HOT REPAIR PROCESS
The use of CMC formwork elements addresses the challenges of complex repair geometries and uneven material distribution in hot repairs by enabling rapid, precise, and continuous operation of industrial installations.
Patent Information
- Application Number
- FR2022012561
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-11-30
AI Technical Summary
Conventional hot repair methods for industrial installations face challenges such as difficulty in creating complex interior formwork, uneven filling of repair material, and slow return to production due to the need for metal formwork that complicates the repair process and requires removal after hardening.
The use of Ceramic Matrix Composite (CMC) formwork elements that can be installed at high temperatures, allowing for precise adaptation to complex geometries and remaining in place after repair, combined with a repair product that can be cast and sintered in situ, eliminating the need for post-repair formwork removal.
Enables rapid and precise repair of industrial installations, maintaining operational continuity by allowing formwork to be left in place, thus reducing downtime and ensuring even distribution of the repair material.
Smart Images

Figure 00000033_0000 
Figure 00000034_0000 
Figure 00000034_0001
Abstract
Description
Title of the invention: HOT REPAIR METHOD Technical field
[0001] The present invention relates to a method for hot repair of an industrial installation, in particular of an industrial installation other than a glass furnace. Prior art
[0002] An industrial installation subjected to high temperatures conventionally comprises parts made of a refractory product, chosen according to the location where they are arranged, so as to withstand local constraints, in particular chemical and / or thermal attacks linked to the operation of said industrial installation, and to provide it with a satisfactory service life. The choice may also be guided by the need not to generate defects during the operation of the industrial installation, in particular when it is a steel melting furnace. For example, in an induction furnace for melting steel, it is necessary to avoid the addition of phosphorus which weakens the steel.
[0003] In order to increase the lifespan of an industrial installation, in particular an industrial furnace, the operator is required to carry out repairs. A repair consists of filling an empty space resulting from wear of the industrial installation with a repair material, that is to say, fixing a repair material in a region initially occupied by a refractory material and which has disappeared due to wear. This region is called the “region to be repaired”.
[0004] [Fig.l] represents a region of an industrial installation 10 such as before wear (on the left), and after wear (on the right). As illustrated in this figure, a region to be repaired 30, can be “hollow”, that is to say in the form of a cavity 30i, for example in a bottom wall 24. It can also be “projecting”, that is to say be a region 302 in the extension of an initially projecting block. The region to be repaired can also pass through the wall of an enclosure, for example the side wall of a tank 31, putting the inside and outside of the enclosure in fluid communication. Such a through region to be repaired can in particular lead to leaks, in particular of gas or product, in particular of molten product. These leaks are dangerous and can lead to a shutdown of the operation. The repair region 303 is an example of a through repair region created in a sidewall 22.
[0005] A region to be repaired is an empty space, i.e. one devoid of refractory material, partially delimited by one or more refractory parts of the industrial installation
[0006] To repair an industrial installation, in particular an industrial furnace, formwork is conventionally produced in order to materialize the region to be repaired and to produce, possibly with the refractory part(s), a mold capable of retaining the repair product before it hardens. The elements of the formwork, for example in the form of plates, flat or not, are conventionally held by accessories in a service position in which they define said mold.
[0007] The formwork comprises or consists of a part arranged on the side where the wear initially occurred. This part of the formwork is called "inner formwork". For example, to repair the wall of a furnace enclosure made of refractory blocks, an inner formwork is arranged to delimit, inside the enclosure, the region to be repaired.
[0008] When wear has led to a passage through the wall, the formwork may also include a portion outside the enclosure, or "external formwork", in order to prevent the repair material from escaping outside the enclosure. The external portion of the formwork is conventionally a veneer.
[0009] A "hot" repair is a repair that is carried out at a temperature typically above 250°C. Hot repairs therefore require only a limited reduction in temperature, or even no reduction in temperature, which considerably limits the duration of interruption of the operation of the industrial installation, or even eliminates it.
[0010] Furthermore, the region to be repaired, particularly inside a closed enclosure, is often difficult to access, which makes it difficult to create the interior formwork for certain regions to be repaired. In particular, the introduction of the interior formwork elements may require passages to be made through the wall of the enclosure. Furthermore, during a hot repair, no operator can sometimes enter the enclosure. The operation of installing the interior formwork must therefore be carried out at a distance from the region to be repaired. The size and weight of the interior formwork elements can therefore considerably slow down the creation of the formwork.
[0011] These constraints also make it very difficult to create interior formwork of complex shape, particularly when the region to be repaired projects towards the interior of the enclosure.
[0012] The mold is then filled with repair product, conventionally by means of a pump. The repair product undergoes a sudden increase in temperature when entering the mold, resulting in particular in a reduction in its ability to flow. It is therefore difficult to fill the mold evenly.
[0013] Conventionally, the inner formwork is made of metal and is cooled by circulating water. After the repair product has hardened, the inner formwork is removed.
[0014] After the repair product has hardened, the removal of the formwork leaves room for reconstructed refractory pieces. However, metal formwork generally does not allow the original shapes to be reconstructed if they are complex.
[0015] There is also a hot repair solution consisting of spraying ("guniting") a repair product into the area to be repaired. However, this repair technique does not allow for repairs of significant thickness.
[0016] There is thus a permanent need for a repair method solving the aforementioned problems, in particular allowing rapid return to production of the industrial installation.
[0017] The present invention aims to satisfy, at least partially, this need. Summary of the invention
[0018] The invention proposes a method for hot repairing a region of an industrial installation at a temperature above 250°C, in particular inside an enclosure of the industrial installation, in particular inside an enclosure of an industrial furnace, called "region to be repaired", the industrial installation preferably being different from a glassmaking furnace, said method comprising the following steps: (a) installation of a formwork in a service position, so as to make a mold around the area to be repaired; b) filling, preferably by pouring, the mold with a repair product, at least part of the formwork being made of a Ceramic Matrix Composite (CMC).
[0019] As will be seen in more detail in the remainder of the description, the inventors have notably discovered that a CMC does not significantly modify the quality of the product manufactured in said installation when it is brought into contact with said product, and / or does not significantly modify the operation of said industrial installation, and therefore does not require removal of the formwork at the end of the repair.
[0020] Furthermore, a CMC - is light, which makes it easy to handle, - is easy to conform to complex geometries, allowing precise adaptation to the configuration of the region to be repaired.
[0021] Additionally, a CMC is highly resistant to thermal shocks, which in particular allows hot repair without degradation of the formwork elements when they are introduced into an enclosure of the industrial installation.
[0022] The invention thus allows a particularly rapid return to production of the industrial installation.
