METHOD FOR CONTROLLING A HEATING STATION
By measuring and correcting the heating radiation power based on the preform's visible light absorption and infrared transmission, the method addresses the issue of inconsistent heating due to preform color, ensuring precise temperature control and preventing neck deformation in the container manufacturing process.
Patent Information
- Application Number
- FR2022014506
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-26
AI Technical Summary
The challenge in manufacturing containers from thermoplastic preforms is that the color of the preforms, whether intentional or unintentional, affects the temperature rise due to electromagnetic heating radiation, particularly in the visible light spectrum, leading to inconsistent heating and potential deformation of the neck region, which is not intended to be deformed during the forming process.
A method and installation for controlling the heating station by measuring the absorption spectrum of preforms in the visible light range and correcting the power of electromagnetic heating radiation based on the measured absorption and transmission factors, using a combination of devices to account for the preform's color and infrared transmission properties.
Ensures precise and consistent heating of the preform bodies to the desired temperature, preventing neck deformation and maintaining the quality of the forming process by accurately controlling the heating radiation power.
Smart Images

Figure 00000025_0000 
Figure 00000026_0000 
Figure 00000027_0000
Abstract
Description
Title of the invention: METHOD FOR CONTROLLING A HEATING STATION Technical field of the invention
[0001] The invention relates to a method for controlling a heating station of an installation for manufacturing containers by forming, in particular by stretch-blow molding, preforms made of thermoplastic material, the preforms being transported along a production path which passes through a heating zone in which the preforms are exposed to continuous spectrum heating electromagnetic radiation, said spectrum extending at least partly into the visible light range. Technical background
[0002] It is known to manufacture containers by forming, in particular by stretch-blow molding, preforms made of thermoplastic material. The material forming the preforms is generally in an amorphous state which is not suitable for cold forming. Prior to the forming operation, the preforms are therefore heated to a temperature greater than or equal to a glass transition temperature which allows them to be shaped into the final container.
[0003] More particularly, the preforms generally have a substantially cylindrical body of revolution with a thick tubular wall which is closed at one of its axial ends by a thick-walled bottom, and which is extended at its other end by a neck, also tubular. The neck is shaped to its final shape and dimensions while the body of the preform is intended to undergo relatively significant deformation to shape it into a container during a forming step.
[0004] For this reason it is preferable that only the body of the preform is heated to a set temperature which is higher than the glass transition temperature, the neck remaining at a temperature lower than said glass transition temperature to avoid its deformation during the manufacture of the container.
[0005] Furthermore, the set temperature must not exceed a crystallization temperature which is higher than the glass transition temperature. Beyond this crystallization temperature, the thermoplastic material crystallizes and no longer has the mechanical properties allowing for forming of the required quality.
[0006] The manufacture of containers in large series is carried out in a production facility in which the preforms travel along a predetermined production path. Each preform is taken care of by conveying means. Such a conveying means may be formed by a rail conveyor along which the preforms are free to come into contact with each other or a conveyor which has members for gripping each preform individually.
[0007] The production facility comprises a heating station which, during a heating step, makes the body of the preform malleable by heating to the set temperature. During the heating step, each preform is exposed to heating radiation as it moves. The power of the heating radiation is controlled so as to make it possible to heat the body of the preforms to the set temperature.
[0008] The production installation also comprises a forming station which is arranged downstream of the heating station according to the direction of circulation of the preforms in the production installation. During the forming step, the hot preform is placed in a forming unit, for example in a mold of the forming station which has a molding impression conforming to the container to be obtained. A pressurized fluid, such as air, is then injected into the malleable body of the preform in order to press the wall against the mold impression. Generally, the injection of pressurized fluid is preceded and / or accompanied by axial stretching of the preform, in particular by means of a stretching rod inserted into the preform. In a known manner, the body is thus subjected to biaxial stretching.
[0009] During its passage through the heating station, each preform is generally exposed to continuous spectrum heating radiation which heats the thermoplastic material. The temperature to which the preforms are heated generally depends on the absorption factor (A) of the preform for the wavelengths of the heating radiation. The absorption factor (A) is sometimes referred to by its English name of “absorptance”.
[0010] The absorption factor (A) is defined as the ratio between the absorbed heating radiation flux and the incident heating radiation flux. The absorbed heating radiation flux causes a rise in temperature of the thermoplastic material making up the preform. The absorption factor (A) of the preform thus makes it possible to know the rise in temperature of a preform as a function of the intensity of the infrared radiation and the duration of exposure to said radiation. Less energy is required to heat a preform having a high absorption factor (A) compared to a preform having a lower absorption factor (A).
[0011] The absorption factor (A) can be deduced from two other parameters called the transmission factor (T) of the preform as well as its reflection factor (R).
[0012] The transmission factor (T), sometimes called “transmittance”, is defined as the ratio between the flux of heating radiation transmitted through at least one wall of the preform and the flux of incident heating radiation.
[0013] The reflection factor (R), also called reflectance, is defined as the ratio between the heating radiation flux reflected by the preform and the incident heating radiation flux. The reflectance (R) is for example calculated as a function of the refractive index (n) of the thermoplastic material according to the following formula: Æ = [(n- !) / (« + 1)]2
[0014] in which the value “1” corresponds to the refractive index of air.
[0015] These three factors depend on the wavelength of the radiation considered.
[0016] The heating radiation extends at least partly into the near infrared range, since it is known that thermoplastic materials, such as PET, absorb this type of radiation very easily. The wavelength considered to define the transmission factor of the preform is therefore generally taken in the near infrared range.
