BIOCOMPATIBLE MATRIX PRODUCT COMPRISING A POLYSACCHARIDE AND CO-RETICULAR CHITOSAN
A biocompatible matrix product with co-crosslinked polysaccharides and chitosan, enhanced by a divalent zinc cation, addresses viscosity loss after heat treatment, ensuring effective use in cosmetic and medical applications.
Patent Information
- Application Number
- FR2021004295
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-04-26
AI Technical Summary
Existing biocompatible products, such as those based on crosslinked hyaluronic acid, suffer from significant viscosity loss after heat treatment, which is necessary for sterilization, limiting their effectiveness in cosmetic and medical applications.
A biocompatible matrix product comprising a polysaccharide co-crosslinked with chitosan and containing a divalent zinc cation, which enhances viscosity and maintains it after heat treatment.
The solution significantly increases viscosity and maintains it after sterilization, improving durability and effectiveness in filling, replacing, or supplementing biological tissues and fluids.
Smart Images

Figure 00000026_0000 
Figure 00000027_0000
Abstract
Description
Title of the invention: BIOCOMPATIBLE MATRIX PRODUCT COMPRISING A POLYSACCHARIDE AND CHITOSAN CO-RETICULES TECHNICAL FIELD OF THE INVENTION
[0001] The present invention relates to the field of biocompatible products for cosmetic and / or medical, particularly surgical, purposes. It relates more specifically to a biocompatible product with a matrix comprising a polysaccharide at least partially co-crosslinked with chitosan, preferably a chitosan derivative or a chitosan salt.
[0002] For a number of years now, there has been a growing interest in products enabling the filling, replacement, increase in volume of a biological tissue and / or the replacement, supplementation of a biological fluid, both in the cosmetic field and in the medical field.
[0003] Thus, for example, the use of products enabling the increase in volume of a biological tissue is particularly interesting in the cosmetic field, to treat wrinkles and fine lines but also to redefine the contours of the face, of the body.
[0004] Volume augmentation, filling, biological tissue replacement, or biological fluid replacement and supplementation products may also be useful in the medical field.
[0005] For example, prior art discloses the use of products intended to supplement synovial fluid in patients with joint degeneration. Such products most often contain hyaluronic acid.
[0006] There are also known so-called "viscoelastic" products which are used in ophthalmic surgeries to replace or supplement the aqueous humor (during cataract surgery or in the context of refractive surgery) or the vitreous humor (in the case of a vitrectomy), as described in US document 4,716,154.
[0007] The rheological properties of the product are of particular importance.
[0008] A number of biocompatible products, particularly those containing cross-linked hyaluronic acid or a salt of cross-linked hyaluronic acid, have been used to fill, replace, or augment the volume of biological tissue and / or to replace or supplement biological fluid. However, some of these products cannot be used effectively in either cosmetic or medical applications due to undesirable side effects and / or limited efficacy.
[0009] The effectiveness of some of these products could be improved by giving them higher rheological properties, and also by limiting the risks of degradation of their rheological properties.
[0010] It is particularly useful and important, for many applications, that the product has a high viscosity, especially at low shear rates.
[0011] Products based on crosslinked hyaluronic acid or crosslinked hyaluronic acid salt exhibit a relatively satisfactory viscosity after crosslinking.
[0012] However, the viscosity of these products tends to decrease significantly after heat treatment. These products must be sterilized before use in humans or animals, and this sterilization is generally achieved by heat treatment (for example, using an autoclave). Description of the invention
[0013] One problem proposed by the present invention is to provide a biocompatible product that allows for better filling, replacing, increasing the volume of a biological tissue and / or replacing, supplementing a biological fluid.
[0014] Simultaneously, the invention aims to provide such a product exhibiting improved rheological properties, particularly in terms of viscosity after application of a heat treatment such as sterilization.
[0015] To achieve these and other objectives, the invention proposes a biocompatible matrix product comprising: - a polysaccharide selected from the group comprising hyaluronic acid, a salt of hyaluronic acid, chondroitin sulfate, cellulosic derivatives, and a mixture thereof, - chitosan, preferably a chitosan derivative or a chitosan salt, and in which: - in said matrix, at least a portion of the polysaccharide is co-crosslinked with at least a portion of the chitosan, chitosan derivative, or chitosan salt, - a divalent zinc cation is present in the matrix.
[0016] For the purposes of this invention, "biocompatible product" means any product which is well tolerated by a living organism and which does not cause rejection, toxic reaction, injury or adverse effect on the biological functions of the latter.
[0017] By "chitosan derivative" is meant a substituted chitosan having a substitution of the D-glucosamine and / or N-acetyl-D-glucosamine units, and in which the substitution group is covalently linked.
[0018] The applicant has observed that co-crosslinking of a polysaccharide (selected from the group comprising hyaluronic acid, a hyaluronic acid salt, chondroitin sulfate, cellulosic derivatives, and a mixture thereof) with chitosan, a A chitosan derivative or chitosan salt, which leads to the formation of covalent bonds between the polysaccharide and chitosan within the matrix, significantly increases the viscosity of the product compared to the cross-linked polysaccharide. However, the applicant also observed that the viscosity of said co-cross-linked product remained highly susceptible to degradation following heat treatment such as autoclaving.
[0019] It was in this context that the applicant was surprised to discover that the co-crosslinking of a polysaccharide (chosen from the group including hyaluronic acid, a hyaluronic acid salt, chondroitin sulfate, cellulosic derivatives, and a mixture thereof) with chitosan, a chitosan derivative, or a chitosan salt, combined with the presence of a divalent zinc cation, not only significantly increases the viscosity of the product, but also effectively limits the decrease in this viscosity after heat treatment such as autoclaving. This reduced decrease in viscosity also suggests improved durability and a better ability to fill, replace, or augment the volume of biological tissue and / or replace or supplement a biological fluid.
[0020] According to a first possibility, the divalent zinc cation can be introduced by adding a zinc saccharide to be cross-linked within the matrix. For the purposes of this invention, "cross-linked within the matrix" means a bond to at least one of the matrix constituents by at least two covalent bonds.
[0021] According to another possibility, the divalent zinc cation can be introduced by adding a zinc saccharide to be grafted into the matrix. For the purposes of this invention, "grafted into the matrix" means a bond to at least one of the matrix constituents by a covalent bond.