[0023] A method according to the invention may also comprise one or more of the following optional and preferred characteristics: - the industrial installation is chosen from: - an iron or steel melting furnace, and part of such a furnace; - a non-ferrous metal melting furnace; - an element configured to transfer molten metal, in particular from a melting furnace of said metal, said element being able to be physically detached from said furnace; - a cement kiln; - an ore reduction furnace; - an incinerator; - a hazardous waste treatment furnace; - a gasifier; - a reformer; - a ceramic firing oven; - a carbon black reactor; - a retention tank intended to retain a molten product at a temperature above 250°C, particularly in the event of accidental spillage of said product; - an aluminum electrolysis cell; - a combustion chamber of a turbine; - a boiler; - the method comprises, after step b), a step 5) of sintering the repair product introduced into the mold in step b), the sintered repair product obtained being made up of a plurality of constituents, the mass content of any constituent of the sintered repair product present in a mass content greater than 5%, - differing by less than 20% from the mass content of said constituent in said ceramic matrix composite, and / or - differing by less than 20% from the mass content of said constituent in a region of the industrial installation delimiting the region to be repaired; - at least one element of said formwork has the shape of a part of the industrial installation which was protruding before said part disappeared through wear; - the manufacture of the formwork involves taking an impression on a replica, at least partial, of said industrial installation as it was before the wear leading to the region to be repaired; - the formwork is abandoned in the area to be repaired after said repair; - the formwork is entirely made of a ceramic matrix composite; - at least one element of the formwork made of a ceramic matrix composite comprises through holes and / or recesses arranged so as to be filled by the repair product during step b); - the formwork includes - formwork elements partially delimiting the area to be repaired, and - accessories for holding said formwork elements in a service position, said accessories being made of a ceramic matrix composite, identical to or different from the ceramic matrix composite of the formwork elements; - the ceramic matrix composite of at least part of the formwork, or even of the entire formwork, and / or the ceramic matrix composite of at least one accessory - is (are) sintered, and / or - have(s) an open porosity greater than 15% and less than 50%, and / or - contain(s) more than 20% and less than 80% by volume of fibers, and / or - comprise(s) fibers of which at least some are fibers comprising more than 95% by mass of oxides, and / or - comprise(s) fibers of which at least some are fibers comprising more than 95% by mass of a material other than an oxide, and / or - comprises a matrix composed of more than 90% oxides and / or carbides and / or nitrides and / or at least one oxynitride compound of at least the elements Si, Al and N, in particular a sialon, in mass percentage, and / or - have(s) an apparent density greater than 1.0 g / cm3 and less than 2 g / cm3; - said method comprises the following steps: 2) optionally, rinsing of the said area to be repaired, 3) optionally, reduction of the temperature in said industrial installation, up to a temperature above 250°C; 4) implementation of steps a) and b); 5) preferably, in particular when the method comprises a step 3), increasing and maintaining the temperature of the industrial installation between 400°C and 1400°C in order to sinter the repair product; 6) if said process includes a step 3), increasing the temperature of said industrial installation to its operating temperature; - the industrial installation comprises an enclosure containing a fluid product, preferably a powdered or molten product, in particular a molten metal, and said method comprises, before step a), the following step: - if the region to be repaired is, at least partially, delimited by a surface of the industrial installation in contact with said fluid product, emptying, at least partially, of said enclosure so as to expose said region to be repaired; and, after step b), the following step: - resumption of normal operations, the temperature of the industrial installation being maintained in the said region to be repaired during all stages of the process; - the industrial installation includes an enclosure containing a fluid product, preferably a powdered or molten product, in particular a molten metal, and said method comprises, before step a), the following steps: 1) if the region to be repaired is, at least partially, delimited by a surface of the industrial installation in contact with said fluid product, emptying, at least partially, of said enclosure, so as to expose said region to be repaired; 3) reduction of the temperature in the area to be repaired to a temperature above 250°C; and, after step b), the following steps: 5) increasing and maintaining the temperature of the region to be repaired between 1000°C and 1400°C in order to sinter the repair product; 6) resumption of normal operation of the industrial installation, i.e. adjustment of the temperature of said industrial installation to its operating temperature; - in step 3) the temperature in the region to be repaired is reduced to a temperature above 900°C and below 1500°C; - said method comprises a step of rinsing the region to be repaired after exposing the region to be repaired; - at least one element of the formwork has the shape of a part of the industrial installation which was protruding before said part disappeared through wear and, preferably, the manufacture of the formwork includes taking an impression on a replica of said part of said industrial installation before wear; - the region to be repaired is at least partly delimited by a side wall and / or a bottom wall of an enclosure, for example a tank intended to contain a molten product, said formwork comprising or being constituted by an internal formwork installed inside said enclosure in step a); - the enclosure is closed and inaccessible to an operator; - the area to be repaired is at least partly delimited by a flow channel.
[0024] The characteristics described in the context of a formwork in general are applicable, in the particular case of the repair of an enclosure, in particular a tank, to an internal formwork, whether or not the formwork used to repair the enclosure includes an external formwork, and whether or not the possible external formwork is made of a CMC. In particular, at least one element of the internal formwork may have the shape of a part of the enclosure which was projecting towards the inside of said enclosure before said part disappeared through wear, the manufacture of the internal formwork possibly including taking an impression on a replica of the part of said unworn enclosure.
[0025] The interior formwork may be left in the area to be repaired after said repair.
[0026] The invention also relates to an industrial installation, in particular an industrial furnace, comprising at least one region repaired according to a method according to the invention. Brief description of the figures
[0027] Other characteristics and advantages of the invention will become apparent upon examination of the description which follows and with regard to the appended drawing in which: - [Fig. 1][Fig. 1] schematically represents part of an enclosure before (left diagram) and after wear (right diagram); - [Fig.2][Fig.2] schematically represents a method according to the invention; - [Fig.3][Fig.3] represents an example of formwork according to the invention; - [Fig.4][Fig.4] represents an example of an interior formwork element comprising through holes; - [Fig.5] [Fig.5] schematically represents a casting channel for liquid iron (or "runner" in English), before wear, after wear and at the end of step b). Definitions
[0028] By "enclosure" is meant a part of an industrial installation which defines a chamber. An enclosure is delimited laterally by a side wall, the shape of which is not limiting, by a bottom wall, and optionally by a vault wall. The side wall, the bottom wall and the vault wall may have one or more openings for access to the chamber.
[0029] The term “tank” means an enclosure which, in service, contains a molten product, in particular a molten metal.
[0030] By “closed” tank or enclosure, we mean a tank or enclosure which an individual cannot enter during operation.
[0031] The invention is particularly well suited to the repair of an enclosure, in particular a tank, but is not limited to this embodiment.
[0032] A “formwork” is a part of the “mold” into which the repair product is introduced.
[0033] It generally results from an assembly of one or more “formwork elements” and a positioning of the assembled formwork element(s) in the “service position”. The part of the mold defined by the formwork is completed with a part of the industrial installation so as to constitute the mold. For example, the part of the interior surface of an enclosure which has been worn can complete the formwork to delimit the region to be repaired.
[0034] In addition to formwork elements, a formwork includes "accessories", used to assemble and fix the formwork elements in the service position, and which are not in contact with the repair material during the repair. Unlike accessories, formwork elements are parts which come into contact with the repair material during the repair.
[0035] The area to be repaired can be compartmentalized by means of partitions. A partition is considered as a formwork element.
[0036] A "passage" is a hole that passes through a wall, for example thus connecting the inside and the outside of an enclosure, for example a tank, a carbon black reactor, or a combustion chamber. It may result from wear of the wall or be provided, for example for the introduction of formwork elements through the wall.
[0037] The “equivalent diameter” of a surface is the diameter of a disk of the same area as that surface.
[0038] A dry particulate mixture is called an “unshaped product”.
[0039] By product “in one material” or “of one material” is meant a product made up for more than 95%, more than 98%, preferably substantially 100% of its mass of said material.