[0017] These three factors are linked together by the following equation: A=1RT
[0018] The transmission factor depends on the wavelength of the radiation passing through it. Thus, a perfectly transparent preform has a transmission factor close to 100% for wavelengths in the visible light range, while it has a significantly lower transmission factor for radiation having a wavelength in the near infrared range. This reflects the fact that the preform can be heated by radiation belonging to the near infrared range, while radiation in the visible light range will have only a negligible influence on the temperature of the preform even at high powers.
[0019] It happens that the preforms are made of a material having a tint.
[0020] This tint can be obtained intentionally by adding colorant to dye the preform in a desired color in order to obtain a colored container.
[0021] This tint can also be experienced involuntarily and uncontrolled, for example when the preform is made of a plastic material consisting at least in part of recycled plastic material. This is for example the case when the preform is made of recycled polyethylene terephthalate (rPET). In this case, the preform has a more or less dark tint depending on the quality and quantity of recycled material incorporated in the composition of the thermoplastic material which constitutes it.
[0022] The inventor has found that in these two cases, the color of the plastic material is likely to influence the temperature of the wall of the preform when it is exposed to heating radiation.
[0023] Indeed, the heating radiation has a spectrum which extends at least in part in the visible light range. However, when the preform has a color, and in particular a dark color, this part of the heating radiation spectrum is likely to significantly heat the thermoplastic material. Summary of the invention
[0024] The invention proposes a method for controlling a heating station of an installation for manufacturing containers by forming, in particular by stretch-blow molding, preforms made of thermoplastic material, the preforms being transported along a production path which passes through a heating zone in which the preforms are exposed to continuous spectrum heating electromagnetic radiation, said spectrum extending at least partly into the visible light range,
[0025] characterized in that the method comprises: - a first step of measuring the absorption spectrum of a wall of a preform in the visible light range in a measurement zone crossed by the production path upstream of the heating zone; - a second step of controlling the power of the heating electromagnetic radiation according to the absorption spectrum measured during the first step to heat the body of the preforms to a set temperature.
[0026] According to another characteristic of the method carried out according to the teachings of the invention, the second control step comprises a first sub-step of calculating a corrected power of the heating electromagnetic radiation as a function of the absorption spectrum measured during the first step, and a second sub-step of controlling the power of the heating electromagnetic radiation to said corrected power calculated during the first sub-step.
[0027] According to another characteristic of the method carried out according to the teachings of the invention, during the first calculation sub-step, the measured absorption spectrum is used to calculate the parameters of the wall of the preform in a determined chromatic space equivalent to the CIELAB chromatic space as defined by the ISO 11664-4: 2019 standard.
[0028] According to another characteristic of the method carried out according to the teachings of the invention, the corrected power is calculated during the first sub-step at least as a function of the value of a parameter representative of the luminance of the wall in the determined chromatic space.
[0029] According to another characteristic of the method carried out according to the teachings of the invention, the corrected power is calculated as a function of a rate of said parameter which is calculated according to the following equation: A PÜP
[0030] in which Pq represents a reference value of the parameter and p represents the parameter calculated from the absorption spectrum measured during the first step.
[0031] According to another characteristic of the method carried out according to the teachings of the invention, the corrected power is calculated as a function of the proportion of the power of the heating electromagnetic radiation extending into the range of visible light.
[0032] According to another characteristic of the method carried out according to the teachings of the invention, the heating radiation extends at least partly in the near infrared range and in that it comprises a fourth step of measuring an infrared transmission factor of a wall of said preform for at least one wavelength belonging to the near infrared range, this fourth step being carried out prior to the first calculation sub-step.
[0033] According to another characteristic of the method carried out according to the teachings of the invention, the corrected power is calculated as a function of a transmission rate which is calculated according to the following equation: a 7>2W2) A 1 (
[0034] in which T0(À2) represents a reference infrared transmission factor value and 7ïz2) represents the infrared transmission factor measured during the fourth step.
[0035] According to another characteristic of the method carried out according to the teachings of the invention, the corrected power is calculated as a function of the proportion of the power of the heating electromagnetic radiation extending into the near infrared range.
[0036] The invention also relates to an installation for implementing the method, the installation comprising means for conveying preforms in a row along a predetermined production path passing successively through a heating zone of a body of the preforms and through a station for forming the preforms into a container, in particular by stretch-blow molding,
[0037] characterized in that the installation comprises a device for measuring the absorption spectrum in the visible light range of at least one wall of the preforms as they pass through an associated measurement zone.
[0038] According to another characteristic of the installation produced according to the teachings of the invention, the absorption spectrum measuring device comprises: - a first light source which emits a first light beam according to a continuous spectrum which extends at least into the visible range, - a spectrometer measuring the intensity and wavelength of the first light beam after passing through at least one thickness of the preform wall.
[0039] According to another characteristic of the installation produced according to the teachings of the invention, it comprises a device for measuring the infrared transmission factor of at least one wall of the preforms as they pass through an associated measurement zone.
[0040] According to another characteristic of the installation produced according to the teachings of the invention, the device for measuring a value representative of the infrared transmission factor comprises: - a light source which emits a light beam having at least a second wavelength in the near infrared range, - a measuring member measuring the intensity for at least one second wavelength of said light beam after having passed through at least one thickness of the wall of the preform.
[0041] According to another characteristic of the installation produced according to the teachings of the invention, the first light beam emitted by the first light source has a continuous spectrum which comprises said at least one second wavelength.
