Multilayer structure with adhesive properties
The multilayer structure with a polyolefin A and functional polyolefin adhesive layer, combined with a polyamide graft polymer support film, addresses manufacturing challenges by improving adhesion and efficiency in photovoltaic modules.
Patent Information
- Application Number
- FR2022013670
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-16
AI Technical Summary
Existing photovoltaic module encapsulant technologies face challenges such as complex and costly manufacturing processes, poor adhesion to metal interconnectors, and limitations in geometric configurations, leading to defects and reduced efficiency and lifespan.
A multilayer structure comprising an adhesive layer with polyolefin A and a functional polyolefin, and a support film with a polyamide graft polymer, providing excellent adhesion and thermal stability, allowing for easier assembly and reliable electrical contact.
The multilayer structure enhances adhesion to metal interconnectors, simplifies assembly, ensures reliable electrical contact, and results in higher quality and cost-effective photovoltaic modules with improved efficiency and lifespan.
Smart Images

Figure 00000027_0000 
Figure 00000027_0001 
Figure 00000027_0002
Abstract
Description
Title of the invention: Multilayer structure with adhesive properties Field of invention
[0001] The invention relates to a multilayer structure, in particular a bilayer structure, useful especially as an encapsulant for photovoltaic modules. It also relates to photovoltaic modules comprising such a multilayer structure. Technical background
[0002] Global warming, linked to greenhouse gases released by fossil fuels, further reinforces the interest in alternative energy solutions that do not emit such gases during their operation, such as photovoltaic modules.
[0003] There are many types of photovoltaic module structure.
[0004] Figure 1 represents a conventional photovoltaic cell; a photovoltaic cell (10) comprises cells (12), each cell containing a photovoltaic sensor (14) in contact with electron collectors (16) located above (upper collectors) and below (lower collectors) the photovoltaic sensor. The upper collectors (16) of one cell are connected to the lower collectors (16) of another cell (12) by conductive bars (18), also referred to as electrical interconnectors, generally made of a metal alloy. In other embodiments, the interconnectors are all located on the same side of the cells. All these cells (12) are connected together, in series and / or in parallel, to form the photovoltaic cell (10). When the photovoltaic cell (10) is placed under a light source, it delivers a direct electric current, which can be recovered at the terminals (19) of the cell (10).
[0005] Figure [Fig. 2] represents a photovoltaic module (20) comprising the photovoltaic cell The photovoltaic cell (10) of [Fig. 1] is encapsulated in a casing (22) consisting of an upper and a lower part. The encapsulated cell is further protected by an upper protective layer (24) (called the "frontsheet") and a protective layer on the back of the module (called the "backsheet") (26). The upper protective layer (24), generally made of glass, provides shock and moisture protection for the photovoltaic cell. The protective layer on the back of the module (26), generally made of thermoplastic or crosslinkable resin, also contributes to its protection against moisture and, in addition, to the electrical insulation of the cells by preventing any contact with the external environment.
[0006] In order to ensure effective protection, it is important that the encapsulant fills by It completely fills the space between the photovoltaic cell and the protective layers. Furthermore, its adhesion to the protective layers must be perfect and durable, even at temperatures of 80°C or higher, which can be reached under solar radiation.
[0007] To promote adhesion, one can use either "chemical" techniques by providing a specific binder or adhesion promoter, or physical techniques such as surface treatment by corona or plasma. However, these methods require additional, sometimes complex, operations for results that are often disappointing and incur a significant cost. Furthermore, physical surface treatments are not stable over time and require precautions for storage and handling.
[0008] Currently, to manufacture a photovoltaic module, the "frontsheet", the encapsulant, the cell and the "backsheet" are assembled simultaneously, most often by a vacuum lamination process. The encapsulant is melted during the lamination step in order to coat the active layers of the cell.
[0009] In addition to the handling of numerous films, this lamination assembly process has drawbacks related to the shrinkage of the encapsulating film, which can reach 10%, or even sometimes 50%. This shrinkage can lead to defects in the photovoltaic module, such as air bubbles, creases, blisters, edge overlap defects, or breaks in the cell connectors. All these defects result in rejects or can reduce the lifespan and efficiency of the photovoltaic modules.
[0010] To limit these problems, the encapsulating film can be produced by an extrusion process followed by a post-annealing step, but this reduces the extrusion speed and therefore increases its cost.
[0011] EP 2 673 809 A1 discloses a bilayer film composed of a backsheet and an encapsulant that addresses at least some of these problems. However, implementing these bilayer structures requires successively stacking a first encapsulant layer, the photovoltaic module, a second encapsulant layer, and finally a layer forming the backsheet, as shown in [Fig. 2]. In addition to a first encapsulant layer 400 µm thick, bilayer structures 800 µm thick are described. The significant thickness of these structures adds considerable weight and cost. Furthermore, the encapsulant does not offer sufficient adhesion to the metal to be used in processes that include a pre-rolling step on the surface of the metallic interconnectors.
[0012] Furthermore, these bilayer films cannot be used for the preparation of photovoltaic modules with certain geometric configurations, in particular connections located on the same side as the photovoltaic cells, such as those described for example in application WO 2004 / 021455, and which require laminating the encapsulant directly onto the surface of the interconnectors.
[0013] There is therefore a need for multilayer structures, particularly for photovoltaic modules, to overcome the disadvantages of the state of the art, in particular to improve the productivity of preparation processes and the quality of photovoltaic modules, and which are versatile and therefore compatible with different geometric configurations and assembly processes of photovoltaic modules. Summary of the invention
[0014] The present invention aims to remedy the problems encountered in the prior art by proposing a multilayer structure, in particular a bilayer structure, comprising an adhesive layer and a support film.
[0015] In its broadest definition, the invention relates to a multilayer structure comprising an adhesive layer that can serve as an encapsulant and a support film that can serve as a backsheet, characterized in that the adhesive layer comprises a polyolefin A and a functional polyolefin and has a specific melting point in that the support film has a specific flow temperature.
[0016] Indeed, it has been observed that by combining a polyolefin A with a functional polyolefin in the adhesive layer, it was possible to obtain a multilayer structure exhibiting both very good thermal stability and excellent adhesion with the metal of the electrical interconnectors of photovoltaic cells.
[0017] The improved adhesion of the multilayer structure to the interconnectors offers a dual advantage. Firstly, it simplifies the assembly process, notably by eliminating the need for pre-treatment of the surface. Secondly, it ensures reliable electrical contact between the interconnectors and the photovoltaic cells, thus providing the photovoltaic modules with greater efficiency and a longer lifespan.
[0018] Finally, the multilayer structures of the invention can be of low thickness, in particular less than 100 pm.
[0019] The multilayer structures according to the invention thus allow the manufacture of photovoltaic modules that are both of better quality and less expensive.
