Diamond element and method for producing a diamond element

The diamond element with a carbon isotope-enriched epitaxial layer system and spin-free buffer layer addresses the issue of unpredictable spin coupling in diamonds, enabling controlled spin distances and improved quantum computing performance.

DE102023206516B3Active Publication Date: 2024-10-24DIATOPE GMBH

Patent Information

Application Number
DE102023206516
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-07-10
Publication Date
2024-10-24
Estimated Expiration
2043-07-10

AI Technical Summary

Technical Problem

Existing methods for generating coupling spin systems in diamonds, such as NV centers, suffer from low success rates and unpredictable coupling strengths due to random spin distances, complicating applications in quantum computing.

Method used

A diamond element with an epitaxial layer system made of carbon isotope-enriched diamond material, featuring spin layers separated by a spin-free buffer layer, allowing controlled adjustment of spin distances and coupling strengths through homoepitaxial growth and ion implantation of spin species.

Benefits of technology

Enables precise control over spin coupling, significantly increasing the likelihood of successful coupling and reducing randomness, thereby enhancing the efficiency of quantum computing applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The invention relates to a diamond element (2, 2') comprising a substrate (4) with an epitaxial layer system (6, 6') of 12C-carbon isotope-enriched diamond material applied thereon, wherein the layer system (6, 6') comprises at least two superimposed spin layers (8a, 8b) each with a spin species (14), and wherein a substantially spin-free buffer layer (10) is arranged between each of the two spin layers (8a, 8b).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a diamond element comprising a substrate with an epitaxial Layer system of carbon isotope-enriched diamond material. The invention further relates to a method for Production of such a diamond element.

[0002] So-called spin impurities or spin defects in solids are among the best known and most quantum systems. In particular, color centers in diamonds, such as negatively charged Nitrogen vacancy (NV) or silicon vacancy (SiV) have been shown to be versatile, atom-sized spin systems with a wide range of applications in quantum optics, quantum computing and of quantum sensing.

[0003] For such applications it is necessary that the spin systems or color centers with a high spatial accuracy in the nanometer range, while simultaneously achieving the highest possible magnetic spin and optical Properties of the color centers are desired. For NV centers, for example, this is regularly achieved by implanting of nitrogen ions with low energies and subsequent thermal annealing. Ion implantations enable a comparatively high positional accuracy of the color centers with a spatial Resolution, for example, in the range of 5 to 10 nm (nanometers) at an implantation energy of about 10 keV (kiloelectronvolts).

[0004] For many applications, especially in the field of quantum computing, coupling spin systems desired, in which, for example, at least two spins interact (measurably) with each other. Since the magnetic Since the interaction between two spins decreases quadratically with the spin separation, it is necessary to determine the spins to be coupled as close to each other as possible in the diamond. In other words, at least two spin systems or Color centers are created at a distance of a few nanometers in the diamond lattice.

[0005] For the generation of coupling spin systems, it is known, for example, from F. Dolde et al., Nature Physics 9, 139-143 (2013), and M. Haruyama et al., Nature Communications 10, 2664 (2019, known, nitrogen molecules (N ) or molecules (C 2 NH ) from an adenine ion source so that the resulting NV centers are as close as possible 5 4 n are arranged relative to each other. 13

[0006] For the coupling between a NV center and a C nuclear spin, for example, it is known from T. Unden et al., npj 13 Quantum Information 4, 39 (2018) announced the implantation of nitrogen into a C-enriched diamond. Alternatively 13 Intrinsic or implanted NV centers can be found in diamonds with natural isotopic composition (approx. 1.1% C) 13 used, with certain NV-C spin configurations occurring purely randomly.

[0007] Experience shows that the chances of success for the generation of coupling (electron-electron) spin systems are the methods described above at about 1:200 to 1:500, so that usually hundreds of spins are examined to identify a coupling spin system. Furthermore, there is essentially no control about the resulting coupling strength, since the distance between the coupling spins is random. Applications in the field of quantum computing are adversely affected.

[0008] The invention is based on the object of specifying a particularly suitable diamond element in which the Spin distances between coupled spin systems can be adjusted. In particular, the randomness of the resulting The coupling strength between the spins can be reduced. The invention is further based on the object of to specify a suitable method for producing the diamond element.

