Exchange-coupled film and magnetoresistive element, and magnetism detection device equipped therewith
The exchange-coupled film with a specific antiferromagnetic layer structure enhances resistance to strong magnetic fields, addressing stability issues in magnetoresistive elements, ensuring reliable operation in high magnetic and temperature environments.
Patent Information
- Application Number
- DE112019006539
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-26
- Filing Date
- 2019-12-11
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2039-12-11
AI Technical Summary
Magnetoresistive elements used in magnetism detection devices face challenges in maintaining stable magnetization direction in high magnetic fields and high-temperature environments, particularly when subjected to solder reflow processing and exposure to strong magnetic fields from sources like high-performance motors.
An exchange-coupled film structure is developed with an antiferromagnetic layer comprising IrMn, PtMn, and PtCr layers stacked in a specific order, enhancing the exchange coupling field to resist magnetization reversal in strong magnetic fields, and allowing for a higher exchange coupling field Hex compared to coercive force Hc, thereby stabilizing the magnetization direction.
The proposed film structure provides excellent resistance to strong magnetic fields and maintains stable magnetization even in harsh environments, ensuring reliable operation of magnetoresistive elements in conditions with high magnetic interference.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical field
[0001] The present invention relates to an exchange-coupled film and a magnetoresistive element or Magnetoresistive element and a magnetism detection device comprising the exchange-coupled film. Relevant state of the art
[0002] Exchange-coupled films with an antiferromagnetic layer and a pinned magnetic layer are known as magnetoresistive elements or magnetic sensors are used. Patent document 1 states that in a magnetic A recording medium, an exchange-coupled film, can be formed by using a co-alloy that acts as ferromagnetic film is used in combination with various alloys that serve as antiferromagnetic films. Examples of antiferromagnetic films include alloys such as CoMn, NiMn, PtMn and PtCr.
[0003] WO 2018 / 029 883 A1 describes an exchange coupling film comprising an antiferromagnetic layer, a It comprises a fixed magnetic layer and a free magnetic layer stacked together. The antiferromagnetic layer consists of a PtCr layer and an XMn layer (where X is Pt or Ir), and the XMn- The layer touches the fixed magnetic layer.
[0004] US 2015 / 0340598A1 describes a magnetic RAM element comprising: a multilayer Germinal structure consisting of alternating layers of a sublayer of the first type and a sublayer of the second type Types are formed to create one or more repetitions of a unit layer structure from the sublayers of the first and of the second type, wherein at least one of the sublayers of the first and second types contains one or more contains ferromagnetic elements; and a first magnetic layer formed on the multilayered nucleus structure is.
[0005] DE 602 00 949 T2 describes a magnetoresistive element with: a multilayer film which at least has two magnetic layers and at least one non-magnetic layer located between the two magnetic layers The layers are arranged, with a resistance value changing with a relative angle determined by the Magnetization directions of the at least two magnetic layers are formed, and wherein at least one of the magnetic layers comprise a ferromagnetic material MX, which is expressed by M100-aXa, where M at least one element is selected from the group consisting of Fe, Co and Ni, where X is represented by X1bX2cX3d is expressed where X1 is at least one element selected from the group consisting of Cu, Ru, Rh, Pd, Ag, Os, Ir, Pt and Au, X2 is at least one element selected from the group consisting of Al, Sc, Ti, V, Cr, Mn, Ga, Ge, Y, Zr, Nb, Mo, Hf, Ta, W, Re, Zn and lanthanide series elements, X3 is at least one element that is selected from the group consisting of Si, B, C, N, O, P and S, where a, b, c, and d satisfy the following equations: 0.05 ≤ a ≤ 60, 0 ≤ b ≤ 60, 0 ≤ c ≤ 30 0 ≤ d ≤ 20, and a = b + c + d.
[0006] JP 2002-298 326 A describes how a spiky noise, caused by a layered arrangement The soft magnetic layer that is created can be reduced by using a vertical magnetic Recording medium that provides an antiferromagnetic layer between a film with vertical Magnetization and the layered soft magnetic layer are formed. This results in a non-magnetic intermediate layer between the film with vertical magnetization and the antiferromagnetic layer arranged, and a layer is provided consisting of the non-magnetic intermediate layer and a ferromagnetic film (soft magnetic layer) between the film with vertical magnetization and the consists of an antiferromagnetic layer. List of state of the art Patent literature
[0007] Patent document 1: Unexamined Japanese patent application publication no. JP 2000-215431A Brief description of the invention Technical problem
[0008] A magnetism detection device must be used in a solder reflow processing (melt processing) are subjected to this when a magnetoresistive element is mounted on a circuit board. The magnetism- The detection device is sometimes used in a high-temperature environment, for example near a motor, used. For an exchange-coupled film used in the magnetism detection device, a Magnetic field (hex) required to reverse the magnetization direction of a pinned magnetic layer, preferably high, to enable the detection of a magnetic field over a wide dynamic range.
[0009] Recently it has become desirable that the magnetization direction of a pinned magnetic layer even in an environment where the magnetism detection device is near a source of a strong magnetic field, such as a high-performance motor, and in an environment where a high magnetic field is applied to it. It will be less affected. That means resistance to strong magnetic fields is required.
[0010] The present invention aims to provide an exchange-coupled film in which a magnetic field (Hex), which is required to reverse the magnetization direction of a ferromagnetic layer, such as a pinned magnetic layer that is exchange-coupled with an antiferromagnetic layer, is high and thus exhibits excellent resistance to strong magnetic fields, as well as providing a magnetoresistive element and a magnetism detection device comprising the exchange-coupled film. Solution to the problem
[0011] According to one aspect of the present invention for solving the above problems, a exchange-coupled film characterized by having an antiferromagnetic layer and a ferromagnetic layer The layer is stacked together, with the antiferromagnetic layer having a structure that incorporates IrMn- The layer includes a first PtMn layer, a PtCr layer, and a second PtMn layer, stacked in that order. are, with the IrMn layer located close to the ferromagnetic layer. The IrMn layer can be stacked in this way. It is possible that it is in contact with the ferromagnetic layer. The structure may also include a PtMn layer which stacked between the IrMn layer and the ferromagnetic layer.
[0012] The units Angström and Oersted used here can be converted into SI units via the following relationships Unit conversion: 1 Å=0.1nm, 1 Oe=(1000 / (4&pgr;))(A / m).
[0013] Fig. 1 shows a hysteresis loop in the magnetization curve of an exchange-coupled film according to the present invention. Typically, a magnetization curve (MH curve) of a soft magnetic material is described. The hysteresis loop formed by the material is symmetrical around the intersection of the H-axis and the M-axis (magnetic field H = 0 A). / m and magnetization M = 0 A / m). However, as shown in Fig. 1, in the exchange-coupled film according to the In the present invention, the hysteresis loop of the exchange-coupled film has a shape that extends along the H-axis. is shifted according to the size of the exchange coupling field Hex, because an exchange coupling field Hex is applied to a The pinned magnetic layer, which contains the ferromagnetic layer, interacts with the antiferromagnetic layer. is exchange-coupled. The pinned magnetic layer of the exchange-coupled film, which has a higher Hex, which exhibits an exchange coupling field, is less likely to cause an effect when an external magnetic field is applied. Reversal of the magnetization direction and is therefore a better pinned magnetic layer.
[0014] The coercive force Hc is defined as the difference between the center of the H-axis shifted along the H-axis. Hysteresis loop (the magnetic field strength at the center corresponds to the exchange coupling field Hex) and the intersection point the hysteresis loop with the H-axis. It is assumed that the coercive force Hc is less than the The exchange coupling field is hex. Even when an external magnetic field is applied to the pinned magnetic layer of the exchange-coupled film in one direction along the external To magnetize a magnetic field, the magnetization direction of the pinned magnetic layer can, in this case, be determined by the Exchange coupling field Hex, which is relatively stronger than the coercive force Hc, when the external connection is terminated be aligned with the magnetic field. That is, if the relationship between the exchange coupling field Hex and the If the coercivity Hc Hex > Hc is, the exchange-coupled film has a satisfactory resistance to strong forces. Magnetic fields.
[0015] In the exchange-coupled film according to one aspect of the present invention, the The antiferromagnetic layer has a structure comprising the IrMn layer, the first PtMn layer, the PtCr layer, and the second layer. The PtMn layer is stacked together, thereby achieving the improvement of the exchange coupling field Hex. In the exchange-coupled film according to the present invention, a high exchange coupling field (Hex) can be achieved. even with a small thickness of the PtCr layer, compared to the case where the second PtMn layer It is not stacked. Therefore, the thickness (total thickness) of the entire antiferromagnetic layer can be relatively reduced. will be what is preferred from the point of view of production efficiency, etc.
[0016] According to a further aspect of the present invention, an exchange-coupled film is provided which characterized by having an antiferromagnetic layer and a ferromagnetic layer which are stacked together, with the antiferromagnetic layer having a structure comprising a first PtMn layer, a It includes a PtCr layer and a second PtMn layer, stacked in this order, with the first PtMn layer being... layer is located close to the ferromagnetic layer, with the thickness of the PtCr layer being greater than both the thickness the thickness of both the first PtMn layer and the second PtMn layer. In the exchange-coupled film, which the The antiferromagnetic layer with its stacked structure exhibits a high exchange coupling field (Hex), and the The relationship between the exchange coupling field Hex and the coercive force Hc tends to be Hex > Hc; thus, the The Hex exchange coupling field exhibits satisfactory resistance to strong magnetic fields. Additionally, the In some cases, exchange-coupled films can have a high blocking temperature.
[0017] The aforementioned antiferromagnetic layer can be a Mn-containing layer with a Mn content of more more than 50 at% between the first PtMn layer and the ferromagnetic layer. The Mn-containing layer can multiple stacked layers. The Mn-containing layer may contain at least one layer consisting of the The group selected consists of an IrMn layer and a Mn layer. In the case where the Mn-containing layer formed from an IrMn layer or a stack of an IrMn layer and a PtMn layer, the The exchange-coupled film has the same structure as the exchange-coupled film according to the aspect mentioned above. of the present invention. From the point of view of suppressing the effect of variations in the thickness of the in the The layers containing the antiferromagnetic layer affect the properties of the antiferromagnetic layer (for For example, the size of the exchange coupling field (Hex) means that in some cases the Mn-containing layer preferably has a thickness of of 12 Å or less.
[0018] In the above-mentioned exchange-coupled film, the second PtMn layer exhibits in some cases preferably has a thickness of more than 0 Å and less than 60 Å. The second PtMn layer exhibits, in some cases, preferably a thickness of 15 Å or more and 55 Å or less. Regarding the above-mentioned In exchange-coupled films, the PtCr layer in some cases preferably has a thickness of 100 Å or more. In some cases, the antiferromagnetic layer preferably has a total thickness of 200 Å or less.
[0019] According to a further aspect of the present invention, a magnetoresistive element is provided which characterized by the fact that it has the aforementioned exchange-coupled film and a free magnetic layer exhibits, which are stacked together, wherein the ferromagnetic layer of the exchange-coupled film is in at least is contained in part of a pinned magnetic layer.
[0020] According to a further aspect of the present invention, a magnetism detection device is provided, which is characterized by having the aforementioned magnetoresistive element.