[0042] According to another characteristic of the installation produced according to the teachings of the invention, the device for measuring a value representative of the infrared transmission factor comprises a second light source which is distinct from the first light source and which emits a second light beam having at least a second wavelength in the near infrared range.
[0043] According to another characteristic of the installation produced according to the teachings of the invention, the first light beam and the second light beam pass through the wall of the preform at the same height.
[0044] According to another characteristic of the installation produced according to the teachings of the invention, the first light beam and the second light beam are merged into a common beam before reaching the preform.
[0045] According to another characteristic of the installation produced according to the teachings of the invention, the measurement of the infrared transmission factor and the measurement of the absorption spectrum are carried out simultaneously in the same measurement zone of the production path.
[0046] According to another characteristic of the installation produced according to the teachings of the invention, the measuring member of the device for measuring the infrared transmission factor and the spectrometer of the device for measuring the absorption spectrum are formed by a single spectrometer common to the two devices. Brief description of the figures
[0047] Other characteristics and advantages of the invention will appear during the reading of the detailed description which follows for the understanding of which one refers will refer to the attached drawings briefly described below.
[0048] [Fig.l] is a top view which schematically represents a container manufacturing installation produced according to the invention comprising a heating station.
[0049] [Fig.2] is a side view showing a preform intended to be processed by the installation of [Fig.l].
[0050] [Fig.3] is a vertical cross-sectional view along section plane 3-3 of the [Fig.l] which represents a device for measuring an absorption spectrum in the visible light range of the walls of a preform circulating in the installation produced according to a first embodiment.
[0051] [Fig.4] is a block diagram which represents a method of implementing the installation of [Fig.l] for controlling the heating station according to a first embodiment of the invention.
[0052] [Fig.5] is a diagram showing luminous intensity values on the ordinate and wavelength values on the abscissa, which represents in broken lines the spectrum of a first light beam emitted by a light source of the device of [Fig.3] and which represents, in continuous lines, the absorption spectrum of the wall of the preform.
[0053] [Fig.6] is a block diagram similar to that of [Fig.4] which represents a method of implementing the installation of [Fig.l] for controlling the heating station according to a second embodiment of the invention.
[0054] [Fig.7] is a vertical cross-sectional view along section plane 3-3 of the [Fig.l] which represents a device for measuring an absorption spectrum in the visible light range combined with a device for measuring an infrared transmission factor of the walls of a preform circulating in the installation produced according to a second embodiment.
[0055] [Fig.8] is a diagram similar to that of [Fig.5] which represents in lines in interrupted the spectrum of a light beam emitted by two light sources of the device of [Fig.7] and which represents, in a continuous line, the absorption spectrum of the wall of the preform as well as the beam transmitted in the near infrared range. Detailed description of the invention
[0056] In the remainder of the description, the terms "top", "bottom", and the derived terms "high", "low", are used for the sake of clarity with reference to the orientation of the figures without this having any limiting scope.
[0057] In the remainder of the description, the wavelengths of the light radiation will be expressed in nanometers, indicated by the abbreviation “nm”.
[0058] In theory, a monochromatic source is an ideal source emitting a sinusoidal wave of single frequency. In other words, its frequency spectrum consists of a single line of zero spectral width (Dirac).
[0059] In practice, such a source does not exist, a real source having a frequency emission spectrum which extends over a band of low but non-zero spectral width, for example of a few tens of nanometers, centered on a main frequency where the intensity of the radiation is maximum.
[0060] In the remainder of the description, such a real source is considered to be monochromatic.
[0061] Subsequently, an absorption spectrum is defined as being a curve which represents the value of the intensity of a light beam with a continuous spectrum as a function of the wavelength after its passage through a medium to be analyzed, in particular the wall of a preform.
[0062] [Fig. 1] schematically illustrates an installation 10 for the manufacture of containers 11 from preforms 12 made of thermoplastic material and more particularly of PET (polyethylene terephthalate) or rPET (recycled polyethylene terephthalate). The thermoplastic material may optionally contain, but not necessarily, additives which artificially increase the absorption factor of the preform, or even a dye to change its color.
[0063] As shown in [Fig. 2], each preform 12 comprises a cylindrical body 14 with axis “X”. The body 14 comprises a transparent lateral wall 16 which delimits an interior volume. The wall 16 has a shape of revolution around the axis “X” so that at a given height, the wall 16 has a constant thickness. However, the thickness of the wall 16 is likely to vary depending on the height. The wall 16 is delimited by an external face 18 which is turned towards the outside of the preform 12 and by an internal face 20 which is turned towards the interior volume.
[0064] An upper end of the body 14 opens out through a neck 22. The neck 22 has the final shape of that of the container 11 to be obtained. As a result, the neck 22 does not undergo the slightest deformation during the manufacture of the container 11. The body 14 has a bottom 24 which closes its lower end and whose shape is generally hemispherical. The neck 22 has a collar 26 arranged at its junction with the body 14. The lower face of the collar 26 is intended to form a support surface 28 to allow the preform 12 to be supported during its molding and / or during its transport.
[0065] At the end of their injection molding, the preforms 12 are cooled abruptly to give the thermoplastic material an amorphous state. It is thus possible to make the thermoplastic material malleable again by heating beyond a glass transition temperature.
[0066] Referring again to [Fig. 1], the manufacturing facility 10 comprises a heating station 30 and a forming station 32. The preforms 12 move in a line along a production path 34 which passes through the heating station 30 and the forming station 32. The direction of movement of the preforms 12 is indicated by the arrows "F1" in [Fig. 1]. During normal operation of the manufacturing facility 10, the preforms 12 are in constant movement along the production path 34.
