Film-forming composition for metallic surfaces, method for applying such a composition, polymeric film obtained by applying such a composition, and pipe comprising such a film

A film-forming composition with vinyl polymer, vinyl copolymer, and alumina particles addresses the fragility and hydrogen compromise issues of existing coatings, forming a stable film that reduces hydrogen embrittlement and maintains purity in gas transport pipes.

FR3126419B1Active Publication Date: 2024-11-15GRTGAZ
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2021009131
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-01
Publication Date
2024-11-15
Estimated Expiration
2041-09-01

AI Technical Summary

Technical Problem

Existing coatings for protecting metal surfaces from hydrogen embrittlement in gas transport pipes are mechanically fragile, require complex application processes, and can compromise hydrogen purity or stability, making them unsuitable for gas transport applications.

Method used

A film-forming composition comprising vinyl polymer, water-soluble vinyl copolymer, and dispersed alumina particles in an aqueous solvent, optionally with a hydrogen adsorption and diffusion inhibitor, applied through spraying and drying/crosslinking, forms a protective polymeric film that limits hydrogen penetration.

Benefits of technology

The composition forms a mechanically stable, homogeneous film that effectively reduces hydrogen embrittlement and maintains hydrogen purity by limiting diffusion and adsorption, suitable for large-scale application on metal surfaces like gas transport pipes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000017_0000
    Figure 00000017_0000
  • Figure 00000017_0001
    Figure 00000017_0001
  • Figure 00000017_0002
    Figure 00000017_0002
Patent Text Reader

Abstract

TITLE OF THE INVENTION: FILM-FORMING COMPOSITION FOR METAL SURFACES, METHOD FOR APPLYING SUCH A COMPOSITION, POLYMERIC FILM OBTAINED BY APPLYING SUCH A COMPOSITION, AND CONDUCTING A CONTAINING SUCH A FILM. The present invention relates to a film-forming composition for metal surfaces (10), comprising at least one water-soluble vinyl polymer and / or vinyl copolymer, an aqueous solvent, and solid particles of alumina (Al2O3) dispersed in the aqueous solvent. In embodiments, the respective proportions of the composition are, relative to the total mass of the composition: - vinyl polymer and / or vinyl copolymer: 5 to 25% by mass, - Al2O3: 0.2 to 10% by mass, and - aqueous solvent: 70 to 95% by mass. The present invention also relates to a method for applying the composition, a film obtained by the method, and a conduit carrying this film (20). Figure for the abstract: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: FILM-FORMING COMPOSITION FOR METAL SURFACE, METHOD FOR APPLYING SUCH A COMPOSITION, POLYMERIC FILM OBTAINED BY APPLYING SUCH A COMPOSITION AND PROCEDURE FEATURING SUCH A FILM Technical field of the invention

[0001] The present invention relates to a film-forming composition for a metal surface, a method of applying such a composition, a polymeric film obtained by applying such a composition and a pipe comprising such a film.

[0002] The invention applies, in particular, to the gas production and transport industry and in particular to the protection of the internal surface of a steel pipe transporting gaseous hydrogen. State of the art

[0003] The physicochemical properties of hydrogen, and in particular its very small size, cause adsorption of hydrogen gas on metal surfaces, such as steel, followed by migration of hydrogen through the metal structure. This mechanism leads to irreversible accelerated aging of the metal structure. This phenomenon is called hydrogen embrittlement (HEB). HEB occurs in pipes, for example made of steel, which transport hydrogen gas.

[0004] Existing solutions mentioned in the prior art consist of protecting steel from FPH by using an inorganic matrix type coating, such as titanium carbide or titanium nitride. However, this type of coating is difficult to apply in existing pipes. For example, before applying the coating, it is necessary to control the atmosphere or create a vacuum. In addition, the use of sensitive products whose handling is delicate is also necessary for the application of the coating on the surface to be protected. When these coatings have been applied to the metal surface, these coatings have the major disadvantage of being mechanically fragile. In addition, the existence of defects or cracks from the application of the coating or generated after, during use of the pipe, compromises the protective effect of the coating.