[0020] Thus, the present invention relates to a multilayer structure comprising an adhesive layer and a layer forming a support film in direct contact therewith, where
[0021] (a) said adhesive layer comprises: - a polyolefin A selected from an ethylene homopolymer and an ethylene copolymer and an α-olefin, an ethylene copolymer and a vinyl ester of carboxylic acid, in particular a vinyl acetate (EVA) or a (co)polymer comprising (meth)acrylate motifs of methyl, ethyl, propyl, n-butyl, sec-butyl, isobutyl or tert-butyl; and - a functionalized polyolefin, distinct from polyolefin A, comprising a polyolefin trunk containing a remnant of at least one unsaturated monomer (Y), the remainder of the unsaturated monomer (Y) being attached to the trunk by grafting or copolymerization;
[0022] the melting temperature of the adhesive layer being between 80°C and 120°C,
[0023] b) said support film comprises a grafted polyamide polymer comprising: - a polyolefin trunk, representing 50% to 95% by mass of the grafted polyamide polymer, containing a remnant of at least one unsaturated monomer (X) and at least one polyamide graft, representing 5% to 50% by mass of said grafted polyamide polymer, in which: • the polyamide graft is attached to the polyolefin trunk by the remainder of the unsaturated monomer (X) comprising a function capable of reacting by a condensation reaction with a polyamide having at least one amine end and / or at least one carboxylic acid end, • the remainder of the unsaturated monomer (X) is fixed to the trunk by grafting or copolymerization, • the polyolefin trunk and the polyamide graft being chosen such that said grafted polyamide polymer has a flow temperature above 160°C, as measured by DSC according to ISO 11357-1:2016, ISO 11357-2:2020, ISO 11357-3:2018, said flow temperature being defined as the highest temperature among the melting temperatures and glass transition temperatures of the polyamide graft and the polyolefin trunk.
[0024] Other advantageous features of the invention are: - the melting temperature of said adhesive layer is between 90°C and 110°C. - said adhesive layer has a Melt Flow Index (MFI), as measured according to ASTP D 1238 at 190°C under 2.16kg, of between 0.2 and 10 g / 10 min, preferably between 0.4 and 3 g / 10 min, and in particular between 0.6 and 2 g / 10 min. - said adhesive layer comprises: • 65% to 95% by weight of polyolefin A; • 5 to 35% by weight of functional polyolefin; and • 0 to 5% by weight of one or more additives. - the thickness of said adhesive layer is between 20 and 60 µm. - the thickness of said support film is between 5 and 40 µm.
[0025]
[0026]
[0027]
[0028]
[0029]
[0030] - the α-olefin comonomer of the polyolefin A of the adhesive layer is chosen from ethylene-propylene, ethylene-butene and ethylene-octene. - the functional polyolefin of the adhesive layer is a polyolefin containing a remnant of at least one unsaturated monomer (Y) which is a maleic anhydride. - said support film has a Melt Flow Index (MFI), as measured according to ASTP D 1238 at 230°C under 2.16kg, of between 0.2 and 10 g / 10 min, preferably between 0.4 and 3 g / 10 min, in particular between 0.6 and 2 g / 10 min. - said support film has said adhesive layer on one of its faces. - said support film carries said adhesive layer on both sides. - said backing film is assembled to said adhesive layer by coextrusion. According to another aspect, the invention aims at the use of such a multilayer structure for the manufacture of photovoltaic modules. According to yet another aspect, the invention relates to a method for preparing a photovoltaic module, in which a photovoltaic cell is encapsulated with such a multilayer structure. In this process, encapsulation may include the following steps: i. fixing an electrically conductive filament to the surface of said adhesive layer of such a multilayer structure at a temperature lower than the melting temperature of said adhesive layer to form an assembly; ii. bringing said assembly into contact with a photovoltaic cell at a temperature between the melting temperature of the adhesive layer and the flow temperature of the support film. Finally, according to a last aspect, the invention aims at a photovoltaic module comprising such a multilayer structure. Description of the Figures The following description is given for illustrative purposes only and is not exhaustive, with reference to the attached figures, in which: - Fig. 1 represents an example of a photovoltaic cell, parts (a) and (b) being three-quarter views, part (a) showing one cell before connection and part (b) a view after connection of two cells; part (c) is a top view of a complete photovoltaic cell; and - Fig. 2 represents a cross-section of a photovoltaic module, whose "classic" photovoltaic sensor is encapsulated by a top encapsulating film and a bottom encapsulating film. Description of the invention Thus, according to a first aspect, the invention relates to a multilayer structure, in particular as an encapsulant for photovoltaic cells, comprising an adhesive layer and a layer forming a support film in direct contact therewith, wherein the adhesive layer comprises a polyolefin A and a functionalized polyolefin, the melting temperature of the adhesive layer being between 80°C and 120°C, and wherein the support film comprises a specific grafted polyamide polymer having a flow temperature above 160°C, as measured by DSC according to ISO 11357-1:2016, ISO 11357-2:2020, ISO 11357-3:2018, the flow temperature being defined as the highest temperature among the melting temperatures and the glass transition temperatures of the polyamide graft and the polyolefin trunk. A. Multilayer structure
[0031] According to the invention, the adhesive layer of the multilayer structure is in direct contact with the support film.
[0032] In the absence of additional layers, the multilayer structure can form a two-layer structure. However, it can also include other layers, in principle any layers. According to a preferred embodiment, the multilayer structure can be a three-layer structure, and in particular include a support film having an adhesive layer as defined below on both of its faces. Al Adhesive layer
[0033] According to the invention, the adhesive layer of the multilayer structure comprises a specific polyolefin A and a distinct functional polyolefin, the melting temperature of the adhesive layer being between 80°C and 120°C. The polyolefins will be described in more detail below. Polyolefin A
[0034] The polyolefin A present in the adhesive layer may be a homopolymer of ethylene or a copolymer of ethylene with a comonomer selected from an α-olefin, an alkyl (meth)acrylate, or a vinyl ester of a carboxylic acid, in particular a vinyl acetate. In the copolymer, the α-olefin may comprise 3 to 30, in particular 3 to 8 carbon atoms. Examples of alpha-olefins include propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicocene, 1-dococene, 1-tetracocene, 1-hexacocene, 1-octacocene, and 1-triacontene. These alpha-olefins can be used alone or in mixtures of two or more.
[0035] Preferably, ethylene-α-olefin copolymers comprise a mass percentage of ethylene greater than 50%.
[0036] Ethylene-α-olefin copolymers are obtained by known processes of the man of the art, such as Ziegler-Natta, metallocene or organo-metallic polymerization described for example in WO 2008 / 036707.
