ALUMINUM ALLOY MATERIAL AND METHOD FOR ITS PRODUCTION

By adding Si and Mo to an Al-Cu-Mg alloy, the alloy composition forms a σ phase that significantly improves high-temperature creep resistance, addressing cost and performance issues in existing alloys.

DE112023001084T5Pending Publication Date: 2024-12-05KOBE STEEL LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
DE112023001084
Authority / Receiving Office
DE · DE
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-15
Filing Date
2023-01-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing aluminum alloys used for high-temperature applications, such as automotive turbochargers and industrial machine parts, suffer from significant strength degradation at temperatures above 120°C due to high creep rates, and techniques involving noble metals like Ag increase costs without sufficient improvement.

Method used

Incorporating specific amounts of Si and Mo into an Al-Cu-Mg-based alloy composition, along with other elements, to form a σ phase that enhances high-temperature creep resistance, while avoiding the use of expensive noble metals.

Benefits of technology

The alloy achieves a minimum creep rate of 8.5 × 10^-10/s at 160°C and 250 MPa, providing excellent high-temperature creep resistance without the cost of noble metals.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides an aluminum alloy material with excellent high-temperature creep resistance and a method for producing the aluminum alloy material. The present invention relates to: an aluminum alloy material with an alloy composition comprising 1.5–6.0 wt% Cu, 1.0–4.0 wt% Mg, 0.5–2.0 wt% Fe, 0.5–2.0 wt% Ni, 0.1–3.0 wt% Si, 0.05–0.7 wt% Mo, 0.01–0.3 wt% Ti, and, as the remainder, Al and incidental impurities; and a method for producing the aluminum alloy material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The present invention relates to an aluminum alloy material and a method for producing the same. Aluminum may also be referred to simply as Al. State of the art

[0002] Al alloy materials with excellent high-temperature properties are used for Al alloy parts operating at high temperatures exceeding 100 °C, such as impellers for automotive turbochargers and pump rotors for industrial machinery (e.g., turbomolecular pumps, vacuum pumps, and diffusion pumps). Furthermore, with the improvement in the performance of automobiles, industrial machinery, and the like, the heat distortion resistance required for heat-resistant Al alloys has also increased, and excellent high-temperature creep strength has been required.

[0003] Until now, 2000 series Al alloys, specified in AA standards or JIS standards (hereinafter referred to simply as the 2000 series), have been used as these so-called heat-resistant Al alloy materials. Examples of Al alloys of this type include 2000 series Al-Cu(-Mg)-based aluminum alloys, such as 2219 and 2618 alloys. However, when these 2000 series Al alloys are used for long periods at high temperatures exceeding 120°C, their strength decreases significantly.

[0004] Therefore, techniques to improve the heat resistance of aluminum alloys have been investigated.

[0005] For example, PTL 1 describes a technique for improving creep strength by adding Ag to an Al-Cu-Mg-based alloy, which is equivalent to a 2000 series aluminum alloy, and further adding Mn and Cr to be dissolved.

[0006] PTL 2 describes a technique for achieving excellent creep resistance by adjusting a crystallized material of an Al-Cu-Mg-based alloy by adjusting the cooling rate during casting.

[0007] PTL 3 describes a technique for improving creep strength by finely dispersing, at partial grain boundaries, an intermetallic compound that crystallizes by adding Zr and Ti.

[0008] PTL 4 describes a technique for improving the high-temperature creep strength by fixing additive elements and coarsening the crystal grains of an Al-Cu-based alloy.