[0067] The heating station 30 has the function of heating the body 14 of the preforms 12 to a set temperature which is greater than or equal to the glass transition of the constituent material, for example greater than 70°C when this material is PET or rPET. The heating station 30 comprises a conveyor 36 (illustrated schematically) for transporting the preforms 12 by rotating them on themselves.
[0068] The conveyor 36 generally comprises mandrels (not shown) which are fitted with the neck 22 to transport the preforms 12. The mandrels move along a closed circuit. The mandrels are for example carried by the links of a chain or by independent shuttles moving along a rail.
[0069] The circuit here comprises two parallel rectilinear sections connected by 180° turning sections. The conveyor 36 further comprises two wheels 38A, 38B for guiding the mandrels in the turning portions of the closed circuit.
[0070] The heating station 30 also comprises heating means 40 for heating the preforms 12. These are, for example, lamps facing reflectors which emit continuous spectrum heating electromagnetic radiation.
[0071] The heating radiation extends at least partly in the near infrared range which is included in a wavelength range between 780 nm and 3000 nm. The intensity of the heating electromagnetic radiation is particularly higher in a higher intensity wavelength range between 800 nm and 1600 nm.
[0072] The heating radiation also extends at least partly into the visible light range which is generally between 380 nm and 780 nm.
[0073] The spectrum of the heating radiation extends for example between 300 nm and 3000 nm.
[0074] The heating means 40 are arranged along a heating zone 42 of the preform production path 34. In the example shown in [Fig.l], the heating station 30 comprises a heating zone 42 divided into two parts arranged upstream and downstream of the turning portion guided by the guide wheel 38B.
[0075] The preforms 12 entering the heating station 30 are taken over individually by the conveyor 36 on which they complete a U-shaped section of their production path 34 passing through the heating zone 42. They are heated as they pass by the heating means 40, which, where appropriate, are placed on one side or on either side of the preforms 12 relative to their direction of travel. The hot preforms 12 are extracted from the heating station 30 after their passage through the heating zone 42 and transferred into molds of the forming station 32 by a first transfer device 44, such as a transfer wheel, interposed between the heating station 30 and the forming station 32.
[0076] The transfer wheel comprises arms (not shown, as they are known per se) which successively grip the preforms 12, as they leave the heating station 30, at the level of their neck 22, to introduce each of them in turn into a mold 46 of the forming station 32. The forming station 32 comprises a rotating carousel 48 at the periphery of which several blowing stations 50 are arranged.
[0077] Each blowing station 50 comprises at least one mold 46 which defines a cavity having the imprint of the container 11. Each blowing station 50 comprises means (not shown) for forming, deforming the body 14 of the preform 12 and pressing it against the imprint of the mold 46, for example by stretch-blow molding.
[0078] Each hot preform 12 leaving the heating station 30 is introduced into a mold 46 of the blowing station 50 to be blown there and transformed into a container 11. Once completed, the container 11 is extracted from the blowing station 50 by a second transfer device 52, similar to the first transfer device 34.
[0079] Generally, the heating means 40 emit the heating radiation at a power determined solely as a function of the absorption factor of the preforms 12 in the near infrared range in order to reach the set temperature. This power is calculated by considering that the preform 12 has walls 16 that are perfectly transparent in the visible light range.
[0080] To enable the preforms 12 to be heated as close as possible to the set temperature, the invention proposes a method for controlling the heating station 30 which consists of measuring an absorption spectrum “o(Xl)” of the wall 16 of the preform 12 in the visible light range in a measurement zone “Z” crossed by the production path 34 upstream of the heating zone 42, then controlling the power of the heating electromagnetic radiation as a function of the measured absorption spectrum “o(Xl)”.
[0081] This process is implemented here automatically by an electronic control unit 54, visible in particular in [Fig.3].
[0082] This method is implemented when the preform 12 is transported by a conveyor along the production path 34 in the installation 10 for manufacturing containers 11. Preferably, the preform 12 is in constant movement during the implementation of the method.
[0083] In the examples shown in the figures, the method is implemented when the preforms 12 are transported by the conveyor 36 of the heating station 30. This conveyor 36 transports the preforms 12 through to the heating zone 42.
[0084] The method is preferably implemented on the preforms 12 before they are heated, therefore upstream of the heating zone 42.
[0085] As shown in [Fig.4], the method thus comprises a first step “El” of measuring the absorption spectrum “o(Xl)” of the wall 16 of a preform 12 in the visible light range.
[0086] The first step “El” of measuring the absorption spectrum “o(Xl)” is carried out here by measuring the attenuation of the intensity “I” of a first light beam 55 with a continuous spectrum “oO” in the visible range for each of the wavelengths of the spectrum “oO”.
[0087] The first light beam 55 is a beam of so-called “white” light which emits in the visible light range, that is to say generally between 380 nm and 780 nm. For example, the spectrum “oO” of the first light beam 55 extends in a wavelength range “XI” which extends between a lower limit “XI-min”, for example equal to 400 nm, and an upper limit “XI-max”, for example equal to 700 nm. The spectrum “oO” of the first light beam 55 is represented by a curve in broken lines in [Fig.5].
[0088] For this purpose, the installation 10 comprises a device 56 for measuring the absorption spectrum “o(Xl)” in the visible light range. As represented in [Fig.5] by a solid line curve, this device 56 is arranged to measure the absorption spectrum “o(Xl)” of a preform 12 passing through the measurement zone “Z” represented in [Fig.l].