[0037] Particularly preferred as polyolefin A is polyethylene, in particular linear low density polyethylene (LLDPE), or a copolymer of ethylene with a single α-olefin, selected from ethylene-propylene, ethylene-butene and ethylene octene.
[0038] According to another embodiment, polyolefin A is a copolymer of ethylene and alkyl (meth)acrylate, the term alkyl (meth)acrylate encompassing alkyl acrylates or methacrylates. The alkyl chains of these (meth)acrylates can have up to 30 carbon atoms. Examples of alkyl chains include methyl, ethyl, propyl, n-butyl, sec-butyl, isobutyl, tert-butyl, pentyl, hexyl, heptyl, octyl, 2-ethylhexyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, hencosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, and nonacosyl. Methyl, ethyl, and butyl (meth)acrylates are preferred.
[0039] Ethylene-(meth)acrylate alkyl copolymers are classically obtained by processes known to those skilled in the art, such as, for example, the high pressure autoclave or tubular process.
[0040] According to a particularly preferred embodiment, polyolefin A is a copolymer of ethylene and vinyl acetate (EVA).
[0041] Preferably, polyolefin A has a melting temperature between 90°C and 110°C, and in particular between 90°C and 105°C.
[0042] According to one embodiment, the enthalpy of fusion of polyolefin A is less than 130 J / g, and in particular between 80 and 120 J / g (2nd heating of DSC according to ISO 11347 at 40°C / min).
[0043] The density of polyolefin A, measured according to ASTM D 1505, is preferably from 0.860 to 0.960, in particular from 0.860 to 0.920.
[0044] Indeed, without wishing to limit itself to a particular theory, the applicant was able to observe that a low enthalpy of fusion, within the range mentioned above, reflecting a low degree of crystallinity, made it possible to favorably influence the adhesion of the adhesive layer on the metal. Functional polyolefin
[0045] The term "functional polyolefin" means, for the purposes of this description, a polyolefin distinct from polyolefin A present in the adhesive layer and comprising reactive functions, and capable of reacting on contact with a metallic surface.
[0046] Such reactive functions include, in particular, epoxide, carboxylic acid, carboxylic acid anhydride, carboxylic acid amide and carboxylic acid ester functions.
[0047] The functionalized polyolefin present in the adhesive layer comprises a polyolefin trunk containing a remnant of at least one unsaturated monomer (Y) selected from an unsaturated epoxide, an unsaturated carboxylic acid anhydride, an unsaturated carboxylic acid, or a salt thereof, the remainder of the unsaturated monomer (Y) being fixed to the trunk by grafting or copolymerization.
[0048] These functions promote interaction with the metallic surface in contact with the electrical interconnectors, which improves adhesion between the multilayer structure and the electrical interconnectors.
[0049] Functional polyolefins can in particular be derived from monomers such as meth(acrylic) acid, (meth)acrylamide or vinyl acetate.
[0050] According to one embodiment, the polyolefin trunk of the functional polyolefin is a polyethylene trunk, in particular a homopolymer or a copolymer of ethylene.
[0051] The unsaturated monomer (Y) may be an unsaturated epoxide, in particular selected from aliphatic glycidyl esters and ethers such as allylglycidyl ether, vinylglycidyl ether, glycidyl maleate and itaconate, glycidyl acrylate and glycidyl methacrylate; alicyclic glycidyl esters and ethers such as 2-cyclohexene-l-glycidyl ether, cyclohexene-4,5-diglycidylcarboxylate, cyclohexene-4-glycidyl carboxylate, 5-norbomene-2-methyl-2-glycidyl carboxylate and endocis-bicyclo(2,2,l)-5-heptene-2,3-diglycidyl dicarboxylate, glycidyl methacrylate being preferred.
[0052] Alternatively, the unsaturated monomer (Y) may be an unsaturated carboxylic acid or one of its salts, in particular acrylic acid or methacrylic acid and their salts.
[0053] Alternatively, the unsaturated monomer (Y) may be an unsaturated carboxylic acid ester, in particular an alkyl (meth)acrylate, the term alkyl (meth)acrylate encompassing alkyl acrylates or methacrylates. The alkyl chains of these (meth)acrylates may have up to 30, in particular up to 24 carbon atoms. Examples of alkyl chains include methyl, ethyl, propyl, n-butyl, sec-butyl, isobutyl, tert-butyl, pentyl, hexyl, heptyl, octyl, 2-ethylhexyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, hencosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, and nonacosyl, particularly methyl, ethyl, and butyl (meth)acrylates.
[0054] Alternatively, the unsaturated monomer (Y) may be a carboxylic acid anhydride, in particular selected from maleic, itaconic, citraconic, allylsuccinic, cyclohex-4-ene-1,2-dicarboxylic, 4-methylenecyclohex-4-ene-1,2-dicarboxylic, bicyclo(2,2,l)hept-5-ene-2,3-dicarboxylic, and x-methylbicyclo(2,2,l)hept-5-ene-2,2-dicarboxylic. Among these, maleic anhydride is preferred.
[0055] The unsaturated monomer (Y) can also be a vinyl ester of carboxylic acid, in particular a vinyl acetate.
[0056] Alternatively, the unsaturated monomer (Y) can also be a (meth)acrylamide, chosen from acrylamide and methacrylamide.
[0057] The unsaturated monomer (Y) in the functional polyolefin is fixed by grafting or copolymerization.
[0058] Preferably, the functional polyolefin does not comprise a polyamide graft.
[0059] Preferably, the functional polyolefin is an ethylene copolymer containing a residue of unsaturated carboxylic acid anhydride, in particular maleic anhydride.
[0060] The ethylene copolymer can be a copolymer of ethylene and a comonomer selected from the esters of unsaturated carboxylic acids such as, for example, alkyl acrylates or alkyl methacrylates grouped under the term (meth)acrylates of alkyls as specified above.
[0061] Ethylene copolymers and unsaturated carboxylic acid esters can be obtained by processes known to those skilled in the art, such as, for example, the high-pressure autoclave or tubular process.
[0062] According to a preferred embodiment, the functional polyolefin is an ethylene-(meth)acrylate alkyl maleic anhydride terpolymer.
[0063] According to one embodiment, the adhesive layer comprises at least 65% by weight of a polyolefin A as defined above.
[0064] According to another embodiment, the adhesive layer comprises at least 5% by weight of a functional polyolefin.
[0065] According to a preferred embodiment, the adhesive layer comprises: - from 65% to 95% by weight of a polyolefin A as defined above; - 5 to 30% by weight of a functional polyolefin; as well as - 0 to 5% by weight of additives, notably chosen from plasticizers, adhesion promoters, UV stabilizers, UV absorbers, antioxidants, and pigments.
