METHOD FOR RECOVERING INDIUM FROM A SUBSTRATE COMPRISING INDIUM TIN OXIDE AND A METALLIC LAYER
The oxalic acid-based process for recovering indium from photovoltaic panels addresses the inefficiencies of current methods by enabling selective indium recovery with reduced environmental harm and cost, using a green solvent to form indium oxalate precipitate.
Patent Information
- Application Number
- FR2022004857
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-05-20
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-05-20
AI Technical Summary
Current processes for recovering indium and silver from photovoltaic panels are complex, expensive, and environmentally hazardous due to the use of toxic chemicals and multiple steps, failing to achieve efficient and sustainable recycling.
A process using oxalic acid to selectively dissolve indium-tin oxide (ITO) in a green solvent, forming indium oxalate precipitate while leaving other elements intact, reducing the need for concentrated acids and simplifying the recycling process.
The method achieves efficient and selective recovery of indium with reduced environmental impact and cost, minimizing reagent consumption and the number of steps, while maintaining the integrity of other panel components.
Smart Images

Figure 00000013_0000 
Figure 00000013_0001 
Figure 00000013_0002
Abstract
Description
Title of the invention: METHOD FOR RECOVERING INDIUM FROM A SUBSTRATE COMPRISING INDIUM TIN OXIDE AND A METAL LAYER Technical field
[0001] The present invention relates to the general field of recycling photovoltaic panels.
[0002] The invention relates more particularly to a method for recovering a transparent conductive oxide from a substrate comprising a transparent conductive oxide locally covered by a metal.
[0003] The invention also relates to a method for recycling a photovoltaic panel, containing photovoltaic cells, for example made of silicon.
[0004] The invention is particularly interesting since it makes it possible to selectively recover the indium present in photovoltaic cells. STATE OF THE PRIOR ART
[0005] The recycling of photovoltaic (PV) panels has become a major issue since August 13, 2012, since, on that date, the Directive on Waste Electrical and Electronic Equipment (WEEE) was extended to photovoltaic (PV) panels.
[0006] Photovoltaic panels generally comprise several photovoltaic cells coated in a polymer, the whole being arranged between two plates, for example made of glass. Existing photovoltaic cells may, for example, be made of silicon. By way of illustration and not limitation, a heterojunction silicon cell (HJT) may comprise a monocrystalline silicon substrate covered, on both sides, by layers of amorphous silicon (P and N+). These layers are themselves covered with the transparent conductive oxide (TCO) film and then by a conductive grid.
[0007] Thus, a photovoltaic module with silicon photovoltaic cells is therefore mainly composed of glass (74% of the total weight), aluminum (10%), polymer (approximately 6.5%) and silicon (approximately 3%). Metals (zinc, lead, copper and silver) represent only a negligible part of the total mass of the photovoltaic panel.
[0008] The minimum recovery and recycling objectives are therefore easily achieved by photovoltaic recovery of the glass and the aluminum frame alone.
[0009] Current processes focus on the dismantling of modules by chemical or thermal means and then on the recycling of the different elements using specialized reprocessing methods.
[0010] Silver represents the metal constituting the highest added value (nearly 90% of the value of the cell). This is why silver recovery represents a major challenge for the sustainability of the recycling sector.
[0011] It is also interesting to recover the silicon plates and the metals from the transparent conductive oxide layers.
[0012] For this, conventionally, the photovoltaic cells of the photovoltaic modules are chemically treated by total dissolution of the metallic elements (Cu, Ag, Sn, Pb, Al, etc.), the anti-reflectors and the n-doped layer to recover the silicon. The dissolution can be carried out in treatment baths composed of various acids (for example, HF, HNO3, H2SO4) concentrated alone or in a mixture and often brought to a boil.