[0009] With regard to the diamond element, the object is achieved by the features of claim 1 and with regard to the Method with the features of claim 10 according to the invention. Advantageous embodiments and Further developments are the subject of the dependent claims. The diamond element The advantages and features mentioned above can also be applied to the procedure and vice versa.

[0010] The diamond element according to the invention comprises a substrate with a epitaxial layer system made of a 12C carbon isotope-enriched diamond material.

[0011] The substrate is designed in particular as a diamond substrate, i.e. as a substrate made of a diamond material, so that the layer system is produced in particular by homoepitaxial growth on the substrate.

[0012] A ´´diamond material´´ here and in the following is understood to mean in particular a synthetic single crystal Diamond material which is deposited in particular by means of chemical vapor deposition (CVD) Deposition (CVD). The diamond material has preferably the highest possible purity and electronic quality as well as the lowest possible number of lattice defects The diamond material, for example, has a nitrogen and / or boron content of less than 1 ppb (parts per billion) and a 13 Isotopic content of C carbon of about 1.1% or less.

[0013] Preferably, a so-called IIa-(100) substrate, i.e. a substrate made of a type IIa diamond material with (100) -surface. In principle, a (111), (110) or (113)-oriented substrate can also be used, which However, the highest purity in terms of nitrogen is offered by (100). At (100) the intrinsic nitrogen content is less than 50 2 ppb, which corresponds to approximately one intrinsic NV center per (20 µm).

[0014] The substrate is preferably thin or flat, in particular the substrate has a thickness or height which is significantly lower than its dimensions along a longitudinal and transverse direction. For example, the substrate has a dimension of 2 mm (millimeters) by 2 mm along the longitudinal and transverse directions and a dimension between 10 µm (micrometers) to 500 µm along the thickness or height direction. 12

[0015] A ´´carbon isotope-enriched diamond material´´ here and in the following means a C- 12 13 enriched diamond material, i.e. a diamond material which, compared to the natural C / C isotope distribution 13 12 has a reduced C content. The proportion of C in the carbon isotope-enriched Diamond material is preferably between 98.9% and 99.99%. The carbon isotope-enriched Diamond material preferably has the same crystal orientation as the substrate, preferably (100) or (111).

[0016] The layer system is in particular in a growth or epitaxy process, for example in a CVD process, preferably in a homoepitaxial diamond synthesis, onto the surface of the substrate grew up.

[0017] According to the invention, the layer system has at least two spin layers arranged one above the other, each with of a spin species, with a buffer layer arranged between each of the spin layers. particularly suitable diamond element.

[0018] A ´´buffer layer´´ is understood here and below to mean in particular a layer made of carbon isotope-enriched diamond material. The buffer layer is essentially spin-free, which means that only a very low concentration or (spin) density of (paramagnetic) spin defects or Spin impurities are present in the crystal lattice. In a (100) buffer layer, the intrinsic nitrogen content is for example less than 50 ppb.

[0019] A ´´spin layer´´ here and in the following is understood to mean in particular a layer of carbon isotope-enriched diamond material, in which an increased proportion of a respective spin species is introduced. The proportion or concentration of spin species in the diamond material is therefore within the Spin layer is increased compared to the buffer layer. The spin species are, for example, by ion implantation (according to layer growth) or by delta doping (during layer growth) into the spin layer. 2 Spin concentration or spin density of the spin species in the spin layer is, for example, 1 to 3 per (100 nm). Spin concentration is in particular between 1 ppm and 100 ppm. The spin concentration within a spin layer is, for example, at least three orders of magnitude higher than in the buffer layer or the pure carbon isotope-enriched diamond material.

[0020] A ´´spin species´´ here and in the following means a type of spin, in particular a spin impurity or a Spin defects, i.e. electron or nuclear spins, in the carbon isotope-enriched diamond material. Preferably, the spin species is an electron spin species, for example electron spins of Color centers, especially NV or SiV centers. A color center is defined as a point or lattice defect in the To understand the solid lattice of the carbon isotope-enriched diamond material, which optically visible light absorbed.

[0021] The spin layers can each have the same spin species, or with different spin species. The spin layers should also have the same spin densities. However, different spin densities in the spin layers are also possible.

