Resin composition and cleaning agent in which it is used, as well as molding machine cleaning processes
Patent Information
- Application Number
- DE112022006089
- Authority / Receiving Office
- DE · DE
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-12-14
- Publication Date
- 2024-10-24
Abstract
Description
Technical field
[0001] The present invention relates to a resin composition, a cleaning agent in which it is used, and a molding machine cleaning method, and in particular to a resin composition with improved handling and safety, a cleaning agent in which it is used, and a molding machine cleaning method. State of the art
[0002] Resins with very good gas-barrier properties, including ethylene-vinyl alcohol copolymers (hereinafter also referred to as "EVOHs"), are widely used in products such as films and containers for food packaging. When a resin is melt extruded in a forming machine to obtain such a product, adhesion of the resin can occur in the flow paths of the forming machine (for example, the resin may stick to a screw). If this adherent resin is left as is for a long period of time, the resin is subject to degradation, such as scorching, gelation, and decomposition. This results in products that have defects, such as streaks, hard spots, and gels, or require an enormous amount of time and material waste to eliminate such defects.
[0003] Several cleaning agents have been proposed. For example, patent document 1 discloses a cleaning agent comprising a hydrophobic thermoplastic resin, such as a polyolefin resin, a hydrophilic thermoplastic resin, such as a saponified ethylene-vinyl acetate copolymer, and water. Patent document 2 discloses a cleaning agent prepared by mixing a saponified ethylene-vinyl ester copolymer or the like with water in a predetermined ratio. Patent document 3 discloses a cleaning agent comprising a polyolefin resin, such as low-density polyethylene (LDPE), a strongly basic compound, such as an alkali metal or alkaline earth metal hydroxide, and a salt that generates free water. Patent document 4 discloses that a resin composition comprising a hydrophilic resin, water, and a basic compound in a predetermined ratio can be used as a cleaning agent. State-of-the-art documents, patent documents Patent Document 1: JP H10-016023 A Patent Document 2: JP 2008-279623 A Patent Document 3: JP 2012-533647 A Patent document 4: WO 2021 / 019873 A1 Summary of the invention Problem to be solved by the invention
[0004] However, it cannot be assumed that the cleaning agents disclosed in Patent Document 1 and Patent Document 2 are capable of sufficiently removing resin (hereinafter also referred to as "resin to be removed by cleaning") adhering to a screw and the like of a molding machine, and an improvement in cleaning performance is required. On the other hand, the cleaning agent disclosed in Patent Document 3 exhibits improved cleaning performance due to one of its components, namely the basic compound, but the cleaning performance is still not satisfactory. With regard to the cleaning agent disclosed in Patent Document 4, a further improvement in cleaning performance is required in order to remove resins with a wider range of viscosities (for example, low viscosities) by cleaning.
[0005] The present invention was made to solve the problems described above, and it is an object of the present invention to provide a cleaning agent that can efficiently discharge a resin to be removed by cleaning, for example a low viscosity resin to be removed by cleaning, in a molding machine, as well as a molding machine cleaning method using the cleaning agent. Means to solve the problem
[0006] According to the present invention, the aforementioned problem can be solved by providing: [1] A resin composition comprising a hydrophilic resin (A), water (B), a basic compound (C) and a polyolefin resin (D), wherein the water content (B) is 10 to 70 parts by mass based on 100 parts by mass of the hydrophilic resin (A), the content of the basic compound (C) is 0.1 to 15 parts by mass per 100 parts by mass of the hydrophilic resin (A), and the polyolefin resin (D) satisfies the following formula (1): 30>X×Y÷(1−Z)≥1 where in formula (1) X represents the MFR (g / 10 min) of the polyolefin resin (D) at 190 °C, Y represents the relaxation time (seconds) of the polyolefin resin (D) at 220 °C and Z represents the density (g / cm³). 3 ) of the polyolefin resin (D); [2] according to the resin composition [1], wherein the hydrophilic resin (A), the water (B) and the basic compound (C) are together in the form of a water-containing hydrophilic resin; [3] according to the resin composition [2], wherein the water-containing hydrophilic resin is in a porous particle form and has a mean pore diameter of 0.01 to 3 µm and an average particle size of 2.5 to 8 mm; [4] the resin composition according to one of [1] to [3], wherein the content of the polyolefin resin (D) is 100 to 5000 parts by mass based on 100 parts by mass of the hydrophilic resin (A); [5] the resin composition according to one of [1] to [4], wherein the hydrophilic resin (A) is an ethylene-vinyl alcohol copolymer; [6] according to the resin composition [5], wherein the ethylene vinyl alcohol copolymer has an ethylene unit content of 15 to 60 mol%; [7] the resin composition according to one of [1] to [6], wherein the basic compound (C) is at least one selected from alkali metal carbonates, alkali metal hydrogen carbonates, alkali metal phosphates, alkali metal acetates, alkali metal hydroxides, ammonia and primary to tertiary amines; [8] the resin composition according to one of [1] to [6], wherein the polyolefin resin (D) is at least a resin selected from the group consisting of polyethylene and polypropylene; [9] the resin composition according to one of [1] to [8], which furthermore includes at least one element selected from the group consisting of silicon and phosphorus in a proportion of 10 to 1000 ppm;
[10] the resin composition according to one of [1] to [9], which further comprises a divalent metal element in a proportion of 100 ppm or less;
[11] of the resin composition according to one of [1] to
[10] , wherein the divalent metal element is at least one element selected from the group consisting of calcium and magnesium;
[12] the resin composition according to one of [1] to
[11] , which is in granular form;
[13] of a cleaning agent comprising the resin composition according to one of [1] to
[12] ;
[14] of the cleaning agent according to
[13] , which is used to clean a molding machine which uses a molding resin composition with an MFR (g / 10 min) that is higher than half the value of that of the polyolefin resin (D) at 190 °C, or whose melt fluidity is higher than half the melt fluidity of the polyolefin resin (D);
[15] of the cleaning agent according to
[14] , which is used to clean a food packaging material forming machine;
[16] a method for cleaning a molding machine in which a resin to be removed by cleaning is present, comprising a step of supplying the cleaning agent to the molding machine according to a
[13] to
[15] and of discharging the cleaning agent together with the resin to be removed by cleaning. Effects of the invention
[0007] According to the present invention, resin that needs to be removed by cleaning can be efficiently discharged from a molding machine. Consequently, defects in products obtained using the molding machine can be reduced. Description of embodiments Resin composition
[0008] A resin composition of the present invention is a resin composition which can be used as a cleaning agent, for example, for cleaning a molding machine in which a resin to be removed by cleaning is present, which will be described later.
[0009] The resin composition of the present invention comprises a hydrophilic resin (A), water (B), a basic compound (C) and a polyolefin resin (D). Hydrophilic resin (A)
[0010] The hydrophilic resin (A) comprises resins exhibiting an affinity for water, and examples include resins exhibiting a contact angle with water of 0° to 90°. The hydrophilic resin (A) is, for example, preferably at least one selected from the group consisting of an EVOH, a polyvinyl alcohol, a polyamide, a polyacrylate, a polyethylene glycol, and a polyacrylamide. An EVOH is particularly preferred with respect to its heat stability and extrusion stability. When the hydrophilic resin (A) is used, an aqueous alkaline solution containing water (B) and the basic compound (C) is kept stable in the hydrophilic resin (A) at room temperature during the storage of a cleaning agent composed of the resin composition of the present invention, and consequently, user safety can be ensured.Furthermore, the hydrophilic resin (A) melts during cleaning, thereby releasing the aqueous alkaline solution, and consequently the resin adhering to a screw, which is to be removed by cleaning, can be effectively decomposed and removed. EVOH
[0011] EVOH is a copolymer obtained, for example, by saponifying an ethylene-vinyl ester copolymer. The ethylene-vinyl ester copolymer can be prepared and saponified using known methods. Examples of vinyl esters that can be used in such a process include fatty acid vinyl esters, such as vinyl acetate, vinyl formate, vinyl propionate, vinyl pivalate, and vinyl verstatate.
[0012] In the present invention, the ethylene unit content in the EVOH is preferably 15 mol% or more, 22 mol% or more, or 24 mol% or more. In the present invention, the ethylene unit content in the EVOH is preferably 60 mol% or less, 55 mol% or less, or 50 mol% or less. If the ethylene unit content is less than 15 mol%, extrusion of the resin composition may be difficult when the temperature of a melting zone of the molding machine is between 105°C and 210°C. If the ethylene unit content is more than 60 mol%, the amount of hydroxyl groups decreases, and it tends to be difficult to ensure a desired water content. The ethylene unit content in the EVOH can be measured, for example, by nuclear magnetic resonance (NMR) spectroscopy.
[0013] In the present invention, the degree of saponification of the EVOH (i.e., the degree of saponification of the vinyl ester component in the EVOH) is, for example, preferably 99 mol% or more, more preferably 99.5% or more, and even more preferably 99.9 mol% or more. If the degree of saponification is 99 mol% or more, it can, for example, prevent the consumption of the basic compound (C) during a saponification reaction. On the other hand, the degree of saponification of the EVOH is, for example, preferably 100 mol% or less and can be 99.99 mol% or less. The degree of saponification of the EVOH can be determined by measuring the peak area of hydrogen atoms contained in the vinyl ester structure and the peak area of hydrogen atoms contained in the vinyl alcohol structure. 1 H-NMR measurement can be calculated.