[0005] Other solutions are taught in the prior art and are applied to the protection of pipes transporting liquid solutions. However, they are not transposable to pipes transporting a gas. In addition, certain inhibitory compounds hydrogen present in such a coating compromises the purity of the hydrogen gas transported.

[0006] Other solutions known to those skilled in the art consist of using an oxide layer type coating on the metal surface. This metal surface coating solution is known, it is used in particular during the passivation steps of metals, corresponding to a treatment making it possible to form an anti-corrosion oxide layer. However, this coating is not stable since it can be reduced by the gaseous hydrogen transported in the pipe. Statement of the invention

[0007] The present invention aims to remedy all or part of these drawbacks.

[0008] To this end, according to a first aspect, the present invention relates to a film-forming composition for a metal surface which comprises at least one vinyl polymer and / or one vinyl copolymer soluble in water, an aqueous solvent and solid particles of alumina (A12O3) dispersed in the aqueous solvent.

[0009] Thanks to these provisions, the film-forming composition which is the subject of the invention can be applied to a metal surface and thus form a protective film against mechanical embrittlement induced by a gas.

[0010] In embodiments, the composition has respective proportions, relative to the total mass of the composition: - vinyl polymer and / or a vinyl copolymer: 5 to 25% by mass, - A12O3: 0.2 to 10% by mass and - aqueous solvent: 70 to 95% by mass.

[0011] Thanks to these provisions, the composition has better solubilization of the polymers and better unit dispersion of the solid alumina particles (A12O3) and thus makes it possible to improve the barrier properties of the film obtained after application of the composition to the metal surface. In addition, the size of the solid alumina particles in such a composition and the viscosity imparted by the polymer allow the particles to be kept in suspension in the composition. Thus, the deposition and agglomeration of the solid alumina particles in the composition are limited.

[0012] In embodiments, the composition comprises at least one inhibitor of adsorption, absorption and / or diffusion of hydrogen.

[0013] Thanks to these provisions, when the composition is applied as a film on the metal surface, the hydrogen adsorption, absorption and / or diffusion inhibitor improves the protection of this surface against mechanical embrittlement by hydrogen. For example, this protection is obtained during the circulation of hydrogen in a steel pipe comprising this film.

[0014] In embodiments, the proportion of adsorption inhibitor, absorption and / or diffusion, of hydrogen is between 0.005% and 2%, relative to the total mass of the composition.

[0015] Thanks to these provisions, when the composition is applied as a film on the metal surface, the hydrogen adsorption, absorption and / or diffusion inhibitor provides optimal protection of this surface against embrittlement by hydrogen.

[0016] In embodiments, the composition comprises at least one vinyl copolymer which is an ethylene vinyl alcohol copolymer (acronym "EVOH").

[0017] Thanks to these provisions, when the composition is applied as a film on the metal surface, the presence of the EVOH copolymer improves the barrier properties of this film against different molecules, for example gases such as air, hydrogen, oxygen, carbon dioxide, methane or water.

[0018] According to a second aspect, the present invention relates to a method of applying the composition which is the subject of the present invention, to a metal surface, which comprises: - at least one step of spraying the composition onto the surface and - at least one step of drying and / or crosslinking the sprayed composition.

[0019] Thanks to these provisions, the application of the film-forming composition on a large scale is implemented, and in particular on a large metal surface, such as the internal surface of a pipe transporting a gas such as hydrogen. This method also makes it possible to form a homogeneous, continuous and mechanically stable film.

[0020] In embodiments, the method comprises at least two iterations of the spraying step and the drying and / or crosslinking step.

[0021] Thanks to these arrangements, a film of several successive layers is formed, the thickness of which thus improves the barrier effect against a gas, such as hydrogen, by optimizing the drying time. The thicker the film, the greater the barrier effect.

[0022] According to a third aspect, the present invention relates to a polymeric film obtained by application of a composition which is the subject of the present invention, which comprises at least one vinyl polymer and / or one vinyl copolymer and dispersed solid particles of alumina (A12O3), the proportions of which are, relative to the total mass of the film: - vinyl polymer and / or a vinyl copolymer: 70 to 95% by mass and - A12O3: 3.5 to 30% by mass.

