Catalyst comprising a very high-purity AFX structural-type IZM-9 zeolite and at least one transition metal for the selective reduction of NOx
The IZM-9 zeolite catalyst, synthesized with specific organic agents and transition metals, addresses the inefficiencies of existing catalysts by achieving lower initiation temperatures and enhanced NOx conversion, meeting stringent emission standards with improved selectivity.
Patent Information
- Application Number
- FR2022013064
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-12-09
AI Technical Summary
Existing catalysts based on small-pore zeolites like Cu-SSZ-13 and Cu-SAPO-34 struggle to meet increasingly stringent NOx emission standards, particularly in terms of conversion efficiency and hydrothermal stability, necessitating improved catalysts for selective catalytic reduction (SCR) of NOx in diesel engine exhausts.
A catalyst is developed using an IZM-9 zeolite of AFX structural type, synthesized with a specific mixture of organic structuring agents and transition metals like iron or copper, through a process involving gel formation, hydrothermal treatment, and ion exchange, resulting in a catalyst with enhanced NOx conversion and selectivity.
The catalyst achieves lower initiation temperatures and improved NOx conversion across a broader temperature range while maintaining good selectivity towards N2O, outperforming prior art catalysts in terms of efficiency and stability.
Smart Images

Figure 00000029_0000 
Figure 00000029_0001 
Figure 00000030_0000
Abstract
Description
Title of the invention: Catalyst comprising a very high purity IZM-9 zeolite of AFX structural type and at least one transition metal for the selective reduction of NO X Technical field
[0001] The subject of the invention is a process for preparing a catalyst based on an IZM-9 zeolite of AFX structural type and at least one transition metal, the catalyst prepared or capable of being prepared by the process, and its use in a process for the selective catalytic reduction of NOx in the presence of a reducing agent, in particular on internal combustion engines. Prior art
[0002] Nitrogen oxide (NOx) emissions resulting from the combustion of fossil fuels are a major concern for society. Increasingly stringent standards are being implemented by government bodies to limit the impact of combustion emissions on the environment and health. For light vehicles in Europe under the Euro 6c regulation, NOx and particulate emissions must reach a very low level for all operating conditions. The new WLTC (Worldwide harmonized Light vehicles Test Cycle) driving cycle and the Real Driving Emissions (RDE) regulation associated with the conformity factors, require the development of a highly efficient pollution control system to achieve these objectives.Selective catalytic reduction, also known as SCR, appears to be an effective technology for removing nitrogen oxides from oxygen-rich exhaust gases typical of lean-burn diesel and spark-ignition engines. Selective catalytic reduction is achieved using a reductant, usually ammonia, and can therefore be referred to as NH3-SCR. The ammonia (NH3) involved in the SCR process is generally generated via the decomposition of an aqueous urea solution (AdBlue or DEF), and produces N2 and H2O upon reaction with NOx.
[0003] Zeolites exchanged with transition metals are used in particular as catalysts for NH3-SCR applications in transport. Small-pore zeolites, in particular copper-exchanged chabazites, are particularly suitable. They exist commercially in the form of silicoaluminophosphate Cu-SAPO-34 and aluminosilicates Cu-SSZ-13 (or Cu-SSZ-62). Their hydrothermal resistance and their NOx conversion efficiency make them the current references. However, as standards become increasingly stringent, the performance of catalysts must still be improved.
[0004] The use of AFX structural type zeolites for NH3-SCR applications is known, but few studies evaluate the effectiveness of catalysts using this zeolite.
[0005] Fickel et al. (Fickel, DW, & Lobo, RF (2009), The Journal of Physical Chemistry C, 114 (3), 1633-1640) investigated the use of a copper-exchanged SSZ-16 (AFX structural type) for NOx removal. This zeolite is synthesized according to US patent 5,194,235, in which copper is introduced by exchange using copper(II) sulfate at 80°C for 1 h. Recent results (Fickel, DW, D'Addio, E., Lauterbach, JA, & Lobo, RF (2011), 102(3), 441-448) show excellent conversion and good hydrothermal performance for a 3.78% wt. copper loading.
[0006] Work on the synthesis of AFX structural type zeolites has been carried out with different structural agents (Lobo, RF, Zones, SI, & Medrud, RC (1996), Chemistry of materials, 8 (10), 2409-2411) as well as work on the optimization of the synthesis (Hrabanek, P., Zikanova, A., Supinkova, T., Drahokoupil, J., Fila, V., Lhotka, M., Bemauer, B. (2016), Microporous and Mesoporous Materials, 228, 107-115).
[0007] Wang et al. (Wang, D. et al., CrystEngComm., (2016, 18 (6), 1000-1008) studied the replacement of the structuring agent TMHD by a TEA-TMA mixture for the formation of SAPO-56 and obtained unwanted phases SAPO-34 and SAPO-20. The incorporation of transition metals is not addressed.
[0008] Patent application US 2016 / 0137518 describes the synthesis of a quasi-pure AFX zeolite, in the presence of a structuring agent of the l,3-Bis(l-adamantyl)imidazolium hydroxide type, the preparation of a catalyst based on the AFX zeolite exchanged with a transition metal and its use for NH3-SCR applications. No particular form of AFX zeolite is mentioned.
[0009] More recently, patent application US 2018 / 0093259 presents the synthesis of small-pore zeolites, such as the AFX structural type zeolite, from a FAU type zeolite in the presence of a structuring agent, such as l,3-bis(l-adamantyl)imidazolium hydroxide and a source of alkaline earth metal. It also presents applications of the obtained AFX structural type zeolite, in particular the use of this zeolite as a catalyst for the reduction of NOx, after exchange with a metal such as iron. At the same time, application US 2016 / 0096169Al presents the use in the conversion of NOx, of a catalyst based on a zeolite of structural type AFX having a Si / Al ratio of between 15 and 50 exchanged with a transition metal, the AFX zeolite being obtained with the use of a structuring agent of type l,3-Bis(l-adamantyl)imidazolium hydroxide. The results obtained, in the conversion of NOx, show in particular a selectivity of the catalysts prepared according to patent applications US 2018 / 0093259 and US 2016 / 0096169 towards nitrous oxide not exceeding 20 ppm.
[0010] Document JP2014-148441 describes the synthesis of a solid related to an AFX zeolite, in particular a SAPO-56 comprising copper usable for the reduction of NOX. The solid is synthesized, then added to a mixture comprising an alcohol and a copper salt, the whole being then calcined. The copper is therefore added after the formation of the SAPO solid related to the AFX structural type zeolite. This exchanged solid appears to have increased stability in the presence of water.
[0011] Ogura et al. (Bull. Chem. Soc. Jpn. 2018, 91, 355-361) show the very good activity of a copper-exchanged SSZ-16 type zeolite compared to other zeolite structures, even after hydrothermal aging.
[0012] Patent application WO2017 / 080722 presents a direct synthesis of a zeolite comprising copper. This synthesis requires starting from a zeolite of structural type FAU and using a complexing agent TEPA and an element M(OH)X to obtain different types of zeolites, mainly of the CHA type. Zeolites of the ANA, ABW, PHI and GME types are also produced.
[0013] Patent applications WO2019 / 224081Al, WO2019 / 224082A1, WO2020 / 212354, WO2019 / 224086A1, WO2021 / 063704 describe catalysts based on a microporous aluminosilicon zeolite material of AFX structural type and a transition metal as well as the use of this material for the selective catalytic reduction of NOx. Summary of the invention
[0014] The applicant has discovered that a catalyst based on an IZM-9 zeolite of AFX structural type prepared according to a particular synthesis method using in particular a mixture of specific organic structuring agents, and at least one transition metal, in particular iron, cerium or copper, exhibited interesting NOX conversion performance and selectivity towards N2O. The NOx conversion performance is improved. In particular, the catalyst prepared according to the invention makes it possible to obtain lower initiation temperatures than those obtained with catalysts of the prior art, such as catalysts based on AFX structural type zeolite synthesized with a single structuring agent, exchanged with copper, while retaining good selectivity towards nitrous oxide N2O.
