Method for manufacturing a flexible substrate coated with a heat-sealing film-forming polymer

The controlled humidity differential drying process addresses curling issues in flexible supports coated with heat-sealing film-forming polymers, ensuring flatness and efficient heat sealing without additional layers, enhancing industrial applicability and environmental friendliness.

FR3141949B1Active Publication Date: 2024-10-25GUYENNE PAPIER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022011896
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-11-16
Publication Date
2024-10-25
Estimated Expiration
2042-11-16

AI Technical Summary

Technical Problem

Conventional processes for manufacturing flexible supports coated with heat-sealing film-forming polymers, such as paper, suffer from significant curling or rolling up of edges due to the retraction of the film-forming polymers, which makes them unsuitable for industrial use and requires additional adhesive layers for heat sealing.

Method used

A process involving controlled humidity differential drying and rapid drying steps to minimize residual moisture, applying a heat-sealing film-forming polymer on one side and moisture on the reverse side to create a humidity gradient, followed by controlled drying to stabilize the support, preventing curling and allowing heat sealing without additional layers.

Benefits of technology

The process achieves flatness and effective heat sealing of the flexible support, reducing the number of layers needed and enhancing environmental sustainability by using fewer materials and energy, while maintaining optimal mechanical and chemical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000025_0000
    Figure 00000025_0000
  • Figure 00000025_0001
    Figure 00000025_0001
  • Figure 00000026_0000
    Figure 00000026_0000
Patent Text Reader

Abstract

Method for manufacturing a flexible substrate coated with a heat-sealing film-forming polymer. The invention relates to a method for manufacturing a coated flexible substrate (4), in particular a coated paper (4), having a front face (6) coated (8) with a heat-sealing film-forming polymer (10). Said method comprises the following steps: a) depositing said heat-sealing film-forming polymer (10) onto the front face (6) of the flexible substrate (12); b) drying said coated flexible substrate (4) so ​​that the moisture content of said coated flexible substrate (4) is less than 4.5%, preferably less than or equal to 3%, more particularly less than or equal to 2.5%; c) applying a moist substance, in particular water, to a back face (16) of the coated flexible substrate (4) so ​​as to create a moisture difference between the front face (6) and the back face (16) of the coated flexible substrate (4); and d) dry said coated flexible support (4). Figure for the abbreviation: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Method for manufacturing a flexible support coated with a heat-sealing film-forming polymer

[0001] The present invention relates to a method for manufacturing a flexible support, in particular paper, having a front face coated with a heat-sealing film-forming polymer.

[0002] The invention also relates to a coated flexible support. The invention also relates to a packaging comprising the coated flexible support obtained by such a method.

[0003] The use of film-forming polymers is widespread in the field of surface coatings, in particular in the field of coating, lamination or complexing on a support, in particular paper or cardboard.

[0004] Indeed, these film-forming polymers make it possible to waterproof a surface in order to make it a barrier to elements such as grease.

[0005] For example, patent application FR 3107529 A describes these film-forming polymers comprising a thermoplastic material based on casein and / or caseinate, intended to coat a layer of paper or cardboard.

[0006] These polymers, for example initially in the form of a solution or a liquid, require a stabilization period so that they are stabilized in order to form a dry film on the support.

[0007] This stabilization period varies depending on the chemical nature of the film-forming polymers and the conditions to which these film-forming polymers have been subjected. During this stabilization period, the film formed by the film-forming polymers may shrink.

[0008] When the surface to be waterproofed is on one of the faces of a flexible support, in particular on a low-weight paper, for example less than 200 g / m2, where the rigidity of the flexible support is not sufficient to counter the shrinkage induced by these film-forming polymers, the edges of the flexible support tend, after a certain time, to curl up on themselves.

[0009] This tendency for the edges of a flexible support coated with the film-forming polymer, initially flat, to rise, then to curl, on each side is defined as being a "rolling effect" or a "curl" (English terminology).

[0010] The “curl” is all the more important as the retraction induced by the film-forming polymers is important.

[0011] Generally speaking, the coated flexible support obtained according to a conventional process is characterized by a very significant “curl”, namely that the edges curl several times towers.

[0012] Too much curl prevents the final coated flexible support from being used in industrial conditions.

[0013] Furthermore, the conventional coated flexible support requires an additional adhesive layer in order to achieve heat sealing with this coated flexible support.

[0014] Furthermore, this type of conventional coated flexible support often requires a multitude of separate layers in order to obtain sufficient barrier properties.

[0015] The invention aims in particular to overcome these drawbacks.

[0016] The present invention thus relates to a method for manufacturing a coated flexible support, in particular a coated paper, having a front face coated with a heat-sealing film-forming polymer, said method being characterized in that it comprises the following steps:

[0017] a) depositing said heat-sealing film-forming polymer on the front face of the flexible support;

[0018] b) drying said coated flexible support so that the humidity of said coated flexible support is less than 4.5%, preferably less than or equal to 3%, more particularly less than or equal to 2.5%;

[0019] c) applying a wet material, in particular water, to a back side of the coated flexible support so as to create a difference in humidity between the front side and the back side of the coated flexible support; and

[0020] d) drying said coated flexible support.

[0021] A distinction is made between “flexible support” and “coated flexible support”. The flexible support is raw, not yet coated. The coated flexible support corresponds to the flexible support having received the heat-sealing film-forming polymer.

[0022] This is also applicable for any type of flexible support, namely “paper” and “coated paper”.

[0023] Thanks to the method according to the invention, the tendency ("curl") of the edges of the coated flexible support to curl up on themselves after the manufacture of said coated flexible support is prevented.

[0024] Thus, the method according to the invention allows the industrial manufacture of said coated flexible support in an automated flexible support manufacturing line whereas such a coated flexible support could not be obtained via this manufacturing line until now because of the winding effect of the coated flexible support.

[0025] This is enabled by the different steps of the method according to the invention, as explained below.

[0026] The second step b) allows the coated flexible support to be dried as much as possible so that said coated flexible support contains as little residual moisture as possible. Following this high-intensity drying, the heat-sealing film-forming polymer causes high stresses on the flexible support, for example, where appropriate, on fibers of this flexible support, stresses which would have the effect of rolling up the coated flexible support laid flat after manufacture. We wish to avoid this rolling up effect.