[0022] According to yet another possibility, the divalent zinc cation can preferably be dispersed in the matrix. "Dispersed in the matrix" means the absence of covalent bonding to the matrix constituents. Dispersion of the divalent zinc cation in the matrix has yielded excellent results in terms of viscosity. Moreover, the manufacturing process is simpler than when adding zinc for crosslinking or grafting, because zinc (in the form of zinc salt or zinc saccharide, in particular) has relatively poor solubility in the pH range required for crosslinking or grafting.
[0023] Advantageously, for a good increase in viscosity, the concentration of divalent zinc cation in the matrix can be between 0.001% and 1% by weight relative to the total weight of the matrix.
[0024] Preferably, in order to maintain good transparency of the product for applications requiring it (particularly in the ophthalmological field or for in (jetions near the skin surface), the concentration of divalent zinc cation in the matrix may be less than or equal to 0.1% by weight relative to the total weight of the matrix.
[0025] Advantageously, the concentration of divalent zinc cation in the matrix can be between 0.002% and 0.06% by weight relative to the total weight of the matrix. With such a concentration, the applicant observed with great surprise but also great interest that the viscosity of the product according to the invention after heat treatment (such as autoclaving) remains high, can be close to its viscosity before heat treatment, or may even be higher than its viscosity before heat treatment.
[0026] Preferably, the divalent zinc cation can be incorporated into the matrix by adding a zinc salt or a zinc saccharide, preferably zinc gluconate, zinc chloride, or zinc sulfate. Zinc gluconate promotes a product with good transparency, particularly for applications requiring it (notably in ophthalmology or for injections near the skin surface). Zinc chloride and zinc sulfate have proven useful for applications in rheumatology, orthopedic surgery, and for the treatment of osteoarthritis or the repair of cartilage defects.
[0027] Advantageously, it can be predicted that: - the concentration of the polysaccharide chosen from the group including hyaluronic acid, a hyaluronic acid salt, chondroitin sulfate, cellulosic derivatives, and a mixture thereof, is between 0.01% and 3% by weight relative to the total weight of the matrix, and / or - the concentration of chitosan, chitosan derivative, or chitosan salt is between 0.01% and 3% by weight relative to the total weight of the matrix.
[0028] Preferably, the chitosan derivative can be a carboxyalkyl chitosan. In particular, good results have been obtained with carboxymethyl chitosan.
[0029] Carboxyalkyl chitosan refers to a chitosan containing glucosamine units, N-acetylglucosamine units, and glucosamine units substituted by a carboxyalkyl group. It is thus referred to as a chitosan derivative or substituted chitosan.
[0030] Advantageously, the polysaccharide can be hyaluronic acid or a salt of hyaluronic acid, and can preferably have a molecular weight between 0.1 and 5 MDa.
[0031] According to another aspect of the present invention, a cosmetic or pharmaceutical composition is proposed comprising a biocompatible product as previously described. This cosmetic or pharmaceutical composition may be in the form of a viscoelastic solution or a hydrogel.
[0032] Advantageously, the cosmetic or pharmaceutical composition may include a physiologically acceptable buffer, preferably containing polyols (mannitol, sorbitol, glycerol) and / or phospholipids.
[0033] Preferably, said composition can be used in a cosmetic treatment method or therapeutic treatment method, including in particular topical application, implantation, instillation or injection by subcutaneous, intradermal, mucosal, ocular, intraocular, or intra-articular route, of said composition.
[0034] Advantageously, said composition can be used for the prevention and / or treatment of pathologies that can be improved or avoided by: - the filling or replacement of biological tissue; and / or - the increase in volume of said biological tissue; and / or - the supplementation or replacement of a biological fluid.
[0035] Preferably, said composition can be used for a method of treating osteoarthritis, or repairing a cartilage defect, the composition being, for example, formulated for administration by injection into the synovial fluid or for implantation into the cartilage after mixing with blood, or for a method of treating dry eye.
[0036] Advantageously, said composition can be used in a method of treatment in therapeutic, surgical, or cosmetic applications, including in particular treatment in rheumatology, ophthalmology, gynecology, aesthetic medicine, plastic surgery, internal surgery, orthopedic surgery, for the prevention of post-surgical tissue adhesions, and in dermatology.
[0037] More particularly preferred, the composition can be used in the therapeutic treatment of dry eye syndrome, corneal lesions, or ocular or joint inflammation.
[0038] Advantageously, said composition can be used in a therapeutic treatment in which said composition is applied by instillation onto the ocular surface to prevent or combat corneal injury or dry eye syndrome, in particular for the purpose of lubricating or regenerating the ocular surface.
[0039] According to another aspect of the present invention, a composition of eye drops is proposed comprising a biocompatible product as previously described.
[0040] According to another aspect of the present invention, a method for manufacturing a biocompatible product as previously described or a composition as previously described is proposed, said method comprising the following steps: a. Dissolve in the same aqueous solution: i. a polysaccharide selected from the group comprising hyaluronic acid hyaluronic acid, a salt of hyaluronic acid, chondroitin sulfate, cellulosic derivatives, and a mixture thereof, preferably hyaluronic acid or a salt of hyaluronic acid, ii. chitosan, preferably a chitosan derivative, or a chitosan salt, b. add a crosslinking agent to said aqueous solution and cause crosslinking of the mixture to form a matrix, c. Add a divalent zinc cation before and / or after step b.
[0041] It should be noted that the invention is not limited to a particular covalent crosslinking method, but a method using a chemical molecule serving as a crosslinking agent, also called a crosslinking agent, such as 1,4-butanediol diglycidyl ether (BDDE) or polyethylene glycol diglycidyl ether (PEGDE) in particular may be preferred.
[0042] When the divalent zinc cation is added before step b, this addition can be in the form of a zinc saccharide, for crosslinking and / or grafting into the matrix, or can be in the form of a zinc salt which will be dispersed in the matrix.
[0043] When the divalent zinc cation is added after step b, this addition is in the form of zinc salt or zinc saccharide which is dispersed in the matrix.
[0044] The two previous possibilities of adding divalent zinc cation can be combined.
[0045] Advantageously, the pH of the biocompatible product or composition can be adjusted between 6 and 8, preferably to 7.