[0089] As shown in [Fig. 3], the device 56 for measuring the absorption spectrum “o(Xl)” in the visible light range comprises a first light source 58 which emits the first light beam 55 with a continuous spectrum “oO”.
[0090] The first light source 58 comprises, for example, a light-emitting diode (LED), a superluminescent diode (SLED) or a lamp. The first light beam 55 is emitted perpendicular to the wall 16 of the preform 12. The first light beam 55 is emitted so as to pass through the preform 12 via its main “X” axis.
[0091] The first light beam 55 is more particularly emitted along an axis which is perpendicular to a tangent to the production path 34 of the preform 12 in the measurement zone “Z”.
[0092] The first light beam 55 passes through the wall 16 at a determined height “h”.
[0093] The first light beam 55 can be guided in the right direction by a optical guiding means such as an optical fiber 60.
[0094] The device 56 for measuring the absorption spectrum “o(Xl)” in the visible light range further comprises a spectrometer 62 which measures the intensity “I” in function of the wavelength “XI” of the spectrum “oO” of the first light beam 55 after having passed at least once through the wall 16 of the body 14 of the preform 12, as shown in [Fig.5].
[0095] The spectrometer 62 is here arranged so as to measure the intensity “I” of the first light beam 55 on the other side of the preform 12 relative to the axis “X” of the preform 12 after it has passed twice through the wall 16 at two diametrically opposite points, at the same height “h” of the preform 12.
[0096] In a variant of the invention not shown, the spectrometer is arranged so as to measure the intensity of the first light beam after it has passed through the wall of the preform once. In this case, a member for intercepting the light beam is introduced into the preform during the first step, the interception member guiding the intercepted light beam to the spectrometer.
[0097] The spectrometer 62 thus makes it possible to obtain the measured absorption spectrum “o(Xl)” represented in [Fig.5].
[0098] As shown in [Fig.4], the method further comprises a second step “E2” of controlling the power of the heating electromagnetic radiation as a function of the absorption spectrum “o(Xl)” measured during the first step “El”. This second control step “E2” is implemented by the electronic control unit 54 which receives the data measured by the spectrometer 62.
[0099] The second control step “E2” comprises a first sub-step “E2-1” for calculating a corrected power “Ptc” of the heating electromagnetic radiation as a function of the absorption spectrum “o(X 1 )” measured during the first step “El”. This corrected power “Ptc” corresponds to the power actually required to heat the preform 12 to the set temperature, taking into account the influence of the color of the preform 12.
[0100] During this first calculation sub-step “E2-1”, the measured absorption spectrum “o(Xl)” is used to calculate the parameters of the color of the wall 16 of the preform 12 in a determined chromatic space.
[0101] As a non-limiting example, such a color space is here formed by the CIELAB color space as defined by the ISO 11664-4:2019 standard, sometimes referred to as “L*a*b* CIE 1976”.
[0102] In a variant of the invention not shown, the determined color space may be another standardized color space equivalent to the CIELAB space such as the CIE RGB color space, defined by the ISO 61966-2-1:2003 standard, or the CIE XYZ color space, defined by the 11664-3:2019 standard, or the CIE 1976 L*u*v* color space, defined by the ISO 1164-5:2016 standard, or the CIE U'V'W' color space. A color space is “equivalent” to the CIELAB space when there is a bijection that allows passage from one space to the other. easily.
[0103] Three parameters characterize the colors in the CIELAB color space. The lightness L* derives from the luminance. The two parameters a* and b* express the deviation of the color from that of a gray surface of the same lightness. A gray, uncolored, achromatic surface is illuminated by a reference light which is here determined as being the standardized daylight D65 according to the ISO 23603:2005 standard.
[0104] The parameters of the L*a*b* system are thus: - the clarity L* which takes values between 0, corresponding to black, to 100, corresponding to white; - a* represents the value on an axis going from green to red; - b* represents the value on an axis going from blue to yellow.
[0105] According to ISO 11664-4:2019, the various parameters are calculated based on the transmission factor T(X1) for each associated wavelength.
[0106] More particularly, the luminous intensity “10” of emission at which the first light beam 55 is emitted as a function of the wavelength “X1” is a known datum. The luminous intensity “10” at which the first light beam 55 is emitted can also be measured directly by the spectrometer 62 when no preform 12 passes into the measurement zone “Z”, as represented by the curve in broken lines in [Fig.5].
[0107] After passing twice through the wall 16 of the preform 12, the light intensity of the first light beam 55 is attenuated. The first light beam 55 then has a light intensity called “transmitted light intensity “Il”, as represented by the solid line curve in [Fig.5].
[0108] Thus, it is easy to deduce the transmission factor of the wall 16 of the preform as a function of the wavelength in the visible light range by calculating the ratio between the emission light intensity “10” and the transmitted light intensity “11”.
[0109] Each parameter in the determined color space, such as the CIELAB space, is then calculated as a function of the transmission factor T(X1) and the associated wavelength “XI”.
[0110] The corrected power “Ptc” is calculated during the first sub-step at least as a function of at least one parameter of the determined chromatic space, such as a parameter representative of the luminance of the wall 16. The corrected power “Ptc” is more particularly calculated as a function of a rate of said parameter “Ap” which is calculated according to the following equation: A POP ^P~ P()
[0111] in which Pq represents a reference value of the parameter and p represents the parameter calculated from the absorption spectrum “o(Xl)” measured during the first step “El”.
[0112] According to an exemplary embodiment, the corrected power “Ptc” is calculated during the first sub-step at least as a function of the lightness parameter “L*” of the CIELAB color space. The corrected power “Ptc” is more particularly calculated as a function of a lightness rate “AL*” which is calculated according to the following equation: AL — L
[0113] in which £* represents a reference clarity value and L* represents the clarity calculated from the absorption spectrum “o(Xl)” measured during the first step “El”.