[0027] Thus, the drying step b) occurs immediately after the deposition of the heat-sealing film-forming polymer so that this heat-sealing film-forming polymer does not yet have time to dry naturally, in order to maximize the stresses to which the heat-sealing film-forming polymer is subjected.

[0028] Step c) following drying step b) aims to create a marked difference in humidity between the front and back sides. The front side has a humidity of less than 4.5%, preferably less than or equal to 3%, more particularly less than or equal to 2.5% while the back side is wet. This humidity after drying step b) can advantageously be between:

[0029] 2.5 and 3.5%;

[0030] 3.5 and 4.5%; or

[0031] 2.5 and 4.5%.

[0032] During the drying step d), the humidity of the front face being very low, the wet material, in particular water, evaporates very largely from the back face, causing a stress on the material forming the flexible support, this material being for example fibers, stress which will induce a rolling effect on the back face. This rolling effect on the back face is opposite to the rolling effect of the front face so that compensation for the rolling effects on the front and back faces can be obtained. This compensation may require a certain duration, so that the coated flexible support stabilizes. During this duration, the coated flexible support stabilizes, for example by remaining on a roll.

[0033] For example, when the flexible support is a paper, the coated paper, namely the paper coated with the heat-sealing film-forming polymer, obtained at the outlet of the machine has a certain winding effect. After a certain period of time, for example five to seven days following production, the film of heat-sealing film-forming polymer present on the surface will stabilize, generating its shrinkage. By shrinking, the winding effect generated during production will fade, until a flat color is obtained when the heat-sealing film-forming polymer is completely stabilized.

[0034] Thus, when these effects have been compensated, the coated flexible support, placed on a flat surface, has satisfactory flatness.

[0035] The drying step d) is carried out by conventional drying means known per se, the drying temperature of which is less than or equal to 120°C, on the one hand, to prevent the difference in humidity between the two front and back faces of the coated flexible support from being cancelled out, and on the other hand, to prevent the coated flexible support at the outlet of the drying means chain from being too dry, which can cause defects such as folds or cords due to moisture absorption of the coated flexible support.

[0036] Furthermore, the drying temperature during step d) is preferably greater than or equal to 45°C to prevent the flexible support from remaining too wet. Thus, it is possible, for example, to dry the flexible support during step d) at a temperature range of between 50 and 90°C, more particularly between 60 and 80°C, ideally between 60 and 70°C to overcome these aforementioned drawbacks.

[0037] After this step d), the humidity of the flexible support is less than 10%, preferably between 2 and 10%, more particularly between 4 and 8% or 6 and 10%. The humidity of the flexible support after step d) may advantageously be between:

[0038] 7 and 9%; or

[0039] 8 and 9%.

[0040] The humidity of the flexible support after step d) can also be approximately 4%.

[0041] In addition to the fact that the invention makes it possible to prevent the tendency ("curl") of the edges of the coated flexible support to curl up on themselves after the manufacture of said coated flexible support, the heat-sealing film-forming polymer deposited on the coated flexible support is sufficient in itself to heat-seal the coated flexible support. In other words, said heat-sealing film-forming polymer does not require an additional adhesive layer or an additional polymer layer in order to heat-seal the coated flexible support.

[0042] Thus, a number of layers required for the coated flexible support is reduced in order to simplify the structure of said coated flexible support, while optimizing the optimal mechanical and chemical properties.

[0043] This is more particularly advantageous in that the method according to the invention is more environmentally friendly and more economical than the conventional method involving several layers, because fewer steps, less material, less energy and less time are necessary to obtain a coated flexible support with optimal properties.

[0044] According to one aspect of the invention, the coated flexible support is dried during step b) and during step d) so that the humidity of the flexible support obtained after step d) is greater than after step b).

[0045] According to one aspect of the invention, the grammage of the flexible support is between 20 and 300 g / m2, is between 20 and 100 g / m2, preferably is between 30 and 60 g / m2. The grammage is more particularly between 50 and 60 g / m2

[0046] According to one aspect of the invention, the surface density of the deposit of the heat-sealing film-forming polymer, measured by the difference in weight between the dry coated flexible support and the dry flexible support, is between 6 and 14 g / m2, more particularly generally between 8 and 12 g / m2 or between 7.5 and 8.4 g / m2.

[0047] In these surface density ranges, the barrier properties can be optimally obtained. The flexible support and the coated flexible support were dried before weighing to remove any traces of residual water.

[0048] According to one aspect of the invention, step a) consists of applying the heat-sealing film-forming polymer at least twice to the front face of the flexible support so as to obtain a layer of the heat-sealing film-forming polymer.

[0049] For example, in the case of a deposition layer of the heat-sealing film-forming polymer of 10 g / m2, this deposition can be carried out by two successive coating stations of the same polymer of 5 g / m2. Thus, the layer of the heat-sealing film-forming polymer has a uniform surface and good sealing.

[0050] According to one aspect of the invention, the difference in humidity between the front face and the rear face at the end of step b) is greater than 95.5%, preferably greater than 97%.

[0051] According to one aspect of the invention, in which the drying is carried out with:

[0052] - an airborne dryer comprising a plurality of hot air dryers; and / or

[0053] - an infrared dryer.

[0054] The hot air dryer is defined as a non-contact drying device using air flow. This hot air dryer allows for a gradual increase in temperature. In addition, said dryer allows for the evaporation of significant quantities of water.

[0055] The infrared dryer is a radiation-based, non-contact drying device that allows high thermal transmission. It is possible to modulate the wavelength depending on the flexible support used. This type of infrared drying is particularly useful for very quickly raising the temperature of the flexible support and / or the heat-sealing film-forming polymer.

[0056] Conversely, a hot air dryer is gentler in its temperature rise but allows significant quantities of water to be evaporated more easily.

[0057] The infrared dryer can be used alone, or coupled to an airborne dryer, for example during step b) and / or during step d) of the process according to the invention.

[0058] According to one aspect of the invention, in which the drying temperature during step b) is greater than or equal to 100°C. It is preferably between 140 and 150°C.

[0059] This drying temperature is dependent on drying adjustment parameters known per se for a given drying device.

[0060] For example, the following two parameters such as the speed at which the flexible support or the coated flexible support advances in a production line, called the “machine speed” and the length of the drying device can be taken into account, the drying temperature will be all the higher as the “machine speed” is high and the length of the drying device will be less.