[0046] Preferably, the biocompatible product or composition can be subjected to a sterilization heat treatment, preferably a heat treatment at a temperature between 120°C and 140°C for a duration of between 1 and 20 minutes.
[0047] Other objects, features and advantages of the invention will become clear to those skilled in the art upon reading the explanatory description which refers to examples and embodiments which are given only by way of illustration and which shall in no way limit the scope of the claims.
[0048] The examples and embodiments form an integral part of the present invention and any feature which appears new in relation to any prior art from the description taken as a whole, including the examples and embodiments, forms an integral part of the invention in its function and in its generality.
[0049] Thus, each example or embodiment has a general scope.
[0050] On the other hand, in the examples or embodiments, all percentages are Given in niasse, unless otherwise stated, temperature is expressed in degrees Celsius unless otherwise stated, and pressure is atmospheric pressure unless otherwise stated. SUMMARY DESCRIPTION OF THE DRAWINGS
[0051] Other objects, features and advantages of the present invention will become apparent from the following description of particular embodiments, made in relation to the accompanying figures, among which:
[0052] [Fig-1] Fig.1 is a histogram of the viscosities of different formulations, measured before and after heat treatment; and
[0053] [Fig. 2] Figure 2 is a graph illustrating the evolution of viscosities of different formulations and different products on the market as a function of shear rate. DESCRIPTION OF PREFERRED EMBODIMENTS
[0054] Materials: - sodium hyaluronate (NaHa) from bio fermentation, - carboxymethyl chitosan (CMCS) with a degree of acetylation less than 10% (expressed as the number of moles of N-acetylglucosamine units relative to the number of moles of total units) and a degree of substitution of 80% (expressed as the number of moles of the substituent relative to the number of moles of total units), - 1,4-butanediol diglycidyl ether (BDDE), - polyethylene glycol diglycidyl ether (PEGDE), - zinc gluconate (ZnGluc), - zinc chloride (ZnC12), - zinc sulfate (ZnSO4), - sodium chloride (NaCl), - physiological tampon, - hydrochloric acid (HCl), - sodium hydroxide (NaOH), - dialysis membranes.
[0055] Preparation of a physiological buffer solution
[0056] A physiological buffer solution is prepared in deionized water to achieve a pH between 6 and 8 and an osmolarity between 250 and 350 mOsm / L.
[0057] Synthesis of a cross-linked phase comprising a polysaccharide (namely acid hyaluronic acid or a hyaluronic acid salt)
[0058] To simplify the reader's understanding, hyaluronic acid or a hyaluronic acid salt is designated by "HA". The cross-linking of HA is achieved by dissolving HA (for example, hyaluronate). sodium hydroxide (NaHA) is dissolved in a 0.25 mol / L aqueous sodium hydroxide solution until completely solubilized. A crosslinking agent (e.g., BDDE or PEGDE) is then added and mixed to homogenize. The mixture is hermetically sealed and placed in a 50°C water bath for 3 hours to induce a crosslinking reaction of the HA. Covalent bonds are thus created between the crosslinking agent and the HA. Bridges can therefore be formed between two HA chains. The gel is then homogenized and neutralized in a container with the addition of an aqueous hydrochloric acid solution to form a homogeneous and transparent phase. Dialysis is then performed to remove the residual crosslinking agent and to stabilize the pH and osmolarity.
[0059] Synthesis of a cross-linked phase comprising a polysaccharide (namely hyaluronic acid or a hyaluronic acid salt) with chitosan, a chitosan derivative, or a chitosan salt
[0060] To simplify the reader's understanding, hyaluronic acid or a salt of hyaluronic acid is designated by "HA", while chitosan, a chitosan derivative or a chitosan salt is designated by "CHITO".
[0061] The crosslinking of HA with CHITO is carried out by dissolving the HA (e.g., sodium hyaluronate (NaHa)) and a CHITO (e.g., a carboxyalkyl chitosan) in a 0.25 mol / L aqueous sodium hydroxide solution until completely dissolved. A crosslinking agent (e.g., BDDE or PEGDE) is then added and mixed to homogenize. The mixture is hermetically sealed and placed in a water bath at 50°C for 3 hours to induce a simultaneous crosslinking (or co-crosslinking) reaction of the HA and the CHITO. "Simultaneous crosslinking" or "co-crosslinking" means that covalent bonds can be formed between the crosslinking agent and the HA, but also between the crosslinking agent and the CHITO. Bridges can thus be formed between two HA chains, between two CHITO chains, or between an HA chain and a CHITO chain.The gel is then homogenized and neutralized in a container with the addition of an aqueous hydrochloric acid solution to form a homogeneous and transparent phase. Dialysis is then performed to remove the residual crosslinking agent and to stabilize the pH and osmolarity.
[0062] Synthesis of a linear (non-crosslinked) phase of a polysaccharide (namely hyaluronic acid or hyaluronic acid salt) with a divalent zinc cation (and with, where appropriate, chitosan, a chitosan derivative or a chitosan salt)
[0063] To simplify the reader's understanding, hyaluronic acid or a hyaluronic acid salt is designated as "HA", while chitosan, a chitosan derivative or a chitosan salt is designated as "CHITO".
[0064] HA, taken alone or with a CHITO, is dissolved in a physicochemical buffer solution The solution is stirred until completely solubilized to form a transparent viscoelastic solution. A divalent zinc cation can be added by incorporating (dispersing) a zinc salt or zinc saccharide (in particular zinc gluconate, zinc chloride, or zinc sulfate) into the solution. A mixing action allows the zinc salt to dissolve and homogenize in the linear phase.
[0065] Heat treatment
[0066] Each formulation undergoes a heat treatment corresponding to a sterilization cycle. This heat treatment is carried out in an HMT 260 MB laboratory autoclave from HMC EUROPE. The sterilization plateau, lasting 1 minute, is set at a temperature of 131°C. The total time of the heat treatment, including heating, plateau, and cooling, is approximately 22 to 23 minutes.
[0067] Method for measuring viscosity
[0068] Rheological characterizations are performed using a Discovery “DHR2” hybrid rheometer from TA Instruments, equipped with a 40 mm diameter cone-plate geometry with a 2-degree angle and a 55-micron truncation. The rheometer is also equipped with a Peltier plate to control the sample temperature during measurement.