[0014] The EVOH may also comprise a unit derived from an additional monomer, different from ethylene, vinyl esters, and saponified products thereof, to an extent that does not impair the object of the present invention. If the EVOH comprises an additional monomer unit, the upper limit of the content of the additional monomer unit in all structural units of the EVOH is, for example, 30 mol% or less, 20 mol% or less, 10 mol% or less, or 5 mol% or less. If the EVOH comprises the unit derived from the additional monomer, its content is, for example, preferably 0.05 mol% or more, and more preferably 0.1 mol% or more.
[0015] Examples of the additional monomer include alkenes such as propylene, butylene, pentene, and hexene; Ester group-containing alkenes, such as 3-acyloxy-1-propene, 3-acyloxy-1-butene, 4-acyloxy-1-butene, 3,4-diacyloxy-1-butene, 3-acyloxy-4-methyl-1-butene, 4-acyloxy-1-butene, 3,4-diacyloxy-1-butene, 3-Acyloxy-4-methyl-1-butene, 4-acyloxy-2-methyl-1-butene, 4-acyloxy-3-methyl-1-butene, 3,4-diacyloxy-2-methyl-1-butene, 4-acyloxy-1-pentene, 5-acyloxy-1-pentene, 4,5-diacyloxy-1-pentene, 4-acyloxy-1-hexene, 5-acyloxy-1-hexene, 6-Acyloxy-1-hexene, 5,6-diacyloxy-1-hexene and 1,3-diacetoxy-2-methylenepropane or saponified products thereof; unsaturated acids, such as acrylic acid, methacrylic acid, crotonic acid and itaconic acid, or anhydrides, salts, monoalkyl esters or dialkyl esters thereof; nitriles, such as acrylonitrile and methacrylonitrile; amides, such as acrylamide and methacrylamide; olefin sulfonic acids, such asVinylsulfonic acid, allylsulfonic acid and methallylsulfonic acid, or salts thereof; vinylsilane compounds, such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane and γ-methacryloxypropylmethoxysilane; alkyl vinyl ethers, vinyl ketones, N-vinylpyrrolidone, vinyl chloride and vinylidene chloride.
[0016] EVOH can be modified by urethanization, acetalization, cyanoethylation, oxyalkylenation, or similar processes. When used in a cleaning agent, the modified EVOH improves its compatibility with a resin to be removed by cleaning, such as a urethane resin, an acetal resin, or an acrylonitrile resin, thus enabling more efficient cleaning.
[0017] A combination of two or more EVOHs that differ in ethylene unit content, degree of saponification, copolymer component, whether they are modified or not, type of modification, or the like, can also be used as the EVOH.
[0018] EVOH can be obtained using a known technique, such as bulk polymerization, solution polymerization, suspension polymerization, or emulsion polymerization. In one embodiment, bulk polymerization or solution polymerization is used, the latter of which can proceed without solvents or in an alcohol solution or the like.
[0019] There is no specific restriction regarding the solvent used in the solution polymerization, and examples include alcohols, preferably lower alcohols such as methanol, ethanol, and propanol. The amount of solvent used in the polymerization reaction solution can be selected taking into account the desired viscosity-averaged degree of polymerization of the EVOH and the chain transfer of the solvent. The ratio (solvent / total monomers) of the mass of solvent contained in the reaction solution to the total mass of monomers contained therein is, for example, 0.01 to 10 and preferably 0.05 to 3.
[0020] Examples of catalysts used in the polymerization described above include azo-based initiators, such as 2,2-azobisisobutyronitrile, 2,2-azobis-(2,4-dimethylvaleronitrile), 2,2-azobis-(4-methoxy-2,4-dimethylvaleronitrile) and 2,2-azobis-(2-cyclopropylpropionitrile); and organic peroxide-based initiators, such as isobutyryl peroxide, cumyl peroxyneodecanoate, diisopropyl peroxycarbonate, di-n-propyl peroxydicarbonate, t-butyl peroxyneodecanoate, lauroyl peroxide, benzoyl peroxide and t-butyl hydroperoxide.
[0021] The polymerization temperature is preferably 20 °C to 90 °C, and more preferably 40 °C to 70 °C. The polymerization time is preferably 2 to 15 hours, and more preferably 3 to 11 hours. The polymerization rate is preferably 10% to 90%, and more preferably 30% to 80%, based on the vinyl ester prepared for polymerization. The resin content in the solution after polymerization is preferably 5% to 85%, and more preferably 20% to 70%.
[0022] In the polymerization described above, after the polymerization has been carried out for a predetermined period or a predetermined polymerization rate has been reached, a polymerization inhibitor is optionally added, unreacted ethylene gas is removed by evaporation, and unreacted vinyl ester is removed. In this way, EVOH can be obtained.
[0023] The copolymer is then saponified by adding an alkaline catalyst to form the copolymer solution. The saponification process can be, for example, either a continuous or a batch process. Examples of alkaline catalysts that can be added include sodium hydroxide, potassium hydroxide, and alkali metal alkoxides.
[0024] After the saponification reaction, the EVOH contains the alkaline catalyst, byproduct salts such as sodium acetate and potassium acetate, and other impurities. Therefore, it is preferred to remove these, if necessary, by neutralization or washing. However, if the EVOH is washed after the saponification reaction with water (e.g., ion-exchanged water) that is essentially free of certain ions (e.g., metal ions and chloride ions), byproduct salts such as sodium acetate and potassium acetate need not be completely removed, and some may remain.
[0025] EVOH may contain an acid, a boron compound, a plasticizer, a filler, an antiblocking agent, a lubricant, a stabilizer, a surfactant, a colorant, an ultraviolet absorber, an antistatic agent, a drying agent, a crosslinking agent, a reinforcing agent, such as various fibers, and other components.
[0026] The aforementioned acid, in view of its ability to increase the thermal stability of the EVOH during melt forming, is preferably a carboxylic acid compound, a phosphoric acid compound, or the like. If the EVOH contains a carboxylic acid compound, the carboxylic acid content (i.e., the carboxylic acid content in the resin composition containing the EVOH) is preferably 1 ppm or more, more preferably 10 ppm or more, and even more preferably 50 ppm or more. On the other hand, the content of the carboxylic acid compound is preferably 10,000 ppm or less, more preferably 1,000 ppm or less, and even more preferably 500 ppm or less. If the EVOH contains a phosphoric acid compound, the phosphoric acid content (i.e., the content of the phosphoric acid compound relative to a phosphate group in the resin composition containing the EVOH) is preferably 1 ppm or more, more preferably 10 ppm or more, and even more preferably 30 ppm or more.On the other hand, the content of the phosphoric acid compound is preferably 10,000 ppm or less, more preferably 1,000 ppm or less, and even more preferably 300 ppm or less. If the content of the carboxylic acid compound or the content of the phosphoric acid compound is in the range described above, the EVOH exhibits good thermal stability during purification.
[0027] If the EVOH contains the aforementioned boron compound, its content (i.e., the content of the boron compound relative to boron in the resin composition containing the EVOH) is preferably 1 ppm or more, more preferably 10 ppm or more, and even more preferably 50 ppm or more. On the other hand, the content of the boron compound is preferably 2000 ppm or less, more preferably 1000 ppm or less, and even more preferably 500 ppm or less. If the content of the boron compound is in the range described above, the EVOH tends to exhibit good thermal stability during cleaning.
[0028] There is no specific restriction regarding the method for causing the carboxylic acid compound, the phosphoric acid compound or the boron compound to be included in the resin composition containing the EVOH, and, for example, the compound can be added to and kneaded into the composition containing the EVOH during granulation of the composition.Furthermore, a method in which the compound is added as a dry powder, a method in which the compound is added as a paste obtained by impregnating the compound with a predetermined solvent, a method in which the compound is added in a state where it is suspended in a predetermined liquid, a method in which the compound is added as a solution in which it is dissolved in a predetermined solvent, a method in which the compound is immersed in a predetermined solution, and the like may also be used. Of these methods, the method in which the compound is added as a solution in which it is dissolved in a predetermined solvent and the method in which the compound is immersed in a predetermined solution are preferred, since these two methods enable a homogeneous dispersion of the compound in the EVOH.The specified solvent is not specifically limited, but with regard to the solubility of the compound to be added, cost, ease of handling, safety of the working environment and the like, water is preferred. Polyvinyl alcohol
[0029] Polyvinyl alcohol is a resin obtained by saponifying a polymer of vinyl ester monomers. Examples of vinyl ester monomers include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, 2,2,4,4-tetramethylvinyl valerate, vinyl benzoate, vinyl pivalate, vinyl verstatate, and the like. Of these, vinyl acetate, vinyl propionate, vinyl pivalate, and vinyl verstatate are preferably used alone or as a mixture.