[0061] In an alternative embodiment, when the drying during step b) is carried out with an infrared dryer, the drying temperature may be greater than 130°C, preferably between 130 and 170°C, more particularly between 150 and 170°C.

[0062] According to one aspect of the invention, the wet material is water in liquid form, in vapor form or a mixture of the two.

[0063] According to one aspect of the invention, the wet material is applied to the back side of the flexible support using a rotating roller.

[0064] According to one aspect of the invention, in which the deposition method according to step a) is chosen between coating or printing.

[0065] According to one aspect of the invention, the flexible support is chosen from paper, plastic films based on polyethylene (PE), polypropylene (PP), and polylactic acid (PLA). Preferably, the paper has at least one smooth face obtained by at least one of the following methods: rubbing, calendering or coating.

[0066] According to one aspect of the invention, the paper is chosen from offset paper, recycled paper, tracing paper, greaseproof paper, and Kraft paper.

[0067] For example, Kraft paper, the characteristics of which are known per se, has optimal mechanical resistance in view of the paper weight.

[0068] According to one aspect of the invention, the paper has a white appearance or a brown appearance.

[0069] According to one aspect of the invention, step a) and / or step c) is carried out in using at least one of the following means: a doctor blade passing over the flexible support, a Meyer bar, a curtain coater equipped with a coating nozzle, or an air knife coater.

[0070] In this way, during step a), the heat-sealing film-forming polymer is coated homogeneously and has a uniform thickness on the front side of the flexible support. Thus, the coating of the heat-sealing film-forming polymer thus obtained is very regular and without marks, scratches or faults through which a fluid (gas, liquid) could enter the coated flexible support and cause softening or leaks of said coated flexible support. In addition, the regular coating obtained makes it possible to achieve high-quality heat sealing.

[0071] Among the different coating techniques, the air knife coater or the curtain coater equipped with a coating nozzle, makes it possible to precisely control the coating deposition with high quality and to ensure a uniform and regular coating on the flexible support. During step c), the wet material, in particular water, can be applied uniformly to the reverse side of the flexible support coated with these different coating techniques.

[0072] According to one aspect of the invention, the air knife coater comprises: - A recovery tank for the heat-sealing film-forming polymer or the wet material, designed to recycle the excess of said heat-sealing film-forming polymer or said wet material.

[0073] According to one aspect of the invention, the heat-sealing film-forming polymer has one or a combination of the following properties: oxygen barrier, oil / grease barrier, water barrier, water vapor barrier, and / or antifungal barrier.

[0074] According to one aspect of the invention, the heat-sealing film-forming polymer has one or a combination of the following properties: oxygen barrier, oil / grease barrier.

[0075] According to one aspect of the invention, the heat-sealing film-forming polymer is food compatible.

[0076] According to one aspect of the invention, the heat-sealing film-forming polymer comprises a thermoplastic polymer.

[0077] According to one aspect of the invention, the heat-sealing film-forming polymer comprises:

[0078] - at least one caseinate and / or at least one casein.

[0079] Thus, caseinate and / or casein correspond to products accessible in large quantities and presenting optimal mechanical and chemical properties at a lower cost, compared to other polymers of natural origin presenting similar properties.

[0080] According to one aspect of the invention, the heat-sealing film-forming polymer has at least one of the following properties: biosourced, biodegradable, compostable.

[0081] According to one aspect of the invention, the heat-sealing film-forming polymer is water-soluble.

[0082] This water-soluble character makes it possible to make the film-forming polymer compatible with the coated flexible support having the following properties: bio-sourced, biodegradable, compostable and / or repulpable, in particular repulpable.

[0083] According to one aspect of the invention, the coated flexible support has at least one of the following properties: biosourced, biodegradable, compostable and / or repulpable.

[0084] According to one aspect of the invention, the coated flexible support has the following properties: biosourced, biodegradable, compostable and repulpable.

[0085] For example, a coated paper manufactured at the end of the process according to the invention with the heat-sealing film-forming polymer comprising at least one caseinate and / or one casein has all these properties.

[0086] According to one aspect of the invention, the heat-sealing film-forming polymer comprising at least one caseinate and / or one casein having oil / grease barrier and oxygen barrier properties.

[0087] According to one aspect of the invention, the heat-sealing film-forming polymer is initially in the form of granules, preferably thermoplastic granules.

[0088] The heat-sealing film-forming polymer, initially in the form of thermoplastic granules, is dissolved in water to form a solution. This solution is intended to form a dry film on the paper in order to form a coated paper. The quantity of water is dependent on the desired final viscosity and may depend on the nature of the flexible support.

[0089] According to one aspect of the invention, said caseinate and / or said casein has a weight which represents from 50 to 80% relative to the weight of the granule, preferably from 55 to 75%, more particularly from 60 to 70%. Said caseinate and / or casein represents from 60 to 65% of the weight of the granule.

[0090] According to one aspect of the invention, the heat-sealing film-forming polymer further comprises:

[0091] -water; and

[0092] - at least one plasticizer other than water.

[0093] According to one aspect of the invention, the water represents from 10 to 15% of the weight of the granule, preferably from 10 to 12% of the weight of the granule.

[0094] According to one aspect of the invention, the heat-sealing film-forming polymer further comprises: - A plasticizer whose weight represents 10 to 30% of the weight of the granule, preferably 15 to 25%; and - A surfactant whose weight represents 1 to 5% of the weight of the granule, preferably 1 to 3%.

[0095] According to one aspect of the invention, the heat-sealing film-forming polymer comprises:

[0096] at least one water-soluble polymer, namely a water-soluble polymer, preferably soluble in water at room temperature when the mass concentration of the water-soluble polymer is greater than or equal to 2.5%.

[0097] Thus, the heat-sealing film-forming polymer has improved mechanical and chemical properties.

[0098] According to one aspect of the invention, the heat-sealing film-forming polymer is associated with: - at least one water-soluble polymer, namely a water-soluble polymer, preferably soluble at room temperature.

[0099] Thus, the heat-sealing film-forming polymer has improved mechanical and chemical properties.

[0100] According to one aspect of the invention, the water-soluble polymer represents from 1 to 7% of the weight of the granule, preferably from 2 to 6% of the weight of the granule, more particu- 3 to 5% of the pellet weight.