[0066] Plasticizers may be added to the adhesive layer to facilitate implementation and improve the productivity of the manufacturing process for multilayer structures and / or photovoltaic modules. Examples include aromatic or naphthalene paraffinic mineral oils, which also improve the adhesion of the structures according to the invention. Other plasticizers that may be used include phthalates, azelates, adipates, and ticresyl phosphate.
[0067] Colouring or brightening compounds may also be added.
[0068] Similarly, adhesion promoters, although not necessary, can be advantageously added to further improve the adhesion power of the Structure. The adhesion promoter is a non-polymeric ingredient; it can be organic, crystalline, mineral, or, more preferably, a semi-organic-mineral compound. Examples include organic titanates or silanes, such as monoalkyl titanates, trichlorosilanes, and trialcooxysilanes. Advantageously, trialcooxysilanes containing an epoxy, vinyl, or amine group are used, particularly when these adhesion promoters are added as a masterbatch. Alternatively, these adhesion promoters may be diluted or mixed with the functional or non-functional polyolefin of the adhesive layer using a technique well known to those skilled in the art, such as compounding.
[0069] Since UV radiation is likely to cause slight yellowing of the adhesive layer, UV stabilizers and UV absorbers such as benzotriazole, benzene and other hindered amines may be added to the adhesive layer and / or to the support film in order to prolong the transparency of the multilayer structure and thus its lifespan.
[0070] The adhesive layer may also comprise 0 to 5% by weight, in particular 0.1 to 4.5%, in particular 0.5 to 4%, and especially 1 to 3% by weight of one or more of these additives, relative to the total weight of the composition.
[0071] The adhesive layer may also include one or more antioxidants to limit yellowing during the manufacture of the adhesive layer. Preferred antioxidants include, for example, phosphorus compounds (phosphonites and / or phosphites) and hindered phenolics.
[0072] The adhesive layer may include, in particular, 0 to 3% by weight, in particular 0.1 to 2.5%, in particular 0.5 to 2%, and especially 1 to 1.5% by weight of one or more antioxidants relative to the total weight of the composition.
[0073] Pigments such as colouring or brightening compounds can also be added to the adhesive layer in proportions generally ranging from 0.01 to 2% relative to the total mass of the composition.
[0074] According to one embodiment, the thickness of the adhesive layer is between 20 and 60 pm.
[0075] The melting temperature of the adhesive layer is preferably between 80 and 110°C, preferably between 90°C and 100°C.
[0076] Indeed, the inventors observed that if the melting temperature is lower, the multilayer structure can be difficult to handle, particularly during the co-extrusion step with the support film and / or during its subsequent use, especially during the lamination step on the surface of the filaments. Conversely, a melting temperature above 120°C is generally accompanied by a higher degree of crystallinity, which can reduce adhesion to the metal filaments.
[0077] According to one embodiment, the adhesive layer has a hot melt index or Melt Flow Index (MFI) between 0.2 and 10 g / 10 min, preferably between 0.4 and 3 g / 10 min, and more preferably between 0.6 and 2 g / 10 min, measured according to ASTM D1238 at 190°C / 2.16kg. A.2. Film support
[0078] The support film comprises a polyamide grafted polymer including a polyolefin trunk containing a remainder of at least one unsaturated monomer (X) and at least one polyamide graft, the polyamide graft being attached to the polyolefin trunk by the remainder of the unsaturated monomer (X) including a function capable of reacting by a condensation reaction with a polyamide, the polyolefin trunk and the polyamide graft being chosen so that said polyamide grafted polymer has a flow temperature above 160°C.
[0079] The flow temperature of the grafted polyamide polymer is defined as the highest of the melting and glass transition temperatures of the polyamide grafts and the polyolefin core. The core and grafts are chosen so that the flow temperature of the grafted polyamide polymer is greater than 160°C.
[0080] The grafted polyamide polymer comprises 50 to 95%, preferably 60 to 90% and in particular 70 to 85% by mass of a polyolefin trunk containing a remnant of at least one unsaturated monomer (X).
[0081] As regards the polyolefin trunk, it is preferably a polymer comprising as a monomer an α-olefin, in particular comprising 2 to 30 carbon atoms.
[0082] Examples of α-olefins include ethylene, propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicocene, 1-dococene, 1-tetracocene, 1-hexacocene, 1-octacocene, and 1-triacontene.
[0083] We can also mention cyclo-olefins having 3 to 30, in particular 3 to 20 carbon atoms, such as cyclopentane, cycloheptene, norbomene, 5-methyl-2-norbomene, tetracyclododecene, and 2-methyl-1,4,5,8-dimethano-1,2,3,4,4a,5,8,8a-octahydronaphthalene; di- and poly-olefins, such as butadiene, isoprene, 4-methyl-1,3-pentadiene, 1,4-pentadiene, 1,5-hexadiene, 1,3-hexadiene, 1,3-octadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, retethylidenenorbomene, vinyl norbornene, dicyclo-pentadiene, 7-methyl-1,6-octadiene, 4-ethylidiene-8-methyl-1,7-nonadiene, and 5,9-dimethyl-1,4,8-decatriene;aromatic vinyl compounds such as mono- or poly alkylstyrenes (including styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, o-ethylstyrene, m-ethylstyrene and p-ethylstyrene), and derivatives comprising functional groups such as methoxystyrene, ethoxystyrene, vinyl benzoic acid, vinyl methyl benzoate, acetate of; benzyl vinyl, hydroxystyrene, o-chlorostyrene, p-chlorostyrene, di-vinyl benzene, 3-phenylpropene, 4-phenylpropene, a-methylstyrene, vinyl chloride, 1,2-difluoroethylene, 1,2-dichloroethylene, tetrafluoroethylene, and 3,3,3-trifluoro-l-propene, with propylene and ethylene preferred.
[0084] Polyolefin can be a homopolymer when a single α-olefin is polymerized. Examples include polyethylene (PE) and polypropylene (PP). It can also be a copolymer when at least two comonomers are copolymerized in the polymer chain, the first of the at least two monomers being an α-olefin and the other comonomers being a monomer capable of polymerizing with the first monomer.
[0085] Other comonomers include: - one of the α-olefins already mentioned above, different from the first α-olefin comonomer; - dienes such as, for example, 1,4-hexadiene, ethylidene, norbomene, butadiene; - unsaturated carboxylic acid esters such as alkyl acrylates or alkyl methacrylates, grouped under the term alkyl (meth)acrylates. The alkyl chains of these (meth)acrylates can have up to 30 carbon atoms. Examples of alkyl chains include methyl, ethyl, propyl, n-butyl, sec-butyl, isobutyl, tert-butyl, pentyl, hexyl, heptyl, octyl, 2-ethylhexyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, hencosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, and nonacosyl, with methyl, ethyl, and butyl (meth)acrylates being preferred; and - vinyl esters of carboxylic acids. Examples of vinyl esters of carboxylic acids include vinyl acetate, vinyl versatate, vinyl propionate, vinyl butyrate, or vinyl maleate, with vinyl acetate being preferred.
