USE OF PHOSPHORUS GROUP CONTAINING COPOLYMERS FOR THE PROTECTION OF METALS AND FOR LUBRICATION

DE602016090176T2Active Publication Date: 2024-11-06SPECIALTY OPERATIONS FRANCE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602016090176
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2015-05-04
Filing Date
2016-05-04
Publication Date
2024-11-06
Estimated Expiration
2036-05-04

AI Technical Summary

Technical Problem

Current lubricating additives, such as phosphonate compounds like LUBRHOPHOS LB-400, do not provide sufficient or durable lubrication and anti-corrosion protection for metal surfaces, particularly under extreme pressure conditions and in repeated contact scenarios.

Method used

The use of specific copolymers obtained by radical copolymerization of phosphorus-containing monomers and hydrophobic monomers, with a high number of phosphorus groups, in naphthenic or paraffinic oils, which provide both lubricating and anti-corrosion effects.

Benefits of technology

These copolymers offer enhanced lubrication and anti-wear properties, reducing metal/metal friction and inhibiting corrosion, especially on aluminum surfaces, while allowing for reduced phosphorus content to comply with regulatory requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to the field of lubricant additives for metals, which are intended to be incorporated in particular: in compositions intended to limit metal / metal friction during occasional metal shaping operations (for example, lubricating compositions for extreme pressure wire drawing or metal cutting compositions); and / or in compositions intended to limit the wear of metal parts intended to be brought into contact repeatedly (oil compositions for engines or gearboxes, typically).

[0002] The aforementioned lubricant additives are generally added to lubricant formulations based on paraffinic or similar oil for metal forming applications. For engine oil or gearbox oil applications, the lubricant formulation that incorporates the lubricant additives is typically based on naphthenic oil or polyalphaolefins (PAO), poly(alkylene glycols) or esters.

[0003] As an example of lubricant additives for metal of the aforementioned type, mention may in particular be made of compounds carrying a phosphonate terminal group, and in particular the additive LUBRHOPHOS ®< LB-400 (polyoxyethylene octadecenyl ether phosphate) available from the company Solvay.

[0004] Documents WO 2006 / 125892, WO 2008 / 012248, US 2008 / 233390 and US 5,191,029 disclose (co)polymers which can be obtained by radical (co)polymerization of at least ethylenically unsaturated monomers carrying phosphorus groups, as well as their use as a protective (anti-corrosion) agent for metal in aqueous phase or in emulsions.

[0005] Documents EP 1 489 158, US 2 956 952, US 3 243 417 and US 3 151 078 disclose oil-soluble copolymers carrying phosphorus groups, as well as their use in lubricating oils as lubricants, in particular as extreme pressure additives.

[0006] An aim of the present invention is to provide lubricating additives ensuring a greater and / or more lasting lubricating effect than that obtained with phosphonate compounds of the LUBRHOPHOS LB-400 type.

[0007] To this end, the present invention proposes the use of specific copolymers based on several units carrying phosphorus groups and hydrophobic units.

[0008] In the context of the present invention, the inventors have demonstrated that these copolymers can be used as a lubricant for metal and to provide a protective effect, in particular an anti-wear effect and an anti-corrosion protection treatment on the surface of metals (temporary passivation effect or more lasting anti-corrosion effect in particular on aluminum surfaces).

[0009] More specifically, according to a first aspect, the invention relates to the use, as a lubricant for metal and as a protective agent for metal in a naphthenic or paraffinic type oil, of a copolymer as obtained by radical copolymerization of a mixture comprising: of the monomersm1, also called “phosphorus monomers”, ethylenically unsaturated and carrying phosphorus groups of monomers m2, also called “hydrophobic monomers”, carrying a saturated or unsaturated hydrocarbon chain, preferably an alkyl or alkenyl group, typically comprising 8 to 30 carbon atoms, these m2 monomers generally being non-phosphorus.

[0010] The copolymers of the invention are typically usable to provide a lubricating effect, in particular to limit metal / metal friction during occasional metal shaping operations (for example during wire drawing of metals under extreme pressure or during metal cutting) and / or to limit the wear of metal parts intended to be brought into contact repeatedly (typically engines or gearboxes).

[0011] The copolymers of the invention simultaneously provide a protective effect on metal surfaces, in particular a passivation effect, and their deposition on the surface of metal surfaces (steel, aluminum, copper or brass for example) makes it possible to reduce, or even completely inhibit, corrosion phenomena.

[0012] According to a specific aspect, the invention relates to lubricating compositions comprising at least one copolymer of the aforementioned type, in a mixture with a paraffinic oil or a naphthenic oil.

