Photomask arrangement with reflective photomask and method for producing a reflective photomask
A removable protective structure on the back of EUV photomasks addresses defects by preventing contamination and mechanical damage, ensuring planarity and functionality, thereby improving EUV lithography processes.
Patent Information
- Application Number
- DE102019100839
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-01-14
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2039-01-14
AI Technical Summary
Defects on the back of EUV photomasks, such as particles caught between the chuck and the photomask, cause planarity issues and focus errors, leading to image shift and potential damage to the chuck.
A protective structure is applied to the back side of the photomask, removable at temperatures below 150 degrees Celsius, which prevents particle contamination and mechanical damage during processing, maintaining planarity and allowing easy detachment without affecting the photomask's functionality.
The protective structure effectively prevents defects on the photomask backside, ensuring planarity and functionality, facilitating easy removal without damaging the photomask, thus enhancing the reliability and usability of EUV lithography processes.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
TECHNICAL AREA
[0001] The present disclosure relates to a photomask arrangement comprising a reflective photomask, in particular an EUV (extreme ultraviolet) photomask. The present disclosure further relates to a method for manufacturing a reflective photomask. BACKGROUND
[0002] Extreme ultraviolet lithography (EUVL) uses electromagnetic radiation at an exposure wavelength of approximately 13.5 nm and is a promising next-generation lithography technology for the mass production of semiconductor devices at resolutions exceeding those achievable with optical lithography at 193 nm. EUVL utilizes reflective optics and a reflective photomask with a multilayer mirror. Typically, an electrostatic chuck or a vacuum chuck holds the photomask in place during the exposure of semiconductor wafers. Defects on the back side of the photomask, such as particles inadvertently trapped between the chuck and the rear surface of the photomask, can affect the planarity of the front side of the photomask, leading to unwanted image shift and focus errors, and can damage the chuck.
[0003] To improve electrostatic clamping (chucking), German patent application DE 11 2012 000 658 T5 describes a conductive backcoat for an EUV mask substrate. The backcoat comprises a first sublayer of chromium (Cr), oxygen (O), and hydrogen (H), and a second sublayer of chromium (Cr), nitrogen (N), and hydrogen (H). The two sublayers are applied by sputtering. The film thickness of the lower sublayer is 2 to 30 nm, and the film thickness of the upper sublayer is 50 to 300 nm. German patent application US 6,352,803 B1 describes another backcoat for EUV mask substrates to improve electrostatic clamping. The backcoat material is, for example, silicon (Si), molybdenum (Mo), chromium (Cr), chromium oxynitride (CrON), or tantalum silicide (TaSi).In German patent application JP 2012-182235 A, a protective film made of an organic polymer is applied by spin coating outside the EUV exposure unit before each exposure of an EUV mask. The protective film contains neither silicon nor fluorine or metal atoms and is decomposed by a high-energy beam after each exposure, still within the EUV exposure unit. German patent application DE 11 2009 002 622 T5 describes the application of a conductive chromium nitride (CrN) layer to the back of a SiO2-TiO2 glass substrate prior to the formation of a multilayer reflective layer of Mo / Si layers on the front of the SiO2-TiO2 glass substrate.
[0004] It is a task of the embodiments to reduce or comprehensively mitigate the frequency of occurrence of critical defects on the back of photomasks. SUMMARY
[0005] The problem is solved by the subject matter of the independent claims. Dependent claims relate to further embodiments.
[0006] The present disclosure relates to a photomask arrangement comprising a reflective photomask and a protective structure. The reflective photomask comprises a substrate, a reflective multilayer, or a reflective multilayer system on a first substrate surface of the substrate at a front face of the photomask. The protective structure on a second substrate surface of the substrate at the rear face of the photomask is removable from the photomask at a temperature below 150 degrees Celsius.
[0007] The present disclosure also relates to a method for producing a reflective photomask. The method comprises forming a reflective photomask, which includes a substrate, a reflective multilayer system on a first substrate surface, and an absorber structure on the multilayer system at a front face of the photomask. Prior to forming the absorber structure, a protective structure is bonded to a second substrate surface at a rear face of the photomask.
[0008] The present disclosure also relates to a further photomask arrangement comprising a reflective photomask and a protective structure. The reflective photomask comprises a substrate, a reflective multilayer system on a first substrate surface of the substrate, and an absorber structure on the multilayer system at a front face of the photomask. The protective structure on a second substrate surface of the substrate at the rear face of the photomask is removable from the photomask at a temperature below 150 degrees Celsius and / or by applying a process fluid inert to the absorber structure.