[0021] In the aforementioned magnetism detection device, the magnetoresistive element of one of a plurality of magnetoresistive elements arranged on the same substrate net are, and the majority of magnetoresistive elements can bind the pinned magnetic layers with different exhibit fixed or pinned magnetization directions. Advantageous effects of the invention
[0022] According to the present invention, the exchange-coupled film has excellent resistance to strong magnetic fields are provided. Thus, the use of the exchange-coupled film according to the present The invention itself provides a stable magnetism detection device in an environment with strong magnetic fields. lead. Brief description of the drawings [Fig. 1] Fig. 1 shows a hysteresis loop in the magnetization curve of an exchange-coupled film according to of the present invention. [Fig. 2] Fig. 2 shows the layer structure of an exchange-coupled film 10 according to a first embodiment of the present invention. [Fig. 3] Fig. 3 shows the layer structure of an exchange-coupled film 20 according to a second embodiment of the present invention. [Fig. 4] Fig. 4 shows a circuit block diagram of a magnetic sensor 30 according to an embodiment of the present invention. [Fig. 5] Fig. 5 shows a top view representing a magnetic detection element 11, which is used for the A magnetic sensor 30 is used. [Fig. 6] Fig. 6 shows the layer structure of a multilayer stack 22 according to Example 1. [Fig. 7] Fig. 7 shows a graphical representation illustrating the dependence of an exchange coupling field Hex on the Thickness (total thickness) of an antiferromagnetic layer 2 illustrated. [Fig. 8] Fig. 8 shows a graphical representation illustrating the dependence of the ratio (Hex / Hc) of the Exchange coupling field Hex to a coercive force Hc of the thickness (total thickness) of the antiferromagnetic Layer 2 illustrated. [Fig. 9] Fig. 9 shows a graphical representation illustrating the dependence of the exchange coupling field Hex on the Thickness d4 of a second PtMn layer 2d illustrated. [Fig. 10] Fig. 10 shows a graphical representation illustrating the dependence of the ratio (Hex / Hc) of the Exchange coupling field Hex to coercive force Hc of thickness d4 of a second PtMn layer 2d illustrated. [Fig. 11] Fig. 11 shows a graphical representation illustrating the dependence of the exchange coupling field Hex on the Total thickness of the antiferromagnetic layer illustrated. [Fig. 12] Fig. 12 shows a graphical representation illustrating the dependence of the ratio (Hex / Hc) of the Exchange coupling field Hex to coercive force Hc of the total thickness of the antiferromagnetic layer illustrated. [Fig. 13] Fig. 13 shows a graphical representation illustrating the dependence of the exchange coupling field Hex on the The measurement temperature is illustrated in comparison examples 11 to 13 and example 12. [Fig. 14] Fig. 14 shows a graphical representation illustrating the dependence of the ratio (Hex / Hc) of the Exchange coupling field Hex to coercive force Hc of the measurement temperature in comparison examples 11 to 13 and example 12 illustrates this. [Fig. 15] Fig. 15 shows a graphical representation illustrating the dependence of the exchange coupling field Hex on the The measurement temperature is illustrated in comparison examples 14 and 15 and examples 11 to 14. [Fig. 16] Fig. 16 shows a graphical representation illustrating the dependence of the ratio (Hex / Hc) of the Exchange coupling field Hex to coercive force Hc of the measurement temperature in comparison examples 14 and 15 and illustrated by examples 11 to 14. [Fig. 17] Fig. 17 shows the layer structure of an exchange-coupled film 70 according to a third embodiment of the present invention. [Fig. 18] Fig. 18 shows the layer structure of an exchange-coupled film 71 according to a modification of the third embodiment of the present invention. [Fig. 19] Fig. 19 shows the layer structure of an exchange-coupled film 72 according to a further Modification of the third embodiment of the present invention. [Fig. 20] Fig. 20 shows the layer structure of an exchange-coupled film 73 according to a further Modification of the third embodiment of the present invention. [Fig. 21] Fig. 21 shows the layer structure of a multilayer stack 221 according to Example 21. [Fig. 22] Fig. 22 shows the layer structure of a multilayer stack 222 according to examples 27 to 31. [Fig. 23] Fig. 23 shows a diagram illustrating the relationship between the exchange coupling field Hex (left) vertical axis) and the thickness of a Mn-containing layer (thickness of Mn or IrMn in intermediate arrangement) and between the ratio (Hex / Hc) (right vertical axis) of the exchange coupling field Hex to the coercive force Hc and illustrates the thickness of the Mn-containing layer (thickness of Mn or IrMn intermediate arrangement). [Fig. 24] Fig. 24 shows a graphical representation illustrating the dependence of the exchange coupling field Hex on the Thickness D4 of a second PtMn layer 8d illustrated. [Fig. 25] Fig. 25 shows a graphical representation illustrating the dependence of the ratio (Hex / Hc) of the Exchange coupling field Hex to coercive force Hc of thickness D4 of a second PtMn layer 8d illustrated. [Fig. 26] Fig. 26 shows a graphical representation illustrating the dependence of the exchange coupling field Hex on the Thickness X of a pinned magnetic layer 3 (Co Fe ) illustrated. 90 At.-% 10 At.-% [Fig. 27] Fig. 27 shows a graphical representation illustrating the dependence of the exchange coupling field Hex on the Thickness X of the pinned magnetic layer 3 (Co Fe ) illustrated. 40 At.-% 60 At.-% [Fig. 28] Fig. 28 shows a graphical representation illustrating the dependence of the ratio (Hex / Hc) of the Exchange coupling field Hex to coercive force Hc of thickness X of the pinned magnetic layer 3 (Co Fe 90% ) illustrated. 10 At.-% [Fig. 29] Fig. 29 shows a graphical representation illustrating the dependence of the ratio (Hex / Hc) of the Exchange coupling field Hex to coercive force Hc of thickness X of the pinned magnetic layer 3 (Co Fe 40% ) illustrated. 60 At.-% [Fig. 30] Fig. 30 shows a graphical representation illustrating the dependence of the exchange coupling field Hex on the Thickness d4 of the second PtMn layer 2d illustrated. [Fig. 31] Fig. 31 shows a graphical representation illustrating the dependence of the exchange coupling field Hex on the Total thickness of the antiferromagnetic layer 2 illustrated. [Fig. 32] Fig. 32 shows a graphical representation illustrating the dependence of the ratio (Hex / Hc) of the The exchange coupling field Hex to the coercive force Hc of the thickness d4 of the second PtMn layer 2d is illustrated. [Fig. 33] Fig. 33 shows a graphical representation illustrating the dependence of the ratio (Hex / Hc) of the Exchange coupling field Hex to coercive force Hc of the total thickness of the antiferromagnetic layer 2 illustrated. [Fig. 34] Fig. 34 shows a graphical representation illustrating the dependence of the exchange coupling field Hex on the Thickness d1 of an IrMn layer 2a illustrated. [Fig. 35] Fig. 35 shows a graphical representation illustrating the dependence of the coercive force Hc on the thickness d1 of the IrMn layer 2a illustrated. [Fig. 36] Fig. 36 shows a graphical representation illustrating the dependence of the ratio (Hex / Hc) of the The exchange coupling field Hex to the coercive force Hc of the thickness d1 of the IrMn layer 2a is illustrated. [Fig. 37] Fig. 37 shows a graphical representation illustrating the dependence of the exchange coupling field Hex on the Total thickness of the antiferromagnetic layer 2 illustrated. Description of the embodiments <Erste Ausführungsform>
[0023] Fig. 2 shows the layer structure of a magnetic detection element 11 with an exchange-coupled film 10 according to a first embodiment of the present invention.
[0024] The magnetic detection element 11 comprises a lower layer or sublayer 1, a antiferromagnetic layer 2, a pinned magnetic layer 3 formed from a ferromagnetic layer, a Layer 4 made of non-magnetic material, a free magnetic layer 5 and a protective layer 6, in this order starting from a surface of a substrate SB, they are stacked (this being referred to as soil type). The antiferromagnetic layer 2 has a stacked structure comprising an IrMn layer 2a, a first PtMn layer 2b, a PtCr- It includes layer 2c and a second PtMn layer 2d, which are stacked in this order, with the IrMn layer 2a is located close to the ferromagnetic layer (pinned magnetic layer 3). The IrMn layer 2a can be stacked in this way. It should be in contact with the pinned magnetic layer 3. These layers are connected, for example, by a A sputtering process or a chemical vapor deposition (CVD) process is used. After formation, a Heat treatment was carried out to improve the exchange coupling between the antiferromagnetic layer 2 and the to create a pinned magnetic layer 3. The antiferromagnetic layer 2 and the pinned magnetic layer 3 serve as exchange-coupled film 10 according to the first embodiment of the present invention.
[0025] The magnetic detection element 11 is a multi-layered element that has a The so-called giant magnetoresistance effect of the single-spin valve type (GMR effect) is used. The electrical Its resistance varies according to the relative relationship between the vector of the pinned magnetization of the pinned magnetic layer 3 and the magnetization vector of the free magnetic layer 5, which according to an external Magnetic field varies.
[0026] For example, a silicon substrate with an aluminum oxide layer arranged on it is used as the substrate SB. used. The sublayer 1, for example, consists of a NiFeCr alloy (nickel-iron-chromium alloy), Cr or Ta. In the exchange-coupled film 10 according to the embodiment, the NiFeCr alloy is preferred to enable the to increase the magnetic field required to reverse the magnetization direction of the pinned magnetic layer 3 (hereinafter also appropriately referred to as "Hex").
[0027] The antiferromagnetic layer 2 has a structure comprising the IrMn layer 2a, the first PtMn layer 2b, the It contains PtCr layer 2c and the second PtMn layer 2d, which are stacked together. This structure leads to a strong exchange coupling field Hex and thus enables the ratio (Hex / Hc) of the exchange coupling field Hex The coercivity Hc is readily 1 or more. Accordingly, the exchange-coupled film 10 exhibits a exhibits excellent resistance to strong magnetic fields.
[0028] The IrMn layer 2a preferably has a thickness of 12 Å or less, more preferably 4 Å or more and 10 Å or less. If the thickness of the IrMn layer 2a is within the range, the exchange coupling field can be Hex. to improve to increase Hex / Hc. If the thickness of IrMn layer 2a is within the range, Furthermore, variations in the thickness of the first PtMn layer 2b have a lesser influence on the exchange coupling field. Hex and Hex / Hc. The second PtMn layer 2d preferably has a thickness of more than 0 Å and less than 60 Å, further preferably 10 Å or more and 50 Å or less or 15 Å or more and 55 Å or less, particularly preferably 20 Å or more and 50 Å or less. If the thickness of the second PtMn layer 2d is within the range, the The exchange coupling field Hex can be improved by increasing Hex / Hc.
[0029] The PtCr layer 2c preferably has a thickness of 100 Å or more, more preferably 110 Å or more. If the If the PtCr layer 2c has a thickness of 100 Å or more, the exchange coupling field can be increased by hexadecimal values. / Hc can be improved. The upper limit of the thickness of the PtCr layer 2c is, from the point of view of In some cases, production efficiency of 200 Å or less is preferred.
[0030] The antiferromagnetic layer 2 preferably has a total thickness of 200 Å or less. Even if the antiferromagnetic layer 2 has a total thickness of 200 Å or less, can The exchange coupling field Hex can be improved; thus, the production efficiency of the exchange-coupled film can be increased. 10 can be improved.
[0031] In the present embodiment, the antiferromagnetic layer 2 is ordered by heat treatment, to establish an exchange coupling (at the interface) between the antiferromagnetic layer 2 and the layer consisting of a to evoke the pinned magnetic layer 3 formed on the ferromagnetic layer. Due to the on this Exchange coupling-based magnetic field (exchange coupling field Hex) can determine the magnetization direction of the The exchange-coupled film 10 cannot be easily reversed even when an external magnetic field is applied, thus the Resistance to strong magnetic fields is improved. During the heat treatment to bring about the In the exchange coupling field Hex in the exchange-coupled film 10, interdiffusion of atoms (Pt, Cr, Mn) occurs. and Ir), which are located in the PtCr layer 2c, the first PtMn layer 2b, the IrMn layer 2a and the second PtMn layer 2d of the are contained in antiferromagnetic layer 2.
[0032] The pinned magnetic layer 3 consists of a ferromagnetic CoFe alloy (cobalt-iron alloy). The CoFe alloys exhibit higher coercivity at higher Fe content. The pinned magnetic layer 3 is a Layer that contributes to a spin-valve giant magnetoresistance effect. One direction in which the pinned The direction of magnetization P of the pinned magnetic layer 3 is the direction of the sensitive axis of the magnetic detection element 11. From the point of view of increasing the resistance of the exchange-coupled In some cases, the pinned magnetic layer 3 of the film 10 preferably has a thickness of a strong magnetic field against a strong magnetic field. 12 Å or more and 30 Å or less.
