NEW CROSSCUTABLE SILYL-TERMINATED POLYMER COMPOSITION AND CORRESPONDING SELF-ADHESIVE ITEM
A crosslinkable adhesive composition with hydrolyzable alkoxysilane groups addresses the challenge of maintaining adhesive power over varying temperatures, achieving efficient crosslinking at low temperatures and improved mechanical strength, thus enhancing PSA performance.
Patent Information
- Application Number
- FR2021007428
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-07-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-07-08
AI Technical Summary
Existing pressure-sensitive adhesive (PSA) technologies face challenges in maintaining adhesive power over a wide temperature range, particularly at high temperatures, and require complex drying or solvent-based processes, leading to industrial hygiene issues and high costs.
A crosslinkable adhesive composition comprising a polymer with hydrolyzable alkoxysilane groups, tackifying resin, fumed silica, and a crosslinking catalyst, which can be crosslinked at low temperatures or ambient conditions without humidity control, forming a self-adhesive support with improved cohesion and mechanical strength.
The composition achieves rapid crosslinking at reduced temperatures, ensuring consistent adhesive properties and enhanced mechanical strength, maintaining cohesion over a wide temperature range, including high weights of PSA, and reducing industrial hygiene concerns.
Abstract
Description
Title of the invention: NEW RECRUITABLE SILYL-TERMINATED POLYMER COMPOSITION AND CORRESPONDING SELF-ADHESIVE ARTICLE FIELD OF INVENTION
[0001] The present invention relates to a novel crosslinkable adhesive composition based on a polymer comprising at least one hydrolyzable alkoxysilane group. It also relates to a self-adhesive article, in particular a self-adhesive substrate comprising a support layer coated with a self-adhesive layer made of said composition in the crosslinked state. Finally, it relates to a method for manufacturing said article. TECHNICAL BACKGROUND
[0002] Pressure-sensitive adhesives (also called self-adhesive adhesives or, in English, "Pressure Sensitive Adhesives" or PSA) are substances that give the coated substrate immediate tack at room temperature. Often referred to by the English term "tack" or sometimes by the term "stickiness," this immediate tack allows the instant adhesion of the self-adhesive substrate to all kinds of surfaces under the effect of light and brief pressure.
[0003] Due to its adhesive power, usually evaluated by a peel test, said self-adhesive support is then firmly fixed to said substrate, by means of an adhesive joint.
[0004] PSAs are widely used for the manufacture of self-adhesive articles, such as, for example, self-adhesive labels which are attached to articles for the purpose of presenting information (such as barcode, name, price) and / or for decorative purposes, whether in permanent or temporary bonding.
[0005] PSAs are also used in the manufacture of self-adhesive tapes for a variety of applications. Examples include, in addition to transparent adhesive tape widely used in everyday life: shaping and assembling cardboard packaging; protecting surfaces for painting work in construction; fixing and holding various elements such as panels, bricks, and protruding objects in the construction of buildings; and fixing and holding flat or profiled metal, plastic, or glass parts, such as electrical cables, plastic films, windows, sheet metal, lettering, logos, seat parts, dashboards, plastic or textile panels, and fluid conduits or pipes, in particular. in the transport industry; the bonding of carpets with double-sided adhesive tapes in the building sector.
[0006] For the manufacture of self-adhesive articles (e.g., self-adhesive labels and / or tapes), self-adhesive coatings (SACs) are generally applied by continuous coating processes over the entire surface of a large (optionally printable) backing layer, at a rate (generally expressed in g / m²) and referred to hereafter as the "basis weight". The backing layer is, for example, paper or a film made of a one- or multi-layered polymer material. The self-adhesive layer covering the backing layer may itself be covered with a protective release liner, for example, made of a silicone film. The resulting multi-layer system is generally wound into large rolls up to 2 m wide and 1 m in diameter, which can be stored and transported.
[0007] These multilayer systems can be subsequently converted into self-adhesive labels applicable by the end user, by means of transformation processes that include printing the desired informational and / or decorative elements on the printable side of the backing layer, and then cutting it to the desired shape and dimensions. The protective backing layer can be easily removed without altering the adhesive layer, which remains attached to the backing layer. After separation of its protective backing layer, the label is applied to the item to be labeled either manually or using labeling machines on automated packaging lines.
[0008] These multilayer systems can also be transformed into self-adhesive tapes by cutting and packaging in rolls of determined widths and lengths with, if necessary, cutting or pre-cutting of particular shapes useful for their final use, such as for the assembly of parts of variable size and shape, in the electronics industry, whether for applications in industry or by the general public.
[0009] Due to their high tack at room temperature, PSAs allow for rapid adhesion of the self-adhesive label and / or tape to the substrate (or article) to be coated (for example, in the case of labels, on bottles or, in the case of tapes, on packaging cartons to be shaped), suitable for achieving high industrial production rates.
[0010] There is an area of application for PSAs in which it is desirable that the adhesive power of the labels and / or tapes on the substrate be maintained even when the adhesive joint ensuring fixation is exposed (as well, consequently, is the article coated with the label and / or tape) to a temperature that may vary in a wide range of applications. Examples include applying labels to certain components of automobiles (or other vehicles) located near the engine, or to packaging designed to hold hot liquids during processing, or to items (such as tires) that are hot-labeled as they come off the production line. Another example is the use of self-adhesive tapes for assembling parts where good thermal resistance is required, such as in the interior trim of aircraft or other vehicles.
[0011] PSAs often used for this application include acrylate-type polymers (or copolymers) with a very high number-average molecular weight (Mn). These are available in the form of either an aqueous emulsion or an organic solution. However, coating such PSAs onto a substrate layer is complicated, from an industrial standpoint, by the need for either an additional emulsion drying step or special equipment that addresses the industrial health and safety issues related to the evaporation of the organic solvent. In both cases, the drawbacks associated with the unpleasant odor of acrylics must also be considered.
[0012] US patent 6486229 describes a UV-curable hot-melt adhesive composition comprising a tackifying resin, a photoinitiator, and a radial styrene-butadiene multiblock copolymer, the butadiene block of which has a high content of pendant vinyl groups. This composition is coated in its uncured state onto a backing layer and then cured by exposure to ultraviolet radiation. The resulting self-adhesive backing is particularly suitable for tape and label applications where good adhesion at elevated temperatures is required. International application WO 2004 / 011559 describes a coatable acrylic composition comprising an acrylic copolymer, a photoinitiator, and a multifunctional (meth)acrylate. This composition can also be cured by exposure to ultraviolet radiation to give a high-performance PSA.
[0013] These techniques for obtaining PSA by UV, however, have drawbacks stemming from industrial hygiene problems related to UV lamps and the costs associated with their short lifespan. Furthermore, in the case of self-adhesive substrates with a high basis weight of PSA, for example, a basis weight exceeding 150 g / m², it is difficult to maintain adhesive strength over a wide temperature range, particularly at high temperatures, due to the difficulty of UV radiation penetrating the entire thickness of the curable adhesive layer. Finally, another disadvantage of UV curing is that the curing process stops as soon as the composition is no longer exposed to UV radiation; thus, the curing reaction cannot continue and be completed after the layer The coated substrate has been removed from the production line, for example, during storage.
[0014] Polyurethane (or polyether) adhesive compositions with alkoxysilane terminations that are heat-curable are already known, notably from the three applications of Bostik SA: WO 09 / 106699, EP2336208 and WO 2020 / 128200. These adhesive compositions are advantageously solvent- and water-free. Their coating on a substrate and their heating, at a temperature between 50 and 150°C, leads, at the end of a chemical crosslinking reaction also carried out in the presence of moisture, to the obtaining of a self-adhesive substrate that exhibits the required adhesive (or peel) and tack properties. This crosslinking reaction leads to the formation of an adhesive joint which has a three-dimensional polymeric network structure comprising siloxane bonds and which ensures the fixation of the self-adhesive support to the substrate.This self-adhesive backing can therefore be used for the manufacture of labels and / or self-adhesive tapes.