[0023] By means of these provisions, a metal surface is protected against gas-induced embrittlement. For example, steel is protected from hydrogen embrittlement by limiting the penetration of hydrogen into the steel surface.

[0024] In embodiments, the polymeric film comprises an inhibitor of adsorption, absorption and / or diffusion of hydrogen, the proportions of the constituents of the film are, relative to the total mass of the film: - vinyl polymer and / or vinyl copolymer: 70 to 95% by mass, - A12O3: 3.5 to 30% by mass and - hydrogen adsorption, absorption and / or diffusion inhibitor: 0.05 to 6% by mass.

[0025] Thanks to these provisions, the hydrogen adsorption, absorption and / or diffusion inhibitor incorporated in the film which is the subject of the present invention improves the protection of the metal surface against embrittlement by hydrogen. For example, this protection is obtained during the circulation of hydrogen in a steel pipe coated with this film.

[0026] In embodiments, the film comprises at least one vinyl copolymer which is an ethylene vinyl alcohol (EVOH) copolymer.

[0027] Thanks to these provisions, the presence of the EVOH copolymer improves the barrier properties against different gases such as air, hydrogen, oxygen, carbon dioxide, methane or water.

[0028] In embodiments, the film has a thickness, after drying, of between 50 micrometers and 1 millimeter.

[0029] Thanks to these provisions, the thickness gives the film improved barrier properties against different gases.

[0030] In embodiments, the Al2O3 particles form fillers having a form factor of between 10 and 1000.

[0031] According to a fourth aspect, the present invention relates to a pipe which comprises a polymeric film which is the subject of the present invention.

[0032] The aims, advantages and particular characteristics of the pipe which is the subject of the present invention being similar to those of the film which is the subject of the present invention, they are not recalled here. Brief description of the figures

[0033] Other advantages, aims and particular characteristics of the invention will emerge from the following non-limiting description of at least one particular embodiment of the composition, the process, the film and the pipe which are the subject of the present invention, with reference to the appended drawings, in which:

[0034] [Fig.l] schematically represents the penetration of hydrogen into the metallic structure, responsible for hydrogen embrittlement,

[0035] [Fig.2] schematically represents the effect of an embodiment of a film po lymeric object of the present invention, on the penetration of hydrogen,

[0036] [Fig.3] schematically represents the effect of an embodiment of a film po lymeric object of the present invention, on the penetration of hydrogen,

[0037] [Fig.4] schematically represents a tortuosity effect linked to the presence of solid alumina particles (A12O3) in the polymer film,

[0038] [Fig.5] schematically represents a tortuosity effect linked to the presence of solid particles of alumina (A12O3) in the polymer film,

[0039] [Fig.6] represents, in the form of a flowchart, a particular embodiment of the method which is the subject of the present invention and

[0040] [Fig.7] schematically represents a particular embodiment of a device for applying the film-forming composition and of a pipe which is the subject of the present invention. Description of the embodiments

[0041] The present description is given without limitation, each characteristic of an embodiment being able to be combined with any other characteristic of any other embodiment in an advantageous manner.

[0042] We recall here the following definitions: - the term “film-forming” refers to a composition forming a film, for example after drying and / or crosslinking; - the term “metal surface” refers to any type of surface comprising a metal, for example an alloy such as steel; - the term “aqueous solvent” means a solvent comprising at least fifty percent water; - the term “hydrogen adsorption, absorption and / or diffusion inhibitor” refers to a compound limiting the propagation and / or adsorption or absorption of hydrogen at the metal surface and / or in the metal structure when applied to the metal surface, - the term “fillers” refers to solid particles.

[0043] It should be noted from now on that the figures are not to scale.

[0044] Film-forming composition

[0045] The film-forming composition which is the subject of the present invention comprises at least one vinyl polymer and / or one vinyl copolymer soluble in water, an aqueous solvent and solid particles of alumina (A12O3) dispersed in the aqueous solvent.

