Method for cutting a sample of amorphous metallic alloy
Femtosecond laser machining with controlled parameters addresses the challenge of maintaining the amorphous structure in AMAs, achieving high precision and industrial production rates while preserving mechanical properties.
Patent Information
- Application Number
- FR2021007113
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-06-30
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-06-30
AI Technical Summary
Existing machining techniques for amorphous metal alloys (AMAs) face challenges in maintaining the amorphous structure during processing, as they often cause thermal heating leading to crystallization, and struggle to achieve high precision, low roughness, and industrial production rates.
A femtosecond laser machining process with specific parameters, including pulse durations of less than 1000 femtoseconds, relative movement between the laser and the sample, and precise control of laser beam characteristics, is used to ablate material while preserving the amorphous state.
The process effectively maintains the amorphous structure of AMAs, achieving high precision, low surface roughness, and industrial production rates, while retaining the material's mechanical properties.
Smart Images

Figure 00000035_0000 
Figure 00000035_0001 
Figure 00000036_0000
Abstract
Description
Title of the invention: Method for cutting a sample of amorphous metal alloy Technical field
[0001] The present invention relates to the field of methods for machining metal microcomponents, in particular parts made of amorphous metal alloy (AMA). Indeed, amorphous alloys have mechanical characteristics that are particularly interesting for technical fields involving very small parts. Prior art
[0002] It is known to obtain amorphous metal preforms by injection into molds of specific shape. By cooling the injected metal sufficiently quickly, crystallization of the alloy can be avoided and an amorphous type structure can be obtained. This type of amorphous alloy structure is also called metallic glass.
[0003] In order to obtain a mechanical part ready to be integrated, for example, into a clockwork mechanism, it is sometimes necessary to machine the molded preform.
[0004] In the general field of alloys, in particular crystalline alloys, numerous machining and / or shaping techniques have been developed (stamping, micro-milling, etc.). However, these techniques cannot be easily transposed to AMAs which have particular chemical compositions and mechanical properties which are generally much higher than crystalline alloys. Machining is therefore more complex to master (obtaining the desired precision and surface finish, perpendicularity of the flanks, tool life, production speed compatible with industrial constraints, etc.).
[0005] On the other hand, many of these techniques cause thermal heating in the machined areas, which then involves local recrystallization of the alloy and the loss of the amorphous structure of the AMA in the machined areas. This is all the more true for AMAs with low thermal stability. Indeed, among the AMAs, some have lower thermal stability than others. This low thermal stability reflects the ease / speed with which the structure of the alloy can be affected by a temperature variation (increase in temperature beyond the glass transition temperature Tg, too slow cooling, etc.). AMAs with lower thermal stability therefore have a capacity to evolve towards a crystalline state more quickly above the glass transition temperature Tg.
[0006] Laser cutting processes are suitable for the manufacture of microcomponents, in particular microcomponents made of crystalline metal alloys. As indicated previously, however, the latter are much less sensitive to temperature than AMAs, in particular than AMAs with low thermal stability.
[0007] Thus, the difficulty is to carry out these machining operations of AMAs while preserving their amorphous structure, guaranteeing a quality of the surface condition of the machined part and maintaining a high cycle time suitable for industrial production. Indeed, a machining operation which would lead to excessive heating of the material would cause crystallization of the heat-affected zone and would therefore lose the advantageous properties conferred by the amorphous structure of the material. Conversely, imagining a laser machining process by leaving long cooling times between two laser pulses is not compatible with industrial production.
[0008] There is therefore a need for a machining process that allows an amorphous microstructure to be maintained while allowing an industrial-level manufacturing rate. Another requirement is to be able to obtain a surface finish with very low roughness and / or excellent perpendicularity of the flanks in the cutting zone, in order to fully exploit the intrinsic qualities of AMA. Summary
[0009] To this end, the invention proposes a method for machining a sample made of amorphous metal alloy using a femtosecond laser, comprising at least one step of irradiating the sample with a laser beam along a reference trajectory to ablate material from the sample, in a through or non-through manner, along the reference trajectory so as to obtain a machined sample maintained in the amorphous state, in which: - the laser beam is pulsed, and - the duration of each pulse is less than 1000 femtoseconds, preferably less than 600 femtoseconds, more preferably between 100 femtoseconds and 600 femtoseconds.
[0010] According to one embodiment, the laser beam is movable so as to move relative to the sample to be machined along the reference trajectory.
[0011] Alternatively, the sample to be machined is movable so as to move relative to the laser beam along the reference trajectory.
[0012] The amorphous metal alloy has: - a critical diameter less than 5 millimeters, preferably less than 3 millimeters, and / or - a difference between the crystallization temperature and the glass transition temperature of less than 60°C, and / or - a quotient of the difference between the crystallization temperature and the glass transition temperature and the difference between the liquidus temperature and the glass transition temperature less than 0.12, preferably less than 0.1.
[0013] These laser beam adjustment parameters make it possible to machine an amorphous sample and obtain a desired geometry while retaining the amorphous character of the alloy structure. It is thus possible to obtain mechanical microcomponents with particularly interesting mechanical properties.
[0014] The features listed in the following paragraphs can be implemented independently of each other or in any technically possible combination:
[0015] According to one embodiment of the method, - the laser beam is movable so as to move relative to the sample to be machined along the reference trajectory; and - the pulse frequency of the laser beam is greater than 1 kHz, preferably greater than 20 kHz; and - the scanning speed of the laser beam is less than 2000 mm / s, preferably less than 1000 mm / s and even more preferably less than 600 mm / s.
[0016] According to one embodiment, the laser beam may be an infrared laser beam, in particular an infrared laser beam having a wavelength of between 800 nm and 1100 nm, in particular a wavelength of 1030 nm ± 5 nm.
[0017] Alternatively, the laser beam may be a green laser beam, in particular a green laser beam having a wavelength of between 500 nm and 540 nm. The wavelength may in particular be equal to 515 nm ± 5 nm.
[0018] As a further variant, the laser beam may be an ultraviolet laser beam, in particular an ultraviolet laser beam having a wavelength of less than 400 nm. The wavelength may in particular be equal to 343 nm ± 25 nm.
[0019] As a further variant, the laser beam may be a blue laser beam, in particular a blue laser beam having a wavelength of between 400 nm and 480 nm.
[0020] According to one aspect of the method, the laser beam has a fluence greater than 15 J / cm2. Preferably, the fluence is greater than 20 J / cm2. The fluence may be in the range of 40 J / cm2 to 400 J / cm2.
[0021] According to one aspect of the method, each pulse of the laser beam irradiates a portion of the sample to be machined on the reference trajectory. The portion irradiated by a pulse at least partially covers the portion irradiated by the previous pulse. The overlap between two portions irradiated by two successive pulses of the laser beam is at least 25% of the surface area of the diameter of a portion irradiated by the laser beam. The overlap between two irradiated portions by two successive pulses of the laser beam is at most 95% of the surface of the diameter of a portion irradiated by the laser beam.
[0022] According to one embodiment of the method, the step of irradiating the sample with a laser beam along the reference trajectory (TRef) is iterated at least once. This step is preferably iterated at least 100 times, and more preferably at least 300 times. The reference trajectory (TRef_p) during an iteration (R_p) is the same as the reference trajectory (TRef_p-1) of the previous iteration (R_p-1).
[0023] According to one aspect of the method, the laser beam has a diameter projected onto the irradiated portion of the sample of less than 100 pm, preferably between 5 and 100 pm, preferably between 10 and 60 pm, more preferably between 10 and 30 pm.
[0024] The laser beam has an average power greater than 0.4 W. The average power is preferably greater than 1.5 W. The average power is more preferably between 1.5 W and 30 W.
[0025] According to one embodiment of the method, the movement of the laser beam comprises a precession movement. A precession angle of the laser beam is less than 10°, preferably less than 8°.
[0026] According to one embodiment, an angle between the average direction of the laser beam and the direction normal to the surface of the irradiated portion of the sample is less than 10°, preferably less than 8°.
[0027] According to one aspect of the method, the laser beam has a variable focusing altitude. The altitude of the focal plane of the precession ring may be movable and move towards the sample as machining progresses; and / or the altitude of the focal plane of the individual beam may move towards the sample or within said sample as machining progresses; the focusing altitude at the start of machining being between the altitude of the focal plane of the precession ring and the altitude of the focal plane of the individual beam.