[0015] Bostik SA's application WO 12 / 090151 describes a method for crosslinking an alkoxysilane-terminated polyurethane (or polyether) based adhesive composition, which employs a Caroll-type guiding means in a climatic chamber with a temperature between 50°C and 200°C and a relative humidity preferably controlled at a value of about 50%.
[0016] Bostik SA's application FR 3013993 describes a method for applying an adhesive composition comprising a reactive prepolymer, in particular an alkoxysilane-terminated prepolymer, said method comprising heating said composition in-line by supplying electricity to an inductor cable, upstream of its hot application to a substrate using an application nozzle and at a temperature between 50°C and 200°C.
[0017] The present invention aims to simplify the manufacturing process of a self-adhesive article, in particular a self-adhesive substrate, by crosslinking a crosslinkable adhesive composition based on an alkoxysilane-terminated polymer
[0018] The present invention also aims to provide a crosslinkable adhesive composition based on an alkoxysilane-terminated polymer, which makes it possible to manufacture a self-adhesive article, in particular a self-adhesive support, by crosslinking at a lower temperature, in particular at a temperature below 50 °C, and even at room temperature.
[0019] The present invention also aims to provide a crosslinkable adhesive composition based on an alkoxysilane-terminated polymer, which makes it possible to manufacture a self-adhesive article, in particular a self-adhesive support, by crosslinking without control or regulation of relative humidity.
[0020] Another object of the present invention is to provide a crosslinkable adhesive composition which crosslinks at ambient temperature and / or humidity in a reduced time.
[0021] Another object of the present invention is to provide a cross-linkable adhesive composition which, after coating on a support and then cross-linking, leads to a pressure-sensitive adhesive having suitable adhesive strength and tack properties.
[0022] Another object of the invention is that the adhesive joint which ensures the fixing of the self-adhesive support thus obtained on a substrate retains the required cohesion over a wide temperature range, including for high PSA weights.
[0023] Another object of the invention is that the adhesive joint has improved mechanical resistance.
[0024] It has now been found that these objectives can be achieved in whole or in part by means of the adhesive composition and the self-adhesive backing described below. DESCRIPTION OF THE INVENTION Crosslinkable adhesive composition:
[0025] The present invention therefore relates primarily to a crosslinkable adhesive composition, characterized in that it comprises:
[0026] - at least one polymer (A) comprising a hydrolyzable alkoxysilane group;
[0027] - at least one tackifying resin (B);
[0028] - at least one fumed silica (C); and
[0029] - at least one crosslinking catalyst (D).
[0030] It has now been found that said crosslinkable composition offers a considerably reduced crosslinking time at ambient temperature and humidity. It can thus advantageously lead, after its coating onto a support layer and its crosslinking, to a self-adhesive support, at the end of a process that involves a heating step at a lower temperature and does not require high relative humidity, or even at the end of a process that does not require a heating step and / or humidity control.
[0031] Furthermore, said self-adhesive support also exhibits suitable adhesive (or peel) properties on a substrate such as stainless steel, enabling it to adhere firmly to said substrate. Surprisingly, the adhesive joint that secures said support to the substrate maintains significantly better cohesion over temperature, thanks to improved resistance to shear tests at a constant temperature of 125°C.
[0032] Finally, the self-adhesive layer made up of the crosslinkable adhesive composition in the crosslinked state is advantageously endowed with greater mechanical resistance, quantified by measuring the breaking stress. Polymer (A):
[0033] For the purposes of the present invention, polymer (A) means comprising a hydrolyzable alkoxysilane group, a polymer comprising at least one, and preferably at least two, hydrolyzable groups of formula (I):
[0034] -Si(R4)p(OR5)3 p (I)
[0035] in which:
[0036] - R4 represents a linear or branched alkyl radical comprising 1 to 4 carbon atoms, with the possibility that when there are several R4 radicals, they may be identical or different; - R5 represents a linear or branched alkyl radical comprising 1 to 4 carbon atoms, with the possibility that when there are several R5 radicals, they may be identical or different, and with the possibility that two OR5 groups may be involved in the same ring; and - p is an integer equal to 0, 1 or 2, preferably equal to 0 or 1.
[0037] The hydrolyzable alkoxysilane group is preferably positioned at the end of said polymer. However, positioning in the middle of the chain is not excluded. The polymer (A) is not crosslinked before the application of the adhesive composition. The adhesive composition is applied under conditions that allow its crosslinking.
[0038] The polymer (A) is therefore a silylated polymer which is generally in the form of a more or less viscous liquid. Preferably, the polymer (A) has a viscosity ranging from 10 to 200 Pa.s, preferably ranging from 20 to 175 Pa.s, said viscosity being measured for example according to a Brookfield-type method at 23°C and 50% relative humidity (needle S28).
[0039] The polymer (A) preferably comprises two formula groups (I), but it can also comprise three to six formula groups (I).
[0040] Preferably, the polymer(s) (A) have a number-average molecular weight (Mn) ranging from 500 to 50,000 g / mol, more preferably from 700 to 20,000 g / mol. The number-average molecular weight (Mn) of the polymer(s) can be calculated or measured by methods well known to those skilled in the art, for example by NMR and size-exclusion chromatography using polystyrene-type standards.
[0041] According to one embodiment of the invention, the polymer (A) conforms to one of the formulas (II), (III) or (IV): neither}
[0042] in which:
[0043] - R4, R5 and p have the same meaning as in formula (I) described above, - P represents a saturated or unsaturated, linear or branched polymeric radical possibly including one or more heteroatoms, such as oxygen, nitrogen, sulfur, silicon, and preferably having a number-average molecular mass (Mn) ranging from 100 g / mol to 48600 g / mol, more particularly from 300 g / mol to 18600 g / mol or from 500 g / mol to 12600 g / mol, - R1 represents a divalent hydrocarbon radical comprising 5 to 15 carbon atoms which may be aromatic or aliphatic, linear, branched or cyclic, - R3 represents a linear or branched alkylene divalent radical comprising 1 to 6 carbon atoms, preferably 1 to 3 carbon atoms, - X represents a divalent radical chosen from -NH-, -NR7- or -S-, - R7 represents a linear or branched alkyl radical comprising from 1 to 20 carbon atoms and possibly also comprising one or more heteroatoms, and - f is an integer from 1 to 6, preferably from 2 to 5, preferably from 2 to 4, preferably again from 2 to 3.
[0044] Preferably, in the formulas (II), (III) and / or (IV) above, P represents a polymeric radical chosen on a non-limiting basis from polyethers, polycarbonates, polyesters, polyolefins, polyacrylates, polyether polyurethanes, polyester polyurethanes, polyolefin polyurethanes, polyacrylate polyurethanes, polycarbonate polyurethanes, polyether / polyester block polyurethanes.
[0045] For example, document EP 2468783 describes silylated polymers of formula (II) in which P represents a polyurethane / polyester / polyether block polymeric radical.
[0046] According to one embodiment, the silylated polymers are chosen from silylated polyurethanes, silylated polyethers, and their mixtures.
[0047] According to a particular embodiment, the silylated polymer (A) corresponds to one of the formulas (II'), (III') or (IV'): M ~ oad (IF) (R^^R^Sf-R—O—R—O—R—SECR^OR^p (III') yb '■ .!! A ys) (IV')
[0048] in which:
[0049] - R1, R3, R4, R5, X, R7 and p have the same meaning as in formulas (II), (III) and (IV) described above, - R2 represents a saturated or unsaturated, linear or branched divalent hydrocarbon radical possibly comprising one or more heteroatoms, such as oxygen, nitrogen, sulfur, silicon, and preferably having a number-average molecular mass (Mn) ranging from 100 g / mol to 48600 g / mol, more particularly from 300 g / mol to 18600 g / mol or from 500 g / mol to 12600 g / mol, and - n is an integer greater than or equal to 0.
[0050] In the silylated polymers of formulas (II'), (III'), or (IV') defined above, when the radical R2 comprises one or more heteroatoms, said heteroatom(s) are not located at the end of the chain. In other words, the free valences of the divalent radical R2, bonded to the neighboring oxygen atoms of the silylated polymer, each originate from a carbon atom. Thus, the main chain of the radical R2 terminates with a carbon atom at each of its two ends, said carbon atom then exhibiting a free valence.