[0009] Finally, the present disclosure relates to another method for producing a reflective photomask. A photomask is formed comprising a substrate and a reflective multilayer system on a first substrate surface at a front face of the photomask. Before forming an absorber structure on the reflective multilayer system, a protective structure is provided on a second substrate surface at the rear face of the photomask. After forming the absorber structure, the protective structure is removed. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] The accompanying drawings are enclosed to provide a further understanding of the embodiments and are incorporated into and form part of this patent description. The drawings illustrate the embodiments of the present disclosure and, together with the description, serve to explain the principles of the embodiments. Other embodiments and intended advantages are immediately appreciated, as they are better understood with reference to the following detailed description. Fig. Figures 1A - 1B illustrate a schematic top view and a schematic vertical cross-sectional view of a photomask arrangement comprising a reflective photomask and a protective structure on a rear side of the photomask, according to one embodiment. Fig. Figures 2A and 2B illustrate schematic vertical cross-sectional views of photomask arrangements comprising a reflective photomask and a protective structure on a rear side of the photomask, according to other embodiments. Fig. Figures 3A - 3C illustrate schematic vertical cross-sectional views of photomask arrangements with reflective photomasks without an electrically conductive backing film. Fig. Figures 4A - 4C illustrate schematic vertical cross-sectional views of photomask arrangements with reflective photomasks featuring an electrically conductive backing film. Fig. Figures 5A and 5B illustrate a schematic top view and a schematic cross-sectional view of a photomask arrangement containing an adapter. Fig. Figures 6A - 6D are schematic vertical cross-sectional views of areas of a reflective photomask and a protective structure to illustrate a method for manufacturing a reflective photomask according to a further embodiment. DETAILED DESCRIPTION
[0011] The following detailed description refers to the accompanying drawings, which form part thereof and in which specific embodiments are shown for illustrative purposes, in which a reflective photomask, a method for manufacturing a reflective photomask, and a method for manufacturing a semiconductor device can be designed. It is understood that other embodiments can be used and structural or logical modifications can be made without departing from the scope of this disclosure. For example, features illustrated or described for one embodiment can be used in or in connection with other embodiments to arrive at yet another embodiment. It is intended that the present invention encompasses such modifications and changes.The examples are described using specific language, which should not be interpreted as limiting the scope of the attached patent claims. The drawings are not to scale and are for illustrative purposes only. Corresponding elements are designated by the same reference numerals in the various drawings unless otherwise stated.
[0012] The terms "have," "contain," "comprise," "exhibit," and similar terms are open-ended, indicating the presence of the identified structures, elements, or features without excluding additional elements or features. Indefinite and definite articles should encompass both the plural and singular unless the context clearly indicates otherwise.
[0013] Furthermore, the term "on" should not be understood as meaning only "directly on". Rather, if an element is positioned "on" another element, e.g., if a layer is "on" another layer or "on" a substrate, another component, e.g., another layer, can be positioned between the two elements. For example, another layer can be positioned between a layer and a substrate if the layer is "on" the substrate.
[0014] The main components of a layer or structure made of a chemical compound or alloy are those elements whose atoms form the chemical compound or alloy. For example, nickel and silicon are the main components of a nickel silicide layer, and copper and aluminum are the main components of a copper-aluminum alloy.
[0015] The terms metal and metallic, as used in the context of this application, do not include semimetals. In particular, the terms metal and metallic do not include the elements boron, silicon, germanium, arsenic, antimony, and / or tellurium. A metallic structure contains at least one metallic region and may, in addition to the metallic region, contain one or more regions of a non-metallic or semimetallic material. Transition metals are the chemical elements with atomic numbers 21 to 30, 39 to 48, 57 to 80, and 89 to 112.
[0016] A photomask assembly comprises a reflective photomask and a protective structure. The reflective photomask has a substrate and a reflective multilayer system on a first substrate surface, with the multilayer system located on the front of the photomask. The protective structure is located on a second substrate surface on the back of the photomask and is removable from the photomask at temperatures below 150°C.
[0017] The substrate may contain a substrate core area made of a low thermal expansion (LTE) material with a coefficient of thermal expansion less than 1 ppm / K. In addition to the substrate core area, the substrate may contain one or more further layers on the side of the substrate core area facing the reflective multilayer system and / or one or more further layers on the side of the substrate core area facing away from the reflective multilayer system.
[0018] The reflective multilayer system can contain a multitude of layer pairs, each consisting of a first layer and a second layer. At the exposure wavelength, the first layers have a first refractive index, and the second layers have a second refractive index. The different refractive indices of the first and second layers result in the reflective multilayer system acting as a Bragg reflector with a reflection maximum typically at or near an exposure wavelength for EUV or BEUV (beyond EUV). For example, the exposure wavelength might be 13.5 nm or 6.7 nm. The reflective multilayer system can include one or more additional layers on the substrate-facing side and / or on the side facing away from the substrate.
[0019] The photomask can further include a non-structured, continuous stack of absorber layers or a structured stack of absorber layers on the reflective multilayer system, wherein the structured stack of absorber layers forms an absorber structure that may have openings exposing areas of the reflective multilayer system. The stack of absorber layers can include at least one absorbing layer with an absorption coefficient of at least 40% at the exposure wavelength, e.g., at 13.5 nm or at 6.7 nm. The stack of absorber layers can include one or more additional layers on the side facing the reflective multilayer system and / or on the side facing away from the reflective multilayer system.
