GATE STRUCTURE WITH OXYGEN BARRIER LAYER AND METHOD FOR ITS MANUFACTURING
An ultra-thin oxygen barrier layer in semiconductor devices addresses oxygen migration issues, enhancing device reliability and threshold voltage tuning, while reducing manufacturing complexity and costs.
Patent Information
- Application Number
- DE102023129331
- Authority / Receiving Office
- DE · DE
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-08-16
- Filing Date
- 2023-10-25
- Publication Date
- 2024-10-24
AI Technical Summary
The migration of oxygen from the gate dielectric into metal gates and interfacial layers during thermal processing in advanced technology nodes leads to oxygen vacancies, impairing the reliability of semiconductor devices by affecting the flat band voltage and device performance.
Incorporation of an ultra-thin oxygen barrier layer in the gate dielectric to prevent oxygen migration, combined with n-dipole or p-dipole processes for threshold voltage tuning, which enhances the stability of metal gates and reduces the need for heat treatments to repair oxygen vacancies.
This approach improves the reliability of semiconductor devices by minimizing oxygen vacancies, maintaining gate resistance, and providing flexibility in threshold voltage tuning, thereby reducing manufacturing complexity and costs.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims priority to U.S. Provisional Patent Application No. 63 / 461,118, filed on 21. April 2023, which is incorporated into the present application by reference. BACKGROUND
[0002] The IC industry (IC: integrated semiconductor circuit) has experienced exponential growth. Technological Advances in IC materials and designs have produced generations of ICs, with each generation producing smaller and more complex circuits than the previous generation. In the course of IC evolution, the functional density (ie, the number of interconnected devices per chip area) has generally increased, while the Structure size (i.e., the smallest component (or line) that can be produced using a manufacturing process) This process of scaling generally offers benefits by increasing production output and reducing the associated costs. However, this scaling also increases the complexity of processing and manufacturing of ICs increased. BRIEF DESCRIPTION OF THE DRAWINGS
[0003] Aspects of the present disclosure are best understood from the following detailed description in in conjunction with the accompanying drawings. It should be noted that, in accordance with industry practice, various features are not shown to scale. In fact, the dimensions of the various Features may be arbitrarily enlarged or reduced for the sake of clarity. Figures 1-5 are perspective views of different stages of the production of a Semiconductor device structure according to some embodiments. Fig. 6A, Fig. 6B and Fig. 6C are side sectional views of the semiconductor device structure taken along the Line AA, line BB and line CC of Fig. 5, respectively. Figures 7A-12A and 17A are side sectional views of various stages of the manufacture of the Semiconductor device structure created along the cross section AA of Fig. 5, according to some Embodiments. Figures 7B-12B and 17B are side sectional views of various stages of the manufacture of the Semiconductor device structure created along the cross section BB of Fig. 5, according to some Embodiments. Figures 7C-12C and 17C are side sectional views of different stages of the manufacture of the Semiconductor device structure created along the cross section CC of Fig. 5, according to some Embodiments. Figures 13-16 are enlarged views of a portion of Figure 12B showing various stages of manufacturing a replacement gate structure for the semiconductor device structure according to some embodiments. Figs. 18A-30A, 18B-30B, 18C-30C, 18D-30D, 18E-30E, 18F-30F show the formation of gate structures 200A- 200F for a semiconductor device according to various embodiments. Fig. 31 shows a flow diagram of a process for forming the gate structures 200A-200F of Figs. 18A-30F according to various embodiments. Fig. 32 is a cross-sectional view of a semiconductor device structure showing an intermediate manufacturing stage according to some embodiments. Fig. 33 shows a cross-sectional view of a part of the semiconductor device structure taken along the cross section E- E of Fig. 32, according to some embodiments. Fig. 34 shows a sectional view of a part of the semiconductor device structure taken along the cross section FF of Fig. 32, according to some embodiments. Figs. 35A-45A, 35B-45B, 35C-45C, 35D-45D, 35E-45E, 35F-45F show the formation of gate structures 300A- 300F for a semiconductor device according to various embodiments. Fig. 46 is a sectional view of a semiconductor device structure showing an intermediate manufacturing stage according to some embodiments. Fig. 47 shows a sectional view of a part of the semiconductor device structure taken along the cross section GG of Fig. 46, according to some embodiments. Fig. 48 shows a sectional view of a part of the semiconductor device structure taken along the cross section HH of Fig. 46, according to some embodiments. Fig. 49 shows a flowchart of a process for forming the gate structures 300A-300F Fig. 35A-45F according to various embodiments. DETAILED DESCRIPTION
[0004] The following disclosure provides many different embodiments or examples for implementing various features of the provided item. Specific examples of components and Arrangements are described to simplify the present disclosure. These are, of course, merely examples and are not intended to be limiting. For example, the manufacture of a first element over or on a second Element in the following description may include embodiments in which the first and second elements are direct contact, and it may also include embodiments in which additional elements between the first and the second element, so that the first and second element are not are in direct contact. Furthermore, in the present disclosure, reference numbers and / or letters may be the various examples. This repetition is for the sake of simplicity and clarity and does not, in itself, prescribe any relationship between the various embodiments and / or configurations discussed.
[0005] In addition, spatially relative terms such as ´´located underneath´´, ´´beneath´´, ´´lower´´ / ´´lower´´, ´´above´´, ´´upper´´ / ´´upper´´ and the like, for easy description of the relationship of an element or structure to one or more other elements or structures that are in The spatially relative terms are intended to be used in addition to the spatial Orientation may include other orientations of the device in use or operation. The device can be oriented differently (rotated by 90 degrees or in a different orientation), and the spatially relative Descriptors used here can also be interpreted accordingly.
[0006] The present disclosure relates generally to semiconductor devices, and more particularly, the present Disclosure Field effect transistors (FETs) (FET: field effect transistor), such as planar FETs, three-dimensional fin-shaped FETs (FinFETs), gate-all-around devices (GAA devices) (e.g. horizontal gate-all-around FETs (HGAA FETs), vertical gate all-around FETs (VGAA FETs), vertical FETs, forksheet FETs or complementary FETs (CFETs). Although the embodiments of this disclosure are discussed with reference to ATM devices, Implementations of some aspects of the present disclosure may also be used in other processes and / or in other A person skilled in the art will readily recognize modifications that may be made without departing from the intended scope of this disclosure.
[0007] With the trend of scaling, the device size and the device mounting area (ie the physical space occupied by a device) is becoming smaller and smaller. In advanced technology nodes, Packaging and bonding processes that include thermal processing, usually with an additional thermal budget, which allows the migration of oxygen from the gate dielectric into metal gates and / or interfacial layers (IL). An additional thermal budget can prevent the oxidation of the metal elements in metal gates, creating a relatively stable state. In addition, oxygen from a first side of the gate dielectric, which is located between the gate dielectric and the metal gate, in metal gates. On the other hand, oxygen can also migrate into the IL, causing a thickening of the IL (as a result of a Regrowth of the IL) from a second side of the gate dielectric, which is located between the gate dielectric and the IL The migration of oxygen from the gate dielectric can lead to the generation of Oxygen vacancies in the gate dielectric, resulting in a shift or controllability of a flat band voltage (V ) of the device. As a result, the reliability of the device is impaired. For Facebook a high-k metal gate (HKMG) configuration (i.e. a structure with a gate dielectric and a Metal gate, where the gate dielectric has a high dielectric constant to achieve high I), which is used in 28 nm DS Technology nodes and below, the reduction of oxygen vacancies in gate dielectrics is subject continuous development to achieve better reliability.
[0008] In gate stack structures disclosed in this specification, an ultra-thin insertion layer (i.e. i.e., oxygen barrier layer) on the gate dielectric is used to prevent oxygen migration from the gate dielectric the metal gate. The ultra-thin insertion layer can block oxygen in insulators (ie, gate dielectrics and interface layers) to reduce the generation of oxygen vacancies in the gate dielectrics, and to protect the metal gate from further oxidation (and consequently increase its resistivity), thereby reducing Device is subject to less impairment and the reliability of the The ultra-thin insertion layer can be fabricated using an n-dipole or p-dipole process combined to achieve a single p-edge or n-edge work function metal knob, thereby Process problems and costs of advanced technology nodes are reduced. Since the generation of Oxygen vacancies can be suppressed by the ultra-thin insertion layer, the number of Heat treatments to repair oxygen vacancies can be reduced, thereby allowing IL regrowth and Diffusion of dopants into the source / drain can be avoided. The planned gate stack structures improve also a gate filling window, and achieve a lower gate resistance for multiple Threshold voltage tuning (Vth tuning) with photolithographic patterning. Multiple Vth tuning can be achieved by embedding n-dipole or p-dipole elements into a high-k dielectric layer of different Gate structures in different device areas with different doping densities, with which Threshold voltages for gate structures can be effectively tuned. These Methods improve the flexibility in tuning the threshold voltage compared to conventional Devices, as will be discussed in more detail below.
[0009] Figures 1-49 show exemplary processes for manufacturing a semiconductor device structure 100 according to Embodiments of the present disclosure. It is understood that further steps before, during, and after the The processes shown in Fig. 1 to 49 can be provided and some of the steps described below can be other embodiments of the method can be replaced or omitted. The order of the steps / Processes is not restrictive; it is interchangeable.
[0010] Figures 1-5 are perspective views of various stages of the manufacture of a Semiconductor device structure 100 (e.g., a nano-FET) according to some embodiments. As shown in Fig. 1, a semiconductor device structure 100 comprises a stack of semiconductor layers 104 disposed over a front side of a Substrate 101. The substrate 101 may be a semiconductor substrate, such as a bulk substrate, or The substrate 101 may be a single-crystal semiconductor material, such as silicon (Si), germanium (Ge), Silicon germanium (SiGe), gallium arsenide (GaAs), indium antimonide (InSb), gallium phosphide (GaP), gallium antimonide (GaSb), indium aluminum arsenide (InAlAs), indium gallium arsenide (InGaAs), gallium antimony phosphide (GaSbP), Gallium arsenic antimonide (GaAsSb) and indium phosphide (InP), but is not limited to these. Embodiments, the substrate 101 is a silicon-on-insulator (SOI) substrate having a Insulation layer (not shown) arranged between two silicon layers for reinforcement. In one aspect The insulation layer is an oxygen-containing layer. Other substrates, such as single-layer, multilayer or gradient substrates can be used.
[0011] The substrate 101 may have various regions coated with dopants (e.g., dopants with p- or n- conductivity). Depending on the circuit design, the dopants can be, for example, boron for a p- Field effect transistor (PFET) (PFET: p-type field effect transistor) and phosphorus for an n-type field effect transistor (NFET) (NFET: n-type field effect transistor).
[0012] The stack of semiconductor layers 104 comprises alternating semiconductor layers of different Materials to facilitate the formation of nanolayer channels in a multi-gate device, such as nanolayer channel FETs. In some embodiments, the stack of semiconductor layers 104 includes first semiconductor layers 106 and second semiconductor layers 108. In some embodiments, the stack of semiconductor layers 104 comprises alternating first semiconductor layers 106 and second semiconductor layers 108. The first semiconductor layers 106 and the second semiconductor layers 108 are made of semiconductor materials with different etch selectivity and / or oxidation rate For example, the first semiconductor layers 106 may be made of a first semiconductor material, suitable for n-nano-FETs, such as silicon, silicon carbide or the like, and the second semiconductor layers 108 may be made of a second semiconductor material suitable for p-nano-FETs, such as Silicon germanium or the like. In some examples, the first semiconductor layers 106 may be made of Si and the second semiconductor layers 108 may be made of SiGe. Alternatively, in some embodiments, each of the two semiconductor layers 106, 108 materials such as Ge, SiC, GeAs, GaP, InP, InAs, InSb, GaAsP, AlInAs, AlGaAs, InGaAs, GaInP, GaInAsP or combinations thereof. Each of the layers of the stack of Semiconductor layers 104 can be deposited using a process such as chemical vapor deposition (CVD) (CVD: chemical vapor deposition), atomic layer deposition (ALD), vapor phase epitaxy (VPE), and atomic layer deposition (ALD). epitaxy), molecular beam epitaxy (MBE) (MBE: molecular beam epitaxy), a metal-organic chemical Deposition process (MOCVD process) (MOCVD: metalorganic chemical vapor deposition (MOCVD) or other suitable processes growth processes epitaxially.