[0040] By "refractory material" is meant a material having a melting temperature greater than 1500°C. This definition is commonly used by those skilled in the art and cited in "Refractory materials and technical ceramics (elements of ceramurgical and technology)", G. Aliprandi, Septima Paris editions, 1979. This work also gives on pages 297 to 301 examples of refractory materials, in particular oxides, carbides and nitrides.
[0041] By "glass transition temperature" of a glass is meant the temperature at which said glass passes from the solid state to the viscous state. The glass transition temperature can be determined by differential thermal analysis (DTA). The glass transition temperature is the temperature at which said glass has a viscosity substantially equal to 1012 Pa.s. A glass is conventionally considered "in the solid state" at a temperature lower than its glass transition temperature.
[0042] By "hot binder" is meant a constituent having a melting temperature above 600°C, and capable of binding together, after hardening under the effect of a drop in temperature, particles with which it has been mixed.
[0043] The term "maximum size" refers to the 99.5 percentile (D99>5) of a powder, this percentile corresponding to the mass percentage of 99.5%, on the cumulative particle size distribution curve of the powder particles, the particle sizes being classified in ascending order. The particle size distributions and the maximum size can be determined using a laser granulometer. The laser granulometer can be a Partica LA-950 from HORIBA.
[0044] By "hot self-pouring" is meant a repair product capable of spreading under its own weight and filling the mold without leading to segregation, in a temperature range between 250°C and 1550°C. Segregation is considered to occur when the casting face of the product obtained after placement of the repair product and sintering has a surface layer of laitance. extending from the said casting face to a depth of 3 mm or more. This surface layer of laitance can easily be revealed after drying or sintering of the product, the sawing being carried out in a plane perpendicular to the casting face.
[0045] When referring to ZrO2 or zirconia, ZrO2 and traces of HfO2 should be understood. Indeed, a little HfO2, chemically inseparable from ZrO2 in a fusion process and having similar properties, is always naturally present in zirconia sources at mass contents generally less than 2%. Hafnium oxide is then not considered an impurity.
[0046] By “Ceramic Matrix Composite”, or “CMC”, we conventionally mean a ceramic composed of a ceramic textile stiffened by a ceramic matrix.
[0047] A “textile” is an assembly of fibers, possibly a yarn, in particular an assembly of yarns. The textile typically represents between 20% and 80% of the volume of a CMC, the remainder to 100% being the matrix.
[0048] Generally speaking, when referring to a volume percentage relative to an object, for example a CMC (for example a percentage of fibers) or the matrix of a CMC (as in the previous sentence), the volume to be considered is that of the object defined by its external surface, that is to say it includes the empty spaces inside the object.
[0049] A “fiber” is a filament whose length is greater than 5 times its equivalent diameter.
[0050] The "equivalent diameter" of a fiber is the diameter of a disk of the same surface area as its cross-section at mid-length.
[0051] In a textile, the fibers may be assembled in a disorderly manner, as in a felt or paper, or in one or more preferred directions, preferably in the form of threads, themselves preferably in the form of one or more fabrics. A thread of a textile may be - a “single yarn”, which is an assembly of fibers which, in cross-section, comprises more than 10 and preferably less than 500,000 fibers, and whose length is greater than 5 times the diameter, or - an “assembled yarn”, which is an assembly of single yarns which, in cross-section, preferably comprises more than 2 and preferably less than 500 single yarns.
[0052] A textile may be in particular: - an organized structure of fibers, and / or threads, simple or assembled, in particular a knit or a fabric, or - a random structure of fibers, and / or threads, single or assembled, for example a veil, and / or fibers not incorporated in the form of threads, said random structure which can be for example paper or felt, a random structure not being preferred.
[0053] A “fabric” consists of a network of parallel warp threads and weft threads crossing transversely said network.
[0054] A “knit” is made up of a network of threads in the form of loops.
[0055] A “sheet” is made up of a set of parallel wires.
[0056] By "ceramic" is meant a product that is neither metallic nor organic. For the purposes of the present invention, carbon is considered a ceramic product.
[0057] A “sialon”, SiAlON, is an oxynitride compound of at least the elements Si, Al and N, in particular a compound respecting one of the following formulas: - SixAlyOuNv, in which: - x is greater than or equal to 0, greater than 0.05, greater than 0.1 or greater than 0.2, and less than or equal to 1, less than or equal to 0.8 or less than or equal to 0.4, - y is greater than or equal to 0, or greater than 0.1, greater than 0.3 or greater than 0.5, and less than or equal to 1, - u is greater than 0, greater than 0.1 or greater than 0.2, and less than or equal to 1 or less than or equal to 0.7, - v is greater than 0, greater than 0.1, greater than 0.2 or greater than 0.5, or greater than 0.7, and less than or equal to 1, - %+y > 0, - x, y, u and v being stoichiometric indices and normalized with respect to the highest one, made equal to 1; - MexSii2-(m+n)Al(m+n)OnNi6_n, with 0 < x < 2, Me a cation chosen from the lanthanide cations, Fe, Y, Ca, Li and their mixtures, Q <m < 12, Q <n < 12 et 0 < n+m <12, les SiAlON suivant cette formule étant généralement appelés « a’ - SiAlON » ou « SiA10N-a’».
[0058] “Behave” or “understand” or “present” must be interpreted non-limiting manner. Detailed description Hot repair
[0059] A method according to the invention is used for the hot repair of a region of an industrial installation.
[0060] Preferably, the industrial installation is chosen from: - an iron or steel melting furnace, and a part of such a furnace, in particular an electric arc furnace (or "electrical arcfumace" in English), a submerged arc furnace (or "submerged arcfumace" in English), an electric furnace with plunging electrodes (or "open slag bath fumace" in English), a blast furnace (or "blast furnace" in English), an oxygen converter (or "basic oxygen fumace" in English), a direct reduction iron shaft furnace (or "direct reduction iron shaft furnace" in English), a casting channel (or "runner" in English), a steel reheating furnace (or "metal and iron reheat fumace" in English), a holding furnace (or "holder and melter furnace" in English), a tundish (or "tundish" in English); - a non-ferrous metal melting furnace, in particular an aluminium melting furnace, a magnesium melting furnace, a copper melting furnace; - an element physically independent of a melting furnace or physically detachable from a metal melting furnace, in contact with said molten metal and allowing said molten metal to be transferred from said melting furnace to another installation, in particular a transfer ladle; - a cement kiln, in particular a rotary kiln; - an ore reduction furnace, in particular an iron ore reduction furnace; - an incinerator, in particular a domestic waste incinerator, a household waste incineration boiler; - a hazardous waste treatment furnace; - a gasifier, in particular a coal gasifier, a petroleum coke gasifier, a biomass gasifier; - a reformer, in particular a methane reformer or a secondary reformer; - a ceramic firing oven; - a carbon black reactor; - a retention tank intended to retain a product at a temperature above 250°C in the event of accidental spillage of said product; - an aluminum electrolysis cell; - a combustion chamber of a turbine, in particular a gas turbine; - a boiler, in particular a thermal power station boiler.
[0061] The region to be repaired may in particular be located in a wall of the industrial installation, for example in the side wall of an enclosure, for example of a tank, of said industrial installation, in particular a wall of a closed enclosure, in particular of a closed tank.
[0062] The region to be repaired may have the shape of a cavity, through or not, for example a region in depression, in particular due to wear, for example opening towards the interior of an enclosure of the industrial installation.