[0028] According to an exemplary implementation, the machining method is carried out by implementing at least one contour along at least one trajectory (TRef+n), n being the total number of contours implemented, the method thus comprising: - optionally at least one step of irradiation (c) of the sample with a laser beam along a reference trajectory (TRef+n) to ablate material from the sample, in a through or non-through manner, along the reference trajectory (TRef+n), - a step of irradiating (b) the sample with a laser beam along a reference trajectory (TRef+1) to ablate material from the sample, in a through or non-through manner, along the reference trajectory (TRef+1), - a step of irradiating (a) the sample with a laser beam along a reference trajectory (TRef) to ablate material from the sample, in a through or non-through manner, along the reference trajectory (TRef), - the reference trajectory (TRef+1) being adjacent to the reference trajectory (TRef) and translated by a given distance gl from said reference trajectory (TRef); and - optionally, the reference trajectory (TRef+n) being adjacent to the reference trajectory (TRef+(nl)) and translated by a given distance g2 from said reference trajectory (TRef+n-1) in the direction opposite to that of the trajectory (TRef), and - the given distances (gl, g2, gn) between two directly adjacent reference trajectories (TRef; TRef+1, TRef+(nl); TRef+n) being such that the pulses of the laser beam, irradiating the sample to be machined on the first reference trajectory (TRef; TRef+1, TRef+(nl) or TRef+n), also irradiate, at least partially, the sample to be machined on the reference trajectory(s) (TRef; TRef+1, TRef+(nl) or TRef+n) which is or are directly adjacent to it.
[0029] Steps (a) and / or (b) and / or, optionally (c) can be repeated, preferably successively, until a machined part is obtained, maintained in the amorphous state.
[0030] According to an example of implementation of the method, the amorphous metal alloy of the sample to be machined contains, in atomic percentage, more than 40% of Ni, Zr, Cu, Ti, Fe or Co. Preferably, the amorphous metal alloy of the sample to be machined contains, in atomic percentage, more than 50% of Ni, Zr, Cu, Ti, Fe or Co.
[0031] According to a variant, the amorphous metal alloy of the sample to be machined contains in atomic fraction more than 50% of the elements Ni and Nb. Preferably the amorphous metal alloy of the sample to be machined contains in atomic fraction more than 60% of the elements Ni and Nb, more preferably more than 70% of the elements Ni and Nb.
[0032] The invention also relates to a method for producing a surface of a sample made of amorphous metal alloy using a femtosecond laser, the method comprising at least one step of irradiating with a laser beam a first surface of the sample so as to obtain a second surface whose roughness Ra is less than 400 nm, preferably less than 200 nm, more preferably less than 100 nm; and in which: - the laser beam is pulsed, and - the duration of each pulse is less than 1000 femtoseconds, preferably less than 600 femtoseconds, more preferably between 100 femtoseconds and 600 femtoseconds, and in which: the amorphous metal alloy has: - a critical diameter less than 5 millimeters, preferably less than 3 millimeters, and / or - a difference between the crystallization temperature and the glass transition temperature of less than 60°C, and / or - a quotient of the difference between the crystallization temperature and the glass transition temperature and the difference between the liquidus temperature and the glass transition temperature less than 0.12, preferably less than 0.1.
[0033] The invention also relates to a method for cutting a sample of amorphous metal alloy using a femtosecond laser, the method comprising at least one step of irradiating with a laser beam a first surface of the sample on a face (F1) so as to obtain a second face (F2) such that at each point of intersection of the faces (F1) and (F2), said faces (F1) and (F2) form between them an angle of 90° ± 1.5°, preferably 90° ± 1°, more preferably 90° ± 0.5°; and in which: - the laser beam is pulsed, and - the duration of each pulse is less than 1000 femtoseconds, preferably less than 600 femtoseconds, more preferably between 100 femtoseconds and 600 femtoseconds, and in which: the amorphous metal alloy has: - a critical diameter less than 5 millimeters, preferably less than 3 millimeters, and / or - a difference between the crystallization temperature and the glass transition temperature of less than 60°C, and / or - a quotient of the difference between the crystallization temperature and the glass transition temperature and the difference between the liquidus temperature and the glass transition temperature less than 0.12, preferably less than 0.1.
[0034] The invention also relates to a method of manufacturing a part made of an amorphous metal alloy, comprising the steps: - melt a mixture of metals to obtain a piece of alloy, - injecting the resulting billet into a mold and cooling the molded alloy with a cooling rate greater than a critical crystallization rate of the alloy, to obtain an amorphous alloy sample, - machining at least one surface of the sample according to the machining method previously described, or according to the method for producing a surface previously described, or according to the preceding cutting method, to obtain a part made of amorphous alloy according to a predetermined geometry, - optionally carry out a finishing step on at least the surface of the machined sample, preferably a tribofinishing step.
[0035] The invention also relates to a microcomponent, in particular a mechanical microcomponent, made of an amorphous metal alloy comprising at least one surface machined according to the machining method as described above, according to the method for producing a surface described previously or according to the cutting method described above. Brief description of the drawings
[0036] Other characteristics, details and advantages will appear on reading the detailed description below and on analyzing the attached drawings, in which:
[0037] [Fig. 1] represents an X-ray diffraction analysis of an amorphous metal alloy,
[0038] [Fig.2] represents an X-ray diffraction analysis of a metal alloy partially amorphous,
[0039] [Fig.3] represents an X-ray diffraction analysis of a metal alloy crystalline,
[0040] [Fig.4] represents a schematic sectional view of a laser beam,
[0041] [Fig.5] is a schematic side view of an installation capable of implementing a process of machining an amorphous metal alloy sample,
[0042] [Fig.6] is a schematic top view illustrating an embodiment of implementation of the machining process,
[0043] [Fig.7] is a schematic side view illustrating two modes of implementation of the machining process,
[0044] [Fig.8] is a schematic view detailing one embodiment of the method machining,
[0045] [Fig.9] is a schematic side view detailing an optional feature of the process,
[0046] [Fig. 10] is a schematic sectional view detailing the optional feature of [Fig.9],
[0047] [Fig. 11] is a schematic view, from above, detailing the optional feature of [Fig.9],
[0048] [Fig. 12] is a schematic top view detailing another optional feature of the process,
[0049] [Fig. 13] is a schematic side view detailing another optional feature of the method,
[0050] [Fig. 14] is a diagram of the geometry machined in Example 1,
[0051] [Fig. 15] is a diagram showing the results of bending tests of example 2. Description of the embodiments
[0052] In order to facilitate reading of the figures, the different elements are not necessarily represented to scale. In these figures, identical elements bear the same references. Certain elements or parameters may be indexed, that is to say designated for example by first element or second element, or first parameter and second parameter, etc. This indexing is intended to differentiate similar, but not identical, elements or parameters. This indexing does not imply a priority of one element, or of one parameter, in relation to another and it is possible to interchange the names.
[0053] For the purposes of this description, the following definitions should be specified.
[0054] The term “amorphous metal alloy” or “AMA” or “metallic glass” means » metals or metal alloys that are not crystalline, that is to say whose atomic distribution is predominantly random. However, it is difficult to obtain a one hundred percent amorphous metallic glass because there most often remains a fraction of the material that is crystalline in nature. We can therefore generalize this definition to metals or metal alloys that are partially crystalline and which, therefore, contain a fraction of crystals, as long as the amorphous fraction is in the majority. Generally, the fraction of the amorphous phase is greater than 50%. We therefore understand by "amorphous metal alloy" or "AMA" or "metallic glass" metals or metal alloys whose fraction of the amorphous phase is greater than 50%, preferably greater than 65%, more preferably greater than 75% and even more preferably greater than 80%.
[0055] It is specified here that a metallurgical structure is said to be amorphous or entirely amorphous when an analysis by X-ray diffraction (analysis method which will subsequently be called DRX) as described below does not reveal any crystallization peaks.