[0013] Due to the high etching selectivity between the first semiconductor materials and the second semiconductor materials the second semiconductor material of the second semiconductor layers 108 can be removed without removing the first semiconductor material of the first semiconductor layers 106, whereby the first semiconductor layers 106 are structured can be used to create one or more nanolayer or nanostructure channels of the semiconductor device structure 100. The term nanolayer is used in this description to Material part with dimensions in the nanoscale or even microscale and with an elongated shape regardless of the The cross-sectional shape of this part is used. Consequently, this term covers both elongated material parts with circular and essentially circular cross-section as well as rod or bar-shaped material parts, such as Example with a cylindrical or substantially rectangular cross-section. One or the Several nanolayer channels of the semiconductor device structure 100 can be enclosed by a gate electrode. The semiconductor device structure 100 may include a nanolayer transistor. The nanolayer transistors may be Nanowire transistors, gate-all-around transistors (GAA transistors), multi-bridge channel transistors (MBC- Transistors) or other transistors with a gate electrode surrounding the channels. The Using the first semiconductor layers 106 to define one or more channels of the Semiconductor device structure 100 is discussed in more detail below.
[0014] Each first semiconductor layer 106 has a thickness in a range between about 5 nm and about 30 nm. Each second semiconductor layer 108 may have a thickness equal to, less than, or greater than the thickness of the first semiconductor layer 106. In some embodiments, every second semiconductor layer 108 has a thickness in a range between about 2 nm and about 50 nm. Three first semiconductor layers 106 and three second semiconductor layers 108 are arranged alternately as shown in Fig. 1, which is for illustrative purposes and does not beyond what is explicitly set forth in the claims. It is understood that any number of first semiconductor layers 106 and second semiconductor layers 108 in the stack of semiconductor layers 104 and that the number of layers depends on the predetermined number of channels for the semiconductor device structure 100. Although the stack of semiconductor layers 104 is shown as a second semiconductor layer 108 as the bottom layer, in some embodiments the bottom layer Layer of the stack of semiconductor layers 104 may be a first semiconductor layer 106.
[0015] In Fig. 2, fin structures 112 are formed from the stack of semiconductor layers 104. Each fin structure 112 has an upper part with the semiconductor layers 106, 108 and a well part 116, which consists of the substrate 101 The fin structures 112 can be formed by patterning a hard mask layer (not shown) on the Stack of semiconductor layers 104 using one or more photolithographic processes and etching processes The etching process can be dry etching, wet etching, reactive ion etching (RIE) and / or other suitable processes. The photolithographic process may include double patterning or In general, double structuring or Multiple structuring processes photolithographic and self-aligned processes with which structures are created which, for example, have pitches smaller than those otherwise possible with a single direct photolithographic process. For example, in a multi-patterning process over a substrate, a A sacrificial layer is produced, which is then structured using a photolithographic process. Along the structured Spacers are manufactured using a self-aligned process for the sacrificial layer. The sacrificial layer is then removed, and the remaining spacers can then be used to pattern the fin structures 112. In any case, with one or more etching processes, trenches 114 in unprotected areas are created by the Hard mask layer, through the stack of semiconductor layers 104 and into the substrate 101, whereby the A plurality of extending fin structures 112 remains. The trenches 114 extend along the x- Direction.
[0016] Fig. 2 further shows the fin structures 112 with substantially vertical side walls, so that a width of the fin structures 112 is substantially the same, and each of the first semiconductor layers 106 and the second Semiconductor layers 108 in the fin structures 112 have a rectangular shape. In some embodiments, the Fin structures 112 have tapered side walls such that a width of each of the fin structures 112 in a continuously increases towards the substrate 101. In such cases, each of the first semiconductor layers 106 and the second semiconductor layers 108 in the fin structures 112 have a different width and be trapezoidal.
[0017] In Fig. 3, after the fin structures 112 have been produced, an insulating material 118 is formed on the substrate 101. The Insulating material 118 fills the trenches 114 between adjacent fin structures 112 until the fin structures 112 are inserted into the insulating material 118. Then, a planarization operation, such as a chemical-mechanical Polishing process (CMP process) (CMP: chemical mechanical polishing) and / or an etching back process, so that the top side of the fin structures 112 is exposed. The insulating material 118 can be made of silicon oxide, silicon nitride, Silicon oxide nitride (SiON), SiOCN, SiCN, fluorine-doped silicate glass (FSG), a low-k dielectric material or a other suitable dielectric material. The insulating material 118 may be made of any suitable Processes such as low-pressure chemical vapor deposition (LPCVD) plasma enhanced chemical vapor deposition (PECVD) (PECVD: plasma enhanced CVD) or flowable CVD (FCVD) (FCVD: flowable CVD).
[0018] Thereafter, the insulating material 118 is cut out to form an insulating region 120. After the cutout Parts of the fin structures 112, such as the stack of semiconductor layers 104, can be sandwiched between adjacent Isolation areas 120 protrude. The isolation areas 120 may have top surfaces that are flat, as shown, convex, concave, or a combination thereof. By removing the insulating material 118, the trenches 114 between the adjacent fin structures 112. The isolation region 120 can be exposed using a suitable process, such as a dry etching process, a wet etching process, or a combination thereof. In this embodiment, the isolation regions 120 are formed using dilute hydrofluoric acid (dHF) (dHF: dilute hydrofluoric acid) which is used for the insulating material 118 in relation to the stack of semiconductor layers 104 selective. After completion of the recessing, a top side of the insulating material 118 can be contacted with a surface of the second Semiconductor layers 108 which are in contact with the well region 116 made from the substrate 101, be at the same height and below this.
[0019] In Fig. 4, one or more sacrificial gate structures 130 are formed over a portion of the fin structures 112. Each sacrificial gate structure 130 may include a sacrificial gate dielectric layer 132, a sacrificial gate electrode layer 134, and a mask layer 136. The dielectric sacrificial gate layer 132, the sacrificial gate electrode layer 134 and the Mask layer 136 can be formed by sequentially depositing unstructured layers of the dielectric sacrificial gate layer 132, the sacrificial gate electrode layer 134 and the mask layer 136 and subsequent structuring these layers into the sacrificial gate structures 130. Gate spacers 138 are then sidewalls of the sacrificial gate structures 130. The gate spacers 138 can be formed, for example, by conformal Depositing one or more layers for the gate spacers 138 and anisotropic etching of the one or more layers. Although one sacrificial gate structure 130 is shown, in some embodiments, two or more sacrificial gate structures 130 may be arranged along the x-direction.
[0020] The sacrificial gate dielectric layer 132 may comprise one or more layers of dielectric material, such as a silicon oxide-based material. The sacrificial gate electrode layer 134 may comprise silicon, such as polycrystalline silicon or amorphous silicon. The mask layer 136 may have more than one layer, such as an oxide layer and a nitride layer. The gate spacer 138 may be made of a dielectric material, such as such as silicon oxide, silicon nitride, silicon carbide, silicon oxide nitride, SiCN, silicon oxide carbide, SiOCN and / or combinations thereof, be manufactured.
[0021] The parts of the fin structures 112 which are formed by the sacrificial gate electrode layer 134 of the sacrificial gate structure 130 serve as channel regions for the semiconductor device structure 100. The fin structures 112, which are opposite sides of the sacrificial gate structure 130 are partially exposed, define source / drain regions (S / D regions) for the semiconductor device structure 100. In some cases, some S / D regions of different transistors For example, different S / D areas can be connected and used as several functional transistors are implemented. It is understood that the source region and the drain region can be used interchangeably, which allows the epitaxial structural elements to be produced in these areas to be are essentially the same.
[0022] In Fig. 5, the parts of the fin structures 112 in the S / D areas (e.g. areas on opposite sides of the sacrificial gate structure 130) to below the top of the insulation region 120 (or the insulation material 118) by removing parts of the fin structures 112 that are not covered by the sacrificial gate structure 130. The recessing of the parts of the fin structures 112 can be carried out with an etching process, either an isotropic or anisotropic etching process, or an etching process which is also selective with respect to one or more crystalline planes of the substrate 101. The etching process may be a dry etch, such as an RIE, NBE or the like, or a wet etching, such as using tetramethylammonium hydroxide (TMAH), Ammonium hydroxide (NH OH) or another suitable etchant. Trenches 119 are formed in the S / D areas in the 4 Result of the recess of the parts of the fin structures 112 manufactured.
[0023] Figures 6A, 6B and 6C are side sectional views of the semiconductor device structure 100 taken along the Line AA, Line BB and Line CC of Fig. 5, respectively. Figs. 7A-12A and 17A are Side sectional views of various stages of fabrication of the semiconductor device structure 100 taken along the Cross section AA of Fig. 6, according to some embodiments. Figs. 7B-12B and 17B are Side sectional views of various stages of fabrication of the semiconductor device structure 100 taken along the Cross section BB of Fig. 5, according to some embodiments. Figs. 7C-12C and 17C are Side sectional views of various stages of fabrication of the semiconductor device structure 100 taken along the Cross section CC of Fig. 5, according to some embodiments. The cross section AA is in a plane of the fin structure 112 (channel / fin section) along the x-direction. The cross section BB is in a plane perpendicular to the cross section AA, and is in the sacrificial gate structure 130 (gate cut). The cross section CC is in a plane which perpendicular to the cross section AA, and is in the source / drain region (e.g. epitaxial S / D structure elements 146, which are in Fig. 9A) along the y-direction.
[0024] In Figs. 7A-7C, edge portions of every second semiconductor layer 108 of the stack of semiconductor layers 104 horizontally along the x-direction. By removing the edge parts of the second semiconductor layers 108, Cavities are formed. In some embodiments, the portions of the second semiconductor layers 108 are selective wet etching process. In cases where the second semiconductor layers 108 are made of SiGe and the first semiconductor layers 106 are made of silicon, the second semiconductor layer 108 can be selectively Using a wet etching agent, such as ammonium hydroxide solution (NH OH solution), 4 Tetramethylammonium hydroxide solution (TMAH solution), ethylenediamine pyrocatechol solution (EDP solution) or Potassium hydroxide solution (KOH solution), but not limited to.
[0025] After removing the edge parts of every second semiconductor layer 108, a dielectric layer is deposited in the cavities deposited to produce dielectric spacers (or so-called inner spacers) 144. The dielectric spacers 144 may be made of a low-k dielectric material such as SiON, SiCN, SiOC, SiOCN or SiN. The dielectric spacers 144 can be manufactured by first conformal dielectric layer is produced using a conformal deposition process such as ALD, after which An anisotropic etching follows to remove parts of the conformal dielectric layer, except for the dielectric spacers 144. The dielectric spacers 144 are removed during the anisotropic etching process protected by the first semiconductor layers 106. The remaining second semiconductor layers 108 are sandwiched between the dielectric spacers 144 along the x-direction.
[0026] In Figs. 8A-8C, epitaxial S / D structural elements 146 in the source / drain regions (S / D regions) The epitaxial S / D structure elements 146 are manufactured such that each sacrificial gate structure 130 is between respective adjacent pairs of S / D regions. In an example shown in Fig. 9A, a pair of epitaxial S / D structure elements 146, which is arranged on one side of the sacrificial gate structure 130, as a source structural element / terminal, and / or the pair of epitaxial S / D structural elements 146 located on the other side of the sacrificial gate structure 130 is referred to as a drain structure element / terminal. The source Structure element / terminal and the drain structure / terminal are separated by the channel layers (e.g. the first semiconductor layers 106). The epitaxial S / D structure elements 146 are connected to the first semiconductor layer 106 under the sacrificial gate structure 130. In some cases, the epitaxial S / D structure elements 146 may be uppermost semiconductor channel, ie the first semiconductor layer 106 is grown under the Sacrificial gate structure 130 is in contact with the gate spacers 138. The second semiconductor layer 108 under the Sacrificial gate structure 130 is separated from the epitaxial S / D structure elements 146 by the dielectric spacers 144 separated.