[0046] This film-forming composition is applicable to any type of surface, for example a metal surface 10, and results in the formation of a film 20.

[0047] Preferably, the dispersion of the solid alumina particles in the composition is homogeneous.

[0048] The use of an aqueous solvent in the composition allows good solubilization of the polymers, as well as good unit dispersion of the solid alumina particles (A12O3) in the composition. When the particles are exfoliated, an improvement in the barrier properties of the polymeric film 20 formed from the film-forming composition is observed. Organic solvents such as dimethyl sulfoxide or cyclohexanone do not allow such a unitary dispersion of solid alumina particles (A12O3).

[0049] Preferably, the aqueous solvent is distilled water.

[0050] Preferably, the composition comprises at least one vinyl copolymer which is an ethylene vinyl alcohol copolymer (EVOH).

[0051] Preferably, the composition has respective proportions, relative to the total mass of the composition: - vinyl polymer and / or a vinyl copolymer: 5 to 25% by mass, - A12O3: 0.2 to 10% by mass and - aqueous solvent: 70 to 95% by mass.

[0052] Thanks to these provisions, the composition has an optimal exfoliation of the solid particles of alumina (A12O3), thus making it possible to improve the barrier properties of the film 20 obtained after application of the composition to the metal surface 10. Such a polymer concentration gives the composition an adequate viscosity to facilitate application, for example by a device and according to a method 30 which is the subject of the present invention. The viscosity of the composition is between 30 and 7500 mPa.s and is thus suitable for forming the film 20 with a thickness of between 50 micrometers and 1 millimeter.

[0053] Even more preferably, the composition has respective proportions, relative to the total mass of the composition: - vinyl polymer and / or vinyl copolymer: 5 to 20% by mass, - A12O3: 0.5 to 5% by mass and - aqueous solvent: 75 to 90% by mass.

[0054] In embodiments, the composition which is the subject of the present invention further comprises at least one inhibitor of adsorption, absorption and / or diffusion of hydrogen.

[0055] Thanks to these provisions, the adsorption, absorption and / or diffusion inhibitor, incorporated in the film 20 and derived from the composition which is the subject of the present invention, has better barrier properties against hydrogen, and thus prevents embrittlement by hydrogen of a metal structure.

[0056] The hydrogen adsorption, absorption and / or diffusion inhibitor limits respectively the dissociative adsorption of gaseous hydrogen on the surface of the metal, and the penetration of hydrogen into the metal surface 10. For example, this protection is obtained during the circulation of hydrogen in a steel pipe comprising this film 20.

[0057] The hydrogen adsorption, absorption and / or diffusion inhibitor can be chosen from the following chemical families: - nitriles, benzonitriles, - alcohols, - alkenes, - alkynes, - conjugated cyclic and heterocyclic compounds, - cyanamides, - acids, - isocyanates, - cyanonaphthalene, - amines and other nitrogen compounds, - salts of nitrogen compounds, - carbides, - nitrides and / or - any mixture or solution containing one or more of the above compounds.

[0058] Preferably, the proportion of hydrogen adsorption, absorption and / or diffusion inhibitor is between 0.005% and 2% by mass, relative to the total mass of the composition.

[0059] By way of example, the proportion of hydrogen adsorption, absorption and / or diffusion inhibitor is between 0.03% and 0.07% by mass, relative to the total mass of the composition. These values ​​correspond to a compromise between the adhesion and the performance of the film 20. If the proportion of hydrogen adsorption, absorption and / or diffusion inhibitor is greater than 0.07% by mass, relative to the total mass of the composition, the adhesion of the film is degraded. If the proportion of hydrogen adsorption, absorption and / or diffusion inhibitor is less than 0.03% by mass, relative to the total mass of the composition, the effectiveness is reduced.

[0060] In embodiments, the composition is prepared by mixing two intermediate compositions, for example one composition comprising solid alumina particles and the other composition comprising at least one vinyl polymer and / or one vinyl copolymer.