[0086] Advantageously, the polyolefin trunk is made up of at least 50 mole percent of the first comonomer.
[0087] Preferred polyolefin trunks are made of alkyl ethylene-(meth)acrylate copolymer. Using this polyolefin trunk provides excellent resistance to aging under light and temperature conditions.
[0088] According to the present invention, the polyolefin trunk contains at least one unsaturated monomer remnant (X) capable of reacting with an acid and / or amine function of the polyamide graft by a condensation reaction. It is specified that this unsaturated monomer (X) is not a "second comonomer".
[0089] Examples of unsaturated monomers (X) include: - unsaturated epoxides. Among these, aliphatic glycidyl esters and ethers such as allylglycidyl ether, vinylglycidyl ether, glycidyl maleate and itaconate, glycidyl acrylate and methacrylate; alicyclic glycidyl esters and ethers such as 2-cyclohexene-l-glycidyl ether, cyclohexene-4,5-diglycidylcarboxylate, cyclohexene-4-glycidyl car-boxylate, 5-norbornene-2-methyl-2-glycidyl carboxylate and endocis-bicyclo(2,2,l)-5-heptene-2,3-diglycidyl dicarboxylate, glycidyl methacrylate being preferred. - unsaturated carboxylic acids and their salts, for example acrylic acid or methacrylic acid and their salts. - carboxylic acid anhydrides, chosen for example from maleic, itaconic, citraconic, allylsuccinic, cyclohex-4-ene-1,2-dicarboxylic, 4-methylenecyclohex-4-ene-1,2-dicarboxylic, bicyclo(2,2,l)hept-5-ene-2,3-dicarboxylic, and x-methylbicyclo(2,2,l)hept-5-ene-2,2-dicarboxylic, in particular maleic anhydride.
[0090] The unsaturated monomer (X) is preferably chosen from an unsaturated carboxylic acid anhydride and an unsaturated epoxide. In particular, to carry out the condensation of the polyamide graft with the polyolefin trunk, in the case where the reactive end of the polyamide graft is a carboxylic acid function, the unsaturated monomer (X) is preferably an unsaturated epoxide. In the case where the reactive end of the polyamide graft is an amine function, the unsaturated monomer (X) is advantageously an unsaturated epoxide and preferably an unsaturated carboxylic acid anhydride.
[0091] According to an advantageous embodiment of the invention, the preferred number of unsaturated monomer (X) fixed on average on the polyolefin trunk is greater than or equal to 1.3 and / or preferably less than or equal to 10.
[0092] Thus, if (X) is maleic anhydride and the number molar mass of the polyolefin is 15,000 g / mol, this was found to correspond to an anhydride proportion of at least 0.8% by mass of the entire polyolefin trunk and at most 6.5%. These values, combined with the mass of the polyamide grafts, determine the proportion of polyamide and trunk in the grafted polyamide polymer.
[0093] The polyolefin trunk containing the remainder of the unsaturated monomer (X) is obtained by polymerization of the monomers (first comonomer, optional second comonomer, and optionally unsaturated monomer (X)). This polymerization can be carried out by a high-pressure radical process or a solution process, in an autoclave or tubular reactor, these processes and reactors being well known to those skilled in the art. When the unsaturated monomer (X) is not copolymerized in the polyolefin trunk The polyolefin monomer is grafted onto the polyolefin core. Grafting is also a known operation in itself. The composition would conform to the invention if several different functional monomers (X) were copolymerized and / or grafted onto the polyolefin core.
[0094] Depending on the types and ratios of monomers, the polyolefin trunk can be semi-crystalline or amorphous. For amorphous polyolefins, only the glass transition temperature is observed, whereas for semi-crystalline polyolefins, both a glass transition temperature and a melting temperature are observed. A polyolefin trunk with the desired glass transition temperature and melting temperature can be obtained by adjusting the type and ratio of monomers. The molar mass of the polyolefin trunk can be modified to obtain the desired viscosity.
[0095] The polyolefin trunk has a Melt Flow Index (MFI) preferably between 3 and 400g / 10min, in particular between 10 and 300g / 10 min and especially between 50 and 200g / 10 min (190°C, 2.16kg, ASTM D 1238).
[0096] Preferably, its density, as measured according to ISO 1183:2019, is advantageously between 0.91 and 0.96.
[0097] The polyamide grafted polymer comprises a polyolefin trunk containing a remnant of at least one unsaturated monomer (X) as described above and at least one polyamide graft attached to the polyolefin trunk via the remnant of the unsaturated monomer (X).
[0098] Polyamide grafts can be homopolyamides or copolyamides. Polyamide grafts can be, in particular, aliphatic, cycloaliphatic or semiaromatic.
[0099] Among homopolyamides, preferred are aliphatic polyamides resulting from the polycondensation of: - a lactam, - of an aliphatic α,Q-aminocarboxylic acid, or - of an aliphatic diamine and an aliphatic diacid.
[0100] Examples of lactam include caprolactam, oenantholactam and lauryllactam.
[0101] Examples of aliphatic α,Q-aminocarboxylic acid include aminocaproic acid, 7-aminoheptanoic acid, 11-aminoundecanoic acid and 12-aminododecanoic acid.
[0102] Examples of aliphatic diamine include rhexa-methylenediamine, dodecamethylenediamine and trimethylhexamethylenediamine.
[0103] Examples of aliphatic diacids include adipic, azelaic, suberic, sebacic and dodecanedicarboxylic acids.
[0104] Among the aliphatic homopolyamides, the following polyamides may be cited by way of example and without limitation: polycaprolactam (PA6); polyundecanamide (PA 11); polylauryllactam (PA12); polybutylene adipamide (PA4.6); Polyhexamethylene adipamide (PA6.6); polyhexamethylene azelamide (PA6.9); polyhexamethylene sebaçamide (PA-6.10); polyhexamethylene dodecanamide (PA6.12); polydecamethylene dodecanamide (PA 10.12); polydecamethylene sebaçanamide (PA 10.10); and polydodecamethylene dodecanamide (PA 12.12). PA 6 is particularly preferred.
[0105] Among the cycloaliphatic homopolyamides, we can notably mention those resulting from the condensation of a cycloaliphatic diamine and an aliphatic diacid.
[0106] As an example of a cycloaliphatic diamine, we can cite 4,4'-methylene-bis(cyclohexylamine), also called para-bis(aminocyclo-hexyl)methane or PACM, 2,2'-dimethyl-4,4'methylene-bis(cyclo-hexyl-amine), also called bis-(3-methyl-4-aminocyclohexyl)-methane or BMACM.