[0069] During a measurement, the sample is placed on the lower plate and the geometry is lowered until it reaches the trim gap (105 µm). The excess product is removed using a spatula. Then, the geometry is lowered to 55 µm from the lower plate.
[0070] The method used consists of a flow ramp at 35°C applying a shear rate varying between 1 s 1 and 1000 s1, with 5 points per decade.
[0071] The viscosities for comparing the different formulations are then taken from the viscosity value corresponding to a shear rate of 8.6 s1.
[0072] Test No. 1: Formulation of a biocompatible product with a crosslinked HA matrix, without divalent zinc cation present in the matrix
[0073] A formulation of HA is prepared comprising a cross-linked HA phase. The final concentration of HA is 0.9% by weight relative to the total weight of the matrix.
[0074] The cross-linked phase of HA is prepared as previously described.
[0075] First, 1.12 g of sodium hyaluronate (NaHA) is weighed and dissolved in 8.7 g of 0.25 mol / L aqueous sodium hydroxide solution. After complete dissolution, the crosslinking agent is added dropwise to the solution. Mixing is performed to homogenize the reaction medium and ensure homogeneous crosslinking. The container holding the mixture is then hermetically sealed and placed in a water bath at 50°C for 3 hours. The gel is then stored overnight between 2°C and 8°C.
[0076] The following day, 9.58 g of gel is collected and placed in a homogenizer, in To which 87.4 g of concentrated aqueous hydrochloric acid (HCl) solution (24 mmol / L) is added. The medium is homogenized using a shearing mixer, resulting in rapid swelling and pH neutralization. The homogenized and neutralized medium is collected and then transferred into closed dialysis membranes using forceps. These membranes are then placed in a buffer solution for a minimum of 24 hours.
[0077] The biocompatible cross-linked matrix product thus obtained is then transferred into 1 mL glass syringes.
[0078] The glass syringes are then subjected to heat treatment as previously described, by passing them through an autoclave with a sterilization tray for a duration of 1 minute at 131°C. The total duration of the heat treatment, including heating, the tray, and cooling, is approximately 22 to 23 minutes.
[0079] The viscosity of the biocompatible cross-linked matrix product obtained (formulation 1) is measured as described previously.
[0080] Test No. 2: Formulation of a biocompatible product with a crosslinked HA matrix, with a divalent zinc cation present in the matrix
[0081] A HA formulation is prepared comprising 90% of a crosslinked HA phase and 10% of a non-crosslinked (linear) HA-based phase. The HA concentration is 0.9% by weight relative to the total weight of the matrix. A divalent zinc cation is added by dispersion in the matrix.
[0082] The crosslinked phase of HA is prepared as previously described in connection with test No. 1.
[0083] In parallel, a linear phase is prepared as previously described.
[0084] 0.21 g of sodium hyaluronate (NaHa) is weighed out, to which 20.0 g of solution is added buffer, and a mixture is made.
[0085] The crosslinked phase and the linear (non-crosslinked) phase are then mixed in a 9:1 ratio. A divalent zinc cation is added to the matrix by incorporating zinc gluconate solution (using a dispersion). Mixing allows the zinc salt to dissolve and homogenize in the linear phase.
[0086] Several concentrations of divalent zinc cation are carried out, namely: 0.0022% (formulation 2a), 0.0072% (formulation 2b) and 0.0144% (formulation 2c) by weight relative to the total weight of the matrix.
[0087] The resulting biocompatible cross-linked matrix product is then transferred into 1 mL glass syringes.
[0088] The glass syringes are then subjected to heat treatment as previously described, by passing them through an autoclave with a sterilization tray of a The duration is 1 minute at 131°C. The total time for the heat treatment, including heating, plateau and cooling, is approximately 22 to 23 minutes.
[0089] The viscosity of the biocompatible cross-linked matrix product obtained (formulations 2a, 2b and 2c) is measured as described above.
[0090] Test No. 3: Formulation of a biocompatible product with a co-crosslinked HA and CHITO matrix, without divalent zinc cation present in the matrix
[0091] A formulation of HA and CHITO is prepared comprising 90% of a co-crosslinked HA-CHITO phase. The concentrations of HA and CHITO are respectively 0.9% and 0.1% by weight relative to the total weight of the matrix.
[0092] The cross-linked phase of HA-CHITO is prepared as follows.
[0093] First, 2.00 g of sodium hyaluronate (NaHA) is weighed out. Then, 0.215 g of carboxymethyl chitosan is weighed out and added to the sodium hyaluronate. The mixture of carboxymethyl chitosan and sodium hyaluronate is dissolved in 20 g of 0.25 mol / L aqueous sodium hydroxide solution. After complete dissolution, the crosslinking agent is added dropwise to the solution. Mixing is performed to homogenize the reaction medium and allow for homogeneous co-crosslinking (or simultaneous crosslinking). Next, the container holding the mixture is hermetically sealed and placed in a water bath at 50°C for 3 hours. The gel is then stored overnight between 2°C and 8°C.
[0094] The following day, 22.02 g of gel is collected and placed in a homogenizer, to which 175.4 g of concentrated aqueous hydrochloric acid (HCl) at 28 mmol / L is added. The medium is homogenized using a shearing mixer, resulting in rapid swelling and pH neutralization. The homogenized and neutralized medium is collected and then transferred into closed dialysis membranes using forceps. These membranes are then placed in a buffer solution for a minimum of 24 hours.
[0095] In parallel, a linear phase is prepared as previously described, with HA and CHITO.
[0096] 0.20 g of sodium hyaluronate (NaHa) and 22 mg of carboxymethyl chitosan are mixed, to which 20.0 g of buffer solution is added. A mixture is made.
[0097] The crosslinked and linear (non-crosslinked) phases are then mixed in a ratio of 9:1.
[0098] The resulting biocompatible cross-linked matrix product is then transferred into 1 mL glass syringes.
[0099] The glass syringes are then subjected to heat treatment as previously described, by passing them through an autoclave with a sterilization tray for a duration of 1 minute at 131°C. The total duration of the heat treatment, including heating, the tray, and cooling, is approximately 22 to 23 minutes.
[0100] The viscosity of the biocompatible cross-linked matrix product obtained (formulation 3) is measured as described previously.