[0020] The protective structure can be a flexible band or a rigid plate containing glass, metal, a semiconductor material (e.g., crystalline or polycrystalline silicon), a ceramic, a sintered material, and / or a hardened resist. The protective structure can cover the entire surface of the second substrate. The outer surfaces of the protective structure and the photomask can be flush. Alternatively, the protective structure can protrude laterally beyond the contour of the photomask.
[0021] The protective structure can be connected to or bonded to the substrate. The connection between the protective structure and the substrate can be an adhesive bond or an adhesive-free bond. For example, the protective structure and the photomask can be directly bonded. Adhesion between a directly bonded protective structure and a photomask can be based on chemical bonds, hydrogen bonds, metallic bonds, ionic and / or covalent bonds between the substrate 110 and the protective structure 200. Direct bonding can involve applying a moderate mechanical force that presses the protective structure and the photomask against each other, thermal treatment of at least one of the two bonding surfaces at a moderate temperature below 120°C, e.g., 100°C, or a combination of both, e.g., fusion bonding, thermo-compressive bonding, or bonding by atomic rearrangement.
[0022] The protective structure can be removed from the photomask at a temperature below a critical temperature at which atoms in the mask stack, e.g., in the reflective multilayer system, begin to diffuse across layer interfaces into adjacent layers to a more than negligible extent. For example, the protective structure can be removed at a temperature below 150 degrees Celsius, e.g., at most 135 degrees Celsius or at most 120 degrees Celsius. Removal can involve debonding the bond between the protective structure and the photomask. Furthermore, removal of the protective structure can involve cleaning the second substrate surface with a rinsing fluid that is inert to the materials of the absorber layer stack and the reflective multilayer system. For example, the rinsing fluid contains a liquid, a gas, or both.
[0023] A protective structure that can be detached from the photomask at temperatures below 150°C can be easily removed from the reflective photomask without adverse effects on the photomask, in particular without adverse effects on the absorber structure, the reflective multilayer system and / or the second substrate surface.
[0024] In particular, the protective structure can be removed in such a way that neither the absorber structure, nor the reflective multilayer system, nor the substrate are affected to a more than negligible extent and without leaving any non-negligible residues on the second substrate surface.
[0025] In other words, after removal of the protective structure, the second substrate surface can still meet the general specifications for EUV mask back surfaces with regard to flatness and planarity. Specifically, the protective structure leaves no residual particles protruding more than 10 µm from the second substrate surface. Furthermore, after removal of the protective structure, the dimensions of the absorber structure and the multilayer system meet the general specifications for absorber structures and multilayer systems, as well as specific specifications for a particular mask layout.
[0026] The protective structure can be removed before installing the reflective photomask in an EUVL apparatus or before shipping the photomask to a semiconductor factory.
[0027] The protective structure can temporarily protect the photomask from particle contamination during processes applied to its front surface, such as deposition of the reflective multilayer system, deposition of the absorber layer stack, structuring of the absorber layer stack, or frame trench formation. Removing the protective layer involves removing particles deposited on the back of the photomask before and / or during front-side processing. Even particles deposited before the protective structure was applied, which were not completely removed by previous rinsing processes but remained adhered to the protective layer, can be removed along with the protective structure.
[0028] Furthermore, the protective structure can prevent direct contact between tools for handling masks and the back of the photomask, thus protecting the back of the reflective photomasks against mechanical damage, for example scratches.
[0029] The protective structure can be provided using tools and methods known from semiconductor wafer technology. For example, the protective structure can include a rigid support or a flexible band of the type that is temporarily attached to semiconductor wafers during wafer thinning, wafer grinding, wafer cutting, and / or wafer inspection.
[0030] The substrate can have a backing film that forms the second substrate surface. This backing film can be electrically conductive, facilitating electrostatic mounting of the reflective photomask in an EUVL apparatus. For example, the backing film can contain chromium (Cr) and nitrogen (N), or tantalum (Ta) and boron (B). The protective structure can be bonded directly to the backing film. Electrostatic mounting, e.g., on a nail bed chuck, can mitigate the adverse effects of backing surface irregularities and / or roughness. Alternatively, the protective structure can be formed directly on the main substrate area using an LTE material.
[0031] The protective structure can be detached from the photomask, e.g., by applying a temperature between 110°C and 150°C, by applying electromagnetic radiation, by applying a debonding fluid that breaks the bond, and / or by applying a moderate mechanical force. A moderate mechanical force is understood to be a mechanical force that is sufficiently weak so as not to damage the photomask. A moderate mechanical force may be in the range of a manually applicable force or less.
[0032] For example, heat treatment can break the bond between the protective structure and the photomask, i.e., completely break it or weaken it by at least 90%. For example, a stream of hot air can be directed onto the back of the photomask assembly, and the protective structure can be mechanically peeled off during / after thermal breakage / weakening of the bond. At a debonding temperature higher than 110°C, it is possible for the protective structure to remain reliably fixed to the photomask during front-side processing of the photomask, e.g., during any processes that structure the absorber layer stack. At a debonding temperature below 150°C, e.g., at most 135°C or at most 120°C, the debonding process does not affect the front of the photomask, e.g., the absorber structure.