[0030] The degree of saponification of the polyvinyl alcohol is not specifically limited, but is preferably 80 mol% or more, more preferably 90 mol% or more, and even more preferably 95 mol% or more. Polyamide
[0031] Polyamide is a polymer with an amide bond in its main chain. Examples of polyamide include polycaproamide (nylon 6), poly-ω-aminoheptanoic acid (nylon 7), poly-ω-aminononanoic acid (nylon 9), polyundecanamide (nylon 11), polylauryllactam (nylon 12), polyethylene diamine adipamide (nylon 26), polytetramethylene adipamide (nylon 46), polyhexamethylene adipamide (nylon 66), polyhexamethylene sebacamide (nylon 610), polyhexamethylene endodecamide (nylon 612), polyoctamethylene adipamide (nylon 86), polydecamethylene adipamide (nylon 106), a caprolactam / lauryllactam copolymer (nylon 6 / 12), a caprolactam / ω-aminononanoic acid copolymer (nylon 6 / 9), a Caprolactam / hexamethylene diammonium adipate copolymer (Nylon 6 / 66), a lauryl lactam / hexamethylene diammonium adipate copolymer (Nylon 12 / 66), an ethylene diammonium adipate / hexamethylene diammonium adipate copolymer (Nylon 26 / 66). Caprolactam / hexamethylene diammonium adipate / hexamethylene diammonium sebacate copolymer (nylon 6 / 66 / 610),An ethylenediammonium adipate / hexamethylenediammonium adipate / hexamethylenediammonium sebacate copolymer (nylon 26 / 66 / 610), polyhexamethylene isophthalamide (nylon 6I), polyhexamethylene terephthalamide (nylon 6T), a hexamethylene isophthalamide / hexamethylene terephthalamide copolymer (nylon 6I / 6T), an 11-aminoundecanamide / hexamethylene terephthalamide copolymer, polynonamethylene terephthalamide (nylon 9T), polydecamethylene terephthalamide (nylon 10T), polyhexamethylenecyclohexylamide, and polynonamethylenecyclohexylamide, as well as those obtained by modifying these polyamides with aromatic amines, such as methylenebenzylamine and metaxylol diamine. Other examples include m-xylylenediammonium adipate and the like.
[0032] The polyamide can be obtained using a process such as melt polymerization, interfacial polymerization, solution polymerization, bulk polymerization, solid-phase polymerization or a combination of these processes. Polyacrylate
[0033] Polyacrylate can be produced, for example, by polymerization of acrylate monomers such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, pentyl acrylate, 2-ethylhexyl acrylate, decyl acrylate, dodecyl acrylate, stearyl acrylate, α-chloroethyl acrylate, cyclohexyl acrylate, phenyl acrylate, methoxyethyl acrylate, ethoxyethyl acrylate, methoxypropyl acrylate or ethoxypropyl acrylate, followed by hydrolysis, or it can also be obtained by polymerizing acrylonitrile and hydrolyzing the resulting polymer.
[0034] Examples of the salt that forms the polyacrylate include alkali metal salts, such as sodium, potassium, and lithium salts; alkaline earth metal salts, such as calcium, magnesium, and barium salts; and ammonium salts, such as quaternary ammonium and quaternary alkylammonium salts. Sodium salts, in particular, are the most commonly used and preferred. Polyethylene glycol
[0035] Polyethylene glycol is produced by an addition polymerization in which ethylene oxide is added to a compound with two or more hydrogen atoms, such as ethylene glycol or diethylene glycol.
[0036] When ethylene oxide is added, an alkali metal compound can be used as a catalyst. The alkali metal compound can be an alkali metal hydroxide (e.g., lithium, sodium, potassium, or the like), an alkali metal alkoxide (e.g., sodium methylate or potassium methylate), or the like. In particular, sodium hydroxide and potassium hydroxide are preferred with respect to reactivity. An alkali metal compound can be used alone, or two or more alkali metal compounds can be used in combination. Polyacrylamide
[0037] The polyacrylamide used is a polyacrylamide that is a homopolymer of acrylamide or a copolymer of acrylamide and another copolymerizable monomer and that has an amide bond.
[0038] Regarding the process for the preparation of the polyacrylamide, there is no specific restriction and (i) a process in which acrylamide or acrylamide and the further copolymerizable monomer are polymerized in methanol using 2,2'-azobisisobutyronitrile as an initiator, (ii) a process in which acrylamide or acrylamide and the further copolymerizable monomer are irradiated with light in ethanol, (iii) a process in which a redox polymerization of acrylamide or acrylamide and the further copolymerizable monomer is carried out in an aqueous solution, (vi) a process in which acrylamide or acrylamide and the further copolymerizable monomer in a solid form are irradiated with γ-rays, and the like may be used.
[0039] Examples of the other monomer that is copolymerizable with acrylamide include acrylic acid, methacrylic acid, styrenesulfonic acid, ethylenesulfonic acid, 2-acrylamide-2-methylpropanesulfonic acid, a methacrylic acid dimethylaminoethyl ester, dimethylaminopropyl methacrylate, dimethylaminoethyl acrylate, dimethylaminopropyl acrylate, diallyldimethylammonium chloride and their quaternary salts, and the like, C1-C 24 -Alkyl esters of acrylic acid, such as methyl(meth)acrylate, ethyl(meth)acrylate and butyl(meth)acrylate, and the like. Water (B)
[0040] The water (B) dissolves the basic compound (C) described later, so that an aqueous solution with a desired pH is produced, and also distributes the aforementioned EVOH extensively in the molding machine to promote the discharge of the resin to be removed by cleaning, which is present in the machine.
[0041] The water (B) forming the resin composition of the present invention can be, for example, pure water, ion-exchanged water, distilled water, tap water, or a combination thereof. Ion-exchanged water is preferred because it prevents accidental salt contamination.
[0042] The water (B) content in the resin composition of the present invention is 10 parts by mass or more, preferably 15 parts by mass or more, and more preferably 20 parts by mass or more, based on 100 parts by mass of the hydrophilic resin (A). Furthermore, the water (B) content is 70 parts by mass or less, preferably 50 parts by mass or less, and more preferably 30 parts by mass or less, based on 100 parts by mass of the hydrophilic resin (A). If the mass ratio between the hydrophilic resin (A) and the water (B) is in the range described above, an uneven distribution of water on the surface of a cleaning agent composed of the resin composition of the present invention can be prevented.Consequently, the resin composition of the present invention can be prevented from adhering to a feed hopper when introduced into the molding machine as a cleaning agent, and the distribution of the aqueous solution containing the basic compound (C) of the cleaning agent can be prevented. For these reasons, it is preferable from a safety perspective that the mass ratio lies within the range described above. The hydrophilic resin (A) in the resin composition of the present invention has a high affinity for water (B) and binds moderately to water via a hydrogen bond. Therefore, during cleaning, water required for cleaning can be released in the molding machine, and sufficient viscosity can be ensured for the discharge of the resin to be removed from the molding machine by cleaning.Furthermore, no unwanted water remains in the forming machine during cleaning, and feeding defects can be reduced.
[0043] In a first embodiment of the resin composition of the present invention, the water (B) is one of the important components for performing the function of removing the resin to be removed by cleaning.
[0044] On the other hand, in a second embodiment of the resin composition of the present invention, the water (B) can be one of the optional components. That is, although the water (B) must be included as a component of the resin composition that passes through the molding machine when the resin to be removed by cleaning is removed, it need not be included in the cleaning agent beforehand, before the latter is fed into the molding machine. For example, the water (B) can be fed into the molding machine separately from the cleaning agent when the cleaning agent is fed into the molding machine, and mixed with the components that form the cleaning agent in the molding machine, so that the resin composition of the present invention is formed. Basic compound (C)
[0045] The basic compound (C) is converted into an aqueous solution by the water (B) described above and creates alkaline conditions (preferably strongly alkaline conditions) in the molding machine, thereby promoting the discharge of the resin present in the molding machine that is to be removed by cleaning.
[0046] Examples of basic compounds (C) include alkali metal carbonates, alkali metal hydrogen carbonates, alkali metal phosphates, alkali metal acetates, alkali metal hydroxides, ammonia and primary to tertiary amines, and combinations thereof.
[0047] When the water (B) and the hydrophilic resin (A) are present together in the form of a water-containing hydrophilic resin, examples of the basic compound (C) include alkali metal carbonates, alkali metal hydrogen carbonates, alkali metal phosphates, alkali metal acetates, alkali metal hydroxides, ammonia, and primary to tertiary amines and combinations thereof. Conversely, when the water (B) and the basic compound (C) are present together in the form of an aqueous alkaline solution, examples of the basic compound (C) include alkali metal carbonates, alkali metal hydrogen carbonates, alkali metal phosphates, alkali metal acetates, ammonia, and primary to tertiary amines and combinations thereof.
[0048] Examples of alkali metal carbonates include sodium carbonate, potassium carbonate, lithium carbonate, and combinations thereof. Examples of alkali metal hydrogen carbonates include sodium hydrogen carbonate, potassium hydrogen carbonate, and combinations thereof. Examples of alkali metal phosphates include trisodium phosphate, disodium hydrogen phosphate, monosodium dihydrogen phosphate, tripotassium phosphate, dipotassium hydrogen phosphate, monopotassium dihydrogen phosphate, trilithium phosphate, dilithium hydrogen phosphate, monolithium dihydrogen phosphate, and combinations thereof. Examples of alkali metal acetates include sodium acetate, potassium acetate, lithium acetate, and combinations thereof. Examples of alkali metal hydroxides include sodium hydroxide, potassium hydroxide, lithium hydroxide, and combinations thereof.Sodium carbonate and potassium carbonate are preferred because they have sufficient cleaning power and ensure that the resulting cleaning agent guarantees the safety of a worker.