[0056] The term "critical diameter" (denoted De) of a specific metal alloy is understood to mean the maximum limit thickness below which the metal alloy has a fully amorphous metallurgical structure or beyond which it is no longer possible to obtain a fully amorphous metallurgical structure, when the metal alloy is molded from a liquid state and is subjected to rapid cooling such that the heat transfer inside the metal alloy is optimal. More specifically, the critical diameter is determined by successive molding of cylindrical bars, generally of a length greater than 50 mm and of different diameters, molded from the liquid state under the following conditions: The alloy is melted at a temperature of Tl + 150°C with Tl, the liquidus temperature of the alloy (in °C); The alloy is cast in a CuCl type copper mold and cooled to a maximum temperature of about twenty degrees Celsius (20°C). The alloy is produced and cast under an inert, high-purity atmosphere (e.g., argon grade 6.0) or under a secondary vacuum (pressure < 10 4 mbar). The alloy is molded with a system that allows the application of a pressure differential to facilitate the molding of the alloy, and to ensure intimate contact between the alloy and the mold walls to ensure rapid cooling of the alloy. The molding step can be carried out under a pressure of 20 MPa. This overpressure application system can be mechanical (piston) or gaseous (application of overpressure). After molding, the bars are cut to obtain a slice, that is, a cross-section of the cylinder preferably located towards the middle of the bar, and with a thickness between 1 and 10 millimeters. The slices obtained are analyzed by X-ray diffraction to determine whether the slices have an amorphous or partially crystalline structure. The critical diameter is then determined as the maximum diameter for which the structure is amorphous. The presence of bumps characteristic of amorphous metal alloys is then highlighted by X-ray diffraction. Since defects are most often present in metallurgical structures, a 100% amorphous alloy is almost impossible to obtain, and the critical diameter can be defined as the diameter above which an X-ray diffraction analysis clearly highlights crystallinity peaks.Such an assessment of the amorphous character of a metallic alloy is detailed in the article Cheung et al., 2007 (Cheung et al. (2007) “Thermal and mechanical properties of Cu-Zr-Al bulk metallic glasses” doi:10.1016 / j.jallcom.2006.08.109). It allows for an average analysis over a surface and to avoid the few inevitable metallurgical defects, while analyzing only crystals of significant size, i.e., larger than a few nanometers and / or in significant quantity. Figures 1, 2 and 3 represent an XRD analysis as described previously. These figures show the intensity of the diffracted beam as a function of the angle between the incident beam and the diffracted beam. [Fig.l] is an XRD analysis of a metallic alloy in the amorphous state. [Fig.2] is a similar analysis carried out on a partially amorphous alloy.In this figure, we find the characteristic hump of amorphous structures, but with the presence of peaks as well. [Fig.3] is a similar analysis carried out on a crystalline alloy. In [Fig.3], the characteristic hump of AMAs is not present, and the crystallinity peaks are clearly visible.
[0057] “Low thermal stability AMA” means a metal alloy having: - a critical diameter of less than 5 millimeters, preferably less than 3 millimeters, and / or - a difference ATx between the crystallization temperature Tx and the glass transition temperature Tg less than 60°C, and / or - a quotient (ATx / (TLTg)), corresponding to the quotient of the difference ATx between the crystallization temperature Tx and the glass transition temperature Tg and the difference between the liquidus temperature TI and the glass transition temperature Tg, less than 0.12, preferably less than 0.1. The critical diameter De, the difference ATx=Tx-Tg between the crystallization temperature Tx and the glass transition temperature Tg, as well as the quotient ATx / (Tl-Tg) are all three quantities which define a criterion for the thermal stability of the metal alloy. The lower the value of each of these three quantities, the more unstable the alloy, in other words the more difficult it is to maintain the metal alloy in an amorphous state.
[0058] The term “machining” means an ablation of material from a sample 1. The term “ablation of material” means a removal of material, the two terms being equivalent. Thus, in the context of the present application, “ablate” material and “remove” material are equivalent terms. The machining may be through-hole, as is the case for cutting or drilling. In other words, the laser beam removes material until it passes through the sample. The machining may be non-through-hole, as is the case for engraving, blind drilling, surfacing, for example to obtain a given roughness, or for producing surfaces or flanks whose angle formed between them has excellent precision, for example an angle of 90° ± 1.5°, preferably 90° ± 1°, more preferably 90° ± 0.5°. Non-through machining leaves a thickness of unmachined material.
[0059] The term “microcomponent” means a component of small dimensions, for example a component of which at least one of the dimensions does not exceed 2 millimeters (mm), or even 1 mm, preferably 200 microns (pm), more preferably 100 pm or even 50 pm. The term “mechanical microcomponent” means a microcomponent capable of cooperating with one or more other microcomponents.
[0060] The term "fluence" of the laser beam means the "peak fluence" of the laser beam, the energy delivered per unit of area. It is expressed in J / cm2.
[0061] The term “diameter D” or “spot diameter” of the laser beam is understood to mean the diameter of the portion 3 irradiated on the sample 1 by the laser beam 2. In other words, the diameter D is therefore the diameter of the laser beam 2 focused on the sample 1. Indeed, and as illustrated in part A of [Fig.4], in practice the laser beam 2 is of Gaussian shape. In other words, the laser beam 2 is a Gaussian beam. Consequently, the diameter of the irradiated portion 3 depends on the distance between the emission point of laser beam 2 and the irradiated portion 3. The diameter D, sometimes called the spot diameter, can also be called the diameter of the portion 3 irradiated on sample 1 or the diameter of the laser beam 2 focused on sample 1.
[0062] The term “Best Focus Individual Beam” (also referred to by the acronym BFI) refers to the plane in which the laser beam 2 is most focused. Part A of [Fig.4] illustrates the concept of BFI. The distance between the irradiated portion 3 of the sample and the BFI impacts the ablation capabilities of the laser beam 2.
[0063] The laser beam 2 can be animated by a precessional movement. The precessional movement of the laser beam 2 is shown diagrammatically in [Fig. 9] and part B of [Fig. 4]. In the latter figure, a schematic sectional view of two positions of the same laser beam 2 animated by a precessional movement is shown diagrammatically. During the machining of a part 4, the actual displacement of the laser beam 2 thus corresponds to the composition of two displacements. As shown in [Fig. 11], the first displacement is a displacement along a reference trajectory TC. The second displacement is the precessional movement. The precessional movement therefore makes it possible to change the angle of incidence of the beam throughout the machining process. Thus, when the reference trajectory TC is rectilinear, the area irradiated by the laser beam 2 on the sample 1 to be machined describes a trochoidal trajectory. In other words, the reference trajectory TRef is then a trochoid.Part B of [Fig.l 1] is an enlargement of a portion of part A. In the schematic diagram of part B of [Fig.l 1], the reference trajectory TC appears to be almost rectilinear. When the movement of the laser beam 2 does not include a precessional movement, the reference trajectory TRef is merged with the reference trajectory TC. With a precessional movement as illustrated in [Fig.l 1], the reference trajectory TRef describes loops moving along the reference trajectory TC.
[0064] When the movement of the laser beam 2 involves a precessional movement, the laser beam 2 oscillates around its mean direction D2 and describes the shape of a cone with an angle of attack relative to the surface of the sample 1. The angle of incidence of the laser beam 2 therefore changes during the machining process.
[0065] The term "precession ring focal plane" ("Best Focus Global Beam" in English, also indicated by the acronym "BFG") means the focal plane where the individual laser beam 2 is defocused and rotates almost on itself during the precession. Part B of [Fig.4] illustrates the concept of the precession ring focal plane (BFG).
[0066] “Focusing altitude” with a precessional movement is understood to mean the distance between the upper surface of the sample 1 and the focal plane where the beam individual laser 2 is defocused and rotates almost on itself during precession (BFG).
[0067] [Fig. 5] schematically shows a laser cutting installation 20. The installation comprises an enclosure 13 in which a laser emitter 14 is arranged which can emit a laser beam 2. A sample 1 is placed opposite the emission point of the laser beam 2. The sample 1 can thus be irradiated by the laser beam 2, that is to say that the laser beam 2 can reach a part of the surface S of the sample 1 and interact with the material of the sample 1. The portion of the sample 1 irradiated by the laser beam 2 is designated by the reference sign 3. The sample 1 can be fixed on a plate 6 acting as a support.
[0068] The interaction between the laser beam 2 and the sample 1 makes it possible to carry out a removal of material in the irradiated portion 3. This removal of material is also called ablation of material. A relative displacement of the laser beam 2 with respect to the sample 1 makes it possible to move the irradiated portion 3 and to carry out an ablation of material along a reference trajectory TRef.
[0069] The laser beam 2 can be mobile so as to move relative to the sample 1. The sample 1 can then be immobilized relative to the enclosure 13 of the installation 20. An electronic control unit 25 makes it possible to control the triggering and interruption times of the laser beam 2, as well as the displacement movements of the laser beam 2 relative to the sample 1. The reference trajectory TRef can thus be controlled in real time.
[0070] Alternatively, the sample 1 to be machined can be mobile so as to move relative to the laser beam 2. For this, the sample 1 to be machined is fixed to a mobile plate along at least 2 axes.