[0009] PTL 5 describes a technique for providing an Al alloy with excellent high-temperature properties (heat resistance, high-temperature fatigue resistance, high-temperature creep resistance, and high-temperature yield strength) and discloses an Al alloy containing Si, Cu, Mn, Mg, Ti, and Ag in predetermined amounts, while Zr is limited to less than a predetermined amount, the remainder being Al and incidental impurities. Document listPatent documents PTL 1: Japanese unexamined patent application with publication number 2013-142168 PTL 2: Japanese unexamined patent application with publication number 2021-134414 PTL 3: Japanese unexamined patent application with publication number 2017-043802 PTL 4: Japanese unexamined patent application with publication number 2020-066785 PTL 5: Japanese unexamined patent application with publication number 2013-014835 Summary of the inventionTechnical problem

[0010] Many of the existing techniques for improving the high-temperature creep strength of a 2000 series aluminum alloy utilize a precious metal such as Ag and therefore have a problem in that the alloy cost increases significantly even though the heat distortion strength increases (PTL 2 and PTL 5).

[0011] In the prior art, where the amounts of elements such as Fe and Ni that form a crystallized material are fixed, sufficient creep strength is not achieved (PTL 2). The technique of adding transition metals such as Zr and Ti, which exhibit a strong oxidation tendency, improves high-temperature strength, but has the problem that the effect is not sufficiently exerted when manufacturing by casting at a low solidification rate for large parts (PTL 5).

[0012] That is, there is a need for a technique to significantly improve the creep strength at high temperatures compared with those of existing aluminum alloys without using an expensive precious metal such as Ag as an additive element, even in a case where an aluminum alloy is applied to large parts.

[0013] In view of the foregoing, it is an object of the present invention to provide an aluminum alloy material having excellent high-temperature creep strength and a method for producing the aluminum alloy material. Solution to the problem

[0014] As a result of extensive research and development to impart excellent high-temperature creep strength to an aluminum alloy material having, for example, an Al-Cu-Mg composition, which is typically a 2618 alloy, the inventors of the present invention have found that the above problems can be solved by adding Si and Mo and have completed the present invention.

[0015] Specifically, the present invention is as follows. [1] Aluminium alloy material having an alloy composition containing: Cu: 1.5 to 6.0 mass%, Mg: 1.0 to 4.0 mass%, Fe: 0.5 to 2.0 mass%, Ni: 0.5 to 2.0 mass%, Si: 0.1 to 3.0 mass%, Mo: 0.05 to 0.7 mass%, and Ti: 0.01 to 0.3 mass%, the remainder being Al and incidental impurities. [2] Aluminium alloy material having an alloy composition containing: Cu: 1.9 to 3.0 mass%, Mg: 1.3 to 3.0 mass%, Fe: 0.9 to 1.3 mass%, Ni: 0.9 to 1.3 mass%, Si: 0.25 to 0.8 mass%, Mo: 0.05 to 0.5 mass%, and Ti: 0.04 to 0.09 mass%, the remainder being Al and incidental impurities. [3] Aluminium alloy material according to [1] or [2], wherein the contents of Si and Mo Si: 0.1 to 0.6 mass% and Mo: 0.3 to 0.7 mass%. [4] Aluminium alloy material according to [1] or [2], wherein the contents of Si and Mo Si: 0.35 to 0.8 mass% and Mo: 0.05 to 0.55 mass%. [5] Aluminium alloy material according to [1] or [2], wherein the aluminum alloy material has a minimum creep rate of 8.5 × 10- 10 / s or less at 160 °C and 250 MPa. [6] A method for producing an aluminum alloy material, the method being a method for producing the aluminum alloy material having the alloy composition according to [1] or [2], the method comprising performing melting a molten metal having the alloy composition, casting, homogenization treatment, hot working, solution treatment, quenching, and aging treatment in this order. Advantageous effects of the invention

[0016] The present invention can provide an aluminum alloy material having excellent high-temperature creep strength.

[0017] Furthermore, the method for producing an aluminum alloy material according to the present invention enables the production of an aluminum alloy material having excellent high-temperature creep strength. Description of embodiments

[0018] Below, embodiments for implementing the aluminum alloy material according to the present invention will be described in detail. It should be noted that "up to," which indicates a numerical range, is used to mean that the numerical values ​​before and after are included as the lower limit and the upper limit, respectively. <aluminiumlegierungsmaterial>

[0019] Aluminum alloy materials according to the embodiments have predetermined alloy compositions as aluminum alloys and are used for manufacturing aluminum alloy materials (aluminum alloy parts) having excellent high-temperature creep strength.