[0027] The epitaxial S / D structure elements 146 can be grown both vertically and horizontally to to form facets that may correspond to crystalline planes of the material used for the substrate 101. In some In these cases, the epitaxial S / D structural elements 146 of a fin structure can be grown and bonded to the epitaxial S / D Structural elements 146 of the adjacent fin structures are fused, as shown in an example in Fig. 8C is.
[0028] The epitaxial S / D structural elements 146 may consist of one or more layers of Si, SiP, SiC, and SiCP for n-channel FETs or Si, SiGe, Ge for p-channel FETs. The epitaxial S / D- Structural elements 146 can be grown using an epitaxial growth process using CVD, ALD or MBE The epitaxial S / D structure elements 146 can be implanted with dopants, followed by a Annealing process is carried out. As n- and / or p-dopants for epitaxial S / D structural elements 146, the dopants discussed above.
[0029] In Figs. 9A-9C, a contact etch stop layer (CESL) 162 is conformally deposited on the exposed surfaces of the semiconductor device structure 100. The CESL 162 covers the sidewalls of the Sacrificial gate structure 130, the insulating material 118, the epitaxial S / D structure elements 146, and the exposed surface of the stack of semiconductor layers 104. The CESL 162 may be an oxygen-containing material or a nitrogen-containing Material such as silicon nitride, silicon carbonitride, silicon oxide nitride, carbon nitride, silicon oxide, silicon carbon oxide or the like or a combination thereof, and can be coated with CVD, PECVD, ALD or another suitable deposition process. Then, a first interlayer dielectric Layer (ILD layer) (ILD: interlayer dielectric) 164 on the CESL 162 above the semiconductor device structure 100 The materials for the first ILD layer 164 may include compounds containing Si, O, C and / or H, such as silicon oxide, TEOS oxide, SiCOH and SiOC. Organic materials such as such as polymers. The first ILD layer 164 can be formed using a PECVD process or another suitable deposition process. In some embodiments, the Semiconductor device structure 100 subjected to a thermal process after the formation of the first ILD layer 164 with which the first ILD layer 164 is annealed.
[0030] In Figs. 10A-10C, after the first ILD layer 164 has been formed, a planarization operation such as CMP is performed on the semiconductor device structure 100 until the sacrificial gate electrode layer 134 is exposed.
[0031] In Figs. 11A-11C, the sacrificial gate structure 130 is removed. The first ILD layer 164 protects the epitaxial S / D Structural elements 146 during the removal of the sacrificial gate structure 130. The sacrificial gate structure 130 can be removed with a plasma dry etching and / or wet etching. For example, in cases where the sacrificial gate electrode layer 134 is polysilicon and the first ILD layer 164 is silicon oxide, a wet etchant, such as Tetramethylammonium hydroxide solution (TMAH solution) can be used to selectively without removing the dielectric materials of the first ILD layer 164, the CESL 162 and the gate spacers 138 The sacrificial gate dielectric layer 132 is then removed using plasma dry etching and / or wet etching. By removing the sacrificial gate structure 130 (ie, the sacrificial gate electrode layer 134 and the dielectric sacrificial gate layer 132), a trench 166 is formed in the areas where the Sacrificial gate electrode layer 134 and the sacrificial gate dielectric layer 132 have been removed. Through the trench 166 the top and sides of the stack of semiconductor layers 104 (e.g., the first semiconductor layers 106 and the second semiconductor layers 108) are exposed.
[0032] In Figures 12A-12C, the exposed second semiconductor layers 108 are removed. By removing the second semiconductor layers 108, the dielectric spacers 144 and the first semiconductor layers 106 The removal process can be any suitable etching process, such as dry etching, wet etching or a combination thereof. The etching process may be a selective etching process with which the second semiconductor layers 108 removed without substantially attacking the first semiconductor layers 106. In some Embodiments, the etching process is an isotropic etching process using an etching gas and optionally a carrier gas, wherein the etching gas comprises F and HF, and the carrier gas is an inert gas such as Ar, He, N , combinations 2 2 thereof or the like. After removing the second semiconductor layers 108, openings 151 are formed around the first semiconductor layers 106, and the part of the first semiconductor layers 106 which is not dielectric spacers 144 is exposed towards the openings 151. The remaining first Semiconductor layers 106 may serve as channel regions for the GAA devices, which in some embodiments may include at least one NFET or one PFET. Although not specifically shown, according to some Embodiments of one of the GAA devices, such as the semiconductor device structure 100, an NFET or a PFET be.
[0033] Figures 13-16 are enlarged views of an area 147 of Figure 12B, showing various stages of manufacturing a replacement gate structure 190 for the semiconductor device structure 100 according to some embodiments. As As discussed above, the substrate 101 may have various regions coated with dopants (e.g. Dopants with p- or n-conductivity). In various embodiments the substrate 101 has a region 153 and a region 155 adjacent to the region 153. The region 153 can be a p-region or an n-region, and the region 155 can be referred to as an n-region or a p-region Alternatively, the two regions 153, 155 can be referred to as a p-region or an n-region. In one embodiment, region 153 is an n-type region and region 155 is a p-type region. Although this may be the case in some Figures are not shown to scale, area 153 and area 155 belong to a continuous substrate 101. In some embodiments of the present disclosure, the p-type region used to create a PMOS structure, while the n-region is used to create an NMOS Depending on the circuit design, the regions 153, 155 can be used to produce different types of circuits. For example, the area 153 can be used to manufacture, for example, Peripheral circuits, input / output circuits (I / O circuits), ESD circuits (ESD: electrostatic discharge - electrostatic discharge) and / or analog circuits, and the area 155 can be used to produce of logic circuits. Other areas for the production of other types of circuits are being considered and are intended to be within the scope of the present disclosure.
[0034] In Fig. 13, an interfacial layer (IL) 150 is prepared to cover the exposed surfaces of the first semiconductor layers 106. In some embodiments, the IL 150 may also be on the Well part 116 of the substrate 101. The IL 150 can be an oxygen-containing material or a silicon-containing material, such as silicon oxide, silicon oxynitride, oxynitride, etc. or made from it In one embodiment, the IL 150 is silicon oxide. The IL 150 can be prepared by the first Semiconductor layers 106 and the exposed well part 116 of the substrate 101 are first subjected to a wet process The wet process can be a suitable wet cleaning process or self-compensation wet process. In some embodiments, the wet process is an etching process using at least ozone (O ) and / or 3 Ammonium hydroxide (NH OH). For example, the wet process can use NH OH, HF or diluted HF, deionized water (DI- 4 4 water) (DI: deionized), tetramethylammonium hydroxide (TMAH), another suitable wet etching solution or a combination thereof. In one embodiment, the wet process may comprise a standard solution 2 (SC2) (SC2: standard clean-2) followed by a standard solution 1 (SC1) (SC1: standard clean-1), where SC2 is a mixture of DI- Water, hydrochloric acid (HCl) and hydrogen peroxide (HO ), and the SC1 is a mixture of DI water, NH OH 2 2 4 and HO. In some embodiments, an isopropyl alcohol (IPA) may be used after the SC. Another 2 2 1 suitable wet cleaning process, such as an APM process, which contains at least water (HO), ammonium hydroxide (NH OH) 2 4 and hydrogen peroxide (HO ), an HPM process comprising at least HO, HO and hydrogen chloride (HCl), 2 2 2 2 2 an SPM process (also known as Piranha cleaning) which contains at least HO and sulphuric acid (H SO ), or a 2 2 2 4 Combination of these can also be used.
[0035] Additionally or alternatively, the IL 150 can be produced by a wet oxidation process by which a outer part of the first semiconductor layers 106 and an outer part of the exposed well part 116 of the substrate 101 oxidized. That is, the outer part of the first semiconductor layers 106 and the exposed well part 116 of the Substrate 101 are the IL 150 or are part of the IL 150. After completion of the oxidation, the outer part encloses the first semiconductor layers 106 and the well portion 116 of the substrate 101 and is in contact with them. In some In embodiments, the IL 150 may be oxidized using an oxidation process, such as a thermal Oxidation process, a rapid thermal oxidation process (RTO process) (RTO: rapid thermal oxidation), a In-situ steam generation (ISSG) process or an enhanced in-situ steam generation process (EISSG process) (EISSG: enhanced in-situ steam generation). In a For example, the IL 150 is manufactured by the first semiconductor layers 106 and the well part 116 of the substrate 101 rapid thermal annealing (RTA) in an oxygen-containing environment The thermal oxidation can be carried out at a temperature of about 600 degrees Celsius to about 1100 degrees Celsius for a period of about 10 seconds to about 30 seconds. The temperature and the The duration of oxidation can contribute to the thickness of the IL 150. For example, higher temperatures and a longer period of time lead to a thicker IL 150. Alternatively, the IL 150 can also be an oxide produced by CVD, ALD or a suitable conformal deposition process is used.
[0036] The IL 150 has a uniform thickness on the exposed surfaces of the first semiconductor layers 106 and on the well portion 116 of the substrate 101. In some embodiments, the IL 150 has a thickness T1 and the first Semiconductor layer 106 has a thickness T0, and a ratio of T1:T0 is in a range from about 1:5 to about 1:30.
[0037] In Fig. 14, a high-k dielectric layer 160 (HK dielectric layer) is deposited on the exposed surfaces of the Semiconductor device structure 100 is fabricated. In some embodiments, the HK dielectric layer 160 is formed manufactured to surround and contact the IL 150. The dielectric HK layer 160 is also deposited on the exposed surface of the insulating material 118. The dielectric HK layer 160 may be a single layer or a multilayer structure. In one embodiment, the dielectric HK layer 160 is a two-layer structure with a first dielectric HK layer 160a and a second dielectric HK layer 160b. For the first dielectric HK layer 160a and the second dielectric HK layer 160b, a material can be used that chemically different from each other. Suitable materials for the dielectric HK layer 160 can, for example, Hafnium oxide (HfO ), hafnium silicate (HfSiO), hafnium silicon oxide nitride (HfSiON), hafnium aluminum oxide (HfAlO), 2 Hafnium lanthanum oxide (HfLaO), hafnium zirconium oxide (HfZrO), hafnium tantalum oxide (HfTaO), hafnium titanium oxide (HfTiO), Lanthanum oxide (LaO), aluminum oxide (AlO), aluminum silicon oxide (AlSiO), zirconium oxide (ZrO), titanium oxide (TiO), tantalum oxide (Ta O ), yttrium oxide (YO ), silicon oxide nitride (SiON) or the like, or a material whose dielectric constant 2 3 2 3 greater than a dielectric constant of silicon oxide. The dielectric HK layer 160 may be a conformal Layer that is produced using a conformal process, such as an ALD process or a CVD process. dielectric HK layer 160 may have a thickness T2 in a range of about 10 angstroms to about 50 angstroms.
[0038] In Fig. 15, an insertion layer 156 is formed on the HK dielectric layer 160. The insertion layer 156 is formed conformally over the HK dielectric layer 160. In embodiments where the dielectric HK layer 160 is a two-layer structure, the insertion layer 156 is placed on and in contact with a top surface of the second dielectric HK layer 160b, as an enlarged view of a part of the Semiconductor device structure 100 in Fig. 15. The insertion layer 156 serves as an oxygen barrier layer that Oxygen migration from the dielectric HK layer 160 to a later fabricated metal gate (e.g. the Gate electrode layer 165 in Fig. 16 ). The insertion layer 156 can block oxygen in insulators (ie, in the dielectric HK layer 160 and the IL 150) to prevent the generation of oxygen vacancies in the dielectric HK layer 160, an increase in the specific resistance of the metal gate due to to prevent oxidation and promote stress relaxation of the channel regions. Since the generation of Oxygen vacancies are suppressed by the insertion layer 156, the number of heat treatments for Repair of oxygen vacancies can be reduced or even eliminated, causing a thickening of the IL 150 (due to IL regrowth) and the diffusion of dopants into source / drain structural elements can be avoided. If the IL 150 is too thick, the gate filling window is reduced, thereby increasing the resistance of the device and also the ability of threshold voltage tuning may be impaired. By producing the Insertion layer 156 between the dielectric HK layer 160 and the metal gate, the overall reliability of the device is improved, and a large gate filling window can be maintained.