[0033] The layer 4 made of non-magnetic material can, for example, consist of Cu (copper).
[0034] The material and structure of the free magnetic layer 5 are not subject to any restrictions. Examples of the Materials that can be used include CoFe alloys (cobalt-iron alloys) and NiFe alloys. (Nickel-iron alloys). The free magnetic layer 5 can be designed to have a single-layer structure, a has a layered structure or a synthetic ferrimagnetic structure.
[0035] The protective layer 6 can, for example, consist of Ta (tantalum). <Zweite Ausführungsform>
[0036] Fig. 3 shows the layer structure of a magnetic detection element 21 with an exchange-coupled film 20 according to a second embodiment of the present invention. In this embodiment, the layers are composed of the same functions as those of the magnetic detection element 11 shown in Fig. 2 with the same Reference symbols are used, and redundant descriptions are not repeated.
[0037] In the magnetic detection element 21 according to the second embodiment, the exchange-coupled film 20, the pinned magnetic layer 3 with a self-pinned structure, and the antiferromagnetic layer 2, which are interconnected. The magnetic detection element 21 distinguishes differs from the magnetic detection element 11 shown in Fig. 2 in that layer 4 consists of non-magnetic material and the free magnetic layer 5 are located closer to the substrate SB than the pinned layer Magnetic layer 3 (which is referred to as the top-side type).
[0038] The magnetic detection element 21 is also a multi-layered element which has a The so-called giant magnetoresistance effect of the single-spin valve type is used. The electrical resistance the same varies depending on the relative relationship between the vector of a first magnetic layer 3A of the pinned magnetic layer 3 and the magnetization vector of the free magnetic layer 5, which depends on a The external magnetic field varies.
[0039] The pinned magnetic layer 3 has a self-pinned structure comprising the first magnetic layer 3A and a second Magnetic layer 3C comprises a non-magnetic intermediate layer 3B provided between these two layers. The pinned magnetization direction P1 of the first magnetic layer 3A is antiparallel to the magnetic field due to the interaction. the pinned magnetization direction P2 of the second magnetic layer 3C. The pinned magnetization direction P1 of the The first magnetic layer 3A, adjacent to layer 4 made of non-magnetic material, is the pinned Magnetization direction of the pinned magnet Layer 3. One direction in which the pinned magnetization direction P1 runs is the direction of the sensitive axis. of the magnetic detection element 11.
[0040] The first magnetic layer 3A and the second magnetic layer 3C consist of an FeCo alloy (iron-cobalt- Alloy). The FeCo alloy has a higher coercivity at a higher Fe content. The first magnetic layer 3A Adjacent to layer 4, which is made of non-magnetic material, is a layer that forms a spin-valve. contributes to the giant magnetoresistance effect.
[0041] The non-magnetic intermediate layer 3B consists, for example, of Ru (ruthenium). The non-magnetic Intermediate layer 3B made of Ru preferably has a thickness of 3 to 5 Å or 8 to 10 Å.
[0042] In the case where an alloy layer, such as the PtCr layer 2c, is used in the production of the exchange-coupled Films 10 are deposited, the different types of metals that make up the alloy (Pt and Cr in the In the case of the PtCr layer 2c), they can be supplied simultaneously. Alternatively, the different types of metals that are in the The alloy components are supplied alternately. A specific example of the former is the simultaneous Sputtering of the different types of metals that make up the alloy. A specific example of the latter is the alternating stacking of different metal films. In some cases, the simultaneous feeding of the different It is preferable to use different types of metals to make up the alloy, rather than alternating the supply, in order to achieve certain results. In some cases, a higher hex value is achieved. <Dritte Ausführungsform>
[0043] Fig. 17 shows the layer structure of a magnetic detection element 110 with an exchange-coupled film 70 according to a third embodiment of the present invention. In this embodiment, the layers are treated with the same functions as those of the magnetic detection element 11 shown in Fig. 2 with the same Reference symbols are used, and redundant descriptions are not repeated.
[0044] The magnetic detection element 110 and the magnetic detection element 11 shown in Fig. 2 have They have in common that layer 4 is made of non-magnetic material and the free magnetic layer 5 is located further away from the Substrate SB is arranged as the pinned magnetic layer 3 (which is referred to as the bottom type).
[0045] An antiferromagnetic layer 80 has a structure comprising a first PtMn layer 8b, a PtCr layer 8c and includes a second PtMn layer 8d, which are stacked together, with the thickness D3 of the PtCr layer 8c being greater as each of the thickness D2 of the first PtMn layer 8b and the thickness D4 of the second PtMn layer 8d. This structure leads to a particularly strong exchange coupling field Hex and thus enables the ratio (Hex / Hc) of the The exchange coupling field Hex to the coercive force Hc is readily 1 or more. Accordingly, the The exchange-coupled film 70 exhibits excellent resistance to strong magnetic fields. Additionally, the Blocking temperature Tb of the exchange-coupled film 70 according to the third embodiment in some cases tends to be higher than the blocking temperature Tb of the exchange-coupled film 10 according to the first embodiment.
[0046] The second PtMn layer 8d preferably has a thickness D4 of more than 0 Å and less than 60 Å, further preferably 10 Å or more and 50 Å or less, or 15 Å or more and 55 Å or less, particularly preferably 20 Å or more and 50 Å or less. If the thickness D4 of the second PtMn layer 2d is within the range, the The exchange coupling field (Hex) can be improved by increasing the Hex / Hc ratio. The thickness ratio (D3) of the PtCr layer is also relevant. 8c to the thickness D2 of the first PtMn layer 8b is in some cases preferably about 2 to about 10 times in the With regard to improving the exchange coupling field Hex and increasing Hex / Hc. The thickness ratio D3 The thickness D4 of the PtCr layer 8c to the thickness D4 of the second PtMn layer 8d is in some cases preferably about 2 to about 10 times in terms of improving the Hex exchange coupling field and increasing Hex / Hc.
[0047] The PtCr layer 8c preferably has a thickness of 100 Å or more, more preferably 110 Å or more. If the If the PtCr layer 8c has a thickness of 100 Å or more, the exchange coupling field can be increased by hexadecimal values. / Hc can be improved. The upper limit of the thickness of the PtCr layer 8c is, from the point of view of In some cases, production efficiency of 200 Å or less is preferred.
[0048] The antiferromagnetic layer 2 preferably has a total thickness of 200 Å or less. Even if the If the antiferromagnetic layer 2 has a total thickness of 200 Å or less, the exchange coupling field Hex can can be improved; thus, the production efficiency of the exchange-coupled film 70 can be improved.
[0049] In the present embodiment, the antiferromagnetic layer 80 is ordered by heat treatment, to establish an exchange coupling (at the interface) between the antiferromagnetic layer 80 and the layer consisting of a to evoke the pinned magnetic layer 3 formed on the ferromagnetic layer. Due to the on this Exchange coupling-based magnetic field (exchange coupling field Hex) can determine the magnetization direction of the The exchange-coupled film 10 cannot be easily reversed even when an external magnetic field is applied, thus the Resistance to strong magnetic fields is improved. During the heat treatment to bring about the In the exchange coupling field Hex in the exchange-coupled film 70, interdiffusion of atoms (Pt, Cr, Mn) occurs. and Ir), which are contained in the layers in the antiferromagnetic layer 80 (the first PtMn layer 8b, the PtCr- are contained in layer 8c and the second PtMn layer 8d).
[0050] As shown in Fig. 18, an exchange-coupled film 71 can be used according to a modification of the present In an embodiment, a Mn-containing layer 8a with a Mn content of more than 50 at% is located between the first PtMn layer. 8b and the pinned magnetic layer 3. The Mn-containing layer 8a may have several stacked layers. The Mn-containing layer 8a may contain at least one layer selected from the group consisting of an IrMn- layer and a Mn layer. In the case where the Mn-containing layer 8a consists of an IrMn layer or a When a stack is formed from an IrMn layer and a Pt-Mn layer, the exchange-coupled film has the same structure. such as the aforementioned exchange-coupled film 10 according to the first embodiment of the present invention. The Mn-containing layer 8a preferably has a thickness of 12 Å or less, more preferably 4 Å or more and 10 Å or less. If the thickness of the IrMn layer 2a is within the range, the exchange coupling field Hex can be under An increase in Hex / HC will improve performance. If the thickness of the Mn-containing layer 8a is within the specified range, then... Furthermore, variations in the thickness of the first PtMn layer 2b have less influence on the exchange coupling field Hex and Hex / Hc.
[0051] Figures 19 and 20 illustrate the layer structures of magnetic detection elements 112 and 113 with top-side-type structures and exchange-coupled films 72 and 73, which have similar structures to the exchange-coupled films 70 and 71 according to the third embodiment and which have the pinned magnetic layer 3 exhibit a self-pinned structure, corresponding to the relationship between the exchange-coupled film 10 according to the first embodiment and the exchange-coupled film 20 according to the second embodiment. <Konfiguration des Magnetsensors>
[0052] Fig. 4 shows a magnetic sensor (magnetism detection device) 30, in which the features shown in Fig. 2 are magnetic detection elements 11 are combined. In Fig. 4, the magnetic detection elements 11 are shown with different pinned magnetization directions P (see Fig. 2) with different reference symbols, i.e. 11Xa, 11Xb, 11Ya and 11Yb, are designated and thus distinguished. In the case of the magnetic sensor 30, the magnetic Detection elements 11Xa, 11Xb, 11Ya and 11Yb arranged on the same substrate.
[0053] The magnetic sensor 30 shown in Fig. 4 has a full bridge circuit 32X and a full bridge circuit 32Y. The full bridge circuit 32X includes two magnetic sensing elements 11Xa and two magnetic Detection elements 11Xb. The full bridge circuit 32Y includes two magnetic detection elements 11Ya and two Magnetic detection elements 11Yb. Each of the magnetic detection elements 11Xa, 11Xb, 11Ya and 11Yb has the Layer structure of the exchange-coupled film 10 of the magnetic detection element 11 shown in Fig. 4. Unless otherwise specifically distinguished below, these may be referred to as "magnetic". Designated as recording element 11''.
[0054] The full bridge circuits 32X and 32Y include the magnetic detection elements 11, which have different exhibit pinned magnetization directions, which are represented by the arrows in Fig. 4, to indicate different They detect magnetization directions and possess the same mechanism for detecting a magnetic field. Accordingly, the mechanism for detecting a magnetic field uses the 32X full bridge circuit. described below.
[0055] The full bridge circuit 32X comprises a first serial section 32Xa and a second serial section 32Xb, which are connected in parallel. The first serial section 32Xa includes the magnetic detection element 11Xa and the Magnetic detection elements 11Xb, connected in series. The second serial section 32Xb includes the magnetic detection element 11Xb and magnetic detection element 11Xa, which are connected in series.
[0056] A power supply voltage Vdd is applied to a power supply terminal 33, which corresponds to the one described in the first serial section 32Xa containing the magnetic detection element 11Xa and the one in the second serial section 32Xb contains a magnetic detection element 11Xb. A ground connection 34, which corresponds to the one in the first serial section 32Xa containing the magnetic detection element 11Xb and the one in the second serial section The magnetic detection element 11Xa contained in 32Xb is set to ground potential GND.
[0057] In the full bridge circuit 32X, the output difference (OutX1) - (OutX2) between the output potential (OutX1) at the midpoint 35Xa of the first serial section 32Xa and the output potential (OutX2) at the Midpoint 35Xb of the second serial section 32Xb as detection output (detection output voltage) VXs in the X- Get directions.