[0022] In the following, information regarding the spatial directions is also particularly in a coordinate system of the diamond element with respect to a growth direction on the substrate. The abscissa axis (X-axis, X- direction) and the ordinate axis (Y-axis, Y-direction) are along the longitudinal direction (length) and transverse direction (width) of the substrate, with the applicator axis (Z-axis, Z-direction) along the substrate height, i.e. along the growth direction along which the layer system has grown. The Z-direction is therefore in Essentially oriented perpendicular or normal to the layers of the layer system.

[0023] According to the invention, the spins to be coupled (nuclear or electron spins, e.g. SiV, NV centers) are arranged in at least arranged in two separate layers (spin layers), which are separated by a nearly spin-free diamond layer (buffer layer). The thickness of the buffer layer thus dominates the Z-component of the distance vector between the Spin species or spins of the spin layers, which allows the coupling strength between the spins to be controlled. In other words, the buffer layer enables the diamond growth during the production of the layer system to Adjusting the coupling strengths between the spins, which is not possible in other material arrangements. The diamond element according to the invention thus realizes a controlled spin coupling between the spins of the spin layers. This is particularly advantageous for applications in the field of quantum information, so that the diamond element for example, can be used as a diamond chip.

[0024] In a suitable further development, the substrate has a carbon isotope-enriched surface layer. The surface layer is made of a carbon isotope-enriched diamond material, so that the first spin layer of the layer system is separated from the substrate material by the surface layer. In particular This eliminates unwanted couplings between the spins of the first spin layer and any existing (intrinsic) spin of the substrate is prevented or at least reduced. The surface layer, for example, has a Layer thickness, i.e. an extension along the Z-direction, from 10 nm (nanometers) to 100 nm, for example about 30 12 12 nm. For example, in an Ila-(100) substrate, a 10 nm to 100 nm thick C layer (98.9 % to 99.99 % C- portion) grown as a surface layer using CVD.

[0025] In a conceivable embodiment, the spin layers each have a layer thickness between 0.1 nm and 3 nm. This ensures that the spins of the spin species have a high accuracy or localization along the Z- direction so that the coupling strength can be adjusted as precisely as possible using the buffer layer.

[0026] In an expedient embodiment, the layer system has a protective layer which is applied to the outermost spin layer is applied. The protective layer is made of carbon isotope-enriched diamond material This protects the spin layer from surface contamination. The protective layer insulates the coupling spins of the spin layers from the surface or the environment.

[0027] In a suitable embodiment, the protective layer has a layer thickness between 0.1 nm and 10,000 nm. Smaller layer thicknesses allow coupling of the spin layer spins to external spins, which, for example, placed on the surface of the protective layer. This is advantageous, for example, in applications of Diamond element as a quantum sensor. Larger layer thicknesses isolate the spins of the layer system from the environment, so that a particularly effective and reliable control of the coupling spins is possible. Furthermore, the Spin properties, especially the coherence time, of deep spins, i.e. with large protective layer thicknesses, are better than with flat spins (small protective layer thicknesses).

[0028] An additional or further aspect of the invention provides that at least one of the spin layers has a The nuclear spin layer is therefore between the spin layer and the Buffer layer (or protective layer) is arranged. In other words, directly or immediately adjacent to the A diamond layer with a high number of nuclear spins is provided for the spin layer. Since nuclear spins have a lower coupling strength than electron spins, it is advantageous to position the nuclear spins immediately adjacent to the spins of the to arrange spin layer. 13

[0029] For example, layers with variable nuclear spin concentration (e.g. 1.5% to 99.99% C) are realized, whereby in addition to the coupling between at least two electron spins, nuclear spins are also incorporated into the spin architecture This creates a spin architecture for the diamond element in which a coupling The spin system of the spin layers is additionally coupled to one or more nuclear spins. This is particularly the case in Applications in quantum information are advantageous, in which the nuclear spins serve as a (quantum) register for the coupling spin system can be used.

[0030] The separation of electron spins in the spin layer from the nuclear spins of the nuclear spin layer enables the control about the nuclear spin environment and the distance between the electron spins and the nuclear spins. The randomness of the coupling strength is thereby minimized.

[0031] Preferably, the or each nuclear spin layer has a layer thickness between 0.1 nm and 2 nm. This means that ensures small distances to the spins of the spin layer, which increases the probability of coupling between Nuclear spin layer and spin layer is increased.