[0114] The reference value is for example the value of the parameter, here the clarity, which corresponds to the specifications of a preform 12, called the reference preform 12. It may also be said parameter, here the clarity, of a preform 12 taken as a sample from the batch of preforms 12 which must be treated by the installation 10, or even the average of the values of said parameter, here the clarity, of a sample of several preforms 12 taken from the batch of preforms 12 which must be treated.
[0115] The rate of said parameter “Ap”, for example the clarity rate “AL*”, is thus likely to vary between 0, for a preform 12 having the same value as the reference preform 12, and 1.
[0116] The corrected power “Ptc” is also calculated based on the proportion of the power of the heating electromagnetic radiation extending into the visible light range. In fact, the heating electromagnetic radiation extends here into the visible light range and, for the most part, into the near infrared range.
[0117] Thus, the total power of the heating electromagnetic radiation can be formulated as follows: PtO = PnirO + PvisO
[0118] in which PtO represents the total instantaneous power of the heating electromagnetic radiation for heating the reference preform 12 to the set temperature, PnirO represents the instantaneous power of the heating electromagnetic radiation emitted in the near infrared range, and PvisO represents the instantaneous power of the heating electromagnetic radiation emitted in the visible light range.
[0119] The corrected power “Ptc” of the heating electromagnetic radiation is then calculated according to the following equation: Ptc = PnirO + FwaOXI-J / ?)
[0120] In the case of using the AL* clarity rate to calculate the corrected power "Ptc" of the heating electromagnetic radiation, the equation becomes: Ptc = PnirG + FvwO.(l- AL*}
[0121] Preferably, but not necessarily, to prevent the power of the heating radiation from changing too chaotically and quickly depending on the different values measured for each preform 12, the corrected power “Ptc” is calculated by taking into account the measurement of said parameter, in particular of the clarity, for several successive preforms 12. The number of preforms 12 is for example equal to the number of preforms likely to be contained simultaneously in the heating zone 42. This is a sliding average which is updated for each new preform 12 received in the measurement zone “Z”.
[0122] During a second sub-step “E2-2” of controlling the second step “E2”, the power of the heating electromagnetic radiation is controlled according to the correction value calculated during the first sub-step “E2-1” to heat the body 14 of the preforms 12 to the set temperature, taking into account the color of the preforms 12.
[0123] According to a second embodiment of the invention shown in [Fig. 6], to enable the power of the heating radiation to be controlled as best as possible, the method described above further comprises a fourth step “E4” of measuring an infrared transmission factor “T(X2)” of the wall 16 of said preform 12 for at least one wavelength “PI” belonging to the near infrared range. This makes it possible in particular to take into account the variation in the infrared transmission factor “T(X2)” of the preforms 12 within the same batch of preforms 12 to be treated in the second step “E2” of the method and in particular in the first sub-step “E2-1” of calculating the corrected power “Ptc”.
[0124] This fourth step “E4” is carried out prior to the first sub-step “E2-1” of calculation. It can be carried out before, after or during the first step “El” of measurement.
[0125] The fourth step “E4” of measuring the infrared transmission factor “T(X2)” is here carried out by measuring the attenuation of the intensity “I” of a second light beam 66 which comprises a second predetermined wavelength “PI”. The second predetermined wavelength “PI” is included in the near infrared range. It preferably belongs to the range of wavelengths of highest intensity of the heating electromagnetic radiation, here between 800 nm and 1600 nm.
[0126] It can also be a range of wavelengths belonging to the near infrared for each of which the transmission factor is measured.
[0127] For this purpose, the installation 10 comprises a device 64 for measuring the infrared transmission factor “T(X2)” shown in [Fig.7]. As shown in [Fig.l], this device 64 is arranged to measure the infrared transmission factor “T(X2)” of a preform 12 passing through said measurement zone “Z”.
[0128] The device 64 for measuring the infrared transmission factor “T(X2)” comprises a second light source 68 which emits the second light beam 66 having the second wavelength “ / .2”. It may be a monochromatic light source, but this is not obligatory.
[0129] The second light source 68 comprises, for example, a light-emitting diode (LED), a superluminescent diode (SLED) or a lamp. The second light beam 66 is emitted perpendicular to the wall 16 of the preform 12. The second light beam 66 is emitted so as to pass through the preform 12 via its main “X” axis.
[0130] The second light beam 66 passes through the wall 16 at said height “h”. Thus, the first light beam 55 and the second light beam 66 pass through the wall 16 of the preform 12 at the same height “h”.
[0131] The second light beam 66 is more particularly emitted along an axis which is perpendicular to a tangent to the production path 34 of the preform 12 in the measurement zone “Z”.
[0132] The second light beam 66 can be guided in the correct direction by an optical guiding means such as an optical fiber.
[0133] The device 64 for measuring the infrared transmission factor “T(X2)” further comprises a member for measuring the intensity “I” of the second light beam 66 after having passed through the wall 16 of the body 14 of the preform 12 at least once.
[0134] The intensity measuring member “I” is here arranged so as to measure the intensity “I” of the second light beam 66 on the other side of the preform 12 relative to the axis “X” of the preform 12 after it has passed twice through the wall 16 at two diametrically opposite points, at the same height “h” of the preform 12.