[0015] The invention relates to a process for preparing a catalyst based on IZM-9 zeolite of AFX structural type exchanged with at least one transition metal comprising at least the following steps: i) the mixture in an aqueous medium of at least one source of silicon (Si) in the form oxide SiO2, at least one source of aluminum (Al) in oxide form A12O3, an organic nitrogen compound RI, and a second organic nitrogen compound R2, at least one source of sodium, the reaction mixture having the following molar composition: SiO2 / Al2O3 between 6.00 and 200, preferably between 6.00 and 100 H2O / SiO2 between 1.00 and 100, preferably between 5 and 60 Rl / SiO2 between 0.01 and 0.60, preferably between 0.015 and 0.50 R2 / SiO2 between 0.01 and 0.60, preferably between 0.05 and 0.50 M2 / nO / SiO2 between 0.005 and 0.45, preferably between 0.05 and 0.25, RI being chosen from the organic compounds tetraethylammonium or tetrapropylammonium, preferably RI is tetraethylammonium and R2 being chosen from the organic compounds l,6-bis(methylpiperidinium)hexane l,5-bis(methylpiperidinium)pentane, or l,7-bis(methylpiperidinium)heptane, preferably R2 is l,6-bis(methylpiperidinium)hexane, the organic compounds RI and R2 being introduced in hydroxide form, until a homogeneous precursor gel is obtained; ii) The curing of the precursor gel of said step i) at a temperature between 20 and 40°C with or without stirring, for a period between 10 minutes and 72 hours, preferably between 5 hours and 48 hours and more preferably between 18 and 24 hours; iii) The addition of FAU structural type zeolite powder having a SiO2 (FAU) / A12O3 (FAU) ratio of between 5.2 and 75 to the gel resulting from step ii), the quantity of silicon SiO2 (FAU) provided by said FAU zeolite representing between 1 and 25%, preferably between 1.5 and 10% by weight of the total quantity of SiO2 in the gel; iv) Maturing the gel containing the FAU zeolite powder obtained in step iii) with stirring at a temperature of between 20 and 40°C for a period of 1 hour to 12 hours, preferably 1 hour to 8 hours and more preferably 1 hour to 3 hours, to obtain a homogeneous precursor gel; v) hydrothermal treatment of said homogeneous precursor gel at a temperature of between 110°C and 220°C for a period of between 5 hours and 10 days, preferably under autogenous reaction pressure, until said IZM-9 zeolite of AFX structural type is formed, said solid phase formed from a zeolite of AFX structural type being filtered, washed and then dried at the end of the hydrothermal treatment; vi) at least one ion exchange comprising bringing said solid obtained at the end of the previous step into contact with a solution comprising at least one species capable of releasing a transition metal, in solution in reactive form with stirring at room temperature for a period of between 1 hour and 2 days, said transition metal released in the exchange solution of step vi) being selected from the group formed from the following elements: Ti, V, Mn, Mo, Fe, Co, Cu, Cr, Zn, Nb, Ce, Zr, Rh, Pd, Pt, Au, W, Ag, preferably from the group formed from the following elements: Fe, Cu, Nb, Ce or Mn, more preferably from Fe, Ce or Cu, alone or in a mixture and even more preferably said transition metal is Cu;
[0016] vii) heat treatment by drying the solid obtained at the end of the previous step at a temperature between 20 and 150°C followed by at least one calcination under air flow at a temperature between 400 and 700°C.
[0017] Steps vi) and vii) may be reversed, and one or both of them may be repeated.
[0018] The precursor gel obtained at the end of step iii) may have a SiO2 / Al2O3 ratio of between 20 and 80, preferably between 25 and 70.
[0019] In step vi) an ion exchange can be carried out by bringing the solid obtained at the end of step v) into contact with an acid or a compound such as ammonium chloride, sulfate or nitrate, before the ion exchange with the transition metal(s), to obtain the protonated form of the IZM-9 zeolite.
[0020] The content of transition metal(s) introduced by the ion exchange step vi) may be between 0.5 and 6% by mass, preferably between 0.5 and 5% by mass, more preferably between 1 and 4% by mass, relative to the total mass of the final anhydrous catalyst.
[0021] Step vi) of heat treatment may comprise drying the solid at a temperature of between 60 and 100°C for a period of between 2 and 24 hours, followed by at least one calcination in air, optionally dry, at a temperature of between 450 and 700°C, preferably between 500 and 600°C, for a period of between 2 and 20 hours, preferably between 5 and 10 hours, more preferably between 6 and 9 hours, the flow rate of optionally dry air preferably being between 0.5 and 1.5 L / h / g of solid to be treated, more preferably between 0.7 and 1.2 L / h / g of solid to be treated.
[0022] The invention also relates to a catalyst based on IZM-9 zeolite of AFX structural type with a SiO2 / Al2O3 molar ratio as determined by X-ray fluorescence of between 6 and 14, comprising at least one transition metal, preferably iron, cerium or copper, very preferably iron or copper, at a content of between 0.5 and 6% by mass relative to the total mass of the catalyst in its anhydrous form, obtained or capable of being obtained by the preparation process according to any one of the variants described.
[0023] The invention also relates to a process for the selective reduction of NOX in a gaseous mixture by a reducing agent such as NH3 or H2 by bringing said gaseous mixture into contact with said catalyst.
[0024] The catalyst can be shaped by deposition in the form of a coating, on a honeycomb structure or a plate structure.
[0025] The honeycomb structure may be formed of parallel channels open at both ends or may comprise porous filtering walls for which the adjacent parallel channels are alternately blocked on either side of the channels.
[0026] The quantity of catalyst deposited on said structure can be between 50 and 180 g / L for filter structures and between 80 and 200 g / L for structures with open channels.
[0027] The catalyst may be combined with a binder such as ceria, zirconium oxide, alumina, non-zeolitic silica-alumina, titanium oxide, a mixed oxide of the ceria-zirconia type, a tungsten oxide and / or a spinel to be shaped by deposition in the form of a coating.
[0028] Said coating may be associated with another coating having NOx adsorption capacities, NOx reduction capacities or promoting the oxidation of ammonia.
[0029] Said catalyst may be in extruded form, containing up to 100% of said catalyst.