[0032] The nuclear spin layers preferably have the same nuclear spin species, but versions with different nuclear spin species. The nuclear spin concentration in the nuclear spin slices can be the same or differentiate. 13

[0033] For example, a diamond material with a C content between 0.1% and 99.9% is used as a nuclear spin layer with a layer thickness between 0.1 nm and 2 nm. The diamond material has a nitrogen content 2 less than 50 ppb, i.e. less than 1 NV center per (20 µm).

[0034] For faster localization of coupling spins in a confocal volume of a confocal microscope, the Surface of the diamond element structured.

[0035] In a preferred embodiment, the layer system has a surface structuring.

[0036] The coupling range for electron spin-electron spin coupling is about 30 nm, and for Electron spin-nuclear spin coupling about 1.5 nm to 2 nm. The surface structuring furthermore realizes a Separation or subdivision of the layer system volume into several smaller sub-areas or coupling volumes, so that coupling spins are easier to select or address.

[0037] Surface structuring is, for example, a structuring or shaping of at least the outermost layers of the layer system. However, surface structuring also includes those To understand structures that essentially completely permeate the layer system.

[0038] Since the spin species of the spin layers are designed in particular as color centers, Surface structuring, for example, a photonic structure, e.g. an optical resonator or a nanolens, for improved coupling and decoupling of light, whereby measurement signals from coupling spin systems be improved.

[0039] The surface structuring is preferably designed as a number of nanopillars (nanopillars), in which several columnar layer systems are released. Such nanopillars act due to their cylindrical, conical, or truncated cone shape as a waveguide for the emitted light of the color centers. The nanopillars have a diameter between 50 nm and 500 nm, for example, between 100 nm and 300 nm. In parallel, the structuring enables selective optical addressing of NV and SiV centers using a laser if the nanopillars are sufficiently far apart.

[0040] In a conceivable further development, the surface structuring, in particular the nanopillars, is provided with a Buffer layer overgrown to improve the coherence and optical properties of the spin species.

[0041] The method according to the invention is intended for producing a diamond element as described above and suitable and designed for this purpose.

[0042] According to the method, a substrate, in particular a diamond substrate, is first provided. Preferably The substrate is cleaned beforehand. To clean the diamond material or the surface, the substrate for example in an acid solution of sulfuric acid (H SO ) and nitric acid (HNO ) and perchloric acid (HClO ) 2 4 3 4 cleaned.

[0043] The layer system with at least two spin layers and one epitaxially grown with a buffer layer arranged in between. In particular, carbon isotope-enriched diamond material. The carbon isotope-enriched Diamond material is particularly used in a growth or epitaxy process, for example in a CVD process. preferably in a homoepitaxial diamond synthesis, onto the surface of the substrate, in particular the surface layer, grown.

[0044] To produce a buffer layer, the carbon isotope-enriched diamond material To produce a spin layer, carbon isotope-enriched diamond material is grown in which a respective spin species is introduced. The spin species is, for example, after growth by means of Ion implantation into the diamond material. Alternatively, the spin species can be introduced in the form of delta doping, in which the grown diamond material is doped with foreign atoms, i.e. atoms which are not carbon, or is offset, into which diamond material is introduced during growth.

[0045] This provides a particularly suitable method. The method enables the controlled realization of electron spin-electron spin coupling of spin systems, which are optionally coupled to nuclear spins can be expanded.

[0046] After the layer system has grown, the diamond element is preferably annealed or baked so that Hydrogen (H2) diffuses out of the diamond lattice or the lattice structure of the diamond material. This improves the quality and purity of the coating system or the diamond material. For example, the diamond element is baked under high vacuum at 700 °C to 1600 °C for at least three hours. In a spin layer produced by ion implantation, the defects created by the implantation diffuse Vancancies through the diamond lattice and combine with the implanted nitrogen to form NV centers or in the case of implanted silicon, to SiV centers. The diamond element is then, for example, an acid solution and, for example, provided with a surface structure. Optionally, the Surface structuring is then finally overgrown with a buffer layer.

[0047] In the following, embodiments of the invention are explained in more detail with reference to the drawings. schematic and simplified representations: Fig. 1 in side view a diamond element in a first embodiment, Fig. 2 is a flow chart for a process for producing a diamond element in a first embodiment, Fig. 3 a diamond element in a second embodiment, and Fig. 4 is a flow chart for a process for producing a diamond element in a first Embodiment.