[0135] In this configuration, it is preferable to choose the second predetermined wavelength “ / .2” from a range of wavelengths for which the thermoplastic material is sufficiently transparent so that the intensity “I” of the second light beam 66 after having passed through the wall 16 twice can be measured with sufficient precision and certainty by the measuring member. Indeed, the intensity “I” of the second light beam 66 would risk being too attenuated after two passages through the wall 16 if it were emitted at a wavelength easily absorbed by the thermoplastic material.
[0136] For example, in the case of a plastic material made of PET or rPET, the second wavelength “ / .2” is in the ranges between 800 nm and 1100 nm, or between 1250 nm and 1300 nm. The second wavelength “ / .2” is for example chosen from the following values: 850 nm, 860 nm, 880 nm, 940 nm, 950nm, 960nm, 980nm, 1050nm or 1300nm.
[0137] In a variant of the invention not shown, the intensity measuring member is arranged so as to measure the intensity of the second light beam for said second wavelength after it has passed through the wall of the preform only once. In this case, the measuring member comprises a member for intercepting the second light beam which is introduced into the preform during the first step, the interception member guiding the intercepted second light beam to an intensity measuring member.
[0138] The second wavelength “ / .2” of the second light beam 66 is here outside the wavelength range “XI” of the first light beam 55.
[0139] The measuring member is here formed by a spectrometer measuring the intensity “I” and the second wavelength “ / .2” of the second light beam 66 after having passed through at least one thickness of the wall 16 of the preform 12.
[0140] The emission light intensity “10” at which the first light beam 66 is emitted is a known datum. The light intensity “10” at which the second light beam 66 is emitted can also be measured directly by the measuring member 62 when no preform 12 passes into the measurement zone “Z”, as shown in broken lines in [Fig.8].
[0141] After having passed through the wall 16 of the preform 12 twice, the light intensity of the second light beam 66 is attenuated. The second light beam 66 then has a light intensity called “transmitted light intensity”.
[0142] Thus, it is easy to deduce the infrared transmission factor “T(X2)” as a function of the ratio between the emission luminous intensity “10” and the transmitted luminous intensity “12”.
[0143] Optionally, to precisely calculate the infrared transmission factor “T(X2)”, it is possible, but not obligatory, to weight this ratio here by taking into account the quantity of the second light beam 68 which is reflected at each entry into a wall 16. This reflected quantity is calculated as a function of the reflectance factor “R” which is a previously known quantity.
[0144] The weighting factor for the passage of the second light beam 66 through a wall thickness 16 is calculated according to the following equation: F = (W 1 1-A
[0145] The weighting factor for the passage of the second light beam 66 through two wall thicknesses 16 is calculated according to the following equation: £ __ 1
[0146] The infrared transmission factor “T(X2)” when passing through two wall thicknesses 16 is thus calculated by applying the following equation:
[0147] The infrared transmission factor “T(X2)” is calculated by the electronic control unit 54 which receives the measurements made by the measuring device.
[0148] Advantageously, the measurement of the representative value of the infrared transmission factor “T(X2)” and the measurement of the absorption spectrum “o(Xl)” of the wall 16 are carried out simultaneously in the same measurement zone Z of the production path 34.
[0149] To do this, the device 56 for measuring the absorption spectrum “o(Xl)” in the visible light range and the member for measuring the infrared transmission factor “T(X2)” are here arranged in the common measurement zone “Z”, as shown in [Fig.7].
[0150] Very advantageously, the spectrometer of the device 56 for measuring the absorption spectrum “o(Xl)” in the visible light range and the spectrometer of the device 64 for measuring the infrared transmission factor “T(X2)” are formed by a single spectrometer 70 common to the two devices 56, 64.
[0151] For this purpose, the first light beam 55 and the second light beam 66 are merged into a common beam 72 before reaching the preform. This merging is for example carried out by means of an optical coupler 74. Thus, the spectrum of the common beam 72 has a continuous portion in the visible light range, and a peak for the value of the second wavelength “ / .2” as represented by the curve “oO” in broken lines in [Fig.8].
[0152] In a variant not shown, the first light beam 55 emitted by the first light source 58 has a continuous spectrum which includes said at least one second wavelength “ / .2”. In this case, the first light beam 55 alone makes it possible to carry out the two measurements simultaneously and the second light source is not necessary. The common spectrometer 72 makes it possible to obtain the two measurements simultaneously from the first light beam 55 alone. Such a first light source 58 is for example formed by a halogen lamp.
[0153] The spectrum measured by the common spectrometer 70 after the common beam 72 has passed through the wall 16 is shown in a continuous line in [Fig.8]. It simultaneously presents the absorption spectrum o(Xl) and the intensity peak “12” for the second wavelength “ / .2”.
[0154] The common light beam 72 is emitted perpendicular to the wall 16 of the preform 12 so as to pass through the wall 16 via its main axis “X”.
[0155] The common light beam 72 is more particularly emitted along an axis perpendicular to a tangent to the trajectory of the preform 12 in the common measurement zone “Z”.
[0156] The common light beam 72 passes through the wall 16 at said height “h”.
[0157] In a variant of the invention not shown, the spectrum measuring device 56 "o(Xl)" absorption in the visible light range and the device 64 for measuring the infrared transmission factor "T(X2)" are arranged in two separate measurement zones of the production path so that the two corresponding measurements are carried out successively on the same preform. In this case, each of the devices comprises a light source and an associated spectrometer.
[0158] The second control step “E2” comprises the first calculation sub-step “E2-1” as described in the first embodiment.