[0030] The structure coated with said catalyst or obtained by extrusion of said catalyst can be integrated into an exhaust line of an internal combustion engine. LIST OF FIGURES
[0031] Other characteristics and advantages of the process for preparing the catalyst according to the invention will appear on reading the following description of non-limiting examples of embodiments, with reference to the appended figures described below. [Fig 1]
[0032] [Fig. 1] represents the X-ray diffraction diagram of the IZM-9 zeolite of AFX structural type obtained according to example 2. [Fig 2]
[0033] [Fig.2] represents the Scanning Electron Microscope (SEM) image of the IZM-9 zeolite obtained according to example 2. [Fig 3]
[0034] [Fig.3] represents the conversion C in % obtained during a catalytic test for the reduction of nitrogen oxides (NOx) by ammonia (NH3) in the presence of oxygen (O2) under Standard SCR conditions as a function of the temperature T in °C for the catalysts synthesized according to example 2 (CuIZM-9, according to the invention, curve symbolized by circles) and example 4 (CuAFX, comparative, curve symbolized by crosses). [Fig 4]
[0035] [Fig.4] represents the conversion C in % obtained during a catalytic test for the reduction of nitrogen oxides (NOx) by ammonia (NH3) in the presence of oxygen (O2 ) under Standard SCR conditions as a function of temperature T in °C for the catalysts synthesized according to example 3 (FeIZM-9, according to the invention, curve symbolized by circles) and example 5 (FeAFX, comparative, curve symbolized by crosses). Description of the embodiments
[0036] The present invention relates to a process for preparing a catalyst comprising an IZM-9 zeolite of AFX structural type and at least one transition metal, comprising at least the following steps:
[0037] i) mixture in aqueous medium of at least one source of aluminum in oxide form A12O3, of at least one source of silicon in oxide form SiO2, of an organic nitrogen compound RI, RI being chosen from tetraethylammonium or tetrapropylammonium, and of a second organic nitrogen compound R2, R2 being chosen from 1,5-bis(methylpiperidinium)pentane, 1,6-bis(methylpiperidinium)hexane or 1,7-bis(methylpiperidinium)heptane, of at least one source of sodium, the reaction mixture having the following molar composition: SiO2 / Al2O3 between 6.00 and 200, preferably between 6.00 and 100 H2O / SiO2 between 1.00 and 100, preferably between 5 and 60 Rl / SiO2 between 0.01 and 0.60, preferably between 0.015 and 0.50 R2 / SiO2 between 0.01 and 0.60, preferably between 0.05 and 0.50 M2 / nO / SiO2 between 0.005 and 0.45, preferably between 0.05 and 0.25, in which, SiO2 is the molar quantity expressed in the form of SiO2 oxide provided by the silicon source, A12O3 is the molar quantity expressed in the form of Al2O3 oxide provided by the aluminum source, H2O is the molar quantity of water present in the reaction mixture, RI is the molar quantity of the first nitrogen compound, and R2 is the molar quantity of the second nitrogen compound, Na2O is the molar quantity of sodium expressed as sodium oxide, step i) being carried out for a period of between 5 and 20 minutes until a homogeneous mixture called precursor gel is obtained; ii) The curing of the precursor gel of said step i) at a temperature of between 20 and 40°C, with or without stirring, for a period of between 10 minutes and 72 hours, preferably between 5 hours and 48 hours and more preferably between 18 and 24 hours; iii) The addition of dealuminated faujasite powder to the gel from step ii) with a SiO2 (FAU) / A12O3 (FAU) ratio of between 5.2 and 75, the quantity of silicon SiO2 (FAU) provided by the powder representing between 1 and 25%, preferably between 1.5 and 10% by weight of the total quantity of SiO2 in the gel; iv) The ripening of the gel containing the faujasite zeolite powder obtained in step iii) with stirring at a temperature between 20 and 40°C for a period of 1 hour to 12 hours, preferably 1 hour to 8 hours and more preferably 1 hour to 3 hours, v) Hydrothermal treatment of the mixture obtained at the end of step iv) at a temperature between 110°C and 220°C, preferably between 115°C and 170°C, for a period between 5 hours and 10 days, preferably between 16 hours and 7 days and more preferably between 16 hours and 5 days to obtain a crystallized solid phase, called “solid”; vi) at least one ion exchange comprising bringing said solid obtained at the end of the previous step into contact with a solution comprising at least one species capable of releasing a transition metal, in particular copper, in solution in reactive form with stirring at room temperature for a period of between 1 hour and 2 days; vii) heat treatment by drying the solid obtained at the end of the previous step at a temperature between 20 and 150°C followed by at least one calcination under air flow at a temperature between 400 and 700°C for a period between 8 and 24 hours.
[0038] Steps vi) and vii) may be reversed, and possibly repeated if necessary.
[0039] The present invention also relates to the catalyst comprising an IZM-9 zeolite of AFX structural type and at least one transition metal capable of being obtained or directly obtained by the method described above.
[0040] The invention finally relates to the use of a catalyst according to the invention for the selective catalytic reduction of NOx in the presence of a reducing agent. The catalyst
[0041] The catalyst according to the invention comprises at least one IZM-9 zeolite of AFX type of very high purity, and at least one additional transition metal, preferably copper.
[0042] According to the invention, the transition metal or metals included in the catalyst is (are) selected from the elements from the group formed by the elements of groups 3 to 12 of the periodic table of elements including the lanthanides.
[0043] In particular, the transition metal or metals included in the catalyst is (are) selected from the group formed by the following elements: Ti, V, Mn, Mo, Fe, Co, Cu, Cr, Zn, Nb, Ce, Zr, Rh, Pd, Pt, Au, W, Ag, preferably from the group formed by the following elements: Fe, Cu, Nb, Ce or Mn, more preferably from Fe, Ce or Cu alone or in a mixture, and even more preferably said transition metal is Cu.
[0044] For the catalysts according to the invention, the transition metal content is between 0.5 and 6% by mass, preferably between 0.5 and 5% by mass, more preferably between 1 and 4% relative to the total mass of the final anhydrous catalyst.
[0045] The catalyst according to the invention may also comprise other elements, such as for example alkali and / or alkaline earth metals, for example sodium, originating in particular from the synthesis, in particular of the compounds of the reaction medium of step i) of the process for preparing said catalyst. Process for preparing the catalyst Step i) of mixing
[0046] Step i) implements: i) the mixture in aqueous medium of at least one source of aluminum A12O3, at least one source of silicon SiO2, an organic nitrogen compound RI, and a second organic nitrogen compound R2, of at least one source of sodium, the reaction mixture having the following molar composition: SiO2 / Al2O3 between 6.00 and 200, preferably between 6.00 and 100 H2O / SiO2 between 1.00 and 100, preferably between 5 and 60 Rl / SiO2 between 0.01 and 0.60, preferably between 0.015 and 0.50 R2 / SiO2 between 0.01 and 0.60, preferably between 0.05 and 0.50 M2 / nO / SiO2 between 0.005 and 0.45, preferably between 0.05 and 0.25,
[0047] According to the invention, RI is chosen from the organic compounds tetraethylammonium or tetrapropylammonium, preferably RI is tetraethylammonium and R2 is chosen from the organic compounds 1,6-bis(methylpiperidinium)hexane 1,5-bis(methylpiperidinium)pentane, or 1,7-bis(methylpiperidinium)heptane, preferably R2 is l,6-bis(methylpiperidinium)hexane, said compounds being incorporated into the reaction mixture for the implementation of step (i), as organic structuring agents, in their hydroxide form. The anion associated with the quaternary ammonium cations present in the structuring organic species for the synthesis of an IZM-9 zeolite of AFX structural type according to the invention is thus the hydroxide anion, which makes it possible to direct the synthesis towards a zeolite of AFX structural type of very high purity.
[0048] According to the invention, the sodium source is preferably sodium hydroxide.
[0049] According to the invention, the source of silica SiO2, may be any of the said sources commonly used for the synthesis of zeolites, for example powdered silica, silicic acid, colloidal silica, dissolved silica or tetraethoxysilane (TEOS). Among the powdered silicas, precipitated silicas may be used, in particular those obtained by precipitation from an alkali metal silicate solution, pyrogenic silicas, for example "CAB-O-SIL®" and gels of silica. Colloidal silicas with different particle sizes, for example with an average equivalent diameter of between 10 and 15 nm or between 40 and 50 nm, such as those marketed under registered trademarks such as "LUDOX®", can be used. Preferably, the source of silicon is Ludox AS-40.
[0050] According to the invention, the source of aluminum A12O3 is preferably an aluminum salt, for example chloride, nitrate, or sulfate, aluminum hydroxide, an aluminum alkoxide, or alumina itself, preferably in hydrated or hydratable form, such as colloidal alumina, pseudo-boehmite, gamma alumina or alpha or beta trihydrate. Mixtures of the sources cited above can also be used.
[0051] According to the invention, the zeolite powder of structural type FAU with a SiO2 / Al2O3 ratio of between 5.2 and 75, preferably a dealuminated zeolite of structural type FAU, which is added to the precursor gel, plays the role of crystalline seeds which promote the formation of said IZM-9 zeolite to the detriment of impurities.
[0052] Step (i) of the process according to the invention consists in preparing an aqueous reaction mixture containing a source of SiO2, at least one source of Al2O3, at least one organic nitrogen compound RI, at least one second organic nitrogen compound R2, in the presence of at least one source of sodium, to obtain a precursor gel of an IZM-9 zeolite of AFX structural type. The quantities of said reagents are adjusted according to the proportions previously described so as to give this gel a composition allowing the crystallization of an IZM-9 zeolite of AFX structural type.
[0053] Step i) of mixing is carried out until a homogeneous mixture is obtained, preferably for a period greater than or equal to 15 minutes, very preferably of the order of 30 minutes, preferably with stirring by any system known to those skilled in the art with low or high shear rate.