[0048] Corresponding parts and sizes are always provided with the same reference numerals in all figures.

[0049] The diamond element 2 shown in Fig. 1 comprises a substrate 4 and an epitaxial layer system 6.

[0050] The substrate 4 comprises, for example, a substrate element 4a and a surface layer 4b grown thereon on.

[0051] In the embodiment shown, the layer system 6 comprises two spin layers 8a, 8b, a buffer layer 10, and a protective layer 12. The spin layer 8a is arranged on the surface of the substrate 4, wherein the Buffer layer 10 is positioned between the spin layers 8a and 8b. The protective layer 12 is applied to the upper spin layer 8b upset.

[0052] In each of the spin layers 8a and 8b, a spin species 14 is introduced. The spins of the spin species 14 are in the Figures are shown only as examples and are provided with reference symbols. The spins of the spin layers 8a and 8b can Spins of the same spin species 14. Alternatively, the spins of the spin layers 8a and 8b are different spin species 14. Below, the spins 14 (without loss of generality) are in particular electron spins of a color center, for example an NV center.

[0053] The substrate element 4a is designed as a IIa (100) diamond, on which the surface layer 4b is deposited in a homoepitaxial growth process. The substrate element 4a points along a Z-direction oriented growth direction W has a layer thickness d. The layer thickness d is, for example, between 10 µm and 2 mm, in particular between 50 µm and 500 µm. In principle, however, the substrate element 4a can have any layer thickness d. 12

[0054] The surface layer 4b is a C layer and is made of an isotopically enriched diamond material with 12 For example, 99.99% C content is grown on the surface of the substrate element 4a by CVD. The intrinsic 2 Nitrogen content of the surface layer 4b is less than 50 ppb or less than one NV per (20 µm). Surface layer 4b has a layer thickness do which is dimensioned between 10 nm and 100 nm. In the In the embodiment shown in Fig. 1, the layer thickness do is, for example, 30 nm. 12

[0055] The spin layer 8a is made of an isotopically enriched diamond material with, for example, 99.99% C content homoepitaxially grown on the surface of the surface layer 4b by CVD. After growth, ion implantation nitrogen is introduced into the diamond material of the spin layer 8a, whereby the NV density after the 2 Completion of the layer system 6 and after annealing is approximately 1 / (100 nm). The spin layer 8a has a Layer thickness d1 between 0.1 nm and 3 nm. In the embodiment shown in Fig. 1, the layer thickness d1 is for example, 3 nm. The nitrogen content in the 3 nm thick spin layer 8a is about 94 ppm.

[0056] The buffer layer 10 is a 0.1 nm to 30 nm thick diamond layer made of an isotopically enriched 12 Diamond material with, for example, 99.99% C content, which is deposited by CVD onto the surface of the spin layer 8a is grown homoepitaxially. The intrinsic nitrogen content of the buffer layer 10 is less than 50 ppb 2 or less than one NV per (20 µm). The buffer layer 10 has a layer thickness dp, which in the Execution case example in Fig. 1 is dimensioned at 15 nm. 12

[0057] The spin layer 8b is made of an isotopically enriched diamond material with, for example, 99.99% C content homoepitaxially grown by CVD on the surface of the buffer layer 10. After growth, ion implantation nitrogen is introduced into the diamond material of the spin layer 8b, whereby the NV density after the 2 Completion of the layer system 6 and after annealing is approximately 1 / (100 nm). The spin layer 8b has a Layer thickness d2 between 0.1 nm and 3 nm. In the example shown in Fig. 1, the layer thickness d2 is for example, 3 nm. The nitrogen content in the 3 nm thick spin layer 8a is about 75 ppm.

[0058] Preferably, the lower spin layer 8a has an increased nitrogen content compared to the upper spin layer 8b In the exemplary embodiment, the nitrogen content of the spin layer 8a is, for example, 94 ppm, and the nitrogen content of spin layer 8b is about 75 ppm. The nitrogen content of the deeper spin layer 8a is chosen to be higher, since Overgrowth of the buffer layer 10 NVs can be lost. Due to the different nitrogen contents thus the probability of obtaining a coupling spin pair. 12

[0059] The protective layer 12 is made of an isotopically enriched diamond material with, for example, 99.99% C content homoepitaxially grown by CVD on the surface of spin layer 8b. The intrinsic nitrogen content of the 2 The protective layer 12 is less than 50 ppb or less than one NV per (20 µm). The protective layer 12 has a Layer thickness ds between 0.1 nm and 10000 nm, which in the embodiment of Fig. 1 is, for example, 30 nm is dimensioned.