[0013] The work carried out by the inventors within the framework of the present invention has now made it possible to demonstrate that the copolymers obtained by radical copolymerization of the mixture of the aforementioned monomers m1 and m2 prove to be particularly effective in ensuring a lubricating effect on a metal surface.

[0014] A particularly interesting effect has been identified by the inventors for the copolymers according to the invention which comprise a large number of phosphorus groups, and this in particular when the monomers m1 are VPA (vinylphosphonic acid) monomers. For this purpose, it is preferable for a copolymer according to the invention to comprise at least 2 phosphorus groups per chain, for example at least 3 and preferably at least 5, more preferably at least 8 and even more preferably at least 10. This number of phosphorus groups per copolymer can typically be between 5 and 50, for example between 10 and 40. It does not generally have to exceed 20 to obtain interesting results, but it can be higher. According to a particular embodiment, it is between 5 and 30. For example, it may typically be between 10 and 15, for example of the order of 12. Alternatively, it may be between 15 and 35, for example of the order of 25 to 30.

[0015] The number of phosphorus groups referred to here typically corresponds to an average number of phosphorus groups across all the chains of the copolymer considered. This number of phosphorus groups per chain can typically be established from: of the ratio m1 / m2 corresponding to the molar ratio of the quantity of monomers m1 to the quantity of monomers m2, which can be obtained in particular by NMR, in particular by proton and / or carbon NMR, and by the conversion rate of the monomers m1, which can be determined in particular by phosphorus NMR; and of the molar mass of the copolymer (which can be determined by any means known per se and in particular by the methods described below in the present description and the examples) knowing the molecular mass and the molar ratio of the 2 monomers, we can go back to the average degree of polymerization in phosphorus units.

[0016] Furthermore, it is preferable that the size of the copolymers according to the invention is as small as possible. Typically, it is preferred that the number-average molecular mass of a copolymer used according to the invention is less than 100 kg / mol, more preferably less than 60 kg / mol, for example between 5 and 50, and more preferably between 10 and 40 kg / mol, and more advantageously between 10 and 30 kg / mol, for example of the order of 20 kg / mol.

[0017] However, it is most often preferable that the number-average molecular mass of a copolymer used according to the invention is not too low, in particular so as to be able to more easily control the number of phosphorus groups per chain. For this purpose, it is most often preferred that the number-average molecular mass remains greater than or equal to 5 kg / mol, more preferably 10 kg / mol.

[0018] In general, for a given number of phosphorus groups per chain, there is an optimal number molecular mass, typically between 10 and 40 kg / mol, for which the copolymer proves particularly effective.

[0019] The number average molecular weight referred to in this specification is the theoretical number average molecular weight of the copolymer, which is calculated as the overall ratio of the total mass of monomers theoretically incorporated into the polymer (which is equal to the sum of the products of the mass of each monomer used in the manufacture of the copolymer multiplied by the conversion of said monomer), divided by the total number of copolymer chains.

[0020] At constant mass, the more the number of phosphorus groups per chain increases, the more it is possible to use the copolymer in a diluted manner. With a relatively low number of phosphorus groups per chain, typically 2 or 3, the copolymers of the invention can be used typically in the same concentration ranges as LUBRHOPHOS LB-400, or even at slightly lower levels, with at least similar performances. When the number of phosphorus groups per chain increases (typically when it is greater than 5, and even more so when it is at least 8, and even more so when it is at least 10), the copolymers according to the invention are generally much more effective than LUBRHOPHOS LB-400, even when used in smaller quantities. The copolymers of the invention constitute an excellent alternative to LUBRHOPHOS LB-400.Another advantage is that, by reducing the polymer content, the phosphorus content can be reduced, in line with regulatory requirements (which notably require, in 2016, less than 800 ppm of phosphorus in engine oils in Europe and North America).

[0021] Various features and embodiments of the invention will now be described in more detail. ▪ m1 monomers

[0022] The phosphorus monomers m1 constituting the copolymers according to the invention are unsaturated monomers carrying at least one phosphorus group.

[0023] The phosphorus group is preferably an acid -P(OH) 2 (=O) (phosphonic acid when the phosphorus is linked directly to a carbon or phosphoric acid when it is linked via an oxygen and is then written -OP(OH) 2 (=O) possibly in whole or in part in a deprotonated form, namely: hydrogen phosphonate: -P(O -< )(OH)(=O); and / or hydrogen phosphate: -OP(O -< )(OH)(=O); and / or phosphonate: -P(O -< )(O -< )(=O); and / or phosphate: -OP(O -< )(O -< )(=O).

[0024] The m1 monomers are typically vinylphosphonic acid (VPA) monomers.