[0054] At the end of step i), a homogeneous precursor gel is obtained. Step ii) of ripening
[0055] The ripening of the precursor gel of said step i) at a temperature between 20 and 40°C with or without stirring, for a period between 10 minutes and 72 hours, preferably between 5 hours and 48 hours and more preferably between 18 and 24 hours. Step iii) addition of faujasite powder
[0056] The addition of dealuminated faujasite powder to the gel resulting from step ii) with a SiO2 (FAU) / A12O3 (FAU) ratio of between 5.2 and 75, the quantity of silicon SiO2 (FAU) provided by the powder representing between 1 and 25%, preferably between 1.5 and 10%, by weight of the total quantity of SiO2 in the gel. Step iv) of ripening
[0057] The maturing of the gel containing the faujasite powder obtained in step iii) is carried out, with stirring, for example magnetic, at a temperature between 20 and 40°C for a period of 1 hour to 12 hours, preferably 1 hour to 8 hours and more preferably 1 hour to 3 hours.
[0058] At the end of step iv), a homogeneous precursor gel is obtained. Step v) of hydrothermal treatment
[0059] In accordance with step v) of the process according to the invention, the precursor gel obtained at the end of step iv) is subjected to a hydrothermal treatment, at a temperature of between 110°C and 220°C for a period of between 5 hours and 10 days, until said IZM-9 zeolite of AFX structural type (or “crystalline solid”) is formed.
[0060] The precursor gel can advantageously be placed under hydrothermal conditions under autogenous reaction pressure, optionally by adding gas, for example nitrogen, at a temperature between 110°C and 220°C, preferably between 115°C and 170°C, until complete crystallization of a zeolite of AFX structural type.
[0061] The time required to obtain crystallization varies between 5 hours and 10 days, preferably between 16 hours and 7 days, and more preferably between 16 hours and 5 days.
[0062] The reaction is generally carried out with stirring or without stirring, preferably with stirring. As stirring system, any system known to those skilled in the art can be used, for example, inclined blades with counterblades, stirring turbines, Archimedes screws.
[0063] Very advantageously, the process of the invention leads to the formation of an IZM-9 zeolite of AFX structural type, free from any other crystallized or amorphous phase. The purity of the IZM-9 zeolite obtained is advantageously greater than or equal to 95% by weight, preferably greater than or equal to 98% by weight, very preferably greater than or equal to 99% by weight.
[0064] The SiO2 / Al2O3 molar ratio of the IZM-9 zeolite of AFX structural type obtained is advantageously between 6 and 14, preferably between 7 and 12. Step vi) exchange
[0065] The process for preparing the catalyst according to the invention comprises at least one ion exchange step comprising bringing the crystallized solid obtained at the end of the previous step (i.e. the IZM-9 zeolite of AFX structural type obtained at the end of step v) or the dried and calcined IZM-9 zeolite obtained at the end of step vii) in the preferred case where steps v) and vii) are reversed) into contact with at least one solution comprising at least one species capable of releasing a metal from transition, preferably copper, in solution in reactive form, with stirring at room temperature for a period of between 1 hour and 2 days, advantageously for a period of between 0.5 days and 1.5 days, the concentration of said species capable of releasing the transition metal in said solution being a function of the quantity of transition metal that it is desired to incorporate into said crystallized solid.
[0066] It is also advantageous to obtain the protonated form of the IZM-9 zeolite of structural type AFX after step v). Said hydrogen form can be obtained by carrying out an ion exchange with an acid, in particular a strong mineral acid such as hydrochloric, sulfuric or nitric acid, or with a compound such as ammonium chloride, sulfate or nitrate, before the ion exchange with the transition metal(s).
[0067] The transition metal released into the exchange solution is selected from the group consisting of the following elements: Ti, V, Mn, Mo, Fe, Co, Cu, Cr, Zn, Nb, Ce, Zr, Rh, Pd, Pt, Au, W, Ag. Preferably, the transition metal may be Fe, Cu, Nb, Ce or Mn, more preferably chosen from Fe, Ce or Cu alone or in a mixture, and even more preferably said transition metal is Cu.
[0068] According to the invention, by "species capable of releasing a transition metal" is meant a species capable of dissociating in an aqueous medium, such as for example sulfates, nitrates, chlorides, oxalates, organometallic complexes of a transition metal or their mixtures. Preferably, the species capable of releasing a transition metal is a sulfate or a nitrate of said transition metal.
[0069] According to the invention, the solution with which the crystallized solid or dried and calcined crystallized solid is brought into contact, comprises at least one species capable of releasing a transition metal, preferably a single species capable of releasing a transition metal, preferably iron or copper or cerium, preferentially copper.
[0070] Advantageously, the process for preparing the catalyst according to the invention may comprise a step vi) of ion exchanges by bringing the crystallized solid into contact with a solution comprising a species capable of releasing a transition metal or by successively bringing the solid into contact with several solutions each comprising a species capable of releasing a transition metal, the different solutions comprising different species capable of releasing a transition metal.
[0071] At the end of the exchange, the solid obtained can advantageously be filtered, washed and then dried to obtain said catalyst in powder form.
[0072] The total quantity of transition metal, preferably iron, copper, or cerium contained in said final catalyst is between 0.5 and 6% by mass relative to the total mass of the catalyst in its anhydrous form.
[0073] According to one embodiment, the catalyst according to the invention can be prepared by a process comprising a step vi) of ion exchange, the solid or the dried solid and calcined being brought into contact with a solution comprising a species capable of releasing copper in solution in reactive form. Advantageously, the total quantity of copper contained in said final catalyst, i.e. at the end of the preparation process according to the invention, may be between 0.5 and 6% by mass, preferably between 1 and 6% by mass, all percentages being percentages by mass relative to the total mass of the final catalyst according to the invention in its anhydrous form, obtained at the end of the preparation process. Step vii) heat treatment
[0074] The preparation process according to the invention comprises a step vii) of heat treatment carried out at the end of step v) of hydrothermal treatment and / or at the end of step vi) of ion exchange. Step vi) of the preparation process can advantageously be interchanged with step vii). Each of the two steps vi) and vii) can also optionally be repeated.
[0075] Said step vii) of heat treatment comprises drying the solid at a temperature of between 20 and 150°C, preferably between 60 and 100°C, advantageously for a period of between 2 and 24 hours, followed by at least one calcination, in air, optionally dry, at a temperature advantageously of between 450 and 700°C, preferably between 500 and 600°C for a period of between 2 and 20 hours, preferably between 5 and 10 hours, more preferably between 6 and 9 hours, the flow rate of optionally dry air being preferably of between 0.5 and 1.5 L / h / g of solid to be treated, more preferably of between 0.7 and 1.2 L / h / g of solid to be treated. The calcination may be preceded by a gradual rise in temperature.
[0076] The catalyst obtained at the end of step vii) of heat treatment is free of any organic species, in particular free of the two organic structuring agents RI and R2.
[0077] In particular, the catalyst based on IZM-9 zeolite and at least one transition metal obtained by a process comprising at least steps i), ii), iii), iv), v), vi) and vii) previously described has improved properties for the conversion of NOX.
[0078] Characterization of the catalyst prepared according to the invention
[0079] The catalyst comprises an IZM-9 zeolite of AFX structural type according to the classification of the International Zeolite Association (IZA), exchanged by at least one transition metal. This structure is characterized by X-ray diffraction (XRD).
[0080] The X-ray diffraction pattern (XRD) is obtained by radiocrystal-lographic analysis using a diffractometer using the classical powder method with Ka radiation, of copper (X = 1.5406Â). From the position of the diffraction peaks represented by the angle 20, the Bragg relation calculates the reticular equidistances dhki characteristic of the sample. The measurement error A(d hki) on dhki is calculated using the Bragg relation as a function of the absolute error A(20) assigned to the measurement of 20. An absolute error A(20) equal to ± 0.02° is commonly accepted. The relative intensity Irei assigned to each value of d^i is measured according to the height of the corresponding diffraction peak. Comparing the diffractogram with the records in the ICDD (International Centre for Diffraction Data) database using software such as DIFFRACT.SUITE also allows us to identify the crystalline phases present in the material obtained.