[0020] An aluminum alloy material according to a first embodiment of the present invention has an alloy composition comprising: Cu: 1.5 to 6.0 mass%, Mg: 1.0 to 4.0 mass%, Fe: 0.5 to 2.0 mass%, Ni: 0.5 to 2.0 mass%, Si: 0.1 to 3.0 mass%, Mo: 0.05 to 0.7 mass%, and Ti: 0.01 to 0.3 mass%, the remainder being Al and incidental impurities.

[0021] An aluminum alloy material according to a second embodiment of the present invention has an alloy composition comprising: Cu: 1.9 to 3.0 mass%, Mg: 1.3 to 3.0 mass%, Fe: 0.9 to 1.3 mass%, Ni: 0.9 to 1.3 mass%, Si: 0.25 to 0.8 mass%, Mo: 0.05 to 0.5 mass%, and Ti: 0.04 to 0.09 mass%, the remainder being Al and incidental impurities.

[0022] In an aluminum alloy material according to a third embodiment of the present invention, the contents of Si and Mo in the aluminum alloy material according to the first embodiment or the second embodiment are preferably Si: 0.1 to 0.6 mass%, and Mo: 0.3 to 0.7 mass%.

[0023] In an aluminum alloy material according to a fourth embodiment of the present invention, the contents of Si and Mo in the aluminum alloy material according to the first embodiment or the second embodiment are preferably Si: 0.35 to 0.8 mass%, and Mo: 0.05 to 0.55 mass%.

[0024] The alloy compositions of the aluminum alloy materials according to the embodiments of the present invention can be adjusted to the above ranges by adding Si and Mo to an Al-Cu-Mg composition, typically an AA2618 aluminum alloy.

[0025] It has been found that a σ-phase (Al5Cu6Mg2), which is a newly precipitated phase, can be introduced into the aluminum alloy material according to an embodiment of the present invention by incorporating Si and Mo in specific amounts, thereby significantly improving the creep strength at high temperatures. [Alloy composition]

[0026] The above alloy compositions are described below. (Cu: 1.5 to 6 mass%)

[0027] Cu is one of the elements essential for the aluminum alloy material according to an embodiment of the present invention so as to provide high-temperature creep strength.

[0028] Cu forms a fine precipitate composed of an S phase (Al2CuMg) during aging after solution treatment in the preparation of the aluminum alloy material when added together with Mg, and improves the high-temperature creep strength as a result of precipitation hardening of the S phase.

[0029] In order to achieve the above effect, the Cu content is in a range of 1.5 to 6.0 mass%. If the Cu content is less than 1.5 mass%, the effect of improving high-temperature creep strength is not sufficiently provided. If the Cu content exceeds 6.0 mass%, a coarse, crystallized Al-Cu-based material is formed during the casting stage, and the solution treatment takes a long time. The lower limit of the Cu content is preferably 1.9 mass% or more, more preferably 2.2 mass% or more. The upper limit of the Cu content is preferably 4.5 mass% or less, more preferably 3.0 mass% or less. (Mg: 1.0 to 4.0 mass%)

[0030] Mg is one of the elements essential for the aluminum alloy material according to an embodiment of the present invention, so that the high-temperature creep strength is provided.

[0031] Mg forms a fine precipitate composed of an S phase (Al2CuMg) during aging after solution treatment in the preparation of the aluminum alloy material when added together with Cu and improves the high-temperature creep strength.