[0051] According to one embodiment, the silylated polymers (A) are obtained from polyols selected from polyether polyols, polyester polyols, polycarbonate polyols, polyacrylate polyols, polysiloxane polyols, and polyolefin polyols and mixtures thereof, and preferably also from diols selected from polyether diols, polyester diols, polycarbonate diols, polyacrylate diols, polysiloxane diols, polyolefin diols, and mixtures thereof. In the case of polymers of formulas (II'), (III'), or (IV') described above, such diols may be represented by the formula H0-R2-OH, where R2 has the same meaning as in formulas (II'), (in')ou (iv').
[0052] For example, among the R2 type radicals that may be present in formulas (II'), (III') or (IV'), the following divalent radicals can be cited, the formulas below showing the 2 free valences:
[0053] - derived from a polypropylene glycol:
[0054] - derived from a polyester diol:
[0055] - derivative of a polybutadiene diol:
[0056] - derived from a polyacrylate diol:
[0057] - derivative of a polysiloxane diol:
[0058] In the above formulas, the meaning of the radicals and subscripts is as follows:
[0059] - q represents an integer such that the number-average molecular mass of the radical R2 ranges from 100 g / mol to 48600 g / mol, preferably from 300 g / mol to 18600 g / mol, and preferably again from 500 g / mol to 12600 g / mol,
[0060] - r and s represent zero or a non-zero integer such that the average molecular mass the number (Mn) of the radical R2 ranges from 100 g / mol to 48600 g / mol, preferably from 300 g / mol to 18600 g / mol, preferably again from 500 g / mol to 12600 g / mol, it being understood that the sum r+s is different from zero,
[0061] - Q1 represents a linear aromatic or aliphatic divalent alkylene radical or branched, saturated or unsaturated, preferably having from 1 to 18 carbon atoms, preferably from 1 to 8 carbon atoms,
[0062] - Q2 represents a linear or branched divalent alkylene radical exhibiting preferably from 2 to 36 carbon atoms, preferably from 1 to 8 carbon atoms,
[0063] - Q3, Q4, Q5, Q6, Q7 and Q8, represent, independently of each other, an atom hydrogen or an alkyl, alkenyl or aromatic radical, preferably having 1 to 12 carbon atoms, preferably 2 to 12 carbon atoms, preferably still 2 to 8 carbon atoms.
[0064] According to an embodiment of the composition according to the invention, the silylated polymer (A) is such that the radical R2 which appears in the formulas (II'), (III') and (IV') represents a polyether radical, preferably a poly(oxyalkylene) radical, and even more preferably a radical derived from a polypropylene glycol corresponding to the formula indicated above.
[0065] According to one embodiment, R1 is chosen from one of the following divalent radicals whose formulas below show the 2 free valences:
[0066] a) the divalent radical derived from isophorone diisocyanate (IPDI): CH3 ch3
[0067] b) the divalent radical derived from dicyclohexylmethane diisocyanate (H12MDI)
[0068] c) the divalent radical derived from toluene diisocyanate (TDI)
[0069] d) divalent radicals derived from the 4,4' and 2,4'- isomers of diphenylmethane diisocyanate (MDI)
[0070] e) the divalent radical derived from hexamethylene diisocyanate (HDI) -(CH2)6-
[0071] f) the divalent radical derived from m-xylylene diisocyanate (m-XDI)
[0072] Polymers of formula (II) or (II') can be obtained by a process described in documents EP 2336208 and WO 2009 / 106699. Those skilled in the art will be able to adapt the manufacturing process described in these two documents when using different types of polyols. Examples of polymers conforming to formula (II) include:
[0073] - GENIOSIL® STP-E10 (available from WACKER): polyether comprising two (I) dimethoxy type groups (n equal to 0, p equal to 1 and R4 and R5 represent a methyl group) having a number average molecular mass of 8889 g / mol where R3 represents a methyl group; - GENIOSIL® STP-E30 (available from WACKER): with a number average molecular mass of 14493 g / mol, it is a polypropylene glycol with 2 terminal groups consisting of a dimethoxy(methyl)silylmethylcarbamate, i.e. in formula (II1): n equals 0; p equals 1; R4 and R5 represent a methyl group and R3 represents a methyl group; - SPUR+® 1050MM (available from MOMENTIVE): polyurethane comprising two (I) trimethoxy type groups (n not equal to 0, p equal to 0 and R5 represents a methyl group) with a number average molecular mass of 16393 g / mol where R3 represents an n-propyl group; - SPUR+® Y-19116 (available from MOMENTIVE): polyurethane comprising two (I) trimethoxy type groups (n not equal to 0 and R5 represents a methyl group) with a number average molecular mass ranging from 15000 to 17000 g / mol g / mol where R3 represents an n-propyl group; - DESMOSEAL® S XP 2636 (available from BAYER): polyurethane comprising two (I) trimethoxy groups (n not equal to 0, p equal to 0 and R5 represents a methyl group) with a number-average molecular weight of 15038 g / mol where R3 represents a n-propylene group.
[0074] Polymers of formula (III) or (III') can be obtained by hydrosilylation of polyether diallylether according to a process described, for example, in document EP 1829928. Among the polymers corresponding to formula (III), the following may be mentioned:
[0075] - the MS SAX® 350 polymer (available from KANEKA) corresponding to a polyether comprising two (I) dimethoxy type groups (p equal to 1 and R4 and R5 represent a methyl group) having a number average molecular mass ranging from 14000 to 16000 g / mol;
[0076] - the MS SAX® 260 polymer (available from KANEKA) corresponding to a polyether comprising two (I) dimethoxy type groups (p equal to 1, R4 and R5 represent a methyl group) having a number average molecular mass of 16000 to 18000 g / mol where R3 represents an ethyl group;
[0077] - the MS S303H polymer (available from KANEKA) corresponding to a polyether comprising two (I) dimethoxy type groups (p is equal to 1 and R4 represents a methyl group) having a number average molecular mass of about 22,000 g / mol.
[0078] Polymers of formula (IV) or (IV') can, for example, be obtained by reacting polyol(s) with one or more diisocyanates followed by a reaction with aminosilanes or mercaptosilanes. A process for preparing polymers of formula (IV) or (IV') is described in document EP 2 583 988. Those skilled in the art will be able to adapt the manufacturing process described in this document for the use of different types of polyols.
[0079] According to a preferred embodiment of the invention, the adhesive composition comprises at least one silylated polymer (A) of formula (II) and / or (II') or at least one silylated polymer (A) of formula (III) and / or (III').
[0080] According to a particularly preferred embodiment of the invention, the polymer (A) is a silylated polymer of formula (II') in which n equals 0, R2 is a divalent radical derived from a polyether, preferably from a poly(oxyalkylene) diol, and even more particularly from a polypropylene glycol.
[0081] Tackifying resin (B):
[0082] The crosslinkable adhesive composition according to the invention also includes at least one tackifying resin (B).
[0083] Said resin can be any resin compatible with the silylated polymer(s) (A).
[0084] The term "compatible tackifying resin" means a tackifying resin which, when mixed in the proportions 50% / 50% with the polymer (A) (or polymers), gives a substantially homogeneous mixture.
[0085] The resins (B) are advantageously selected from:
[0086] - (i) resins obtained by polymerization of terpene hydrocarbons and phenols, in the presence of Friedel-Crafts catalysts;
[0087] - (ii) resins obtained by a process comprising polymerization of alpha-methyl styrene, said process possibly also including a reaction with phenols;
[0088] - (iii) natural or modified rosins (such as, for example, rosin extracted from pine gum, wood rosin extracted from tree roots and their hydrogenated, dimerized, polymerized or esterified derivatives by monoalcohols or polyols, such as glycerol or pentaerythritol);
[0089] - (iv) resins obtained by hydrogenation, polymerization or copolymerization (with an aromatic hydrocarbon) of mixtures of unsaturated aliphatic hydrocarbons having about 5, 9 or 10 carbon atoms from petroleum cuts;
[0090] - (v) terpene resins, (which generally result from polymerization terpenic hydrocarbons - such as mono-terpene (or pinene) - in the presence of Friedel-Crafts catalysts);
[0091] - (vi) copolymers based on natural terpenes, (such as, for example, styrene / terpene, alpha-methyl styrene / terpene and vinyl toluene / terpene); or
[0092] - (vii) acrylic resins having a viscosity at 100°C of less than 100 Pa.s;
[0093] as well as among mixtures of these resins.