[0013] For example, in document CN 102 343 352 A describes a multi-step process for recovering silicon wafers without damaging the anti-reflective layer or the PN junction. The process is divided into several steps. First, organic solvents such as ethanol, acetone or isopropyl alcohol are used to dissolve the organic part of the metallization and thus separate it from the silicon wafer. This step can be carried out under ultrasound. Then, nitric acid (concentration of 50 to 65% by mass) or sulfuric acid (concentration of 70 to 98% by mass) is used to remove the remaining metal and glass residues. Then hydrochloric acid is used to remove the metal ions. Finally, a final cleaning with hydrofluoric acid removes the remaining silicon oxide. Between each step, the cells are rinsed with water. This allows the silicon wafer to be recycled.
[0014] Document US 2011 / 0083972 A1 describes an electrolytic process for recycling active elements, specifically aimed at removing the transparent conductive oxide coating, for example indium tin oxide (or ITO for 'indium tin oxide'). The substrate is immersed in an acidic (hydrochloric acid or sulfuric acid) or basic (sodium hydroxide or potassium hydroxide) bath. It is connected to a DC power source, to which a voltage is applied so that it acts as a cathode (negative electrode). The cathodic potential generates protons which cause the layer to dissolve. The system is closed with an anode immersed in the solution which is connected to the power source. This electrolytic process is not concerned with the recovery of silver.
[0015] However, these processes have many drawbacks, particularly due to the nature of the chemical baths and the complexity of the processes (numerous stages).
[0016] The publication “Optimization of indium recovery from waste crystalline Silicon heterojunction solar cells by acid leaching”. (Solar Energy Materials and Solar Cells 2021, 230, 111218) describes a method for treating HJT cells having an indium-tin layer covered by silver metallizations. First, the HJT cell is immersed in a basic sodium hydroxide bath to separate the metallizations from the cell surface, then the cell is immersed in an acid bath (hydrochloric, sulfuric or nitric) to dissolve the indium. The optimal conditions were obtained for a sodium hydroxide concentration of 10% at 90°C and for an H2SO4 concentration of 6 mol.L 1 at 93°C. However, such conditions can generate significant effluents that must subsequently be neutralized, which increases the cost of the process, and also poses significant risks to humans and the environment.
[0017] Currently, the processes implemented for the recovery of indium are complex, expensive, reagent-intensive and / or dangerous and, consequently, induce a significant economic and environmental cost.
[0018] Thus, none of the current processes allows the recovery of silver and indium in a satisfactory manner. Statement of the invention
[0019] An aim of the present invention is to propose a method for recovering the indium present in a substrate containing indium-tin oxide and a metal layer made of a platinum group metal or silver, the substrate originating for example from a photovoltaic module to be recycled, the method having to be simple to implement, inexpensive and not requiring the use of a product toxic to the environment and / or to the health of the people implementing the method.
[0020] For this purpose, the present invention proposes a method for recovering the indium contained in a substrate comprising an indium-tin oxide film locally covered by a metal layer of a platinum group metal or silver, the method comprising a dissolution step during which the substrate is immersed in a dissolution solution comprising oxalic acid, whereby the indium-tin layer is selectively dissolved and an indium oxalate precipitate is formed, the dissolution of the indium-tin oxide leading to the release of the metal layer.
[0021] The invention is fundamentally distinguished from the prior art by the use of an oxalic acid solution to carry out the dissolution step. The selective dissolution of the thin transparent oxide layer into indium tin oxide (ITO) is followed by precipitation of the indium in the form of an indium oxalate. At the same time as the indium dissolves, the tin dissolves. However, it does not precipitate and remains in solution. Thus, at the end of this step, a moderately acidic liquid enriched in tin is obtained, comprising solids: the indium oxalate precipitate and the metal layer in solid form.
[0022] This approach makes it possible, in a single step, to dissolve the indium and precipitate it in the form of oxalate and thus to easily separate it from the other elements in the dissolution solution.
[0023] Furthermore, this dissolution is carried out in a green solvent which accepts numerous treatment cycles, increasing the economic and environmental interest. This approach makes it possible to limit the consumption of reagents, avoids the use of various concentrated acids and reduces the number of steps.
[0024] Advantageously, the concentration of oxalic acid is between 0.1 M and 2 M.
[0025] Advantageously, the dissolution step is carried out at a temperature between 20°C and 120°C, and preferably between 50°C and 80°C.