[0032] In order to achieve the above effect, the Mg content is in a range of 1.0 to 4.0 mass%. If the Mg content is less than 1.0 mass%, the effect of improving high-temperature creep strength is not sufficiently provided. If the Mg content exceeds 4.0 mass%, the amount of coarse Mg2Si increases and the toughness deteriorates. The lower limit of the Mg content is preferably 1.2 mass% or more, more preferably 1.3 mass% or more. The upper limit of the Mg content is preferably 3.5 mass% or less, more preferably 3.0 mass% or less. (Fe: 0.5 to 2.0 mass%)

[0033] Fe together with Ni forms a compound based on Al-Fe-Ni, such as Al g FeNi, and has a function of preventing excessive coarsening of the crystal grain size and a function of preventing deformation near crystal grain boundaries, so that the high-temperature creep strength is slightly improved.

[0034] In view of providing the above effect, the Fe content is in a range of 0.5 to 2.0 mass%. If the Fe content is less than 0.5 mass%, the effect of preventing the crystal grain size from becoming coarser cannot be sufficiently provided. If the Fe content exceeds 2.0 mass%, the amount of a crystallized material increases excessively, and properties other than strength, such as ductility and toughness, are impaired. The lower limit of the Fe content is preferably 0.7 mass% or more, more preferably 0.9 mass% or more. The upper limit of the Fe content is preferably 1.6 mass% or less, more preferably 1.3 mass% or less. (Ni: 0.5 to 2.0 mass%)

[0035] Ni forms an Al-Fe-Ni-based compound such as Al9FeNi together with Fe, and has a function of preventing excessive coarsening of the crystal grain size and a function of preventing deformation near crystal grain boundaries, so that the high-temperature creep strength is slightly increased.

[0036] The Ni content is in a range of 0.5 to 2.0 mass%. If the Ni content is less than 0.5 mass%, the above effect cannot be sufficiently provided. If the Ni content exceeds 2.0 mass%, the amount of a crystallized material increases excessively, and properties other than strength, such as ductility and toughness, are impaired. The lower limit of the Ni content is preferably 0.7 mass% or more, more preferably 0.9 mass% or more. The upper limit of the Ni content is preferably 1.6 mass% or less, more preferably 1.3 mass% or less. (Si: 0.1 to 3.0 mass%)

[0037] Si is one of important elements essential for further improving the high-temperature creep strength of the aluminum alloy material according to an embodiment of the present invention, compared with the high-temperature creep strength of existing Al-Cu-Mg-based aluminum alloys.

[0038] Si has a function of promoting the nucleation of σ-phase (Al5Cu6Mg2) by forming a cluster in the early stage of aging and attracting Cu with a compressive stress formed around the cluster as a driving force.

[0039] The inventors of the present invention have conducted investigations and found the following: Since the aluminum alloy material according to one embodiment of the present invention contains Si in a predetermined amount, the function of improving the high-temperature creep strength can be provided by the effect of Si alone; however, when the aluminum alloy material contains both Si and Mo in predetermined amounts, the amount of a σ phase formed is increased and the high-temperature creep strength can be further improved.

[0040] The Si content is in a range of 0.1 to 3.0 mass%. If the Si content is less than 0.1 mass%, the σ phase is not sufficiently stabilized and the effect of σ phase precipitation is not sufficiently provided. If the Si content exceeds 3.0 mass%, a Si phase with an extremely brittle diamond structure is formed, resulting in a problem of deterioration in ductility and toughness. The lower limit of the Si content is preferably 0.25 mass% or more, 0.3 mass% or more, 0.35 mass% or more, or 0.4 mass% or more. The upper limit of the Si content is preferably 1.5 mass% or less, more preferably 0.8 mass% or less, even more preferably 0.75 mass% or less, and even more preferably 0.6 mass% or less. (Mo: 0.05 to 0.7 mass%)

[0041] Mo is an important element essential for further improving the high-temperature creep strength of the aluminum alloy material according to an embodiment of the present invention, compared with the high-temperature creep strength of existing Al-Cu-Mg-based aluminum alloys.