[0101] Preferably, the water-soluble polymers comprise hydrophilic units. For example, the water-soluble polymers may comprise heteroatoms such as O or N in their main chain. The water-soluble polymers may also comprise hydrophilic groups such as -OH, -NH2, -NH-, -CO2-, or -SO3-

[0102] According to one aspect of the invention, the water-soluble polymer is chosen from non-ionic water-soluble polymers, amphoteric water-soluble polymers, cationic water-soluble polymers, anionic water-soluble polymers, and mixtures thereof.

[0103] According to one aspect of the invention, the water-soluble polymer is chosen from polyvinyl alcohols, polyoxyalkylenes, polyvinylpyrrolidones, poly(meth)acrylic acids, cationic polymers, and mixtures thereof.

[0104] Among the water-soluble polymers, polyacrylamides may also be mentioned.

[0105] According to one aspect of the invention, the plasticizer is chosen from polyols, glycerol acetates, glycerol propionates and mixtures thereof. Examples of polyols that may be mentioned are glycerol, hexane triol, mannitol, sorbitol, glycols, including ethylene glycol and their derivatives. Preferably, the plasticizer is chosen from glycerol, sorbitol, and mixtures thereof. According to one embodiment, the plasticizer is glycerol.

[0106] Thus, said plasticizer makes it possible to increase the mechanical properties of the heat-sealing film-forming polymer against humidity.

[0107] According to one aspect of the invention, the surfactant is chosen from lecithin, diacetylenic phosphonates, polysorbates. Preferably, the surfactant is lecithin.

[0108] According to one aspect of the invention, the hydrophobic agent may be chosen from:

[0109] - polycarboxylic acid esters;

[0110] - C3-C33 carboxylic acids, preferably C4-C28 fatty acids, and, even more preferentially unsaturated fatty acids in C6-C28; and [YES] - their s mixture s.

[0112] The polycarboxylic acid esters may be derived from at least one polycarboxylic acid and at least one alcohol, preferably a Cl-Cl8 alcohol.

[0113] Among the polycarboxylic acids preferentially retained within the framework of the invention, mention may be made of citric acid, hydroxycitric acid, tartaric acid, malic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, maleic acid, fumaric acid.

[0114] Among the preferred alcohols in accordance with the invention, mention may be made of C2-C6 alcohols, such as, for example, ethanol, n-propanol, iso-propanol, n-butanol and tert-butanol.

[0115] According to one aspect of the invention, the hydrophobic agent is chosen from triethyl citrate, tributyl O-acetyl citrate, tributyl citrate and mixtures thereof.

[0116] According to one aspect of the invention, the hydrophobic agent is a C3-C33 carboxylic acid, preferably a C4-C28 fatty acid, and even more preferably an unsaturated C6-C28 fatty acid.

[0117] Among the C4-C28 fatty acids retained within the scope of the invention, mention may be made of caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, and mixtures thereof.

[0118] Among the particularly interesting C6-C28 unsaturated fatty acids, mention may be made of palmitoleic acid, oleic acid, linoleic acid, and mixtures thereof.

[0119] According to one aspect of the invention, the heat-sealing film-forming polymer can be printable and / or printed.

[0120] According to one aspect of the invention, the oil and / or grease barrier property of the heat-sealing film-forming polymer has a Cobb 1800 index of less than 10 g / m2, preferably less than 6 g / m2, more particularly less than 3 g / m2. The Cobb 1800 index is ideally between 1 and 2.5 g / m2.

[0121] The Kit level for obtaining the oil and / or grease barrier property of the heat-sealing film-forming polymer is greater than or equal to 7, preferably greater than or equal to 10.

[0122] According to one aspect of the invention, the oxygen barrier property of the heat-sealing film-forming polymer has a permeability level of less than or equal to 1000 cm3 / (m2.24h), preferably less than or equal to 100 cm3 / (m2.24h), more particularly less than or equal to 100 cm3 / (m2.24h).

[0123] According to one aspect of the invention, the water barrier property of the heat-sealing film-forming polymer has a Cobb 1800 index of less than or equal to 15 g / m2, preferably less than or equal to 5 g / m2, more particularly between 1 and 2.5 g / m2.

[0124] According to one aspect of the invention, the water vapor barrier property of the heat-sealing film-forming polymer has a water vapor transmission coefficient (WVTR) of less than or equal to 10 g / (m2.24h) and ideally less than or equal to 5 g / (m2.24h) under standard conditions (23°C / 50%RH). Under tropical conditions (38°C / 90%RH), the WVTR is less than or equal to 100 g / (m2.24h) and ideally less than or equal to 50 g / (m2.24h).

[0125] The present invention also relates to a method for manufacturing a coated flexible support, in particular a coated paper, having a front face and a back face, characterized in that said method comprises the following steps: a. depositing a first film-forming polymer on the front face; b. depositing a second film-forming polymer on the back face, one of the first and second film-forming polymers being heat-sealing; and a. drying said coated flexible support.

[0126] Thus, the first and second film-forming polymers, one of which is heat-sealing, after drying c), exhibit “curls” which will compensate each other so that the coated flexible support exhibits good flatness.

[0127] According to one aspect of the invention, one of the first and second film-forming polymers contains at least one caseinate and / or one casein.

[0128] These film-forming polymers may exhibit some or all of the characteristics described above in connection with the heat-sealing film-forming polymer comprising caseinate and / or casein.

[0129] According to one aspect of the invention, the first and second film-forming polymers both comprise at least one caseinate and / or one casein.

[0130] According to another embodiment of the invention, the deposition method according to step a) is chosen from extrusion-coating and lamination, complexing.

[0131] At the end of this step a), the deposition of the heat-sealing film-forming polymer in the form of a film with low humidity, namely less than 8%, can be carried out on the front side of the flexible support in order to form a coated flexible support. The heat emitted by the machine used to make the deposition makes it possible to remove this residual humidity.

[0132] The invention also relates to a coated flexible support obtained by the method according to the invention.

[0133] The invention also relates to packaging comprising the coated flexible support obtained by the method according to the invention.

[0134] According to one aspect of the invention, the packaging comprises a stack of several flexible supports obtained by the method according to the invention.

[0135] According to one aspect of the invention, the packaging is obtained from a coated flexible support by heat-sealing certain areas of coated flexible support together.