[0058] The full bridge circuit 32Y operates similarly to the full bridge circuit 32X; thus, the output difference (OutY1) - (OutY2) between the output potential (OutY1) at the midpoint 35Ya of a first serial section 32Ya and the output potential (OutY2) at the midpoint 35Yb of a second serial section 32Yb as Detection output (detection output voltage) VYs in the Y direction are obtained.
[0059] As shown by the arrows in Fig. 4, the direction of the sensitive axis of each of the in the Full bridge circuit 32X containing magnetic sensing elements 11Xa and 11Xb perpendicular to the direction of the sensitive axis of each of the magnetic sensing elements 11Ya contained in the full bridge circuit 32Y and 11Yb.
[0060] In the magnetic sensor 30 shown in Fig. 4, the orientation of the free magnetic layer 5 changes every magnetic detection element 11 such that it follows the direction of an external magnetic field H. The Resistance based on the vector relationship between the pinned magnetization direction P of the pinned Magnetic layer 3 and the magnetization direction of the free magnetic layer 5.
[0061] For example, if the external magnetic field H acts in the direction shown in Fig. 4, the electrical The resistance of the magnetic sensing element 11Xa contained in the full bridge circuit 32X is due to the direction the sensitive axis coincides with the direction of the external magnetic field H. In contrast, the electrical resistance of the magnetic sensing element 11Xb because the direction of the sensitive axis is towards the The direction of the external magnetic field H is opposite. The change in electrical resistance maximizes the The detection output voltage VXs = (OutX1) - (OutX2). The detection output voltage VXs decreases as the voltage changes. the external magnetic field H changes to the right with respect to the plane of the paper. When the external magnetic field H in With reference to the paper plane of Fig. 3, directed upwards or downwards, the detection output voltage VXs Zero.
[0062] In the full bridge circuit 32Y, the magnetization direction of the free magnetic layer 5 of each magnetic Detection element 11 perpendicular to the direction of the sensitive axis (pinned magnetization direction P), when the external magnetic field H is directed to the left with respect to the plane of the paper, as shown in Fig. 4; thus The magnetic detection elements 11Ya and 11Xb have an identical electrical resistance. Accordingly, The detection output voltage VYs is zero. When the external magnetic field H is applied relative to the plane of the paper in Fig. 4 The downward effect maximizes the detection output voltage VYs = (OutY1) - (OutY2) of the full bridge circuit 32Y. The detection output voltage VYs decreases to the extent that the direction of the external magnetic field H changes. The reference to the paper plane changes upwards.
[0063] As described above, the detection output voltages VXs and VYs of the full bridge circuits vary. 32X and 32Y when the direction of the external magnetic field H changes. Accordingly, the Direction of movement and the distance of movement (relative position) of a detection target based on the detection output voltages VXs and VYs, which are detected by the full bridge circuits 32X and 32Y will be received.
[0064] Fig. 4 illustrates the magnetic sensor 30, which is designed to generate a magnetic field in the X direction. and can detect the Y-direction, which is perpendicular to the X-direction. However, the magnetic sensor 30 can only detect the The full bridge circuit 32X or the full bridge circuit 32Y include a magnetic field only in the X direction or the Y-direction detected.
[0065] Fig. 5 illustrates the planar structure of each of the magnetic detection elements 11Xa and 11Xb. In the Figures 4 and 5 illustrate BXa-BXb, the X-direction. In (A) and (B) of Figure 5, the pinned Magnetization directions P of the magnetic detection elements 11Xa and 11Xb are shown by arrows. In the The pinned magnetization directions P of the magnetic detection elements 11Xa and 11Xb are the X- Direction, and they are opposite to each other.
[0066] As shown in Fig. 5, the magnetic detection elements 11Xa and 11Xb each have strip-shaped Element sections 12. The longitudinal direction of each element section 12 is directed in the BYa-BYb direction. The several Element sections 12 are arranged parallel to each other. The right end regions of adjacent The element sections 12 in the figure are connected to each other by means of conductive areas 13a. The left end areas Adjacent element sections 12 in the figure are connected to each other by means of conductive areas 13b The conductive areas 13a and 13b are connected alternately to the right and left end regions of the Element sections 12 are connected. The element sections 12 are connected to each other in a so-called meandering shape. coupled. In the magnetic detection elements 11Xa and 11Xb, the conductive area 13a, which is located in the lower The right-hand section shown in the figure is connected to a connection terminal 14a. The conductive area 13b, The one shown in the upper left section of the figure is connected to a connection port 14b.
[0067] Each of the element sections 12 is formed from several metal layers (alloy layers) that are stacked. Fig. 2 shows the multilayer structure of element section 12. Element section 12 can be a structure shown in Fig. 3. exhibit a multi-layered structure.
[0068] In the magnetic sensor 30 shown in Fig. 4 and Fig. 5, the magnetic detection element 11 can be replaced by the magnetic detection element 21 is replaced according to the second embodiment shown in 3.
[0069] The embodiments explained so far are described to aid in understanding the present invention. facilitate and are not intended to limit the present invention. It is therefore intended that the following should be made easier: The elements disclosed in the foregoing embodiments include all design changes and equivalents that are described in the technical scope of the present invention falls. For example, in the aforementioned exchange-coupled film, the IrMn layer 2a is in contact with the pinned magnetic layer 3, in other words, the IrMn- Layer 2a is stacked directly onto the pinned magnetic layer 3. Another layer containing Mn (examples of this) (include a Mn layer and a PtMn layer), can be placed between the IrMn layer 2a and the pinned magnetic layer 3 be stacked. Additionally, in the exchange-coupled film according to the present invention, the ferromagnetic The layer in contact with the antiferromagnetic layer is not limited to the pinned magnetic layer. For example The exchange-coupled film according to the present invention can have an antiferromagnetic layer and a have a ferromagnetic layer that is contained in at least part of a free magnetic layer. In the In the above description, the element with giant magnetoresistance (GMR) is exemplified as the magnetic The detection element is shown, which comprises the exchange-coupled film according to the present invention. magnetic detection element comprising the exchange-coupled film according to the present invention, can However, it could also be an element with a tunnel magnetoresistance effect. EXAMPLES
[0070] The present invention will now be described in more detail with reference to examples and the like. described, however, the scope of the present invention is not limited to these examples and the like. (Examples 1 to 7 and comparative examples 1 to 10-2)
[0071] Multilayer stacks 22 with a layer structure described below (see Fig. 6) were used for the purpose of Evaluation of the properties of exchange-coupled films 40 produced. In the following examples and In comparative examples, the values in parentheses indicate the thickness (Å). Each of the multilayer stacks 22 was subjected to a heat treatment at 350 °C for 20 hours in a magnetic field of 15 kOe to change the magnetization of the pinned magnetic layer 3 formed from a ferromagnetic layer and the antiferromagnetic layer 2 fix or pin, thereby creating the multilayer stack 22 which contains the exchange-coupled film 40.
[0072] Substrate SB: Silicon substrate with aluminum oxide layer formed on the surface / Sublayer 1: NiFeCr (42) / Layer 4 made of non-magnetic material: [Cu (30) / Ru (20)] / pinned magnetic layer 3: Co Fe (18,5) / 40 At.-% 60 At.-% antiferromagnetic layer 2 [IrMn layer 2a: Ir Mn (d1) / first PtMn layer 2b: Pt Mn (d2) / 22At, -% 78At.-% 50At.-% 50At. -% PtCr layer 2c: Pt Cr (d3) / second PtMn layer 2d: Pt Mn (d4)] / protective layer 6: Ta (100). 51At.-% 49At.-% 50At.-% 50At.-%
[0073] The IrMn layers 2a had different thicknesses d1 in the range of 0 Å to 8 Å. The first PtMn layers 2b They had different thicknesses d2 in the range of 0 Å to 300 Å. The PtCr layers 2c had different thicknesses d3 in The second PtMn layers (2d) had different thicknesses D1 in the range of 0 Å to 300 Å. Tables 1 and 2 illustrate d1 to d4 and the thickness (total thickness) of the entire antiferromagnetic layer. 2 in each of the examples and comparison examples. [Table 1] thickness of the antiferromagnetic layer (Å) Hc (Oe) Hex (Oe) Hex / Hc d1 d2 d3 d4 Total thickness Comparative example 1 0 300 0 0 300 965 812 0.84 Comparative example 2 0 0 0 180 180 1008 700 0.69 Comparative example 3 0 0 300 0 300 529 341 0.64 Comparative example 4 8 12 300 320 800 848 1.06 Comparative example 5 240 260 812 879 1.08 Comparative example 6 200 220 825 901 1.09 Comparative example 7 160 180 683 590 0.86 Comparative example 8 120 140 476 50 0.10 Example 1 8 12 120 40 180 892 1102 1.24 [Table 2] Hc Hex Hex / He (Oe) (Oe) thickness of the antiferromagnetic layer (Å) In total- d1 d2 d3 d4 thickness Comparative example 7 8 12 160 0 180 683 590 0.86 Example 7 150 10 685 615 0.90 Example 2 140 20 798 913 1.14 Example 3 130 30 872 1238 1.42 Example 1 120 40 892 1102 1.24 Example 4 100 60 889 685 0.77 Example 5 80 80 840 608 0.72 Example 6 40 120 871 657 0.75 Comparative example 10- 10,150,920,470 0.51 1 Comparative example 10- 5,155,900,460 0.51 2 Comparative example 9 0 160 835 495 0.59
[0074] The magnetization curves of the exchange-coupled films 40 according to the examples and the comparative examples were measured using a vibrating probe magnetometer (VSM). The exchange coupling fields Hex (unit: Oe), which Coercive forces Hc (unit: Oe) and the ratios (Hex / Hc) of the exchange coupling fields Hex to the coercive forces Hc The values were determined from the resulting hysteresis loops. Tables 1 and 2 illustrate the results.
[0075] Fig. 7 is based on the results presented in Table 1 and shows a graphical representation illustrating the Dependence of the exchange coupling field Hex on the thickness (total thickness) of the antiferromagnetic layer 2 Figure 8 is based on the results presented in Table 1 and shows a graphical representation illustrating the Dependence of the ratio (Hex / Hc) of the exchange coupling field Hex to the coercive force Hc on the thickness (Total thickness) of the antiferromagnetic layer 2 illustrated. As shown in Table 1 and Figures 7 and 8. As can be seen, the exchange-coupled film 40 containing the antiferromagnetic layer 2 had the Structure according to Example 1, the exchange coupling field Hex itself at a total thickness of 200 Å or less, a Value of up to 1000 Oe or more, and Hex / Hc was greater than 1. Accordingly, a magnetic Detection element (for example, a magnetoresistive element) that detects the exchange-coupled film according to Example 1 includes excellent performance even in high-temperature environments or environments with strong magnetic fields. exhibit magnetic properties.
[0076] In contrast, in the case of the PtMn layer (Comparison Examples 1 and 2) or the PtCr layer (Comparative example 3) formed antiferromagnetic layer the exchange coupling field Hex compared to the Coercivity Hc was relatively low and Hex / Hc was less than 1.
[0077] In the case where the IrMn layer 2a, the first PtMn layer 2b and the PtCr layer 2c were stacked and the Since the second PtMn layer 2d was not deposited (comparative examples 4 to 8), a smaller thickness of the PtCr layer resulted. Layer 2c tended to be in a lower exchange coupling field Hex, and Hex / Hc was approximately 1.0 or less.