[0071] Alternatively, the laser beam 2 and the sample 1 to be machined may both be mobile, successively or concomitantly, in particular to facilitate the machining of complex parts. In all cases, there is a relative movement of the laser beam 2 with respect to the sample 1 so as to obtain a displacement of the laser beam 2 along the reference trajectory TRef.
[0072] The sample 1 to be machined can have any shape and the portion of sample 1 to be ablated can also be of any shape, whether or not it opens out.
[0073] By way of example, in one embodiment, the sample 1 to be machined is flat. In other words, the sample 1 to be machined is a plate of amorphous metal alloy. The thickness of the sample 1 to be machined is preferably between 5 μm and 2 mm, preferably between 10 μm and 1 mm.
[0074] In another embodiment, the sample 1 to be machined is a cylinder or comprises a cylindrical part and the method aims to arrange an axis, passing through or not, within said cylinder or said cylindrical part. The diameter of the microcomponent resulting from the machining process preferably has a diameter, preferably a maximum diameter, less than or equal to 2 mm.
[0075] The amorphous metal alloy of sample 1 to be machined may, for example, contain in atomic fraction more than 40% of Nickel (Ni), preferably more than 50% of Nickel (Ni).
[0076] According to another example of application of the method compatible with the previous mode, the amorphous metal alloy of sample 1 to be machined contains in atomic fraction more than 50% of the elements Nickel (Ni) and Niobium (Nb), preferably more than 60% of the elements Nickel (Ni) and Niobium (Nb), more preferably more than 70% of the elements Nickel (Ni) and Niobium (Nb).
[0077] The alloy with low thermal stability can also be chosen from alloys based on Zr, Cu, Ti, Fe or Co. Here, the term "based on" means that the element cited constitutes the majority element of the alloy.
[0078] Alloys with low thermal stability as described above are particularly difficult to shape while retaining their amorphous character. The method described here is therefore particularly advantageous for shaping such alloys.
[0079] The present invention proposes a method for machining a sample 1 made of amorphous metal alloy using a femtosecond laser, comprising at least one step of irradiating the sample 1 with a laser beam 2 along a reference trajectory TRef to ablate material from the sample 1, in a through or non-through manner, along the reference trajectory TRef so as to obtain a sample 1 machined and maintained in the amorphous state, in which: - laser beam 2 is pulsed, and - the duration of each pulse is less than 1000 femtoseconds, preferably less than 600 femtoseconds, more preferably between 100 femtoseconds and 600 femtoseconds, and in which: - the laser beam 2 is movable so as to move relative to the sample 1 to be machined along the reference trajectory TRef, or - the sample 1 to be machined is mobile so as to move relative to the laser beam 2 along the reference trajectory TRef. The amorphous metal alloy of sample 1 is an alloy of low thermal stability.
[0080] According to a variant of implementation of the method: - the laser beam 2 is movable so as to move relative to the sample 1 to be machined along the reference trajectory TRef; and - the pulse frequency f of the laser beam 2 is greater than 1 kHz, preferably greater than 20 kHz; and - the scanning speed of the laser beam 2 is less than 2000 mm / s, preferably less than 1000 mm / s and even more preferably less than 600 mm / s.
[0081] [Fig.6] illustrates the concept of sample 1, machined sample 1 and / or part 4. Sample 1 forms the raw material or preform to be machined. After one or more machining operations, a machined sample 1 or a part 4, also called a microcomponent, is obtained. Part 4 may be a detached part of sample 1, in particular when the process is a cutting process, also called through machining. The sign 9 schematizes the perimeter 9 of part 4. The shape of part 4 may be arbitrary. In the example of [Fig.6], part 4 is entirely included within the perimeter 21 of sample 1. According to an example not shown, a part of the perimeter 21 of sample 1 may be part of part 4.
[0082] The relative trajectory TRef can define a part of the periphery 9 of the part 4. In other words, the machining method can be implemented in order to form only a part of the periphery 9 of the part 4. The remainder of the periphery 9 of the part 4 can be obtained by other transformation methods or processes. A part of the periphery 9 of the microcomponent 4 can also be formed by a portion of the periphery 21 of the sample 1, which then remains raw in this area.
[0083] According to an alternative embodiment compatible with the previous embodiment, the machined sample or part 4 may be sample 1 from which a portion of the initial material has been ablated without the ablation of material being open. The concept of non-open ablation is illustrated in particular in [Fig.8].
[0084] As an example illustrated in part A of [Fig.7], the sample 1 may be a cylinder and the portion to be ablated 8 may be such that it allows a bearing to be machined in the part 4. It may for example be a bore, whether or not it opens out, within the part 4, which may cooperate with an axis.
[0085] According to an alternative embodiment compatible with the preceding embodiments and illustrated in part B of [Fig.7], the machining method can make it possible to machine a pivot, for example of conical shape, terminating a cylindrical portion, in particular an axis. The ablated zone is shown in dotted lines in [Fig.7] and bears the reference 21.
[0086] Pulsed laser means that the laser beam 2 is applied in successive pulses. In other words, a pulse of the laser beam 2 is applied for a duration t1, then the application of the laser beam is stopped for another duration t2. The frequency f at which the pulses are applied is called the frequency of pulsation or repetition rate of the laser beam 2. This frequency f is equal to the inverse of the period T, which is the sum of the durations tl and t2.
[0087] [Fig.8] illustrates the application of successive pulses of the laser beam 2. The Column A of [Fig.8] is a top view of sample 1. Column B is the corresponding side view. Each pulse of the laser beam 2 irradiates a portion 3 of the sample 1 to be machined, and the portion 3 irradiated by a pulse I_n at least partially covers the portion 3 irradiated by the previous pulse I_n-1.
[0088] In [Fig.8], the successive pulses are applied from left to right. The sign I_1 schematizes the portion irradiated by the first applied pulse. I_2 schematizes the portion irradiated by the second applied pulse. I_7, which schematizes the portion irradiated by the seventh applied pulse, is the last pulse represented. The pulses can of course continue.
[0089] Two successive pulses are applied with a spatial shift d. The shift d between two portions irradiated by two successive pulses I_n-1,1_n of the laser beam 2 is preferably such that there is at least partial overlap for two successive irradiated portions I_n-1,1_n. According to one embodiment, each pulse of the laser beam 2 irradiates a portion 3 of the sample 1 to be machined on the reference trajectory Tref, the portion 3 irradiated by a pulse I_n at least partially covers the portion 3 irradiated by the previous pulse I_n-1, and the overlap between two portions 3 irradiated by two successive pulses I_n-1, I_n of the laser beam 2 is at least 25% of the surface area of the diameter D of a portion 3 irradiated by the laser beam 2 and at most 95% of the surface area of the diameter D of a portion 3 irradiated by the laser beam 2.
[0090] In other words, the portion 3 irradiated by a pulse I_n of the laser beam 2 is here offset relative to the portion 3 irradiated by the previous pulse I_n-1 by a distance d less than the diameter D of the laser beam 2. For reasons of clarity, the offset between the successive pulses has been exaggerated in [Fig.8]. The diameter D of an irradiated portion 3 corresponds to the spot diameter of the laser beam 2.
[0091] The diameter D of the spot of the laser beam 2 or diameter D of the laser beam projected onto the portion 3 of the sample 1, is preferably less than 100 pm, preferably between 5 and 100 pm, preferably from 10 to 60 pm, more preferably from 10 to 30 pm.
[0092] The pulse frequency f of the laser beam 2 is preferably greater than 1 kHz. Preferably, the pulse frequency f of the laser beam 2 is greater than 20 kHz. More preferably, the pulse frequency f of the laser beam 2 is between 20 kHz and 400 kHz, preferably between 20 kHz and 300 kHz.
[0093] The laser beam 2 may be an infrared laser beam, in particular an infrared laser beam having a wavelength of between 800 nm and 1100 nm, in particular a wavelength of 1030 nm ± 5 nm. The laser beam 2 may also be a green laser beam, in particular a green laser beam having a wavelength between 500 nm and 540 nm, in particular a wavelength of 515 nm ± 5 nm. The laser beam 2 may also be an ultraviolet laser beam, in particular an ultraviolet laser beam having a wavelength of less than 400 nm, in particular a wavelength of 343 nm ± 25 nm. The laser beam 2 may also be a blue laser beam, in particular a blue laser beam having a wavelength between 400 nm and 480 nm. The absorption rate of the material in sample 1 is a function of the wavelength / material pair of said sample 1. For certain materials, for example metals, wavelengths in the green range generally have a better absorption rate, which promotes the ablation of the material. However, the lower the wavelength, the more expensive the process will be.