[0081] A pure AFX structural type IZM-9 zeolite is used as a reference.
[0082] The qualitative and quantitative analysis of the chemical species present in the materials obtained is carried out by X-ray fluorescence spectrometry (FX). This is a chemical analysis technique using a physical property of matter, X-ray fluorescence. The spectrum of X-rays emitted by the matter is characteristic of the composition of the sample; by analyzing this spectrum, the elemental composition, i.e. the mass concentrations of elements, can be deduced.
[0083] The loss on ignition (LAI) of the catalyst obtained after the drying step (and before calcination) or after the calcination step of step vii) of the process according to the invention is generally between 4 and 15% by weight. The loss on ignition of a sample, designated by the acronym LAI, corresponds to the difference in mass of the sample before and after a heat treatment at 1000°C for 2 hours. It is expressed in % corresponding to the percentage loss of mass. The loss on ignition generally corresponds to the loss of solvent (such as water) contained in the solid, but also to the elimination of organic compounds contained in the mineral solid constituents.
[0084] Advantageously, the catalyst according to the invention comprises an IZM-9 zeolite of AFX structural type with a purity greater than 95%, preferably greater than 98%, even more preferably greater than 99% by weight.
[0085] The catalyst according to the invention advantageously has a SiO2 / Al 2O3 molar ratio as determined by X-ray fluorescence of between 6 and 14. Use of the catalyst according to the invention
[0086] The invention also relates to the use of the catalyst according to the invention, directly prepared or capable of being prepared by the process described above for the selective reduction of NOX in a gas mixture containing NOX, for example of the exhaust gas type of an internal combustion engine, by a reducing agent such as NH3 or H2, advantageously formed by deposition in the form of a coating ("washcoat" according to the English terminology) on a honeycomb structure mainly for mobile applications or a plate structure that found particularly for stationary applications.
[0087] The honeycomb structure is formed of parallel channels open at both ends (flow-through in English) or comprises porous filtering walls and in this case the adjacent parallel channels are alternately blocked on either side of the channels in order to force the gas flow to pass through the wall (wall-flow monolith in English). Said honeycomb structure thus coated constitutes a catalytic bread. Said structure can be composed of cordierite, silicon carbide (SiC), aluminum titanate (AITi), alpha alumina, mullite or any other material whose porosity is between 30 and 70%. Said structure can be made of metal sheet, stainless steel containing chromium and aluminum, FeCrAl type steel.
[0088] The quantity of catalyst according to the invention deposited on said structure can be between 50 and 180 g / L for filtering structures and between 80 and 200 g / L for structures with open channels.
[0089] The coating itself ("washcoat") comprises the catalyst according to the invention, advantageously combined with a binder such as ceria, zirconium oxide, alumina, non-zeolitic silica-alumina, titanium oxide, a mixed oxide of ceria-zirconia type, a tungsten oxide, a spinel. Said coating is advantageously applied to said structure by a deposition method (washcoating in English) which consists of dipping the monolith in a suspension (slurry in English) of catalyst powder according to the invention in a solvent, preferably water, and potentially binders, metal oxides, stabilizers or other promoters. This dipping step can be repeated until the desired quantity of coating is reached. In certain cases the slurry can also be sprayed within the monolith. Once the coating is deposited, the monolith is calcined at a temperature of 300 to 600°C for 1 to 10 hours.
[0090] Said structure may be coated with one or more coatings. The coating comprising the catalyst according to the invention is advantageously associated with, i.e. covers one or is covered by, another coating having capacities for adsorbing pollutants, in particular NOx, for reducing pollutants, in particular NOx, or promoting the oxidation of pollutants, in particular that of ammonia.
[0091] Another possibility is to put the catalyst in extruded form. In this case, the structure obtained can contain up to 100% of catalyst according to the invention.
[0092] Said structure coated with the catalyst according to the invention is advantageously integrated into an exhaust line of an internal combustion engine operating mainly in a lean mixture, that is to say in excess air compared to the stoichiometry of the combustion reaction as is the case for Diesel engines for example. Under these engine operating conditions, the gases exhaust gases contain in particular the following pollutants: soot, unburned hydrocarbons (HC), carbon monoxide (CO), nitrogen oxides (NOx). Upstream of said structure coated with the catalyst according to the invention can be placed an oxidation catalyst whose function is to oxidize the HC and CO as well as a filter to remove the soot from the exhaust gases, the function of said coated structure being to remove the NOx, its operating range being between 100 and 900°C and preferably between 150°C and 500°C. ADVANTAGES OF THE INVENTION
[0093] The catalyst according to the invention, based on an IZM-9 zeolite of AFX structural type and at least one transition metal, in particular copper, iron or cerium, exhibits a notable gain in initiation temperature (usually referred to as "light-off") compared to catalysts prepared based on a zeolite of AFX structure synthesized with a single organic molecule. In particular, the use of the catalyst according to the invention makes it possible to obtain lower initiation temperatures for the NOx conversion reaction and better NOX conversion over the entire operating temperature range (150°C - 500°C), while maintaining good N2O selectivity. EXAMPLES
[0094] Example 1; preparation of 1,6-bis(methylpiperidinium)hexane dihydroxide (structuring agent R2).
[0095] 50 g of 1,6-dibromohexane (0.20 mol, 99%, Alfa Aesar) are added to a flask of 1 L containing 50 g of N-methylpiperidine (0.51 mol, 99%, Alfa Aesar) and 200 mL of ethanol. The reaction medium is stirred and refluxed for 5 hours. The mixture is then cooled to room temperature and filtered. The mixture is poured into 300 mL of cold diethyl ether, then the precipitate formed is filtered and washed with 100 mL of diethyl ether. The solid obtained is recrystallized from an ethanol / ether mixture. The solid obtained is dried under vacuum for 12 hours. 71 g of a white solid is obtained (i.e. a yield of 80%).
[0096] The product has the expected 'H NMR spectrum. 'H NMR (D2O, ppm / TMS): 1.27
[0097] (4H,m); 1.48 (4H,m); 1.61 (4H,m); 1.70 (8H,m); 2.85 (6H,s); 3.16 (12H,m).
[0098] 18.9 g of Ag2O (0.08 mole, 99%, Aldrich) are added to a Teflon beaker of 250 mL containing 30 g of the prepared structuring agent l,6-bis(methylpiperidinium)hexane dibromide (0.07 mol) and 100 mL of deionized water. The reaction medium is stirred away from light for 12 hours. The mixture is then filtered. The filtrate obtained is composed of an aqueous solution of l,6-bis(methylpiperidinium)hexane dihydroxide. The determination of this species is carried out by proton NMR using formic acid as a standard.