[0061] Preferably, the two intermediate compositions are prepared simultaneously.

[0062] In other embodiments, the two compositions are prepared successively. For example, the composition comprising the solid alumina particles is obtained by adding a predetermined amount of alumina to water, followed by stirring at room temperature. Then, the composition comprising a polymer is obtained by adding a predetermined amount of solid polymer to water followed by stirring. The composition which is the subject of the present invention is obtained by mixing predetermined amounts of these two compositions, followed by stirring at room temperature. room temperature.

[0063] Preferably, the stirring of the compositions is carried out by an industrial stirrer, for example a mechanical stirrer. Thanks to these arrangements, the preparation of the composition which is the subject of the present invention is possible on an industrial scale.

[0064] In embodiments, the composition comprising the solid alumina particles is subjected to ultrasound.

[0065] In embodiments, the composition comprising the polymer is heated to 90°C and then cooled to room temperature.

[0066] Thanks to these provisions, the solubilization of the polymer in the composition is optimal.

[0067] In embodiments, the composition further comprises a gelling agent configured so that the composition forms a gel. Preferably, the proportion of gelling agent is between 0.01% and 5% by mass and preferably between 1% and 2% by mass, relative to the total mass of the composition. The viscosity of the composition is then increased.

[0068] Example of realization of the composition

[0069] All percentages expressed below are mass percentages (m / m).

[0070] An example of preparation of the composition called “composition C” is described below.

[0071] Two intermediate compositions, called “intermediate compositions A and B” are prepared and then mixed to obtain “composition C”, corresponding to an embodiment of the subject of the invention.

[0072] Intermediate composition A corresponds to a dispersion of alumina (A12O3) at 24% m / m in distilled water. Composition A is obtained by adding 12 grams of alumina (A12O3) in 38 grams of distilled water, followed by stirring with a magnetic bar for 30 minutes at room temperature and exposure to ultrasound for a further 30 minutes using an ultrasonic bath.

[0073] Intermediate composition B corresponds to a composition of 10% EVOH copolymer in distilled water. It is obtained by adding 10 grams of EVOH copolymer, for example Exceval 2117 (registered trademark), to 90 grams of distilled water, followed by stirring with a magnetic bar while heating to 90°C until the copolymer is completely dissolved.

[0074] Composition C is then obtained by mixing 25 grams of composition B, 0.7 grams of composition A and 0.0135 grams of hydrogen adsorption, absorption and / or diffusion inhibitor, for example SurTec 424 (registered trademark), followed by stirring with a magnetic bar at room temperature for 30 minutes.

[0075] Polymeric film

[0076] The polymeric film 20 which is the subject of the present invention is obtained from an embodiment of the composition which is the subject of the present invention described above.

[0077] Preferably, the polymeric film 20 is obtained according to an embodiment of the method which is the subject of the present invention described below.

[0078] Preferably, the proportions are, relative to the total mass of the film: - vinyl polymer and / or a vinyl copolymer: 70 to 95% by mass and - A12O3: 3.5 to 30% by mass.

[0079] Given the composition from which the film is derived, the film 20 has a composite polymer matrix in which the alumina particles are dispersed individually.

[0080] The film 20 is applied as a coating to a metal surface 10 and, thanks to its barrier properties, protects this surface against mechanical embrittlement induced by a gas. For example, this film 20 protects the steel from embrittlement by hydrogen by limiting the contact between the hydrogen and the surface of the steel.

[0081] The barrier properties of this film 20 for coating a metal surface 10 allow: - a slowing down of the diffusion of a gas, such as hydrogen gas, towards the metal surface 10, and - a local decrease in the concentration of a gas, such as hydrogen gas, on the metal surface 10.

[0082] Thus, the permeability of the gas in the polymeric film 20 and the penetration of the gas into the metal surface 10 are greatly reduced. For example, the permeability is divided by two, three or four.

[0083] [Fig.l], which is not to scale, shows a schematic representation of a metal surface 10 in which hydrogen penetrates and diffuses into the metal surface 10. The metal surface 10 does not have a polymeric film which is the subject of the present invention.