[0025] Alternatively, the monomers m1 may carry a phosphate ester group -OP(OA)(OB)(=O) or a phosphonate ester group -P(OA)(OB)(=O) where A and B are alkyl groups, identical or different, typically comprising from 1 to 4 carbon atoms (methyl or ethyl for example). In this context, vinyl acid esters may be used as all or part of the monomers m1, such as for example diallyl dimethylammoniummethyl phosphonate (DALP). ▪ m2 monomers

[0026] The hydrophobic monomers m2 can vary to a large extent, as long as they are monomers copolymerizable in radical polymerization with the phosphorus monomers m1.

[0027] In a non-limiting manner, the monomers m2 can for example be chosen from: acrylic acid esters, of formula: CH 2 =CH-C(=O)-OR h where R h is a saturated or unsaturated hydrocarbon chain, preferably an alkyl or alkenyl group, typically comprising 8 to 30 carbon atoms methacrylic acid esters, of formula: CH 2 =C(CH 3 )-C(=O)-OR h where R h is a saturated or unsaturated hydrocarbon chain, preferably an alkyl or alkenyl group, typically comprising 8 to 30 carbon atoms allyl ethers, of formula: CH 2 =CH-COR h where R h is a saturated or unsaturated hydrocarbon chain, preferably an alkyl or alkenyl group, typically comprising 8 to 30 carbon atoms metallyl ethers, of formula: CH 2 =C(CH 3 )-COR h where R h is a saturated or unsaturated hydrocarbon chain, preferably an alkyl or alkenyl group, typically comprising 8 to 30 carbon atoms, alkenes such as butylenes and isobutylene.

[0028] According to an interesting embodiment, the monomers m2 can for example be 2-ethylhexyl esters of acrylic acid (2-ethylhexyl acrylate called “2EHA”). ▪ Preparation of the copolymers according to the invention

[0029] The copolymers useful according to the invention can be prepared according to any radical polymerization process using the monomers m1 and m2 as a mixture.

[0030] The copolymers used according to the invention are typically statistical copolymers based on the monomers m1 and m2, it being understood that they may have concentration gradients in said monomers, in particular taking into account the difference in reactivity between the monomers.

[0031] In general, the copolymers according to the invention are not block copolymers, although this embodiment is not excluded from the scope of the invention.

[0032] According to a possible embodiment, the copolymers according to the invention are prepared by controlled radical copolymerization of a mixture comprising the monomers m1 and m2.

[0033] "Controlled radical polymerization" is a technique well known in itself, which makes it possible, using a polymerization control agent, to obtain polymers of controlled masses and in particular block polymers in which both the architecture and the size of each of the blocks can be controlled. Controlled radical polymerization processes well suited to the synthesis of the copolymers useful according to the invention are the so-called RAFT or MADIX processes, which typically implement a reversible transfer process by addition-fragmentation using control agents (also called reversible transfer), for example of the xanthate type (compounds carrying functions - SC=SO-). As examples of such methods, mention may in particular be made of those described in WO96 / 30421, WO 98 / 01478, WO 99 / 35178, WO 98 / 58974, WO 00 / 75207, WO 01 / 42312, WO 99 / 35177, WO 99 / 31144, FR2794464 or WO 02 / 26836.

[0034] These controlled radical polymerization processes lead in a well-known manner to the formation of polymer chains which all grow at approximately the same speed, which results in a substantially linear increase in molecular masses with the conversion and a tight mass distribution, with a number of chains which typically remains approximately fixed throughout the duration of the reaction, which makes it possible to very easily control the average molar mass of the synthesized polymer (the initial monomer / control agent ratio defines the degree of polymerization obtained for the synthesized chains). The chains obtained also generally have a "living" character: they have at the end of the chain the reactive group present on the control agent.It is therefore possible to continue the polymerization on the polymer chain obtained, while retaining the controlled nature of the polymerization, which can in particular be used to synthesize at the end of a first polymer block of controlled size another block of different composition and also of controlled size.

[0035] In a controlled radical polymerization of the aforementioned type, the size of the polymer being formed is controlled by the monomer / control agent molar ratio corresponding to the initial quantity of monomers relative to the quantity of control agent: schematically, all the chains grow from each of the control agents present and the monomers are distributed homogeneously over all the growing chains. The monomer / control agent molar ratio therefore dictates the degree of polymerization of the block synthesized in each of the stages, and therefore makes it possible to define the theoretical number-average molecular mass expected for each of the blocks.

[0036] According to an advantageous embodiment, the useful copolymer according to the invention is prepared by bringing into contact: ethylenically unsaturated monomers m1 and m2 a source of free radicals; and a radical polymerization control agent.