[0078] Fig. 9 is based on the results presented in Table 2 and shows a graphical representation illustrating the Dependence of the exchange coupling field Hex on the thickness d4 of the second PtMn layer 2d illustrated. Fig. 10 based on the results shown in Table 2, it presents a graphical representation illustrating the dependence of Ratio (Hex / Hc) of the exchange coupling field Hex to the coercive force Hc of the thickness d4 of the second PtMn layer 2d illustrated. Table 2 and Figures 9 and 10 clearly showed that in the case where the second PtMn- Layer 2d had a thickness d4 of more than 0 Å and less than 60 Å, in the case where the second PtMn layer 2d preferably had a thickness d4 of more than 10 Å and less than 60 Å, in the case where the second Pt-Mn layer 2d in a further preferred manner had a thickness d4 of 15 Å or more and 55 Å or less, or in the case where the second PtMn layer 2d in a particularly preferred thickness d4 of 20 Å or more and 50 Å or less (Examples 1 up to 3), the exchange coupling field Hex and Hex / Hc were significantly increased, compared to the case where the first PtMn layer 2b and PtCr layer 2c were stacked, and the second PtMn layer 2d was not deposited. (Comparative example 7). With a thickness d4 of the second PtMn layer 2d of 60 Å or more (Examples 4 to 6), the Results showed that the exchange coupling field Hex was increased compared to the case where the antiferromagnetic Layer 2 had an identical thickness (total thickness), but did not have a second PtMn layer 2d (comparative example 7), or compared to the case where the antiferromagnetic layer 2 had an identical thickness (total thickness), but the possessed a multilayer structure consisting of the IrMn layer and the Pt-Mn layer (comparative example 9). (Examples 11 to 15 and comparative examples 11 to 15)
[0079] Multilayer stacks 22 and 221 with the layer structures described below (see Fig. 6 and Fig. 21) were Produced to evaluate the properties of the exchange-coupled films 40 and 74. The following examples In comparative examples, the values in parentheses represent the thickness (Å). The multilayer stack 22 was subjected to a heat treatment at 350 °C for 20 hours in a magnetic field of 10 kOe to change the magnetization of the pinned magnetic layer 3 formed from a ferromagnetic layer and the antiferromagnetic layer 2 pinning, thereby creating the multilayer stack 22 with the exchange-coupled film 40.
[0080] Substrate SB: Silicon substrate with aluminum oxide layer formed on the surface / Sublayer 1: NiFeCr (42) / Layer 4 made of non-magnetic material: [Cu (30) / Ru (20)] / pinned magnetic layer 3: Co Fe (100) / 40 At.-% 60 At.-% antiferromagnetic layer 2 [IrMn layer 2a: Ir22 Mn (d1) / first PtMn layer 2b: Pt Mn (d2) / At.-% 78At.-% 50At.-% 50At.-% PtCr layer 2c: Pt Cr (d3) / second PtMn layer 2d: Pt Mn (d4)] / protective layer 6: [Ru (20) / Ta 51At.-% 49At.-% 50At.-% 50At.-% (100)].
[0081] The IrMn layers 2a had different thicknesses d1 in the range of 0 Å to 80 Å. The first PtMn layers 2b They had different thicknesses d2 in the range of 0 Å to 300 Å. The PtCr layers 2c had different thicknesses d3 in The thickness ranged from 0 Å to 250 Å. The second PtMn layers 2d had different thicknesses d4 in the range of 0 Å to 30 Å. Table 3 illustrates d1 to d4 and the thickness (total thickness) of the entire antiferromagnetic layer 2 in each Examples and comparative examples. [Table 3] Thickness of the antiferromagnetic layer (Å) Hex (Oe) Hc (Oe) Hex / Hc d1 d2 d3 d4 Total thickness Comparative example 11 0 0 180 0 180 46 162 0.29 Comparative example 12 0 20 160 180 116 354 0.33 Comparative example 13 8 12 160 180 139 217 0.64 Comparative example 14 0 300 0 300 140 166 0.84 Comparative example 15 80 0 0 80 114 143 0.80 Example 11 8 12 110 30 160 184 215 0.85 Example 12 130 180 227 190 1.19 Example 13 150 200 259 185 1.40 Example 14 250 300 263 139 1.90 Example 15 0 20 250 30 300 363 377 0.96
[0082] The magnetization curves of the exchange-coupled films 40 according to the examples and the comparative examples were measured using a vibrating probe magnetometer (VSM). The exchange coupling fields Hex (unit: Oe), which Coercive forces Hc (unit: Oe) and the ratios (Hex / Hc) of the out Exchange coupling fields Hex to the coercive forces Hc were determined from the resulting hysteresis loops. Table Figure 3 illustrates the results.
[0083] Fig. 11 is based on the results presented in Table 3 and shows a graphical representation illustrating the Dependence of the exchange coupling field Hex on the thickness (total thickness) of the antiferromagnetic layer 2 Figure 12 illustrates this. It is based on the results presented in Table 3 and shows a graphical representation that illustrates the Dependence of the ratio (Hex / Hc) of the exchange coupling field Hex to the coercive force Hc on the thickness (Total thickness) of the antiferromagnetic layer 2 illustrated. As shown in Table 3 and Figures 11 and 12. As can be seen, the exchange coupling fields Hex of the exchange-coupled films 40 were with the antiferromagnetic Layers 2 with the structures according to examples 11 to 14 are larger than those of the exchange-coupled films 40 with the antiferromagnetic layers 2 with the structures according to comparison examples 11 to 14. Comparisons of the Examples 11 to 14 showed that a greater thickness d3 of the PtCr layer 2c leads to a higher exchange coupling field Hex and higher hex / HC, and that in the exchange-coupled films 40 with the antiferromagnetic layers 2 with the structures according to examples 12 to 14 Hex / Hc was greater than 1. Accordingly, magnetic Detection elements (for example, magnetoresistive elements) with the exchange-coupled films according to the Examples 11 to 14 act as sensors in a suitable manner, even in an environment with a strong Magnetic field, so that in other words they are resistant to strong magnetic fields. More specifically, they possess magnetic detection elements with the exchange-coupled films according to examples 12 to 14 excellent resistance to strong magnetic fields, as the magnetization directions are aligned in the directions are based on the exchange coupling fields Hex when the application of an external magnetic field is lifted becomes.
[0084] The magnetization curves of the exchange-coupled films 40 according to comparative examples 11 to 15 and the Examples 11 to 15 were tested at different ambient temperatures (unit: °C) using a The exchange coupling fields (Hex, unit: Oe) at the temperatures were measured using a vibrating probe magnetometer (VSM). were determined from the resulting hysteresis loops. Tables 4 to 12 show the exchange coupling fields. Hex at the temperatures and values obtained by normalizing the exchange coupling fields Hex at the temperatures to the exchange coupling field Hex at room temperature (normalized exchange coupling fields with respect to the room temperature). [Table 4] Comparative example 11 Temperature (°C) Hex (Oe) Normalized Hex 25 48 1.00 50 48 0.99 80 47 0.97 110 47 0.97 140 46 0.96 170 45 0.93 200 43 0.89 230 42 0.87 260 40 0.83 290 37 0.76 320 30 0.62 350 25 0.52 380 20 0.41 410 13 0.27 440 10 0.21 470 3 0.06 500 0 0.00 [Table 5] Comparative example 12 Temperature (°C) Hex (Oe) Normalized Hex 25 98 1.00 50 96 0.98 80 90 0.92 110 84 0.85 140 82 0.83 170 75 0.76 200 72 0.73 230 63 0.64 260 57 0.58 290 50 0.51 320 40 0.41 350 36 0.37 380 29 0.29 410 20 0.20 440 10 0.10 470 3 0.03 500 0 0.00 [Table 6] Comparative example 13 Temperature (°C) Hex (Oe) Normalized Hex 25 135 1.00 50 125 0.93 80 124 0.92 110 118 0.88 140 113 0.84 170 109 0.81 200 101 0.75 230 97 0.72 260 87 0.65 290 78 0.58 320 64 0.48 350 40 0.30 380 27 0.20 410 9 0.07 440 0 0.00 [Table 7] Comparative example 14 Temperature (°C) Hex (Oe) Normalized Hex 22 140 1.00 44 140 1.00 65 139 0.99 85 137 0.98 105 136 0.97 125 135 0.96 145 134 0.96 165 129 0.92 185 124 0.88 204 116 0.83 224 106 0.76 268 72 0.52 306 34 0.24 323 16 0.11 342 8 0.06 362 3 0.02 380 0 0.00 [Table 8] Comparative example 15 Temperature (°C) Hex (Oe) Normalized Hex 22 114 1.00 42 110 0.97 64 104 0.91 84 96 0.85 105 90 0.79 125 82 0.72 144 74 0.65 165 66 0.58 185 56 0.49 205 39 0.34 224 22 0.20 244 6 0.05 264 0 0.00 [Table 9] Example 11 Temperature (°C) Hex (Oe) Normalized Hex 25 187 1.00 50 180 0.96 80 169 0.91 110 163 0.87 140 156 0.83 170 151 0.81 200 143 0.77 230 138 0.74 260 120 0.64 290 107 0.57 320 83 0.44 350 52 0.28 380 22 0.12 410 4 0.02 440 0 0 [Table 10] Example 12 Temperature (°C) Hex (Oe) Normalized Hex 25 225 1.00 50 225 1.00 80 218 0.97 110 214 0.95 140 207 0.92 170 199 0.88 200 190 0.84 230 187 0.83 260 180 0.80 290 149 0.66 320 98 0.44 350 67 0.30 380 31 0.14 410 7 0.03 440 0 0.00 [Table 11] Example 13 Temperature (°C) Hex (Oe) Normalized Hex 23 253 1.00 50 250 0.99 80 239 0.94 110 235 0.93 140 238 0.94 170 217 0.86 200 217 0.86 230 200 0.79 260 195 0.77 290 175 0.69 320 127 0.50 350 77 0.30 380 37 0.15 410 8 0.03 440 0 0.00 [Table 12] Example 14 Example 15 Temperature (°C) Hex (Oe) Normalized Hex Temperature (°C) Hex (Oe) Normalized Hex 23,282 1.00 23,360 1.00 50 279 0.99 50 353 0.98 80 263 0.93 80 351 0.98 110 265 0.94 110 344 0.96 140 262 0.93 140 333 0.93 170 257 0.91 170 314 0.87 200 248 0.88 200 298 0.83 230 236 0.84 230 290 0.81 260 223 0.79 260 266 0.74 290 198 0.70 290 244 0.68 320 148 0.52 320 216 0.60 350 75 0.27 350 198 0.55 380 30 0.11 380 167 0.46 410 8 0.03 410 145 0.40 440 0 0.00 440 106 0.29 470 66 0.18 500 22 0.06
[0085] The blocking temperatures Tb (unit: °C) in these examples were determined based on the values in Tables 4 to 12. The results shown were determined. Table 13 shows the results. As shown in Table 13, the exchange-coupled films 40 with the IrMn layers 2a, which served as Mn-containing layers (Examples 11 to 14), a Blocking temperature Tb of 410 °C. The exchange-coupled film 74 without a Mn-containing layer (exchange-coupled film) 74 (according to Example 15) had a blocking temperature Tb of 510 °C. Accordingly, it was suggested that it was preferentially It may be possible to use the exchange-coupled film 40 without a Mn-containing layer. [Table 13] Tb (°C) Comparative example 11,470 Comparative example 12,470 Comparative example 13,410 Comparative example 14 362 Comparative example 15 244 Example 11,410 Example 12 410 Example 13,410 Example 14 410 Example 15 510
[0086] Fig. 13 shows a graphical representation illustrating the dependence of the exchange coupling fields Hex of the exchange-coupled films 40 according to comparison examples 11 to 13 and example 12 from the measurement temperature Figure 14 illustrates the dependence of the normalized values. Exchange coupling fields Hex in relation to the room temperature of the exchange-coupled films 40 according to the Comparison examples 11 to 13 and example 12 illustrate the measured temperature. Fig. 15 shows a graphical representation. Representation showing the dependency of the exchange coupling fields Hex of the exchange-coupled films 40 according to the The comparison examples 14 and 15 and examples 11 to 14 illustrate the measured temperature. Fig. 16 shows a graphical representation showing the dependence of the normalized exchange coupling fields (Hex) on the Room temperature of the exchange-coupled films 40 according to comparison examples 14 and 15 and examples 11 to 14 illustrated.