[0039] The insertion layer 156 may be a precious metal or a semi-precious metal, such as gold (Au), platinum (Pt), iridium (Ir), Palladium (Pd), osmium (Os), silver (Ag), rhodium (Rh), ruthenium (Ru) or the like or made from In some embodiments, the insertion layer 156 is a single layer of pure noble metal or nearly pure precious metal with less than 0.01% impurities. In some embodiments, the insertion layer 156 have a noble metal oxide that is electrically conductive, such as ruthenium oxide (RuO ). In some 2 In some embodiments, the insertion layer 156 may comprise tungsten nitride (WN), titanium nitride (TiN), or the like. Insertion layer 156 may be a multilayer structure comprising two or more of the materials discussed herein. For example, the insertion layer 156 may comprise a first layer with a noble metal and a second layer with a noble metal oxide The insertion layer 156 may be formed by ALD, PVD, CVD or other suitable process The insertion layer 156 may have a thickness T3 in a range of about 2 Ångstroms to about 10 Ångstroms If the thickness T3 of the insertion layer 156 is less than about 2 Ångstroms, the insertion layer 156 may not function as intended to effectively block oxygen. On the other hand, if the thickness T3 of the insertion layer 156 is greater than 10 Ångströms, the gate filling window is negatively affected.
[0040] In Fig. 16, a gate electrode layer 165 is formed on the insertion layer 156. The Gate electrode layer 165 encloses a part of each first semiconductor layer 106 and fills the opening 151 (Fig. 15) in the region 153, 155. The gate electrode layer 165 can be deposited such that at least the Nanolayer transistors in the regions 153, 155 are submerged in the gate electrode layer 165. In some Embodiments, the gate electrode layer 165 to to a height above a top surface of the insertion layer 156 over the first semiconductor layer 106. At In some embodiments, the gate electrode layer 165 may be formed using multiple layers with each layer sequentially adjacent to each other using a highly conformal deposition process such as ALD. Other deposition methods such as PVD, CVD, or electroplating may be used. Although not shown, the gate electrode layer 165 a capping layer, a barrier layer, an n-metal work function layer, a p-metal work function layer and a filler material. The capping layer and the barrier layer can be metal oxides, metal nitrides, metal silicates, Transition metal oxides, transition metal nitrides, transition metal silicates, oxide nitrides of metals, metal aluminates, Zirconium silicate, zirconium aluminate, combinations thereof, or the like. The barrier layer may be made of a material which is different from the material of the capping layer. The n-metal work function layer can made of a metallic material, such as W, Cu, AlCu, TiAlC, TiAlN, Ti, TiN, Ta, TaN, Co, Ni, Ag, Al, TaAl, TaAlC, TaC, TaCN, TaSiN, Mn, Zr, other suitable n-work function materials or combinations thereof. The p- Metal work function layer can be made of a metallic material such as W, Al, Cu, TiN, Ti, TiAlN, Ta, TaN, Co, Ni, TaC, TaCN, TaSiN, TaSi , NiSi , Mn, Zr, ZrSi , TaN, Ru, AlCu, Mo, MoSi , WN, other metal oxides, metal nitrides, metal silicates, 2 2 2 2 Transition metal oxides, transition metal nitrides, transition metal silicates, oxide nitrides of metals, metal aluminates, Zirconium silicate, zirconium aluminate, combinations thereof, or the like. After the n-metal work function layer and the p-metal work function layer have been produced, the filler material is deposited, to fill a remainder of the opening 151. The filling material may be a material such as W, Al, Cu, AlCu, W, Ti, TiAlN, TaC, TaCN, TaSiN, Mn, Zr, TiN, Ta, TaN, Co, Ni, combinations thereof, or the like.
[0041] In some embodiments, the gate electrode layer 165 may be the same material as a metal layer 258 ( Figs. 30A-30F) or a metal layer 358 (Figs. 45A-45F), as discussed in more detail below.
[0042] In Figs. 17A-17C, contact openings are made through the ILD layer 164 and the CESL 162 to epitaxial S / D structure element 146. A silicide layer 178 is then deposited on the epitaxial S / D structure elements 146 to make the epitaxial S / D structural elements 146 conductive with later fabricated S / D contacts 176 The silicide layer 178 can be formed by depositing a metal source layer over the epitaxial S / D structural elements 146 and performing a rapid thermal annealing process. Metal source layer comprises a metal layer selected from W, Co, Ni, Ti, Mo and Ta, or a Metal nitride layer selected from tungsten nitride, cobalt nitride, nickel nitride, titanium nitride, molybdenum nitride and tantalum nitride During the rapid annealing process, the part of the metal source layer reacts via the epitaxial S / D structural elements 146 with silicon in the epitaxial S / D structural elements 146 to form the silicide layer 178. Not Reacted parts of the metal source layer are then removed.
[0043] After the silicide layer 178 has been formed, a conductive material is formed in the contact openings and the S / D Contacts 176 are made. The conductive material may be made of a material that is one or several of Ru, Mo, Co, Ni, W, Ti, Ta, Cu, Al, TiN and TaN. Although not shown, a Barrier layer (e.g. TiN, TaN or the like) on sidewalls of the contact openings before fabricating the S / D contacts 176 Then a planarization process, such as CMP, is performed to remove excess deposition of the contact material and expose the top surface of the gate electrode layer 165.
[0044] It is understood that the semiconductor device structure 100 may include further complementary metal oxide semiconductor processes (CMOS processes) CMOS: complementary metal oxide semiconductor) and / or back-end-of-line processes (BEOL processes) For example, gate contacts can be made that provide an electrical connection to the Gate electrode layer 165. An interconnect structure can be formed over the S / D contacts 176 and the gate contacts The interconnect structure may comprise a plurality of dielectric layers and metallic Structural elements, such as conductive traces and conductive vias, embedded in the dielectric Layers that form an electrical connection between various devices on the substrate 101. The semiconductor device structure 100 may also include backside contacts (not shown) on the backside of the substrate 101 by folding the semiconductor device structure 100, removing the substrate 101 and selectively connecting Source or drain structure elements / terminals of the epitaxial S / D structure elements 146 with a rear power rail (e.g. positive voltage VDD or negative voltage VSS) through the rear contacts. Depending on the application, the source or drain structure element / terminal of the epitaxial S / D Structural elements 146 and the gate electrode layer 172 are connected to a front-side power source.
[0045] In some embodiments, the insertion layer (ie, oxygen barrier layer) discussed above may be used to Simplify the complexity of the process, increase throughput (ie, productivity) and reduce Costs can be combined with an n-dipole or p-dipole process. By combining oxygen barrier layer (e.g. the insertion layer 156) with n-dipole or p-dipole processes, a single p-edge work function metal button knob (ie, a single film process) or a single n-edge work function metal knob in advanced technology nodes can be achieved.
[0046] Figures 18A to 30F show the fabrication of gate structures 200A-200F for a semiconductor device 201, such as for example, a GAA-FET structure with multiple threshold voltages, according to various embodiments. Fig. 31 shows a flow diagram of a process 2000 for manufacturing the gate structures 200A-200F shown in Figs. 18A-30F are, according to various embodiments. Figures 18A-30A show the fabrication of a transistor with an n- Gate structure with extremely low threshold voltage (n-eLVT gate structure), such as the gate structure 200A. Fig. 18B- 30B show the fabrication of a transistor with an n-gate structure with ultra-low threshold voltage (n-uLVT- gate structure), such as gate structure 200B. Figures 18C-30C show the fabrication of a transistor with an n- Gate structure with standard threshold voltage (n-sVT gate structure), such as the 200C gate structure. Figures 18D-30D show the fabrication of a transistor with a p-gate structure with standard threshold voltage (p-sVT gate structure), such as the gate structure 200D. Figures 18E-3oE show the fabrication of a transistor with a p-gate structure with ultra-low threshold voltage (p-uLVT gate structure), such as the gate structure 200E. Figures 18F-30F show the Fabrication of a transistor with a p-gate structure with extremely low threshold voltage (p-eLVT gate structure), such as such as the gate structure 200F. The gate structures 200A-200F can be used for FinFETs, GAA-FETs, CFETs, forksheet FETs, vertical FETs, etc.
[0047] A transistor with an n-gate structure with standard threshold voltage (n-sVT gate structure) can threshold voltage with a first value to create a conductive path between source and drain terminals generate, a transistor with an n-gate structure with ultra-low threshold voltage (n-uLVT gate structure) can produce a threshold voltage with a second threshold voltage value to create a conductive path between the source and drain terminals, and a transistor with an n-gate structure with extremely low threshold voltage (n- eLVT gate structure) may require a threshold voltage with a third threshold voltage value to achieve a conductive path between source and drain terminals. In some cases, the first value is larger than the second value, and the second value is greater than the third value.
[0048] Similarly, a transistor with a p-gate structure with standard threshold voltage (p-sVT gate structure) require a threshold voltage with a fourth threshold voltage value to create a conductive path between source and drain terminals, a transistor with a p-gate structure with ultra-low threshold voltage (p-uLVT- Gate structure) may require a threshold voltage with a fifth threshold voltage value to achieve a conductive path between source and drain terminals, and a transistor with a p-gate structure with extremely low Threshold voltage (p-eLVT gate structure) can have a threshold voltage with a sixth threshold voltage value to create a conductive path between the source and drain terminals. In some cases, the fourth Value greater than the fifth value, and the fifth value is greater than the sixth value.
[0049] In some embodiments, the gate structures 200A-200F may be fabricated on the same wafer and / or may be parts of the same IC device. Therefore, at least some of the Manufacturing processes on all gate structures 200A-200F are performed simultaneously. For FinFET embodiments the gate structures 200A-200F each enclose at least three surfaces of the fin structures (e.g., channel layer). In GAA-FET embodiments, the gate structures 200A-200F channel regions of the fin structures can be completely enclose.
[0050] In block 2100, the gate structures 200A-200F are shown at an intermediate stage of fabrication, such as stage shown in Fig. 12B, in which the sacrificial gate structure and the second semiconductor layers 108 have been removed, to expose parts of the first semiconductor layers 106. As can be seen in Figs. 18A-18F, each gate structure 200A-200F have an IL 250 formed over first semiconductor layers 206 (ie, channel regions), such as the first Semiconductor layer 106 of the semiconductor device structure 100 shown in Fig. 12A and Fig. 12B For the sake of simplicity, only a fraction of the first semiconductor layers 206 is shown. In some In some embodiments, the IL 250 comprises an oxide of the semiconductor material of the substrate 101, such as silicon oxide. In other embodiments, the IL 250 may comprise another suitable type of dielectric material. The IL 250 can be formed by a wet process or a wet oxidation process such as those described above under Referring to Fig. 13, the manufacturing steps for the IL 150 have been discussed. The IL 250 can have a thickness in a range between about 5 angstroms and about 50 angstroms, such as about 7 angstroms to about 10 angstroms.
[0051] In block 2102, a first high-k dielectric (HK dielectric) 260a is formed over the IL 250, as shown in Figs. 19A-19F. The first HK dielectric 260a may be the same material as the first HK dielectric 160a discussed above with reference to Fig. 14. In some embodiments, the first dielectric HK layer 260a is formed using an ALD process to determine the thickness of the deposited layer with The ALD process can be performed using between about 20 and about 40 deposition cycles at a temperature range between about 200 degrees Celsius and about 300 degrees Celsius. In some Embodiments are used in the ALD process HfCl and / or HO as precursors. With such an ALD 4 2 process, the first HK dielectric 260a can be manufactured to have a thickness in a range of about 5 Angstroms up to about 15 angstroms.