[0049] The content of the basic compound (C) is 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, based on 100 parts by mass of the hydrophilic resin (A). Furthermore, the content of the basic compound (C) is 15 parts by mass or less, preferably 12 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the hydrophilic resin (A). If the content of the basic compound (C) is less than 0.1 parts by mass, the aqueous solution formed by the basic compound (C) and the water (B) tends to be nearly neutral, which leads to a reduced efficiency in the discharge of the resin to be removed by cleaning in the molding machine.If the content of the basic compound (C) is more than 15 parts by mass, the aqueous alkaline solution tends to become saturated, causing salt precipitation during storage of the cleaning resin.
[0050] When the water (B) and the basic compound (C) are present together in the form of an aqueous alkaline solution, the pH of the aqueous alkaline solution and / or the resin composition of the present invention is preferably 8 to 14 and more preferably 10 to 13. If the pH is less than 8, the efficiency with which the resulting resin composition discharges the resin to be removed by cleaning in the molding machine tends to be low. Water-containing hydrophilic resin
[0051] In the resin composition of the present invention, the hydrophilic resin (A), the water (B) and the basic compound (C) described above can be contained together in the form of a water-containing hydrophilic resin.
[0052] The water-containing hydrophilic resin is preferably in a porous particle form, since, when the resin composition of the present invention is used as a cleaning agent, water contained in the particles can be released in the molding machine.
[0053] Such porous particles have a large number of pores on their surface and can retain water contained within the porous particles in a suitable manner and release water in the forming machine in a suitable manner.
[0054] The mean pore diameter of the porous particles is preferably 0.01 to 3 µm and more preferably 0.05 to 2 µm. The mean pore diameter of the porous particles is measured using a mercury penetration test. If the mean pore diameter is less than 0.01 µm, the amount of water absorption is low, and the resulting resin composition may not exhibit effective cleaning properties when used as a detergent. If the mean pore diameter is not less than 3 µm, water cannot be retained in the porous particles because water release is too rapid, and the resulting resin composition may not exhibit effective cleaning properties when used as a detergent.
[0055] The pore surface area of the porous particles is preferably 25 to 60 m². 2 / g and more preferably 30 to 45 m 2 / g. If the pore surface area of the porous particles is within the range described above, the basic compound (C) can be moderately adsorbed. The pore surface area of the porous particles is measured using a mercury penetration method. If the pore surface area is less than 25 m² 2 If the water content is less than 1 / g, the water content of the porous particles can decrease. If the pore surface area is more than 60 m² 2 If the density is / g, the strength of the porous particles decreases, leading to impaired handling, and the likelihood of generating fine particles and chipped parts of a granulate that occurs in the resin composition obtained as the final product may also increase.
[0056] An example of a method for adjusting the mean pore diameter and pore surface area of porous particles is adjusting the water content, alcohol content, and extrusion temperature of an EVOH paste when producing water-containing EVOH granules. It should be noted that when water-containing EVOH granules are obtained by precipitation of strand-like products, it is also possible to adjust the mean pore diameter and pore surface area by adjusting the concentration of the EVOH solution, the temperature and alcohol concentration of the precipitation bath, and the washing temperature of the resulting water-containing EVOH granules.
[0057] Furthermore, the porous particles have an average particle size of preferably 2.5 to 8 mm, and more preferably 3 to 6 mm. If the average particle size of the porous particles is less than 2.5 mm, separation of the porous particles from other resins may occur during feeding into an extruder. If the average particle size is greater than 8 mm, wear on a feed hopper during feeding into an extruder may be reduced.
[0058] In the present invention, examples of the process for producing a water-containing hydrophilic resin from the hydrophilic resin (A), water (B), and basic compound (C) described above include, but are not limited to, a process in which the water (B) containing the basic compound (C) is sprayed onto the hydrophilic resin (A); a process in which the hydrophilic resin (A) is immersed in the water (B) containing the basic compound (C); a process in which a mixture of the hydrophilic resin (A) and the basic compound is brought into contact with water vapor, which is a form of water (B); a process in which the hydrophilic resin (A), the water (B), and the basic compound (C) are extruded together; and the like.In particular, a process in which the hydrophilic resin (A) is subjected to autoclave treatment in the presence of the water (B) containing the basic compound (C); a process in which the hydrophilic resin (A) is placed in an extruder and subjected to wet extrusion while the water (B) and the basic compound (C) are added in the middle of the stream; and the like may be used. Polyolefin resin (D)
[0059] The polyolefin resin (D) serves, for example, to improve the compatibility between the resin composition of the present invention and the resin to be removed by cleaning (e.g. the low viscosity resin to be removed by cleaning) in the molding machine and the safety of the worker.
[0060] In the resin composition of the present invention, the polyolefin resin (D) is a resin that satisfies the following formula (1): 30>X×Y÷(1−Z)≥1 where in formula (1) X represents the MFR (g / 10 min) of the polyolefin resin (D) at 190 °C, Y represents the relaxation time (seconds) of the polyolefin resin (D) at 220 °C and Z represents the density (g / cm³). 3 ) of the polyolefin resin (D). The relaxation time correlates with the time required for the stress in the resin to dissipate and can be measured, in particular, using a method described later in the section of examples.
[0061] In the present invention, the left-hand side P (i.e., X × Y ÷ (1 - Z), hereinafter also referred to as the “characteristic value P of the polyolefin resin (D)”) of the above formula (1) is preferably 1 or more (as in the above formula (1)), more preferably 3 or more, and more preferably 5 or more. Furthermore, the characteristic value P of the polyolefin resin (D) is preferably less than 30, more preferably 20 or less, and more preferably 10 or less. If the characteristic value P of the polyolefin resin (D) meets the range described above, the viscosity, which is related to the cleaning power of the resin composition, and the factors, namely the density and the relaxation time, which are related to the replaceability for the resin to be removed by cleaning, can be simultaneously satisfied, and both can be effectively improved.The higher the viscosity of the polyolefin resin (D), the more predominant the physical release of a degradation product during cleaning, but the lower the replaceability. Metal release properties are important for improving the replaceability of the polyolefin resin (D). In particular, the metal release properties are improved by increasing the density, which correlates with the elastic modulus of the polyolefin resin (D), and by increasing the relaxation time, thereby improving replaceability. In the present invention, the characteristic value P is set such that it lies within a range in which these factors are well balanced.
[0062] The polyolefin resin (D) can be, for example, the same resin as the resin to be removed by cleaning, a resin compatible with the resin to be removed by cleaning, or a combination of both. Specific examples of the polyolefin resin (D) include polyethylene (including, for example, high-density polyethylene (HDPE), low-density polyethylene (LDPE), and linear low-density polyethylene (LLDPE)), polypropylene, EVAs (ethylene-vinyl acetate copolymers), EMMAs (ethylene-methyl methacrylate copolymers), and combinations thereof. Polyethylene, polypropylene, and combinations thereof are preferred as the polyolefin resin (D) because they are very versatile and allow the resulting resin composition to exhibit excellent cleaning properties when used as a cleaning agent.
[0063] The polyolefin resin (D) content is preferably 100 parts by mass or more, more preferably 200 parts by mass or more, and even more preferably 300 parts by mass or more, based on 100 parts by mass of the hydrophilic resin (A). Furthermore, the polyolefin resin (D) content is preferably 5000 parts by mass or less, more preferably 4000 parts by mass or less, and even more preferably 3000 parts by mass or less, based on 100 parts by mass of the hydrophilic resin (A). When the polyolefin resin (D) content is in the range described above, the compatibility between the resin composition of the present invention and the resin to be removed by cleaning in the molding machine is improved, the efficiency of the discharge of the resin to be removed by cleaning in the molding machine is further improved, and worker safety can also be enhanced. Additional additive
[0064] The resin composition of the present invention may contain an additional additive to such an extent that the effects of the present invention are not inhibited. Examples of the additional additive include an abrasive, a filler, a heat stabilizer, a processing aid, an antiblocking agent, an antistatic agent, an adhesion promoter, an antioxidant, a lubricant, a blowing agent, a surfactant, a plasticizer, and combinations thereof. In particular, the abrasive is used for the removal of the resin to be removed by cleaning in the molding machine by means of a physical grinding action, and examples include those composed of an inorganic compound such as aluminum oxide, zirconium oxide, silicon dioxide, titanium dioxide, or calcium carbonate.