[0094] Such resins are commercially available and among those of type (i), (ii), (iii) and (iv) defined above, the following products may be mentioned:
[0095] - resins of type (i): Dertophene® 1510 available from DRT having a number average molecular mass (Mn) of about 870 Da; Dertophene® H150 available from the same company with a number average molecular mass (Mn) of about 630 Da; Sylvarez® TP 95 available from Arizona Chemical with a number average molecular mass (Mn) of about 1200 Da;
[0096] - resins of type (ii): Cleartack® W100 available from Cray Valley, which is obtained by polymerization of alpha-methyl styrene without the action of phenols, with a number-average molecular weight (Mn) of 900 Da; Sylvarez® 510 which is also available from Arizona Chemical with a number-average molecular weight (Mn) of approximately 1740 Da, the process of which also includes the addition of phenols;
[0097] - resins of type (iii): Sylvalite® RE 100 which is an ester of colophony and pentae- rethritol available from Arizona Chemical and number average molecular mass (Mn) of approximately 1700 Da;
[0098] - resins of type (iv): Picco® AR100 available from Eastman and number average molecular mass (Mn) of approximately 550 g / mol.
[0099] According to a preferred variant, resin (B) is used as resin (B) a resin chosen from those of type (i) or (iv). Fumed silica (C):
[0100] Fumed silica (also known as fumed silica) is in the form of very fine silica particles (on the order of nanometers), with a very low apparent density and a very high specific surface area. Fumed silica can be obtained by pyrolysis, in the presence of hydrogen and oxygen, of silicon compounds, such as silicon tetrachloride, itself prepared from silicon and chlorine.
[0101] Pyrogenized silica is initially hydrophilic, due to the presence of silanol groups (Si-OH) on the surface of its constituent particles. It can be made hydrophobic by reacting these silanol groups with various reagents, generally a silicone oil, such as PolyDiMethylSiloxane (PDMS).
[0102] Preferably, the fumed silica (C) is a hydrophobic fumed silica.
[0103] According to one embodiment, hydrophobic pyrogenated silica (C) is obtained by treating pyrogenated silica with a PolyDiMethylSiloxane.
[0104] According to one embodiment, the fumed silica (C) has a specific surface area BET of at least 10 m² / g, preferably from 50 to 400 m² / g, and even more preferably from 80 to 290 m² / g. The specific surface area BET is measured, in a manner well known to those skilled in the art, by determining an adsorption isotherm based on the Brunauer, Emmett and Teller (BET) method, for example according to ISO 9277 of September 2010.
[0105] According to another embodiment, the fumed silica (C) is obtained by a compaction treatment, for example from a roller compactor or the process described in patent EP 0 280 851. The apparent density is quantified by a measurement of the apparent packed density, measured according to ISO 787 / 11 of August 1983, which is generally in the range of 50 to 200 g / l.
[0106] Such pyrogenated silicas, in particular hydrophobic ones, are commercially available, such as the products in the AEROSIL® range from the company EVONIK.
[0107] A notable example of hydrophobic (C) fumed silica is AEROSIL® R202, which has a specific surface area BET of 100+20 m² / g, a packed apparent density of approximately 60 g / L, and is rendered hydrophobic by treatment with polydimethylsiloxane. The constituent particles of AEROSIL® R202 have a size of approximately 16 nm. Crosslinking catalyst (D):
[0108] The crosslinking catalyst (D) usable in the composition according to the invention may be any catalyst known to those skilled in the art for the condensation of silanol. Examples of such catalysts include organic derivatives of titanium such as titanium acetyl acetonate (commercially available under the name TYZOR® AA75 from DuPont), of aluminum such as aluminum chelate (commercially available under the name K-KAT® 5218 from King Industries), and amines such as 1,8-diazobicyclo(5.4.0)undecene-7 or DBU.
[0109] Silsesquioxane resin (E):
[0110] In addition to ingredients (A), (B), (C) and (D), the crosslinkable adhesive composition according to the invention may also optionally include a silsesquioxane resin (E).
[0111] According to a preferred embodiment of the invention, the crosslinkable adhesive composition according to the invention comprises at least one such silsesquioxane resin.
[0112] Silsesquioxane resins are organic silicon compounds that can adopt a polyhedral or polymeric structure, with Si-O-Si bonds. They generally have the following general formula:
[0113] [RSiO3 / 2]t
[0114] in which R, of the same or different nature, represents an organic radical, and t is an integer that can vary from 6 to 12, preferably t equal to 6, 8, 10 or 12.
[0115] According to one embodiment, silsesquioxane (E) has a polyhedral structure (or POSS for "Polyhedral Oligomeric Silsesquioxane" in English).
[0116] Preferably, silsesquioxane (E) corresponds to the following general formula (V):
[0117] (V)
[0118] in which each from R'1 to R'8 represents, independently of each other, a group chosen from:
[0119] - a hydrogen atom, - a radical chosen from the group consisting of a linear or branched C1-C4 alkoxy radical, a linear or branched alkyl radical comprising 1 to 30 carbon atoms, an alkenyl radical comprising 2 to 30 carbon atoms, an aromatic radical comprising 6 to 30 carbon atoms, a an allyl radical comprising 3 to 30 carbon atoms, an aliphatic cyclic radical comprising 3 to 30 carbon atoms, an acyl radical comprising 1 to 30 carbon atoms, and - a group -OSiR'9R'10 in which R'9 and R'10 each represent, independently of each other, a hydrogen atom or a radical chosen from the group consisting of linear or branched C1-C4 alkyls, linear or branched C1-C4 alkoxys, C2-C4 alkenyls, a phenyl, a C3-C6 allyl radical, a C3-C8 cyclic aliphatic radical, and a C1-C4 acyl radical;
[0120] provided that:
[0121] - that at least one radical among the radicals R'1 to R'8 is a C1-C4 alkoxy radical; and - that at least one radical among the radicals R'1 to R'8 is a phenyl radical.
[0122] Silsesquioxanes are known compounds which are described in particular in application WO 2008 / 107331. Some are also commercially available, such as the DOW product marketed under the names: DOW CORNING® 3074 and DOW CORNING® 3037 (CAS number = 68957-04-0). Other additives:
[0123] The crosslinkable adhesive composition according to the invention may also include one or more additives selected from the group consisting of moisture absorbers, plasticizers, antioxidants, pigments, dyes, adhesion promoters, UV stabilizers, flame retardant additives or fillers such as carbonate fillers, for example of the calcium carbonate type.
[0124] The moisture absorber (or desiccant) may, for example, be selected from hydrolyzable, non-polymer alkoxysilane derivatives with a molecular mass of less than 500 g / mol, preferably from trimethoxysilane and triethoxysilane derivatives. Such an agent can typically prolong the shelf life of the composition during storage and transport prior to use. Examples include gamma-metacryloxypropyltrimethoxysilane (for example, available under the trade name SILQUEST® A-174 from MOMENTIVE), methacryloxymethyltrimethoxysilane (for example, available under the trade name GENIOSIL® XL33 from WACKER), vinyltrimethoxysilane, isooctyltrimethoxysilane, or phenyltrimethoxysilane.
[0125] When present, the moisture absorber can, for example, represent from 0.1% to 3% by weight or from 1% to 2% by weight relative to the total weight of the composition according to the invention.
[0126] The composition according to the invention may also include a plasticizing agent.