[0094] According to an advantageous embodiment, the laser beam 2 has a peak fluence greater than 15 J / cm2, preferably greater than 20 J / cm2, from 40 J / cm2 to 400 J / cm2. The fluence is the energy level required per unit area to ablate the material, i.e. to remove material in the area irradiated by the laser beam. It depends on the energy and the diameter of the laser beam. For example, for a Gaussian type beam, the fluence is calculated using the following formula:
[0095] [Math.l] F = 2 x A zrr2
[0096] with: r: the radius of the laser beam at the irradiated portion of the sample E: the laser energy F: fluence, expressed in J / cm2 The fluence is calculated in the initial configuration, i.e. from the diameter D of the beam at time tO of the machining process. There are other types of laser beam, for which the calculation of the fluence is then different.
[0097] According to one embodiment, the laser beam 2 has an average power greater than 0.4 W, preferably greater than 1.5 W, more preferably from 1.5 W to 30 W. The power (in watts W) is the product of the energy (in joules J) and the laser frequency (in s1). For a sample 1 in Ni-based AMA, the power of the laser beam 2 selected is preferably between 0.425 W and 20 W.
[0098] According to an advantageous embodiment, the laser beam 2 is moved along the reference trajectory TRef at a scanning speed of less than 2000 mm / s. Preferably, the scanning speed is less than 1000 mm / s, and even more preferably is less than 600 mm / s.
[0099] According to one embodiment, the step of irradiating the sample 1 with a laser beam 2 along a relative reference trajectory TRef is iterated at least once, preferably at least 100 times, more preferably at least 300 times. The number of iterations is adapted according to the quantity of material to be ablated. The relative reference trajectory TRef during an iteration R_p coincides with the relative reference trajectory Tref of the previous iteration R_p-1. Line L1 of [Fig.8] schematizes the first pass of the laser beam 2. Line L2 schematizes the second pass of the laser beam 2, that is to say the iteration of higher rank compared to the previous iteration. Line L3 schematizes the third pass, again the iteration of higher rank compared to the previous iteration.The solid circles describe the portions irradiated during the current iteration and the dotted circles describe the portions irradiated during a previous iteration. In other words, the laser beam 2 can always scan the same trajectory until the material ablation corresponding to the desired remaining material thickness is obtained. The remaining material thickness is zero when the machining is through. In [Fig.8], the depth p of the area where the material has been ablated increases progressively, as the laser beam 2 is repeated along the relative reference trajectory TRef.
[0100] According to an optional embodiment of the machining method, the movement of the laser beam 2 comprises a precession movement. The precession movement makes it possible in particular to more easily obtain straight-sided machining.
[0101] As shown schematically in [Fig.9], the precession angle Al of the laser beam 2 is preferably less than 10°, preferably less than 8°. The precession movement of the laser beam 2 delimits a zone of width dp. The precession angle Al corresponds to the angle between the mean direction D2 of the laser beam 2 and the instantaneous direction Di of the laser beam 2 during the precession. Advantageously, the precession speed of the laser beam 2 is between 500 rpm and 40,000 rpm.
[0102] As illustrated in [Fig.10], the ablation of material carried out by the laser beam 2 to which a precessional movement is applied can have a substantially W shape, thus making it possible to limit the concentration of energy in a precise zone of the sample 1 to be machined.
[0103] According to an alternative embodiment which is particularly advantageous for obtaining perpendicular flanks 16, in particular flanks 16 such that they form between them an angle Ad of 90° ± 1.5°, preferably 90° ± 1°, more preferably 90° ± 0.5°, the average direction D2 of the laser beam 2 forms an angle A2 with the direction normal to the surface of the portion 3 irradiated by said laser beam 2 of between 80° and 90°, preferably of between 82° and 90°. This embodiment is illustrated in [Fig. 13]. In other words, an angle A2 between the average direction D2 of the laser beam 2 and the direction normal to the surface of the irradiated portion 3 of the sample 1 is less than 10°, preferably less than 8°.
[0104] The laser beam 2 is thus inclined relative to the direction Y normal to the surface of the irradiated portion 3 of the sample 1. This angle of inclination A2 makes it possible to improve the perpendicularity of the flanks 16 of the machined part 4. Indeed, the angle of inclination A2 makes it possible to compensate for the perpendicularity defects linked to the fact that the laser beam 2 is Gaussian.
[0105] Advantageously, and in particular in association with the preceding embodiment, the laser beam 2 may have a variable focusing altitude. The altitude of the focal plane of the precession ring (BFG) may be movable and descend towards the sample as the machining progresses; and / or the altitude of the focal plane of the individual beam (BFI) may move towards the sample 1 or within said sample 1 as the machining progresses; the focusing altitude at the start of machining being between the altitude of the focal plane of the precession ring (BFG) and the altitude of the focal plane of the individual beam (BFI).
[0106] Indeed, when the focusing altitude is fixed, the diameter D of the irradiated portion depends on the thickness of material already removed by the laser beam 2. This embodiment is therefore particularly advantageous for maintaining a constant irradiated diameter D over at least part of the machining process, as the machining progresses and the material is ablated. This embodiment makes it possible in particular to improve the cycle time of the machining process.
[0107] According to an embodiment compatible with the preceding embodiments, the machining of the sample 1 can be carried out by a strategy of successive cuts which converge towards the final shape desired for the part 4. Thus, the first cut(s) made are one or more contours. The last cut made gives the part the desired geometry in the area treated by the laser beam.
[0108] For this, the machining process is carried out by implementing at least one contour (also called “outline” in English) along at least one trajectory TRef+n, n being the total number of contours implemented. This embodiment is illustrated in [Fig. 12]. In this figure, three contours have been produced. The first contour is produced along the reference trajectory TRef2. The second contour, represented by a second reference trajectory TRefl, is offset by a distance g2 from the first contour. The third contour, represented by a third reference trajectory, corresponds to the final reference trajectory for machining part 4, i.e. the reference trajectory TRef. The trajectory TRef is offset by a distance gl from the second contour.
[0109] Thus, according to the preceding embodiment, the method comprises: - optionally at least one step of irradiation (c) of the sample 1 with a laser beam 2 along a reference trajectory TRef+n to ablate material from the sample 1, in a through or non-through manner, along the reference trajectory TRef+n, - a step of irradiating (b) the sample 1 with a laser beam 2 along a reference trajectory TRef+1 to ablate material from the sample 1, in a through or non-through manner, along the reference trajectory TRef+1, - a step of irradiating (a) the sample 1 with a laser beam 2 along a reference trajectory TRef to ablate material from the sample 1, in a through or non-through manner, along the reference trajectory TRef, - the reference trajectory TRef+1 being adjacent to the reference trajectory TRef and translated by a given distance gl from said reference trajectory TRef; and - optionally, the reference trajectory TRef+n is adjacent to the reference trajectory TRef+(nl) and translated by a given distance g2 from said reference trajectory TRef+n-1 in the direction opposite to that of the trajectory TRef. The given distances gl, g2, gn between two directly adjacent reference trajectories TRef; TRef+1, TRef+(nl); TRef+n are such that the pulses of the laser beam 2, irradiating the sample 1 to be machined on the first reference trajectory TRef; TRef+1, TRef+(nl) or TRef+n, also irradiate, at least partially, the sample 1 to be machined on the reference trajectory(ies) TRef; TRef+1, TRef+(nl) or TRef+n which is or are directly adjacent to it. The distances gl, g2, gn may be identical or different. Steps (a) and / or (b) and / or, optionally (c) can be repeated, preferably successively, until a part 4 is obtained, machined according to the desired final geometry, and maintained in the amorphous state.
[0110] The implementation of one or more contours as described above makes it possible in particular to limit the risks of crystallization of the sample 1 in amorphous alloy. It also makes it possible to improve the surface condition of the cut sides.
[0111] The machining process using the laser beam 2 can, optionally, be coupled with the presence of a gas flow on the sample 1 to be machined. The machining process can thus comprise the step: - send a flow of gas 10 onto the sample 1 to be machined. The gas flow 10 is then maintained during all or part of the machining process.