[0063] [Fig.2] illustrates an example of a method according to the invention.
[0064] In one embodiment, in particular for the repair of an enclosure comprising a wall in contact with a fluid product, in particular a product in melting or powder, in the area to be repaired, for example for the repair of a tank of an iron or steel melting furnace, or of a non-ferrous metal melting furnace, in particular an aluminium melting furnace, a magnesium melting furnace, a copper melting furnace, or for the repair of a casting channel, in particular for such furnaces, or for the repair of a tank of an incinerator, the method comprises a step 1) of emptying, at least partially, said enclosure so as to expose said region to be repaired.
[0065] The fluid product may in particular be in liquid form or in powder form, for example in the form of ash.
[0066] The emptying can be carried out using any technique known to those skilled in the art.
[0067] For example, it is possible to evacuate the fluid product, in particular the molten product or the ashes through passages, for example pierced in the bottom wall of the enclosure or created by the dismantling of one or more electrodes or one or more burners.
[0068] Step 1) is optional for the repair of an enclosure whose part to be repaired is exposed, for example a part to be repaired which is not in contact with a fluid product, in particular with a molten product or with ash, such as for example for the repair of a vault wall, or of a wall of a turbine chamber, or of a ceramic firing furnace.
[0069] In step 2), optional, the region to be repaired is rinsed, that is to say freed from a large quantity of product residues with which it has been in contact during use of the industrial installation, according to any conventional technique. Preferably, a suitable product is sprayed, at least on the region to be repaired, in particular to fluidize the product residues with which it has been in contact during use, so that the evacuation of said residues is easier. For example, spraying sodium carbonate is well suited to fluidize a metallurgical slag residue.
[0070] In step 3), optional, the temperature in the region to be repaired may be reduced to a temperature above 250°C, preferably above 400°C, preferably above 500°C, preferably above 600°C, preferably above 700°C, preferably above 800°C, preferably above 900°C, and preferably below 1550°C, preferably below 1500°C, or even below 1450°C or 1400°C.
[0071] In one embodiment, the repair product used in step b) contains a hot binder, and in step 3), the temperature in the region to be repaired is reduced to a temperature at which the hot binder is not in the solid state. In particular, when the hot binder is a glass, the temperature is reduced to a temperature which remains su higher than the glass transition temperature of said glass. Said glass is preferably chosen so that its glass transition temperature is between 600°C and 1350°C, preferably between 900°C and 1350°C, preferably between 1000°C and 1300°C, preferably between 1150°C and 1250°C.
[0072] In step 4), the repair product is put in place following steps a) and b).
[0073] In step a), the region to be repaired is delimited using formwork 32, so as to constitute, with the industrial installation, in particular an industrial oven, a mold for the repair product.
[0074] The formwork 32 comprises, or is even made up ([Fig.3]) of, an internal formwork 32i, which delimits the mold inside the industrial installation. The internal formwork follows in particular the opening of the regions to be repaired 30i in the form of a cavity.
[0075] When the region to be repaired passes through a wall of the industrial installation, in particular the wall of an enclosure, for example the wall of a tank containing, in service, molten product, it opens through internal and external openings on internal and external faces of the wall, respectively. The formwork 32 then preferably comprises an external formwork, not shown, which delimits the external opening of the region to be repaired. The internal and external formwork retain the repair product before it is hardened, preferably sintered, so that it does not escape through the internal and external openings, respectively.
[0076] According to the invention at least part of the interior formwork, preferably all of the interior formwork, is made of a CMC.
[0077] In one embodiment, at least a portion of the exterior formwork, or even all of the exterior formwork, is made of a CMC.
[0078] In one embodiment, the outer formwork is made of a CMC, preferably identical to that of the inner formwork.
[0079] The manufacture of a CMC can be carried out by any conventional method.
[0080] The person skilled in the art knows how to adjust the parameters of the process chosen for the manufacture of the CMC, and in particular how to determine the particle size of the raw materials, the water content during shaping, and the sintering temperature if the CMC is sintered.
[0081] The manufacture of a CMC may in particular comprise the following steps: i) arrangement, on or in a textile, of a slip capable of forming a ceramic matrix after consolidation; ii) before or after step i), shaping of the textile; iii) consolidation of the preform obtained after the previous steps, preferably by drying and / or sintering, so as to form said matrix and obtain the CMC.
[0082] In step i), the textile is a set of fibers, preferably assembled in the form of threads, a thread typically comprising several hundred to several thousand fibers. The fibers, preferably the yarns, preferably have a length greater than 50 mm, or even greater than 100 mm. In one embodiment, the fibers, preferably the yarns, are arranged in the form of at least one fabric.
[0083] The textile may in particular have the form of a felt of unordered threads and / or fibers, of a sheet, for example a sheet made up of threads extending substantially parallel to one another (said threads being called "unidirectional threads"), of a knit, of a fabric (i.e. a woven textile) or of a stack of one or more felts and / or sheets, and / or knits and / or fabrics.
[0084] The textile preferably has the form of a felt or a fabric or a sheet or a stack of felt(s) and / or sheet(s) and / or fabric(s). The stacking of the fabrics and / or sheets can be carried out in such a way that the threads of the different fabrics or sheets extend substantially all in the same direction, or in 2, 3, 4, 5 or 6 different directions, depending in particular on the desired mechanical properties.
[0085] Preferably, at least a portion, preferably all of said ceramic fibers of the textile, optionally assembled in the form of single and / or assembled threads, are - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides, and / or - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide.
[0086] Preferably, said ceramic fibers of the textile comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides are: - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides and having a chemical analysis such as SiO2 + A12O3 + ZrO2 > 50%, preferably SiO2 + A12O3 + ZrO2 > 60%, or even SiO2 + A12O3 + ZrO2 > 70%, or even SiO2 + A12O3 + ZrO2 > 80%, or even SiO2 + A12O3 + ZrO2 > 90%, as a percentage by mass, and / or - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides and having a chemical analysis such as SiO2 > 70%, preferably SiO2 > 80%, preferably SiO2 > 90%, or even SiO2 > 99%, as a percentage by mass, and / or - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides and having a chemical analysis such that A12O3 > 65%, preferably A12O3 > 70%, or even A12O3 > 80%, or even A12O3 > 90%, or even A12O3 > 95%, as a percentage by mass.
[0087] More preferably, at least a portion, preferably all of said ceramic fibers, are: - fibers composed of more than 95%, preferably more than 98%, preferably more than 99%, preferably substantially 100% by mass of alumina, and / or - fibers composed of more than 95%, preferably more than 98%, preferably more than 99%, preferably substantially 100% by mass of silica, preferably composed of more than 95%, preferably more than 98%, of amorphous silica, and / or - fibers composed of more than 95%, preferably more than 98%, preferably more than 99%, preferably substantially 100% by mass of mullite and corundum, and / or - fibers composed of more than 95%, preferably more than 98%, preferably more than 99%, preferably substantially 100% by mass of glass, preferably washed, and / or - a mixture of said fibers.
[0088] Preferably, said ceramic fibers of the textile comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide are: - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a carbide, preferably chosen from silicon carbide, boron carbide and mixtures thereof, and / or - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a boride, preferably a titanium boride, and / or - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a nitride, preferably a silicon nitride, and / or - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbon.
[0089] Preferably, said ceramic fibers of the textile comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide are: - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of silicon carbide, and / or - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbon.