[0033] Alternatively or additionally, the connection between the photomask and the protective structure can be completely broken or weakened by at least 90% by irradiating the protective structure with electromagnetic radiation of a specific wavelength range, e.g. with ultraviolet light (UV light).
[0034] Alternatively or additionally, the bond between the photomask and the protective structure can be completely dissolved or weakened by at least 90% by applying a suitable debonding fluid, e.g. a fluid containing a solvent for the bond.
[0035] The protective structure can include a main support and an adhesive layer that reversibly bonds the main support to the reflective photomask.
[0036] In general, breaking a reversibly bonded connection leaves the reversibly bonded structures intact. More specifically, breaking the reversibly bonded primary support from the photomask leaves both the photomask and the primary support intact. A photomask that meets predefined requirements before the reversibly bonded connection is broken will meet the same requirements after the reversibly bonded connection is broken, possibly at least after a further cleaning step. A primary support detached from the reversibly bonded connection can be reused for the same purpose without functional limitations, possibly at least after a further cleaning step.
[0037] The primary support can be a rigid support made of a solid material, e.g., a continuous, unstructured plate or a plate with depressions, where the depressions may expose areas of the secondary substrate surface. For example, the primary support can take the form of a framed grid or a frame formed along the edge of the photomask.
[0038] The adhesive layer can contain an adhesive that is applied to a mounting surface of the main carrier, to the second substrate surface, or to both, prior to bonding the main carrier to the second substrate surface. Alternatively, the adhesive layer can be an adhesive film that is inserted between the main carrier and the second substrate surface prior to bonding the main carrier to the second substrate surface.
[0039] The rigid main support can be reused, if necessary after a further cleaning process to remove any remaining adhesive layer. With a reusable main support, it is possible to use comparatively expensive protective structures without drastically increasing costs. Residue-free adhesives and adhesive films are proven and tested in processes related to back-grinding of wafers, wafer cutting, and / or wafer inspection for semiconductors.
[0040] The protective structure can include a carrier tape and an adhesive layer that bonds the carrier tape to the photomask. The carrier tape can be any of the tapes used in semiconductor manufacturing for temporarily stabilizing a semiconductor wafer, e.g., during grinding, cutting, and / or inspection. Alternatively, the carrier tape can be any of the tapes used as a receiving tape.
[0041] The protective structure is, for example, a UV tape that exhibits strong adhesion immediately after bonding. The UV tape covers the back of the photomask during at least some of the front-facing processes. Irradiation with UV light reduces the adhesion by at least 90%, and the photomask can then be easily removed from the UV tape.
[0042] The photomask assembly may include a mechanical adapter with a receiving bore suitable for supporting the reflective photomask. The contour of the mechanical adapter corresponds to the contour of a standard wafer. For example, the contour of the mechanical adapter may correspond to the contour of a standard wafer with a diameter of 200 mm or 300 mm. The mechanical adapter facilitates the use of tools that bond rigid primary supports and / or support strips to semiconductor wafers to bond such supports to reflective photomasks. For example, the mechanical adapter may facilitate the application of a back-grinding strip or a receiving strip to the second substrate surface of the photomask to a laminating tool, such as those typically used for laminating semiconductor wafers with a back-grinding strip, a slicing strip, or a receiving strip.
[0043] A method for fabricating a reflective photomask includes forming a reflective photomask comprising a substrate, a reflective multilayer system on a first substrate surface, and an absorber structure on the multilayer system at a front face of the photomask. Prior to structuring the absorber structure, a protective structure is bonded to a second substrate surface at a rear face of the photomask.
[0044] Bonding the protective structure to the photomask allows the protective structure to be detached or debonded, resulting in temporary protection of the back of the photomask without adversely affecting the photomask.
[0045] The protective structure is removable from the photomask at temperatures below 150°C. Removing the protective structure from the photomask may involve debonding the bond between the protective structure and the photomask, and debonding may involve complete separation of the bond or a weakening of the bond by at least 90% combined with mechanical peeling. With a debonding temperature below 150°C, e.g., at most 135°C or at most 120°C, the debonding process does not affect the front surface of the photomask, e.g., the absorber structure.
[0046] The protective structure can be provided before the reflective multilayer system is formed, preventing particle contamination on the second substrate surface during and between all relevant deposition processes. Alternatively, the protective structure can be provided after the formation of the reflective multilayer system and before the deposition of an absorber layer stack from which the absorber structure is formed, preventing particle contamination on the second substrate surface during and between all processes used to form the absorber structure.
[0047] The protective structure can be removed from the photomask after the absorber structure has formed. The protective structure provides temporary protection for the back of the photomask without affecting its use in an EUVL apparatus.