[0112] For this, a blowing nozzle 11, shown diagrammatically in [Fig. 5], guides the gas flow 10 towards the sample 1. The gas flow 10, sent onto the sample 1 to be cut, allows the sample 1 to be cooled and helps to avoid excessive heating of said sample 1. The gas flow 10 also allows the particles resulting from the ablation of material by the laser beam 2 to be evacuated. For example, the gas flow 10 sent onto the sample 1 to be machined is an air flow. The gas flow 10 sent onto the sample 1 to be machined can also be an inert gas flow. In the example shown diagrammatically in [Fig. 5], the gas flow 10 sent onto the sample 1 is blown in a direction coaxial with the direction of the laser beam. The gas flow may also not be coaxial with the direction of the beam.
[0113] Also optionally, the sample 1 to be machined may be protected from oxidation during the cutting operation. For this, the cutting process may comprise the step: - place the sample 1 to be machined by the laser beam 2 in a medium 12 protecting against oxidation.
[0114] The enclosure 13 in which the sample 1 and the laser beam 2 are advantageously contained can thus contain a protective medium 12. According to an exemplary implementation, the protective medium 12 from oxidation is a gas whose pressure is lower than atmospheric pressure. According to a variant, the protective medium 12 from oxidation is an inert gas.
[0115] In addition and concomitantly, the method may include the step: - aspirating the gases in the vicinity of the irradiated portion of sample 1.
[0116] The suction of gases in the vicinity of the irradiated portion 3 of the sample 1 makes it possible to promote the evacuation of the metal particles detached from the sample 1 by the effect of the laser beam 2. In [Fig.5], the gas suction system has not been shown.
[0117] Still optionally, the sample 1 can be cooled during the cutting operation. Thus, and as illustrated in [Fig.5], the sample 1 to be machined is thermally coupled to a platen 6 comprising a cooling system 7 configured to absorb heat from the sample 1 to be machined. The sample 1 to be machined can be fixed to the platen 6. The cooling system 7 also helps to avoid an excessive temperature rise of the sample 1 during the machining process.
[0118] The cooling system 7 may comprise a Peltier effect module configured to exchange heat with the plate 6. Alternatively or in addition, the cooling system 7 may comprise a heat transfer fluid circuit configured to exchange heat with the plate 6. Other cooling means are also conceivable.
[0119] Sample 1 may also be completely or partially immersed in a heat transfer fluid. The heat transfer fluid may be static or in motion (flow).
[0120] The invention also relates to a method for producing a surface of a sample 1 made of an amorphous metal alloy with low thermal stability using a femtosecond laser. Said method comprises at least one step of irradiating with a laser beam 2 a first surface of the sample 1 so as to obtain a second surface whose roughness Ra is less than 400 nm, preferably less than 200 nm, more preferably less than 100 nm. In such a method, the laser beam 2 is pulsed and the duration of each pulse is less than 1000 femtoseconds, preferably less than 600 femtoseconds, more preferably between 100 femtoseconds and 600 femtoseconds.
[0121] The embodiments of the machining method described above also apply to said method of producing a surface of a sample 1 in AMA.
[0122] The invention also relates to a method for cutting a sample 1 made of an amorphous metal alloy with low thermal stability using a femtosecond laser.
[0123] In this cutting method, the method comprises at least one step of irradiating with a laser beam 2 a first surface of the sample 1 on a face F1 so as to obtain a second face F2 such that at each point of intersection of the faces F1 and F2, said faces F1 and F2 form between them an angle Ad of 90° ± 1.5°, preferably 90° ± 1°, more preferably 90° ± 0.5°. The laser beam 2 is pulsed, and the duration of each pulse is less than 1000 femtoseconds, preferably less than 600 femtoseconds, more preferably between 100 femtoseconds and 600 femtoseconds.
[0124] The embodiments of the machining method described above also apply to said method of cutting a sample 1 in AMA.
[0125] The processes described above thus make it possible to obtain AMA parts having very precise dimensions and an excellent surface condition, while retaining the amorphous state of the alloy. In addition, the operating parameters of said processes allow industrial-type production, because the cycle time to obtain a part is sufficiently low.
[0126] The invention also relates to a method of manufacturing a part 4 made of an amorphous metal alloy. The manufacturing method comprises the steps: - melt a mixture of metals to obtain a piece of alloy, - injecting the resulting billet into a mold and cooling the molded alloy with a cooling rate greater than a critical crystallization rate of the alloy, to obtain a sample 1 of amorphous alloy, - machining at least one surface of the sample 1 according to the machining method described previously or according to the method for producing a surface described previously or according to the cutting method previously to obtain a part 4 made of amorphous alloy according to a predetermined geometry. Optionally, the manufacturing process includes the step: - carry out a finishing step on at least the surface of the machined sample 1, preferably a tribofinishing step.
[0127] The invention finally relates to a microcomponent, in particular a mechanical microcomponent made of AMA comprising at least one surface 8 machined according to at least one of the preceding methods.
[0128] The AMA microcomponent advantageously has an elastic deformation capacity of at least 1.2%, preferably at least 1.5%.
[0129] The micromechanical component may, for example, be an element of a clockwork mechanism for a mechanical watch, such as a date finger, a toothed wheel, or even an axle. The combination of the intrinsic mechanical properties of amorphous alloys and the precision of the cutting carried out by the process makes it possible to provide micromechanical components that are particularly suitable for this application. It may also be a microcomponent for the medical field, such as an implant. List of reference signs
[0130] 1: Sample to be machined 2: Laser beam 2 3: Serving 3 4: Workpiece 6: Platinum 7: Cooling system 8: Portion to be ablated 9: Surrounding the room 10: Gas flow 11: Blow nozzle 12: Protective environment against oxidation 13: Pregnant 14: Laser transmitter 16: Flanks 20: Laser cutting installation 21: Perimeter of sample 1 25: Electronic control unit 25 Examples Example 1 - Conservation of amorphous structure
[0131] Samples of alloy of formula Ni(57-67)Nb(28-38)Zr(0-10) (atomic percentages) were cut with different sets of parameters detailed in Table 1 to validate the maintenance of the amorphous structure of the alloy of the samples machined according to the method of the invention. The alloy Ni(57-67)Nb(28-38)Zr(0-10) (atomic percentages) has a low thermal stability within the meaning of the invention. Indeed, its critical diameter De is only 3 mm, its stability coefficient, i.e. its quotient (ATx / (TI-Tg)), is 0.07 and its ATx is equal to 40.
[0132] The samples were cut from 500 μm thick preforms and a pyramidal shape was chosen to study the influence of the cutting width on the thermal allocation of the material.
[0133] [Fig. 14] shows a diagram of the machined geometry.
[0134] Table 1 below summarizes the range of parameters tested. Three sets of settings were tested.
[0135] [Tables 1] Parameter Set 1 Set 2 Set 3 Pulsed laser Wavelength 515nm Pulse duration 230 femtoseconds Peak fluence (pj) 19 38 77 Power (W) 0.425 3.4 6.8 Frequency (kHz) 25 50 100 Scan speed (mm / s) 50 100 200 Number of outlines (“outline s”) 3 3 3
[0136] Table 2 below summarizes the structural state of the samples after cutting.
[0137] [Tables2] Parameter Set 1 Set 2 Set 3 Vulkalloys® Nickel base Amorphous Amorphous Amorphous
[0138] Microstructural analyses as well as X-ray diffraction analyses showed a conservation of the amorphous microstructure for all the tested clearances even for the finest areas of the sample, which are the peaked areas.
[0139] The surface conditions and roughness of the flanks after cutting are also in accordance with the levels of requirement necessary for the manufacture of parts in the targeted applications, for which the roughness Ra is less than 0.4. Example 2 - Maintaining mechanical performance
[0140] It should be noted here that the properties of amorphous metal alloys are linked to their microstructure. Thus, a modification of the atomic arrangement due to the thermal effect of the laser beam would modify the mechanical properties of the material.
[0141] Bars 200 pm wide in Ni(57-67)Nb(28-38)Zr(0-10) alloy (atomic percentage), whose characteristics are detailed in Table 3, were machined by laser cutting and by micro-cutting machine with the aim of quantifying this time the influence of the laser for this type of thickness by means of mechanical tests. Cutting by micro-cutting machine is a controlled cutting method which does not affect the material, but does not allow to obtain optimal surface conditions and perpendicularity of the flanks nor to produce complex and precise micro-component geometries.
[0142] The laser parameters used for these samples are presented below. - Pulsed laser - Period 230 femtoseconds - Wavelength 515 nm - Peak fluence 77 J / cm2 - Power 6.8 W - Scan speed 100 mm / s - Number of outlines = 3
[0143] 3-point bending tests were carried out on the machined samples. The bending machine used is an MTS with a 1 kN force cell in compression mode. The test parameters are as follows: - Length between supports L0= 5 mm - Crosshead speed v=0.005 mm / s - Total length of sample 1=15 mm - Sample width L=500 pm - Sample thickness e=200 pm
[0144] The dimensions of the samples are shown in Table 3 below.