[0042] Mo is an element with an extremely low diffusion coefficient and is an element that has a high affinity for Si (which easily forms a compound or cluster with Si). Consequently, Mo, which is stable in a dissolved state, promotes the formation of Si clusters, so that the amount of σ-phase formed is increased, thereby maximizing the precipitation-strengthening effect of the σ-phase obtained by adding Si and significantly improving the high-temperature creep strength.

[0043] The Mo content is 0.05 to 0.7 mass%. If the Mo content is less than 0.05 mass%, the σ phase is not sufficiently formed, and the effect of σ phase precipitation is not sufficiently provided. If the Mo content exceeds 0.7 mass%, the amount of a coarse Al-Mo-Mg-based crystallized material is increased, resulting in a problem of deterioration of high-temperature creep strength. The lower limit of the Mo content is preferably 0.05 mass% or more, more preferably 0.1 mass% or more, even more preferably 0.15 mass% or more, even more preferably 0.2 mass% or more. The lower limit of the Mo content may be 0.3 mass% or more. The upper limit of the Mo content is preferably 0.6 mass% or less, 0.55 mass% or less, 0.5 mass% or less, or 0.4 mass% or less.

[0044] The aluminum alloy material according to another embodiment of the present invention preferably has a Si content of 0.1 to 0.6 mass% and a Mo content of 0.3 to 0.7 mass%.

[0045] The aluminum alloy material of another embodiment of the present invention preferably has a Si content of 0.35 to 0.8 mass% and a Mo content of 0.05 to 0.55 mass%.

[0046] When the Si content and Mo content are within the above ranges, the effect of improving the high-temperature creep strength is more likely to be provided. (Ti: 0.01 to 0.3 mass%)

[0047] Ti is an element that is effective for refining the crystal grains.

[0048] The Ti content is in a range of 0.01 to 0.3 mass%. If the Ti content is less than 0.01 mass%, the effect of stabilizing a fine crystal grain structure is not sufficiently provided. If the Ti content exceeds 0.1 mass%, for example, a coarse Ti-based compound is formed, resulting in a reduction in high-temperature creep strength. The lower limit of the Ti content is preferably 0.02 mass% or more, more preferably 0.04 mass% or more. The upper limit of the Ti content is preferably 0.15 mass% or less, more preferably 0.09 mass% or less. (Remainder: Al and incidental impurities)

[0049] The remainder of the aluminum alloy material according to one embodiment of the present invention is Al and incidental impurities. The incidental impurities are impurities that, in practical operation, originate, for example, from the raw materials used or are randomly mixed in during the melting of the raw materials. Examples of the incidental impurities include Zn, Mn, Cr, Zr, and V.

[0050] One or two or more of these may be included as long as the advantages of the present invention are not impaired. The contents of Zn, Mn, Cr, Zr, and V mentioned as the above examples are each preferably 0.15 mass% or less. Even if the aluminum alloy material according to one embodiment of the present invention contains each of Zn, Mn, Cr, Zr, and V in an amount of 0.15 mass% or less, the advantages of the present invention are not impaired. [Minimal creep rate]

[0051] The aluminum alloy material according to an embodiment of the present invention preferably has a minimum creep rate of 8.5 × 10- 10 / s or less at 160 °C and 250 MPa.

[0052] The minimum creep rate can be determined by a uniaxial high-temperature creep rate tensile test according to JIS Z 2271:2010. For the high-temperature creep rate test, the test conditions are set such that the temperature is 160 °C and the load is 250 MPa, and the test is conducted by holding the test temperature for 1.5 hours or more and then applying the test load.

[0053] A creep rate corresponding to the "slope" of the relationship between test time and creep strain obtained in the high-temperature creep rate test is calculated, and the smallest creep rate can be determined as the minimum creep rate. A lower value of the minimum creep rate represents better high-temperature creep strength.

[0054] As described above, the aluminum alloy material according to an embodiment of the present invention has a predetermined alloy composition and therefore excellent high-temperature creep strength can be provided. <Verfahren zur Herstellung eines Aluminiumlegierungsmaterials>

[0055] Next, an embodiment of a method for producing an aluminum alloy material according to an embodiment of the present invention will be described. In the following description of the manufacturing method, detailed explanations of the items already described are omitted.

