
Foil, especially for use in trenchless sewer rehabilitation
DE102014111427A1
Liner with a tubular film that is coated with a nonwoven
EP1180225A1
UV and light protective film
EP2379625B1
Process for making a tubular cladding hose
WO1995004646A1