[0101] Test No. 4: Formulation of a biocompatible product with a co-crosslinked HA and CHITO matrix, with a divalent zinc cation present in the matrix by addition of zinc gluconate
[0102] A formulation of HA and CHITO is prepared comprising 90% of a co-crosslinked HA-CHITO phase and 10% of a non-crosslinked (linear) HA-CHITO-based phase. The concentrations of HA and CHITO are 0.9% and 0.1% by weight, respectively, relative to the total weight of the matrix.
[0103] The crosslinked phase of HA-CHITO is prepared as previously described in connection with test No. 3.
[0104] In parallel, a linear phase with HA and CHITO is prepared as previously described in connection with Test No. 3, except that after complete dissolution of sodium hyaluronate (NaHA) and carboxymethyl chitosan, a divalent zinc cation is added to the matrix by incorporation into the zinc gluconate solution (using a dispersion). A mixture is then used to dissolve and homogenize said zinc salt in the linear phase.
[0105] Several concentrations of divalent zinc cation are carried out, namely: 0.0072% (formulation 4a) and 0.0144% (formulation 4b) by weight relative to the total weight of the matrix.
[0106] The crosslinked and linear (non-crosslinked) phases are then mixed in a ratio of 9:1.
[0107] The biocompatible cross-linked matrix product thus obtained is then transferred into 1 mL glass syringes.
[0108] The glass syringes are then subjected to heat treatment as previously described, by passing them through an autoclave with a sterilization tray for a duration of 1 minute at 131°C. The total duration of the heat treatment, including heating, the tray and cooling, is approximately 22 to 23 minutes.
[0109] The viscosity of the biocompatible cross-linked matrix product obtained (formulations 4a and 4b) is measured as described previously.
[0110] Test No. 5: Formulation of a biocompatible product with a co-crosslinked HA and CHITO matrix, with a divalent zinc cation present in the matrix by addition of zinc chloride
[0111] A formulation of HA and CHITO is prepared comprising 90% of a co-crosslinked HA-CHITO phase and 10% of a non-crosslinked (linear) HA-CHITO-based phase. The concentrations of HA and CHITO are 0.9% and 0.1% respectively by weight relative to the total weight of the matrix.
[0112] The cross-linked phase of HA-CHITO is prepared as previously described in relation with essay No. 4.
[0113] In parallel, a linear phase with HA and CHITO is prepared as previously described in connection with Test No. 4, except that after complete dissolution of sodium hyaluronate (NaHA) and carboxymethyl chitosan, a divalent zinc cation is added to the matrix by incorporation into the zinc chloride (ZnCl2) solution (using a dispersion). A mixture is then used to dissolve and homogenize said zinc salt in the linear phase.
[0114] Several concentrations of divalent zinc cation are carried out, namely: 0.0072% (formulation 5a), 0.0144% (formulation 5b) and 0.048% (formulation 5c) by weight relative to the total weight of the matrix.
[0115] The crosslinked and linear (non-crosslinked) phases are then mixed in a ratio of 9:1.
[0116] The biocompatible cross-linked matrix product thus obtained is then transferred into 1 mL glass syringes.
[0117] The glass syringes are then subjected to heat treatment as previously described, by passing them through an autoclave with a sterilization tray for a duration of 1 minute at 131°C. The total duration of the heat treatment, including heating, the tray, and cooling, is approximately 22 to 23 minutes.
[0118] The viscosity of the biocompatible cross-linked matrix product obtained (formulations 5a, 5b and 5c) is measured as described previously.
[0119] Test No. 6: Formulation of a biocompatible product with a co-crosslinked HA and CHITO matrix, with a divalent zinc cation present in the matrix by addition of zinc sulfate
[0120] A formulation of HA and CHITO is prepared comprising 90% of a co-crosslinked HA-CHITO phase and 10% of a non-crosslinked (linear) HA-CHITO-based phase. The concentrations of HA and CHITO are 0.9% and 0.1% by weight, respectively, relative to the total weight of the matrix.
[0121] The crosslinked phase of HA-CHITO is prepared as previously described in connection with test No. 4.
[0122] In parallel, a linear phase with HA and CHITO is prepared as previously described in connection with Test No. 4, except that after complete dissolution of sodium hyaluronate (NaHA) and carboxymethyl chitosan, a divalent zinc cation is added to the matrix by incorporation into the zinc sulfate (ZnSO4) solution (using a dispersion). A mixture is then used to dissolve and homogenize said zinc salt in the linear phase.
[0123] Several concentrations of divalent zinc cation are carried out, namely: 0.0072% (formulation 6a), 0.0144% (formulation 6b) and 0.0360% (formulation 6c) by weight relative to the total weight of the matrix.
[0124] The crosslinked and linear (non-crosslinked) phases are then mixed in a ratio of 9:1.
[0125] The biocompatible cross-linked matrix product thus obtained is then transferred into 1 mL glass syringes.
[0126] The glass syringes are then subjected to heat treatment as previously described, by passing them through an autoclave with a sterilization tray for a duration of 1 minute at 131°C. The total duration of the heat treatment, including heating, the tray and cooling, is approximately 22 to 23 minutes.
[0127] The viscosity of the biocompatible cross-linked matrix product obtained (formulations 6a, 6b and 6c) is measured as described previously.
[0128] Viscosity measurements before and after heat treatment
[0129] The viscosities of formulations 1, 2a to 2c, 3, 4a, 4b, 5a to 5c and 6a to 6c were measured using a Discovery “DHR2” hybrid rheometer from TA Instruments as previously explained, before and after application of the heat treatment previously explained (sterilization with a plateau lasting 1 minute at a temperature of 131°C, total duration of the heat treatment including heating, plateau and cooling is approximately 22 to 23 minutes).