[0136] According to one aspect of the invention, the flexible support has an appearance chosen from: white appearance, brown appearance, matt appearance, silk effect appearance, or shiny appearance.

[0137] According to one aspect of the invention, the packaging is manufactured by lamination, coating, laminating, co-extrusion or extrusion-coating processes.

[0138] The invention also relates to a packaged product comprising:

[0139] - a content, for example a foodstuff; and

[0140] - the packaging according to the invention enveloping the contents.

[0141] According to one aspect of the invention, the product is in solid or liquid form.

[0142] According to one aspect of the invention, the content is chosen from pharmaceutical products maceuticals, food, chemicals and cosmetics.

[0143] According to one aspect of the invention, the foodstuff of the contents of the packaged product is, for example, chosen from meat, fish, vegetables, fruits, pastries, Viennese pastries, food additives, ingredients, dry foods, dry preparations, food powders, tea and herbal tea bags, dried tea leaves, animal feed.

[0144] According to one aspect of the invention, the content is chosen from newspapers, magazines and advertisements.

[0145] Definitions

[0146] By “coating” is meant, for example, a surface treatment consisting of applying a generally liquid coating to a support. The coating may have a composition such as a film-forming polymer.

[0147] By “complexing” is meant, for example, a mechanical action making it possible to inseparably assemble two or more materials with different mechanical and physicochemical properties.

[0148] By "lamination" is meant, for example, a mechanical action allowing a film to be applied to a support

[0149] By “extrusion-coating” is meant, for example, the technique consisting of coating a support by depositing a layer of molten polymer thereon by extrusion.

[0150] By “printing” is meant, for example, an application of a coating via a flexographic or gravure printing system.

[0151] By "humidity" is meant the water or water vapor content in a substance. It can be expressed as a mass percentage, namely a ratio of the mass of water to the total mass of the substance.

[0152] “Grammage” is a quantity characterizing a flexible support, not yet coated, such as paper, corresponding to its surface mass, that is to say its mass per unit of surface. The grammage includes a residual humidity which varies in particular between 4 and 8% of the total weight of the flexible support, in particular paper.

[0153] The weight of a flexible support such as paper is between 10 and 300 g / m2, preferably between 20 and 100 g / m2, more preferably between 30 and 60 g / m2.

[0154] A “thin” paper has a weight between 10 and 60 g / m2, advantageously between 30 and 50 g / m2.

[0155] By "heat sealing" is meant, for example, a process during which the The edges of the support are welded using heat, with or without direct contact with the support.

[0156] By "heat sealant" is meant, for example, the quality that a material has to be welded by heat sealing without adding an additional adhesive layer, an additional polymer layer or an additive. In other words, the heat-sealing material is sufficient in itself to achieve a heat seal.

[0157] By "barrier" is meant, for example, the properties which protect the contents of a package formed by the support against external aggressions and substances, or which protect the exterior of the contents of the package. The most common barriers are those against oxygen, oil, grease, water, water vapor, and fungi and microorganisms.

[0158] By "oxygen barrier" is meant, for example, a barrier with a low oxygen permeability level, i.e. less than 100 cm3 / (m2.24h) and preferably less than 10 cm3 / (m2.24h). This property may be required, for example, for food products requiring protection from oxidation such as chocolate, cheese or dry foods.

[0159] By "oil or fat barrier" is meant, for example, a barrier whose Kit level is between 6 and 12. This property may be required, for example, for food products such as pastries or fast food.

[0160] By "water barrier" is meant, for example, a barrier whose Cobb index is advantageously less than or equal to 15 g / m2, preferably less than or equal to 5 g / m2 and for the Cobb duration of 1800 seconds. This property may be required, for example, for food products such as fruits and vegetables and disposable tableware.

[0161] By "water vapor barrier" is meant, for example, a barrier whose water vapor transmission coefficient (WVTR) is less than 10 g / (m2.24h) and ideally less than 5 g / (m2.24h) under standard conditions (23°C / 50%RH). The WVTR coefficient is less than 100 g / (m2.24h) and ideally less than 50 g / (m2.24h) under tropical conditions (38°C / 90%RH).

[0162] By "antifungal barrier" is meant, for example, a resistant barrier against the proliferation of fungi and microorganisms. This property may be required, for example, for food products such as soft fruits, such as strawberries or raspberries.

[0163] The "Cobb" test consists of measuring the quantity of water that the flexible support, in particular paper, can absorb over a defined time. For example, the Cobb index 1800 means that the Cobb test was carried out for 1,800 seconds, or 30 minutes.

[0164] This Cobb 1800 index is expressed in grams per square meter (g / m2). The lower the Cobb 1800 index value, the better the water barrier. Values ​​below 15 g / m2 correspond to very good water barriers for Cobbl800.

[0165] This Cobb test is carried out by pouring 100 ml of distilled or demineralized water onto a sample of treated paper with a surface area of ​​100 cm2 for 30 minutes (ISO 535:2014 standard). The difference in weight before and after the test corresponds to the quantity of water absorbed and therefore to the Cobb index.

[0166] Measurements of vapor permeation or water vapor transmission coefficient (Water Vapor Transmission Rate (WVTR) in English terminology),

[0167] These measurements assess the amount of water vapor that passes through the support in 24 hours at predefined temperature and humidity conditions. Generally, these tests are either carried out in “standard” conditions at 23°C / 50% relative humidity (RH), or in “tropical” conditions at 38°C / 90% RH.

[0168] The test is carried out according to ISO 2528, a cup of anhydrous CaCl2 is sealed by the support to be tested. The assembly is placed in a regulated climatic chamber. The water vapor which passes through the support is trapped by the CaCl2. The difference in weight of the CaCl2 measured between the initial moment and that measured after 24 h corresponds to the value of the WVTR expressed in g / m2 / 24 h.

[0169] The lower the WVTR value, the better the water vapor barrier.

[0170] The “Test Kit” makes it possible to determine the resistance of a paper to the penetration of fatty products such as fats or oil.

[0171] This test kit comprises, for example, at least 12 reagent mixtures containing varying amounts of castor oil, toluene and heptane. The test consists of determining the number of the highest mixture for which there is no penetration or soiling of the surface. The barrier level increases from 1 to 12.

[0172] A drop of the mixture is placed on a sheet, then it is wiped off after 15 seconds, and the appearance of the paper is observed (ISO 16532-2 standard).