[0065] The content of the additional additive in the resin composition of the present invention is not specifically limited and can be adjusted by a person skilled in the art to an extent in a suitable manner so that the cleaning efficiency of a combination of the hydrophilic resin (A), water (B), basic compound (C) and polyolefin resin (D) described above is not impaired. Additional component
[0066] The resin composition of the present invention preferably contains at least one element selected from the group consisting of silicon and phosphorus. The content of the at least one element is preferably 10 ppm or more, more preferably 30 ppm or more, and even more preferably 50 ppm or more, based on the resulting resin composition. With respect to the content of the at least one element, the content of silicon and phosphorus is preferably 1000 ppm or less, more preferably 500 ppm or less, and even more preferably 250 ppm or less, based on the resulting resin composition. Elements such as silicon and phosphorus can, for example, be included as part of an additive in the polyolefin resin (D).In the present invention, the addition of the at least one element in the area described above reduces the friction between resins in the feed hopper when the resulting resin composition is used as a cleaning agent, thereby ensuring a sufficient discharge volume, and the increased discharge volume can maintain the shear stress and a high cleaning capacity. Divalent metal element
[0067] It is preferred that contamination of the resin composition of the present invention with a divalent metal element is prevented. Examples of the divalent metal element include calcium, magnesium, and a combination thereof.
[0068] A divalent metal element can be present in a resin composition, for example, in the form of a divalent metal salt. However, if a resin composition containing a divalent metal element is used as a cleaning agent, sufficient cleaning power may not be achieved. This is primarily because the divalent metal element can inhibit the basicity of potassium ions in the resin composition through salt exchange with the potassium ions.
[0069] Therefore, in the resin composition of the present invention, the content of the divalent metal element is preferably adjusted to 100 ppm or less (i.e., 0 to 100 ppm), more preferably 70 ppm or less (i.e., 0 to 70 ppm) and particularly 50 ppm or less (i.e., 0 to 50 ppm), based on the resulting resin composition.
[0070] The resin composition of the present invention is preferably in granular form, as it is suitable for use as a cleaning element. Cleaning agent
[0071] In the first embodiment, a cleaning agent of the present invention is composed of the resin composition described above, or, in other words, a resin composition comprising a hydrophilic resin (A), water (B), a basic compound (C), a polyolefin resin (D), and an additional additive, which is an optional component. In the present description, the cleaning agent composed of the resin composition described above is referred to as a "first cleaning agent".
[0072] Furthermore, in the second embodiment of the present invention, the cleaning agent is composed of the resin composition described above, excluding water (B), or, in other words, a resin composition comprising a hydrophilic resin (A), a basic compound (C), a polyolefin resin (D), and an additional additive, which is an optional component. In the present description, the cleaning agent composed of the resin composition described above, excluding water (B), is referred to as a "second cleaning agent".
[0073] Regarding the types and amounts of the hydrophilic resin (A), the basic compound (C), the polyolefin resin (D), and the additional additive in the second cleaning agent of the present invention, the types and amounts can be selected according to the types and amounts of those contained in the first cleaning agent. Furthermore, the ethylene unit content and the degree of saponification of the hydrophilic resin (A) contained in the second cleaning agent of the present invention can also be adjusted according to those of the hydrophilic resin (A) contained in the first cleaning agent.
[0074] The first cleaning agent of the present invention offers excellent safety, since the operator does not need to adjust the concentrations of the cleaning agent's components when introducing it into the molding machine. On the other hand, the second cleaning agent of the present invention can improve the efficiency of transporting and storing the cleaning agent, since the second cleaning agent does not contain water (B) beforehand, and the overall mass and volume of the cleaning agent can be reduced compared to those of the first cleaning agent.
[0075] In the present invention, the first cleaning agent can be introduced directly into the molding machine, in which the resin to be removed by cleaning is located, and used, for example, by means of a feed funnel.
[0076] On the other hand, in the case of the second cleaning agent of the present invention, a predetermined quantity of water (B) is added to the second cleaning agent before use, so that a resin composition of the present invention is produced, and the produced composition can be introduced, e.g., through the feed hopper into the molding machine in which the resin to be removed by cleaning is present, and used. Alternatively, in the case of the second cleaning agent of the present invention, it is also possible that the second cleaning agent without water (B) is introduced, e.g., through the feed hopper into the molding machine in which the resin to be removed by cleaning is present, and is kneaded in a cylinder, with the water (B) being removed by a section (e.g.,an opening which passes through the cylinder) is introduced, which is provided separately in the molding machine, and a resin composition of the present invention produced in this way is used.
[0077] Examples of forming machines in which the first cleaning agent and the second cleaning agent of the present invention can be used include extruders (including, for example, single-screw extruders, twin-screw extruders and the like), injection molding machines, blow molding machines and the like.
[0078] Method for cleaning a molding machine in which a resin to be removed by cleaning is present
[0079] In a cleaning process of the present invention, for example, a resin composition comprising the hydrophilic resin (A), the water (B), the basic compound (C), the polyolefin resin (D), and an additional additive, which is an optional component, as described above, is fed into a molding machine, and the resin composition is discharged together with a resin to be removed by cleaning. In this description, the cleaning process carried out using the resin composition in this manner is referred to as a "first cleaning process".
[0080] In the first cleaning method of the present invention, the resin composition can be supplied to the molding machine, for example, by separately supplying the hydrophilic resin (A), the water (B), the basic compound (C), and the polyolefin resin (D), and an additional additive, which is an optional component, as described above, through a feed hopper and / or other sections (e.g., an opening that passes through a cylinder) of the molding machine. However, the resin composition is preferably supplied to the molding machine in the form of one of the first or second cleaning agents of the present invention.
[0081] As one embodiment, a case is described below in which the forming machine is an extruder. If the resin composition is to be fed into the extruder in the form of the first cleaning agent of the present invention, the first cleaning agent of the present invention is introduced directly into the extruder, e.g., through its feed hopper, and then the rotation of a screw in a cylinder causes the first cleaning agent to be fed into the cylinder.
[0082] If the resin composition is to be fed into the extruder in the form of the second cleaning agent of the present invention, a predetermined amount of water (B) is added to the second cleaning agent of the present invention before use. The resulting composition is introduced into the extruder, for example, through the feed hopper, and then the rotation of the screw in the cylinder causes the resin composition containing the second cleaning agent to be fed into the cylinder. In this case, to prevent corrosion of metal sections, such as the feed hopper, it is preferred to use a compound different from the alkali metal hydroxides described above as the basic compound (C) that forms the second cleaning agent.
[0083] Alternatively, the second cleaning agent of the present invention is introduced into the extruder, e.g., through the feed hopper, in a state in which the second cleaning agent contains no water (B), and then kneaded in the cylinder by rotating the screw, with the water (B) being added through a section (e.g., an opening that passes through the cylinder) that is provided separately in the molding machine. The resin composition is supplied in this way.
[0084] When the resin composition is fed into the molding machine, the cleaning temperature in the molding machine (i.e., the temperature of a melting zone of the molding machine) is preferably set to 105 °C to 170 °C, and more preferably 110 °C to 160 °C. If this temperature is lower than 105 °C, the resin composition in the molding machine may not melt sufficiently, making it difficult to efficiently discharge the resin to be removed by cleaning. If this temperature is higher than 170 °C, the cleaning efficiency may be significantly reduced due to a decrease in the viscosity of the resin.
[0085] The quantity of resin composition supplied to the molding machine preferably corresponds to 1 to 1000 times, and more preferably 2 to 100 times, the volume of resin to be removed by cleaning that remains in the molding machine (for example, if the molding machine is an extruder, this volume corresponds to the volume obtained by subtracting the volume of a screw from the volume of a cylinder). If the quantity of resin composition supplied is less than one times the volume of resin to be removed by cleaning that remains in the molding machine, there is a risk that the resin to be removed by cleaning will remain in the molding machine.If the amount of resin composition supplied is more than 1000 times the volume of resin to be removed by cleaning that remains in the molding machine, there is a risk that the resin composition will be supplied excessively after the cleaning effect in the molding machine has already been sufficiently achieved, leading to a reduction in the efficiency of the cleaning agent use.
[0086] Alternatively, instead of the first cleaning method, the cleaning method of the present invention can also be carried out by introducing an aqueous alkaline solution containing water (B) and the basic compound (C) into the molding machine and then discharging the aqueous alkaline solution along with the resin to be removed by cleaning. In this description, the cleaning method carried out using the aqueous alkaline solution in this way is referred to as a “second cleaning method”.
[0087] The water (B) used in the second purification process of the present invention is identical to the water used in the resin composition of the present invention.
[0088] The basic compound (C) used in the second purification process of the present invention contains an alkali metal, such as lithium, sodium, or potassium. Examples of the salt that can form the basic compound (C) include carbonates, hydrogen carbonates, and phosphates.
[0089] Examples of the basic compound (C) include sodium carbonate, potassium carbonate, lithium carbonate, sodium bicarbonate, potassium bicarbonate, trisodium phosphate, disodium hydrogen phosphate, monosodium dihydrogen phosphate, tripotassium phosphate, dipotassium hydrogen phosphate, monopotassium dihydrogen phosphate, trilithium phosphate, dilithium hydrogen phosphate, monolithium dihydrogen phosphate, sodium acetate, potassium acetate, lithium acetate, and combinations thereof. Sodium carbonate and potassium carbonate are preferred with regard to ensuring worker safety.