[0060] The diamond element 2 is intended and configured to realize coupling spin systems. In particular coupling spin systems consisting of at least one spin 14 of the spin layer 8a and one spin 14 of the spin layer 8b. In the figures, the coupling K or interaction between the spins 14 is shown as a double arrow shown schematically.

[0061] The spins 14 to be coupled are arranged in the two separate spin layers 8a, 8b, which are separated by the nearly spin-free buffer layer 10. The layer thickness dp of the buffer layer 10 thus dominates the Z- Component of the distance vector between the spins 14 of the spin layers 8a, 8b, which increases the coupling strength of the coupling K between the spins 14. In other words, the buffer layer 10 thus enables Diamond growth during the production of the layer system 6 the adjustment of coupling strengths between the spins 14, which is not yet possible in other material arrangements.

[0062] A method for producing a diamond element 2 is explained in more detail below with reference to Fig. 2.

[0063] In a first method step 16, the substrate element 4a is provided. Preferably, the Substrate element 4a is first cleaned in an acid solution.

[0064] In process step 18, a diamond layer of carbon isotope-enriched diamond material. In this case, a layer thickness is grown which corresponds to the sum of the layer thicknesses do and d1 of the surface layer 4b and the spin layer 8a. 15+

[0065] In a subsequent process step 20, N ions are implanted into the diamond lattice of the Layer thickness d1 is introduced, thus forming the spin layer 8a.

[0066] In the subsequent process step 20, a diamond layer of carbon isotope-enriched diamond material. In this case, a layer thickness is grown which corresponds to the sum of the layer thicknesses dp and d2 of the buffer layer 10 and the spin layer 8b. 15+

[0067] In a subsequent process step 22, N ions are implanted into the diamond lattice of the Layer thickness d2 is introduced, thus forming the spin layer 8b.

[0068] Thereafter, in process step 24, a diamond layer of carbon isotope-enriched Diamond material with the layer thickness ds is grown as a protective layer 12 on the surface of the spin layer 8b.

[0069] After the growth of the layer system 6, the diamond element 2 is tempered in a process step 26 or baked. After baking, the diamond element 2 is again immersed in an acid solution cleaned.

[0070] In an optional process step 28, the surface of the diamond element 2, in particular the Layer system 6, structured. Nanopillars of layer system 6 are used as surface structuring in particular. For this purpose, a corresponding lithographic mask is applied to the surface of the protective layer 12 on and then the diamond element 2 is etched, for example by means of a reactive plasma, so that individual Nanopillars of layer system 6 are exposed. The nanopillars can then be covered with another buffer layer become overgrown.

[0071] In the following, a second embodiment of the diamond element 2' and a The corresponding (manufacturing) process is explained in more detail.

[0072] The diamond element 2' has a surface structuring of the layer system 6' in the form of nanopillars. Nanopillars, for example, have a diameter D between 10 nm and 1000 nm, with a distance A between two adjacent nanopillars is, for example, between 500 nm and 50 µm. The nanopillars are thus far enough apart that using a confocal microscope the spins 14 or color centers of a individual nanocolumn are measurable.

[0073] The diamond element 2' or the layer system 6' in this embodiment has two additional Nuclear spin layers 30a, 30b, each of which is grown on one of the spin layers 8a, 8b. The nuclear spin layer 30a is between the spin layer 8a and the buffer layer 10 and the nuclear spin layer 30b is between the Spin layer 8b and the protective layer 12.