[0173] For certain particular applications, more drastic tests can be carried out by increasing the surface area to be tested, and by carrying out tests at high temperature, namely above room temperature, or by increasing the proportion of the most aggressive reagent in the mixtures, namely heptane.

[0174] The oil Cobb test is based on the same principle as the aforementioned water Cobb test but this time using castor oil (SCAN-P 37 standard).

[0175] A palm oil impermeability test can also be carried out (ISO 16532-1 standard), if the results are good enough, the turpentine test can be carried out (ISO 16532-3 standard).

[0176] By "film-forming" is meant, for example, a material that can be applied in a thin layer, mainly in liquid form, on a support, and which then becomes a solid film, a film, or a sheet. This film-forming material can also be applied in another form, for example by extrusion-coating in the form of a softened or molten material. Generally speaking, by "film-forming" is meant, in particular, the tendency of a material to form a film.

[0177] By "polymer" is meant, for example, long-chain molecules of high molecular mass. A polymer can in particular be a substance consisting of molecules characterized by the sequence of one or more types of monomeric units. A "natural" polymer may include, for example, proteins.

[0178] By "thermoplastic" is meant, for example, a material which becomes malleable and pliable above a given temperature, the glass transition temperature Tg, but which below this Tg becomes hard again, these transformations being reversible.

[0179] By “plasticizer” is meant, for example, a substance making it possible to lower the glass transition temperature Tg of the material.

[0180] By "surfactant" is meant, for example, an amphiphilic molecule, that is to say a molecule possessing both hydrophilic and hydrophobic properties.

[0181] By "hydrophobic" is meant, for example, a compound having little affinity for water and tending not to dissolve in it. Typically, this is a predominantly apolar compound.

[0182] By "hydrophilic" is meant, for example, a compound having an affinity for water and having a tendency to dissolve therein. Typically, it is a compound having polar groups capable of forming hydrogen bonds.

[0183] By "water-soluble" is meant, for example, that which dissolves in water, preferably at room temperature. The water solubility of a polymer can be measured as follows: a polymer is added to water at a mass concentration of 2.5%. After stirring for 48 hours, the solution is filtered to check whether any particles remain. When there are no particles in the filter, the polymer is considered water-soluble. This water-soluble character does not concern certain polymers such as waxes, for example polyethylene or alkane-based waxes, or ester waxes, for example beeswax. Indeed, these waxes are not soluble in water.

[0184] By "bio-sourced" is meant, for example, a material containing all or part of elements of natural or renewable origin. The bio-sourced material is, for example, paper comprising cellulose that is extracted from trees or plants for different applications.

[0185] By "biodegradable" we mean a material that can be decomposed under the action of micro-organisms (bacteria, fungi, algae etc.). The result of this decomposition is the formation of water, CO2 and / or methane and possibly by-products (residues, new biomass) that are non-toxic to the environment. This is, for example, a biodegradable material according to the European standard EN NF 13432.

[0186] By "compostable" we mean, for example, a biodegradable product which completes the product cycle according to standard EN 13432.

[0187] According to this standard EN13432, a material can be described as “compostable” if it has the following characteristics:

[0188] - be able to achieve 90% biodegradation in less than 6 months if it is subjected to an environment rich in carbon dioxide; these values ​​are tested with the standard method EN14046 (also called ISO 14855);

[0189] - when brought into contact with organic waste for 3 months, the mass of material must consist of at least 90% of residues less than 2 mm in diameter; these values ​​are tested with the standard method EN14045;

[0190] - the material must not have negative effects on the composting process;

[0191] - a low concentration of heavy metals;

[0192] - pH values ​​within established limits;

[0193] - a mineral salt content within the established limits;

[0194] - a concentration of volatile solid elements within the established limits;

[0195] - a concentration of nitrogen, phosphorus, magnesium and potassium within the limits established.

[0196] It is noted that a “bio-sourced” material can be compostable.

[0197] By "repulpable" is meant, for example, a fibrous material, in particular paper, for which it is possible to disperse the fibers in an aqueous medium in order to produce a paste called pulp. Thus, the repulpable material can be reintegrated into the paper processing chain. This "repulpable" characteristic does not concern certain polymers such as polyolefins, for example polyethylene, or polypropylene. These polymers are not soluble in water and interfere with the process of dispersing the fibers in an aqueous medium, thus preventing a flexible support coated with such polyolefins or polypropylene from being made "repulpable". This "repulpable" characteristic also does not concern waxes, for example polyethylene- or alkane-based waxes, or ester waxes, for example beeswax.In fact, these waxes are not water-soluble, thus making it possible to make a flexible support coated with such waxes "repulpable".

[0198] By “caseinate” is meant, for example, a casein salt whose counter cation is chosen from the group comprising calcium, potassium, ammonium, sodium and magnesium.

[0199] "Casein" is a protein derived from milk which is mainly obtained by precipitation by adding an acid (acid casein) or rennet (rennet casein) to the milk, or by filtration (micellar casein). There are several types of casein in milk, namely alpha, beta, gamma and kappa caseins.

[0200] Caseinate and casein form a biodegradable, compostable, and food-compatible heat-sealing film-forming polymer. Casein and caseinate are also compatible with a bio-sourced, biodegradable, compostable, and / or repulpable coated flexible support.

[0201] Unless otherwise indicated, percentages are expressed by mass relative to the total mass of the material. Brief description of the figures

[0202] Other characteristics, details and advantages of the invention will emerge more clearly on reading the detailed description given below, and several examples of embodiment given for informational and non-limiting purposes with reference to the attached schematic drawings on the other hand, in which:

[0203] [Fig.l] is a schematic view of the automated manufacturing line of the coated flexible support according to the invention,

[0204] [Fig.2] is a schematic view of a coated paper, in cross-section, obtained by the process according to the invention,

[0205] [Fig.3] is a schematic view of a coated paper, in cross-section, obtained by a variant of the process according to the invention,

[0206] [Fig.4] is a schematic view, in cross-section, of an assembly of two heat-sealed coated papers,

[0207] [Fig.5] represents schematic views of the three samples of flexible supports obtained under various experimental conditions seven days after drying in ambient air,

[0208] Detailed description of the figures

[0209] [Fig.l] shows an automated manufacturing line 2 for implementing the method according to the invention to manufacture coated paper samples 4 having a front face 6 coated 8 with a heat-sealing film-forming polymer 10 comprising a caseinate and a casein.