[0084] Figures 2 and 3, which are not to scale, show the barrier properties of the polymeric film, 20 or 21, serving as a coating for the metal structure 10. Figures 2 and 3, unlike [Fig.l], show that the polymeric film, 20 or 21, limits the penetration of hydrogen into the metal surface 10.

[0085] The presence of at least one vinyl polymer and / or vinyl copolymer forming the film gives the film its barrier properties against different gases such as air, hydrogen, oxygen, carbon dioxide, methane or water.

[0086] Preferably, the film 20 comprises at least one vinyl copolymer which is an ethylene vinyl alcohol copolymer (EVOH).

[0087] Dispersed solid particles of alumina (A12O3) allow an improvement of the barrier properties of the film, notably by an increase in tortuosity.

[0088] In embodiments, as shown in [Fig. 3], the film 21 comprises several successive layers 210, 211 and 212, bonded together. Each layer is obtained after application and drying of the composition which is the subject of the present invention. [Fig. 3], which is not to scale, shows the barrier properties of the film serving as a coating for the metal structure 10 and consisting of three successive layers 210, 211 and 212. Preferably, each layer has a thickness of between 20 and 30 micrometers.

[0089] Thanks to these provisions, the barrier effect against a gas, such as hydrogen, is improved.

[0090] Preferably, the polymeric film is a film of a composite nature consisting of a polymeric matrix, and one or more fillers formed by the alumina particles having a high form factor, that is to say having a dimension much smaller than the other two, for example by a factor of 10 to 1000, thus allowing a tortuosity effect.

[0091] Figures 4 and 5, which are not to scale, show a schematic representation of two tortuosity effects applied to a gas within the films 22 or 23, which are the subject of the present invention. The gas paths 221 or 231, used to illustrate the tortuosity effect, are represented by dotted arrows.

[0092] The tortuosity effects correspond to an extension of the diffusion path of the diffusing molecules, such as the constituent molecules of a gas, for example hydrogen gas. This extension implies a reduction in the diffusion coefficient through the polymer film, and therefore a reduction in the permeability of the diffusing molecules through this film. Thus the penetration of the diffusing molecules into the metal surface 10 is very limited.

[0093] In [Fig.4], the tortuosity effect illustrated by the path 221 is linked to the shape of the solid particles 220 dispersed in the film 22. The particles 220 have a substantially spherical shape. This effect is present, for example, in a composite polymer matrix.

[0094] In [Fig. 5], the tortuosity effect illustrated by the path 231 is linked to the shape of the solid particles 230 dispersed in the film 23. This effect is present, for example, in a composite polymer matrix. The solid particles 230 have a substantially platelet-like shape. The path 231 created by the substantially platelet-like particles 230 and traveled by the diffusing molecules is greater than the path 221 created by the substantially spherical particles 220. Thus, the tortuosity within the film 23 is greater than the tortuosity within the film 22. The film 23 has better barrier properties compared to the film 22.

[0095] Preferably, the film which is the subject of the present invention comprises a structure similar to film 23, i.e. with substantially platelet-like solid particles.

[0096] In embodiments, the polymeric film comprises an inhibitor of adsorption, absorption and / or diffusion of hydrogen, the proportions of the constituents of the film are, relative to the total mass of the film: - vinyl polymer: and / or a vinyl copolymer: 70 to 95% by mass, - A12O3: 3.5 to 30% by mass and - hydrogen adsorption, absorption and / or diffusion inhibitor: 0.05 to 6% by mass.

[0097] In embodiments, the film has a thickness of between 50 micrometers and 1 millimeter and preferably greater than 250 micrometers.