[0087] Figures 13 and 14 show comparisons with a total thickness of the antiferromagnetic layer 2 of 180 Å. carried out: the case in which the antiferromagnetic layer 2 consists only of the PtCr layer (comparative example 11), the case in which an area of the PtCr layer adjacent to the pinned magnetic layer 3 is replaced by the PtMn layer (Comparative Example 12), in comparison to Comparative Example 11, the case in which a region of the PtMn layer is adjacent to the the pinned magnetic layer 3 is replaced by the IrMn layer (comparative example 13), compared to comparative example 12, as well as the case in which an area of the PtCr layer adjacent to the protective layer 6 is covered by the PtMn layer (Example 12) is replaced, compared to comparison example 13. In comparison example 11, the exchange coupling field was Hex 50. Oe or less. Replacing the region of the PtCr layer adjacent to the pinned magnetic layer 3 with the Pt-Mn- The layer enabled the improvement of the exchange coupling field Hex to approximately 100 Oe or less (comparative example). 12). Furthermore, replacing the area of the PtMn layer adjacent to the pinned magnetic layer enabled 3 The IrMn layer improves the exchange coupling field Hex to approximately 150 Oe or less. (Comparative example 13). However, the blocking temperature Tb of the exchange-coupled film 40 decreased by about 50 °C. Additionally, replacing the area of the PtCr layer adjacent to the protective layer 6 with the PtMn layer made it possible the improvement of the exchange coupling field Hex to about 200 Oe (Example 12).
[0088] Figures 15 and 16 show comparisons between the antiferromagnetic layers 2 and the structures carried out according to the examples and cases in which only one between the PtCr layer and the pinned The film located in magnetic layer 3 forms the respective antiferromagnetic layer 2. More specifically, in the In comparative example 14, the antiferromagnetic layer 2 is formed from the PtMn layer. In comparative example 15, the The antiferromagnetic layer 2 is formed from the IrMn layer. As shown in As can be seen particularly clearly in Fig. 16, the blocking temperatures Tb of the exchange-coupled films were 40 according to In the examples, regardless of the thickness of the PtCr layers, the temperature is approximately 410 °C. The blocking temperature Tb of the exchange-coupled film 40 including any antiferromagnetic layer consisting of the PtMn layer Layer 2, including the antiferromagnetic layer 2 consisting of the IrMn layer, was lower than the Blocking temperatures Tb of the exchange-coupled films 40 according to the examples. Accordingly, the exchange-coupled film according to the present invention compared to exchange-coupled films according to the The relevant state of the art functions stably in a high-temperature environment. The blocking temperature Tb of the The temperature of the exchange-coupled film 74 according to Example 15 is higher than the blocking temperature Tb of the exchange-coupled film. 40; therefore, the exchange-coupled film 74 according to Example 15 should be used in a particularly harsh high-temperature environment function properly. (Example 21)
[0089] A multilayer stack 221 with a layer structure described below (see Fig. 21) was produced, to evaluate the properties of the exchange-coupled film 74. In the following examples and In comparative examples, the values in parentheses represent the thickness (Å). The multilayer stack 221 was one Heat treatment at 350 °C for 20 hours in a magnetic field of 15 kOe to alter the magnetization of the a ferromagnetic layer and an antiferromagnetic layer 84 formed pinned magnetic layer 3 to pinning, thereby creating the multilayer stack 221 containing the exchange-coupled film 74.
[0090] Substrate SB: Silicon substrate with aluminum oxide layer formed on the surface / Sublayer 1: NiFeCr (42) / Layer 4 made of non-magnetic material: [Cu (30) / Ru (10)] / pinned magnetic layer 3: Co Fe (18) / 40 At.-% 60 At.-% antiferromagnetic layer 84 [first PtMn layer 8b: Pt Mn (16) / PtCr layer 8c: Pt Cr (130) / 50At-% 50At.-% 51At.-% 49At.-% second PtMn layer 8d: Pt Mn (30)] / protective layer 6: Ta (100). 50At-% 50At.-% (Examples 22 to 26)
[0091] Multilayer stacks 22 with a layer structure described below (see Fig. 6) were used for the purpose of Evaluation of the properties of the exchange-coupled film 40 was carried out. In the following examples and In comparative examples, the values in parentheses represent the thickness (Å). Each of the multilayer stacks 22 was subjected to a heat treatment at 350 °C for 20 hours in a magnetic field of 15 kOe to change the magnetization of the pinned magnetic layer 3 formed from a ferromagnetic layer and the antiferromagnetic layer 2 pinning, thereby creating the multilayer stack 22 containing the exchange-coupled film 40.
[0092] Substrate SB: Silicon substrate with aluminum oxide layer formed on the surface / Sublayer 1: NiFeCr (42) / Layer 4 made of non-magnetic material: [Cu (30) / Ru (10)] / pinned magnetic layer 3: Co Fe (18) / 40 At.-% 60 At.-% antiferromagnetic layer 2 [IrMn layer 2a: Ir Mn (d1) / first PtMn layer 2b: Pt Mn (16) / 20At.-% 80At.-% 50At.-% 50At.-% PtCr layer 2c: Pt Cr (130) / second PtMn layer 2d: Pt Mn (30)] / protective layer 6: Ta (100). 51At.-% 49At.-% 50At.-% 50At.-%
[0093] The IrMn layers 2a had different thicknesses d1 in the range of 2 Å to 10 Å. Table 14 illustrates d1 in each of the examples. [Table 14] thickness of the antiferromagnetic Hex (Oe) Hc (Oe) Hex / Hc Layer (Å) Mn layer or PtCr- Second PtMn- First PtMn layer total IrMn layer layer layer Example 21 IrMn layer 0 16 130 30 176 1950 1550 1.26 Example 22 2 178 2350 1350 1.74 Example 23 4 180 2,000 1,100 1.82 Example 24 6 182 1,800 1,000 1.80 Example 25 8 184 1,450 850 1.71 Example 26 10 186 1,315 865 1.52 Example 21 Mn layer 0 176 1950 1550 1.26 Example 27 2 178 2450 1750 1.40 Example 28 4 180 2,250 1,700 1.32 Example 29 6 182 2,000 1,550 1.29 Example 30 8 184 1,900 1,400 1.36 Example 31 10 186 1.725 1.125 1.53 (Examples 27 to 31)
[0094] Multilayer stacks 222 with a layer structure described below (see Fig. 22) were developed for the purpose of Evaluation of the properties of exchange-coupled films 75 produced. In the following examples and In comparative examples, the values in parentheses represent the thickness (Å). The multilayer stack 222 was one Heat treatment at 350 °C for 20 hours in a magnetic field of 15 kOe to alter the magnetization of the a ferromagnetic layer and an antiferromagnetic layer 85 formed pinned magnetic layer 3 to pinning, thereby creating the multilayer stack 222 containing the exchange-coupled film 75.
[0095] Substrate SB: Silicon substrate with aluminum oxide layer formed on the surface / Sublayer 1: NiFeCr (42) / Layer 4 made of non-magnetic material: [Cu (30) / Ru (10)] / pinned magnetic layer 3: Co Fe . (18) / 40 At.-% 60 At.-% antiferromagnetic layer 85 [Mn layer 8a1: Mn (D1) / first PtMn layer 8b: Pt Mn (16) / PtCr layer 50 At.-% 50 At.-% 8c: Pt Cr (130) / second PtMn layer 8d: Pt Mn (30)] / protective layer 6: Ta (100). 51% atm 49% atm 50% atm 50% atm
[0096] The Mn layers 2a1 had different thicknesses d1 in the range of 2 Å to 10 Å. Table 14 illustrates d1 in each of the examples.
[0097] The magnetization curves of the exchange-coupled films 74, 40 and 75 according to the examples were obtained using a Measurements were taken using a vibrating sample magnetometer (VSM). The exchange coupling fields Hex (unit: Oe) and the coercive forces Hc were measured. (Unit: Oe) and the ratios (Hex / Hc) of the exchange coupling fields Hex to the coercive forces Hc were derived from the The resulting hysteresis loops were determined. Table 14 and Figure 22 illustrate the results.
[0098] As shown in Table 14 and Fig. 22, the exchange-coupled films 74, 40 and 75 had according to the Examples 21 to 31 high exchange coupling fields Hex. For each of the exchange-coupled films 74, 40 and 75 according to In examples 21 to 31, Hex / Hc was greater than 1. Thus, magnetic detection elements (for example, magnetoresistive elements), which include the exchange-coupled films according to Examples 21 to 31, even in a environments with strong magnetic fields exhibit excellent magnetic properties. (Examples 41 to 48 and comparative examples 41 to 47)
[0099] Multilayer stacks 221 with a layer structure described below (see Fig. 21) were developed for the purpose of Evaluation of the properties of exchange-coupled films 74 produced. In the following examples and In comparative examples, the values in parentheses represent the thickness (Å). Each of the multilayer stacks 221 was subjected to a heat treatment at 350 °C for 20 hours in a magnetic field of 10 kOe to change the magnetization of the pinned magnetic layer 3 formed from a ferromagnetic layer and an antiferromagnetic layer 84 pinning, thereby creating the multilayer stack 221 containing the exchange-coupled film 74.
[0100] Substrate SB: Silicon substrate with aluminum oxide layer formed on the surface / Sublayer 1: NiFeCr (42) / Layer 4 made of non-magnetic material: [Cu (30) / Ru (10)] / pinned magnetic layer 3: Co Fe (100) / 90% At 10% At antiferromagnetic layer 84 [first PtMn layer 8b: Pt Mn (D2) / PtCr layer 8c: Pt Cr (D3) / 50At.-% 50At.-% 51At.-% 49At.-% second PtMn layer 8d: Pt Mn (D4)] / protective layer 6: Ta (100). 50 At.-% 50 At.-%
[0101] The thickness D2 of each first PtMn layer 8b was 0 Å or 20 Å. The PtCr layers 8c had different Thickness D3 ranged from 0 Å to 180 Å. The second PtMn layers 8d had varying thicknesses D4 in the range of 0 Å to 160 Å. The total thickness (overall thickness) of each of the antiferromagnetic layers 84 was set to 180 Å. defined. Table 15 illustrates D2, D3, and D4 for each of the examples. [Table 15] Thickness of the antiferromagnetic layer (Å) Hex (Oe) Hc (Oe) Hex / Hc - D2 D3 D4 Total thickness Comparative example 41 0 180 0 180 3 29 0.10 Comparative example 42 150 30 14 38 0.37 Comparative example 43 20 160 0 20 120 0.17 Example 41 150 10 23 123 0.18 Example 42 140 20 215 385 0.56 Example 43 130 30 305 520 0.59 Example 44 120 40 257 523 0.49 Example 45 100 60 120 470 0.26 Example 46 80 80 66 426 0.15 Example 47 60 100 60 365 0.16 Example 48 40 120 60 370 0.16 Comparative example 44 20 140 57 378 0.15 Comparative example 45 10 150 85 375 0.23 Comparative example 46 5 155 98 358 0.27 Comparative example 47 0 160 160 330 0.48
[0102] The magnetization curves of the exchange-coupled films 74 according to the examples were obtained with a Measurements were taken using a vibrating sample magnetometer (VSM). The exchange coupling fields Hex (unit: Oe) and the coercive forces Hc were measured. (Unit: Oe) and the ratios (Hex / Hc) of the exchange coupling fields Hex to the coercive forces Hc were derived from the The resulting hysteresis loops were determined. Table 15 and Figures 24 and 25 illustrate the results.