[0056] The method for producing an aluminum alloy material according to the present embodiment is a method for producing the aluminum alloy material having the above-mentioned alloy composition, and includes performing melt-adjusting a molten metal having the alloy composition, casting, homogenization treatment, hot working, solution treatment, quenching, and aging treatment in this order.

[0057] In particular, the method for producing an aluminum alloy material according to the embodiment is a method for producing an aluminum alloy material having an alloy composition including: Cu: 1.5 to 6.0 mass%, Mg: 1.0 to 4.0 mass%, Fe: 0.5 to 2.0 mass%, Ni: 0.5 to 2.0 mass%, Si: 0.1 to 3.0 mass%, Mo: 0.05 to 0.7 mass%, and Ti: 0.01 to 0.3 mass%, the remainder being Al and incidental impurities, the process comprising: Performing melting of a molten metal having the above alloy composition, casting, homogenization treatment, hot working (plastic working), solution treatment, quenching, and aging treatment in this order.

[0058] The method for producing an aluminum alloy material according to the present invention, that is, melting of a molten metal, casting, homogenization treatment, hot working, solution treatment, quenching and aging treatment can be carried out under general conditions for an aluminum alloy material made of, for example, an AA2618 aluminum alloy.

[0059] Hereinafter, the case where the hot working is forging is described as an example, but the hot working may be any of forging, extrusion, rolling, forming rolling, compression molding, and the like.

[0060] For example, the melting of the molten metal can be carried out at 700 °C to 900 °C.

[0061] The homogenization treatment can be performed at 450 °C to 550 °C. However, when the Cu concentration is about 2.7% or more, eutectic melting may occur, and therefore, it is preferable to set the homogenization treatment temperature to a low value within the above range.

[0062] Forging can be carried out at temperatures between 200 °C and 500 °C. Solution treatment can be carried out at temperatures between 500 °C and 550 °C.

[0063] Quenching can be carried out using water or oil at a temperature of 90 °C to 100 °C, but can also be carried out with water or typical heat treatment oil at room temperature (about 25 °C).

[0064] The aging treatment can be carried out at 170 °C to 220 °C.

[0065] Specifically, this manufacturing method can be performed by T6 treatment or T61 treatment, and is preferably performed by T61 treatment. Under the above manufacturing conditions, this manufacturing method can produce the aluminum alloy material according to the embodiment. It should be noted that this manufacturing method is not limited to the general conditions described here as examples.

[0066] The method for producing an aluminum alloy material according to the embodiment is as described above; however, with respect to conditions not explicitly described, known conditions may be employed in each of the above processes, and the conditions may be appropriately changed as long as the effect obtained by the treatment is achieved in each process. [Aluminum alloy parts]

[0067] The aluminum alloy materials according to the embodiments can be subjected to hot working to provide near-net-shape shapes, followed by machining to produce rotary parts and direct-acting parts (aluminum alloy parts), such as drive wheels or impellers for engines, compressors and turbochargers.