[0048] A photomask assembly can comprise a reflective photomask and a protective structure. The reflective photomask can include a substrate, a reflective multilayer system on a first substrate surface, and an absorber structure on the multilayer system, with the multilayer system and the absorber structure being located on the front of the photomask. The protective structure is located on a second substrate surface on the rear of the photomask and can be removed from the photomask at a temperature below 150°C and / or by applying a process fluid that is inert to at least the absorber structure. The process fluid can also be inert to the reflective multilayer system and / or the substrate. The process fluid can be a solvent-based fluid.
[0049] A protective structure that can be removed at temperatures below 150°C and / or by applying a process fluid inert to the absorber structure can provide temporary protection for the photomask against backside contamination and / or defects caused by mechanical contact with mask handling tools. It is possible that this temporary protection will not adversely affect the use of the photomask in an EUVL apparatus, and in particular, will not negatively affect the absorber structure, the reflective multilayer system, and / or the secondary substrate surface.
[0050] The reflective photomask can have a backing film formed directly on the second substrate surface. This backing film can be electrically conductive, enabling electrostatic holding or clamping of the reflective photomask in an EUVL apparatus. For example, the backing film can contain chromium (Cr) and nitrogen (N), or tantalum (Ta) and boron (B). The protective structure can be formed directly on the backing film. Electrostatic clamping on a bed-of-needles chuck can mitigate the adverse effects of backing irregularities and / or roughness. Alternatively, the protective structure can be formed directly on the main substrate area using LTE material.
[0051] The protective structure can be chemically or physically removable, for example by grinding, CMP (chemical-mechanical polishing), mechanical polishing, or dry etching. For instance, a protective structure based on an oxide and / or a silicon compound, e.g., Si3N4 or SiO2, can be removed by RIE (reactive ion etching) or IBE (ion beam etching).
[0052] The protective structure can be made of a material that is completely soluble in a solvent fluid.
[0053] The protective structure can consist of one or more polymer materials, or it can contain one or more polymer materials in addition to non-polymer materials, with the solvent fluid being a liquid containing an organic solvent. The polymer materials can, for example, contain a polyimide or PTFE (polytetrafluoroethylene).
[0054] The protective structure can comprise at least one layer consisting of a metal layer, an oxide layer, and a layer of a silicon compound, with the solvent fluid potentially containing an acid. If the photomask has a metallic backing film, the solvent fluid can contain an etchant that removes the protective structure with high selectivity with respect to the backing film. For example, the protective structure can comprise at least one layer containing titanium (Ti), one containing aluminum (Al), one containing titanium (Ti) and / or aluminum (Al), one containing a silicon oxide layer such as a silicon dioxide (SiO2) layer formed using TEOS (tetraethoxysilane) as a precursor material, and one containing silicon nitride (Si3N4).
[0055] According to another example, the solvent fluid is an activated etching gas that dissolves a protective structure based on an oxide and / or a silicon compound, e.g. Si3N4 or Si2O, in a plasma etching process.
[0056] The protective structure can be sprayed onto the second substrate surface, applying it in a simple and cost-effective manner. During photomask manufacturing, requirements concerning the back surface planarity and / or flatness of both the photomask and the protective structure are relatively relaxed and can therefore be met using cost-effective spraying methods.
[0057] The present disclosure relates to a further method for forming a reflective photomask. The photomask comprises a substrate and a reflective multilayer system on a first substrate surface at a front face of the photomask. Before forming an absorber structure on the multilayer system, a protective structure is provided on a second substrate surface at a rear face of the photomask. After forming the absorber structure, the protective structure can be removed. The protective structure provides effective temporary protection of the rear face of the photomask against particle contamination and mechanical defects caused, for example, by tools used to handle the masks.
[0058] The protective structure can be removed from the photomask at a temperature of no more than 150 degrees Celsius and / or by applying a process fluid inert to the absorber structure. The protective structure can be applied and removed easily and cost-effectively.
[0059] The protective structure can be removed from the photomask, whereby the application and removal of the protective structure can utilize processes that have proven effective and tested in combination with grinding, cutting and / or examining semiconductor wafers or for imaging processes.
[0060] Fig. Figures 1A-1B show a photomask arrangement 900 comprising a reflective photomask 100 and a protective structure 200 for an exposure wavelength in the range of 1 nm to 15 nm. The photomask 100 can, for example, be an EUVL mask for an exposure wavelength of approximately 13.5 nm. According to another embodiment, the photomask 100 can be a BEUVL (beyond extreme ultraviolet lithography) mask for an exposure wavelength in the range of 1 nm to 10 nm, e.g., approximately 6.7 nm.
[0061] The photomask 100 can have an approximately rectangular shape with a border length of a few centimeters. A structural section 191 of the photomask 100 contains the image to be projected onto a semiconductor wafer, wherein the structural section 191 contains the image information of a single semiconductor device or a plurality of semiconductor devices. A frame section 192 can laterally surround the structural section 191. The frame section 192 does not contain image information about semiconductor devices. The frame section 192 can include a frame trench 180 extending from a first principal surface 101 into the photomask 100.