[0052] In block 2104, a tuning layer 261 is deposited on the first HK dielectric 260a of the gate structures 200A-200F and a patterned resist layer 263-1 is formed over the gate structures 200A, 200B, 200C, as shown in Figs. 20A-20F. The tuning layer 261 allows for later tuning of the threshold voltage in the Gate structures 200A, 200B, 200C. The tuning layer 261 is deposited directly on the first HK dielectric 260a in the Gate structures 200A-200F are deposited. The tuning layer 261 may be a dielectric material comprising one or has several dipole elements suitable for tuning Vth for n-type devices. The tuning layer 261 may be an oxide-based or non-oxide-based dielectric material. In some embodiments, the Tuning layer 261 a metal oxide material in which the metal is, for example, lanthanum (La), lutetium (Lu), scandium (Sc), Yttrium (Y), Thulium (Tm), Gadolinium (Gd), Magnesium (Mg) or combinations thereof, but it is not limited thereto. Exemplary metal oxide for the tuning layer 261 can be La O , LuO , ScO , YO , Tm O , Gd O , MgO 2 3 xx 2 3 2 3 2 3 or the like. The tuning layer 261 may be formed using a conformal deposition process such as such as an ALD process. For the gate structures 200A-200C, the tuning layer 261 may Increase or compensate for the threshold voltage Vth required for n-type transistor devices. Tuning layer 261 may have a thickness in a range between about 3 angstroms and about 12 angstroms, for example about 5 Ångström to about 8 Ångström. If the thickness of the tuning layer 261 is less than 3 Ångström, the Tuning layer 261 is not sufficient to provide the required tuning effect for the n-devices. If On the other hand, if the thickness of the tuning layer 261 is greater than about 12 Ångströms, the space available for later Layers remain, reduce and production costs increase without any significant benefit.
[0053] After the tuning layers 261 have been deposited on the gate structures 200A-200F, a patterned resist layer 263-1 is fabricated to form gate structures for n-FETs, such as gate structures 200A-200C. while gate structures for p-FETs, such as the gate structures 200D-200F, remain uncovered. structured resist layer 263-1 protects the tuning layer 261 on the gate structures 200A-200C, so that the Tuning layer 261 on the gate structures 200D-200F can be removed. The patterned resist layer 263-1 can by first depositing an unstructured layer over the gate structures 200A-200F followed by structuring and etching processes to remove parts of the unstructured layer in selected areas (e.g. areas where the gate structures 200D-200F are located) in order to remove the patterned resist layer 263- 1. The patterned resist layer 263-1 may comprise any suitable masking material, such as a Photoresist layer, a bottom anti-reflective coating (BARC) layer, a spin-on Glass layer (SOG layer) or a spin-on-carbon layer (SOC layer) and can be spin-coated or another suitable deposition process.
[0054] In block 2106, after the patterned resist layer 263-1 has been formed, the tuning layers 261 on the gate structures 200D-200F, and then the patterned resist layer 263-1 is removed, as shown in the Fig. 21A-21F. The tuning layers 261 can be formed using the patterned resist layer 263-1 as Mask with a suitable etching process, such as dry etching, wet etching or a combination thereof, In some embodiments, an etchant used for such an etching process may Hydrochloric acid (HCl), alkali (NH ), oxidizing agent or other suitable caustic. 4 structured resist layer 263-1 can be used under using a suitable process, such as a stripping process.
[0055] In block 2108, a first n-dipole layer 265 is formed globally on the gate structures 200A-200F, and a structured resist layer 263-2 is formed on the first n-dipole layer 265 of the gate structures 200A and 200D, as shown in Figs. 22A-22F. The first n-dipole layer 265 is deposited on the tuning layers 261 of the gate structures 200A- 200C and on the first HK dielectric 260a of the gate structures 200D-200F. The first n-dipole layer 265 is a material with an inherent negative polarity. In some embodiments, the first n-dipole layer 265 is a dielectric material that has one or more dipole elements suitable for n-type devices. The first n- Dipole layer 265 can be selected from the material used for tuning layer 261. In some Embodiments, the first n-dipole layer 265 may comprise the same material as the tuning layer 261. In In some embodiments, the first n-dipole layer 265 may comprise a material that is chemically different from that of the tuning layer 261. An exemplary material for the first n-dipole layer 265 can be La O , LuO , ScO , YO 2 3 xx 2 , Tm O , Gd O , MgO or the like. For the gate structures 200A-200C, the first n-dipole layer 265 3 2 3 2 3 increase the threshold voltage Vth required for n-type transistor devices. For gate structures 200D-200F, the p-transistor devices, the first n-dipole layer 265 can set the threshold voltage Vth for p- reduce transistor devices.
[0056] The first n-dipole layer 265 may be formed using a conformal deposition process, such as an ALD process. The tuning layer 261 can be formed using a first number of cycles of the ALD process deposited, and the first n-dipole layer 265 can be deposited using a second cycle number of the ALD process which is less than the first number of cycles. Therefore, the tuning layer 261 has a thickness which is greater than that of the first n-dipole layer 265. Each of the first n-dipole layers 265 may have a thickness in a range between about 1 angstrom and about 6 angstroms, for example about 2 angstroms to about 3 angstroms.
[0057] After the first n-dipole layers 265 have been formed on the gate structures 200A-200F, the patterned resist layer 263-2 is fabricated to form certain gate structures for n-FETs and p-FETs, such as the Gate structures 200A and 200D, while gate structures for certain n-FETs and p-FETs, such as the Gate structures 200B, 200C, 200E and 200F remain uncovered. The patterned resist layer 263-2 protects the first n- Dipole layers 265 on the gate structures 200A and 200D, so that the first n-dipole layers 265 on the Gate structures 200B, 200C, 200E and 200F can be removed. The patterned resist layer 263-2 can be removed in a similar manner as discussed above with respect to the patterned resist layer 263-1.
[0058] In block 2110, the first n-dipole layers 265 on the gate structures 200B, 200C, 200E and 200F are removed, and then the patterned resist layer 263-2 is removed, as shown in Figs. 23A-23F. The first n-dipole Layers 265 can be formed using the patterned resist layer 263-2 as a mask with a suitable etching process, such as those discussed above for removing the tuning layer 261. The patterned resist layer 263-2 can be removed by a suitable process, such as a stripping process. become.
[0059] In block 2112, a second n-dipole layer 267 is formed globally on the gate structures 200A-200F, and a structured resist layer 263-3 is deposited on the second n-dipole layer 267 of the gate structures 200A, 200B, 200D and 200E as shown in Figures 24A-24F. The second n-dipole layer 267 is deposited on the first n-dipole layer 265 of the Gate structures 200A and 200D, on the tuning layers 261 of the gate structures 200B and 200C and on the first HK- Dielectric 260a of the gate structures 200E and 200F. The second n-dipole layer 267 can be made of the material used for the first n-dipole layer 265. In some embodiments, the second n- Dipole layer 267 may comprise the same material as the first n-dipole layer 265. In some embodiments, the second n-dipole layer 267 may comprise a material that is chemically different from that of the first n-dipole layer 265. The patterned resist layer 263-3 can be formed in a similar manner as described above with respect to the structured resist layer 263-1 has been discussed.
[0060] In block 2114, the second n-dipole layers 267 on the gate structures 200C and 200F are removed, and then The patterned resist layers 263-3 are removed, as shown in Figs. 25A-25F. The second n-dipole layers 267 can be removed using the patterned resist layer 263-3 as a mask with a suitable etching process such as one of those discussed above for the tuning layer 261. The structured Resist layer 263-3 can be removed using a suitable process.
[0061] In block 2116, the gate structures 200A-200F are subjected to a heat treatment 268. The heat treatment causes the dipole elements in the tuning layer 261, the first n-dipole layer 265 and the second n-dipole layer 267 penetrate into (or react with) the first HK dielectric 260a to form a modified first HK dielectric 260a-1. The dipole elements can increase the polarity of the first HK dielectric 260a, and can consequently used to adjust the threshold voltage Vth of the gate structures 200A-200F. In some Embodiments, the modified first HK dielectric 260a-1 is the first HK dielectric 260a that is dipole elements and / or with materials from the tuning layer 261, the first n-dipole layer 265 and the second n-dipole layer 267. The heat treatment 268 can be carried out in-situ or ex-situ and can be any tempering method such as rapid thermal tempering, spike annealing, soak annealing Tempering, laser annealing, etc. The heat treatment 268 can be for about 1 second to about 3 minutes and in a Temperature range from about 500 degrees Celsius to about 850 degrees Celsius. The heat treatment 268 can be used in a gas atmosphere such as an oxygen-containing gas, a hydrogen-containing gas, an argon-containing Gas, a helium-containing gas or a combination thereof. Example gases can be N , NH , O , N 2 3 2 O, Ar, He, H , etc., but is not limited to these. 2 2
[0062] The annealing temperature causes the dipole elements (e.g. La) to be embedded in a part of the first HK dielectric 260a diffused or driven in. The heat treatment 268 can be carried out in such a way that the Dipole elements are finally distributed in the first HK dielectric 260a and it is incorporated into the modified first HK dielectric 260a-1. Alternatively, the dipole elements can be gradually added along the thickness of the modified first HK- dielectric 260a-1. In such cases, the dipole elements can be located at and / or near an interface of the modified first HK dielectric 260a-1 and the tuning layer 261 on, for example, the gate structures 200A-200C have a first doping concentration, and the dipole elements are located at and / or near an interface of the modified first HK dielectric 260a-1 and the IL 250 may have a second doping concentration that is lower than the first doping concentration.
[0063] In some embodiments, a portion of the tuning layer 261, the first n-dipole layer 265, or the second n-dipole layer 267 react with the first HK dielectric 260a, resulting in the modified first HK- Dielectric 260a-1, which is a compound, composition or mixture of the first HK dielectric 260a and the tuning layer 261, the first n-dipole layer 265 and the second n-dipole layer 267.
[0064] In some embodiments, a portion of the IL 250, such as the region 269 of the IL 250, may be near or at a The interface between the modified first HK dielectric 260a-1 and the IL 250 can also be modified. Similarly, the modified IL 250 can be a layer doped with the dipole element and / or with materials of the tuning layer 261, the first n-dipole layer 265 and the second n-dipole layer 267, which is used heat treatment and the duration of the heat treatment 268. In such cases, the Dipole elements at and / or near an interface between the modified first HK dielectric 260a-1 and the IL 250 on, for example, the gate structures 200A-200C have a third doping concentration, and the dipole elements on and / or near an interface of the IL 250 and the channel region (ie, the first semiconductor layer 106) may have a fourth doping concentration which is lower than the third doping concentration.
[0065] It is contemplated that although the heat treatment 268 is discussed herein as being performed after manufacture the tuning layer 261, the first n-dipole layer 265 and the second n-dipole layer 267, the Heat treatment 268 also separately after production of the tuning layer 261 and / or after production of the first n- Dipole layer 265 can be carried out.
[0066] Therefore, the multiple structuring processes discussed above lead to different numbers of first and second n-dipole layers and tuning layers 261, which are located above the first HK dielectric 260a on the Gate structures 200A-200F. Since different numbers of the first n-dipole layer 265, the second n-dipole layer 267 and the tuning layer 261 are arranged on the gate structures 200A-200F, the modified first HK- Dielectric 260a-1 on certain gate structures may have a doping concentration (of the dipole elements) that depends on the of the modified first HK dielectric 260a-1 on other gate structures for different Threshold voltage requirements required for the n-type devices and the p-type devices are different. For example, the modified first HK dielectrics 260a-1 on the gate structures 200A and 200D may have a first doping concentration, and the modified first HK dielectrics 260a-1 on the gate structures 200B and 200E may have a second doping concentration, and the modified first HK dielectrics 260a-1 on the Gate structures 200C and 200F may have a third doping concentration. In some embodiments, due to the presence of the first n-dipole layer 265, the second n-dipole layer 267 and the tuning layer 261, the first doping concentration greater than the second doping concentration, and due to the inclusion of the tuning layer 261, the Doping concentration of the modified first HK dielectric 260a-1 on the gate structure 200A is greater than the Doping concentration of the modified first HK dielectric 260a-1 on the gate structure 200D. In some Embodiments, due to the presence of the second n-dipole layer 267 and the tuning layer 261, the second doping concentration is greater than the third doping concentration. Due to the inclusion of the tuning layer 261, the doping concentration of the modified first HK dielectric 260a-1 on the gate structure 200B is greater than the doping concentration of the modified first HK dielectric 260a-1 on the gate structure 200E. Finally, the first n-dipole layer 265 and the second n-dipole layer 267 are not present for the gate structures 200C and 200F. Due to the presence of the tuning layer 261, the modified first HK dielectric 260a-1 can therefore lowest doping concentration for the gate structure 200C, and the modified first HK dielectric 260a-1 on the gate structure 200F may have the fewest dipole elements or be substantially free of dipole elements.