[0098] Permeability tests

[0099] Helium permeability tests were carried out in order to highlight the tortuosity effect of the solid alumina particles (A12O3) in the polymeric film obtained after applying the composition C described above to samples. The samples used are prepared by depositing a porous fabric disc in a silicone mold in the shape of a disc of the same diameter as the porous fabric disc. Then, 13 grams of the composition C, described above, is applied and impregnated into the fabric uniformly. Then, the fabric impregnated with composition C is dried for 72 hours at room temperature and 6 hours at 60°C. The following table shows the results of the permeability measurements for the polymeric films composed of the EVOH copolymer with or without solid alumina particles (A12O3)•

[0100] [Tableauxl] Nature of the film Permeability coefficient P, g / (msbar) EVOH alone 9.44 xlO9 EVOH + A12O3 3.21 xlO9

[0101] The permeability coefficient P is divided by three when the film composed of the EVOH copolymer includes solid alumina particles (A12O3), highlighting the tortuosity effect of these particles and thus the reduction in the permeability of helium.

[0102] Method of applying the composition

[0103] The present invention also relates to a method 30 for applying the film-forming composition to a metal surface which is the subject of the present invention, which comprises: - at least one step 301 of spraying the composition onto the surface and - at least one step 302 of drying and / or crosslinking the sprayed composition.

[0104] In embodiments, when the composition forms a gel, the step of pul Verification 301 is replaced by an application step. Application can be carried out using a brush or a reservoir and a piston applicator. In other words, the gel is deposited by contact.

[0105] [Fig. 6] shows a flowchart representing a particular embodiment of the method which is the subject of the present invention. The optional steps are shown in dotted lines. The embodiments of the method 30 which is the subject of the present invention are illustrated by means of the device 50 and the pipe 40 shown in [Fig. 7],

[0106] In embodiments, the metal surface corresponds to the internal surface 400 of pipe 40 used for transporting a gas. For example, pipe 40 is a pipe for transporting and supplying natural gas, such as methane, into which hydrogen gas has been injected.

[0107] In embodiments, the spraying step 301 is implemented by a spraying device 50.

[0108] Thanks to these provisions, the spraying step 301 of the composition which is the subject of the present invention is carried out on the internal surface 400 of a previously installed pipe 40. For example, the pipe 40 has a diameter of less than 1.2 meters and includes bent parts.

[0109] In embodiments, such as shown in [Fig.7], the spraying device 50 comprises: - a means of transport, - a storage tank 500 for the composition which is the subject of the present invention to be sprayed and - at least one spray head 503 connected to the reservoir 500 and sending the sprayed composition 505.

[0110] Preferably, the device 50 comprises a movement means comprising a carriage 501 mounted on wheels 502. The carriage supports the tank 500. Even more preferably, the carriage 501 comprises a motor configured to actuate at least one wheel 502 and cause the carriage 501 to move in the pipe 40.

[0111] In embodiments (not shown), the carriage comprises pads. Preferably, the pads are arranged radially around the tank.

[0112] In embodiments (not shown), the pads rest totally or partially on the internal surface of the pipeline.

[0113] In embodiments, as shown in [Fig.7], the device 50 comprises an electrical power source. The electrical power source comprises a cable 504 connected to an electrical network. In embodiments (not shown), the electrical power source is a self-contained electrical power source, for example a battery. The electrical power source A self-contained device is mounted on the carriage and supplies electrical power to the motor. In embodiments (not shown), the device is manually pulled inside the conduit 40.

[0114] Preferably, the composition is sprayed, during the spraying step 301 by means of a spray head 503, having the shape of a truncated cone provided with orifices through which the composition is ejected. The spraying 505 of the composition is represented by the dotted arrows in [Fig.7]. For example, the device 50 carries out the spraying step 301 in pipes which may have a length of at least 100 kilometers and a diameter of between 2.5 centimeters and 1.5 meters.

[0115] In embodiments (not shown), the spraying device comprises several spraying heads.

[0116] In other embodiments (not shown), the spray head performs the spraying step by rotation. For example, the rotation speed is between 5 and 50 revolutions per minute. The spraying step 301 is thus implemented by the centrifugal force linked to the rotation speed of the spray head.

[0117] In embodiments, the spray head performs the spraying step by ejecting a static mixture under pressure. For example, the spraying pressures are between 20 and 200 bar.