[0127] By way of example of a usable plasticizing agent, any agent may be used plasticizer commonly used in the field of adhesives, such as for example phthalates, benzoates, trimethylolpropane esters, trimethylolethane esters, trimethylolmethane esters, glycerol esters, pentaerythritol esters, naphthenic mineral oils, adipates, cyclohexanedicar-boxylates, paraffinic oils, natural oils (possibly epoxidized), polypropylenes, polybutylenes, hydrogenated polyisoprenes, and mixtures thereof.
[0128] Examples of phthalates include diisononyl phthalate, di-isobutyl phthalate, dioctyl phthalate, dicyclohexyl phthalate, diisooctyl phthalate, diisododecyl phthalate, dibenzyl phthalate or butylbenzyl phthalate.
[0129] Examples of benzoates include: neopentylglycol dibenzoate (for example, available under the name UNIPLEX ® 512 from LANXESS), dipropylene glycol dibenzoate (for example, available under the name BENZOFLEX ® 9-88SG from EASTMAN), a mixture of diethylene glycol dibenzoate and dipropylene glycol dibenzoate (for example, available under the name K-FLEX ® 850 S from KALAMA CHEMICAL), or a mixture of diethylene glycol dibenzoate, dipropylene glycol dibenzoate and triethylene glycol dibenzoate (for example, available under the name BENZOFLEX ® 2088 from EASTMAN).
[0130] Among the esters of pentaerythritol, one can cite for example pentaerythritol tetravalerate (for example available under the name PEVALEN™ from the company PESTORP).
[0131] Among the cyclohexanedicarboxylates, we can cite for example diisononyl 1,2-cyclohexanedicarboxylate (for example available under the name HEXAMOLL DINCH ® from BASF) ) and l,4-bis(2-ethylhexyl)-l,4-cyclohexanedicarboxylate (for example available under the name DEHCH from CONNECT CHEMICALS).
[0132] The total plasticizer content in the composition according to the invention can range from 0% to 30% by weight, preferably from 1% to 30% by weight, or even, for example, from 1% to 15% by weight relative to the total weight of said composition.
[0133] The composition according to the invention may also include an antioxidant (also referred to as a UV stabilizing agent).
[0134] Antioxidants are compounds that can be introduced to protect the composition from degradation resulting from a reaction with oxygen, which is likely to be formed by the action of heat or light. These compounds may include primary antioxidants that scavenge free radicals. Primary antioxidants can be used alone or in combination with other secondary antioxidants or UV stabilizers.
[0135] One can cite, for example, IRGANOX ® 1010,1TRGANOX ® B561,1TRGANOX ® 245, IRGANOX ® 1076, IRGAFOS ® 168 marketed by BASF.
[0136] An amount of antioxidant ranging from 0.1% to 3%, preferably from 1% to 3% by weight, based on the total weight of the composition according to the invention is generally used.
[0137] According to one embodiment, the crosslinkable adhesive composition according to the invention comprises:
[0138] - from 3% to 90% by weight, preferably from 5% to 80% by weight, preferably from 10% to 70% by weight, advantageously 20% to 60% by weight of at least one polymer (A) comprising a hydrolyzable alkoxysilane group;
[0139] - from 15% to 80% by weight, preferably from 20% to 70%, preferably from 25% to 70%, in particular from 30% to 60%, advantageously from 40% to 60% by weight of at least one tackifying resin (B);
[0140] - from 1 to 10%, preferably from 2 to 8%, advantageously from 2 to 6% of the silica pyrogenated (C); and
[0141] - from 0.01% to 10%, preferably from 0.01% to 5%, preferably from 0.05% to 4%, advantageously from 0.1% to 3%, in particular from 0.5% to 2%, by weight of crosslinking catalyst (D);
[0142] these percentages by weight being indicated on the basis of the total weight of said composition.
[0143] When, according to a preferred embodiment of the invention, the crosslinkable adhesive composition further comprises a silsesquioxane resin (E), the quantity of the latter may vary from 0.1 to 20% by weight, preferably from 1% to 20% by weight, preferably from 2% to 15% by weight, advantageously from 3% to 12% by weight, based on the total weight of said composition.
[0144] The crosslinkable adhesive composition according to the invention can be prepared by a process which comprises:
[0145] - a mixing step, protected from air, preferably under an inert atmosphere, of the polymer (A), tackifying resin (B), and, where applicable, other optional additives, to form a part (PA); then
[0146] - a step of mixing the crosslinking catalyst (D) with, when it is presents, the silsesquioxane resin (E); to form a part (PB); then
[0147] - a step of incorporating the fumed silica (C) into the part (PA), at a temperature temperature between 50 and 180°C, preferably between 100 and 150°C, until a homogeneous mixture (PC) is obtained; and finally
[0148] - a mixing step of (PC) with (PB). Self-adhesive item:
[0149] The present invention also relates to a self-adhesive article comprising a support layer coated with a self-adhesive layer, characterized in that said self-adhesive layer is made up of the adhesive composition according to the invention. the reticulated state.
[0150] For the purposes of the present invention, the term “self-adhesive article” includes any article which can be stuck to a surface only by the action of pressure with the hand or equipment, without the use of additional glues or adhesives.
[0151] The self-adhesive article is a pressure-sensitive self-adhesive article.
[0152] The support layer coated with a self-adhesive layer is also referred to as the "self-adhesive support".
[0153] These articles are intended, in particular, to be applied to a surface to be bonded in order to bring together, hold, fix, assemble, or simply immobilize, or to display, shapes, logos, images, or information. These articles can be used in many fields, such as medicine, clothing, packaging, automotive (for example, for applying logos, lettering, interior soundproofing, interior trim, and interior decals), or construction (for example, for sound and thermal insulation and window assembly). They can be shaped according to their final application, for example, as tapes, such as industrial tapes, DIY tapes, or tapes for securing materials on construction sites, single or double-sided tapes, or as labels, bandages, dressings, patches, or graphic films.
[0154] According to one embodiment, the self-adhesive article is a self-adhesive multi-layer system, and in particular a self-adhesive label or tape, which may be single or double-sided.
[0155] The material that can be used for the support layer can, for example, be any type of rigid or flexible support. Examples include foams, felts, non-woven materials, plastics, membranes, papers, or a film of a polymer material in one or more layers, in particular a non-stick protective paper or plastic film.
[0156] The support layer is made of a material, for example, selected from polyolefins, such as polyethylene, including high-density polyethylene, low-density polyethylene, linear low-density polyethylene and linear ultra-low-density polyethylene, polypropylene and polybutylenes; polystyrene; natural or synthetic rubber; vinyl copolymers, such as plasticized or unplasticized polyvinyl chloride and poly(vinyl acetate); olefinic copolymers, such as ethylene / methacrylate copolymers, ethylene / vinyl acetate copolymers, acrylonitrile / butadiene / styrene copolymers, and ethylene / propylene copolymers; acrylic polymers and copolymers; polyurethanes; polyethers; polyesters; and mixtures thereof.Preferably, the support layer is based on acrylic polymers, polyethylene (PE), oriented, non-oriented or bi-oriented polypropylene (PP), polyimide, polyurethane, polyester such as polyethylene terephthalate. (PET), or paper.
[0157] According to one embodiment, the self-adhesive article obtained from the adhesive composition according to the invention comprises a permanent support layer coated with an adhesive layer. Preferably, the adhesive layer is further coated with a non-stick protective plastic film or paper, preferably silicone-coated.
[0158] According to another embodiment, the self-adhesive article obtained from the adhesive composition according to the invention comprises a non-permanent support layer consisting of a first non-stick protective plastic or paper film, preferably silicone-coated, said layer being coated with an adhesive layer, which may itself also be coated with a second non-stick protective plastic or paper film. This embodiment is particularly suitable for the bonding of windows, more particularly for the bonding of the rigid panel consisting of double or triple glazing to the window frame.According to this embodiment, said non-permanent support layer is intended to be removed by the user at the time of implementation of the self-adhesive article for the purpose of assembling the window, so as to reveal only the cross-linked adhesive layer, whose mechanical properties, in particular resistance to breakage, are, in accordance with the invention, particularly improved.