[0210] The heat-sealing film-forming polymer 10 used for the three coated paper samples 4, namely comparative example 100, example 1 (200) and example 2 (300), is initially in the form of thermoplastic granules and comprises: - caseinate, the weight of which represents 63% of the weight of the granule; - water, the weight of which represents 10% of the weight of the granule; - A glycerol as a plasticizer whose weight represents 23.5% of the weight of the granule; - Lecithin as a surfactant whose weight represents 2.3% of the weight of the granule; - oleic acid as a fatty acid, the weight of which represents 1.2% of the weight of the granule.

[0211] The paper 12 used for the coated paper 4 has a weight of 50 g / m2.

[0212] The heat-sealing film-forming polymer 10, initially in the form of thermoplastic granules, are dissolved in water to form a solution. This solution is intended to form a dry film on the paper 12 in order to form a coated paper 4. The quantity of water is dependent on the desired final viscosity and may depend on the nature of the paper 12.

[0213] Experimental tests have shown that the amount of water added to dissolve the thermoplastic granules does not significantly influence the winding effect of the coated paper 4.

[0214] The method according to the invention comprises the following steps:

[0215] a) depositing the heat-sealing film-forming polymer 10 on the front face 6 of each paper 12;

[0216] b) drying the coated papers 4 so that the humidity of the coated paper 4 is greater than 5% (comparative example 100), of the order of 5% (example 1 (200)) and of the order of 3% (example 2 (300));

[0217] c) applying water to a back face 16 of each coated paper 4 so as to create a humidity difference between the front face 6 and the back face 16 of each coated paper 4; and

[0218] d) drying each coated paper 4.

[0219] Step a) of the method according to the invention is implemented by means of a coating technique which is an air knife coater 18 which comprises rollers 22, an air knife 24 and a tank of heat-sealing film-forming polymer 26.

[0220] The heat-sealing film-forming polymer 10, contained in a heat-sealing film-forming polymer tank 26, is abundantly deposited on the front face 6 of the paper 12 by one of the rollers 22 which is directly in contact with said heat-sealing film-forming polymer 10.

[0221] The excess of the heat-sealing film-forming polymer 10 is removed by means of an air jet emitted by the air blade 24. This excess is recovered in the recovery tank 28 arranged to recycle said excess in the tank of the heat-sealing film-forming polymer 10.

[0222] This air knife coater 18 makes it possible to control the coating deposition with high quality and to ensure a uniform and regular coating on the paper 12.

[0223] The coating deposit having a surface density of 8 to 12 g / m2, produced with this air knife coater 18 makes it possible to confer the grease and oxygen barrier properties to the coated paper 4. The oxygen barrier properties are improved compared to the case where the paper 12 is not coated.

[0224] Thus, the coated paper 4 has a Cobb index 1800 of the order of 1 to 4 g / m2 and a Kit level of the order of 7 to 12.

[0225] Step b) of the method according to the invention is implemented by means of an airborne dryer 30 comprising a plurality of hot air dryers (not shown), each dryer being maintained at a temperature of around 145°C, taking into account the drying adjustment parameters such as the speed at which the paper 12 advances or the coated paper 4 in a manufacturing line 2, called the "machine speed" and the length of the airborne dryer 30.

[0226] For example, the following two parameters such as the speed at which the paper 12 advances in a manufacturing line 2, called the “machine speed” and the length of the airborne dryer 30 can be taken into account. The drying temperature will be higher the higher the “machine speed” and the shorter the length of the airborne dryer 30.

[0227] This step b) makes it possible to dry the coated paper 4 as much as possible so that said coated paper 4 contains as little residual moisture as possible.

[0228] Following this high-intensity drying, the heat-sealing film-forming polymer 10 causes high stresses on the paper 12, on fibers of this paper 12, stresses which would have the effect of rolling up the coated paper 4 laid flat after manufacture. It is desired to avoid this rolling up effect.

[0229] Thus, the drying step b) occurs immediately after the deposition of the heat-sealing film-forming polymer 10 so that this heat-sealing film-forming polymer 10 does not yet have time to dry naturally, in order to maximize the stresses to which the heat-sealing film-forming polymer 10 is subjected.

[0230] Step c) following drying step b) aims to create a marked difference in humidity between the front 6 and back 16 faces. The front 6 face has a humidity of less than or equal to 3%, while the back 16 face is wet.

[0231] Step c) of the method according to the invention is carried out with water applied to the back face 16 of the coated paper 4 using a rotating roller 22 in contact with water contained in a water tank 32. The purpose of this step is to create a marked difference in humidity between the front 6 and back 16 faces.

[0232] Step d) of the method according to the invention is carried out with an airborne dryer 30 comprising a plurality of hot air dryers (not shown), each dryer being maintained at a temperature of around 65°C in order to evaporate the excess water which has been added to the back face 16 of the coated paper 4 so as to achieve a humidity of approximately 6%.

[0233] During the drying step d), the humidity of the front face 6 being very low, water evaporates very largely from the back face 16, causing stress on the fibers forming the paper 12, stress which will induce a winding effect on the back face 16. This winding effect on the back face 16 is opposite to the winding effect of the front face 6 so that compensation for the winding effects on the front faces 6 and back faces 16 can be obtained. This compensation may require a certain duration for the coated paper 4 to stabilize.

[0234] Thus, when these effects have compensated for each other, the paper 12, placed on a flat surface, has satisfactory flatness.

[0235] The coated paper 4 with the heat-sealing film-forming polymer 10, obtained at the outlet of the machine, has a certain winding effect. Five to seven days following production, the film of heat-sealing film-forming polymer 10 present on the surface will stabilize, generating its shrinkage. By shrinking, the winding effect generated during production will fade, until a flattening is obtained when the heat-sealing film-forming polymer 10 is completely stabilized.

[0236] [Fig.2] shows schematically, in cross-section, a coated paper 4 obtained by the method according to the invention.

[0237] The coated paper 4 comprising the front 6 and back 16 faces, comprises on its front 6 face a layer of said film-forming polymer 10 comprising the caseinate with the composition described above while the back 16 face of said coated paper 4 does not comprise heat-sealing film-forming polymer 10.

[0238] [Fig. 3] shows schematically, in cross-section, a coated paper 400 obtained by a variant of the method according to the invention.