[0090] In one embodiment, at least a portion, preferably all of said ceramic fibers, are fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides.
[0091] In one embodiment, at least a portion, preferably all of said ceramic fibers, are fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide.
[0092] In one embodiment, substantially all of the fibers have the same composition.
[0093] The arrangement of the slip on or in the textile can be for example by impregnation. Said stacking can be carried out by pressing, or under vacuum, preferably after impregnation.
[0094] The manufacture of slip is well known to those skilled in the art. Slip is conventionally a suspension, for example of an aqueous base or an organic solvent, containing - ceramic particles and / or precursors of ceramic particles, i.e. compounds which transform into ceramic particles during the manufacture of the CMC, and in particular during hardening, in particular sintering, and - optionally dispersants, plasticizers, lubricants, and / or temporary binders.
[0095] The composition of the slip, the size distribution of the ceramic particles or ceramic precursors and the mineral filler of the slip are adapted to the type of fibers and the shaping technique. For example, the slip can be placed on or in the textile, in particular by direct lamination, by infusion, injection, infiltration or deposition, under atmospheric pressure or under higher pressure or under vacuum, at room temperature or at higher temperature.
[0096] In step ii), the textile obtained, preferably impregnated with the slip, is shaped. The desired shape is preferably the final shape of the CMC. In one embodiment, the shape can however be modified after hardening of the matrix, for example by machining or by deformation.
[0097] Preferably, to produce the interior formwork, the textile is shaped so that the shape of the CMC is adapted so that, after installation of the formwork, the repair material only replaces material that has been extracted by wear, preferably replaces all the material that has been extracted by wear.
[0098] The shape can be given by making, with the textile (before or preferably after introduction of the slip), an imprint on a reproduction of the part to be repaired of the industrial installation before wear. The mold is then a “negative” of the region to be repaired. For example, if the region to be repaired is a pouring channel, the CMC can be carried out by depositing the textile, preferably in the form of a fabric or a superposition of several fabrics, on a replica of said pouring channel, before or after impregnation with the slip but before consolidation, so that this textile fits the surface of the pouring channel, at least in the region corresponding to the region to be repaired. The use of a CMC advantageously makes it possible to easily produce complex shapes, possibly non-developable. The repair thus makes it possible to precisely reconstitute the initial profile of the surface of the industrial installation, in particular the interior surface of an enclosure, for example a tank, of the industrial installation.
[0099] The CMC can be manufactured by arranging prepregs on top of each other, each consisting of a fabric impregnated with a slip of ceramic particles. The prepregs are flexible, so that they can take the desired shape.
[0100] In step iii), consolidation, preferably by sintering, is preferably carried out before installation of the formwork, which facilitates this installation.
[0101] Generally speaking, the characteristics of CMC result from its manufacturing process.
[0102] Preferably, the CMC has one or more of the following optional characteristics: - the CMC is preferably sintered; - the CMC preferably has an open porosity, measured by imbibition, according to the principle of Archimedes' thrust, greater than 10%, preferably greater than 15%, preferably greater than 20%, preferably greater than 25%, preferably greater than 30%, and preferably less than 50%, preferably less than 45%, preferably less than 40%; - preferably, the CMC comprises more than 20%, preferably more than 25%, preferably more than 30%, preferably more than 40%, preferably more than 50%, preferably more than 60% and / or less than 80%, preferably less than 70% by volume of fibers;
[0103] - at least a portion, preferably all of the ceramic fibers of the CMC, are fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides; - at least a portion, preferably all of the ceramic fibers of the CMC, are fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide; - the CMC matrix is composed of more than 90%, preferably more than 95%, preferably more than 97%, preferably more than 98%, preferably for more than 99%, preferably for more than 99.5% by mass - oxides, and / or - carbides and / or nitrides and / or sialons, in particular of the type described above; - the CMC has an apparent density greater than 1.0 g / cm3, preferably greater than 1.20 g / cm3, preferably greater than 1.40 g / cm3 and / or less than 2.50 g / cm3, preferably less than 2.00 g / cm3, preferably less than 1.90 g / cm3.
[0104] In a first embodiment, the CMC consists of oxides for more than 90% of its mass, preferably for more than 95% of its mass, preferably for more than 98% of its mass, preferably for more than 99% of its mass, preferably for more than 99.5% of its mass.
[0105] In said first embodiment, the CMC has one or more of the following optional and preferred features: - the CMC comprises fibers, said fibers being composed of oxides for more than 90%, preferably for more than 95%, preferably for more than 97%, preferably for more than 98%, preferably for more than 99%, preferably for more than 99.5% by mass; - at least a portion, preferably all of said ceramic fibers, are: - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides and having a chemical analysis such as SiO2 + A12O3 + ZrO2 > 50%, preferably SiO2 + A12O3 + ZrO2 > 60%, or even SiO2 + A12O3 + ZrO2 > 70%, or even SiO2 + A12O3 + ZrO2 > 80%, or even SiO2 + A12O3 + ZrO2 > 90%, as a percentage by mass, and / or - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides and having a chemical analysis such as SiO2 > 70%, preferably SiO2 > 80%, preferably SiO2 > 90%, or even SiO2 > 99%, as a percentage by mass, and / or - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides and having a chemical analysis such that A12O3 > 65%, preferably A12O3 > 70%, or even A12O3 > 80%, or even A12O3 > 90%, or even A12O3 > 95%, or even A12O3 > 97%, or even A12O3 > 98%, as a percentage by mass; - the matrix of said CMC is composed of oxides for more than 90%, preferably for more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass; - preferably, the CMC matrix is substantially made up of oxides; - the CMC matrix comprises A12O3 and / or SiO2 and / or ZrO2 and / or Cr2O3; - preferably, the CMC matrix comprises A12O3 and SiO2; - in one embodiment, the content of A12O3 in the CMC matrix, in percentage by mass based on the mass of the matrix, is greater than 65%, preferably greater than 70%; - in one embodiment, the SiO2 content in the CMC matrix, as a percentage by mass based on the mass of the matrix, is greater than 15%, preferably greater than 20% and / or less than 35%, preferably less than 30%; - in one embodiment, the SiO2 content in the CMC matrix, as a percentage by mass based on the mass of the matrix, is greater than 60%, preferably greater than 70%, preferably greater than 80%; - in one embodiment, the content of oxides other than Al2O3 and SiO2 in the CMC matrix, in mass percentage based on the mass of the matrix, is less than 3%, preferably less than 2%, preferably less than 1%; - in one embodiment, the total content of Al2O3 and SiO2 in the CMC matrix is greater than 80%, preferably greater than 85%, preferably greater than 90%, preferably greater than 95%, as a percentage by mass based on the mass of the matrix; - in one embodiment, the silica of the CMC matrix is amorphous; - preferably, the CMC has a total mass content of SiO2+Al2O3+ZrO2+Cr2O3 greater than 80%, preferably greater than 85%, preferably greater than 90%, preferably greater than 95%, preferably greater than 97%, preferably greater than 97%. More preferably, the CMC has a total mass content of SiO2+Al2O3 greater than 80%, preferably greater than 85%, preferably greater than 90%, preferably greater than 95%, preferably greater than 97%, preferably greater than 97%;
[0106] - in a preferred embodiment, the CMC has the following chemical analysis, as a percentage by mass and for a total of 100%: - SiO2: 47% - 67%, - A12O3: 32% - 52%, - species other than A12O3 and SiO2: < 5%, preferably < 4%, preferably < 3%, preferably < 2%; - in one embodiment, the CMC is preferably amorphous, and has the following chemical analysis, in percentage by mass and for a total of 100%: - SiO2: > 95%, preferably > 96%, preferably > 97%, preferably > 98%, preferably >99%.