[0026] Advantageously, the solid / liquid ratio is between 1 and 40%, and preferably between 10% and 20%.
[0027] Advantageously, the solution further comprises an additional acid at a concentration of less than 1 M, and preferably less than 0.2 M. Preferably, the additional acid is sulfuric acid.
[0028] Advantageously, the substrate further comprises a support, the indium-tin oxide film being arranged between the support and the metal layer, the support containing silicon or copper, indium and gallium selenide (CIGS).
[0029] Advantageously, the substrate is a photovoltaic cell or photovoltaic cell waste, for example a heterojunction cell or a CIGS cell. The metal layer, preferably silver, forms the current collectors. The method makes it possible to selectively dissolve the ITO layer of the photovoltaic cell, for example a heterojunction silicon cell (HJT), which separates the collectors from the body of the silicon cell, without dissolving elements other than the transparent conductive oxide layer of indium-tin oxide.
[0030] According to an advantageous embodiment, the method comprises the following steps:
[0031] a) providing a photovoltaic panel comprising cables, a junction box, a metal frame, photovoltaic cells encapsulated in a polymer layer and electrical connectors,
[0032] b) remove the cables, the junction box and the metal frame of the photovoltaic panel,
[0033] c) carrying out a thermal, chemical and / or mechanical treatment to remove the polymer layer encapsulating the photovoltaic cells,
[0034] d) recovering the photovoltaic cells, the photovoltaic cells forming a substrate containing a film of indium tin oxide locally covered by a metallic layer, preferably silver,
[0035] e) implementing the indium recovery step as defined previously.
[0036] Advantageously, the method comprises, after step e), the following subsequent steps: recovery of the indium precipitate, thermal treatment of the indium precipitate, for example at a temperature between 600°C and 700°C, whereby an indium oxide is formed.
[0037] The process has many advantages:
[0038] - the process does not require the use of a highly concentrated acid solution or ionic liquid,
[0039] - considerably reduce the constraints linked to the use of concentrated acid and to temperature, such as the use of nitric acid for the dissolution of silver and / or indium,
[0040] - the process does not release harmful gases and does not degrade the reaction medium,
[0041] - the process can be carried out under atmospheric conditions (in air),
[0042] - the process can be carried out at room temperature (typically 25°C), which avoids the supply of thermal energy,
[0043] - the metal layer is not dissolved and is thus easily recoverable,
[0044] - allow selective dissolution of the transparent oxide layer, avoiding the dissolution of the collector, which reduces the consumption of reagents and reduces the number of steps,
[0045] - using an oxalate ion to selectively dissolve and precipitate indium by compared to tin; thus, the number of treatment cycles is increased and effluents are considerably reduced,
[0046] - not to implement an electrodissolution or electrodeposition step (process said electroless) to dissolve and recover the indium.
[0047] Other characteristics and advantages of the invention will emerge from the additional description which follows.
[0048] It goes without saying that this additional description is given only as an illustration of the subject of the invention and must in no case be interpreted as a limitation of this subject. Brief description of the drawings
[0049] The present invention will be better understood on reading the description of exemplary embodiments given purely for informational purposes and in no way limiting, with reference to the appended drawings in which:
[0050] [Fig. 1a]
[0051] [Fig.lb] are photographic images taken at different times during the dissolution of an ITO salt in an oxalic acid solution at 1M and 70°C, according to a particular embodiment of the invention.
[0052] [Fig. 1e] is a photographic image of an ITO powder (left) and an indium oxalate precipitate (right) obtained after the dissolution step shown in Figures 1a and 1b.
[0053] [Fig.2] is a diffractogram of the indium oxalate precipitate of [Fig. 1c] (black) and the product In(C2O4)i 5(H2O)3 (card 01-73-2642 in gray).
[0054] [Fig.3a]
[0055] [Fig.3b] are photographs of an HJT plate before treatment in IM oxalic acid at 22°C.
[0056] [Fig.3c]
[0057] [Fig.3d] are photographs of an HJT plate after treatment in IM oxalic acid at 22°C, according to a particular embodiment of the invention.