[0159] As an alternative to the non-stick protective film, the back face of the permanent support layer which is not coated with the adhesive layer may have a non-stick surface, for example a silicone protective layer.
[0160] According to another embodiment, the permanent support layer is coated on both sides with an adhesive composition, which may be identical or different, at least one of the two adhesive compositions being, according to the invention, advantageously leading to the manufacture of so-called double-sided tapes
[0161] Preferably, the support layer has a thickness ranging from 10 micrometers to 50 mm, more preferably ranging from 10 micrometers to 20 mm, more preferably ranging from 20 micrometers to 10 mm, more preferably ranging from 20 micrometers to 1 mm.
[0162] In certain specific cases, it is necessary to carry out a surface treatment of the support layer to increase the adhesion of the adhesive layer during the coating step on it.
[0163] The self-adhesive article according to the invention can thus bond two substrates. The substrate onto which the self-adhesive article is intended to be applied (referred to as the "substrate to be bonded") can be flexible or rigid. In particular, it can have the same flexibility properties as the backing layer described above, so as to be wound and packaged in the form of a reel, for example as described previously.
[0164] Alternatively, the substrate to be bonded may be rigid. In this case, the substrate cannot It can be wound and packaged in the form of a reel, for example as described previously. The substrate to be bonded can, for example, be chosen from concrete, paper, polyolefin-type substrates, glass, ceramics and metals, including aluminum.
[0165] The self-adhesive layer, which consists of the adhesive composition according to the invention in the crosslinked state, and which covers the support layer, in the self-adhesive article according to the invention can have a very variable thickness, ranging from 10 pm to 5000 pm, preferably.
[0166] A thickness ranging from 10 pm to 100 pm, preferably from 20 to 50 pm, is particularly preferred in the case of self-adhesive labels; while a thickness in a much wider range of 3 to 5000 pm can be encountered for self-adhesive tapes.
[0167] According to one embodiment, the self-adhesive article further comprises a protective non-stick layer (“release liner”).
[0168] According to one embodiment, said anti-adhesive layer is applied to the adhesive layer, after crosslinking of the adhesive composition.
[0169] The backing layer can be covered on the side of its two surfaces not coated with the adhesive layer by a non-stick protective layer, for example, a silicone film. In this way, the self-adhesive article can be rolled up and then unrolled without any problems because the adhesive layer does not stick to the silicone-coated side.
[0170] Method for manufacturing the self-adhesive article:
[0171] The present invention also relates to a method for manufacturing the self-adhesive article as defined above, said method being characterized in that it comprises:
[0172] - (a) the application of said composition by coating on a carrier surface;
[0173] - (b) crosslinking said composition by heating to a temperature ranging from 15°C to 200°C; then
[0174] - (c) the counter-bonding or transfer of the crosslinked adhesive composition layer on a support layer or on a non-stick protective film.
[0175] For the purposes of this invention, "carrying surface" means either a belt conveyor covered with a non-stick layer, or a non-stick protective film ("release liner"), or a support layer.
[0176] In the case where the carrier surface is a non-stick protective film, the manufacturing process of the self-adhesive article according to the invention may include step (c) of transferring the crosslinked adhesive layer onto a support layer.
[0177] In the case where the carrier surface is a support layer or a non-stick protective film, the manufacturing process of the self-adhesive article according to the invention may still understand step (c) of counter-bonding the adhesive layer onto a non-stick protective film.
[0178] According to a preferred embodiment of the invention, step (c) of the above-described process consists of transferring the crosslinked adhesive layer onto a flexible support layer (which may be a plastic film), where appropriate after cooling the crosslinked adhesive layer to a temperature below the degradation or softening temperature of the material composing the support layer.
[0179] According to one embodiment, the manufacturing process for the self-adhesive article according to the invention further comprises a step (d) of coating a second layer of adhesive composition according to the invention onto the substrate layer, followed by a step (e) of cross-linking the adhesive composition coated in step (d) by heating at a temperature ranging from 15°C to 200°C, preferably from 15°C to 45°C, preferably at room temperature. According to this embodiment, a double-sided self-adhesive article is obtained.
[0180] The coating step (a) can be carried out using known coating devices, such as a lip or curtain nozzle, or a roller. It uses an adhesive composition basis weight ranging from 10 g / m² to 5000 g / m².
[0181] The basis weight of adhesive composition required for the manufacture of self-adhesive labels can range from 10 to 100 g / m2, preferably from 20 to 50 g / m2. That required for the manufacture of self-adhesive tapes can vary in a much wider range from 3 to 5000 g / m2, preferably from 15 to 250 g / m2 per side.
[0182] The crosslinking step (b) is, according to a preferred embodiment of the invention, carried out at a temperature ranging from 15°C to 45°C, preferably at room temperature.
[0183] According to one embodiment, the coated adhesive composition is further subjected, during the crosslinking step (b), to treatment in a humid atmosphere characterized by its level of humidity and, in particular, in a gaseous environment where water molecules are present between 10 and 200 g per m3 of gas.
[0184] Preferably, the humid atmosphere is an atmosphere in which 2 to 100% of the molecules are water molecules, preferably 3 to 50%, preferably again 3 to 10% of the molecules are water molecules.
[0185] Humidity is expressed as a percentage of water per unit volume, which corresponds to the number of water molecules divided by the total number of molecules in a unit volume. Thanks to the linear nature of this scale, humidity is easily measured and controlled using, for example, PID (Proportional-Integral-Derivative) monitors. The weight percentage can be calculated by multiplying the percentage of water molecules relative to the total number of molecules by a factor of 0.622. General information on the rate humidity in various environments is described by W. Wagner et al., in “International Steam Tables - Properties of Water and Steam based on the Industrial Formulation IAPWS-IF97,.
[0186] The crosslinking step (b) is, according to yet another preferred embodiment of the invention, carried out without control of humidity, particularly with respect to the humidity of the ambient atmosphere.
[0187] This crosslinking step (b) results in the creation—between the hydrolyzable alkoxysilane terminal polymer chains of the adhesive composition and under the influence of atmospheric humidity—of siloxane-type bonds that lead to the formation of a three-dimensional polymer network. The crosslinked adhesive composition is, in particular, a pressure-sensitive adhesive that imparts the desired adhesive strength and tack to the substrate layer coated with it.
[0188] Preferably, the coating is applied uniformly to the backing layer or to the non-stick protective layer, but the coating can also be adapted to the desired shape of the final self-adhesive article.
[0189] According to one embodiment, the adhesive composition is applied to at least a portion of both sides of the substrate layer. If both sides of the substrate layer are coated, the adhesive composition may be identical or different on both sides, and the basis weight may be identical or different on both sides.
[0190] According to one embodiment of the invention, the self-adhesive article comprises an adhesive layer on at least part of one face or on at least part of both faces of the backing layer, said adhesive layer(s) optionally being coated with a protective non-stick layer. In one embodiment, the self-adhesive article comprises two protective non-stick layers on each of the two adhesive layers. In this case, the two protective layers may be made of the same or different materials and / or they may have the same or different thicknesses.
[0191] The present invention finally relates to a bonding method using the self-adhesive article, as defined above, characterized in that it comprises the following steps:
[0192] a) the removal of the non-stick protective layer, where such a layer is present;
[0193] b) the application of the self-adhesive article to a surface of a product; and
[0194] c) the application of pressure on said article.
[0195] In step b), the self-adhesive article is applied so that the self-adhesive part of the article (formed by the self-adhesive layer) is facing the surface of the product.
[0196] According to an embodiment in which the self-adhesive article is a double article In addition, the bonding method includes a step in which either a second surface of a product is applied to the article bonded to the first surface of a product, or the article bonded to the first surface of a product is applied to a second surface of a product.
[0197] The following examples are given purely to illustrate the invention and should not be interpreted to limit its scope.
[0198] Example A (comparative according to WO 2020 / 128200):
[0199] Heat-curable adhesive composition based on GENIOSIL® STP-E30
[0200] Al. Preparation of the composition:
[0201] The composition shown in Table 1 is prepared by first introducing the Picco® AR100 tackifying resin into a glass reactor under vacuum and heated to approximately 160°C. Then, once the resin is thoroughly melted, GENIOSIL® STP-E30 is added.