[0107] In a second embodiment, the CMC is made of a material other than an oxide, for more than 90% of its mass, preferably for more than 95% of its mass, preferably for more than 98% of its mass, preferably for more than 99% of its mass, preferably for more than 99.5% of its mass.
[0108] In said second embodiment, the CMC has one or more of the following optional and preferred features: - the CMC comprises fibers, said fibers being composed of a non-oxide material for more than 90%, preferably for more than 95%, preferably for more than 97%, preferably for more than 98%, preferably for more than 99%, preferably for more than 99.5% by mass; - at least a portion, preferably all of said ceramic fibers, are: - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbon, and / or - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a carbide, preferably chosen from silicon carbide, boron carbide and mixtures thereof, and / or - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a boride, preferably a titanium boride, and / or - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a nitride, preferably a silicon nitride, and / or - fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbon.
[0109] In said second embodiment, the CMC has one or more of the following optional and preferred characteristics: - preferably, said ceramic fibers of the textile comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide are fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of silicon carbide, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbon; - the matrix of said CMC is composed for more than 90%, preferably for more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide, preferably chosen from carbides, borides, nitrides, SiAlON and their mixtures; - preferably, the CMC matrix comprises, or even consists of, silicon carbide, silicon nitride, metallic silicon, or a mixture thereof;
[0110] - in a particular embodiment of the second embodiment, the CMC comprises fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of silicon carbide, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbon, and a matrix composed of more than 90%, preferably more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of silicon carbide, silicon nitride, metallic silicon, and mixtures thereof.In said embodiment, the matrix is preferably composed, for more than 90%, preferably for more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass, of silicon carbide or of a mixture of silicon carbide and metallic silicon or of a mixture of silicon carbide and silicon nitride; . - in one embodiment, the silicon carbide of the matrix is a recrystallized silicon carbide.
[0111] In a third embodiment, the CMC comprises - fibers composed of a non-oxide material for more than 90%, preferably for more than 95%, preferably for more than 97%, preferably for more than 98%, preferably for more than 99%, preferably for more than 99.5% by mass and - a matrix composed of oxides for more than 90%, preferably for more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass.
[0112] In said third embodiment, the CMC has one or more of the following optional and preferred features: - at least a portion, preferably all of the fibers composed of a non-oxide material for more than 90%, preferably for more than 95%, preferably for more than 97%, preferably for more than 98%, preferably for more than 99%, preferably for more than 99.5% by mass, are fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbon and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbide, preferably silicon carbide, and / or - the CMC matrix comprises, or is made up of, A12O3 and / or SiO2 and / or ZrO2 and / or Cr2O3; - preferably, the CMC matrix comprises, or even consists of, A12O3 and SiO2; - in one embodiment, the content of A12O3 in the CMC matrix, in percentage by mass based on the matrix, is greater than 65%, preferably greater than 70%; - in one embodiment, the SiO2 content in the CMC matrix, as a percentage by mass based on the matrix, is greater than 15%, preferably greater than 20% and / or less than 35%, preferably less than 30%; - in one embodiment, the SiO2 content in the CMC matrix, as a percentage by mass based on the matrix, is greater than 60%, preferably greater than 70%, preferably greater than 80%; - in one embodiment, the content of species other than Al2O3 and SiO2 in the CMC matrix, in mass percentage based on the matrix, is less than 3%, preferably less than 2%, preferably less than 1%; - in one embodiment, the total content of Al2O3 and SiO2 in the CMC matrix is greater than 80%, preferably greater than 85%, preferably greater than 90%, preferably greater than 95%, as a percentage by mass based on the matrix; - in one embodiment, the silica of the CMC matrix is amorphous.
[0113] In a fourth embodiment, the CMC comprises - fibers composed of oxides for more than 90%, preferably for more than 95%, preferably for more than 97%, preferably for more than 98%, preferably for more than 99%, preferably for more than 99.5% by mass, and - a matrix composed of more than 90%, preferably more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide, preferably chosen from carbon, carbides, borides, nitrides, and SiAlON.
[0114] In said fourth embodiment, the CMC preferably has one or more of the following optional features: - the CMC comprises fibers having a chemical analysis such as SiO2 + A12O 3 + ZrO2 > 50%, preferably SiO2 + A12O3 + ZrO2 > 60%, or even SiO2 + A12O3 + ZrO2 > 70%, or even SiO2 + A12O3 + ZrO2 > 80%, or even SiO2 + A12O3 + ZrO2 > 90%, in percentage by mass; - the CMC comprises fibers having a chemical analysis such as SiO2 > 70%, preferably SiO2 > 80%, preferably SiO2 > 90%, or even SiO2 > 99%, in percentage by mass; - the CMC comprises fibers having a chemical analysis such that A12O3 > 65%, preferably A12O3 > 70%, or even A12O3 > 80%, or even A12O3 > 90%, or even Al2 O3 > 95%, or even A12O3 > 97%, or even A12O3 > 98%, as a percentage by mass; - the CMC matrix is preferably composed, for more than 90%, preferably for more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass, of silicon carbide or of a mixture of silicon carbide and metallic silicon or of a mixture of silicon carbide and silicon nitride
[0115] In one embodiment, the CMC is chosen so as to have a chemical analysis close to that of the material of the industrial installation which delimits the region to be repaired, preferably so that the content of any constituent of the sintered repair product present in a mass content greater than 5%, differs by less than 20%, preferably by less than 10% from the content of said constituent in said material.
[0116] The formwork is then installed by assembling its elements.
[0117] Installing interior formwork in an enclosure can be tricky given the difficulty of access.
[0118] The interior formwork elements can be introduced through a passage which opens inside the enclosure, in the region to be repaired or not.
[0119] When being installed, the interior formwork elements which have two large opposite faces can be held by the large face which, in the service position, is exposed inside the industrial installation, or by the large opposite face.
[0120] In one embodiment, as illustrated in [Fig.4], at least one element of the formwork, in particular the interior formwork, in a CMC comprises through holes and / or recesses. Filling these holes and recesses with the repair product during step b) advantageously allows better immobilization of the interior formwork and makes it possible to reduce the thermal gradient in the repair product during step 5). Preferably, the average equivalent diameter of the holes is greater than 8 mm and preferably less than 20 mm, preferably less than 15 mm.
[0121] In one embodiment, said formwork element in a CMC is in the form of a grid, the holes preferably being distributed homogeneously, the total surface area of the holes representing more than 10%, preferably more than 15% and preferably less than 50%, preferably less than 40% of the interior surface area of said formwork element, i.e. the surface area participating in the definition of the mold around the region to be repaired (surface area of the holes and of the material of the grid).
[0122] In one embodiment, said holes are located on the lower two-thirds of said formwork element, and preferably distributed homogeneously. More preferably, in said embodiment, the total surface area of the holes represents more than 1% and less than 5% of the interior surface area of said formwork element (surface area holes and material of said formwork element).