[0062] During exposure of a semiconductor wafer in an EUVL apparatus, the photomask 100 is fixed to a mask table, and the photomask 100 may have a second primary surface 102 at its rear. The exposure radiation strikes the first primary surface 101 at the front of the photomask 100. The portion of the exposure radiation reflected from the first primary surface 101 encodes the image information, which is projected onto a photoresist layer that covers the semiconductor wafer during exposure.
[0063] The second principal surface 102 on the back side of the photomask 100 is planar and flat. Directions parallel to the second principal surface 102 are lateral directions. The first principal surface 101 may contain surface sections 105 parallel to the second principal surface 102. A surface normal 104 to the surface sections 105 parallel to the second principal surface 102 defines a vertical direction.
[0064] The photomask 100 comprises a substrate 110, which contains at least one main substrate region made of an LTE material. The substrate 110 may include further layers, e.g., a backside film on the back of the LTE material. A second substrate surface 112 of the substrate 110 forms the second main surface 102 of the photomask 100.
[0065] A reflective multilayer system 120 is formed on a first substrate surface 111 at the front of the substrate 110. The reflective multilayer system 120 can contain a plurality of layer pairs, each layer pair comprising a first layer 121 and a second layer 122. The first and second layers have different refractive indices. For example, the first layers 121 can be molybdenum (Mo) layers with a thickness in the range of 2 nm to 5 nm, and the second layers 122 can be silicon (Si) layers with a thickness in the range of 2 nm to 5 nm. The number of layer pairs can range from 20 to 70. The different refractive indices of the first and second layers 121, 122 result in the reflective multilayer system 120 effectively acting as a Bragg reflector with a reflection maximum at a predefined exposure wavelength of, for example, 13.5 nm or 6.7 nm.A minimum reflectance of the reflective multilayer system 120 at the exposure wavelength is at least 50%, for example greater than 60%.
[0066] An absorber structure 130 is formed on the reflective multilayer system 120 on a side facing away from the substrate 110, such that the reflective multilayer system 120 lies between the absorber structure 130 and the substrate 110. The absorber structure 130 can have an absorption coefficient of at least 50% at the exposure wavelength. The thickness of the absorber structure 130 can be in the range of 10 nm to 90 nm. The absorber structure 130 can be formed from a stack of absorber layers, which includes at least one absorber layer, wherein the absorber layer can be based on a metal nitride, for example, a transition metal nitride such as tantalum nitride (TaN) or titanium nitride (TiN). For example, the absorber layer can be based on a tantalum nitride which may contain other main components, for example boron (B) or oxygen (O), where the absorber layer is a layer of tantalum boron nitride (TaBN) or a layer of tantalum boron oxide (TaBO).Alternatively, the absorber layer can contain chromium (Cr). The absorber layer can, for example, consist of or contain chromium nitride (CrN). The frame trench 180 can extend through the reflective multilayer system 120 to or into the substrate 110.
[0067] A protective structure 200 is provided on the back side of the photomask 100. The protective structure 200 can be formed directly on the second substrate surface 112, e.g., deposited, or it can be bonded to the second substrate surface 112. A lateral surface 203 of the protective structure 200 can be flush with a lateral surface 103 of the photomask 100. The thickness d1 of the protective structure 200 can be in a range of 50 µm to 2000 µm, e.g., from 80 µm to 1000 µm, if the protective structure 200 is bonded to the photomask 100, and in a range of 0.1 µm to 30 µm if the protective structure 200 is formed directly on the photomask 100, e.g., deposited.
[0068] The protective structure 200 can comprise a single layer or at least two different structures, for example a rigid support or a flexible band and an adhesive layer that adheres the rigid support or the flexible band to the photomask 100.
[0069] Fig. Figure 2A shows a photomask arrangement 900 with the absorber structure 130 and without a frame trench.
[0070] The photomask arrangement 900 of Fig. 2B comprises a photomask 100 with a non-structured absorber layer stack 134.
[0071] In other words, the photomask 100 represents a mask blank in a state prior to the formation of an absorber structure by structuring the absorber layer stack 134.
[0072] Fig. 3A - 3C refer to photomasks 100 without a backing film, wherein in all figures the protective structure 200 is formed directly on a surface of a substrate main area 115 made of an LTE material.
[0073] The absorber structure 130 is formed from an absorber layer stack comprising an absorber layer 135 and a buffer layer 131 formed between the absorber layer 135 and the reflective multilayer system 120, wherein the buffer layer 131 can effectively act as an etch stop layer during the formation of the absorber structure. Alternatively or additionally to the buffer layer 131, the absorber layer stack can include an antireflection layer 139 on the front side of the absorber layer 135.
[0074] At an inspection wavelength typically longer than the EUV inspection wavelength, the antireflection layer 139 is less reflective than the absorber layer 135. The antireflection layer 139 may contain or consist of a metal nitride, for example, a transition metal nitride such as titanium nitride or tantalum nitride, and may contain one or more additional components selected from a group containing chlorine, fluorine, argon, hydrogen, or oxygen. The antireflection layer 139 can be formed by treating a surface of the absorber layer 135 in an environment containing another component or its starting materials or precursors. According to another embodiment, the antireflection layer 139 may be a silicon nitride layer or may be formed from tantalum oxide, which may contain other major components, for example, boron, or may be a material containing chromium, e.g.,It contains a chromium oxide CrO.