[0058] [Fig.4] is a photograph of an HJT plate after treatment in acid IM oxalic acid at 100°C for 2 hours, according to a particular embodiment of the invention.
[0059] DETAILED DESCRIPTION OF PARTICULAR EMBODIMENTS
[0060] Subsequently, even if the description refers to the recovery of photovoltaic panels or modules; the invention is transposable to other substrates containing indium-tin oxide and a metallic layer of silver or a platinum group metal (PGM). The invention is for example transposable to fields related to optics and / or electronic conduction such as electrochromic devices, organic flexible solar cells, screens (TV, telephones, etc.), deformation sensors, or even electromagnetic shielding.
[0061] The process for recycling a photovoltaic panel to recover indium includes the following steps:
[0062] a) provide a photovoltaic panel,
[0063] b) remove the cables, the junction box and the metal frame of the photovoltaic panel,
[0064] c) carrying out a thermal, chemical and / or mechanical treatment to remove the polymer layer encapsulating the photovoltaic cells and the electrical connectors,
[0065] d) recovering the photovoltaic cells, the photovoltaic cells forming a substrate containing an indium-tin oxide film locally covered by a metal layer, and more particularly by a silver layer,
[0066] e) implementing an indium recovery step.
[0067] The photovoltaic panel to be recycled includes cables, a junction box and a metal frame, a polymer layer (typically ethyl vinyl acetate (EVA)), electrical connectors and photovoltaic cells.
[0068] The method is more particularly described for a photovoltaic panel but several photovoltaic panels could be treated simultaneously.
[0069] The photovoltaic cell comprises a substrate with various recoverable elements. In particular, the substrate may successively comprise a support, a transparent conductive oxide (TCO) film, and a metallization layer partially covering the TCO. The TCO film is thus accessible for etching.
[0070] Hereinafter, we will describe more particularly a substrate comprising a support, a transparent conductive oxide film and a metal layer (also called a metallization layer). However, the method can also be implemented for a substrate formed from a transparent conductive film and a metal layer.
[0071] Photovoltaic cells can be made of crystalline silicon, polycrystalline silicon, CIGS or even perovskite.
[0072] A heterojunction cell (HJT) will preferably be chosen.
[0073] By way of illustration and not limitation, the HJT cell may comprise a monocrystalline silicon substrate covered, on both sides, by layers of amorphous silicon (P and N+). The amorphous silicon layers may have a thickness of around ten nanometers. These layers are themselves covered with the conductive transparent oxide film and then by a conductive grid.
[0074] In the context of the invention, the TCO film is an indium-tin oxide (or ITO for "Indium Tin Oxide") film. LTTO comprises, for example, 97% indium oxide (In2O3) and 3% tin oxide SnO2.
[0075] The metallization layer forms a conductive grid.
[0076] The metallization layer can represent from 0.01% to 1% by mass of the cell.
[0077] The metallization layer is a metallic layer made of a metal from the group of platinum or silver.
[0078] The platinum group metal is selected from ruthenium, rhodium, palladium, osmium, iridium and platinum. Preferably, it is platinum.
[0079] For example, for an HJT cell, an indium metallization layer may represent 0.27% by mass of the cell.
[0080] Preferably, the metal layer is silver.
[0081] The metallic layer may be made of pure silver (i.e. the layer contains at least 99% silver). It is, for example, made with a silver metallization paste.
[0082] Alternatively, it may contain one or more other elements, for example, selected from lead, tin and copper. The connectors are, for example, formed from a copper core coated with Sn62Pb36Ag2.
[0083] Steps b) and c) make it possible to separate and detach the photovoltaic cells as well as the electrical connectors containing silver from the other elements of the photovoltaic panel. Once the photovoltaic cells have been detached, they are advantageously disconnected from each other and, optionally, from the electrical connectors not containing silver.
[0084] At the end of steps b) and c), the elements of interest of the photovoltaic panel have been separated.
[0085] The photovoltaic cells are thus recovered (step d).
[0086] Each photovoltaic cell represents a substrate containing indium and silver to be recovered during step e).