[0130] [Table 1] Results in terms of viscosities before and after heat treatment Formulations Matrix Nature [Zn2+] (source) Viscosity BEFORE heat treatment (cP) Viscosity AFTER heat treatment (cP) Variations 1 Crosslinked HA No 677 271 -59.97% 2a Crosslinked HA 0.0022% (ZnGluc) 918 495 -46.08% 2b Crosslinked HA 0.0072% (ZnGluc) 932 496 -46.78% 2c Crosslinked HA 0.0144% (ZnGluc) 978 571 -41.62% 3 Co-crosslinked HA+CHITO No 4560 912 -80.00% 4a Co-crosslinked HA+CHITO 0.0072% (ZnGluc) 5218 2028 -61.13% 4b HA+CHITO 0.0144% 4808 4907 2.06% co-crosslinked (ZnGluc) 5a HA+CHITO co-crosslinked 0.0072% (ZnCl2) 5297 4776 -9.84% 5b HA+CHITO co-crosslinked 0.0144% (ZnCl2) 5018 4790 -4.54% 5c HA+CHITO co-crosslinked 0.048% (ZnCl2) 2931 3926 33.95% 6a HA+CHITO co-crosslinked 0.0072% (ZnSO4) 5482 3084 -43.74% 6b HA+CHITO co-crosslinked 0.0144% (ZnSO4) 4749 4903 3.24% 6c HA+CHITO co-crosslinked 0.0360% (ZnSO4) 3050 3922 28.59%
[0131] These results are shown graphically in [Fig. 1] using a histogram. The tested formulations are shown on the x-axis, and the measured viscosities (in cP) are shown on the y-axis. Viscosities before heat treatment are shown as solid bars, while viscosities after heat treatment are shown as dashed bars.
[0132] A first observation, based on formulations 1 and 2a to 2c, is that while the addition of a divalent zinc cation significantly increases the viscosity of a crosslinked HA matrix, a substantial loss of viscosity remains after heat treatment. This loss appears to be almost constant (approximately 400 cP in this example) and independent of the divalent zinc cation concentration.
[0133] A second observation, based on formulations 1 and 3, is that the co-crosslinking of HA and CHITO significantly increases the viscosity of the matrix before and after heat treatment. However, a significant drop (-80%) in viscosity persists after heat treatment.
[0134] A third observation, based on formulations 4a, 4b, 5a to 5c and 6a to 6c, is that the addition of a divalent zinc cation in a co-crosslinked matrix of HA and CHITO at a relatively low concentration of between 0.002% and 0.06% by weight relative to the total weight of the matrix allows the matrix to retain, after heat treatment, a higher viscosity (at least twice as high) than that of formulation 3 (co-crosslinked matrix of HA and CHITO without divalent zinc cation).
[0135] The addition of a divalent zinc cation to a co-crosslinked matrix of HA and CHITO at a concentration between 0.001% and 1% thus makes it possible to obtain simul resulting in a high matrix viscosity and a significantly reduced loss of viscosity after heat treatment.
[0136] A fourth observation, based more particularly on formulations 4b, 5a to 5c, 6b and 6c, is that the addition of a divalent zinc cation in a co-crosslinked matrix of HA and CHITO at a concentration between about 0.005% and about 0.06% makes it possible to obtain a viscosity after heat treatment almost close to the viscosity before heat treatment (formulations 5a, 5b), or even higher than the viscosity before heat treatment (formulations 4b, 5c, 6b and 6c).
[0137] This last observation is very surprising: conventionally, heat treatment of a cross-linked matrix tends to degrade the cohesion of said matrix and therefore to lower its viscosity. This unexpected phenomenon, even going so far as a "viscosity inversion" (meaning that the viscosity of the matrix is higher after heat treatment than before heat treatment), therefore proves particularly advantageous for all applications requiring sterilization of a composition comprising the biocompatible product, in particular for use in a cosmetic or therapeutic treatment method, including in particular the topical application, implantation, instillation or injection by subcutaneous, intradermal, mucosal, ocular, intraocular, or intra-articular route of said composition.
[0138] The present invention, which makes it possible to obtain a high viscosity after heat treatment, even higher than the viscosity before heat treatment, proves to be very valuable for the prevention and / or treatment of pathologies that can be improved or avoided by: - the filling or replacement of a biological tissue; and / or - the increase in volume of said biological tissue; and / or - the supplementation or replacement of a biological fluid.
[0139] The present invention, which allows obtaining a high viscosity after heat treatment, even higher than the viscosity before heat treatment, is also very valuable for a method of treating osteoarthritis, or repairing a cartilage defect, the composition being formulated for example for administration by injection into the synovial fluid or for implantation in the cartilage after mixing with blood, or for a method of treating dry eye.
[0140] The present invention, which makes it possible to obtain a high viscosity after heat treatment, even higher than the viscosity before heat treatment, is also very valuable for use in a treatment method in therapeutics, surgery, or cosmetics, including in particular treatments in rheumatology, ophthalmology, gynecology, aesthetic medicine, and surgery. plastic surgery, internal surgery, orthopedic surgery, prevention of post-surgical tissue adhesions, dermatology.
[0141] The present invention, which allows obtaining a high viscosity after heat treatment, even higher than the viscosity before heat treatment, is also very valuable for use in the therapeutic treatment of dry eye syndrome, corneal lesions or ocular or joint inflammation.
[0142] The present invention, which allows obtaining a high viscosity after heat treatment, even higher than the viscosity before heat treatment, is also very valuable for use in therapeutic treatment in which said composition is applied by instillation onto the ocular surface to prevent or combat corneal damage or dry eye syndrome, in particular for the purpose of lubricating or regenerating the ocular surface.
[0143] In particular, an ophthalmic drop composition can be developed comprising a biocompatible product with a co-crosslinked matrix of HA and CHITO as described above.
[0144] Intracutaneous biocompatibility trials and tests
[0145] Biocompatibility trials and tests were carried out (in adaptation of the standard ISO 10993 - part 10) by intracutaneous injections of 0.2 mL doses onto the backs of rabbits at separate sites. The sites were observed immediately after injection. Observations were made in terms of erythema and edema after 24 h (1 day), 48 h (2 days), 72 h (3 days), 7 days, and 14 days.
[0146] The following products were tested: - Sample A: a biocompatible product according to formulation 2a, the divalent zinc cation being added to the matrix by the incorporation of zinc gluconate at a zinc gluconate concentration of 20 ppm (i.e. a divalent zinc cation concentration in the matrix of 0.002%), - Sample B: a biocompatible product according to the invention and differing from formulations 4a and 4b only by a zinc gluconate concentration of 20 ppm (i.e. a divalent zinc cation concentration in the matrix of 0.002%), it being specified that the carboxymethyl chitosan is of plant (fungal) origin, - Sample C: a biocompatible product according to the invention and differing from formulations 4a and 4b only by a zinc gluconate concentration of 20 ppm (i.e. a divalent zinc cation concentration in the matrix of 0.002%), it being specified that the carboxymethyl chitosan is of animal origin, - Sample D: a product marketed under the brand name PERFECTHA® DERM (batch number: 190625-2) by the company Sinclair France SAS, - Sample E: a physiological buffer solution, - Sample F: a sodium chloride solution (physiological serum) at 9 g / L (i.e. 0.9% by weight by volume).