[0103] As shown in Table 15 and Figures 24 and 25, the exchange-coupled films 74 had according to the Examples 41 to 48 high exchange coupling fields Hex. The Hex / Hc of each of the exchange-coupled films 74 according to the Examples 41 to 48 were higher than in the comparison example 41 (0.10). Furthermore, the results show that in this case, in which the second PtMn layer 8d had a thickness D4 of more than 10 Å and less than 60 Å, in the case where the second PtMn layer 8d preferably one thickness D4 of 15 Å or more and 55 Å or less, or in the case where the second PtMn layer was 8d further preferably had a thickness D4 of 20 Å or more and 50 Å or less (Examples 42 to 44), that The exchange coupling field (Hex and Hex / Hc) was significantly increased. Thus, the magnetic detection elements (for Example magnetoresistive elements), which include the exchange-coupled films 74 according to examples 41 to 48, exhibit excellent magnetic properties even in environments with strong magnetic fields. Compare The comparison between Example 42 and Example 43 showed that in the structure of Example 43, in which the The exchange coupling field Hex and Hex / Hc were remarkably high, the exchange coupling field Hex and the Coercivity force Hc by changing the first PtMn layer 8b, which is adjacent to the pinned magnetic layer 3, to the Pt-Cr layer was significantly reduced. In other words, it was found that the first PtMn layer 8b with a thickness of 20 Å, which is very small compared to the antiferromagnetic layer 84 with a total thickness of 180 Å is, plays a particularly important role in increasing the exchange coupling field Hex and Hex / Hc. (Examples 51 to 56 and comparative examples 51 to 56)
[0104] Multilayer stacks 221 with a layer structure described below (see Fig. 21) were developed for the purpose of Evaluation of the properties of exchange-coupled films 74 produced. In the following examples and In comparative examples, the values in parentheses represent the thickness (Å). Each of the multilayer stacks 221 was subjected to a heat treatment at 350 °C for 20 hours in a magnetic field of 15 kOe to change the magnetization of the pinned magnetic layer 3 formed from a ferromagnetic layer and an antiferromagnetic layer 84 pinning, thereby creating the multilayer stack 221 containing the exchange-coupled film 74.
[0105] Substrate SB: Silicon substrate with aluminum oxide layer formed on the surface / Sublayer 1: NiFeCr (42) / Layer 4 made of non-magnetic material: [Cu (30) / Ru (10)] / pinned magnetic layer 3: Co Fe10 (X) or Co 90At-% At-% 40At. Fe (X) / antiferromagnetic layer 84 [first PtMn layer 8b: Pt Mn (D2) / PtCr layer 8c: Pt -% 60At. -% 50At.-% 50At.-% 51At.-% Cr (D3) / second PtMn layer 8d: Pt Mn (D4)] / protective layer 6: Ta (100). 49% 50% -% 50%
[0106] The thickness D2 of each of the first PtMn layers 8b was 20 Å or 180 Å. The thickness D3 of each of the PtCr layers 8c The thickness D4 of each of the second PtMn layers 8d was 0 Å or 30 Å. The total thickness of each of the antiferromagnetic layers 84 was set at 180 Å. The composition of each of the The pinned magnetic layers 3 were CoFe or CoFe. These had different thicknesses (X) in the 90At.-% 10At.-% 40At.-% 60At.-% -% Range from 18 Å to 100 Å. Table 16 illustrates D2, D3, D4 and X in the examples. [Table 16] thickness of Pinned antiferromagnetic Hex (Oe) Hc (Oe) Hex / Hc Magnetic layer Layer (Å) D2 D3 D4 Total thickness Composition X (Å) comparative example 180 0 0 180 90CoFe 18 1105 755 1.46 51 comparative example 24 930 750 1.24 52 comparative example 100 160 330 0.48 53 comparative example 60FeCo 18 875 925 0.95 54 comparative example 24 660 840 0.79 55 comparative example 100 110 420 0.26 56 Example 51 20 130 30 90CoFe 18 2650 1420 1.87 Example 52 24 2090 1380 1.51 Example 53 100 305 520 0.59 Example 54 60FeCo 18 2050 1530 1.34 Example 55 24 1420 1540 0.92 Example 56 100 190 470 0.40
[0107] The magnetization curves of the exchange-coupled films 74 according to the examples were obtained with a Measurements were taken using a vibrating sample magnetometer (VSM). The exchange coupling fields Hex (unit: Oe) and the coercive forces Hc were measured. (Unit: Oe) and the ratios (Hex / Hc) of the exchange coupling fields Hex to the coercive forces Hc were derived from the The resulting hysteresis loops were determined. Table 16 and Figures 26 to 29 illustrate the results.
[0108] As shown in Table 16 and Figures 26 to 29, a smaller thickness of the pinned magnetic layer 3 resulted tending towards a higher exchange coupling field Hex and a higher Hex / Hc, regardless of the Composition of the pinned magnetic layer 3. Thus, magnetic detection elements (for example, magnetoresistive elements), which the exchange-coupled films 74 exhibit according to Examples 51 to 56, even in exhibit excellent magnetic properties in an environment with a strong magnetic field. In particular, where the thickness of the pinned magnetic layer 3 can be small, a higher exchange coupling field Hex and a Higher hex / hc values can be achieved by adjusting the thickness of the pinned magnetic layer 3. (Examples 61 to 78 and comparative examples 61 and 62)
[0109] Multilayer stacks 22 with a layer structure described below (see Fig. 6) were used for the purpose of Evaluation of the properties of exchange-coupled films 40 produced. In the following examples and In comparative examples, the values in parentheses represent the thickness (Å). Each of the multilayer stacks 22 was subjected to a heat treatment at 350 °C for 20 hours in a magnetic field of 15 kOe to change the magnetization of the pinned magnetic layer 3 formed from a ferromagnetic layer and the antiferromagnetic layer 2 pinning, thereby creating the multilayer stack 222 containing the exchange-coupled film 40.
[0110] Substrate SB: Silicon substrate with aluminum oxide layer formed on the surface / Sublayer 1: NiFeCr (42) / Layer 4 made of non-magnetic material: [Cu (30) / Ru (10)] / pinned magnetic layer 3: Co Fe (100) / 90 At.-% 10 At.-% antiferromagnetic layer 2 [IrMn layer 2a: IrMn (8) / first PtMn- 20 At.- % 80 At. %, Layer 2b: Pt Mn (12) / PtCr layer 2c: Pt Cr (d3) / second PtMn layer 2d: Pt Mn 50At.-% 50At.-% 51At.-% 49At.-% 50At.-% 50At.-% (d4)] / Protective layer 6: Ta (100).
[0111] The thickness d3 of each of the PtCr layers 2c was 130 Å or 160 Å. The second Pt-Mn layers 2d had Different thicknesses d4 in the range from 0 Å to 80 Å. Table 17 illustrates d3 and d4 in each of the examples. [Table 17] Thickness of the antiferromagnetic layer (Å) Hex (Oe) Hc (Oe) Hex / Hc d1 d2 d3 d4 Total thickness Comparative example 61 8 12 130 0 150 110 118 0.93 Example 61 10 160 146 137 1.07 Example 62 20 170 288 198 1.45 Example 63 25 175 331 192 1.73 Example 64 30 180 334 182 1.84 Example 65 35 185 319 174 1.84 Example 66 40 190 300 160 1.88 Example 67 50 200 272 160 1.70 Example 68 60 210 264 156 1.69 Example 69 80 230 246 166 1.48 Comparative example 62 8 12 160 0 180 233 188 1.24 Example 70 10 190 228 183 1.25 Example 71 20 195 328 198 1.66 Example 72 25 200 364 226 1.61 Example 73 30 205 361 192 1.88 Example 74 35 210 353 181 1.95 Example 75 40 220 327 178 1.84 Example 76 50 230 305 170 1.79 Example 77 60 240 299 161 1.86 Example 78 80 260 285 153 1.86
[0112] The magnetization curves of the exchange-coupled films 40 according to the examples were obtained with a Measurements were taken using a vibrating sample magnetometer (VSM). The exchange coupling fields Hex (unit: Oe) and the coercive forces Hc were measured. (Unit: Oe) and the ratios (Hex / Hc) of the exchange coupling fields Hex to the coercive forces Hc were derived from the The resulting hysteresis loops were determined. Table 17 and Figures 30 to 33 illustrate the results.
[0113] As shown in Table 17 and Figures 30 and 32, when the second PtMn layer had a thickness of 2d of more than 10 Å and less than 60 Å, the exchange coupling field Hex and Hex / Hc tended to increase, namely regardless of the thickness d3 of the PtCr layer 2c. If the second PtMn layer 2d has a thickness of more than 10 Å and Furthermore, the values of the exchange coupling fields Hex and the values of Hex / Hc were less than 60 Å. The thickness d3 of the PtCr layer 2c of 130 Å is essentially the same as that of a thickness d3 of the PtCr layer 2c of 160 Å. Thus, these results showed that when the second PtMn layer 2d of the exchange-coupled film 40 has a thickness of more than 10 Å and less than 60 Å, variations in the thickness of the PtCr layer 2c had less influence on the had magnetic properties.
[0114] Typically, a greater thickness of the antiferromagnetic layer tends to result in a higher Exchange coupling field Hex and a higher Hex / Hc result. However, as shown in Table 17 and Figures 31 and 33. is shown, in the case where the antiferromagnetic layer 2 of the exchange-coupled film 40 according to each The examples had a high overall thickness, tending to show a thickness range in which the The exchange coupling field Hex and Hex / Hc were particularly high. (Examples 81 to 105 and comparative examples 81 to 83)
[0115] Multilayer stacks 22 and 221 with layer structures described below (see Fig. 6 and Fig. 21) were produced for the purpose of evaluating the properties of the exchange-coupled films 40 and 74. In the following In examples and comparisons, the values in parentheses represent the thickness (Å). The multilayer stack 22 was subjected to heat treatment at 350 °C for 20 hours in a magnetic field of 15 kOe to... Magnetization of the pinned components formed from a ferromagnetic layer and the antiferromagnetic layer 2 to pin magnetic layer 3, thereby forming the multilayer stacks 22 containing the exchange-coupled films 40 and 74 and 221 were produced.
[0116] Substrate SB: Silicon substrate with aluminum oxide layer formed on the surface / Sublayer 1: NiFeCr (42) / Layer 4 made of non-magnetic material: [Cu (30) / Ru (10)] / pinned magnetic layer 3: Co Fe (100) / 90 At,-% 10 At% antiferromagnetic layer 2 [IrMn layer 2a: Ir Mn (d1) / first PtMn layer 2b: Pt Mn (d2) / 20At. -% 80At.-% 50At.-% 50At. -% PtCr layer 2c: Pt Cr (130) / second PtMn layer 2d: Pt Mn (30)] / protective layer 6: Ta (100). 51At.-% 49At.-% 50At.-% 50At.-%
[0117] The IrMn layers 2a had different thicknesses d1 in the range of 0 Å to 20 Å. The first PtMn layers 2b They had different thicknesses d2 in the range of 0 Å to 22 Å. This resulted in the exchange-coupled films 40 with Different overall thicknesses in the range of 180 Å to 186 Å were obtained. Table 18 shows d1, the thickness d2 of the first PtMn- Layer 2b and the total thickness in each of the examples. [Table 18] Thickness of the antiferromagnetic layer (Å) Hex (Oe) Hc (Oe) Hex / Hc - d1 d2 d3 d4 Total thickness Example 81 0 20 130 30 180 305 520 0.59 Example 82 2 18 315 365 0.86 Example 83 4 16 348 323 1.08 Example 84 6 14 353 228 1.55 Example 85 8 12 336 166 2.02 Example 86 10 10 285 150 1.90 Example 87 12 8 202 97 2.09 Comparative example 81 14 6 120 90 1.33 Comparative example 82 16 4 63 68 0.93 Comparative example 83 20 0 24 57 0.42 Example 88 0 22 182 288 543 0.53 Example 89 2 20 304 464 0.66 Example 90 4 18 331 306 1.08 Example 91 6 16 346 229 1.51 Example 92 8 14 336 186 1.81 Example 93 10 12 300 146 2.06 Example 94 0 24 184 249 532 0.47 Example 95 2 22 270 406 0.66 Example 96 4 20 305 295 1.03 Example 97 6 18 334 239 1.40 Example 98 8 16 333 223 1.49 Example 99 10 14 308 156 1.97 Example 100 0 26 186 223 450 0.49 Example 101 2 24 238 413 0.58 Example 102 4 22 298 353 0.84 Example 103 6 20 315 266 1.18 Example 104 8 18 324 204 1.59 Example 105 10 16 306 164 1.87
[0118] The magnetization curves of the exchange-coupled films 40 according to the examples were obtained with a Measurements were taken using a vibrating sample magnetometer (VSM). The exchange coupling fields Hex (unit: Oe) and the coercive forces Hc were measured. (Unit: Oe) and the ratios (Hex / Hc) of the exchange coupling fields Hex to the coercive forces Hc were derived from the The resulting hysteresis loops were determined. Table 18 and Figures 34 to 36 illustrate the results.