[0037] Any known source of free radicals can be used. This could be, for example, one of the following initiators: hydrogen peroxides such as: tertiary butyl hydroperoxide, cumene hydroperoxide, t-butyl peroxyacetate, t-butyl peroxybenzoate, t-butylperoxyoctoate, t-butylperoxyneodecanoate, t-butylperoxyisobutarate, lauroyl peroxide, t-amylperoxypivalte, t-butylperoxypivalate, dicumyl peroxide, benzoyl peroxide, potassium persulfate, ammonium persulfate, azo compounds such as: 2-2'-azobis(isobutyronitrile), 2,2'-azobis(2-butanenitrile), 4,4'-azobis(4-pentanoic acid), 1,1'-azobis(cyclohexanecarbonitrile), 2-(t-butylazo)-2-cyanopropane, 2,2'-azobis[2-methyl-N-(1,1)-bis(hydroxymethyl)-2-hydroxyethyl]propionamide, 2,2'-azobis(2-methyl-N-hydroxyethyl]-propionamide, 2,2'-azobis(N,N'-dimethyleneisobutyramidine) dichloride, 2,2'-azobis(2-amidinopropane) dichloride, 2,2'-azobis(N,N'-dimethyleneisobutyramide), 2,2'-azobis(2-methyl-N-[1,1-bis (hydroxymethyl)-2-hydroxyethyl] propionamide), 2,2'-azobis(2-methyl-N-[1,1-bis (hydroxymethyl)ethyl] propionamide), 2,2'-azobis[2-methyl-N-(2-hydroxyethyl) propionamide], 2,2'-azobis(isobutyramide) dihydrate, redox systems comprising combinations such as: mixtures of hydrogen peroxide, alkyl, peresters, percarbonates and the like and any of the iron salts, titanium salts, zinc formaldehyde sulfoxylate or sodium formaldehyde sulfoxylate, and reducing sugars, alkali metal or ammonium persulfates, perborate or perchlorate in combination with an alkali metal bisulfite, such as sodium metabisulfite, and reducing sugars, and alkali metal persulfates in combination with an acid arylphosphinic acid, such as benzenephosphonic acid and the like, and reducing sugars.

[0038] Particularly in the case of polymerizations carried out in an aqueous medium, it may be possible to consider using a redox-type radical initiator, which has the advantage of not requiring heating of the reaction medium (no thermal initiation), which makes it possible to better manage the exothermicity of the reaction.

[0039] Thus, the source of free radicals used can typically be chosen from the redox initiators conventionally used in radical polymerization, typically not requiring heating for their initiation. It is typically a mixture of at least one oxidizing agent with at least one reducing agent.

[0040] Possible redox systems include combinations such as: mixtures of water-soluble persulfates with water-soluble tertiary amines, mixtures of water-soluble bromates (e.g., alkali metal bromate) with water-soluble sulfites (e.g., alkali metal sulfites), mixtures of hydrogen peroxide, alkyl peresters, percarbonates and the like and any of the iron salts, titanium salts, zinc formaldehyde sulfoxylate or sodium formaldehyde sulfoxylate, and reducing sugars, alkali metal or ammonium persulfates, perborate or perchlorate in combination with an alkali metal bisulfite, such as sodium metabisulfite, and reducing sugars, and alkali metal persulfates in combination with an arylphosphinic acid, such as benzenephosphonic acid and the like, and reducing sugars.

[0041] An interesting redox system includes (and preferably consists of) for example the combination of ammonium persulfate and sodium formaldehyde sulfoxylate.

[0042] When the copolymer of the invention is prepared according to a controlled radical polymerization process, its theoretical number-average molecular mass can be easily approximated by the total mass of the incorporated monomers relative to the number of control agents introduced, according to the formula given in the attached examples. The number-average molecular mass, in this case, can be quite easily measured experimentally, typically by proton NMR (by integrating the proton NMR signal characteristic of a termination of the polymer provided by the control agent and relating it to the contribution of the signals integrating the entire chain, according to a method known per se - phosphorus NMR allows access to the conversion rate of the monomers m1).

[0043] The nature of the control agent can vary widely. According to an interesting variant, the control agent used is a compound carrying a thiocarbonylthio group -S(C=S)-. According to a particular embodiment, the control agent can carry several thiocarbonylthio groups.

[0044] More generally, a control agent suitable for the synthesis of the polymer (P) useful according to the invention advantageously corresponds to formula (A) below: in which: Z represents: . a hydrogen atom, . a chlorine atom, . an optionally substituted alkyl radical, optionally substituted aryl radical, . an optionally substituted heterocycle, . an optionally substituted alkylthio radical, . an optionally substituted arylthio radical, . an optionally substituted alkoxy radical, . an optionally substituted aryloxy radical, . an optionally substituted amino radical, . an optionally substituted hydrazine radical, . an optionally substituted alkoxycarbonyl radical, . an optionally substituted aryloxycarbonyl radical, . a carboxy radical, optionally substituted acyloxy radical, . an optionally substituted aroyloxy radical, . an optionally substituted carbamoyl radical, . a cyano radical, . a dialkyl- or diaryl-phosphonato radical, . a dialkyl-phosphinato or diaryl-phosphinato radical, or . a polymer chain, and R 1 represents: . an optionally substituted alkyl, acyl, aryl, aralkyl, alkene or alkyne group, .a carbon cycle or a heterocycle, saturated or not, aromatic optionally substituted, or . a polymer chain. .