[0099] Example 2: preparation of a 1ZM-9 zeolite of AFX structural type according to the invention 3% Cu
[0100] Preparation of IZM-9 zeolite of AFX structural type
[0101] 46.75 g of TEAOH (35% by weight, Sigma-Aldrich) was mixed with 442.31 g of an aqueous solution of 1,6-bis(methylpiperidinium)hexane dihydroxide (MPC6) (21.85% by weight) prepared according to Example 1. The preparation obtained is kept stirring for 10 minutes. 23.92 g of sodium hydroxide (98% by weight, Aldrich) are added to the previous mixture and kept stirring for 15 minutes. 4.56 g of sodium aluminate (53% by weight Al2O3, 42.32% by weight Na2O, Carlo Erba) are then added to the reaction medium and the preparation is kept stirring for 10 minutes. Subsequently, 229.34 g of Ludox® AS-40 (silica gel, Aldrich) is dripped into the beaker. The synthesis gel at this time has the following molar ratios: SiO2 / Al2O3 65.55 - H2O / SiO218.9 - TEAOH / SiO20.073 - MPC6OH / SiO2 0.2 - Na2O / SiO2 0.22
[0102] The molar composition of the precursor gel can be written in the following form: 1 SiO2: 0.015 A12O3: 0.073 TEAOH: 0.2 MPC60H: 0.22 Na2O: 18.9 H2O
[0103] The gel is then allowed to mature under stirring at a speed of 350 rpm for 23 hours at room temperature. After this period, 10 g of zeolite Y powder (CBV 720, Zeolyst®, SiO2 / Al2O3 = 32), i.e. a quantity of silicon SiO2(FAU) provided by the powder representing 10% by weight of the total quantity of SiO2 in the gel, are introduced into the reaction mixture. This then has the following molar ratios: - SiO2 / Al2O360 - H2O / SiO2 17.4 - TEAOH / SiO2 0.067 - MPC6OH / SiO2 0.18 - Na2O / SiO2 0.2
[0104] The molar composition of the precursor gel can then be written in the following form: 1 SiO2: 0.017 A12O3: 0.067 TEAOH: 0.18 MPC60H: 0.2 Na2O: 17.4 H2O
[0105] The ripening is continued and the synthesis gel containing the seeds is left stirring at a speed of 350 rpm for 1 hour at room temperature before being transferred to a 1 liter stainless steel reactor. The reactor is closed, then heated for 5 days at 130°C under autogenous pressure. The crystallized solid product obtained is filtered, washed with deionized water, then dried overnight at 100°C. The PAF of the solid dried is 15%.
[0106] The solid is then introduced into a muffle furnace where a calcination step is carried out: the calcination cycle includes a temperature rise of 1.5°C / min up to 200°C, a hold at 200°C maintained for 2 hours, a temperature rise of 1°C / min up to 550°C followed by a hold at 580°C maintained for 12 hours, then a return to room temperature.
[0107] The calcined solid product was analyzed by X-ray diffraction and identified as consisting of a zeolite of structural type AFX, with a purity greater than 99%. The diffraction pattern performed on this solid is given in [Fig.l]. The product has a SiO2 / Al2O3 molar ratio of 9.66 as determined by X-ray fluorescence. A Scanning Electron Microscope (SEM) image of the IZM-9 zeolite is given in [Fig.2].
[0108] Ion exchange with Cu
[0109] The calcined IZM-9 zeolite is brought into contact with a solution of [Cu(NH3)4](NO3 )2 for 1 day under stirring at room temperature. The ratio between the volume of [Cu(NH3)4](NO3)2 solution and the mass of solid is 30. The final solid is separated, washed and dried for 12 hours at 100°C.
[0110] The exchanged solid Cu-IZM-9 obtained after contact with the Cu(NH3)4](NO3)2 solution is calcined under air flow at 580°C for 8 hours.
[0111] The calcined solid product is analyzed by X-ray diffraction and identified as a zeolite of structural type AFX.
[0112] The product has a SiO2 / Al2O3 molar ratio of 9.7 and a mass percentage of Cu of 3% as determined by X-ray fluorescence.
[0113] The catalyst obtained is denoted CuIZM-9.
[0114] Example 3 preparation of an IZM-9 zeolite of AFX structural type according to the invention at 2.7% Fe
[0115] Preparation of IZM-9 zeolite of AFX structural type
[0116] 46.75 g of TEAOH (35% by weight, Sigma-Aldrich) was mixed with 442.31 g of an aqueous solution of l,6-bis(methylpiperidinium)hexane dihydroxide (MPC6) (21.85% by weight) prepared according to Example 1. The preparation obtained is kept stirring for 10 minutes. 23.92 g of sodium hydroxide (98% by weight, Aldrich) are added to the previous mixture and kept stirring for 15 minutes. 4.56 g of sodium aluminate (53% by weight Al2O3, 42.32% by weight Na2O, Carlo Erba) are then added to the reaction medium and the preparation is kept stirring for 10 minutes. Subsequently, 229.34 g of Ludox® AS-40 (silica gel, Aldrich) are added drop by drop into the beaker. The synthesis gel has at this time the following molar ratios: - SiO2 / Al2O3 65.55 - H2O / SiO218.9 - TEAOH / SiO2 0.073 - MPC6OH / SiO2 0.2 - Na2O / SiO2 0.22
[0117] The molar composition of the precursor gel can be written in the following form: 1 SiO2: 0.015 A12O3: 0.073 TEAOH: 0.2 MPC6OH: 0.22 Na2O: 18.9 H2O
[0118] The gel is then allowed to mature under stirring at a speed of 350 rpm for 23 hours at room temperature. After this period, 10 g of zeolite Y powder (CBV 720, Zeolyst®, SiO2Al2O3 = 32), i.e. a quantity of silicon SiO2(FAU) provided by the powder representing 10% by weight of the total quantity of SiO2 in the gel, are introduced into the reaction mixture. This then has the following molar ratios: - SiO2 / Al2O360 - H2O / SiO2 17.4 - TEAOH / SiO2 0.067 - MPC6OH / SiO2 0.18 - Na2O / SiO2 0.2
[0119] The molar composition of the precursor gel can then be written in the following form: 1 SiO2: 0.017 A12O3: 0.067 TEAOH: 0.18 MPC6OH: 0.2 Na2O: 17.4 H2O
[0120] The ripening is continued and the synthesis gel containing the powder is left stirring at a speed of 350 rpm for 1 hour at room temperature before being transferred to a 1 liter stainless steel reactor. The reactor is closed and then heated for 5 days at 130°C under autogenous pressure. The crystallized solid product obtained is filtered, washed with deionized water and then dried overnight at 100°C. The PAF of the dried solid is 15%.
[0121] The solid is then introduced into a muffle furnace where a calcination step is carried out: the calcination cycle includes a temperature rise of 1.5°C / min up to 200°C, a plateau at 200°C maintained for 2 hours, a temperature rise of 1°C / min up to 550°C followed by a plateau at 580°C maintained for 12 hours, then a return to room temperature.
[0122] The calcined solid product was analyzed by X-ray diffraction and identified as consisting of a zeolite of structural type AFX, with a purity greater than 99%. The product has a SiO2 / Al2O3 molar ratio of 9.66 as determined by X-ray fluorescence.
[0123] Ionic exchange with Fe
[0124] The calcined IZM-9 zeolite in protonated form is brought into contact with a solution of Fe(NO3)3 for 1 day under stirring at room temperature. The ratio between the volume of Fe(NO3)3 solution and the mass of solid is 200. The final solid is separated, washed and dried for 12 hours at 100°C.
[0125] The exchanged solid FeIZM-9 obtained after contact with the Fe(NO3)3 solution is calcined under air flow at 580°C for 8 hours.
[0126] The calcined solid product is analyzed by X-ray diffraction and identified as a zeolite of structural type AFX.
[0127] The product has a mass percentage of Fe of 2.7% as determined by X-ray fluorescence.
[0128] The catalyst obtained is noted FeIZM-9.
[0129] Example 4: In this example, a Cu-exchanged AFX structural type zeolite is synthesized according to the prior art. In this example, the zeolite was prepared with a single structuring agent (R2)
[0130] Preparation of the AFX structural type zeolite
[0131] 95.04 g of a zeolite of structural type FAU (CBV712, SiO2 / Al2O3= 11.47, Zeolyst, PAF = 12.81%) were mixed with 627.7 g of an aqueous solution of l,6-bis(methylpiperidinium)hexane dihydroxide (18.36% by weight) prepared according to Example 1. The resulting mixture is kept stirring for 10 minutes. 12.08 g of sodium hydroxide (98% by weight, Aldrich) and 27.7 g of deionized water are added to the synthesis mixture which is kept stirring for 10 minutes. Subsequently, 37.7 g of Cab-O-Sil M5 fumed silica (100% by weight SiO2, Cabot), are incorporated into the synthesis mixture which is kept stirring for one hour. The precursor gel obtained has the following molar composition: 1 SiO2: 0.05 Al2O3: 0.20 R: 0.083 Na2O: 17 H2O, i.e. a SiO2 / Al2O3 ratio of 20. The precursor gel is then transferred, after homogenization, into a 160 mL stainless steel reactor equipped with a four-blade inclined stirring system. The reactor is closed and then heated for 10 hours at 170°C with stirring at 250 - 300 rpm.The crystallized product obtained is filtered, washed with deionized water and then dried overnight at 100°C.