[0075] The reflective multilayer system 120 can include a cover layer 129 on a side facing away from the substrate 110. The cover layer 129 can be a layer consisting of or containing ruthenium (Ru). The thickness of the cover layer 129 can be in the range of approximately 2 nm to 4 nm. The cover layer 129 can protect the multilayer system 120 during the fabrication of the absorber structure 130. According to another embodiment, the cover layer 129 can be a titanium oxide (TiO) layer.
[0076] The substrate 110 can contain a conductive interface layer 119 between the reflective multilayer system 120 and the main substrate region 115. The conductive interface layer 119 can be a metal film containing or consisting of, for example, tantalum (Ta) or chromium (Cr). The conductive interface layer 119 can at least locally connect a region of the multilayer system 120 in the structural section 191 with the frame section 192 and can prevent the structural section 191 from becoming charged during exposure, so that exposure is not affected by electrostatic charge.
[0077] The frame trench 180 can extend down to an upper edge of the conductive interface layer 119, can extend into the conductive interface layer 119, or can partially penetrate the conductive interface layer 119, with remnants of the conductive interface layer 119 forming bridges between the structural section 191 and the frame section 192.
[0078] In Fig. 3A The protective structure 200 is a single layer that is directly bonded or deposited onto a surface of the substrate main area 115. Adhesion between a directly bonded protective structure 200 and the substrate main area 115 can be based on chemical bonds, hydrogen bonds, metallic bonds, ionic and / or covalent bonds between the substrate main area 115 and the protective structure 200. Direct bonding can involve applying a moderate mechanical force that presses the protective structure 200 and the photomask 100 against each other, thermal treatment of at least one of the two bonding surfaces at a moderate temperature below 120°C, e.g., below 100°C, or a combination of both, e.g., fusion bonding, thermo-compressive bonding, or bonding by means of atomic rearrangement.Direct bonding can involve the absence of any additional intermediate layer, particularly the absence of resin-containing adhesives.
[0079] Alternatively, the protective structure 200 can be deposited onto the exposed surface of the substrate main area 115, e.g. by spraying, whereby the formation of the protective structure 200 can include baking the sprayed protective structure 200 at moderate temperatures below 120°C, e.g. below 110°C, in order to drive off volatile substances.
[0080] In Fig. 3B The protective structure 200 comprises a rigid main support 230 and an adhesive layer 220 that bonds the rigid main support 230 to the substrate main area 115 of the reflective photomask 100. The main support 230 can comprise a plate or frame containing glass, metal, a semiconductor material, e.g., crystalline or polycrystalline silicon, a ceramic, silicon oxide, a sintered material, and / or a rigid resist.
[0081] The adhesive layer 220 reversibly bonds or connects the main carrier 230 and the main substrate 110. For example, the adhesive layer 220 contains an adhesive, an adhesive film, and / or an adhesive foil. The adhesive layer 220 can, for example, contain a polyacrylate.
[0082] In Fig. 3C comprises the protective structure 200, a flexible carrier tape 240, and an adhesive layer 220, which reversibly bonds the flexible carrier tape 240 to the substrate main area 115. The flexible carrier tape 240 can, for example, consist of or contain polyolefin, PET (polyethylene), or PVC (polyvinyl chloride). The thickness of the flexible tape can, for example, be in the range of 60 µm to 100 µm. The adhesive layer 200 can contain an adhesive film.
[0083] Fig. 4A - 4C refer to photomasks 100 whose substrates 110 contain backside films 114. The protective structures 200 are formed directly on a surface of the backside film 114. The backside films 114 may contain a conductive layer, e.g., a CrN (chromium nitride) layer. For further details of the protective structures 200 and the photomasks 100, reference is made to the preceding description and the figures.
[0084] Fig. Figures 5A to 5B show a mechanical adapter 300 with a right-angled receiving bore 310 suitable for supporting a reflective photomask 100. The receiving bore 310 can be a recess formed in an upper surface of the mechanical adapter 300. The lateral dimensions d2, d3 of the receiving bore 310 can be equal to or slightly larger than the lateral dimensions of the photomask 100.
[0085] The contour 303 of the mechanical adapter 300 can be the same as, or approximate, the contour of a standard semiconductor wafer. For example, the mechanical adapter 300 can be round with a radius r1 of 150 mm. For tools designed to apply temporary carriers, back-grinding belts, slicing belts, or receiving belts to semiconductor wafers, for example, for a laminating tool, the mechanical adapter 300, equipped with a photomask 100 in the receiving bore 310, can simulate the presence of a semiconductor wafer.
[0086] Fig. Figures 6A to 6D illustrate the use of a protective structure 200 in a method for producing a photomask 100, wherein the protective structure 200 is bonded to the photomask 100 in a processing phase when the photomask 100 is in the state of a mask blank with an unstructured absorber layer stack 134. Other embodiments can bond the protective structure 200 to the photomask 100 in an earlier processing phase, e.g., before depositing the absorber layer stack 134 or before forming the reflective multilayer system 120.