[0119] Table 18 and Figures 34 to 36 showed that the exchange coupling field Hex itself under a different The thickness d2 of the first PtMn layer 2b could be kept at a high level as long as the thickness d1 of the IrMn- Layer 2a was in the range of 12 Å or less. In particular, it was determined that states that if the IrMn layer 2a had a thickness of 4 Å or more and 10 Å or less, a high A stable exchange coupling field of Hex and a high Hex / Hc (especially 1.0 or more) could be achieved. In other words, the results showed that in the production of the exchange-coupled film 40, the relatively loose The tolerance of the thickness d2 of the first PtMn layer 2b can be specified. (Examples 111 to 128 and comparative examples 111 to 131)
[0120] Multilayer stacks 22 with a layer structure described below (see Fig. 6) were used for the purpose of Evaluation of the properties of exchange-coupled films 40 produced. In the following examples and In comparative examples, the values in parentheses represent the thickness (Å). Each of the multilayer stacks 22 was subjected to a heat treatment at 350 °C for 20 hours in a magnetic field of 10 kOe to change the magnetization of the pinned magnetic layer 3 formed from a ferromagnetic layer and the antiferromagnetic layer 2 pinning, thereby creating the multilayer stacks 22 having the exchange-coupled film 40.
[0121] Substrate SB: Silicon substrate with aluminum oxide layer formed on the surface / Sublayer 1: NiFeCr (42) / Layer 4 made of non-magnetic material: [Cu (30) / Ru (20)] / pinned magnetic layer 3: Co Fe (100) / 90 At.-% 10 At.-% antiferromagnetic layer 2 [IrMn layer 2a: Ir Mn (d1) / first PtMn layer 2b: Pt Mn (d2) / 22At.-% 78At.-% 50At.-% 50At.-% PtCr layer 2c: Pt Cr (d3) / second PtMn layer 2d: Pt Mn (d4)] / protective layer 6: / Ta (100). 51At-% 49At.-% 50At.-% 50At.-%
[0122] The IrMn layers 2a had different thicknesses d1 in the range of 0 Å to 8 Å. The first PtMn layers 2b They had different thicknesses d2 in the range of 0 Å to 300 Å. The PtCr layers 2c had different thicknesses d3 in The second PtMn layers 2d had different thicknesses d4 in the range of 0 Å to 300 Å. Table 19 illustrates d1 to d4 and the thickness (total thickness) of the entire antiferromagnetic layer 2 in each of the examples and comparative examples. [Table 19] thickness of the antiferromagnetic layer (Å) Hex (Oe) d1 d2 d3 d4 Total thickness Comparative example 111 0 0 300 0 300 10 Comparative example 112 180 180 0 Comparative example 113 120 120 0 Comparative example 114 0 20 280 0 300 349 Comparative example 115 180 200 63 Comparative example 116 160 180 25 Comparative example 117 140 160 0 Comparative example 118 120 140 0 Comparative example 119 100 120 0 Comparative example 120 4 16 280 0 300 368 Comparative example 121 180 200 173 Comparative example 122 160 180 98 Comparative example 123 140 160 48 Comparative example 124 120 140 16 Comparative example 125 100 120 3 Comparative example 127 200 200 210 Comparative example 128 180 180 170 Comparative example 129 160 160 135 Comparative example 130 140 140 100 Comparative example 131 120 120 35 Example 111 0 20 250 30 300 520 Example 112 150 200 365 Example 113 130 180 285 Example 114 110 160 190 Example 115 90 140 93 Example 116 70 120 10 Example 117 4 16 250 30 300 445 Example 118 150 200 384 Example 119 130 180 352 Example 120 110 160 310 Example 121 90 140 239 Example 122 70 120 150 Example 123 8 12 250 30 300 362 Example 124 150 200 346 Example 125 130 180 338 Example 126 110 160 313 Example 127 90 140 275 Example 128 70 120 220
[0123] The magnetization curves of the exchange-coupled films 40 according to the examples and the comparative examples were measured using a vibrational probe magnetometer (VSM). The exchange coupling fields are hex (unit: Oe). were determined from the resulting hysteresis loops. Table 19 and Figure 37 illustrate the results.
[0124] As shown in the results of Examples 111 to 116 in Fig. 37 (black filled circles and a solid line), led in the case where the IrMn layer 2a, serving as the Mn-containing layer, was not provided As is the case with the exchange-coupled film 74, a greater thickness of the antiferromagnetic layer 2 was required. a higher exchange coupling field Hex, and the exchange coupling field Hex was 500 Oe or more at a Total thickness of the antiferromagnetic layer 2 of 300 Å. If a high magnetic field resistance is specifically required Therefore, the exchange-coupled film 40 with a structure that does not have a Mn-containing layer may be preferred. As shown in the results of examples 123 to 128 in Fig. 37 (open circles, dashed line), in the In the case where the IrMn layer 2a was provided, as is the case with the exchange-coupled film 40, the strength The exchange coupling field Hex is relatively less affected by the total thickness of the antiferromagnetic layer 2. In particular, the results showed that when the total thickness of the antiferromagnetic layer 2 is in the area the ΔH range was from 150 Å to 300 Å, the strength of the exchange coupling field was stable in the range of 300 Å to 350 Å; thus The exchange-linked film 40 with this structure was less affected by film formation during the production process. influenced by variations. Reference symbol list Hex exchange coupling field Hc coercivity M0 remanent magnetization Ms saturation magnetization 10, 20, 40, 70, 71, 72, 73, 74, 75 exchange-linked film 1 lower class 2, 80, 81, 82, 83, 84, 85 antiferromagnetic layer 2a IrMn layer 2b, 8b first PtMn layer 2c, 8c PtCr layer 2d, 8d second PtMn layer 3-pin magnetic layer (ferromagnetic layer) 3A first magnet layer 3B non-magnetic interlayer 3C second magnetic layer 4 layers of non-magnetic material 5 free magnetic layer 6 protective layer 8a Mn-containing layer 8a1 Mn layer D1 Thickness of the IrMn layer 2a D1 Thickness of the Mn-containing layer d2 D2 Thickness of the first PtMn layer 2b d3, D3 Thickness of the PtCr layer 2c d4, D4 Thickness of the first PtMn layer 2b 11, 11Xa, 11Xb, 11Ya, 11Yb, 21, 110, magnetic detection element 111 22, 221, 222 Multi-layer stack 30 Magnetic sensor (magnetism detection device) P pinned magnetization direction of the pinned magnetic layer 3 P1 pinned magnetization direction of the first magnetic layer 3A P2 pinned magnetization direction of the second magnetic layer 3C 32X, 32Y full bridge circuit 33 Power supply connection Vdd power supply voltage 34 Ground connection GND ground potential 32Xa first serial section of the full bridge circuit 32X 35Xa Midpoint of the first serial section 32Xa Initial potential at midpoint 35Xa of the first serial section 32Xa OutX1 32Xb second serial section of the full bridge circuit 32X 35Xb Midpoint of the second serial section 32Xb OutX2 output potential at midpoint 35Xb of the second serial section 32Xb 32Ya first serial section of the full bridge circuit 35Ya Midpoint of the first serial section 32Ya OutY1 Output potential at midpoint 35Ya of the first serial section 32Ya 32Yb second serial section of the full bridge circuit 32Y 35Yb Midpoint of the second serial section 32Yb OutY2 output potential at midpoint 35Yb of the second serial section 32Yb H external magnetic field 12 Element section 13a, 13b conductive area 14a, 14b Connection SB Substrat
Claims
1. Exchange-coupled film (10), comprising: an antiferromagnetic layer (2) and a ferromagnetic layer (3) stacked together, wherein the antiferromagnetic layer (2) has a structure comprising an Ir-Mn layer (2a), a first PtMn layer (2b, 8b), a PtCr layer (2c, 8c) and a second PtMn layer (2d, 8d) stacked in this order, wherein the IrMn layer (2a) is located close to the ferromagnetic layer (3).
2. Exchange-coupled film (10) according to claim 1, wherein the structure further includes a PtMn layer sandwiched between the IrMn layer (2a) and the ferromagnetic layer (3) are stacked.
3. Exchange-coupled film (10), comprising: an antiferromagnetic layer (2) and a ferromagnetic layer (3) stacked together, wherein the antiferromagnetic layer (2) has a structure comprising a first PtMn layer (2b, 8b), a PtCr layer (2c, 8c) and a second PtMn layer (2d, 8d) stacked in this order, wherein the first PtMn Layer (2b, 8b) is located close to the ferromagnetic layer (3) and a thickness of the PtCr layer (d3, D3) is greater than both a thickness of the first PtMn layer (d4, D4) and a thickness of the second PtMn layer.
4. Exchange-coupled film (10) according to claim 3, wherein the antiferromagnetic layer (2) comprises a Mn-containing layer with a Mn content of more than 50 at.% between the first PtMn layer (2b, 8b) and the ferromagnetic layer (3) has.
5. Exchange-coupled film (10) according to claim 4, wherein the Mn-containing layer comprises a plurality of layers stacked together has.
6. Exchange-coupled film (10) according to claim 4 or 5, wherein the Mn-containing layer comprises at least one layer, which is selected from the group consisting of an IrMn layer and a Mn layer.
7. Exchange-coupled film (10) according to one of claims 4 to 6, wherein the Mn-containing layer has a thickness of 1.2 nm or less.
8. Exchange-coupled film (10) according to one of claims 1 to 7, wherein the second PtMn layer (2d, 8d) has a thickness of more than 0 nm and less than 6.0 nm.
9. Exchange-coupled film (10) according to one of claims 1 to 7, wherein the second PtMn layer (2d, 8d) has a thickness of 1.5 nm or more and 5.5 nm or less.
10. Exchange-coupled film (10) according to one of claims 1 to 7, wherein the PtCr layer (2c, 8c) has a thickness of 10.0 nm or more.
11. Exchange-coupled film (10) according to one of claims 1 to 10, wherein the antiferromagnetic layer (2) has a total thickness of 20.0 nm or less.
12. A magnetoresistive element comprising the exchange-coupled film (10) according to any one of claims 1 to 11 and a free magnetic layer (5) stacked together, wherein the ferromagnetic layer (3) of the exchange-coupled film (10) is contained in at least a part of a pinned magnetic layer (3).
13. A magnetism detection device (30) comprising the magnetoresistive element according to claim 12.
14. Magnetism detection device (30) according to claim 13, wherein the magnetoresistive element according to claim 12 is one of a plurality of magnetoresistive elements arranged on the same substrate (SB), and wherein the plurality of magnetoresistive elements have the pinned magnetic layers (3, 3A, 3C) with different pinned magnetization directions (P, P1, P2).
Citation Information
Patent Citations
Magnetic recording medium
JP2000215431A
MAGNETORESISTIVE ELEMENT AND MAGNETORESISTIVE READING HEAD, MAGNETIC RECORDING DEVICE AND MAGNETORESISTIVE MEMORY USING THEM
DE60200949T2
Vertical magnetic recording medium and magnetic storage device
JP2002298326A
Magnetic random access memory with multilayered seed structure
US20150340598A1
Exchange-coupling film, and magneto-resistive element and magnetic detection device using same
WO2018029883A1