[0090] The pH of the aqueous alkaline solution added to the molding machine is preferably 8 to 14 and more preferably 10 to 13. If the pH is less than 8, the efficiency with which the resulting aqueous alkaline solution carries out the resin to be removed by cleaning in the molding machine tends to be low.
[0091] In the second cleaning method of the present invention, the aqueous alkaline solution can be supplied to the molding machine, for example, using a method in which the water (B) and the basic compound (C) are pre-mixed to produce an aqueous alkaline solution, and the produced aqueous alkaline solution is then supplied to the molding machine through a feed hopper and / or other sections (e.g., an opening that passes through a cylinder) of the molding machine. However, an aqueous alkaline solution in which a hydroxide is used as the basic compound (C) can cause undesirable corrosion if it adheres to a metal section, such as the feed hopper. For this reason, it is preferred to control the fluidity of the aqueous alkaline solution for introducing the aqueous alkaline solution into the cylinder by means of a hose or other means.To use a tube made of a chemical-resistant material (e.g., silicone rubber, Teflon (registered trademark), or the like), thereby reducing the likelihood of the aqueous alkaline solution coming into contact with a metal section other than the interior of the molding machine. Alternatively, the aqueous alkaline solution can be supplied to the molding machine by separately feeding water (B) and the basic compound (C) through the feed hopper and / or other sections (e.g., an opening that passes through the cylinder), thus creating an aqueous alkaline solution within the molding machine.
[0092] When the aqueous alkaline solution is introduced into the molding machine, the temperature in the molding machine (i.e., the temperature of the melting zone of the molding machine) is preferably set to 100 °C to 180 °C, and more preferably 105 °C to 170 °C. If this temperature is lower than 100 °C, it may be difficult to efficiently discharge the resin to be removed by cleaning. If this temperature is higher than 180 °C, there is a risk that some of the water will evaporate, preventing the aqueous alkaline solution from reacting efficiently with the resin to be removed by cleaning.
[0093] When the aqueous alkaline solution is supplied according to the second cleaning method of the present invention, the interior of the forming machine can subsequently be washed with a suitable amount of water (e.g. pure water, ion-exchanged water, distilled water, tap water or a combination thereof) to prevent corrosion in the forming machine.
[0094] According to the present invention, various resins that can be removed by cleaning can be removed by cleaning. In particular, according to the present invention, a resin that can be removed by cleaning and that has a melting index (MFR; g / 10 min) at 190 °C, which is, for example, similar to or higher than the MFR at 190 °C of the polyolefin resin (D), can be effectively removed by cleaning.
[0095] The resin to be removed by cleaning can be, for example, a thermoplastic resin or a mixture (molding resin composition) containing the thermoplastic resin. Examples of thermoplastic resins that constitute the resin to be removed by cleaning include EVOHs; polyolefin resins, such as polyethylene (including, for example, high-density polyethylene (HDPE) and low-density polyethylene (LDPE)) and polypropylene; polyester resins, such as polyethylene terephthalate (PET), polyethylene 2,6-naphthalate, polybutylene terephthalate, and copolymers thereof; polyamide resins, such as nylon-6, nylon-66, and nylon-12; hydroxyl-containing polymers, such as polyvinyl alcohol; polystyrene; poly(meth)acrylic esters; polyacrylonitrile; polyvinyl acetate; polycarbonate; polyallylate; regenerated cellulose; polyimide; polyetherimide; polysulfone; polyethersulfone; polyetheretherketone; ionomer resins; and the like.
[0096] The cleaning method of the present invention can be used for cleaning forming machines in which various resins are used that are to be removed by cleaning. In particular, the cleaning method of the present invention is suitable for cleaning not only blow molding machines, but also inflation molding machines and casting molding machines for forming general packaging materials, since it can exhibit excellent cleaning power even for relatively low-viscosity resins that are to be removed by cleaning. Examples
[0097] The present invention is described in detail below by means of examples, however, the present invention is not limited to these examples. (1) Method for measuring the mean pore diameter
[0098] The EVOH granules used in the examples and comparisons were frozen at -80 °C and then freeze-dried to produce pore size samples. Approximately 0.5 g of each sample was placed in a 5 cm³ 3 -Standard powder cell (stem volume: 0.4 cm³) 3 The sample was introduced and subjected to measurement using a Micromeritics pore distribution measuring device (AutoPore V 9620, available from Shimadzu Corporation) under an initial pressure of 2.6 kPa. The mercury contact angle was set to 130° and the mercury surface tension to 485 dyn / cm², and calculations were performed within a pore diameter range of 0.005 to 100 µm. (2) Methods for measuring the average particle size
[0099] 100 g of each of the freeze-dried pore measurement samples was subjected to dynamic image analysis according to ISO 13322-2 (2006) using a “CAMSIZER XT” from Verder Scientific and the particle size (Q3 50.0 %) at 50% (on a volume basis) from the side of a small particle size in a cumulative particle size distribution of the calculated equivalent circle diameters of particles was determined as average particle size (mm). (3) Content of the basic compound (C)
[0100] 0.5 g of each EVOH granule used in the examples and comparison examples were placed in a Teflon (registered trademark) pressure vessel to which 5 mL of concentrated nitric acid were added and then allowed to decompose at room temperature for 30 minutes. After 30 minutes, the pressure vessel was sealed, and the granules were decomposed by heating at 150 °C for 10 minutes and then at 180 °C for 5 minutes using a wet decomposition apparatus (MWS-2, available from ACTAC Co., Ltd.), and subsequently cooled to room temperature. This treated solution was transferred to a 50 mL volumetric flask (manufactured by TPX) and diluted with pure water. Metals present in this solution were analyzed using an ICP emission spectrometer (“OPTIMA 4300 DV”, available from PerkinElmer), and the potassium content was determined.Based on the obtained content of the element potassium, a value was obtained that was calculated from the molecular weight of a carbonate containing this element. (4) Calculation of the characteristic value P of the polyolefin resin used (D)
[0101] Polyolefin resins (D) used in the examples and comparison examples were subjected to measurement using a melt flow index analyzer in accordance with JIS K7210:2014 and the MFR (X) (g / cm³) 3The storage modulus (X) of each polyolefin resin (D) at 190 °C and 2160 g was determined. On the other hand, with reference to the polyolefin resins (D) used in the examples and comparison examples, the relaxation time (Y) (seconds) of each polyolefin resin (D) at 220 °C was determined by dividing the storage modulus by the loss modulus at an angular frequency of 1 rad / s, derived from the frequency-dependent measurement at a strain of 1% using ARES-G2, available from TA Instruments Japan Inc. Using the X and Y values thus obtained, as well as the density (Z) (g / cm³), the relaxation time (Y) (seconds) was calculated. 3 The characteristic value P of the polyolefin resin (D) used was calculated using the following equation: P=X×Y÷(1−Z) (5) Contents of silicon (Si), phosphorus (P) and a divalent metal
[0102] The amounts of silicon (Si), phosphorus (P), and a divalent metal contained in each of the polyolefin resins (D) used in the examples and comparison examples were measured using an X-ray fluorescence spectrometer (ZSX Primus-µ, available from Rigaku Corporation). Based on the obtained measurement results, the proportions of silicon (Si), phosphorus (P), and the divalent metal element in the resin composition were calculated. (6) Assessment of cleaning capacity (replaceability)
[0103] A single-screw extruder (available from Toyo Seiki Seisaku-sho, Ltd.; 20 mm φ) and a coat hanger die were used, and each of the resin compositions (with an MFR of 1.6 g / 10 min at 190 °C) obtained in the examples and comparison samples was processed at an extrusion temperature of 190 °C and 100 rpm for 15 minutes. Then, an EVOH (“EVAL F101”, available from Kuraray Co., Ltd.) was processed at 100 rpm for 30 minutes, and a film was peeled at a pull-off speed of 2 m / min. The appearance of the film was evaluated, and its substitutability was assessed based on the following criteria, as determined by consultation with three experts. The film was then cut to A4 size, and its appearance was evaluated.It should be noted that a "streak" refers to a defect that is a continuous line 1 mm wide extending in the MD direction, and a "hard spot" refers to a defect with a diameter of 1 mm or more. A film that meets any of the following criteria A to C can be considered capable of withstanding actual use. A: The film has 0 to 10 defects (streaks, hard spots). B: The film has 11 to 30 or more defects (streaks, hard spots). C: The film has 31 to 100 defects (streaks, hard spots). D: The film has 101 defects (streaks, hard spots). (7) Measurement of the cleaning capacity (amount of incinerated deposit residues)
[0104] An EVOH (“EVAL F101”, available from Kuraray Co., Ltd.), serving as a purification resin (1), was processed through a twin-screw extruder (2D25W, available from Toyo Seiki Seisaku-sho, Ltd.; L / D = 25) for 10 minutes, leaving the purification resin in the extruder. After stopping screw rotation and leaving the resin in the forming machine for 30 minutes, high-density polyethylene (“HI-ZEX 7000F”, available from Prime Polymer Co., Ltd.) was processed through the forming machine for 5 minutes, and the die was removed. The cylinder was then heated to 290 °C and subsequently heated for 3 hours at a screw speed of 10 rpm while air was introduced, causing oxidative degradation of the purification resin.