[0068] As described above, the following subjects are disclosed herein. [1] Aluminium alloy material having an alloy composition containing: Cu: 1.5 to 6.0 mass%, Mg: 1.0 to 4.0 mass%, Fe: 0.5 to 2.0 mass%, Ni: 0.5 to 2.0 mass%, Si: 0.1 to 3.0 mass%, Mo: 0.05 to 0.7 mass%, and Ti: 0.01 to 0.3 mass%, the remainder being Al and incidental impurities. [2] Aluminium alloy material having an alloy composition containing: Cu: 1.9 to 3.0 mass%, Mg: 1.3 to 3.0 mass%, Fe: 0.9 to 1.3 mass%, Ni: 0.9 to 1.3 mass%, Si: 0.25 to 0.8 mass%, Mo: 0.05 to 0.5 mass%, and Ti: 0.04 to 0.09 mass%, the remainder being Al and incidental impurities. [3] Aluminium alloy material according to [1] or [2], wherein the contents of Si and Mo Si: 0.1 to 0.6 mass% and Mo: 0.3 to 0.7 mass%. [4] Aluminium alloy material according to [1] or [2], wherein the contents of Si and Mo Si: 0.35 to 0.8 mass% and Mo: 0.05 to 0.55 mass%. [5] An aluminum alloy material according to any one of [1] to [4], wherein the aluminum alloy material has a minimum creep rate of 8.5 × 10- 10 / s or less at 160 °C and 250 MPa. [6] A method for producing an aluminum alloy material, the method being a method for producing the aluminum alloy material having the alloy composition according to any one of [1] to [5], the method comprising performing melt-setting of a molten metal having the alloy composition, casting, homogenization treatment, hot working, solution treatment, quenching, and aging treatment in this order. EXAMPLES

[0069] The present invention will be described more specifically below with reference to examples and comparative examples; however, the present invention is not limited to these examples. The present invention can be implemented in various modifications without departing from the gist of the present invention, and such modifications are all included within the technical scope of the present invention. (Examples and comparison examples)

[0070] Small ingots with the compositions (balance: Al and incidental impurities) shown in Tables 1 and 2, each having a mass of about 1.6 kg, were produced by "ingot casting," in which casting was carried out by pouring a molten metal made of an aluminum alloy into a mold with dimensions of 170 mm × 110 mm × 28 mm.

[0071] The concentration of each element was analyzed by plasma emission spectrometry.

[0072] The ingots were each held at 500 °C for 12 hours as a homogenization treatment, then formed into a rectangular material with dimensions of 40 mm × 40 mm by hammer forging, including one reheating, and subjected to a T61 treatment of holding at 530 °C for 6 hours, followed by immersion water cooling at 90 °C and aging treatment at 200 °C for 22 hours, followed by natural cooling, so that aluminum alloy materials Nos. 1 to 11 were produced, which are used as sample materials. (Measurement of the minimum creep rate)

[0073] To evaluate the mechanical properties, a uniaxial high-temperature creep rate tensile test was performed according to JIS Z 2271:2010.

[0074] The test was carried out using a single-type creep testing machine and the creep strain during the test was also measured combined with a dial gauge strain gauge.

[0075] A test specimen has a round bar shape with a total length of 80 mm and was made by cutting from the above-mentioned rectangular material, and has a measuring section with a projecting edge, the measuring section having dimensions with a length of φ6 mm × 30 mm and gripping sections with an M12 screw shape.

[0076] The test conditions were set so that the temperature was 160 °C and the load was 250 MPa. After maintaining the test temperature for 1.5 hours or more, the test load was applied to start the test.

[0077] A creep rate corresponding to the "slope" of the relationship between test time and creep strain obtained in the creep rate test was calculated, and the smallest creep rate was determined as the minimum creep rate. A smaller value of the minimum creep rate represents better high-temperature creep strength. A minimum creep rate of 8.5 × 10 -10 / s or less was considered a pass (o), and a minimum creep rate exceeding this was considered a failure (x). It should be noted that these pass or failure criteria correspond to a threshold that means the fatigue life is approximately 1.7 times that of existing materials when used under the same conditions.

[0078] The above results are shown in Tables 1 and 2. [Table 1]

[0079] As shown in Table 1, the aluminum alloy materials Nos. 1 to 4, which correspond to examples of the present invention, exhibited excellent high-temperature creep strength. The aluminum alloy materials Nos. 5 to 7 correspond to comparative examples in which the Mo content is outside the range specified in the present invention. It is considered that in the aluminum alloy materials Nos. 5 to 7, the formation of the σ phase was not promoted and precipitation hardening did not occur sufficiently, resulting in high minimum creep rates, that is, poor high-temperature creep strength. [Table 2] Table 2