[0087] In step e), a dissolution step is carried out during which the substrate is immersed in a dissolution solution. The dissolution solution comprises oxalic acid. This step leads to the selective dissolution of indium and the formation of an indium oxalate precipitate. The metal layer is thus released from the rest of the substrate.
[0088] This step prevents the emission of gas (flammability, volatility) and / or degradation of the solution.
[0089] The dissolving solution is an aqueous medium comprising oxalate ions. It is obtained by mixing oxalic acid and water. The oxalate ions are necessary to promote dissolution and allow precipitation.
[0090] Silver is not dissolved or is very little dissolved in the acid solution. The dissolution of silver is considered negligible during this step. The same applies to a platinum group metal.
[0091] The dissolving solution is a low concentration oxalic acid solution. By low, it is meant that the oxalic acid concentration is between 0.1 and 2 mol / L and preferably between 0.1 and 1 mol / L.
[0092] According to a particular embodiment, it is also possible to make a mixture of oxalate ions with another mineral or organic acid. Preferably, these are mineral acids, in particular sulfuric acid and hydrochloric acid. An acid which avoids the dissolution of silver and more specifically sulfuric acid which is inexpensive will preferably be used.
[0093] This additional acid preferably has a concentration of less than 1 M, and preferably less than 0.2 M.
[0094] The solid / liquid ratio is between 1% and 40%, and preferably, the solid / liquid ratio is between 1% and 30%. This ratio is noted S / L. Preferably, the S / L ratio is of the order of 15%. The solid phase corresponds to the substrate immersed in the dissolution solution. The liquid phase corresponds to the acid solution. This ratio corresponds to the mass of solid, in grams, divided by the volume of the solution, in milliliters. Thus, an S / L ratio between 1% and 40% corresponds to a mass concentration of the metal oxide in the acid solution between 0.01 g / mL and 0.4 g / mL. For S / L values of less than 1%, the dissolution efficiency is also high. However, the quantity of acid used is considerably high compared to the quantity of metal to be dissolved, and the quantity of reagents lost is substantial.
[0095] The temperature of the acid solution is advantageously between 15°C and 100°C. Preferably, the temperature is between 20°C and 70°C, for example around 50°C to minimize toxicity and reduce the energy consumption of the process. There is advantageously no need to supply thermal energy to dissolve the TCO. However, an increase in temperature may advantageously be carried out to improve the dissolution rate without degradation of the medium. To improve the kinetics, a temperature between 50°C and 100°C and even more preferably between 70°C and 100°C will preferably be chosen.
[0096] The pressure is preferably ambient pressure (typically 1 bar).
[0097] A control can be carried out to maintain the pH between 1 and 4.
[0098] Optionally, the solution may comprise a drying agent, and / or an agent promoting the transport of matter (viscosity, ionic conductivity).
[0099] The dissolution step can be carried out with stirring.
[0100] At the end of the process, the indium precipitate can be recovered. Advantageously, the precipitate is subjected to a heat treatment at a temperature between 600°C and 700°C in order to form indium oxide.
[0101] The silver layer, in solid form, can also be easily extracted from the dissolution solution.
[0102] The tin dissolved in solution can be recovered, for example by an electrodeposition step.
[0103] A person skilled in the art may choose different separation and recovery techniques depending on the elements. For example, he may choose to implement: an ionic flotation step, screening, or even electrostatic separation.
[0104] The dissolution solution can then be used for a new treatment cycle.
[0105] Illustrative and non-limiting examples of embodiments j.
[0106] Test 1: Dissolution of ITO in oxalic acid medium:
[0107] An ITO powder is leached at 70 °C in an oxalic acid bath with a concentration of IM. The treatment time is 5 hours with a solid ratio liquid of 1 / 1000 corresponding to an indium concentration in solution of 0.745 g / L (Figures 1a and 1b). This test simulates the treatment of HJT cells with a ratio of 15%. A color change is observed: the ITO powder is yellow and the precipitate is white ([Fig. 1c]). XRD analysis indicates that the white product resulting from the leaching is a precipitate of hydrated indium oxalate ([Fig. 2]).