[0123] The provision of through holes and / or recesses may be carried out by any technique known to those skilled in the art. In particular, through holes may be made by drilling or water jet cutting of the CMC obtained after sintering. The through holes and / or recesses may also be made on the textile, preferably a woven fabric, before coating with the slip.
[0124] Accessories are then conventionally used to hold the formwork elements in the service position.
[0125] In one embodiment, the sealing between the formwork, in particular the interior formwork, and the surface of the industrial installation defining the region to be repaired is increased by placing a sheet of ceramic fibers between said formwork and said surface.
[0126] [Fig. 3] illustrates an example of internal formwork according to the invention. In particular, the internal formwork 32i can be seen, and in particular three adjacent panels 351 and 352 and 353 held in position by means of metal clamps 39, wedging bricks 43 and cooled tubes 45. Repair product 47 fills the region to be repaired 30i delimited by the surface of the worn region and the internal formwork.
[0127] After the formwork has been installed, the repair product may be introduced into the area to be repaired, for example via a water-cooled cane.
[0128] In step b), the mold which delimits the region to be repaired is filled with a repair product, preferably by casting. Repair product
[0129] The repair product may be a conventional repair product and may be prepared by any known technique.
[0130] Preferably, the repair product is the result of the humidification of an unshaped product. Said humidification can be carried out according to any known technique, for example in a mixer. The person skilled in the art knows how to determine the quantity of solvent, preferably water, to be used to humidify the unshaped product and obtain the repair product.
[0131] The unshaped product may in particular be: - Pural T concrete and / or Pural M concrete, in particular when the industrial installation is an iron or steel melting furnace, and a part of such a furnace, a non-ferrous metal melting furnace, or an element configured to transfer molten metal, in particular from a melting furnace of said metal, said element being able to be physically separated from said furnace, - Sialfrax 18 Cast, Sialfrax 30 Shot, Alfrax 60 Shot or Castfrax 902, especially when the industrial installation is a casting channel.
[0132] These unshaped products are marketed by the company Saint-Gobain Per- formance Ceramics & Refractories.
[0133] Preferably, the maximum particle size of the repair product or, equivalently, of the unshaped product, is less than 10 mm, preferably less than 8 mm, preferably less than 6 mm.
[0134] The particle size distribution of the repair product or, equivalently, of the unshaped product is preferably determined so that the repair product is self-flowing when hot.
[0135] Preferably, the repair product is chosen so as to present, after sintering, a chemical analysis close to that of the material of the industrial installation which delimits the region to be repaired, preferably so that the mass content of any constituent of the sintered repair product present in a mass content greater than 5%, differs by less than 20%, preferably by less than 10% from the content of said constituent in said material.
[0136] In one embodiment, the repair product is chosen so as to have, after sintering, a chemical analysis close to that of the CMC of the formwork elements, preferably so that the mass content of any constituent of the sintered repair product present in a mass content greater than 5%, differs by less than 20%, preferably by less than 10% from the content of said constituent in said CMC.
[0137] For example, if the region to be repaired is delimited by one or more refractory blocks made of a product with a high alumina content, the unshaped product for manufacturing the repair product is preferably Pural T concrete.
[0138] The repair product can be brought to the region to be repaired using any technique known to the person skilled in the art.
[0139] If access to the region to be repaired is difficult, one or more passages, for example made by drilling, can be provided to facilitate this access. These passages advantageously allow the introduction of a device for conveying the repair product, for example a cooled rod, to the region to be repaired.
[0140] In one embodiment, the repair product is pumped by means of a pump producing a suction pressure preferably less than or equal to 180 bar and preferably conveyed to the region to be repaired by means of a water-cooled rod or a nozzle.
[0141] Throughout step b), the region to be repaired is preferably maintained at a temperature above 300°C, preferably above 400°C, preferably above 500°C, preferably above 600°C, preferably above 700°C, preferably above 800°C, preferably above 900°C, and / or preferably below 1550°C, preferably below 1500°C.
[0142] In step 5), optional, and in particular if the method includes a step 3), the industrial installation is maintained at a temperature between 400°C and 1400°C, preferably between 600°C and 1400°C, preferably between 1000°C and 1400°C, in order to allow sintering of the repair product, preferably for a period of more than 8 hours, preferably more than 10 hours and preferably less than 15 hours.
[0143] In step 6), normal operation of the installation is resumed, and if the process includes a step 3), the temperature of the industrial installation is increased to restart operation. Examples
[0144] The following non-limiting examples are given with a view to illustrating the invention.
[0145] In a first particular embodiment, in particular when the region to be repaired belongs to a wall separating an “interior” space and an “exterior” space, the interior formwork is made of a CMC, preferably one or more plates made of a CMC, preferably held against the healthy part of the wall using one or more metal rods, preferably cooled using water circulation. If the region to be repaired opens out on the exterior side of the wall, an exterior formwork, preferably made of a ceramic, preferably in the form of a CMC, is fixed so as to externally seal the region to be repaired.
[0146] The area to be repaired is then filled with the repair product. The repair product is preferably conveyed from the outside by a pipe passing through one or more passages made through the wall, then poured into the area to be repaired using a rod cooled by circulating water.
[0147] Preferably, at least the interior formwork, preferably the formwork, is not removed after installation of the repair product.
[0148] In a second particular embodiment, in particular when the region to be repaired results from wear of a tank of the industrial installation, at least partial emptying of said tank is carried out. The internal formwork is made of a CMC, preferably one or more plates of a CMC, preferably held against the tank using one or more tubes of a ceramic, preferably in the form of a CMC, and / or one or more metal rods, preferably cooled using a circulation of water. If the region to be repaired opens out to the outside of the tank, a plating, constituting the external formwork, preferably made of a ceramic, preferably in the form of a CMC, is fixed so as to externally seal the region to be repaired.
[0149] The area to be repaired is then filled with the repair product. The repair product is preferably conveyed, from outside the tank, by a pipe passing through one or more passages made through the wall of the tank, then poured into the area to be repaired using a rod cooled by circulating water.
[0150] Preferably, the CMC formwork is not removed after installation of the repair product.
[0151] [Fig. 5] illustrates the repair of a pouring channel initially consisting, from the outside to the inside, of a metal casing 50, a thermal insulation layer 52, an outer coating 54 and an inner coating 56 (left diagram). The central diagram illustrates the pouring channel after wear of the inner coating 56 and the right figure illustrates the pouring channel after repair.
[0152] The following example was carried out.
[0153] To manufacture the repair product, the unshaped product Castfrax 902 SRAW, marketed by Saint-Gobain Performance Ceramics & Refractories, was mixed for 1 minute in a mixer with a rotating blade and fixed bowl, with 0.15% of a modified polycarboxylate ether, as a percentage by mass based on the unshaped product. Then 8% of water, as a percentage by mass based on the unshaped product, was added and mixing continued until a homogeneous repair product was obtained.
[0154] 160 kg of repair product were prepared. This repair product was self- hot-pourable.
[0155] A one-piece mold in a CMC was produced.
[0156] This mold had a general rectangular parallelepiped shape, with a length equal to 600 mm, a width equal to 150 mm, and a height equal to 450 mm, the thickness of the walls of said mold being substantially constant and equal to 10 mm.
[0157] The CMC constituting the mold had a thermal conductivity between 20°C and 500°C of less than 0.6 Wm *.K '.