[0202] The mixture is stirred under vacuum for 15 minutes, then cooled to 70°C. The catalyst (K-KAT® 5218) and DOW CORNING® 3074 silsesquioxane are then added. The mixture is maintained under vacuum and stirred for a further 10 minutes.
[0203] A2. Measurement of crosslinking time at room temperature:
[0204] The composition of example A is applied so as to fill a mold corresponding to a test specimen of type H2, as defined by standard NF T46-002, the thickness of which is 4 mm and the central part of which has a rectangular section of 4 x 2 mm over a length of 25 mm.
[0205] The mold is left at room temperature and the behavior of the composition is observed. The time required for complete crosslinking is 24 hours.
[0206] A3. Measurement of stress and elongation at break by tensile test:
[0207] The principle of the measurement consists of stretching in a tensile machine, the movable jaw moves at a constant speed of 100 mm / minute, a type H2 specimen, as defined above, made up of the crosslinked adhesive composition and to record, at the moment when the specimen breaks, the applied stress (in MPa) as well as the elongation of the specimen or elongation (in %).
[0208] The results of the measurements obtained are shown in Table 1.
[0209] A4. Preparation of a PET support layer coated with the crosslinked composition, to due to a weight of 60 g / m2:
[0210] A rectangular sheet of Polyethylene Te-rephthalate (PET) with a thickness of 50 µm and dimensions of 20 cm by 40 cm is used as a support layer.
[0211] The composition obtained at point AL is preheated to a temperature close to 100°C and introduced into a cartridge from which a cord is extruded and deposited near the edge of the sheet parallel to its width.
[0212] The composition contained in this cord is then spread over the entire surface of the sheet to obtain a uniform layer of substantially constant thickness. This is achieved using a film puller (also called a film-mograph) which is moved from one edge of the sheet to the opposite edge. A layer of composition corresponding to a basis weight of 60 g / m² is thus deposited, representing a thickness of approximately 60 µm.
[0213] The PET sheet thus coated is then placed in an oven at 120 °C and under a humid atmosphere (4% relative humidity) for 5 minutes for crosslinking of the composition, then laminated onto a protective non-stick layer consisting of a rectangular silicone film sheet of the same dimensions.
[0214] The resulting trilayer is subjected to the tests described below.
[0215] A4.1 Peeling at room temperature:
[0216] Adhesive strength is evaluated by the 180° peel test on a stainless steel plate as described in FINAT Method No. 1, published in the FINAT Technical Manual, 6th edition, 2001. FINAT is the international federation of manufacturers and converters of self-adhesive labels. The principle of this test is as follows.
[0217] A test specimen in the form of a rectangular strip (2.54 cm x 15 cm) is cut from the previously obtained trilayer.
[0218] This test specimen is kept at ambient temperature (approximately 23°C and 50% humidity) for 7 hours. Then, after removing the corresponding portion of the protective anti-stick coating, it is fixed along 2 / 3 of its length to a substrate consisting of a stainless steel plate.
[0219] The resulting assembly is left at room temperature for 20 minutes. It is then placed in a tensile testing device capable of peeling or separating the strip from the free end of the rectangular strip at an angle of 180° and with a separation speed of 300 mm per minute. The device measures the force required to separate the strip under these conditions.
[0220] The corresponding result is expressed in N / 2.54 cm and shown in Table 1.
[0221] A4.2 Peeling after 7 days of storage at 50°C:
[0222] The previous test is repeated, except that after cutting the test specimen into a rectangular strip, it is stored for 7 days at a temperature of 50°C and in an atmosphere with 50% humidity, before being fixed onto the stainless steel plate.
[0223] The corresponding result is expressed in N / 2.54 cm and shown in Table 1.
[0224] A4.3 Instant adhesion (also known as loop test):
[0225] Immediate stickiness or tack is evaluated by the instant adhesion test known as the loop test, described in FINAT method no. 9, the principle of which is as follows.
[0226] A test specimen in the form of a rectangular strip (25 mm x 175 mm) is cut from the PET support layer coated with the cross-linked composition obtained previously.
[0227] After removing all of the protective anti-adhesive layer, the two ends of this strip are joined to form a loop with the adhesive layer facing outwards. The two joined ends are placed in the moving jaw of a tensile device capable of applying a travel speed of 300 mm / minute along a vertical axis with the possibility of back-and-forth movement. The lower part of the loop, positioned vertically, is first brought into contact with a horizontal glass plate measuring 25 mm by 30 mm over a square area of approximately 25 mm per side. As soon as this contact is made, the direction of movement of the jaw is reversed. The immediate adhesive strength is the maximum value of the force required to completely detach the loop from the plate.
[0228] The result is expressed in N / (2.54 cm)2 and is shown in Table 1.
[0229] A4.4 Shear strength time at 125°C:
[0230] The maintenance at high temperature of the adhesive power of the previously obtained PET support layer is evaluated by a test which determines the resistance time of the adhesive joint to static shear at 125°C. Reference is made for this test to the FINAT method no. 8. The principle is as follows.
[0231] A test specimen in the form of a rectangular strip (25 mm x 75 mm) is cut from the previously obtained trilayer and is kept at room temperature (23 °C, 50% humidity) for 24 hours.
[0232] After removing all of the protective non-stick layer, a 25 mm square portion located at the end of the adhesive strip is fixed to a glass plate.
[0233] The test plate thus obtained is placed, using a suitable support, in a substantially vertical position in an oven at 125°C, with the unbonded portion of the 50 mm long strip positioned below the plate. After thermal equilibration, the remaining free portion of the strip is attached to a 1 kg mass, the entire apparatus remaining in the oven at 125°C throughout the test.
[0234] Under the effect of this mass, the adhesive joint that secures the strip to the plate is subjected to a shear stress. To better control this stress, the test plate is actually positioned at an angle of 2° to the vertical.
[0235] The time at which the strip detaches from the plate following the rupture of the adhesive joint under the effect of this stress is noted.
[0236] The result, expressed in hours, is shown in Table 1.
[0237] A4.5 Shear strength time at 125°C after 7 days of storage the test tube at 50°C:
[0238] The previous test is repeated, except that after cutting the test specimen into a rectangular strip, it is stored for 7 days at a temperature of 50°C and in an atmosphere with 50% humidity, before being fixed onto the glass plate.
[0239] The result, expressed in hours, is shown in Table 1.
[0240] Examples 1 and 2: Room temperature curable adhesive compositions based on GENIOSIL® STP-E30
[0241] The preparation of the composition of example A is repeated as indicated in point A1, except that, after adding the catalyst and silsesquioxane and stirring for 10 minutes, AEROSIL® R202 is introduced, and the mixture is stirred again for about 10 minutes.
[0242] The measurement of the curing time at room temperature and the tensile test are repeated, as indicated in points A2 and A3. The results shown in Table 1 are obtained. For example 2, it is observed that the curing time at room temperature is, compared to example A, considerably reduced (by more than a factor of 3) and that the breaking stress is significantly increased.
[0243] The preparation of the self-adhesive PET backing layer, as indicated in section A4, is also repeated, except that the coated PET sheet is left at room temperature (approximately 23°C) for 7 hours for curing before being laminated onto the protective anti-adhesive layer. The resulting three-layer system is then subjected to the tests described in sections A4.1 to A4.5, which lead to the results shown in Table 1.
[0244] For Examples 1 and 2, the peel results (at room temperature or after 7 days of storage at 50°C) are substantially identical to those of Example A. The instant adhesion (or tack) values obtained for these two examples, although lower than those of Example A, are quite suitable for a self-adhesive substrate. Finally, the shear strength values at 125°C measured for the self-adhesive PET layers of these two examples demonstrate significantly superior cohesion at temperature, even after 7 days of storage at 50°C.