[0045] The R 1 or Z groups, when substituted, may be substituted by optionally substituted phenyl groups, optionally substituted aromatic groups, saturated or unsaturated carbon rings, saturated or unsaturated heterocycles, or groups: alkoxycarbonyl or aryloxycarbonyl (-COOR), carboxy (-COOH), acyloxy (-O 2 CR), carbamoyl (-CONR 2 ), cyano (-CN), alkylcarbonyl, alkylarylcarbonyl, arylcarbonyl, arylalkylcarbonyl, phthalimido, maleimido, succinimido, amidino, guanidimo, hydroxy (-OH), amino (-NR 2 ), halogen, perfluoroalkyl C n F 2n+1 , allyl, epoxy, alkoxy (-OR), S-alkyl, S-aryl, groups having a hydrophilic or ionic character such as alkali salts of acids carboxylic acids, alkali salts of sulfonic acid, polyalkylene oxide chains (PEO, POP), cationic substituents (quaternary ammonium salts), R representing an alkyl or aryl group, or a polymer chain.

[0046] According to a particular embodiment, R 1 is a substituted or unsubstituted alkyl group, preferably substituted.

[0047] The optionally substituted alkyl, acyl, aryl, aralkyl or alkyne groups generally have 1 to 20 carbon atoms, preferably 1 to 12, and more preferably 1 to 9 carbon atoms. They can be linear or branched. They can also be substituted by oxygen atoms, in particular in the form of esters, sulfur or nitrogen atoms.

[0048] Among the alkyl radicals, we can notably cite the methyl, ethyl, propyl, butyl, pentyl, isopropyl, tert-butyl, pentyl, hexyl, octyl, decyl or dodecyl radical.

[0049] Alkyne groups are radicals generally of 2 to 10 carbon atoms, they have at least one acetylenic unsaturation, such as the acetylenyl radical.

[0050] The acyl group is a radical generally having from 1 to 20 carbon atoms with a carbonyl group.

[0051] Among the aryl radicals, we can notably cite the phenyl radical, possibly substituted in particular by a nitro or hydroxyl function.

[0052] Among the aralkyl radicals, we can notably cite the benzyl or phenethyl radical, optionally substituted in particular by a nitro or hydroxyl function.

[0053] When R 1 or Z is a polymer chain, this polymer chain can be derived from a radical or ionic polymerization or from a polycondensation.

[0054] In the context of the present invention, it is particularly advantageous to use xanthates, trithiocarbonates, dithiocarbamates, or dithiocarbazates as control agents.

[0055] Advantageously, compounds carrying a xanthate function -S(C=S)O- are used as control agent, for example carrying an O-ethyl xanthate function of formula -S(C=S)OCH 2 CH 3 , such as for example O-ethyl-S-(1-methoxycarbonyl ethyl) xanthate of formula (CH 3 CH(CO 2 CH 3 ))S(C=S)OEt.

[0056] Another possible control agent in step (E) is dibenzyltrithiocarbonate of formula PhCH 2 S(C=S)SCH 2 Ph (where Ph=phenyl).

[0057] A copolymer resulting from a controlled radical polymerization of the aforementioned type carries at the end of the chain a reactive group giving it a living character.

[0058] According to one embodiment, the copolymer useful according to the invention is a copolymer directly resulting from a controlled radical polymerization.

[0059] Alternatively, the copolymer used in the context of the invention may be obtained from a controlled radical polymerization step followed by a polymer deactivation step, this step being able to be carried out according to any method known per se, for example by ozonolysis or by reaction with peracetic acid. A usable deactivation method is for example described in application WO 2005 / 040233.

[0060] By way of example, a particularly interesting copolymer according to the invention is a copolymer of VPA and 2EHA obtained by controlled radical copolymerization using O-ethyl-S-(1-methoxycarbonyl ethyl) xanthate as polymerization control agent, having 12 VPA units per chain and a number-average molecular weight of 20 kg / mol. The inventors have shown that this polymer makes it possible to obtain very good lubricating properties. More generally, polymers obtained by controlled radical copolymerization using O-ethyl-S-(1-methoxycarbonyl ethyl) xanthate as polymerization control agent, having from 10 to 15 VPA units per chain and a number-average molecular weight of 10 to 40 kg / mol have good lubricating properties.