[0147] [Table 2] Mean irritation scores according to the ISO 10993-10 standard rating system Day 1 Day 2 Day 3 Day 7 Day 14 Sample A 2.00 0.75 1.50 1.00 0.00 Sample B 2.00 0.00 0.00 0.00 0.00 Sample C 3.75 2.00 2.00 1.75 0.00 Sample D 8.00 7.25 7.00 7.00 3.50 Sample E 0.25 0.00 0.00 0.00 0.00 Sample F 0.00 0.00 0.00 0.00 0.00
[0148] The biocompatible products according to the present invention thus have satisfactory biocompatibility when injected intracutaneously.
[0149] Eye irritation trials and tests
[0150] Eye irritation tests (adapted from ISO 10993 - Part 10) were carried out by instilling 0.1 mL doses of the samples to be tested into the lower conjunctival sac of the left eye of rabbits, while a 0.1 mL dose of a 9 g / L (0.9% w / v) sodium chloride solution (physiological saline) was instilled into the lower conjunctival sac of the right eye of said rabbits as a control. Observations were made regarding ocular reactions after 1 hour, 24 hours (1 day), 48 hours (2 days), and 72 hours (3 days). Each sample was tested on two rabbits.
[0151] The following products were tested: - Sample G: a biocompatible product according to formulation 2a, the divalent zinc cation being added to the matrix by the incorporation of zinc gluconate at a zinc gluconate concentration of 20 ppm (i.e. a divalent zinc cation concentration in the matrix of 0.002%), - Sample H: a biocompatible product according to the invention and differing from formulations 4a and 4b only by a zinc gluconate concentration of 20 ppm (i.e. a divalent zinc cation concentration in the matrix of 0.002%), it being specified that the carboxymethyl chitosan is of plant (fungal) origin, - Sample I: a biocompatible product according to the invention and differing from formulations 4a and 4b only by a zinc gluconate concentration of 20 ppm (i.e. a divalent zinc cation concentration in the matrix of 0.002%), it being specified that the carboxymethyl chitosan is of animal origin.
[0152] [Table 3] Ocular scores of sample G and control Rabbit Observations Ih 24h 48h 72h ECE c E c E c No. 1 Cornea Degree of opacity 0 0 0 0 0 0 0 Area 0 0 0 0 0 0 0 0 Iris 0 0 0 0 0 0 0 0 Conjunctiva Redness 0 0 0 0 0 0 0 0 Chemosis 0 0 0 0 0 0 0 Discharge 0 0 0 0 0 0 0 No. 2 Cornea Degree of opacity 0 0 0 0 0 0 0 Area 0 0 0 0 0 0 0 Iris 0 0 0 0 0 0 0 0 Conjunctiva Redness 0 0 0 0 0 0 0 0 Chemosis 0 0 0 0 0 0 0 Flow 0 0 0 0 0 0 0 0 E: sample C: control
[0153] [Table 4] Ocular scores of sample H and control Rabbit Observations Ih 24h 48h 72h ECE c E c E c No. 1 Cornea Degree of opacity 0 0 0 0 0 0 0 Area 0 0 0 0 0 0 0 0 Iris 0 0 0 0 0 0 0 0 Conjunctiva Redness 0 0 0 0 0 0 0 0 Chemosis 0 0 0 0 0 0 0 Discharge 0 0 0 0 0 0 0 0 No. 2 Cornea Degree of opacity 0 0 0 0 0 0 0 Area 0 0 0 0 0 0 0 0 Iris 0 0 0 0 0 0 0 0 Conjunctiva Redness 0 0 0 0 0 0 0 0 Chemosis 0 0 0 0 0 0 0 0 Discharge 0 0 0 0 0 0 0 0 E: sample C: control
[0154] [Table 5] Ocular scores of sample I and control Rabbit Observations Ih 24h 48h 72h ECE c E c E c No. 1 Cornea Degree of opacity 0 0 0 0 0 0 0 Area 0 0 0 0 0 0 0 0 Iris 0 0 0 0 0 0 0 0 Conjunctiva Redness 0 0 0 0 0 0 0 0 Chemosis 0 0 0 0 0 0 0 Discharge 0 0 0 0 0 0 0 No. 2 Cornea Degree of opacity 0 0 0 0 0 0 0 Area 0 0 0 0 0 0 0 Iris 0 0 0 0 0 0 0 0 Conjunctiva Redness 0 0 0 0 0 0 0 0 Chemosis 0 0 0 0 0 0 0 Flow 0 0 0 0 0 0 0 0 E: sample C: control
[0155] The biocompatible products according to the present invention are non-irritating and thus have satisfactory ocular safety.
[0156] Suitability for use in an ophthalmic drop composition
[0157] The safety of the products according to the present invention has been evaluated for use In the therapeutic treatment of dry eye syndrome, corneal lesions, or ocular or joint inflammation, viscoelastic products are generally used. Hyaluronic acid-based products, cross-linked or non-cross-linked, are widely used.
[0158] For such use, a key property that the products must exhibit is adaptive viscoelastic behavior. A product with adaptive viscoelastic behavior is defined as a product exhibiting: - a sufficiently high viscosity at rest (i.e., at a low shear rate) to have good residual activity and ensure satisfactory protection of the cornea, and - a viscosity that decreases during blinking (i.e. at a high shear rate) to improve comfort and satisfactory distribution of the product on the ocular surface.
[0159] The evaluation was carried out by comparison in terms of viscosity with commercially available products on the market, namely the following products: - VisulXL® Gel from the company VISUfarma (sample J); - OPTIVE FUSION® from the company ALLERGAN (sample K); - HYLO-FORTE® from Ursapharm Arzneimittel GmbH (sample L).
[0160] The biocompatible products according to the present invention that have been tested (after heat treatment) are: - formulation 4a (sample M), - formulation 4b (sample N).
[0161] Formulation 1 (sample O) and formulation 3 (sample P) were also tested.
[0162] The results are illustrated graphically in [Fig.2].