[0107] Among the cycloaliphatic homopolyamides, we can mention in particular the polyamides PACM. 12, BMACM. 10 and BMACM. 12.
[0108] Semi-aromatic homopolyamides can result from the condensation of: - an aliphatic diamine and an aromatic diacid, such as terephthalic acid (T) and isophthalic acid (I). The polyamides obtained are then commonly called "polyphthalamides" or PPA; - of an aromatic diamine, such as xylylenediamine, and more particularly metaxylylenediamine (MXD) and of an aliphatic diacid.
[0109] In this family of polyamides, we can mention in particular polyamides 6.T, 6.1, MXD.6 and MXD.10.
[0110] Alternatively, the polyamide grafts are copolyamides. These result from the polycondensation of at least two of the monomers stated above to obtain homopolyamides.
[0111] The term "monomer" in this description of copolyamides should be understood as "repeating unit." The case where a repeating unit of the PA is formed by the association of a diacid with a diamine is a special one. It is considered that the association of a diamine and a diacid, that is, the diamine-diacid pair (in equimolar quantities), constitutes the monomer. This is because, individually, the diacid or the diamine is only a structural unit, which is not sufficient on its own to polymerize to give a polyamide.
[0112] Thus, copolyamides cover in particular condensation products: - of at least two lactams, - of at least two aliphatic α,Q-aminocarboxylic acids, - of at least one lactam and at least one aliphatic α,Q-aminocarboxylic acid, - of at least two diamines and at least two diacids, - of at least one lactam with at least one diamine and at least one diacid, - of at least one aliphatic α,Q-aminocarboxylic acid with at least one diamine and at least one diacid,
[0113] the diamine(s) and the diacid(s) being able to be, independently of each other, aliphatic, cycloaliphatic or aromatic.
[0114] Depending on the types and ratio of monomers, copolyamides can be semi-crystalline or amorphous. Examples of amorphous copolyamides include copolyamides containing semi-aromatic monomers.
[0115] Semi-crystalline copolyamides, and particularly PA 6 / 11, PA6 / 12 and PA6 / 11 / 12 copolyamides, may also be used.
[0116] The number-average molecular mass Mn of copolyamides, as measured according to ISO 16014-5:2019, can vary in large proportions, but is advantageously less than 10000 g / mol.
[0117] Advantageously, polyamide grafts are monofunctional.
[0118] To ensure that the polyamide graft has a monoamine termination, a chain limiter of the following formula can be used:
[0119] RiR2NH
[0120] in which:
[0121] • RI is hydrogen or a linear or branched alkyl group containing up to 20 carbon atoms,
[0122] • R2 is a group having up to 20 alkyl or alkenyl carbon atoms linear or branched, a saturated or unsaturated cycloaliphatic radical, an aromatic radical, or a combination of the above. The chain limiter could be, for example, laurylamine or oleylamine.
[0123] In order for the polyamide graft to have a monocarboxylic acid termination, a chain limiter of formula R'1-COOH, R'1-CO-O-CO-R'2 or a dicarboxylic acid can be used.
[0124] R'1 and R'2 are linear or branched alkyl groups containing up to 20 carbon atoms.
[0125] Advantageously, the polyamide graft has an amine functional end. Preferred monofunctional polymerization chain restrictors are laurylamine and oleylamine.
[0126] Advantageously, the polyamide grafts have a molar mass between 1000 and 5000 g / mol and preferably between 2000 and 3000 g / mol.
[0127] The polycondensation defined above is carried out according to known processes, for example at a temperature between 200 and 300°C, under vacuum or under an inert atmosphere, with stirring of the reaction mixture. The average chain length of the graft is determined by the initial molar ratio between the polycon- monomer densatable or lactam and chain limiter. For the calculation of the average chain length, one molecule of chain limiter is usually counted for one graft chain.
[0128] A polyamide graft can be prepared with the desired glass transition and melting point by selecting the appropriate types and ratios of monomers. The viscosity of the polyamide graft can be adjusted by modulating its molar mass.
[0129] The condensation reaction of the polyamide graft onto the polyolefin stem containing the remainder of (X) is carried out by the reaction of an amine or acid function of the polyamide graft with the remainder of (X). Advantageously, monoamine polyamide grafts are used, and amide or imide bonds are created by reacting the amine function with the function of the remainder of (X).
[0130] This condensation is preferably carried out in the molten state.
[0131] To manufacture the composition, conventional mixing and / or extrusion techniques can be used. The components of the composition are thus mixed to form a compound which can optionally be granulated at the die exit. Advantageously, coupling agents are added during compounding.
[0132] To obtain a nanostructured composition, the polyamide graft and the core can be mixed in an extruder at a temperature generally between 200 and 300 °C. The average residence time of the molten material in the extruder can be between 5 seconds and 5 minutes, and preferably between 20 seconds and 1 minute. The yield of this condensation reaction is evaluated by selectively extracting the free polyamide grafts, i.e., those that have not reacted to form the grafted polyamide polymer.
[0133] The preparation of amine-terminated polyamide grafts and their addition to a polyolefin core containing the remainder of (X) is described in patents US3976720, US3963799, US5342886, and FR2291225. The grafted polyamide polymer of the present invention advantageously exhibits a nanostructured organization. To obtain this type of organization, grafts with a number molar mass (Mn) between 1000 and 5000 g / mol, and more preferably between 2000 and 3000 g / mol, are preferably used.
[0134] The particularly preferred polyamide grafted polymer contains the remainder of a carboxylic acid anhydride monomer, in particular a maleic anhydride monomer and polyamide 6 (PA6) grafts.
[0135] The grafted polymer comprises 5 to 50% by mass and preferably 15 to 30% by mass of polyamide grafts.
[0136] According to one embodiment, the grafted polyamide polymer has a melting temperature greater than 120°C.
[0137] Advantageously, the melting temperature of the support film is also higher than that of the adhesive layer, which provides thermomechanical stability to the structure. Preferably, the difference between the melting temperature of the support film and the melting temperature of the adhesive layer is between 30 and 60 °C.
[0138] According to one embodiment, the support film has a Melt Flow Index (MFI) of between 0.2 and 10 g / 10 min, preferably between 0.4 and 3 g / 10 min, and more preferably between 0.6 and 2 g / 10 min (230°C, 2.16 kg, ASTM D 1238).
[0139] According to another embodiment, the thickness of the support film is between 15 and 60 µm and is in particular around 20 µm.
[0140] As mentioned above, the support film can be in direct contact with a second adhesive layer so as to form a three-layer structure adhesive layer / support film / adhesive layer, the second adhesive layer being as defined above, identical or different from the first.
[0141] B. Method for preparing the multilayer structure
[0142] The multilayer structure according to the invention can be obtained from the mixtures intended for the adhesive layer and the support film by conventional techniques for making films, sheets or plates.