[0061] According to another embodiment, the copolymers of the invention can be prepared by radical polymerization in the absence of a control agent. The polymers obtained by uncontrolled radical copolymerization, having from 8 to 50 units, in particular from 10 to 40 VPA units per chain and a number-average molecular mass of 10 to 40 kg / mol, have good lubricating properties. They also prove to be, most often, thermally stable and typically retain their properties, in particular lubricating properties, even when subjected to temperatures of 100°C for several days (which typically corresponds to the conditions of use of a lubricating oil in a gearbox). They can be treated at higher temperatures, for several days at 150°C (which reflects the conditions of use of an engine oil).Typically, they retain their properties substantially even after two days of heat treatment, or even after 5 days or more (as shown in the examples).

[0062] The number-average molecular mass in the case of polymers prepared by an uncontrolled radical route can be measured in particular by size exclusion chromatography (SEC) possibly coupled with a measurement of the radius of gyration by light scattering (typically MALLS-type laser scattering).

[0063] Regardless of their preparation process, whether by controlled radical or uncontrolled radical route, the polymers of the invention can be synthesized in a continuous, batch or semi-batch mode. It is particularly advantageous to synthesize them in continuous mode, which allows, among other things, to more finely regulate the incorporation of phosphorus groups within their structure. ▪ Lubricating compositions comprising the copolymer according to the invention

[0064] The lubricating compositions according to the present invention comprise a polymer of the aforementioned type, in a paraffinic or naphthenic oil, with optionally other additives.

[0065] The copolymer according to the invention is typically present at a rate of 0.2 to 5% by mass relative to the total mass of the composition and the copolymer is typically present at a rate of 0.4% to 2% by mass, for example between 0.5 and 2% by mass. In particular when the number of phosphorus groups per chain is high (above 5, in particular greater than or equal to 8, or even 10), the copolymer can advantageously be used at a concentration of 0.4% to 1% by mass relative to the total mass of the composition.

[0066] According to a particular embodiment, a lubricating composition according to the invention may be a composition for cutting metal or for drawing wire under high pressure (in which case the copolymer is typically in a paraffinic type oil).

[0067] According to another embodiment, the lubricating composition according to the invention is an engine oil or a gearbox oil. In this case, the copolymer is typically in a naphthenic type oil.

[0068] For applications as lubricants, it is preferable to limit the mass of the copolymers used (in particular to prevent them from inducing too significant an increase in the lubricating compositions in which they are used). In this perspective, it will therefore be advantageous to use copolymers with a mass of less than 80 kg / mol, more preferably less than 60 kg / mol and even less than 50 kg / mol, or even 40 kg / mol. ▪ Protective compositions comprising the copolymer according to the invention

[0069] The protective compositions, and in particular passivating or anti-corrosion compositions, according to the present invention comprise a polymer of the aforementioned type, and are intended to be applied to the surface of metals to ensure a protective effect - temporary or more lasting - of the surface, in particular against corrosion.

[0070] In these compositions, the polymer is generally carried in a solvent, which may for example be an oil, with possibly other additives.

[0071] The invention will now be illustrated by the following examples, in which copolymers of vinylphosphonic acid and 2-ethylhexyl acrylate according to the invention were prepared and the performances of which were evaluated by extreme pressure FALEX tests. Example 1: Synthesis of a random copolymer of vinylphosphonic acid and 2-ethylhexyl acrylate (2EHA) by controlled radical polymerization

[0072] control agent: O-ethyl-S-(1-methoxycarbonyl ethyl) xanthate initiator: 2,2'-Azobis(2-methylbutyronitrile) VPA: 15 mol% - 2EHA: 85 mol% M n = 19,700 g mol -1< )

[0073] In a 6L jacketed reactor equipped with a condenser and mechanical stirring, 164.3 g of vinylphosphonic acid (85.4% purity), 1320.7 g of 2-ethylhexyl acrylate, 3409 g of ethyl acetate and 15.64 g of O-ethyl-S-(1-methoxycarbonyl ethyl) xanthate of formula CH 3 CH(CO 2 CH 3 ))SC(=S)OEt were introduced at room temperature (20°C). The mixture was degassed by bubbling nitrogen for 60 minutes corresponding to the heating time of the reactor for a temperature set at 70°C. After 15 minutes (stabilization of the reactor temperature at 70°C) and still under nitrogen flow, 3.6 g of AMBN initiator (2,2'-azobis(2-methylbutyronitrile)) was added to the medium in one go, in the form of a solution in ethyl acetate at 8.2% by mass. After 180 minutes of stirring at 70°C, 3.6 g of AMBN initiator, in solution in ethyl acetate at 4.3% by mass, was added over 3 hours.At the end of the addition, 3.6 g of AMBN initiator are again added to the reaction medium, all at once, in the form of a solution in ethyl acetate at 8.2% by mass. The reaction is then continued for another 11 hours. At the end of the polymerization, a sample is taken to be analyzed by 1< H and 31< P NMR and thus obtain the conversions into monomers.