[0105] Next, each of the resin compositions obtained in the examples and comparison examples, which were used as the cleaning agent, was fed through a feed hopper of this extruder at a cleaning temperature of 190 °C and a screw speed of 100 rpm with an extrusion rate of 3.2 kg / hour for 40 minutes. Then, low-density polyethylene (LC-600A, available from Japan Polyethylene Corporation) was processed for 3 minutes, followed by 10 minutes of processing while the cylinder was heated to 220 °C. Afterward, high-density polyethylene (HI-ZEX 7000F, available from Prime Polymer Co., Ltd.) was processed for 5 minutes. Finally, the die was disassembled, the twin screws were removed, and the resin adhering to the screws, which was to be removed by cleaning, was collected with a copper spatula.The total mass of the collected resin to be removed by cleaning was measured. If the total mass of the resin to be removed by cleaning (the amount of incinerated deposit residue) was less than 3.0 g, it can be assumed that the cleaning agent used may have a better cleaning capacity. Example 1: Production of a resin composition (JE1)
[0106] An EVOH solution containing 100 parts by mass of an EVOH (hydrophilic resin (A)) with an ethylene content of 32 mol% and a saponification of 99.98 mol%, 60 parts by mass of methanol, and 40 parts by mass of water, was continuously fed from the top tray of a 10-tray column with a column diameter of 0.3 m. Steam was introduced through the bottom tray, creating a countercurrent contact between the EVOH solution and the steam. The column temperature was 130 °C and the column pressure was 0.3 MPa. The water-containing EVOH granules obtained through the countercurrent contact with the steam were collected from the bottom of the column.The resulting water-containing EVOH granules were fed into a twin-screw extruder at a rate of 42 kg / hour and extruded under the following conditions through a die attached to the front end of the extruder, which had 8 holes with a diameter of 30 mm, and the melt was cut by a hot cutting device with two blades at a distance of 0.05 mm from the die, and in this way a water-containing EVOH granule with a flat spherical shape was obtained. <Bedingungen des Doppelschneckenextruders> - L / D: 14 - Hole diameter: 30 mm - Snails: Fully functional - Speed: 300 rpm - Cylinder temperature: 90 °C - Nozzle temperature: 120 °C - Number of nozzle holes: 8
[0107] Then, 3 kg of the resulting water-containing EVOH granules were washed in ion-exchanged water (bath ratio: 20) at 50 °C for 1 hour with stirring and the liquid was removed. This process was repeated twice. Subsequently, the washed water-containing EVOH granules were placed in an aqueous 1 g / L acetic acid solution (bath ratio: 20) at 25 °C for 2 hours with stirring and then the liquid was removed. This process was repeated twice. Furthermore, the washed water-containing EVOH granules were placed in ion-exchanged water (bath ratio: 20) at 25 °C for 2 hours with stirring and the liquid was removed. This process was repeated twice. Finally, the electrical conductivity of the wash solution was measured using a CM-30ET electrical conductivity meter, available from TOA Electronics Ltd.Since the electrical conductivity of the washing solution was 10 µS / cm, a third washing was carried out accordingly. The electrical conductivity of the washing solution after the third washing was measured at 3 µS / cm, and therefore the washing was stopped.
[0108] The washed, water-containing EVOH granules were immersed in an aqueous 1 mol / L potassium carbonate solution, prepared using water (B) and potassium carbonate as the basic compound (C), and chemically treated for 2 hours with periodic stirring. The treated water-containing EVOH granules were then desiccated and dried at 60 °C for 5 hours under reduced pressure, yielding porous particles with a water content of 24 wt%. The resulting water-containing porous particles were dry-mixed with 2500 wt high-density polyethylene (HDPE) (“NOVATEC (registered trademark) HY540”, available from Japan Polyethylene Corporation), serving as the polyolefin resin (D), to obtain a resin composition (JE1). The cleaning power of this resin composition (JE1) was evaluated as described above. Table 1 shows the results. Example 2: Production of a resin composition (JE2)
[0109] A resin composition (JE2) was obtained in the same manner as in Example 1, except that 2500 parts by mass of low-density polyethylene (LDPE) (“NOVATEC (registered trademark) LJ400”, available from Japan Polyethylene Corporation) was used as the polyolefin resin (D) instead of the HDPE, and the cleaning power of the resin composition (JE2) was evaluated as described above. Table 1 shows the results. Example 3: Production of a resin composition (JE3)
[0110] A resin composition (JE3) was obtained in the same manner as in Example 1, except that 2500 parts by mass of LDPE (“NOVATEC (registered trademark) LF342”, available from Japan Polyethylene Corporation) was used as the polyolefin resin (D) instead of the HDPE, and the cleaning power of the resin composition (JE3) was evaluated as described above. Table 1 shows the results. Example 4: Production of a resin composition (JE4)
[0111] A resin composition (JE4) was obtained in the same manner as in Example 1, except that 2500 parts by mass of a linear low-density polyolefin resin (LLDPE) (“NOVATEC (registered trademark) UF230”, available from Japan Polyethylene Corporation) was used as the polyolefin resin (D) instead of the HDPE, and the cleaning power of the resin composition (JE4) was evaluated as described above. Table 1 shows the results. Example 5: Production of a resin composition (JE5)
[0112] A resin composition (JE5) was obtained in the same manner as in Example 1, except that 2500 parts by mass of LDPE (“NOVATEC (registered trademark) LF128”, available from Japan Polyethylene Corporation) was used as the polyolefin resin (D) instead of the HDPE, and the cleaning power of the resin composition (JE5) was evaluated as described above. Table 1 shows the results. Example 6: Production of a resin composition (JE6)
[0113] An EVOH solution at 60 °C, containing 100 parts by mass of an EVOH (hydrophilic resin (A)) with an ethylene content of 32 mol% and a degree of saponification of 99.98 mol%, 60 parts by mass of methanol, and 40 parts by mass of water, was extruded in a strand-like form through a metal plate with a circular opening of 3.5 mm diameter into a mixed solution of water and methanol (mass ratio: water / methanol = 9 / 1) kept at 5 °C. The strands were then precipitated and allowed to solidify, and subsequently cut with a cutting device to obtain EVOH granules. These EVOH granules were then stirred into warm water at 30 °C for 4 hours, resulting in water-containing EVOH granules.
[0114] The water-containing EVOH granules were then subjected to washing and a specified chemical treatment in the same way as in Example 1, and porous particles were obtained in this way.
[0115] A resin composition (JE6) was obtained in the same manner as in Example 1, except that the porous particles thus obtained were used instead of the porous particles used in Example 1, and the cleaning power of the resin composition (JE6) was evaluated as described above. Table 1 shows the results. Example 7: Production of a resin composition (JE7)
[0116] The evaluation was carried out in the same manner as in Example 1, except that a resin composition (JE7) was obtained by dry mixing the water-containing porous particles obtained in Example 1 with 4268 parts by mass of high-density polyethylene (HDPE) (“NOVATEC (registered trademark) HY540”, available from Japan Polyethylene Corporation), serving as the polyolefin resin (D), and potassium stearate. Table 1 shows the results. Example 8: Production of a resin composition (JE8)
[0117] The evaluation was carried out in the same manner as in Example 1, except that a resin composition (JE8) was obtained by dry-mixing the water-containing porous particles obtained in Example 1 with 2500 parts by mass of high-density polyethylene (HDPE) (“NOVATEC (registered trademark) HY540”, available from Japan Polyethylene Corporation), serving as the polyolefin resin (D), and calcium stearate. The amount of calcium stearate added was adjusted to achieve a calcium content of 80 ppm, including the calcium naturally present in NOVATEC HY540. Table 1 shows the results. Comparative example 1: Production of a resin composition (JC1)
[0118] A resin composition (JC4) was obtained in the same manner as in Example 1, except that 2500 parts by mass of HDPE (“NOVATEC (registered trademark) HB111R”, available from Japan Polyethylene Corporation) was used as the polyolefin resin (D) instead of the HDPE used in Example 1. It should be noted that the characteristic value P of the polyolefin resin (D) used in this comparative example was 0.5. The cleaning performance of this resin composition (JC1) was evaluated in the manner described above. Table 1 shows the results. Comparative example 2: Production of a resin composition (JC2)
[0119] A resin composition (JC2) was obtained in the same manner as in Example 1, except that 2500 parts by mass of LDPE (“NOVATEC (registered trademark) LC600”, available from Japan Polyethylene Corporation) was used as the polyolefin resin (D) instead of the HDPE. It should be noted that the characteristic value P of the polyolefin resin (D) used in this comparative example was 31.8. The cleaning performance of this resin composition (JC2) was evaluated as described above. Table 1 shows the results. Comparative example 3: Production of a resin composition (JC3)