[0132] The solid is then introduced into a muffle furnace where a calcination step is carried out: the calcination cycle includes a temperature rise of 1.5°C / min up to 200°C, a plateau at 200°C maintained for 2 hours, a temperature rise of 1°C / min up to 550°C followed by a plateau at 550°C maintained for 12 hours and then a return to room temperature.
[0133] The calcined solid product was analyzed by X-ray diffraction and identified as consisting of a zeolite of structural type AFX, with a purity greater than 99%. The product has a SiO2 / Al2O3 molar ratio of 10.16 as determined by X-ray fluorescence
[0134] Ion exchange with Cu
[0135] The calcined AFX type zeolite is brought into contact with a solution of [Cu(NH3)4 ](NO3)2 for 1 day with stirring at room temperature. The final solid is separated, washed and dried and calcined under dry air flow at 550°C for 8 hours
[0136] Chemical analysis by X-ray fluorescence (FX) gave a SiO2 / Al2O3 molar ratio of 10.2 and a mass percentage of Cu of 2.9%.
[0137] The catalyst obtained is denoted CuAFX.
[0138] Example 5: In this example, a Fe-exchanged AFX structural type zeolite is synthesized according to the prior art. In this example, the zeolite was prepared with a single structuring agent (R2)
[0139] Preparation of the AFX structural type zeolite
[0140] 95.04 g of a zeolite of structural type FAU (CBV712, SiO2 / Al2O3= 11.47, Zeolyst, PAF = 12.81%) were mixed with 627.7 g of an aqueous solution of l,6-bis(methylpiperidinium)hexane dihydroxide (18.36% by weight) prepared according to Example 1. The resulting mixture is kept stirring for 10 minutes. 12.08 g of sodium hydroxide (98% by weight, Aldrich) and 27.7 g of deionized water are added to the synthesis mixture and kept stirring for 10 minutes. Subsequently, 37.7 g of Cab-O-Sil M5 fumed silica (100% by weight SiO2, Cabot), are incorporated into the synthesis mixture which is kept stirring for one hour. The precursor gel obtained has the following molar composition: 1 SiO2: 0.05 Al2O3: 0.20 R: 0.083 Na2O: 17 H2O, i.e. a SiO2 / Al2O3 ratio of 20. The precursor gel is then transferred, after homogenization, into a 160 mL stainless steel reactor equipped with a four-blade inclined stirring system. The reactor is closed, then heated for 10 hours at 170°C with stirring at 250 - 300 rpm.The crystallized product obtained is filtered, washed with deionized water and then dried overnight at 100°C.
[0141] The solid is then introduced into a muffle furnace where a calcination step is carried out: the calcination cycle includes a temperature rise of 1.5°C / min up to 200°C, a plateau at 200°C maintained for 2 hours, a temperature rise of 1°C / min up to 550°C followed by a plateau at 550°C maintained for 12 hours and then a return to room temperature.
[0142] The calcined solid product was analyzed by X-ray diffraction and identified as consisting of a zeolite of the AFX structural type, with a purity greater than 99%. The product has a SiO2 / Al2O3 molar ratio of 10.16 as determined by X-ray fluorescence.
[0143] Ionic exchange with Fe
[0144] The calcined AFX structural type zeolite in protonated form is brought into contact with a Fe(NO3)3 solution for 1 day under stirring at room temperature. The ratio between the volume of Fe(NO3)3 solution and the mass of solid is 200. The final solid is separated, washed and dried for 12 hours at 100°C.
[0145] The exchanged solid FeAFX obtained after contact with the Fe(NO3)3 solution is calcined under air flow at 580°C for 8 hours.
[0146] The calcined solid product is analyzed by X-ray diffraction and identified as a zeolite of structural type AFX.
[0147] The product has a mass percentage of Fe of 3.1% as determined by X-ray fluorescence.
[0148] The catalyst obtained is noted FeAFX.
[0149] Example 6: Conversion of NOx to Standard SCR: comparison of copper catalysts according to the invention with the prior art
[0150] A catalytic test for the reduction of nitrogen oxides (NOx) by ammonia (NH3) in the presence of oxygen (O2) under Standard SCR conditions is carried out at different operating temperatures for the catalysts synthesized according to Example 2 (CuIZM-9), and Example 4 (CuAFX).
[0151] For the test of each sample, 200 mg of catalyst in powder form is placed in a quartz reactor. 145 L / h of a load representative of a mixture of exhaust gases from a diesel engine are fed into the reactor.
[0152] This charge has the following molar composition: 400 ppm NO, 400 ppm NH3, 8.5% O2, 9% CO2, 10% H2O, qpc N2.
[0153] An FTIR analyzer allows the concentration of NO, NO2, NH3, N2O, CO, CO2, H2O, O2 species to be measured at the reactor outlet. The NOx conversions are calculated as follows:
[0154] Conversion = (NOx input -NOx output) / NOx input
[0155] The NOx conversion results are shown in [Fig. 3], the curves marked by circles and crosses corresponding respectively to the tests carried out with the catalysts synthesized according to Example 2 according to the invention (CuIZM-9) and Example 4 according to the prior art (CuAFX). The catalyst according to the invention offers an optimized initiation temperature and therefore makes it possible to convert NOx at a lower temperature than the catalyst synthesized according to the prior art.
[0156] The CuIZM-9 catalyst synthesized according to the invention is particularly effective at low temperatures with 70% NOx conversion at 170°C whereas the CuAFX catalyst only offers 55% NOx conversion at this same temperature.
[0157] The CuIZM-9 catalyst offers a maintained efficiency greater than 95% from 210 to 420°C.
[0158] The initiation temperatures of catalysts containing 3% copper are given below for Standard-SCR conditions:
[0159] [Tables 1] T50 T80 T90 T100 CuIZM-9 161°C 181°C 198°C 260°C CuAFX 169°C 194°C 209°C 270°C
[0160] T50 corresponds to the temperature at which 50% of the NOx in the gas mixture are converted by the catalyst. T80 corresponds to the temperature at which 80% of the NOx in the gas mixture is converted by the catalyst. T90 corresponds to the temperature at which 90% of the NOx in the gas mixture is converted by the catalyst. T100 corresponds to the temperature at which 100% of the NOx in the gas mixture is converted by the catalyst.
[0161] The CuIZM-9 catalyst synthesized according to the invention gives superior performances to the CuAFX catalyst synthesized according to the prior art in terms of initiation temperatures and NOx conversion at low temperatures (T<300°C) in Standard SCR conditions. Indeed, at the same conversion rate (50% or 80%), the initiation temperatures obtained with the CuIZM-9 catalyst according to the invention are lower compared to those obtained with the CuAFX catalyst.
[0162] Nitrous oxide (N2O) emissions are comparable for both catalysts tested (<7ppm).
[0163] Example 7: Conversion of NOx to Standard-SCR - comparison of iron catalysts according to the invention with the prior art
[0164] A catalytic test for the reduction of nitrogen oxides (NOx) by ammonia (NH3) in the presence of oxygen (O2) under Standard SCR conditions is carried out at different operating temperatures for the synthesized catalyst FeIZM-9 according to the invention (example 3) and the FeAFX sample synthesized according to the prior art (example 5).
[0165] 200 mg of catalyst in powder form is placed in a quartz reactor. 218 L / h of a load representative of a diesel engine exhaust gas mixture are fed into the reactor. This load has the following molar composition: 400 ppm NO, 400 ppm NH3, 8.5% O2, 9% CO2, 10% H2O, qpc N2.
[0166] An FTIR analyzer allows the concentration of NO, NO2, NH3, N2O, CO, CO2, H2O, O2 species to be measured at the reactor outlet. The NOx conversions are calculated as follows:
[0167] Conversion = (NOx input -NOx output) / NOx input
[0168] The NOx conversion results are shown in [Fig.4], the curves marked by circles and crosses corresponding respectively to the tests carried out with the catalysts synthesized according to Example 3 (FeIZM-9) and Example 5 (FeAFX).