[0074] After cooling the reaction mixture, the ethyl acetate solvent is then gradually removed by evaporation under reduced pressure and at the same time replaced by NYFLEX 800 naphthenic oil until a final mass concentration of the copolymer in the oil equal to 50% is obtained. Conversion of VPA monomer (31< P NMR) = 79% Conversion of 2-EHA monomer (1< H NMR) = 96% Number average molar mass: 18.6 kg·mol -1< (18,600 g / mol)

[0075] The average molar mass of the copolymer (theoretical average mass as defined in this description) was calculated according to the following formula (where the number of polymer chains directly resulting from the decomposition of the initiator is neglected in the denominator): M ‾ n théo = m 1 0 × M m 1 × Conv . m 1 + m 2 0 × M m 2 × Conv . m 2 X 0 + M x Or: M n(theo) = the number-average molar mass according to the present description [m1] 0 and [m2] 0 - the initial concentrations of monomers m1 and m2 respectively [X] 0 = the initial concentration of control agent M m1 and M m2 = the molar masses of the monomers m1 and m2 respectively Conv.(m1) and Conv.(m2) - the conversions of the monomers m1 and m2 respectively (reaction yield) M X = the molar mass of the control agent Example 2: Synthesis of a copolymer of vinylphosphonic acid and 2-ethylhexyl acrylate by conventional radical polymerization initiator: 2,2'-Azobis(2-methylbutyronitrile)

[0076] VPA = 17 mol % − 2 EHA = 83 mol %

[0077] In a 2L jacketed reactor equipped with a condenser and mechanical stirring, 84.2 g of vinylphosphonic acid (85.4% purity), 88.5 g of 2-ethylhexyl acrylate (15% of its total mass to be added) and 795 g of ethyl acetate were introduced at room temperature (20°C). The mixture was degassed by bubbling nitrogen while the reactor was heating up to a temperature set at 70°C. Once the temperature set was reached, 1.6 g of AMBN initiator (2,2'-azobis(2-methylbutyronitrile)) was added to the medium in one go, in the form of a solution in ethyl acetate at 8% by mass. After addition, the remaining 85% of 2-ethylhexyl acrylate (501.4 g), dissolved in ethyl acetate at 60% by mass, is added continuously over 10 hours. After 180 minutes of reaction with stirring at 70°C, 1.6 g of AMBN initiator, dissolved in ethyl acetate at 2% by mass, is added continuously over 7 hours.At the end of the addition, a final addition of 1.6 g of AMBN initiator is made in one go in the form of a solution in ethyl acetate at 8% by mass. The reaction is then continued for another 11 hours. At the end of the polymerization, a sample is taken to be analyzed by 1< H and 31< P NMR and thus obtain the conversions into monomers.

[0078] After cooling the reaction mixture, the ethyl acetate solvent is then gradually removed by evaporation under reduced pressure and at the same time replaced by NYFLEX 800 naphthenic oil until a final mass concentration of the copolymer in the oil equal to 30% is obtained. Conversion of VPA monomer (31< P NMR) = 84% Conversion of 2-EHA monomer (1< H NMR) = 98% Number average molecular mass: 31.2 kg / mol (31200 g·mol -1< )

[0079] In this, the number-average (theoretical) molar mass was calculated according to the following formula, taking into account the amount of decomposed initiator. M ‾ n théo = m 1 0 × M m 1 × Conv . m 1 + m 2 0 × M m 2 × Conv . m 2 I 2 cons . + M l2 2 Or: M n(theo) = the average molar mass in the sense of the present description [m1] 0 and [m2] 0 - the initial concentrations of monomers m1 and m2 respectively [I 2 ] cons . = the concentration of initiator actually consumed during the polymerization M m1 and M m2 = the molar masses of the monomers m1 and m2 respectively Conv.(m1) and Conv.(m2) - the conversions of the monomers m1 and m2 respectively (reaction yield) M l2 = the molar mass of the initiator Example 3 : Performance of the copolymers of examples 1 and 2 in the extreme pressure FALEX test

[0080] The polymers synthesized in Examples 1 and 2 were tested on a Falex tribometer (of the "pin and V blocks" type) where a small cylindrical metal specimen is placed between two "V" jaws, immersed in the lubricating composition to be tested, and subjected to an increasing breaking load until it breaks. The polymers were used as additives at different concentrations in a naphthenic oil (concentrations given as a mass percentage of polymer relative to the total mass of the lubricating composition).