[0145] [Tables3] Sample Width b (mm) Height h (mm) L0 / b Bar No. 1 after laser cutting (3.1) 0.2 0.53 27 Bar No. 2 after laser cutting (3.2) 0.2 0.53 27 Bar No. 3 after laser cutting (3.3) 0.2 0.53 27 Bar No. 4 after molding / after micro-cutting (3.4) 0.2 0.53 27
[0146] [Fig. 15] represents the value of the elastic limit in bending, expressed in MPa, for the four samples in Table 3. Sample 3.4 has not undergone laser machining and serves as a representative control of the properties in the amorphous state. By comparison, we clearly observe a conservation of the PAMA properties before and after laser machining for all the samples tested in bending. There is no dispersion in the results and the elastic limit value in bending is indeed equal to that obtained for the micro-sectioned sample. Similarly, we observe a conservation of the properties in the plastic zone.
[0147] The elastic limit and plastic deformation values are also consistent with the values observed on directly molded parts for which no machining step or other treatment has been carried out.
[0148] The developed machining strategy therefore prevents excessive heat input which could modify the microstructure of the material and consequently its properties. The cut parts are therefore not thermally affected, which allows the material to retain its mechanical properties.
[0149] The properties of the parts after machining are therefore identical to those of the material obtained after molding. No degradation of the mechanical properties is observed.
[0150] Example 3 - Obtaining the desired quality (dimensional and geometric) and influence on the rates
[0151] The surface condition after machining is an essential property for many microcomponents. Indeed, for the type of application targeted, for example watch movement parts, a low Ra and good perpendicularity of the flanks are essential to control tribological contacts and obtain low friction coefficients and wear rates, which make it possible to optimize the efficiency of mechanical systems (energy conservation) and their service life.
[0152] Important quality criteria include the roughness of the machined surfaces, obtaining straight flanks, i.e. the perpendicularity between the machined flank and the adjacent flanks, as well as obtaining non-oxidized parts without redeposition of particles (burrs).
[0153] The quality analyses were therefore carried out according to the criteria detailed in Table 4 below:
[0154] [Tables4] Quality criterion Level 1 (Compliant) Level 2 (Acceptable) Level 3 (Non-compliant) Conicity <0.5° Between 0.5° and 1 O > 1° Roughness < N5 = N5 > N5 Surface quality (qualitative analysis) No redeposition of particles AND no oxidation Little redeposition of particles AND little oxidation Too much redeposition of particles OR oxidation
[0155] Table 5 below summarizes the results for parameter sets (machining in air, without nozzle) of preforms, in AMA such as example 1, machined by a pulsed laser beam of 320 fs and having a wavelength of 532 nm: - Game 1: Low power during machining - Set 2, 3 and 4: Increase in machining parameters (power, peak fluence, etc.)
[0156] [Tables 5] Parameter sets Set 1 Set 2 Set 3 Set 4 Power 0.4 W 3.4 W 6.8 W 7.2 W Pulse frequency kHz 25 kHz 50 kHz 100 kHz 100 kHz Scan speed 100 mm / s 100 mm / s 100 mm / s 200 mm / s Machining time 62 min 8 min 4 min 2 min Number of contours 3 3 3 3 Taper Level 1 Level 1 Level 1 Level 2 Roughness Level 1 Level 1 Level 1 Level 1 Surface quality (qualitative analysis) Level 1 Level 1 Level 1 Level 2
[0157] Machining preforms from sets No. 1 and 2 makes it possible to obtain results that comply with the specifications defined for machining microcomponents.
[0158] Nevertheless, for set No. 1, it took a machining time more than 7 times longer than for parameter set No. 2. The low power levels used made it possible to obtain good surface finishes and low roughness, as well as to maintain the amorphous state, but the machining time required to obtain these results is not part of an industrial development approach for a viable cutting solution.
[0159] For sets No. 2 and 3, microscopic analysis of the post-machining parts reveals a homogeneous surface and surface conditions characteristic of successful laser machining. Indeed, we observe a diffraction of light at the flanks which is explained by the passage of the laser which creates a "striated" surface condition. The gap between each groove is sub-micrometric, characteristic of the wavelength of the laser used. The small width between each groove is responsible for the diffraction of light while the regular gap is responsible for the interference phenomenon which creates the colored effect that can be observed.
[0160] In a logic of economic optimization and in order to increase machining rates, the scanning speed was multiplied by 2 on set no. 4.
[0161] To increase the range of possible parameters and avoid quality degradation for ranges close to set No. 4 described above, means for better thermal control must be used. In this case, a nozzle projecting gas (air) onto the cutting area was used.
[0162] Table 6 below summarizes the results obtained using a nozzle projecting air:
[0163] [Tableauxô] Parameter sets Set 4 Set 4 bis Nozzle No Yes Power 7.2 W 7.2 W Taper Level 2 Level 1 Roughness Level 1 Level 1 Surface quality Level 2 Level 1
[0164] This example illustrates the thermal effect on machining. The supply of air evacuates any projections of ablated material as well as the calories linked to laser machining which are responsible for the degradation of surface conditions (oxidized surface) and conicities greater than 1° even for a higher number of repetitions.
[0165] The material can therefore be machined with higher powers, which makes it possible from an economic point of view to increase cutting rates. Example 4 - Optimizing cutting rates
[0166] Conventionally, during laser machining, the focusing altitude is fixed at the start of machining. It is this which makes it possible in particular to define the theoretical spot diameter at the start of machining as well as the fluence. In reality, the focusing altitude remains fixed during machining. The process becomes less efficient as the cutting depth increases, that is to say as one moves away from the ideal focusing point for ablating the material.
[0167] A so-called "top-down" strategy was used to machine the material not with a static focus point on the irradiated surface, but with a focus point moving towards the sample (1) during machining.
[0168] Table 7 below summarizes the results obtained during machining of AMA samples according to Example 1 machined with a static focusing point (Set 2) or a mobile focusing altitude (Set 2 - “Top-Down”).
[0169] [Tables7] Parameters Set 2 Set 2 - "Top-Down" Number of repetitions 1060 760 Taper Level 1 Level 1 Roughness Level 1 Level 1 Surface quality Level 1 Level 1
[0170] The results show a gain of approximately 30% with the use of this new strategy. Indeed, for equivalent surface qualities, 300 fewer passes will have been necessary to machine the part with the “top-down” process.
[0171] The use of such a strategy in an industrialization logic makes it possible to significantly increase cutting rates while retaining the material and dimensional characteristics essential for the machining of microcomponents.
Claims
Claims
1. Method for machining a sample (1) made of amorphous metal alloy using a femtosecond laser, comprising at least one step of irradiating the sample (1) with a laser beam (2) along a reference trajectory (TRef) to ablate material from the sample (1), in a through or non-through manner, along the reference trajectory (TRef) so as to obtain a sample (1) machined and maintained in the amorphous state, in which: - the laser beam (2) is pulsed, and - the duration of each pulse is less than 1000 femtoseconds, preferably less than 600 femtoseconds, more preferably between 100 femtoseconds and 600 femtoseconds, and in which: - the laser beam (2) is movable so as to move relative to the sample (1) to be machined along the reference trajectory (TRef),or - the sample (1) to be machined is movable so as to move relative to the laser beam (2) along the reference trajectory (TRef),and - the pulse frequency (f) of the laser beam (2) is greater than 20 kHz; and wherein: the amorphous metal alloy has: - a critical diameter (De) of less than 5 millimeters, preferably less than 3 millimeters, and / or - a difference (ATx) between the crystallization temperature (Tx) and the glass transition temperature (Tg) of less than 60°C, and / or - a quotient (ATx / (TI-Tg)) of the difference (ATx) between the crystallization temperature (Tx) and the glass transition temperature (Tg) and the difference between the liquidus temperature (TI) and the glass transition temperature (Tg) of less than 0.12, preferably less than 0.1.,
2. Method according to claim 1, characterized in that: - the laser beam (2) is movable so as to move relative to the sample (1) to be machined along the reference trajectory (TRef); and - the scanning speed of the laser beam (2) is less than 2000 mm / s, preferably less than 1000 mm / s and even more preferably less than 600 mm / s.