[0163] First of all, it is observed that samples J (VisulXL® Gel from VISUfarma), K (OPTIVE FUSION® from ALLERGAN) and Q (formulation 1) have a very low adaptive viscoelastic behavior, with a low viscosity and substantially constant over the entire range of shear rates tested.
[0164] Although sample L (HYLO-FORTE® from Ursapharm Arzneimittel GmbH) shows a significantly more adaptive viscoelastic behavior, its viscosity remains low over the entire range of shear rates tested.
[0165] It is observed that the formulations according to the present invention (samples M and N) all have a viscosity that is high at low shear rates and that decreases fairly regularly (more or less rapidly) to a significantly lower viscosity at high shear rates. The formulations according to the invention thus have adaptive viscoelastic behavior, making them suitable for use in an ophthalmic drop composition, and the concentration of divalent zinc cation in The matrix and the degree of crosslinking of the matrix allow the viscosity to be adapted to the desired use.
[0166] The formulations according to the present invention are thus particularly interesting for therapeutic treatment by instillation onto the ocular surface to prevent or combat corneal injury or dry eye syndrome, in particular for the purpose of lubricating or regenerating the ocular surface.
[0167] At low shear rates, the viscosity of the formulations according to the invention (M and N) is significantly higher than the viscosity of products available on the market.
[0168] The present invention is not limited to the embodiments that have been explicitly described, but includes the various variants and generalizations contained within the scope of the following claims.
Claims
Claims
1. Biocompatible matrix product comprising: - a polysaccharide selected from the group comprising hyaluronic acid, a hyaluronic acid salt, chondroitin sulfate, cellulose derivatives, and a mixture thereof, - a divalent zinc cation present in the matrix, characterized in that: - the matrix comprises chitosan, preferably a chitosan derivative or a chitosan salt, - in said matrix, at least part of the polysaccharide is co-crosslinked with at least part of the chitosan, the chitosan derivative, or the chitosan salt, - the concentration of divalent zinc cation in the matrix is between 0.001% and 1% by weight relative to the total weight of the matrix.
2. Biocompatible product according to claim 1, characterized in that the concentration of divalent zinc cation in the matrix is less than or equal to 0.1% by weight relative to the total weight of the matrix.
3. Biocompatible product according to one of claims 1 or 2, characterized in that the concentration of divalent zinc cation in the matrix is between 0.002% and 0.06% by weight relative to the total weight of the matrix.
4. Biocompatible product according to any one of claims 1 to 3, characterized in that the divalent zinc cation is included in the matrix by the addition of a zinc salt or a zinc saccharide, preferably zinc gluconate, zinc chloride or zinc sulfate.
5. Biocompatible product according to any one of claims 1 to 4, characterized in that: - the concentration of polysaccharide chosen from the group comprising hyaluronic acid, a hyaluronic acid salt, chondroitin sulfate, cellulose derivatives, and a mixture thereof, is between 0.01% and 3% by weight relative to the total weight of the matrix, and / or - the concentration of chitosan, chitosan derivative, or chitosan salt is between 0.01% and 3% by weight relative to the total weight of the matrix.
6. Biocompatible product according to any one of claims 1 to 5, characterized in that the chitosan derivative is a carboxyalkyl chitosan, preferably a carboxymethyl chitosan.
7. Biocompatible product according to any one of claims 1 to 6, characterized in that the polysaccharide is hyaluronic acid or a hyaluronic acid salt, and preferably has a molecular weight of between 0.1 and 5 MDa.
8. Cosmetic or pharmaceutical composition comprising a biocompatible product according to any one of claims 1 to 7.
9. Cosmetic or pharmaceutical composition according to claim 8, comprising a physiologically acceptable buffer, preferably containing polyols and / or phospholipids.
10. Composition according to one of claims 8 or 9, for use in a method of cosmetic treatment or therapeutic treatment, comprising in particular the topical application, implantation, instillation or injection by subcutaneous, intradermal, mucosal, ocular, intraocular or intra-articular route, of said composition.
11. Composition for use according to claim 10, for the prevention and / or treatment of pathologies which can be improved or avoided by: - filling or replacing a biological tissue; and / or - increasing the volume of said biological tissue; and / or - supplementing or replacing a biological fluid.
12. A composition for use according to either of claims 10 or 11, for use in a method of treating osteoarthritis, or repairing a cartilage defect, the composition being for example formulated for administration by injection into synovial fluid or for implantation into cartilage after mixing with blood, or for a method of treating dry eye.
13. Composition according to one of claims 9 or 10, for use in a method of treatment in therapy, surgery, or cosmetics, including in particular a treatment in rheumatology, ophthalmology, gynecology, aesthetic medicine, plastic surgery, internal surgery, orthopedic surgery, for the prevention of post-surgical tissue adhesions, in dermatology.
14. Composition according to one of claims 8 or 9, for use in a therapeutic treatment of dry eye syndrome, corneal injury or ocular or joint inflammation.
15. Composition according to one of claims 8 or 9, for use in a therapeutic treatment during which said composition is applied by instillation onto the ocular surface to prevent or combat corneal damage or dry eye syndrome, in particular for the purpose of lubricating or regenerating the ocular surface.
16. An eye drop composition comprising a biocompatible product according to any one of claims 1 to 7.
17. A method of manufacturing a biocompatible product according to any one of claims 1 to 7 or a composition according to any one of claims 8 to 16, said method comprising the following steps: a. dissolving in the same aqueous solution: i. a polysaccharide selected from the group comprising hyaluronic acid, a hyaluronic acid salt, chondroitin sulfate, cellulose derivatives, and a mixture thereof, preferably hyaluronic acid or a hyaluronic acid salt, ii. chitosan, preferably a chitosan derivative, or a chitosan salt, b. adding to said aqueous solution a crosslinking agent and causing crosslinking of the mixture to form a matrix, c. adding a divalent zinc cation before and / or after step b.
18. Manufacturing method according to claim 17, characterized in that the pH of the biocompatible product or composition is adjusted between 6 and 8, preferably to 7.
19. Manufacturing method according to one of claims 17 or 18, characterized in that the biocompatible product or the composition is subjected to a sterilization heat treatment, preferably to a heat treatment at a temperature between 120°C and 140°C for a duration between 1 and 20 minutes.