[0081] The tests were carried out on freshly prepared compositions, as well as on heat-treated compositions, i.e. placed at 100°C or 150°C as the case may be for one or more days.

[0082] For comparison, we also tested the LUBRHOPHOS LB-400

[0083] Table 1 below shows, in non-bold, the value of the breaking load, expressed in Ibs (when the table indicates “>3000” it means that there was no break at the maximum value of 3000 Ibs) for the different tests.

[0084] The mass loss of the test piece, which reflects wear, is also reported in parentheses in the case where there has been no rupture (the table thus shows a general effect observed for the polymers of the invention, namely that they provide an anti-wear effect in addition to a lubricating effect). Table 1 Additive used Aging Concentration 0.75% 0.5% 0.4% Witness : Lubrophos LB400 - 600 600 <500 Polymer of Example 1 - >3000 (loss: 100 mg) >3000 (loss: 200 mg) 2450 Polymer of Example 2 >3000 (loss: 30 mg) >3000 (loss: 40 mg) >3000 (loss: 60 mg) 24h - 150°C >3000 (loss: 35 mg) >3000 (loss: 55 mg) 2710 48h - 150°C >3000 (loss: 70 mg) 2700 Not tested 6 days - 150°C >3000 (loss: 120 mg) 2470 Not tested 10 days - 150°C >3000 (loss: 200 mg) 1980 Not tested 48h - 100°C >3000 (loss: 45 mg) >3000 (loss: 60 mg) 2870 6 days - 100°C >3000 (loss: 50 mg) >3000 (loss: 60 mg) 2720 14 days - 100°C >3000 (loss: 55 mg) >3000 (loss: 80 mg) 2450 Example 4 : Comparative performance of copolymers according to the invention in extreme pressure FALEX test

[0085] Polymers were produced according to the protocol of Example 1 by modifying the number of VPA groups per chain (n VPA ) and the molecular mass (Mn expressed in kg / mol ). Table 2 below reflects the values ​​of the breaking loads in Ibs (in non-bold in the table) obtained in the Falex test (under the same conditions as Example 3). Table 2 Additive concentration in lubricant (naphthenic oil + additive) 2% 1% 0.75% 0.5% 0.4% 0.25% Witness LB400 900 600 600 500 Not tested Not tested n VPA =8 Mn=10 >3000 >3000 900 1000 Not tested Not tested n VPA =8 Mn=20 >3000 >3000 800 600 Not tested Not tested n VPA =8 Mn=30 >3000 1200 700 600 Not tested Not tested n VPA =8 Mn=40 >3000 1500 700 500 Not tested Not tested n VPA =8 Mn=50 1200 1200 700 500 Not tested Not tested n VPA =12 Mn=20 >3000 >3000 >3000 2700 2700 600 n VPA =15 Mn=20 >3000 >3000 >3000 2700 2700 700

Claims

1. Use of a copolymer capable of being obtained by radical copolymerization of a mixture comprising: - monomers m1 which are ethylenically unsaturated and which carry phosphorus groups, - monomers m2 which carry a saturated or unsaturated hydrocarbon chain, as protective agent for metals and lubricating agent for metals in a naphthenic or paraffinic oil.

2. Use according to Claim 1, where the copolymer comprises at least 2 phosphorus groups per chain, preferably at least 5.

3. Use according to Claim 2, where the copolymer comprises between 10 and 15 phosphorus groups per chain.

4. Use according to one of Claims 1 to 3, where the copolymer has a number-average molecular weight of less than 60 kg / mol, for example between 5 and 50.

5. Use according to Claim 4, where the copolymer has a number-average molecular weight between 10 and 40 kg / mol, preferably between 10 and 30 kg / mol.

6. Use according to one of Claims 1 to 5, where the phosphorus group carried by the monomers m1 is a - P(OH)2(=O) or -O-P(OH)2(=O) group, optionally in all or part in a deprotonated form, or else a -P(OA)(OB)(=O) or -O-P(OA) (OB) (=O) group where A and B are identical or different alkyl groups.

7. Use according to Claim 6, where the monomers m1 are vinylphosphonic acid (VPA) monomers.

8. Use according to one of Claims 1 to 7, where the monomers m2 are chosen from: - acrylic acid esters, of formula:         CH2=CH-C(=O)-O-Rh - methacrylic acid esters, of formula:         CH2=C(CH3)-C(=O)-O-Rh where Rh is a saturated or unsaturated hydrocarbon chain, preferably an alkyl or alkenyl group, typically comprising from 8 to 30 carbon atoms.

9. Use according to one of Claims 1 to 7, where the copolymer of use according to the invention is prepared by bringing into contact: - the ethylenically unsaturated monomers m1 and m2, - a source of free radicals, and - optionally, an agent for controlling the radical polymerization.