[0143] By way of example, one can cite the techniques of blown film extrusion, laminating extrusion, coating extrusion, flat film extrusion (also called cast film), or sheet extrusion. All these techniques are known to those skilled in the art, who will be able to adapt the implementation conditions of the different techniques (extruder temperature, fitting, dies and feedblock, screw rotation speed, cooling cylinder temperatures, etc.) to form the structure according to the invention having the desired shape and thickness. The invention would not depart from the final structure if it were obtained by pressing techniques, laminating with solvent- or aqueous adhesives, or if the final structure underwent an additional annealing step.
[0144] The multilayer structure is preferably prepared by coextrusion, in particular by flat film coextrusion.
[0145] During the co-extrusion of the two layers, the support film layer is generally heated to a higher temperature than the adhesive layer, so that their viscosities, at their respective temperatures, are as close as possible.
[0146] C. Use for the manufacture of a photovoltaic module
[0147] According to a second aspect, the invention relates to the use of a multilayer structure as defined above for the manufacture of a photovoltaic module.
[0148] The multilayer structure according to the invention is advantageous in this application because it greatly facilitates the assembly of the photovoltaic cell with the encapsulant and the upper (referred to as the "front-sheet") and rear (referred to as the "back-sheet") protective layers of the module. In particular, this structure is suitable for manufacturing modules as described in WO 2004 / 021455, which requires laminating the encapsulant directly to the surface of the interconnectors. Indeed, the good adhesion of the adhesive layer of the multilayer structure of the invention to the metal allows the interconnectors to be pre-laminated to the multilayer structure, thus simplifying the assembly of the photovoltaic module considerably.
[0149] It may be advantageous to use the multilayer structure according to the invention with coated interconnectors. In particular, the interconnectors can be coated with a material having a lower melting point than the adhesive layer, which facilitates soldering onto the photovoltaic cell.
[0150] In this use, it is particularly advantageous that the support film forms the protective layer on the back of the photovoltaic module called the "backsheet" of the photovoltaic module. D. Photovoltaic module
[0151] According to yet another aspect, the invention relates to a photovoltaic module comprising at least one multilayer structure as described above.
[0152] The multilayer structure can serve in particular as an encapsulant for at least one photovoltaic cell (10). The film supporting the multilayer structure can also, according to a preferred embodiment, serve as a protective layer on the back of the module (“back-sheet”) (26).
[0153] E. Method for manufacturing a photovoltaic module
[0154] According to yet another aspect, the invention relates to a method for preparing a photovoltaic module comprising a step of encapsulating at least one photovoltaic cell (10) with a multilayer structure as defined above.
[0155] The multilayer structure, more particularly its adhesive layer, is in direct contact with said photovoltaic cell (10), in particular with at least one electrical interconnector (18) linking two photovoltaic cells (12).
[0156] According to one embodiment, the encapsulation step of at least one photovoltaic cell (10) comprises the steps of:
[0157] i) bringing the adhesive layer (22) of the multilayer structure into contact with at least one electrical interconnector (18) at a temperature lower than the melting temperature of the adhesive layer (22), in particular 5 to 20°C lower than the melting temperature of the adhesive layer (22), classically at a temperature between 70 and 80°C, thereby obtaining at least one electrical interconnector (18) fixed to the surface of the adhesive layer of the multilayer structure;
[0158] ii) lamination of the multilayer structure fixing at least one electrical interconnector obtained in the previous step on the other components of the photovoltaic cell (10), in particular at a temperature between the melting temperature of the adhesive layer and the flow temperature of the backsheet, in particular between 140 and 160°C.
[0159] According to a particular embodiment, the electrical interconnectors (18) can be arranged on the surface of the adhesive layer (22) of the multilayer structure in the form of parallel wires or strips. They can be attached to the surface of the adhesive layer (22) by contact with the adhesive layer (22), which may have been heated to a temperature between 50 and 100 °C to make it sticky. The multilayer structure, incorporating the interconnectors (18), obtained in step i), can then be placed on the other components of the photovoltaic module, in particular the photovoltaic cells (10).
[0160] To facilitate the assembly of the module, the interconnectors can be coated with a polymer having a lower temperature than the adhesive layer.
[0161] Preferably, the peel force of the interface between the adhesive layer (22) and the metallic filaments used as electrical interconnectors (18) in the module is at least 0.1 N / cm, preferably at least 0.2 N / cm at an angle of 90°, at room temperature. EXAMPLES Materials used: Polyolefins A
[0162] A Affinity PL188OG: Ethylene-octene copolymer, marketed by Dow Chemicals
[0163] B EVA 1010 VN3: Ethylene-vinyl acetate copolymer, marketed by Total
[0164] C LDPE 1022 FN24: Linear low-density polyethylene, marketed by Total. Functionalized polyolefin.
[0165] Lotader® 3210: ethylene terpolymer, butyl acrylate and maleic anhydride, marketed by SK Functional Polyolefins Additives
[0166] - Adhesive masterbatch MB4 marketed by Arkema France: adhesion promoter for glass containing a silane - UVB Masterbatch: masterbatch containing a UV stabilizer
[0167] Apolhya Solar® LP91H3-UVB containing 80% by weight of polyolefin forming a core with maleic anhydride functions bonded to 20% by weight of polyamide 6 grafts. The product has a Melt Flow Index (MFI) of 0.5 g / 10 min at 230°C under 2.16 kg and a melting point of 216°C
[0168] Apolhya Solar® LC3-UV containing 80% by weight of trunk-forming polyolefin with maleic anhydride functions bound to 20% by weight of copolyamide 6.12 grafts. The product has a Melt Flow Index (MFI) of 10 g / 10 min at 230°C under 2.16 kg and a melting point of 130°C.