[0067] Although not shown, integrated circuit devices such as the Semiconductor device structure 100, having different transistors with different threshold voltages, which are their function in the IC device. For example, input / output transistors (I / O transistors) have the highest threshold voltages due to the high current load required by the I / O transistors. Core logic transistors can have the lowest threshold voltages to achieve higher switching speeds at A third threshold voltage between that of the I / O transistors and that of the Core logic transistors can be used for other functional transistors, such as SRAM transistors (SRAM: static random access memory). In some embodiments, the semiconductor device structure 100 may include two or more NFETs and / or PFETs with two or more different threshold voltages.
[0068] In block 2118, the first n-dipole layer 265, the second n-dipole layer 267 and the tuning layer 261 are the gate structures 200A-200F, as shown in Figures 27A-27F. The first n-dipole layer 265, the second n- Dipole layer 267 and tuning layer 261 can be removed using a suitable removal process, such as a wet etching process or the processes discussed above for removing the tuning layer 261. The removal process can be time-controlled or run until the modified first HK Dielectrics 260a-1 are exposed.
[0069] In block 2120, a second HK dielectric 260b is globally deposited on the modified first HK dielectric 260a-1 of the gate structures 200A-200F, as shown in Figs. 28A-28F. The second HK dielectric 260b may same material as the second HK dielectric 160b, and can be formed using an ALD process such as those discussed above with reference to Fig. 14. The ALD process can be carried out using of between about 20 and about 40 deposition cycles at a temperature range between about 200 degrees Celsius and about 300 degrees Celsius. In some embodiments, the ALD process uses HfCl and / or H 4 2 O as a precursor. With such an ALD process, the second HK dielectric 260b can be manufactured in such a way that that it has a thickness in a range of about 5 angstroms to about 15 angstroms. In some embodiments the modified first HK dielectric 260a-1 and the second HK dielectric 260b may have a combined thickness in a range of about 10 Ångströms to about 30 Ångströms.
[0070] In block 2122, an insertion layer 256 is globally deposited over the second HK dielectric 260b of the gate structures 200A-200F, as shown in Figures 29A-29F. The insertion layer 256 may be the same material as the insertion layer 156 and may be conformally deposited on the second dielectric HK layer 260b in a similar manner as discussed above with reference to Fig. 15. Like the insertion layer 156, the Insertion layer 256 as an oxygen barrier layer that prevents oxygen migration from the gate dielectrics (e.g., the modified first dielectric HK layer 260a and the second dielectric HK layer 260b) to a later fabricated metal gate (e.g., metal layer 258, Fig. 30A). The insertion layer 256 can block the generation of oxygen vacancies in the modified first dielectric HK layer 260a and the second dielectric HK Layer 260b, prevent the increase in the resistivity of the metal gate due to oxidation and promote stress relaxation of the channel regions. Since the generation of oxygen vacancies by the Insertion layer 256 is suppressed, the number of heat treatments for repairing oxygen vacancies be reduced or they can even be eliminated, causing a thickening of the IL 250 (due to IL regrowth) and the diffusion of dopants into the source / drain structural elements can be avoided. The insertion layer 256 may have a thickness T4 in a range of about 2 angstroms to about 10 angstroms.
[0071] In block 2124, a metal layer 258 and a metal fill layer 259 are deposited globally over the insertion layer 256 of the gate structures 200A-200F, as shown in Figures 30A-30F. The metal layer 258 forms the Electrode part of the gate structures 200A-200F. The metal layers 258 may be a low-resistance metal with a effective p-band edge work function value (p-metal). That is, the metal layer 258 is a p-band edge Work function metal with an effective work function value higher than the mid-gap work function value (about 4.5 eV), which lies in the middle of the valence band and the conduction band of silicon. The work function value, which is higher than the mid-gap work function is called a p-work function, and the respective metal that has the p-work function is referred to as a p-metal. In some embodiments, the metal layer 258 is a pure metal having a effective work function (eWF) in a range of about 4.7 eV to about 5.7 eV. In some embodiments, the metal layer 258 has an effective work function value in a range of about 4.9 eV to about 5.2 eV. The Metal layer 258 can be tungsten (W), chromium (Cr), ruthenium (Ru), molybdenum (Mo), osmium (Os), titanium (Ti), rhenium (Re), Rhodium (Rh), iridium (Ir), platinum (Pt), nickel (Ni) or another low-resistance pure metal with an effective p- band edge work function value. The metal layer 258 can be formed using a suitable conformal deposition process, such as ALD, so that the metal layer 258 has the smallest vacancies or has other defects that could increase the gate resistance.
[0072] After the metal layer 258 has been deposited, the metal fill layer 259 is deposited over the metal layer 258 The metal filling layer 259 may be an electrically conductive material such as W, cobalt (Co), Ru, Ir, Mo, copper (Cu), aluminum (Al), Ti, tantalum (Ta) or the like or combinations thereof. The metal fill layer 259 may made of a material different from the material of the metal layer 258. The metal fill layer 259 can be deposited using CVD, PVD, plating and / or other suitable deposition techniques.
[0073] Although not shown, a capping layer, a barrier layer, an n-metal work function layer, a p-metal work function layer and / or an adhesive layer between the insertion layer 256 and the metal filling layer 259. The capping layer and the barrier layer may be metal oxides, Metal nitrides, metal silicates, transition metal oxides, transition metal nitrides, transition metal silicates, oxide nitrides of metals, metal aluminates, zirconium silicate, zirconium aluminate, combinations thereof, or the like. Barrier layer can be made of a material different from the material of the capping layer. The n-metal work function layer may be made of a metallic material such as W, Cu, AlCu, TiAlC, TiAlN, Ti, TiN, Ta, TaN, Co, Ni, Ag, Al, TaAl, TaAlC, TaC, TaCN, TaSiN, Mn, Zr, other suitable n-work function materials or combinations thereof. The p-metal work function layer can be made of a metallic material such as such as W, Al, Cu, TiN, Ti, TiAlN, Ta, TaN, Co, Ni, TaC, TaCN, TaSiN, TaSi, NiSi, Mn, Zr, ZrSi, TaN, Ru, AlCu, Mo, MoSi, WN, 2 2 2 2 other metal oxides, metal nitrides, metal silicates, transition metal oxides, transition metal nitrides, Transition metal silicates, oxide nitrides of metals, metal aluminates, zirconium silicate, zirconium aluminate, combinations thereof or the like. The adhesive layer may be made of a metal nitride such as TiN, TaN, MoN, WN or another suitable material, using an ALD process.
[0074] After the gate structures 200A-200F have been formed, S / D contacts 176 can be formed through the ILD layer 164 and the CESL 162 are fabricated to expose the epitaxial S / D structure element 146. A silicide layer 178 is arranged on the epitaxial S / D structure elements 146 to connect the epitaxial S / D structure elements 146 with the S / D contacts 176. Fig. 32 is a sectional view of a semiconductor device structure 201 having a Intermediate stage of production shows how the stage after the production of the replacement gates (e.g. the gate structures 200A- 200F) and the S / D contacts 176. The semiconductor device structure 201 is essentially similar to the Semiconductor device structure 100 shown in Fig. 17A, except that the gate structure 190 is formed by the gate structures 200A-200F, shown in Figs. 30A-30F.
[0075] Fig. 33 shows a sectional view of a part of the semiconductor device structure 201 taken along the cross section EE of Fig. 32, according to some embodiments. Fig. 33 shows an exemplary embodiment of a channel region (ie, the first semiconductor layer 206) provided with an n-gate structure with extremely low threshold voltage (n-eLVT gate structure), an n-gate structure with ultra-low threshold voltage (n-uLVT- gate structure) or an n-gate structure with standard threshold voltage (n-sVT gate structure). Fig. 34 shows a sectional view of a part of the semiconductor device structure 201, which was created along the cross section FF of Fig. 32, according to some embodiments. Fig. 34 shows a exemplary embodiment of a channel region (ie, the first semiconductor layer 206) provided with a p-gate structure with standard threshold voltage (p-sVT gate structure), a p-gate structure with ultra-low threshold voltage (p-uLVT- gate structure) and a p-gate structure with extremely low threshold voltage (p-eLVT gate structure). Both Fig. 33 and Fig. 34 show that the first semiconductor layers 206 are deposited in this order by the IL 250, the modified first HK dielectric 260a-1, the second HK dielectric 260b, the insertion layer 256 and the metal layer 258 be enclosed.
[0076] The ultra-thin oxygen barrier layer (e.g., the insertion layer 256) can also be formed with a mature p- Dipole process to achieve a single n-edge work function metal knob. Fig. 35A to 45F show the fabrication of gate structures 300A-300F for a semiconductor device 301, such as a GAA FET structure with multiple threshold voltages according to various embodiments. Fig. 49 shows a Flowchart of a process 3000 for manufacturing the gate structures 300A-300F shown in Figs. 35A-45F, according to various embodiments. Figures 35A-45A show the fabrication of a transistor with an n- Gate structure with extremely low threshold voltage (n-eLVT gate structure), such as the gate structure 300A. Fig. 35B- 45B show the fabrication of a transistor with an n-gate structure with an ultra-low threshold voltage (n-uLVT- gate structure), such as gate structure 300B. Figures 35C-45C show the fabrication of a transistor with an n- Gate structure with standard threshold voltage (n-sVT gate structure), such as the 300C gate structure. Figures 35D-45D show the fabrication of a transistor with a p-gate structure with standard threshold voltage (p-sVT gate structure), such as the gate structure 300D. Figures 35E-45E show the fabrication of a transistor with a p-gate structure with ultra-low threshold voltage (p-uLVT gate structure), such as the gate structure 300E. Figures 35F-45F show the Fabrication of a transistor with a p-gate structure with extremely low threshold voltage (p-eLVT gate structure), such as such as the gate structure 300F. Similarly, the gate structures 300A-300F can be applied to FinFETs, GAA-FETs, CFETs, Forksheet FETs, vertical FETs, etc.
[0077] In some embodiments, the gate structures 300A-300F may be fabricated on the same wafer and / or may be parts of the same IC device. Therefore, at least some of the Manufacturing processes on all gate structures 300A-300F are performed simultaneously.
[0078] In block 3100, the gate structures 300A-300F are shown at an intermediate stage of fabrication, with each Gate structure 300A-300F first semiconductor layers 306 (such as the first semiconductor layers 206 shown in Figs. 20A-20F shown), an IL 350 (such as the IL 250, Fig. 20A-20F), a first HK dielectric 360a (such as the first HK Dielectric 260a shown in Figs. 20A-20F) and a tuning layer 361 (such as tuning layer 261, shown in Figs. 20A-20F), as shown in Figs. 35A-35F. A patterned resist layer 363-1 (such as the patterned resist layer 263-1 shown in Figs. 20A-20C) is then selectively deposited over the Gate structures 300D-300F are fabricated in a similar manner as discussed above with reference to Figs. 20A-20F The tuning layer 361 may be a dielectric material having one or more dipole elements that are used to Tuning Vth for p-type devices. The tuning layer 361 may be an oxide-based or non- oxide-based dielectric material. In some embodiments, the tuning layer 361 is a Metal oxide material in which the metal is zinc (Zn), germanium (Ge), aluminum (Al), titanium (Ti), vanadium (V) or Combinations thereof, but not limited to. An exemplary metal oxide for the tuning layer 361 may comprise ZnO, GeO, AlO, TiO, VO or the like. The tuning layer 361 may be formed using a xxxxx conformal deposition process, such as an ALD process. For the gate structures 300D-300F the tuning layer 361 can increase the threshold voltage Vth required for p-type transistor devices or Similar to the tuning layer 261, the tuning layer 361 may have a thickness in a range between about 3 Angstroms and about 12 angstroms, for example about 5 angstroms to about 8 angstroms.
[0079] In block 3102, the tuning layers 361 are deposited on the gate structures 300A-300C using the patterned resist layer 363-1 as a mask is removed, and then the patterned resist layer 363-1 is removed as shown in Figs. 36A-36F. The tuning layers 361 and the patterned resist layer 363-1 can be appropriate removal process, such as those discussed with reference to Figures 21A-21F.