3. Method according to any one of the preceding claims, characterized in that the laser beam (2) is: - an infrared laser beam, in particular an infrared laser beam having a wavelength between 800 nm and 1100 nm, in particular a wavelength of 1030 nm ± 5 nm, or - a green laser beam, in particular a green laser beam having a wavelength between 500 nm and 540 nm, in particular a wavelength of 515 nm ± 5 nm, or - an ultraviolet laser beam, in particular an ultraviolet laser beam having a wavelength of less than 400 nm, in particular a wavelength of 343 nm ± 25 nm, or - a blue laser beam, in particular a blue laser beam having a wavelength between 400 nm and 480 nm.
4. Method according to any one of the preceding claims, characterized in that the laser beam (2) has a fluence greater than 15 J / cm2, preferably greater than 20 J / cm2, from 40 J / cm2 to 400 J /
5. cm . Method according to any one of the preceding claims, characterized in that each pulse of the laser beam (2) irradiates a portion (3) of the sample (1) to be machined on the reference trajectory (Tref), the portion (3) irradiated by a pulse (I_n) at least partially covers the portion (3) irradiated by the previous pulse (I_n-1), and the overlap between two portions (3) irradiated by two successive pulses I_n-1,1_n of the laser beam (2) is at least 25% of the surface area of the diameter (D) of a portion (3) irradiated by the laser beam (2) and at most 95% of the surface area of the diameter (D) of a portion (3) irradiated by the laser beam (2).
6. Method according to any one of the preceding claims, wherein the step of irradiating the sample (1) with a laser beam (2) along the reference trajectory (TRef) is iterated at least 1 time, preferably at least 100 times, more preferably at least 300 times, the reference trajectory (TRef_p) during a iteration (R_p) being confused with the reference trajectory (TRef_p-l) of the previous iteration (R_p-1).
7. Method according to any one of the preceding claims, in which each pulse of the laser beam (2) irradiates a portion (3) of the sample (1) to be machined on the reference trajectory (Tref), and in which the laser beam (2) has a diameter (D) projected onto the irradiated portion (3) of the sample (1) of less than 100 pm, preferably between 5 and 100 pm, preferably between 10 and 60 pm, more preferably between 10 and 30 pm.
8. Method according to one of the preceding claims, in which the laser beam (2) has an average power greater than 0.4 W, preferably greater than 1.5 W, more preferably between 1.5 W and 30 W.
9. Method according to one of the preceding claims, wherein the movement of the laser beam (2) comprises a precession movement, and wherein a precession angle (Al) of the laser beam (2) is less than 10°, preferably less than 8°.
10. Method according to one of the preceding claims, in which an angle (A2) between the average direction (D2) of the laser beam (2) and the direction normal to the surface of the irradiated portion (3) of the sample (1) is less than 10°, preferably less than 8°.
11. Method according to one of the preceding claims in combination with claim 9, wherein: - the laser beam (2) has a variable focusing altitude, characterized in that the altitude of the focal plane of the precession ring (BFG) is movable and moves towards the sample (1) as the machining progresses; and / or the altitude of the focal plane of the individual beam (BFI) moves towards the sample (1) or within said sample (1) as the machining progresses; and the focusing altitude at the start of the machining is between the altitude of the focal plane of the precession ring (BFG) and the altitude of the focal plane of the individual beam (BFI).
12. Method according to any one of the preceding claims, characterized in that the machining method is carried out by implementing at least one contour along at least one trajectory (TRef
13. +n), n being the total number of contours implemented, the method thus comprising: - optionally at least one step of irradiation (c) of the sample (1) with a laser beam (2) along a reference trajectory (TRef+n) to ablate material from the sample (1), in a through or non-through manner, along the reference trajectory (TRef+n), - a step of irradiating (b) the sample (1) with a laser beam (2) along a reference trajectory (TRef+1) to ablate material from the sample (1), in a through or non-through manner, along the reference trajectory (TRef+1), - a step of irradiating (a) the sample (1) with a laser beam (2) along a reference trajectory (TRef) to ablate material from the sample (1), in a through or non-through manner, along the reference trajectory (TRef), - the reference trajectory (TRef+1) being adjacent to the reference trajectory (TRef) and translated by a given distance gl from said reference trajectory (TRef); and - optionally, the reference trajectory (TRef+n) is adjacent to the reference trajectory (TRef+(nl)) and translated by a given distance g2 from said reference trajectory (TRef+n-1) in the direction opposite to that of the trajectory (TRef), and - the given distances (gl, g2, gn) between two directly adjacent reference trajectories (TRef; TRef+1, TRef+(nl); TRef+n) being such that the pulses of the laser beam (2), irradiating the sample (1) to be machined on the reference trajectory (TRef+1, TRef+(nl) or TRef+n), also irradiate, at least partially, the sample (1) to be machined on the reference trajectory(ies) (TRef; TRef+1, TRef+(nl)) which is or are directly adjacent to it; and - steps (a) and / or (b) and / or, optionally (c) can be repeated, preferably successively, until a part 4 is obtained, machined and maintained in the amorphous state. Method according to one of the preceding claims, in which the amorphous metal alloy of the sample (1) to be machined contains, in atomic percentage, more than 40% of Ni, Zr, Cu, Ti, Fe or Co, preferably more than 50% of Ni, Zr, Cu, Ti, Fe or Co or in which the amorphous metal alloy of the sample (1) to be machined machine contains in atomic fraction more than 50% of the elements Ni and Nb, preferably more than 60% of the elements Ni and Nb, more preferably more than 70% of the elements Ni and Nb.
14. Method according to one of the preceding claims, such that it is a method for producing a surface of a sample (1) made of amorphous metal alloy using a femtosecond laser, the method comprising at least one step of irradiation with a laser beam (2) of a first surface of the sample (1) so as to obtain a second surface whose roughness Ra is less than 400 nm, preferably less than 200 nm, more preferably less than 100 nm; and in which: - the laser beam (2) is pulsed, and - the duration of each pulse is less than 1000 femtoseconds, preferably less than 600 femtoseconds, more preferably between 100 femtoseconds and 600 femtoseconds, and in which: the amorphous metal alloy has: - a critical diameter (De) less than 5 millimeters, preferably less than 3 millimeters, and / or - a difference (ATx) between the crystallization temperature (Tx) and the glass transition temperature (Tg) of less than 60°C, and / or - a quotient (ATx / (TI-Tg)) of the difference (ATx) between the crystallization temperature (Tx) and the glass transition temperature (Tg) and the difference between the liquidus temperature (TI) and the glass transition temperature (Tg) of less than 0.12, preferably less than 0.
1.
15. Method according to one of claims 1 to 13 such that it is a method of cutting a sample (1) of amorphous metal alloy using a femtosecond laser, the method comprising at least one step of irradiation with a laser beam (2) of a first surface of the sample (1) on a face (F1) so as to obtain a second face (F2) such that at each point of intersection of the faces (F1) and (F2), said faces (F1) and (F2) form between them an angle (Ad) of 90° ± 1.5°, preferably 90° ± 1°, more preferably 90° ± 0.5°; and - the laser beam (2) is pulsed, and - the duration of each pulse is less than 1000 femtoseconds, preferably less than 600 femtoseconds, more preferably between 100 femtoseconds and 600 femtoseconds, and in which: the amorphous metal alloy has: - a critical diameter (De) less than 5 millimeters, preferably less than 3 millimeters, and / or - a difference (ATx) between the crystallization temperature (Tx) and the glass transition temperature (Tg) of less than 60°C, and / or - a quotient (ATx / (TI-Tg)) of the difference (ATx) between the crystallization temperature (Tx) and the glass transition temperature (Tg) and the difference between the liquidus temperature (TI) and the glass transition temperature (Tg) of less than 0.12, preferably less than 0.
1.
16. Method for manufacturing a part (4) made of amorphous metal alloy, comprising the steps: - melting a mixture of metals to obtain a piece of alloy, - injecting the piece obtained into a mold and cooling the molded alloy with a cooling rate greater than a critical crystallization rate of the alloy, to obtain a sample (1) of amorphous alloy, - machining at least one surface of the sample (1) according to the machining method of one of claims 1 to 13 or according to the method of producing a surface of claim 14 or according to the cutting method of claim 15 to obtain a part (4) made of amorphous alloy according to a predetermined geometry, - optionally carry out a finishing step on at least the surface of the machined sample (1), preferably a tribofinishing step.
17. Microcomponent, in particular mechanical microcomponent, made of amorphous metal alloy comprising at least one surface (8) machined according to the method for producing a surface of claim 14 or according to the cutting method of claim 15.