[0245] [Tables 1] Ingredient Content in % wt / w Example A Example 1 Example 2 (A) GENIOSIL® STP-E30 42.4 40.84 40.19 (B) Picco® AR100 51.6 49.71 48.94 (C) AEROSIL® R202 - 3.5 5.0 (D) K-KAT® 5218 1 0.98 0.98 (E) DOW CORNING® 3074 5 4.97 4.89 Curing time at room temperature (hours) 24 ND 7 Peel at room temperature (N / 2.54 cm) 19 21 20 Peel after 7 days at 50°C (N / 2.54 cm) 22 21 20 Instant adhesion (N / (2.54 cm)2) 36 23 18 Shear strength time at 125°C (hours) 24 70 40 Shear strength time at 125°C after 7 days at 50°C (hours) 25 70 42 Tensile strength (in MPa) 0.16 ND 0.39 Elongation at break (in %) 326 ND 300
[0246] ND = Not Determined
Claims
Claims
1. Crosslinkable adhesive composition, characterized in that it comprises: - at least one polymer (A) comprising a hydrolyzable alkoxysilane group; - at least one tackifying resin (B); - at least one pyrogenic silica (C); - at least one crosslinking catalyst (D); and - a silsesquioxane resin (E).
2. Adhesive composition according to claim 1, characterized in that the polymer (A) comprises at least one, and preferably at least two, hydrolyzable groups of formula (I): -Si(R4)p(OR5)3_p (I) in which: - R4 represents a linear or branched alkyl radical comprising from 1 to 4 carbon atoms, with the possibility that when there are several R4 radicals, the latter are identical or different; - R5 represents a linear or branched alkyl radical comprising from 1 to 4 carbon atoms, with the possibility that when there are several R5 radicals, the latter are identical or different, with the possibility that two OR5 groups can be engaged in the same cycle; and - p is an integer equal to 0, 1 or 2, preferably equal to 0 or 1.
3. Adhesive composition according to claim 2, characterized in that the polymer (A) corresponds to one of the formulas (II), (III) or (IV): (10) (IV) in which: - P represents a saturated or unsaturated, linear or branched polymeric radical optionally comprising one or more heteroatoms, such as oxygen, nitrogen, sulfur, silicon, and preferably having a number-average molar mass ranging from 100 g / mol to 48600 g / mol, more particularly from 300 g / mol to 18600 g / mol or from 500 g / mol to 12600 g / mol, - R1 represents a divalent hydrocarbon radical comprising from 5 to 15 carbon atoms which can be aromatic or aliphatic, linear, branched or cyclic, - R3 represents a linear or branched divalent alkylene radical comprising from 1 to 6 carbon atoms, preferably from 1 to 3 carbon atoms, - X represents a divalent radical chosen from -NH-, -NR7- or -S-, - R7 represents a linear or branched alkyl radical comprising from 1 to 20 carbon atoms and which may also comprise one or more heteroatoms, and - f is an integer ranging from 1 to 6, preferably ranging from 2 to 5, preferably from 2 to 4, more preferably ranging from 2 to 3.
4. Adhesive composition according to claim 3, characterized in that the polymer (A) corresponds to one of the formulas (II'), (III') or (IV'): -R—NH- ”n Sii'R (ID ^4^2 ^ 4 (FFQ^RO—R—OR—SI(R ^or:^ (HD (IV') in which: - R2 represents a saturated or unsaturated, linear or branched divalent hydrocarbon radical optionally comprising one or more heteroatoms, such as oxygen, nitrogen, sulfur, silicon, and preferably having a number-average molar mass ranging from 100 g / mol to 48600 g / mol, more particularly from 300 g / mol to 18600 g / mol or from 500 g / mol to 12600 g / mol, and - n is an integer greater than or equal to 0.
5. Adhesive composition according to one of claims 1 to 4, characterized in that the tackifying resin (B) is chosen from: - (i) resins obtained by polymerization of terpenic hydrocarbons and phenols, in the presence of Friedel-Crafts catalysts; - (ii) resins obtained by a process comprising the polymerization of alpha-methyl styrene, said process possibly also comprising a reaction with phenols; - (iii) rosins of natural or modified origin (such as, for example, rosin extracted from pine gum, wood rosin extracted from tree roots and their hydrogenated, dimerized, polymerized or esterified derivatives with monoalcohols or polyols, such as glycerol or pentaerythritol); - (iv) resins obtained by hydrogenation, polymerization or copolymerization (with an aromatic hydrocarbon) of mixtures of unsaturated aliphatic hydrocarbons having approximately 5, 9 or 10 carbon atoms from petroleum fractions; - (v) terpene resins, (which generally result from the polymerization of terpene hydrocarbons - such as mono-terpene (or pinene) - in the presence of Friedel-Crafts catalysts); - (vi) copolymers based on natural terpenes, (such as, for example example, styrene / terpene, alpha-methyl styrene / terpene and vinyl toluene / terpene); or - (vii) acrylic resins having a viscosity at 100°C of less than 100 Pa.s.
6. Adhesive composition according to one of claims 1 to 5, characterized in that the pyrogenic silica (C) is hydrophobic.
7. Adhesive composition according to claim 6, characterized in that the hydrophobic fumed silica (C) is obtained by treatment of a fumed silica with a PolyDiMethylSiloxane.
8. Adhesive composition according to one of claims 1 to 7, characterized in that the pyrogenic silica (C) has a BET specific surface area of at least 10 m2 / g, preferably ranging from 50 to 400 m2 / g.
9. Adhesive composition according to one of claims 1 to 8, characterized in that the silsesquioxane resin (E) corresponds to the following general formula (V): 4 oA 15¾ O / \ \ / Xi \ O ' s \ VSS (V) in which each of R'1 to R'8 represents, independently of one another, a group chosen from: - a hydrogen atom, - a radical chosen from the group consisting of a linear or branched C1-C4 alkoxy radical, a linear or branched alkyl radical comprising from 1 to 30 carbon atoms, an alkenyl radical comprising from 2 to 30 carbon atoms, an aromatic radical comprising from 6 to 30 carbon atoms, an allyl radical comprising from 3 to 30 carbon atoms, an aliphatic cyclic radical comprising from 3 to 30 carbon atoms, an acyl radical comprising from 1 to 30 carbon atoms of carbon, and - a group -OSiR'9R'10 in which R'9 and R'10 represent each, independently of the other, a hydrogen atom or a radical selected from the group consisting of linear or branched C1-C4 alkyls, linear or branched C1-C4 alkoxys, C2-C4 alkenyls, a phenyl, a C3-C6 allyl radical, a C3-C8 cyclic aliphatic radical, and a C1-C4 acyl radical; provided: - that at least one radical among the radicals R'1 to R'8 is a C1-C4 alkoxy radical; and - that at least one radical among the radicals R'1 to R'8 is a phenyl radical.
10. Adhesive composition according to one of claims 1 to 9, characterized in that it comprises: - from 3% to 90% by weight of at least one polymer (A); - from 15% to 80% by weight of at least one tackifying resin (B); - from 1 to 10% of the fumed silica (C); - from 0.01% to 10% by weight of crosslinking catalyst (D); and - from 0.1 to 20% by weight of silsesquioxane resin (E); these percentages by weight being indicated on the basis of the total weight of said composition.
11. Self-adhesive article comprising a support layer coated with a self-adhesive layer, characterized in that said self-adhesive layer consists of the adhesive composition, as defined in one of claims 1 to 10, in the crosslinked state.
12. A method of manufacturing the self-adhesive article as defined in claim 11, characterized in that it comprises: - (a) applying said composition by coating on a carrier surface; - (b) crosslinking said composition, by heating to a temperature ranging from 15°C to 200°C; then - (c) laminating or transferring the crosslinked adhesive composition layer onto a support layer or onto a non-stick protective film.
13. A method of manufacturing the self-adhesive article according to claim 12, characterized in that the crosslinking step (b) is carried out at a temperature ranging from 15°C to 45°C, preferably at room temperature.
14. A bonding method using the self-adhesive article, as defined in claim 11, characterized in that it comprises the following steps: (a) the removal of the protective anti-adhesive layer, where such a layer is present; (b) applying the self-adhesive article to a surface of a product; and (c) applying pressure to said article.