[0074] In the nuclear spin layers 30a and 30b, nuclear spins of a nuclear spin species 32 are introduced. The nuclear spins The nuclear spin species 32 are shown in Fig. 3 only as examples and are provided with reference symbols. The nuclear spins 32 of the nuclear spin layers 30a and 30b can be nuclear spins of the same nuclear spin species. Alternatively, the nuclear spins 32 the nuclear spin layers 30a,30b also belong to different nuclear spin species. 13

[0075] Preferably, the nuclear spins 32 are C nuclear spins. The nuclear spin layers 30a, 30b thus have 13 compared to the diamond material of layers 4a, 8a, 8b, 10, and 12 has an increased proportion of C. 13 For example, the nuclear spin layers 30a, 30b are each a diamond material with a C content between 0.1% and 99.9% with a layer thickness dk1, dk2 between 0.1 nm and 2 nm. The diamond material of the 2 Nuclear spin layers 30a, 30b have a nitrogen content of less than 50 ppb, i.e. less than 1 NV center per (20 µm) on.

[0076] The process for producing the diamond element 2' shown in Fig. 4 differs from the described above in Fig. 2 by two additional process steps 34, 36 during the growth of the Layer system 6'.

[0077] Method step 34 is carried out between method steps 20 and 22. In method step 34 13 the C-enriched diamond material of the nuclear spin layer 30a is grown on the surface of the spin layer 8a. A layer thickness dk1 is grown which is dimensioned between 0.1 nm and 2 nm.

[0078] Accordingly, method step 36 is carried out between method steps 24 and 26. Here, 13 the surface of the spin layer 8b the C-enriched diamond material of the nuclear spin layer 30b with a layer thickness dk2, which is dimensioned between 0.1 nm and 2 nm.

[0079] The claimed invention is not limited to the embodiments described above. Rather Other variants of the invention can also be derived by the person skilled in the art within the scope of the disclosed claims without departing from the subject matter of the claimed invention. In particular, all individual features described with the various embodiments within the scope of the disclosed claims also can be combined in other ways without departing from the subject matter of the claimed invention.

Claims

1. Diamond element (2, 2'), comprising a substrate (4) with an epitaxial layer system (6, 6') applied thereon 12 made of C-carbon isotope-enriched diamond material, - wherein the layer system (6, 6') comprises at least two spin layers (8a, 8b) arranged one above the other, each with a spin species (14), and - wherein a substantially spin-free buffer layer (10) is arranged between each two spin layers (8a, 8b). 12 2. Diamond element (2, 2') according to claim 1, characterized in that the substrate (4) has a C- carbon isotope-enriched surface layer (4b).

3. Diamond element (2, 2') according to claim 1 or 2, characterized in that the spin layers (8a, 8b) each have a Layer thickness (d1, d2) between 0.1 nm and 3 nm.

4. Diamond element (2, 2') according to one of claims 1 to 3, characterized in that the or each buffer layer (10) has a layer thickness (dp) between 0.1 nm and 30 nm.

5. Diamond element (2, 2') according to one of claims 1 to 4, characterized in that the layer system (6, 6') has a protective layer (12) which is applied to the outermost spin layer (8b).

6. Diamond element (2, 2') according to claim 5, characterized in that the protective layer (12) has a layer thickness (ds) between 0.1 nm and 10000 nm.

7. Diamond element (2, 2') according to one of claims 1 to 6, characterized in that at least one of the Spin layers (8a, 8b) a nuclear spin layer (30a, 30b) with a nuclear spin species (32) is applied.

8. Diamond element (2, 2') according to claim 7, characterized in that the or each nuclear spin layer (30a, 30b) has a Layer thickness (dk1, dk2) between 0.1 nm and 2 nm.

9. Diamond element (2, 2') according to one of claims 1 to 8, characterized in that the layer system (6, 6') has a has surface structuring.

10. A method for producing a diamond element (2, 2') according to one of claims 1 to 9, - wherein a substrate (4) is provided, - wherein at least two spin layers (8a, 8b) are applied to the substrate (4) with a buffer layer (10) arranged therebetween are grown as an epitaxial layer system (6, 6'), 12 - wherein, to produce a spin layer (8a, 8b), C-carbon isotope-enriched diamond material is grown into which a respective spin species (14) is introduced, and 12 - wherein C-carbon isotope-enriched diamond material is grown to produce a buffer layer (10).

Citation Information

Patent Citations

  • Method for producing color centers in diamond and substrate produced therewith

    DE102021210096B3

  • Diamond material

    US20120051996A1

Cited By

  • Spin information transport device and method for its manufacture

    DE102024004624A1

  • Spin information transport device and method for its manufacture

    DE102024139460B3