[0087] The upper half of Fig. Figure 6A shows a photomask 100 with a substrate 110 containing a backside film 114 formed on a surface on the back side of a substrate main region 115. For further details of the photomask 100, reference is made to the description of the preceding figures. The lower half of Fig. Figure 6A shows a protective structure 200 with a rigid main support 230. An adhesive 221 is applied, for example, by dripping or by applying an adhesive film to an upper surface of the main support 230. Alternatively, an adhesive can be applied to the exposed surface of the backing film 114 or to both the main support 230 and the backing film 114. The protective structure 200 and the photomask 100 are brought into contact with each other along the upper surface of the main support 230 and along the exposed surface of the backing film 114.
[0088] As in Fig. As shown in 6B, the adhesive 221 is formed by Fig. 6A an adhesive layer 220 bonds the main carrier 230 to the photomask 100. The adhesive layer 220 and the main carrier 230 form a protective structure 200 for the back side of the photomask 100. The photomask 100 and the protective structure 200 form a photomask assembly 900 as described above. Processing on the front side of the photomask 100 can be continued, for example, by structuring the absorber layer stack 134 and / or forming a frame trench.
[0089] Fig. 6C shows one from the absorber layer stack 134 of Fig. 6B formed absorber structure 130. The protective structure 200 can then be removed by means of UV radiation and mechanical peeling.
[0090] Fig. 6D shows the 200 of the protective structure. Fig. 6C disassembled photomask 100.
[0091] A method for fabricating a semiconductor device may include providing a reflective photomask comprising a substrate, a reflective multilayer system on a first substrate surface, and an absorber structure on the reflective multilayer system at a front face of the photomask; providing a protective structure on a second substrate surface at a rear face of the photomask; exposing a semiconductor in an EUVL apparatus with EUV light reflected by the reflective photomask equipped with the protective structure; and removing the protective structure after exposing the semiconductor substrate. More than one exposure may be performed, and the photomask may be reassembled in the EUVL apparatus more than once before the protective structure is replaced. For details of the photomask and the protective structure, reference is made to the preceding parts of the description and the figures.
Claims
[1] Photomask assembly comprising: a reflective photomask (100) with a substrate (110), and a reflective multilayer system (120) on a first substrate surface (111) of the substrate (110) on a front side of the photomask (100); and a protective structure (200) on a second substrate surface (112) of the substrate (110) on a backside of the photomask (100), wherein the protective structure (200) is glued or bonded directly to the second substrate surface (112) and is removable from the photomask (100) at a temperature below 150 degrees Celsius. [2] Photomask assembly according to the preceding claim, wherein the substrate (110) has a backside film (114) and wherein the protective structure (200) is formed directly on the backside film (114). [3] Photomask assembly according to one of the preceding claims, wherein the protective structure (200) is removable from the photomask (100) by applying a temperature between 110 degrees Celsius and 150 degrees Celsius, applying electromagnetic radiation, applying a debonding fluid configured to release a connection (290) between the photomask (100) and the protective structure (200), and / or applying a moderate mechanical force. [4] Photomask assembly according to one of the preceding claims, wherein the protective structure (200) comprises a main carrier (230) and an adhesive layer (220), wherein the adhesive layer (220) adheres the main carrier (230) to the photomask (100). [5] The photomask assembly of any one of claims 1 to 3, wherein the protective structure (200) comprises a carrier tape (240) and an adhesive layer (220), the adhesive layer (220) adhering the carrier tape (240) to the reflective photomask (100). [6] Photomask assembly according to any one of the preceding claims, further comprising: a mechanical adapter (300) having a receiving bore (310) suitable for supporting the reflective photomask (100), wherein a contour (305) of the mechanical adapter (300) corresponds to a contour of a standard wafer. [7] A method of manufacturing a reflective photomask, the method comprising: Forming a reflective photomask (100) with a substrate (110), a reflective multilayer system (120) on a first substrate surface (111) of the substrate (110), and an absorber structure (130) on the multilayer system (120) on a front side of the photomask (100); and Bonding or gluing, before forming the absorber structure (130), a protective structure (200) to a second substrate surface (112) of the substrate (110) on a back side of the photomask (100), wherein the protective structure (200) is removable from the photomask (100) at a temperature below 150 degrees Celsius. [8] Method according to the preceding claim, wherein the protective structure (200) is bonded or glued to the photomask (100) before forming the reflective multilayer system (120). [9] Method according to one of the two preceding claims, wherein the protective structure (200) is removed from the photomask (100) after formation of the absorber structure (130).
Citation Information
Patent Citations
Worm casting substrate
DE112009002622T5
Substrate with conductive film, substrate with multi-layer reflective film and reflection mask blank for EUV lithography
DE112012000658T5
Reflective mask and exposure device
JP2012182235A
Coatings on reflective mask substrates
US6352803B1