[0239] The coated paper 400 thus obtained has a front face 6 on which a first film-forming polymer 50 is deposited and a back face 16 on which a second film-forming polymer 60 is deposited, the first and second polymers 50, 60 being heat-sealing and comprising the caseinate with the compositions presented above. The first and second film-forming polymers 50, 60, after a drying step, have “curls” which will compensate each other so that the coated paper 400 has good flatness.

[0240] [Fig.4] shows schematically, in cross-section, an assembly 70 by heat-sealing two coated papers 4 obtained by the method according to the invention.

[0241] Two coated papers 4 having a front face 6 and a back face 16, each coated paper 4 having on its front face 6 a layer of the heat-sealing film-forming polymer 10 comprising the caseinate, are assembled without the need to insert an additional adhesive layer (not shown) between each layer of the heat-sealing film-forming polymer 10 comprising the caseinate.

[0242] [Fig. 5] schematically shows three samples of coated papers 4, namely the sample of comparative example 100, the sample of example 1 (200) and the sample of example 2 (300), placed on a flat surface. These samples 100, 200, 300 are obtained after seven days of drying in ambient air after production. The experimental conditions, namely the nature of the heat-sealing film-forming polymer 10, the nature of the paper 12 as well as the aforementioned tools and machines for the manufacture of these three samples of coated papers 100, 200, 300 are identical, with the exception of the drying step b) for drying the samples of coated papers 100, 200, 300 so as to obtain a paper humidity desired which is detailed below.

[0243] From left to right, we first see the sample of comparative example 100 obtained according to standard drying conditions (humidity greater than 5%).

[0244] Then, the sample corresponding to example 1 (200) obtained with the process according to the invention with a humidity of 5% obtained after the first drying (step b)).

[0245] Finally, the sample corresponding to example 2 (300) obtained with the process according to the invention with a humidity of 3% obtained after the first drying (step b)).

[0246] For the sample of comparative example 100, the winding effect is very pronounced. The coated paper 4 has wound itself, forming several turns. The presence of these turns does not make the sample of comparative example 100 usable in industry.

[0247] With regard to Example 1 (200), each edge of the coated paper 4 forms a half-turn of winding, while the middle of the coated paper 4 remains flat. The presence of the half-turn of winding does not make Example 1 (200) usable in industry.

[0248] With regard to Example 2 (300), the coated paper 4 is completely flat, highlighting the elimination of the curling effect observed with the sample of Comparative Example 100 and Example 1 (200). Thus, a coated paper 4 with very good flatness is obtained in the case of Example 2 (300).

[0249] Thus, it is notable to observe that the greater the difference in humidity between the front 6 and back 16 faces during the second drying (step d), the curling effect observed after production is reduced, or even eliminated.

[0250] Furthermore, in the absence of the implementation of the method according to the invention, despite drying in ambient air for a period of seven days after production, the curling effects persist as illustrated by the sample of comparative example 100 and example 1 (200). Conversely, this same drying in ambient air makes it possible to completely compensate for the curling effects of the sample of example 2 (300) placed on a flat surface.

[0251] It is remarkable to note that the method according to the invention makes it possible to obtain a coated paper 4 intended for packaging, said coated paper 4 being biosourced, biodegradable, compostable and repulpable with mechanical and chemical properties equivalent to a plastic film or a paper coated with a non-biodegradable film-forming polymer (not shown), namely a rot-proof film-forming polymer commonly used commercially.

[0252] In particular, said coated paper 4 obtained with the method according to the invention has the barrier properties to oil and grease (a Cobb index 1800 of the order of 1 to 4 g / m2 and a Kit level of the order of 7 to 12) and to oxygen (oxygen permeability level less than 10 cm3 / (m2.24h)) in combination with the ther- moscellantes. Said coated paper 4 therefore does not require an additional layer.

[0253] Furthermore, the method according to the invention allows the industrial manufacture of said coated paper 4 in an automated paper manufacturing line whereas such coated paper 4 could not be obtained via this manufacturing line until now because of the winding effect of the coated paper 4.

[0254] Furthermore, the method according to the invention makes it possible to reduce the number of layers required for the coated paper 4 while making it more ecological, economical and compatible with various applications such as packaging applications, in particular food packaging applications.

Claims

Claims

1. Method for manufacturing a coated flexible support (4), in particular a coated paper (4), having a front face (6) coated (8) with a heat-sealing film-forming polymer (10), said method being characterized in that it comprises the following steps: a) depositing said heat-sealing film-forming polymer (10) on the front face (6) of the flexible support (12); b) drying said coated flexible support (4) so ​​that the humidity of said coated flexible support (4) is less than 4.5%, preferably less than or equal to 3%, more particularly less than or equal to 2.5%;c) applying a wet material, in particular water, to a back face (16) of the coated flexible support (4) so ​​that the front face (6) has a humidity of less than 4.5%, preferably less than or equal to 3%, more particularly less than or equal to 2.5% while the back face is wet, to create a humidity difference between the front face (6) and the back face (16) of the coated flexible support (4); and d) drying said coated flexible support (4).;

2. Method according to claim 1, in which the heat-sealing film-forming polymer (10) has at least one of the following properties: bio-sourced, biodegradable, compostable.

3. The method of claim 1 or 2, wherein the heat-sealing film-forming polymer (10) is water-soluble.

4. Method according to claim 3, in which the coated flexible support (4) has at least one of the following properties: biosourced, biodegradable, compostable, repulpable.

5. A method according to any preceding claim, wherein the heat-sealing film-forming polymer (10) comprises a thermoplastic polymer.

6. Method according to any one of the preceding claims, in which the heat-sealing film-forming polymer (10) comprises: - at least one caseinate and / or at least one casein.

7. Method according to any one of the preceding claims, in which the weight of the coated flexible support (4) is between 20 and 100 g / m2, preferably between 30 and 60 g / m2.

8. A method according to any preceding claim, in in which the drying temperature during step b) is greater than or equal to 100°C.

9. A method according to any one of the preceding claims, the heat-sealing film-forming polymer (10) having at least one of the following properties: oxygen barrier, oil / grease barrier.

10. Coated flexible support (10) obtained by the method according to one of claims 1 to 9.

11. Packaging comprising the coated flexible support (10) obtained according to claim 10.