[0158] The CMC was made up of: - a superposition of fabrics (or "woven fabrics" in English) made of washed glass fibers (or "leached glass" in English) with a silica content greater than 90% by mass, representing 44% of the mass of the CMC, and - an alumina and silica matrix, representing 56% of the mass of the CMC.
[0159] Said CMC had an open porosity equal to 38%, an apparent density equal to 1.65 g / cm3, an Al2O3 content equal to 42%, a SiO2 content equal to 57% and a content of other constituents, for example oxides, equal to 1%, the contents of Al2O3, SiO2 and other constituents being expressed as mass percentages on the basis of said CMC.
[0160] The mold was placed in an oven with a gas burner.
[0161] The furnace was then started up so as to reach a temperature of 1200°C in 2 hours and 40 minutes, simulating a hot introduction of the CMC mold into an industrial installation, in particular a cast iron casting channel of a blast furnace.
[0162] The casting of the repair product into the mold, maintained at 1200°C, was carried out using a metal chute placed above an opening made in the vault of the furnace.
[0163] The repair product was poured continuously, with a flow rate substantially equal to 100 kg / min.
[0164] During filling, it was found that the CMC mold resisted the thrust of the repair product, without breaking or opening.
[0165] After filling the mold, the temperature was maintained at 1200°C for 4 hours. The temperature was then gradually reduced to 800°C, at a rate substantially equal to 25°C / h. Then the burner was switched off and the temperature was lowered naturally, without opening the furnace.
[0166] The sintered repair product in the mold was then recovered.
[0167] After sawing, it presented a homogeneous texture, without cracks or internal cavities. which may correspond to a power outage.
[0168] As is now clearly apparent, the invention thus provides a hot repair method which uses CMC elements, in particular to produce the interior formwork, which: - allows rapid manufacturing that is perfectly adapted to the region to be repaired, in particular because a CMC can be shaped into complex forms, and in particular in such a way as to match the profile of the region to be repaired; - facilitates the introduction of these elements to the area to be repaired; - facilitates their arrangement, these elements being light; - allows a sacrifice of the formwork element, i.e. its maintenance in position after the repair, in particular because the composition of a CMC can be chosen to be similar to that of the repair product.
[0169] Of course, the present invention is not limited to the embodiments described or represented, provided as illustrative and non-limiting examples.
[0170] In particular, the compositions of the CMCs of the different parts of the formwork and / or accessories may be identical or different.
Claims
Claims
1. Method for hot repair of a region of an industrial installation, said region being at a temperature above 250°C, called "region to be repaired" (30i, 302,303), said method comprising the following steps: a) installation of a formwork (32) in a service position, so as to produce a mold around the region to be repaired; b) filling, preferably by pouring, the mold with a repair product (47), at least part of the formwork being made of a Ceramic Matrix Composite, the industrial installation being different from a glassmaking furnace.
2. Method according to the preceding claim, in which the industrial installation is chosen from: - an iron or steel melting furnace, and a part of such a furnace; - a non-ferrous metal melting furnace; - an element configured to transfer molten metal; - a cement kiln; - an ore reduction furnace; - an incinerator; - a hazardous waste treatment furnace; - a gasifier; - a reformer; - a ceramic firing furnace; - a carbon black reactor; - a holding tank intended to retain a molten product at a temperature above 250°C; - an aluminum electrolysis cell; - a combustion chamber of a turbine; - a boiler.
3. Method according to any one of the preceding claims, comprising, after step b), a step 5) of sintering the repair product introduced into the mold in step b), the sintered repair product obtained being made up of a plurality of constituents, the mass content of any constituent of the sintered repair product present in a mass content greater than 5%, - differing by less than 20% from the mass content of said constituent in said ceramic matrix composite, and / or - differing by less than 20% from the mass content of said constituent in a region of the industrial installation delimiting the region to be repaired.
4. A method according to any preceding claim, wherein at least one element of said formwork has the shape of a part of the industrial installation which was protruding before said part disappeared through wear.
5. Method according to any one of the immediately preceding claims, in which the manufacture of the formwork comprises taking an impression on a replica, at least partial, of said industrial installation as before the wear having led to the region to be repaired.
6. A method according to any preceding claim, wherein the formwork is left in the region to be repaired after said repair.
7. A method according to any preceding claim, wherein the inner formwork is entirely of a ceramic matrix composite.
8. A method according to any one of the preceding claims, wherein at least one element of the formwork made of a ceramic matrix composite comprises through holes and / or recesses arranged to be filled by the repair product during step b).
9. Method according to any one of the preceding claims, in which the formwork comprises - formwork elements partially delimiting the region to be repaired, and - accessories for holding said formwork elements in a service position, said accessories being made of a ceramic matrix composite, identical to or different from the ceramic matrix composite of the formwork elements.
10. A method according to any preceding claim, wherein the ceramic matrix composite of at least one part of the formwork and / or, where the immediately preceding claim applies, the ceramic matrix composite of at least one accessory - is (are) sintered, and - has (have) an open porosity greater than 15% and less than 50%, and - comprises (have) more than 20% and less than 80% by volume of fibers, and and - comprise(s) a matrix composed of more than 90% oxides and / or carbides and / or nitrides and / or oxynitride compound(s) of at least the elements Si, Al and N, in mass percentage, and - have(s) an apparent density greater than 1.0 g / cm3 and less than 2 g / cm3.
11. A method according to any one of the preceding claims, said method comprising the following steps: 3) reducing the temperature in said industrial installation to a temperature above 250°C; 4) carrying out steps a) and b); 5) increasing and maintaining the temperature of the industrial installation between 400°C and 1400°C in order to sinter the repair product; 6) increasing the temperature of said industrial installation to its operating temperature.
12. Method according to any one of claims 1 to 10, the industrial installation comprising an enclosure containing a fluid product, said method comprising, before step a), the following step: - if the region to be repaired is, at least partially, delimited by a surface of the industrial installation in contact with said fluid product, emptying, at least partially, said enclosure so as to expose said region to be repaired; and, after step b), the following step: - resumption of normal operation, the temperature of the industrial installation being maintained in said region to be repaired during all the steps of the method.
13. Method according to any one of claims 1 to 10, the industrial installation comprising an enclosure containing a fluid product, said method comprising, before step a), the following steps: 1) if the region to be repaired is, at least partially, delimited by a surface of the industrial installation in contact with said fluid product, emptying, at least partially, said enclosure, so as to expose said region to be repaired; 3) reducing the temperature in the region to be repaired to a temperature above 250°C; and, after step b), the following steps: 5) increasing and maintaining the temperature of the region to be repaired between 1000°C and 1400°C in order to sinter the repair product; 6) resumption of normal operation of the industrial facility.
14. Method according to the immediately preceding claim, in which, in step 3) the temperature in the region to be repaired is reduced to a temperature above 900°C and below 1500°C.
15. A method according to any one of the three immediately preceding claims, comprising a step of rinsing the region to be repaired after exposing the region to be repaired.
16. Method according to any one of the preceding claims, in which the region to be repaired is at least partly delimited - by a pouring channel or - by a side wall (22) or a bottom wall (24) of a tank (31) intended to contain a molten product, said formwork (32) comprising or being constituted by an internal formwork (32i) installed inside said tank in step a).
17. A method according to the immediately preceding claim, wherein the tank defines a closed enclosure inaccessible to an operator.