[0120] The hydrophilic resin (A) “EVAL (registered trademark) H171”, available from Kuraray Co., Ltd. (an EVOH with an ethylene content of 38 mol%, a degree of saponification of 99.9 mol%, a mean pore diameter of 0.005 µm, and a mean particle size of 3.5 mm) was used instead of the washed EVOH in Example 1. A chemical treatment was carried out for 2 hours with periodic stirring. The water-containing EVOH granules after treatment were desalinated and dried at 60 °C for 5 hours under reduced pressure to obtain porous particles with a water content of 5 wt%. Otherwise, the same procedure as in Example 1 was carried out, and consequently, a resin composition (JC3) was obtained. The cleaning power of the obtained resin composition (JC3) was evaluated in the manner described above. Table 1 shows the results. Comparative example 4: Production of a resin composition (JC4)
[0121] A resin composition (JC4) was obtained in the same manner as in Example 1, except that 2500 parts by mass of a high-density polyethylene (“HI-ZEX 7000F”, available from Prime Polymer Co., Ltd.) was used as the polyolefin resin (D). It should be noted that the characteristic value P of the polyolefin resin (D) used in this comparative example was 0.7. The cleaning power of the obtained resin composition (JC4) was evaluated in the manner described above. Table 1 shows the results. [Table 1] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Resin composition Designation of resin composition JE1 JE2 JE3 JE4 JE5 JE6 JE7 JE8 Hydrophilic resin (A) Art - EVOH EVOH EVOH EVOH EVOH EVOH EVOH EVOH Salary Mass parts 100 100 100 100 100 100 100 100 Mean pore diameter µm 0,11 0,11 0,11 0,11 0,11 4 0,11 0,11 Average particle size mm 3,2 3,2 3,2 3,2 3,2 4,2 3,2 3,2 Water (B) Salary Mass parts 25 25 25 25 25 25 25 25 Basic compound (C) Art - K2CO3 K2CO3 K2CO3 K2CO3 K2CO3 K2CO3 K2CO3 K2CO3 Salary Mass parts 7 7 7 7 7 1 7 7 Polyolefin resin (D) Art - HDPE LDPE LDPE LLDPE HDPE HDPE HDPE HDPE Salary Mass parts 2500 2500 2500 2500 2500 2394 4268 2500 brand - HY540 LJ400 LF342 U F230 LF128 HY540 HY540 HY540 Density (Z) g / c m3 0,96 0,921 0,924 0,921 0,922 0,96 0,96 0,96 MFR at 190 °C, 2.16 kg (X) g / 10 min 1 1,5 1 1 0,25 1 1 1 Relaxation time at 220 °C (Y) seconds 0,20 0,36 0,48 0,17 0,82 0,20 0,20 0,20 X × Y / (1 - Z) - 5,1 6,8 6,4 2,1 2,6 5,1 5,1 5,1 Si Salary ppm 100 40 20 120 10 100 168 100 P Salary ppm 80 30 30 70 10 80 134 80 Divalent metal Art - Approx Approx Approx Approx Approx Approx Approx Approx Salary ppm 40 40 70 30 50 20 67 80 Mixing ratio ((A) + (B) + (C)) / (D) - 5 / 95 5 / 95 5 / 95 5 / 95 5 / 95 5 / 95 3 / 97 5 / 95 Evaluation Cleaning power Replaceability - A B B C C A B A Amount of incinerated deposit residue g 1,1 0,9 1,3 1,2 1,0 2,9 1,9 1,6 [Table 1] (continued) Comparative example 1 Comparative example 2 Comparative example 3 Comparative example 4 Resin composition Designation of resin composition JC1 JC2 JC3 JC4 Hydrophilic resin (A) Art - EVOH EVOH EVOH EVOH Salary Mass parts 100 100 100 100 Mean pore diameter µm 0,11 0,11 0,005 0,11 Average particle size mm 3,2 3,2 3,5 3,2 Water (B) Salary Mass parts 25 25 5 25 Basic compound (C) Art - K2CO3 K2CO3 K2CO3 K2CO3 Salary Mass parts 7 7 0,05 7 Polyolefin resin (D) Art - HDPE LDPE HDPE HDPE Salary Mass parts 2500 2500 2500 2500 brand - HB111R LC600 HY540 7000F Density (Z) g / cm 3 0,945 0,918 0,960 0,951 MFR at 190 °C, 2.16 kg (X) g / 10 min 0,03 7 1 0,04 Relaxation time at 220 °C (Y) seconds 0,92 0,37 0,20 0,91 X × Y / (1-Z) - 0,5 31,8 5,1 0,7 Si Salary ppm 150 5 100 20 P Salary ppm 60 10 80 20 Divalent metal Art - Approx Approx Approx Approx Salary ppm 0 60 30 140 Mixing ratio ((A) + (B) + (C)) / (D) - 5 / 95 5 / 95 5 / 95 5 / 95 Evaluation Cleaning power Replaceability - D A A D Amount of incinerated deposit residue g 0,8 3,5 4,1 2,2
[0122] As shown in Table 1, all resin compositions (JE1) to (JE8) obtained in Examples 1 to 6 exhibited excellent cleaning properties with respect to both the replaceability and the amount of burnt residue. In particular, when resin compositions (JE1) to (JE5) obtained in Examples 1 to 5 were used, the amount of resin adhering to the screws and requiring cleaning was reduced to a very low value of about 1 g, demonstrating that these resin compositions are extremely useful as cleaning agents.In contrast, the resin compositions (JC1), (JC2), (JC3) and (JC4) obtained in comparative examples 1 to 4 showed good cleaning performance either with respect to the replaceability or the quantity of a burnt deposit residue, but did not show good results with respect to both the replaceability and the quantity of a burnt deposit residue. Commercial applicability
[0123] The present invention is useful, for example, in the field of plastics molding in that it enables the reduction of defects in products obtained by a molding machine and the reduction of the significant time and material losses required to eliminate such defects. QUOTES INCLUDED IN THE DESCRIPTION
[0000] This list of documents cited by the applicant was automatically generated and is included solely for the reader's convenience. The list is not part of the German patent or utility model application. The DPMA accepts no liability for any errors or omissions. Cited patent literature
[0000] JP H10016023 A
[0003] JP 2008279623 A
[0003] JP 2012533647 A
[0003] WO 2021 / 019873 A1
[0003]
Claims
[1] Resin composition comprising a hydrophilic resin (A), water (B), a basic compound (C) and a polyolefin resin (D), wherein the content of water (B) is 10 to 70 parts by mass based on 100 parts by mass of the hydrophilic resin (A), the content of the basic compound (C) is 0.1 to 15 parts by mass based on 100 parts by mass of the hydrophilic resin (A), and the polyolefin resin (D) satisfies the following formula (1): 30>X×Y÷(1−Z)≥1 where in the formula (1), X represents the MFR (g / 10 min) of the polyolefin resin (D) at 190 °C, Y represents the relaxation time (seconds) of the polyolefin resin (D) at 220 °C, and Z represents the density (g / cm 3 ) of the polyolefin resin (D). [2] The resin composition according to claim 1, wherein the hydrophilic resin (A), the water (B) and the basic compound (C) are contained together in the form of a water-containing hydrophilic resin. [3] The resin composition according to claim 2, wherein the water-containing hydrophilic resin is in a porous particle form and has an average pore diameter of 0.01 to 3 µm and an average particle size of 2.5 to 8 mm. [4] The resin composition according to any one of claims 1 to 3, wherein the content of the polyolefin resin (D) is 100 to 5000 parts by mass based on 100 parts by mass of the hydrophilic resin (A). [5] The resin composition according to any one of claims 1 to 4, wherein the hydrophilic resin (A) is an ethylene-vinyl alcohol copolymer. [6] The resin composition according to claim 5, wherein the ethylene-vinyl alcohol copolymer has an ethylene unit content of 15 to 60 mol%. [7] The resin composition according to any one of claims 1 to 6, wherein the basic compound (C) is at least one selected from alkali metal carbonates, alkali metal hydrogencarbonates, alkali metal phosphates, alkali metal acetates, alkali metal hydroxides, ammonia, and primary to tertiary amines. [8] The resin composition according to any one of claims 1 to 6, wherein the polyolefin resin (D) is at least one resin selected from the group consisting of polyethylene and polypropylene. [9] The resin composition according to any one of claims 1 to 8, further comprising at least one element selected from the group consisting of silicon and phosphorus in a proportion of 10 to 1000 ppm. [10] The resin composition according to any one of claims 1 to 9, further comprising a divalent metal element in a proportion of 100 ppm or less. [11] The resin composition according to any one of claims 1 to 10, wherein the divalent metal element is at least one element selected from the group consisting of calcium and magnesium. [12] A resin composition according to any one of claims 1 to 11, which is in a granular form. [13] A cleaning agent comprising the resin composition according to any one of claims 1 to 12. [14] A cleaning agent according to claim 13, which is used for cleaning a molding machine using a molding resin composition having an MFR (g / 10 min) higher than half that of the polyolefin resin (D) at 190 °C, or whose melt fluidity is higher than half that of the polyolefin resin (D). [15] A cleaning agent according to claim 14, which is used for cleaning a food packaging material forming machine. [16] A method for cleaning a molding machine in which a resin to be removed by cleaning is present, the method comprising a step of supplying the cleaning agent according to any one of claims 13 to 15 into the molding machine and discharging the cleaning agent together with the resin to be removed by cleaning.
Citation Information
Patent Citations
Purging agent
JP1998016023A
Purging material and purging method using the material
JP2008279623A
Reactive purging compounds for polymer removal
JP2012533647A
Purging agent and method for purging molding machine using same
WO2021019873A1