[0080] In block 3104, a first p-dipole layer 365 is formed globally on the gate structures 300A-300F, and a structured resist layer 363-2 is deposited over the first p-dipole layer 365 of the gate structure 300A and 300D are fabricated as shown in Figs. 37A-37F. The first p-dipole layer 365 is deposited on the Tuning layers 361 of the gate structures 300D-300F and on the first HK dielectric 360a of the gate structures 300A- 300C. The first p-dipole layer 365 is a material with an inherent positive polarity. In some Embodiments, the first p-dipole layer 365 is a dielectric material that includes one or more dipole elements suitable for p-type devices. The first p-dipole layer 365 may be selected from the material used for the tuning layer 361. In some embodiments, the first p-dipole layer 365 may be the the same material as the tuning layer 361 or a different material than this. An example material for The first p-dipole layer 365 may comprise ZnO, GeO, AlO, TiO, VO, or the like. For the gate structures 300D- xxxxx 300F, the first p-dipole layer 365 can provide the threshold voltage Vth required for p-transistor devices. For the gate structures 300A-300C, which correspond to n-type transistor devices, the first p-type dipole layer 365 reduce the threshold voltage Vth for n-type transistor devices. The first p-dipole layer 365 and the Tuning layer 361 may be formed using a conformal deposition process, such as an ALD process. Each of the first p-dipole layers 365 may have a thickness in a range between about 1 angstrom and about 6 angstroms, for example about 2 angstroms to about 3 angstroms.
[0081] In block 3106, the first p-dipole layers 365 are deposited on the gate structures 300B, 300C, 300E and 300F under Using the patterned resist layer 363-2 as a mask, and then the patterned resist layer 363-2 removed, as shown in Figs. 38A-38F. The first p-dipole layers 365 and the patterned resist layer 363-2 can be removed using any suitable removal process, such as those described above with reference to Figures 23A-23F have been discussed.
[0082] In block 3108, a second p-dipole layer 367 is formed globally on the gate structures 300A-300F, and a structured resist layer 363-3 is deposited on the second p-dipole layer 367 of the gate structures 300A, 300B, 300D and 300E as shown in Figures 39A-39F. The second p-dipole layer 367 is deposited on the first p-dipole layer 365 of the Gate structures 300A and 300D, on the tuning layers 361 of the gate structures 300E and 300F, and on the first HK- Dielectric 360a of the gate structures 300B and 300C. The second n-dipole layer 367 can be made of the material used for the first p-dipole layer 365. The second p-dipole layer 367 may have the same material such as the first p-dipole layer 365 or a different material than this. The patterned resist layer 363- 3 can be manufactured in a similar manner as described above with respect to the patterned resist layer 363-1 has been discussed.
[0083] In block 3110, the second p-dipole layers 367 are formed on the gate structures 300C and 300F using the patterned resist layer 363-3 as a mask is removed, and then the patterned resist layers 363-3 removed, as shown in Figs. 40A-40F. The second p-dipole layers 367 and the patterned resist layer 363-3 can be removed by any suitable process, such as those discussed with reference to Figs. 25A-25F are.
[0084] In block 3112, the gate structures 300A-300F are subjected to a heat treatment 368 (such as the heat treatment 268 shown in Figs. 26A-26F) as shown in Figs. 41A-41F. Similarly, the Heat treatment 368 that the dipole elements in the tuning layer 361, the first p-dipole layer 365 and the second p-dipole layer 367 penetrate into (or react with) the first HK dielectric 360a to form a modified first HK- Dielectric 360a-1. The dipole elements can increase the polarity of the first HK dielectric 360a, and can therefore be used to adjust the threshold voltage Vth of the gate structures 300A-300F. In some Embodiments, the modified first HK dielectric 360a-1 is the first HK dielectric 360a that is dipole elements and / or with materials from the tuning layer 361, the first p-dipole layer 365 and the second p-dipole layer 367 is mixed.
[0085] The annealing temperature causes the dipole elements (e.g. Ge) to be embedded in a part of the first HK dielectric 360a diffused or driven in. The heat treatment 368 can be carried out in such a way that the Dipole elements are finally distributed in the first HK dielectric 360a and it is incorporated into the modified first HK dielectric 360a-1. Alternatively, the dipole elements can be gradually introduced along the thickness of the modified first HK- dielectric 360a-1. In such cases, the dipole elements can be located at and / or near an interface of the modified first HK dielectric 360a-1 and the tuning layer 361 on, for example, the gate structures 300D-300F have a first doping concentration, and the dipole elements are located at and / or near an interface of the modified first HK dielectric 360a-1 and the IL 350 may have a second doping concentration that is lower than the first doping concentration.
[0086] In some embodiments, a portion of the tuning layer 361, the first n-dipole layer 365, or the second n- Dipole layer 367 reacts with the first HK dielectric 360a, resulting in the modified first HK dielectric 360a-1 which is a compound, composition or mixture of the first HK dielectric 360a and the tuning layer 361, the first n-dipole layer 365 and the second n-dipole layer 367.
[0087] In some embodiments, a portion of the IL 350, such as the region 369 of the IL 350, may be near or at a The interface between the modified first HK dielectric 360a-1 and the IL 350 can also be modified. Similarly, the modified IL 350 may be a layer doped with the dipole elements and / or with Materials from the tuning layer 361, the first p-dipole layer 365 and the second p-dipole layer 367 are mixed. In In such cases, the dipole elements can be located at and / or near an interface between the modified first HK- Dielectric 360a-1 and the IL 350 on, for example, the gate structures 300D-300F a third doping concentration and the dipole elements are located at and / or near an interface of the IL 350 and the channel region (ie, the first semiconductor layer 306) may have a fourth doping concentration that is lower than the third doping concentration.
[0088] It is contemplated that although the heat treatment 368 is discussed herein as being performed after manufacture the tuning layer 361, the first p-dipole layer 365 and the second p-dipole layer 367, the Heat treatment 368 also separately after production of the tuning layer 361 and / or after production of the first p- Dipole layer 365 can be carried out.
[0089] Therefore, the multiple structuring processes discussed above lead to different numbers of first and second p-dipole layers and tuning layers 361, which are located above the first HK dielectric 360a on the Gate structures 300A-300F. Since different numbers of the first p-dipole layer 365, the second p-dipole layer 367 and the tuning layer 361 are arranged on the gate structures 300A-300F, the modified first HK- Dielectric 360a-1 on certain gate structures may have a doping concentration (of the dipole elements) that is of the modified first HK dielectric 360a-1 on other gate structures for different Threshold voltage requirements required for the n-type devices and the p-type devices are different. For example, the modified first HK dielectrics 360a-1 on the gate structures 300A and 300D may have a first doping concentration, and the modified first HK dielectrics 360a-1 on the gate structures 300B and 300E may have a second doping concentration, and the modified first HK dielectrics 360a-1 on the Gate structures 300C and 300F may have a third doping concentration. In some embodiments, due to the presence of the first p-dipole layer 365, the second p-dipole layer 367 and the tuning layer 361 the first doping concentration is greater than the second doping concentration, and due to the inclusion of the Tuning layer 361 is the doping concentration of the modified first HK dielectric 360a-1 on the gate structure 300D greater than the doping concentration of the modified first HK dielectric 360a-1 on the gate structure 300A. In some embodiments, due to the presence of the second p-dipole layer 367 and the tuning layer 361 the second doping concentration is greater than the third doping concentration. Due to the inclusion of the Tuning layer 361 is the doping concentration of the modified first HK dielectric 360a-1 on the gate structure 300E is greater than the doping concentration of the modified first HK dielectric 360a-1 on the gate structure 300B. Finally, the first p-dipole layer 365 and the second p-dipole layer 367 for the gate structures 300C and 300F are not Due to the presence of the tuning layer 361, the modified first HK dielectric 360a- 1 have the lowest doping concentration for the gate structure 300F, and the modified first HK dielectric 360a- 1 on the gate structure 300C may have the fewest dipole elements or be substantially free of dipole elements be.
[0090] In block 3114, the first p-dipole layer 365, the second p-dipole layer 367 and the tuning layer 361 are the gate structures 300A-300F, as shown in Figures 42A-42F. The first p-dipole layer 365, the second p- Dipole layer 367 and tuning layer 361 can be removed using a suitable removal process, such as a wet etching process or the processes discussed above for removing the tuning layer 361. The removal process can be time-controlled or run until the modified first HK Dielectrics 360a-1 are exposed.
[0091] In block 2120, a second HK dielectric 360b is globally deposited on the modified first HK dielectric 360a-1 of the gate structures 300A-300F, as shown in Figs. 43A-43F. The second HK dielectric 360b may same material as the second HK dielectric 260b, and can be formed using an ALD process such as those discussed above with reference to Figs. 28A-28F. The second HK dielectric 360b may have a thickness in a range of about 5 Ångströms to about 15 Ångströms In some embodiments, the modified first HK dielectric 360a-1 and the second HK dielectric 360b have a combined thickness in a range of about 10 angstroms to about 30 angstroms.
[0092] In block 3118, an insertion layer 356 is globally deposited over the second HK dielectric 360b of the gate structures 300A-300F, as shown in Figures 44A-44F. The insertion layer 356 may be the same material as the insertion layer 256, and may be conformally deposited on the second HK dielectric layer 360b to a similar manner as discussed above with reference to Fig. 15. How the insertion layer 256 serves also the insertion layer 356 as an oxygen barrier layer that prevents oxygen migration from the gate dielectrics (e.g. the modified first dielectric HK layer 360a and the second dielectric HK layer 360b) to a later fabricated metal gate (e.g., metal layer 358, Fig. 45A-45F). The insertion layer 356 can Generation of oxygen vacancies in the modified first dielectric HK layer 360a and the second dielectric HK layer 360b and protect the metal gate from further oxidation. Since the generation of Oxygen vacancies are suppressed by the insertion layer 356, the number of heat treatments for Repair of oxygen vacancies can be reduced, resulting in thickening of the IL 350 (as a result of regrowth of the IL) and the diffusion of dopants into the source / drain structural elements can be avoided. Since precious metal is used for the oxygen barrier layer has a work function close to that of a p-edge work function metal, the thickness of the Insertion layer 356 is thinner than that of insertion layer 256. In some embodiments, the Insertion layer 356 may have a thickness T5 in a range of about 1 angstrom to about 8 angstroms. In some In some embodiments, the thickness T5 is smaller than the thickness T4 (Fig. 29A-29F).
[0093] In block 3120, a metal layer 358 and a metal fill layer 359 are deposited globally over the insertion layer 356 of the gate structures 300A-300F, as shown in Figures 45A-45F. The metal layer 358 forms the Electrode part of the gate structures 300A-300F. The metal layer 358 may be a low-resistance metal with an effective n- band edge work function value (n-metal). That is, the metal layer 358 is an n-band edge work function metal with an effective work function value lower than the mid-gap work function value (about 4.5 eV) used in the The work function value, which is lower than the mid-gap work function is called an n-work function, and the respective metal that has the n-work function is called an n-metal. In some embodiments, the metal layer 358 is a pure metal with an effective Work function value (eWF) in a range of about 3.8 eV to about 4.2 eV. The metal layer 358 may be tantalum (Ta), Zirconium (Zr), Cadmium (Cd), Indium (In), Al or another low-resistance pure metal with effective n-band edge The metal layer 358 can be formed using a suitable conformal deposition process such as ALD.
[0094] After the metal layer 358 has been deposited, the metal fill layer 359 is deposited over the metal layer 358 The metal fill layer 359 may comprise the same material as the metal fill layer 259, and may be using any suitable deposition technique. The metal fill layer 359 may be material different from that of the metal layer 358.
[0095] Although not shown, a capping layer, a barrier layer, an n-metal Work function layer, a p-metal work function layer and / or an adhesive layer such as those described above with Reference to Fig. 32 may be disposed between the insertion layer 356 and the metal fill layer 359. After the gate structures 300A-300F have been fabricated, S / D contacts 176 can be formed through the ILD layer 164 and the CESL 162 are fabricated to expose the epitaxial S / D structure element 146. A silicide layer 178 is deposited on the epitaxial S / D structure elements 146 to conductively connect the epitaxial S / D structure elements 146 to the S / D contacts 176. Fig. 46 is a sectional view of a semiconductor device structure 301 having a Intermediate stage of production shows how the stage after the production of the replacement gates (e.g. the gate structures 300A- 300F) and the S / D contacts 176. The semiconductor device structure 301 is essentially similar to the Semiconductor device structure 100 shown in Fig. 17A, except that the gate structure 190 is formed by the gate structures 300A-300F, shown in Figs. 45A-45F.