[0169] The catalyst initiation temperatures are given below for Standard-SCR conditions:
[0170] [Tables2] T50 T80 T90 T100 FeIZM-9 328°C 393°C 422°C - FeAFX 401°C 455°C 481°C -
[0171] T50 corresponds to the temperature at which 50% of the NOx in the gas mixture are converted by the catalyst. T80 corresponds to the temperature at which 80% of the NOx in the gas mixture is converted by the catalyst. T90 corresponds to the temperature at which 90% of the NOx in the gas mixture is converted by the catalyst. T100 corresponds to the temperature at which 100% of the NOx in the gas mixture is converted by the catalyst.
[0172] The FeIZM-9 catalyst synthesized according to the invention gives superior performances to the FeAFX catalyst synthesized according to the prior art in terms of initiation temperatures and NOx conversion at temperatures below 480°C in Standard SCR conditions. Indeed, at the same conversion rate (50% or 80%), the initiation temperatures obtained with the catalyst according to the invention FeIZM-9 are lower compared to those obtained with the FeAFX catalyst.
[0173] Nitrous oxide (N2O) emissions are almost zero for the two catalysts tested (<0.5 ppm).
Claims
Claims
1. Process for preparing a catalyst based on zeolite of AFX structural type exchanged with at least one transition metal comprising at least the following steps: i) the mixture in aqueous medium of at least one source of silicon (Si) in oxide form SiO2, of at least one source of aluminum (Al) in oxide form A12O3, of an organic nitrogen compound RI, and of a second organic nitrogen compound R2, of at least one source of sodium Na, the reaction mixture having the following molar composition: SiO2 / Al2O3 between 6.00 and 200, preferably between 6.00 and 100 H2O / SiO2 between 1.00 and 100, preferably between 5 and 60 Rl / SiO2 between 0.01 and 0.60, preferably between 0.015 and 0.50 R2 / SiO2 between 0.01 and 0.60, preferably between 0.05 and 0.50 Na2O / SiO2 between 0.005 and 0.45, preferably between 0.05 and 0.25, RI being chosen from the organic compounds tetraethylammonium or tetrapropylammonium, preferably RI is tetraethylammonium and R2 being chosen from the organic compounds 1,6-bis(methylpiperidinium)hexane 1,5-bis(methylpiperidinium)pentane, or l,7-bis(methylpiperidinium)heptane, preferably R2 is l,6-bis(methylpiperidinium)hexane, the organic compounds RI and R2 being introduced in hydroxide form; until a homogeneous precursor gel is obtained; ii) The curing of the precursor gel of said step i) at a temperature between 20 and 40°C with or without stirring, for a period between 10 minutes and 72 hours, preferably between 5 hours and 48 hours, and more preferably between 18 and 24 hours; iii) The addition of FAU structural type zeolite powder having a SiO2 (FAU) / A12O3 (FAU) ratio of between 5.2 and 75 to the gel resulting from step ii), the quantity of silicon SiO2 (FAU) provided by said FAU zeolite representing between 1 and 25%, preferably between 1.5 and 10% by weight of the total quantity of SiO2 in the gel; iv) Maturing the gel containing the FAU zeolite powder obtained in step iii) with stirring at a temperature of between 20 and 40°C for a period of 1 hour to 12 hours, preferably 1 hour to 8 hours and more preferably 1 hour to 3 hours, to obtain a gel homogeneous precursor; v) hydrothermal treatment of said homogeneous precursor gel at a temperature between 110°C and 220°C for a period of between 5 hours and 10 days, preferably under autogenous reaction pressure, until said zeolite of AFX structural type is formed, said solid phase formed from a zeolite of AFX structural type being filtered, washed and then dried at the end of the hydrothermal treatment;vi) at least one ion exchange comprising bringing said solid obtained at the end of the preceding step into contact with a solution comprising at least one species capable of releasing a transition metal, in solution in reactive form with stirring at room temperature for a period of between 1 hour and 2 days, said transition metal released in the exchange solution of step vi) being selected from the group formed by the following elements: Ti, V, Mn, Mo, Fe, Co, Cu, Cr, Zn, Nb, Ce, Zr, Rh, Pd, Pt, Au, W, Ag, preferably from the group formed by the following elements: Fe, Cu, Nb, Ce or Mn, more preferably from Fe, Ce or Cu, alone or as a mixture, and even more preferably said transition metal is Cu; vii) heat treatment by drying the solid obtained at the end of the previous step at a temperature between 20 and 150°C followed by at least one calcination under air flow at a temperature between 400 and 700°C.;
2. A process for preparing a catalyst according to claim 1 in which steps vi) and vii) are reversed, and one or both of them optionally repeated.
3. Preparation process according to one of claims 1 or 2 in which the precursor gel obtained at the end of step iii) has a SiO2 / Al2O3 ratio of between 20 and 80, preferably between 25 and 70.
4. Preparation process according to one of the preceding claims in which in step vi) an ion exchange is carried out by bringing the solid obtained at the end of step v) into contact with an acid or a compound such as ammonium chloride, sulfate or nitrate, before the ion exchange with the transition metal(s), to obtain the protonated form of the zeolite.
5. Preparation process according to claim 4 in which the content of transition metal(s) introduced by the ion exchange step vi) is advantageously between 0.5 and 6% by mass, preferably between 0.5 and 5% by mass, more preferably between 1 and 4% by mass, relative to the total mass of the final anhydrous catalyst.
6. Preparation process according to one of the preceding claims in which step vi) of heat treatment comprises drying the solid at a temperature of between 60 and 100°C for a period of between 2 and 24 hours, followed by at least one calcination in air, optionally dry, at a temperature of between 450 and 700°C, preferably between 500 and 600°C, for a period of between 2 and 20 hours, preferably between 5 and 10 hours, more preferably between 6 and 9 hours, the flow rate of optionally dry air being preferably between 0.5 and 1.5 L / h / g of solid to be treated, more preferably between 0.7 and 1.2 L / h / g of solid to be treated.
7. Zeolite-based catalyst of AFX structural type with a SiO2 / Al2O3 molar ratio as determined by X-ray fluorescence of between 6 and 14, comprising at least one transition metal, preferably iron, cerium or copper, very preferably iron or copper, at a content of between 0.5 and 6% by mass relative to the total mass of the catalyst in its anhydrous form, obtained or capable of being obtained by the preparation process according to one of claims 1 to A
8. U. A method for selectively reducing NOX in a gas mixture by a reducing agent such as NH3 or H2 by contacting said gas mixture with a catalyst according to claim 7.
9. A method for selectively reducing NOx according to claim 8 wherein the catalyst is formed by deposition in the form of a coating, on a honeycomb structure or a plate structure.
10. A method for selectively reducing NOx according to claim 9, wherein the honeycomb structure is formed of parallel channels open at both ends or comprises porous filtering walls for which the adjacent parallel channels are alternately blocked on either side of the channels.
11. Method for selective reduction of NOx according to claim 10, for which the quantity of catalyst deposited on said structure is between 50 and 180 g / L for filtering structures and between 80 and 200 g / L for structures with open channels.
12. Process for selective reduction of NOx according to one of claims 8 to 11, for which the catalyst is associated with a binder such as ceria, zirconium oxide, alumina, non-zeolitic silica-alumina, titanium oxide, a mixed oxide of ceria-zirconia type, an oxide of tungsten and / or spinel to be shaped by deposition in the form of a coating.
13. Method for selective reduction of NOx according to one of claims 9 to 12, for which said coating is associated with another coating having NOx adsorption capacities, NOx reduction capacities or promoting the oxidation of ammonia.
14. A process for selective reduction of NOx according to claim 8, wherein said catalyst is in extrudate form, containing up to 100% of said catalyst.
15. Method for selective reduction of NOx according to one of claims 8 to 14, for which the structure coated by said catalyst or obtained by extrusion of said catalyst is integrated into an exhaust line of an internal combustion engine.