[0080] As shown in Table 2, the aluminum alloy materials of Nos. 8 and 9, which are examples of the present invention, exhibited excellent high-temperature creep strength. The aluminum alloy material of No. 10 corresponds to a comparative example in which the Mo content is outside the range specified in the present invention. It is presumed that in the aluminum alloy material of No. 10, the Mo concentration was insufficient and consequently the σ phase was not sufficiently precipitated, resulting in a high minimum creep rate, that is, poor high-temperature creep strength. The aluminum alloy material of No. 11 corresponds to a comparative example in which the Si content is outside the range specified in the present invention. Presumably, in the aluminum alloy material of No.11, because the Si concentration was excessive, a fine precipitated structure such as the S phase, which an aluminum alloy material with an Al-Cu-Mg composition originally exhibits, was inhibited and a basic hardening mechanism was impaired, resulting in a high minimum creep rate, that is, poor high-temperature creep strength.

[0081] It has been demonstrated that aluminum alloy materials having excellent high-temperature creep strength can be provided because the aluminum alloy materials according to embodiments of the present invention have predetermined alloy compositions.

[0082] Although various embodiments have been described above, it is to be understood that the present invention is not limited to these examples.

[0083] It is clear that a person skilled in the art can make various variations and modifications within the scope defined in the claims, and it is understood that such variations and modifications are also encompassed by the technical scope of the present invention. The components in the above embodiments can be freely combined without departing from the essence of the invention.

[0084] This application is based on a Japanese patent application (No. 2022-027200) filed on February 24, 2022, and a Japanese patent application (No. 2022-182576) filed on November 15, 2022, the contents of which are incorporated herein by reference. QUOTES CONTAINED IN THE DESCRIPTION

[0000] This list of documents submitted by the applicant was generated automatically and is included solely for the convenience of the reader. This list is not part of the German patent or utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature

[0000] 2022-027200

[0084] 2022-182576

[0084] Cited non-patent literature

[0000] JIS Z 2271:2010

[0052] < / aluminiumlegierungsmaterial>

Claims

[1] An aluminum alloy material comprising an alloy composition containing: Cu: 1.5 to 6.0 mass%, Mg: 1.0 to 4.0 mass%, Fe: 0.5 to 2.0 mass%, Ni: 0.5 to 2.0 mass%, Si: 0.1 to 3.0 mass%, Mo: 0.05 to 0.7 mass%, and Ti: 0.01 to 0.3 mass%, the remainder being Al and incidental impurities. [2] An aluminum alloy material comprising an alloy composition containing: Cu: 1.9 to 3.0 mass%, Mg: 1.3 to 3.0 mass%, Fe: 0.9 to 1.3 mass%, Ni: 0.9 to 1.3 mass%, Si: 0.25 to 0.8 mass%, Mo: 0.05 to 0.5 mass%, and Ti: 0.04 to 0.09 mass%, the remainder being Al and incidental impurities. [3] An aluminum alloy material according to claim 1 or 2, wherein contents of Si and Mo Si: 0.1 to 0.6 mass% and Mo: 0.3 to 0.7 mass%. [4] An aluminum alloy material according to claim 1 or 2, wherein the contents of Si and Mo Si: 0.35 to 0.8 mass% and Mo: 0.05 to 0.55 mass%. [5] An aluminum alloy material according to claim 1 or 2, wherein the aluminum alloy material has a minimum creep rate of 8.5 × 10- 10 / s or less at 160 °C and 250 MPa. [6] A method for producing an aluminum alloy material, the method being a method for producing the aluminum alloy material having the alloy composition according to claim 1 or 2, the method comprising performing melt-setting of a molten metal having the alloy composition, casting, homogenization treatment, hot working, solution treatment, quenching, and aging treatment in this order.

Citation Information

Patent Citations

  • Power storage module

    JP2022027200A

  • Suspended scaffold construction method and device for construction

    JP2022182576A

  • method of manufacturing aluminum alloy sheet

    CH468472A

  • JP002013014835A

  • JP002013142168A