[0169] [Tables 1] Example 1 Example 2 Example 3 Adhesive layer (40 µm) Functionalized polyolefin 20% 20% 20% Polyolefin A 71% (A) 71% (B) 71% (C) Adhesive masterbatch MB4 5% 5% 5% Masterbatch UVB 4% 4% 4% Support film (30 µm) Apolhya Solar LP91H3-UV B Apolhya Solar LP91H3-UV B Apolhya Solar LP91H3-UV B Film composition according to examples 1 to 3 Film preparation
[0170] Films 70 µm thick were produced by flat film extrusion (CAST) on a Dr. Collin extrusion line. This extrusion line consists of three extruders equipped with a standard polyolefin screw profile, a variable feed block, and a 250 mm coat hanger die. The feed block allows the production of a two-layer film (Layer 1 / Layer 2) with a variable thickness distribution. EXAMPLES 1 to 3
[0171] The adhesive layer formulations were prepared by dry-blending a functionalized polyolefin and a polyolefin A as shown in Table 1 below. Films comprising an adhesive layer and a backing film were then prepared by co-extrusion as shown in Table 1 under the following conditions: - Adhesive layer extrusion temperature: 150°C, - Backing film extrusion temperature: 240°C, - Coextrusion head and die temperature: 220°C - Line speed: 6 m / min. EXAMPLE 4 (COMPARATIVE)
[0172] A film was prepared by co-extrusion as indicated in the preceding examples except that the functionalized polyolefin formulation and polyolefin A was replaced by Apolyha Solar LC3-UV. EXAMPLE 5 (COMPARATIVE)
[0173] A monolayer film of Apolhya Solar LP91H3-UVB was prepared by extrusion under the following conditions: - Extrusion temperature, co-extrusion head and die: 240°C, - Line speed: 6 m / min. Film rating
[0174]
[0175]
[0176]
[0177] The films were characterized by measuring the melting temperature of the adhesive layer, by DSC according to ISO11357-1 / -3. Furthermore, the adhesion between the films and the metal filaments used as connections for the photovoltaic modules was evaluated according to the following protocol: - 10 tin filaments with a diameter of 25 µm are placed side by side in such a way parallel to the contact with the adhesive layer of the films; - A weld is performed by pressing at 130°C under 5 bar for 2 seconds; and - The adhesion strength between the filaments and the film is evaluated using a Free-angle peel test, using a dynamometer in which the filaments are held by one jaw and the film by the other. The equilibrium force is measured during the propagation of delamination. The results of these evaluations are presented in Table 2 below. [Tables2] Ex 1 Ex 2 Ex 3 Ex 4 Ex 5 Melting point of adhesive layer (°C) 99 98 110 130 216 Peel force on filament (N) 0.25 0.39 0.12 <0.1 0 Film evaluation results
[0178] These results show that the multilayer structures according to the invention are characterized by a peel strength greater than those obtained with a structure whose adhesive layer does not comprise a combination of functional polyolefin and a polyolefin A as defined in the present invention, but rather a polyolefin grafted with polyamide grafts with a melting point of 130°C (Example 4) or monolayer structures (Example 5).
[0179] Furthermore, these results show that adhesive layer matrices with a melting point between 80 and 120°C make it possible to considerably increase adhesion to metallic filaments.
Claims
Claims
1. A multi-layer structure comprising an adhesive layer and a carrier film-forming layer in direct contact therewith, wherein (a) said adhesive layer comprises: - a polyolefin A chosen from a homopolymer of ethylene and a copolymer of ethylene and an α-olefin, a copolymer of ethylene and a vinyl ester of carboxylic acid, in particular a vinyl acetate (EVA) or a (co)polymer comprising methyl, ethyl, propyl, n-butyl, sec-butyl, isobutyl or tert-butyl (meth)acrylate units; and - a functionalized polyolefin, distinct from polyolefin A, comprising a polyolefin backbone containing a residue of at least one unsaturated monomer (Y), the residue of the unsaturated monomer (Y) being attached to the backbone by grafting or copolymerization; the melting temperature of the adhesive layer being between 80°C and 120°C, b) said support film comprises a polyamide grafted polymer comprising: - a polyolefin backbone, representing from 50% to 95% by mass of the polyamide graft polymer, containing a residue of at least one unsaturated monomer (X) and at least one polyamide graft, representing from 5% to 50% by mass of said polyamide graft polymer, in which: • the polyamide graft is attached to the polyolefin backbone by the remainder of the unsaturated monomer (X) comprising a function capable of reacting by a condensation reaction with a polyamide having at least one amine end and / or at least one carboxylic acid end, • the remainder of the unsaturated monomer (X) is fixed to the trunk by grafting or copolymerization, • the polyolefin trunk and the polyamide graft being chosen so that said grafted polymer polyamide has a flow temperature above 160°C, as measured by DSC according to ISO 11357-1:2016, ISO 11357-2:2020, ISO 11357-3:2018, said flow temperature being defined as the higher of the melting temperatures and the glass transition temperatures of the polyamide graft and the polyolefin backbone.
2. A multi-layer structure according to claim 1, wherein the melting temperature of said adhesive layer is between 90°C and 110°C.
3. A multilayer structure according to any preceding claim, wherein said adhesive layer has a Melt Flow Index (MFI), as measured according to ASTP D 1238 at 190°C under 2.16 kg, of between 0.2 and 10 g / 10 min, preferably between 0.4 and 3 g / 10 min, and in particular between 0.6 and 2 g / 10 min.
4. Multilayer structure according to one of claims 1 to 3, in which said adhesive layer comprises: - from 65% to 95% by weight of polyolefin A; - from 5 to 35% by weight of functional polyolefin; and - from 0 to 5% by weight of one or more additives.
5. Multilayer structure according to one of claims 1 to 4, wherein the thickness of said adhesive layer is between 20 and 60 pm.
6. Multilayer structure according to one of claims 1 to 5, wherein the thickness of said support film is between 5 and 40 μm.
7. Multilayer structure according to one of claims 1 to 6, in which the α-olefin comonomer of the polyolefin A of the adhesive layer is chosen from ethylene-propylene, ethylene-butene and ethylene-octene.
8. A multilayer structure according to one of claims 1 to 7, wherein the functional polyolefin of said adhesive layer is a polyolefin containing a residue of at least one unsaturated monomer (Y) which is a maleic anhydride.
9. Multilayer structure according to one of claims 1 to 8, wherein said support film has a Melt Flow Index (MFI), as measured according to ASTP D 1238 at 230°C under 2.16 kg, of between 0.2 and 10 g / 10 min, preferably between 0.4 and 3 g / 10 min, in particular between 0.6 and 2 g / 10 min.
10. Multilayer structure according to one of claims 1 to 9, characterized in that said support film carries said adhesive layer on one of its faces.
11. Multilayer structure according to one of claims 1 to 9, characterized in that said support film carries said adhesive layer on both of its faces.
12. A method of preparing a multilayer structure according to one of claims 1 to 11, wherein said support film is assembled to said adhesive layer by coextrusion.
13. Use of a multilayer structure according to one of claims 1 to 11 for the manufacture of photovoltaic modules.
14. A method of preparing a photovoltaic module, wherein a photovoltaic cell is encapsulated with a multilayer structure according to one of claims 1 to 11.
15. The method of claim 14, wherein the encapsulation comprises the steps of: i. attaching an electrically conductive filament to the surface of the adhesive layer of a multilayer structure according to one of claims 1 to 11 at a temperature below the melting temperature of the adhesive layer to form an assembly; ii. contacting said assembly with a photovoltaic cell at a temperature between the melting temperature of the adhesive layer and the flow temperature of the support film.
16. A photovoltaic module comprising a multilayer structure as defined in claims 1 to 11.