[0118] Thanks to these provisions, the device makes it possible to spray the composition which is the subject of the present invention over the entirety of an internal surface 400 of a pipe 40 with a diameter of between 200 and 1200 millimeters.

[0119] In embodiments (not shown), the spraying device 50 comprises a camera connected to a terminal which comprises: - at least one screen for displaying the information given by the camera and - at least one human-machine interface, for example a keyboard and a mouse, configured to control the spraying device 50.

[0120] Thanks to these provisions, the spraying step 301 is monitored and controlled remotely by an operator during use of the device 50.

[0121] In embodiments, the step of drying and / or crosslinking 302 of the sprayed composition is carried out by pulsing and / or by circulating a flow of hot air. For example, one or more fans are installed in the duct to circulate the flow of hot air.

[0122] Thanks to these provisions, the drying and / or crosslinking step is accelerated.

[0123] In embodiments, the step of drying and / or crosslinking the sprayed composition is carried out by emitting infrared radiation, from one or more infrared radiation emitting lamps.

[0124] In embodiments, the method comprises at least two iterations 303 of the spraying step 301 and the drying and / or crosslinking step 302. For example, the iterations 303 are carried out by circulation of two spraying devices in the pipe carrying out the spraying step 301, the time interval between the passage of the two robots being configured so that the drying step 302 of the first iteration is carried out between the passage of the two robots.

[0125] In embodiments, the method 30 comprises, upstream of the spraying step 301, a step 300 of preparing the metal surface. For example, the preparation step 300 comprises a step of stripping by projection of abrasives, these abrasives then being removed from the metal surface, for example, by means of a vacuum cleaner or an oil-free compressed air hose.

[0126] Pipe coated with polymeric film

[0127] The present invention also relates to a pipe which comprises a polymeric film having the characteristics stated above. For example, the pipe 40 comprises a polymeric film 20 obtained by applying a composition which is the subject of the present invention according to the method 30. These elements are described above with reference to FIGS. 2, 6 and 7.

Claims

Claims

1. Film-forming composition for a metal surface (10) characterized in that it comprises at least: - a vinyl polymer and / or a vinyl copolymer soluble in water, - an aqueous solvent, - solid particles of alumina (A12O3) dispersed in the aqueous solvent and - an inhibitor of adsorption, absorption and / or diffusion of hydrogen.

2. Composition according to claim 1, in which the respective proportions are, relative to the total mass of the composition: - vinyl polymer and / or a vinyl copolymer: 5 to 25% by mass, - A12O3: 0.2 to 10% by mass, - aqueous solvent: 70 to 95% by mass and - hydrogen adsorption, absorption and / or diffusion inhibitor: 0.005% and 2% by mass.

3. Composition according to one of claims 1 or 2, in which at least one vinyl copolymer is an ethylene vinyl alcohol copolymer (EVOH).

4. Method (30) for applying the composition according to one of claims 1 to 3, on a metal surface, characterized in that it comprises: - at least one step of spraying (301) the composition on the surface and - at least one step of drying and / or crosslinking (302) the sprayed composition.

5. Method (30) according to claim 4, which comprises at least two iterations (303) of the spraying step (301) and the drying and / or crosslinking step (302).

6. Polymeric film (20, 21) obtained by applying a composition according to one of claims 1 or 2, in which the proportions are, relative to the total mass of the film: - vinyl polymer and / or a vinyl copolymer: 70 to 95% by mass, - A12O3: 3.5 to 30% by mass, and - hydrogen adsorption, absorption and / or diffusion inhibitor: 0.05 to 6% in bulk.

7. The polymeric film (20, 21) of claim 6, wherein at least one vinyl copolymer is an ethylene vinyl alcohol copolymer (EVOH).

8. Polymeric film (20, 21) according to one of claims 6 or 7, which has a thickness, after drying, of between 50 micrometers and 1 millimeter.

9. Polymeric film (20, 21) according to one of claims 6 to 8, in which the Al2O3 particles form fillers having a form factor of between 10 and 1000.

10. A conduit (40) which comprises a polymeric film (20, 21) according to one of claims 6 to 9.