[0108] An ICP-OES analysis was performed. The following table lists the results of the analysis obtained on the ITO powder before leaching and on the white precipitate formed after leaching. Indium Tin In / Sn ITO Powder (%m) 74.5 4.2 18 Precipitate (%m) 36.0 0.16 225
[0109] It is observed that the powder is purified 225 times in tin, confirming the selectivity of the process of dissolution / precipitation of indium by an acid bath composed of oxalates.
[0110] Test 2: Treatment of an HJT cell in IM oxalic acid medium at 22°C:
[0111] In this test, HJT cells comprising ITO disposed between the silicon and silver connectors. The dissolution solution is a 1M oxalic acid solution at 22 °C (200 mL). The cells are immersed in this solution for 48 hours. The solution is stirred (400 rpm). As observed in Figures 3a and 3b, before treatment the cell is intact, with the presence of silver metallization ("fingers") (white), then after treatment the plate is completely devoid of metal (Figures 3c and 3d). This is solid in solution. The detachment of the silver collectors is associated with the dissolution of the ITO layer. There is a physical separation of silver and silicon.
[0112] Test 3: Treatment of an HJT cell in IM oxalic acid medium at 100°C:
[0113] The treatment of an HJT cell is carried out in IM oxalic acid medium at 100°C. for 2 hours, with a volume of 200 mL. The HJT cell is immersed in the bath with stirring at 400 rpm. As observed in [Fig.4], after treatment the silver metallizations ("fingers") are detached from the silicon and intact. After treatment the silicon is completely free of metal. The detachment of the silver collectors is associated with the dissolution of the ITO layer. There is a physical separation of silver and silicon.
Claims
Claims
1. A method for recovering indium contained in a substrate comprising an indium-tin oxide film locally covered by a metallic layer, made of silver or a platinum group metal, the method comprising a dissolution step during which the substrate, locally covered by the metallic layer, is immersed in a dissolution solution comprising oxalic acid, whereby the indium-tin layer is selectively dissolved and an indium oxalate precipitate is formed, the dissolution of the indium-tin oxide leading to the release of the metallic layer.
2. Method according to claim 2, characterized in that the concentration of oxalic acid is between 0.1 and 2 mol / L.
3. Method according to one of claims 1 and 2, characterized in that the dissolution step is carried out at a temperature between 20°C and 120°C, and preferably between 50°C and 80°C.
4. Method according to any one of the preceding claims, characterized in that the solid / liquid ratio is between 1 and 40%, and preferably between 10% and 20%.
5. Method according to any one of the preceding claims, characterized in that the solution further comprises an additional acid at a concentration lower than 1 M, and preferably lower than 0.2 M.
6. A method according to claim 5, characterized in that the additional acid is sulfuric acid.
7. A method according to any one of the preceding claims, characterized in that the substrate further comprises a support, the indium-tin oxide film being disposed between the support and the metal layer, the support containing silicon or copper indium gallium selenide (CIGS).
8. A method according to any one of the preceding claims, characterized in that the substrate is a photovoltaic cell or photovoltaic cell waste, for example a heterojunction cell or a CIGS cell.
9. Method for recycling a photovoltaic panel, characterized in that it comprises the following steps:
10. a) providing a photovoltaic panel comprising cables, a junction box, a metal frame, photovoltaic cells encapsulated in a polymer layer and electrical connectors, b) removing the cables, the junction box and the metal frame from the photovoltaic panel, c) carrying out a thermal, chemical and / or mechanical treatment to remove the polymer layer encapsulating the photovoltaic cells, d) recovering the photovoltaic cells, the photovoltaic cells forming a substrate containing an indium tin oxide film locally covered by a metal layer, preferably silver, e) implementing the indium recovery step as defined in one of claims 1 to 8. Method according to the preceding claim, characterized in that the method comprises, after step e), the following subsequent steps: recovery of the indium precipitate, thermal treatment of the indium precipitate, for example at a temperature between 600°C and 700°C, whereby an indium oxide is formed.