[0096] Fig. 47 shows a sectional view of a part of the semiconductor device structure 301 taken along the cross section GG of Fig. 46, according to some embodiments. Fig. 47 shows an exemplary embodiment of a channel region (ie, the first semiconductor layer 306) provided with an n-gate structure with extremely low threshold voltage (n-eLVT gate structure), an n-gate structure with ultra-low threshold voltage (n-uLVT- gate structure) or an n-gate structure with standard threshold voltage (n-sVT gate structure). Fig. 48 shows a sectional view of a part of the semiconductor device structure 301 taken along the cross section HH of Fig. 46 has been, according to some embodiments. Fig. 48 shows an exemplary embodiment of a channel region (ie, the first semiconductor layer 306), which is provided with a p-gate structure with standard threshold voltage (p-sVT gate structure), a p-gate structure with ultra-low threshold voltage (p-uLVT gate structure) and a p-gate structure with extremely low threshold voltage (p-eLVT gate structure). Both Fig. 47 and Fig. 48 show that the first semiconductor layers 306 in this order from the IL 350, the modified first HK dielectric 360a-1, the second HK dielectric 360b, the insertion layer 356 and the metal layer 358.
[0097] The various embodiments or examples described herein offer various advantages compared to the prior art. According to embodiments of the present disclosure, an ultra-thin Oxygen barrier layer (ie, insertion layer 156, 256, 356) disposed between gate dielectrics and a metal gate, to prevent oxygen migration from the gate dielectric to the metal gate. The oxygen barrier layer keeps the oxygen in the gate dielectrics (consequently less generation of oxygen vacancies in the gate dielectrics) and protects the metal gate from further oxidation, resulting in a high R (specific resistance of the metal gate) G caused by metal gate oxidation during the subsequent process (e.g. packaging and / or bonding processes). The oxygen barrier layer can be formed using an n-dipole or p-dipole process to simplify the complexity of the process, increase throughput and reduce costs. Since the Generation of oxygen vacancies is suppressed by the oxygen barrier layer, the number of Heat treatments to repair oxygen vacancies can be reduced, thereby facilitating IL regrowth and Diffusion of dopants into the source / drain structural elements is avoided.
[0098] One embodiment is a semiconductor device structure. The structure comprises: a Semiconductor channel layer over a substrate and a dielectric gate layer over the semiconductor channel layer The gate dielectric layer comprises: a first high-k dielectric layer having a first Doping concentration of dipole elements, and a second dielectric high-k layer with a second Doping concentration of dipole elements that is different from the first doping concentration. The structure also includes a gate electrode layer disposed over the gate dielectric layer, and a Insertion layer disposed between the gate dielectric layer and the gate electrode layer, wherein the Insertion layer is made of a precious metal.
[0099] Another embodiment is a semiconductor device structure. The structure has a first gate structure, enclosing a first semiconductor layer. The first gate structure comprises: a first dielectric layer with a first doping concentration of dipole elements, a first metal layer over the first dielectric layer, and a first insertion layer disposed between the first dielectric layer and the first metal layer wherein the first insertion layer is made of a noble metal. The structure also has a second gate structure enclosing a second semiconductor layer, wherein the second gate structure comprises: a second dielectric layer having a second doping concentration of dipole elements which are separated from the first Doping concentration of dipole elements is different. The structure also includes a second metal layer over the second dielectric layer, and a second insertion layer disposed between the second dielectric layer and the second metal layer, wherein the second insertion layer is made of the noble metal.
[0100] Another embodiment is a method for manufacturing a semiconductor device structure. The method comprises: forming an interface layer over a plurality of semiconductor channel layers in a first and a second device region; forming a first high-k dielectric over the interface layer; Producing a tuning layer over the first high-k dielectric, the tuning layer having dipole elements, suitable for tuning a threshold voltage for devices having a first conductivity type. The The method also includes: removing the tuning layer over the selected semiconductor channel layers in the second Device region; forming a first dipole layer over each semiconductor channel layer in the first and second Device region, wherein the first dipole layer comprises dipole elements suitable for devices with the first conductivity type. The process also includes: removing the first dipole layer over the selected Semiconductor channel layers in the first and second device regions; forming a second dipole layer over each semiconductor channel layer in the first and second device regions, wherein the second dipole layer dipole elements suitable for devices with a second conductivity type. The method comprises also: removing the second dipole layer over the selected semiconductor channel layers in the first and second Fixture area; driving in of dipole elements from the tuning layer, the first dipole layer and the second dipole layer into the first high-k Dielectric; removing the tuning layer, the first dipole layer and the second dipole layer above each semiconductor channel layer in the first and second device regions; forming an insertion layer over the first high-k dielectric, wherein the insertion layer is made of a noble metal. The method comprises also: producing a metal layer on the insertion layer.
[0101] Features of various embodiments have been described above so that experts will be able to understand the aspects of It will be clear to those skilled in the art that they can use the present disclosure without Further as a basis for designing or modifying other procedures and structures to achieve the same objectives and / or to achieve the same benefits as in the embodiments presented here. Experts should also recognize that such equivalent interpretations do not deviate from the basic idea and scope of the present disclosure and that they may include various changes, substitutions and Modifications may be made without departing from the spirit and scope of the present disclosure to deviate. QUOTES CONTAINED IN THE DESCRIPTION
[0000] This list of documents submitted by the applicant was generated automatically and is intended solely for This list is not part of the German patent or trademark law. Utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature
[0000] US 63461118
[0001]
Claims
1. Semiconductor device structure comprising: a semiconductor channel layer over a substrate; a dielectric gate layer disposed over the semiconductor channel layer, comprising: a first high-k dielectric layer having a first doping concentration of dipole elements; and a second high-k dielectric layer having a second doping concentration of dipole elements separated from the first doping concentration is different; a gate electrode layer deposited over the gate dielectric layer; and an insertion layer disposed between the gate dielectric layer and the gate electrode layer, wherein the insertion layer contains a precious metal.
2. A semiconductor device structure according to claim 1, further comprising: an interface layer disposed between the semiconductor channel layer and the first high-k dielectric layer wherein the interface layer has a third doping concentration of dipole elements which is smaller than the first doping concentration.
3. A semiconductor device structure according to claim 1 or 2, wherein the noble metal is gold (Au), platinum (Pt), iridium (Ir), palladium (Pd), osmium (Os), silver (Ag), rhodium (Rh), ruthenium (Ru) or the like.
4. A semiconductor device structure according to any one of the preceding claims, wherein the noble metal is an oxide of a precious metal.
5. A semiconductor device structure according to any one of the preceding claims, wherein the insertion layer comprises a Multilayer structure comprising a first layer comprising the noble metal and a second layer comprising a noble metal oxide includes.
6. A semiconductor device structure according to any one of the preceding claims, wherein the insertion layer is between and in Contact with the second high-k dielectric layer and the gate electrode layer.
7. A semiconductor device structure according to any one of the preceding claims, wherein the gate electrode layer comprises a p- Band edge work function metal with an effective work function value in a range of about 4.7 eV to about 5.7 eV is.
8. A semiconductor device structure according to any one of the preceding claims, wherein the gate electrode layer comprises an n- Band edge work function metal with an effective work function value in a range of about 3.8 eV to about 4.2 eV is.
9. Semiconductor device structure comprising: a first gate structure enclosing a first semiconductor layer, the first gate structure comprising: a first dielectric layer having a first doping concentration of dipole elements; a first metal layer over the first dielectric layer; and a first insertion layer disposed between the first dielectric layer and the first metal layer, wherein the first insertion layer is made of a noble metal; and a second gate structure enclosing a second semiconductor layer, the second gate structure comprising: a second dielectric layer having a second doping concentration of dipole elements which are separated from the first Doping concentration of dipole elements is different; a second metal layer over the second dielectric layer; and a second insertion layer disposed between the second dielectric layer and the second metal layer wherein the second insertion layer is made of the noble metal.
10. The semiconductor device structure of claim 9, further comprising: a third gate structure enclosing a third semiconductor layer, the third gate structure comprising: a third dielectric layer substantially free of dipole elements; a third metal layer over the third dielectric layer; and a third insertion layer disposed between the third dielectric layer and the third metal layer, wherein the third insertion layer is made of the precious metal.
11. A semiconductor device structure according to claim 10, wherein the first gate structure is an n-gate structure having an extremely low threshold voltage, and the second gate structure is an n-gate structure with an ultra-low threshold voltage, and the third gate structure is a p-gate structure with an extremely low threshold voltage.
12. A semiconductor device structure according to claim 10 or 11, further comprising: a fourth gate structure enclosing a fourth semiconductor layer, the fourth gate structure comprising: a fourth dielectric layer having a third doping concentration of dipole elements separated from the first and the second doping concentration of dipole elements is different; a fourth metal layer over the fourth dielectric layer; and a fourth insertion layer disposed between the fourth dielectric layer and the fourth metal layer, wherein the fourth insertion layer is made of the noble metal.
13. A semiconductor device structure according to claim 12, wherein the fourth gate structure comprises an n-gate structure with standard threshold voltage.
14. A semiconductor device structure according to claim 12 or 13, wherein the first, second, third and fourth Metal layer a p-band edge work function metal with an effective work function value in a range of approximately 4.7 eV to about 5.7 eV.
15. A semiconductor device structure according to any one of claims 9 to 14, wherein the noble metal is gold (Au), platinum (Pt), iridium (Ir), palladium (Pd), osmium (Os), silver (Ag), rhodium (Rh), ruthenium (Ru) or the like.
16. A semiconductor device structure according to any one of claims 9 to 15, wherein the noble metal is an oxide of a noble metal, which is electrically conductive.
17. A method of manufacturing a semiconductor device structure comprising the following steps: Forming an interface layer over a plurality of semiconductor channel layers in a first and a second device area; Producing a first high-k dielectric over the interface layer Producing a tuning layer over the first high-k dielectric, wherein the tuning layer comprises dipole elements which are used to tune a threshold voltage suitable for devices having a first conductivity type; removing the tuning layer over selected semiconductor channel layers in the second device region; Forming a first dipole layer over each semiconductor channel layer in the first and second device regions, wherein the first dipole layer comprises dipole elements suitable for devices having the first conductivity type; Removing the first dipole layer over the selected semiconductor channel layers in the first and second device area; Forming a second dipole layer over each semiconductor channel layer in the first and second device regions, wherein the second dipole layer comprises dipole elements suitable for devices having a second conductivity type are; Removing the second dipole layer over the selected semiconductor channel layers in the first and second device area; Driving dipole elements from the tuning layer, the first dipole layer and the second dipole layer into the first high-k dielectric; Removing the tuning layer, the first dipole layer and the second dipole layer above each semiconductor channel layer in the first and second device areas; Producing an insertion layer over the first high-k dielectric, wherein the insertion layer is made of a noble metal is manufactured; and Fabricating a metal layer on the insertion layer.
18. The method of claim 17, further comprising: before forming the insertion layer, forming a second high-k dielectric on the first high-k Dielectric.
19. The method of claim 17 or 18, wherein the first high-k dielectric is formed over a first semiconductor channel layer in the first device region has a first doping concentration of dipole elements, and the first high-k Dielectric over a second semiconductor channel layer in the first device region, a second Doping concentration of dipole elements which differs from the first doping concentration of dipole elements is different.
20. The method according to any one of claims 17 to 19, wherein the first high-k dielectric is disposed over a first semiconductor channel layer in the second device region has a third doping concentration of dipole elements, and the third doping concentration of dipole elements from the first and second doping concentrations of Dipole elements are different.
Citation Information
Patent Citations
Gate stack structure with oxygen barrier and method for manufacturing the same
US63461118P0
GATE STRUCTURES FOR SEMICONDUCTOR DEVICES
DE102020110789A1
DIPOLIG-FABRICATED HIGH-K-GATE DIELECTRIC AND METHOD FOR FORMING THE SAME
DE102020130401A1
Capacitor, semiconductor memory device, and method for manufacturing the same
US20020195633A1
Method of modifying capping layer in semiconductor structure
US20170125536A1