[0159] This first sub-step “E2-1” uses the same calculations as described in the first embodiment, but it is supplemented by taking into account the infrared transmission factor “T(X2)” measured during the fourth step “E4” for the calculation of the corrected power “Ptc” of the heating electromagnetic radiation.
[0160] According to an exemplary embodiment, the corrected power “Ptc” is also calculated during the first sub-step “E2-1” as a function of the measured infrared transmission factor “T(X2)”. The correction value is more particularly calculated as a function of a transmission rate “AT(X2)” which is calculated according to the following equation: 7^2)-7^2)
[0161] in which “T0(X2)” represents a reference infrared transmission factor value and “T(X2)” represents the infrared transmission factor measured during the fourth step “E4”.
[0162] The reference value is for example the first preform 12 at the start of production, called the reference preform 12.
[0163] The reference value is for example the infrared transmission factor “T0(X2)” which corresponds to the specifications of a preform 12, called the reference preform 12. It may also be the infrared transmission factor “T0(X2)” measured for a preform 12 taken as a sample from the batch of preforms 12 which must be treated by the installation 10, or even the average of the infrared transmission factors “T0(X2)” measured for a sample of several preforms 12 taken from the batch of preforms 12 which must be treated.
[0164] The transmission rate “AT(X2)” is thus likely to vary between 0, for a preform 12 having the same infrared transmission factor “T(X2)” as the reference preform 12, and 1.
[0165] The corrected power “Ptc” is also calculated based on the proportion of the power of the heating electromagnetic radiation extending into the near infrared range.
[0166] The power of the heating electromagnetic radiation is then corrected according to the following equation: Ptc = PnirO.(l- ATQ2)) + Pt 750.(1 -AL*}
[0167] During the second sub-step “E2-2” of controlling the second step “E2”, the power of the heating electromagnetic radiation is controlled as a function of the corrected power “Ptc” calculated during the first sub-step “E2-1” to heat the body 14 of the preforms 12 to the set temperature, taking into account the color of the preforms 12 and the infrared transmission factor “T(X2)” of the preforms 12 in the near infrared range.
[0168] Preferably, but not necessarily, to prevent the power of the heating radiation from changing too chaotically and quickly depending on the different values measured for each preform 12, the corrected power “Ptc” is calculated by taking into account the measurement of the clarity for several successive preforms 12. The number of preforms 12 is for example equal to the number of preforms likely to be contained simultaneously in the heating zone 42. This is a sliding average which is updated for each new preform 12 received in the measurement zone “Z”.
[0169] As a variant applicable to all the embodiments described above, the corrected power can also be calculated even more precisely by taking into account the parameters a* and b* measured for each preform 12 in order to define a correction factor which depends even more precisely on the different wavelengths belonging to the visible light range. Such a correction would thus take into account not only the clarity of the wall 16 of the preform 12 but also its color.
Claims
Claims
1. Method for controlling a heating station (30) of an installation (10) for manufacturing containers (11) by forming, in particular by stretch-blow molding, preforms (12) made of thermoplastic material, the preforms (12) being transported along a production path (34) which passes through a heating zone (42) in which the preforms (12) are exposed to continuous spectrum heating electromagnetic radiation, said spectrum extending at least partly into the visible light range, characterized in that the method comprises: - a first step (El) of measuring the absorption spectrum (o(Xl)) of a wall (16) of a preform (12) in the visible light range in a measurement zone (Z) crossed by the production path (34) upstream of the heating zone (42);- a second step (E2) of controlling the power of the heating electromagnetic radiation as a function of the absorption spectrum (o(Xl)) measured during the first step to heat the body (14) of the preforms to a set temperature.;
2. Method according to the preceding claim, characterized in that the second control step (E2) comprises a first sub-step (E2-1) of calculating a corrected power (Ptc) of the heating electromagnetic radiation as a function of the absorption spectrum (o(Xl)) measured during the first step (El), and a second sub-step (E2-2) of controlling the power of the heating electromagnetic radiation to said corrected power (Ptc) calculated during the first sub-step (E2-1).
3. Method according to the preceding claim, characterized in that during the first calculation sub-step (E2-1), the measured absorption spectrum (o(Xl)) is used to calculate the parameters of the wall (16) of the preform in a determined chromatic space equivalent to the CIELAB chromatic space as defined by the ISO 11664-4:2019 standard.
4. Method according to the preceding claim, characterized in that the corrected power (Ptc) is calculated during the first sub-step (E2-1) at least as a function of the value of a parameter (p) representative of the luminance of the wall (16) in the determined chromatic space.
5. Method according to the preceding claim, characterized in that the corrected power (Ptc) is calculated according to a rate of said parameter (p) which is calculated according to the following equation: A P0P AP~~ in which Pq represents a reference value of the parameter and p represents the parameter calculated from the absorption spectrum (o(Xl )) measured during the first step (El).
6. Method according to the preceding claim, characterized in that the corrected power (Ptc) is calculated as a function of the proportion of the power (Pvis) of the heating electromagnetic radiation extending into the visible light range.
7. Method according to any one of the preceding claims, characterized in that the heating radiation extends at least partly in the near infrared range and in that it comprises a fourth step (E4) of measuring an infrared transmission factor (T(X2)) of a wall (16) of said preform (12) for at least one wavelength (X2) belonging to the near infrared range, this fourth step (E4) being carried out prior to the first sub-step (E2-1) of calculation.
8. Method according to the preceding claim, characterized in that the corrected power (Ptc) is calculated as a function of a transmission rate (AT(X2)) which is calculated according to the following equation: . -ZW)-T(X2) in which T0(X2) represents a reference infrared transmission factor value and T(X2) represents the infrared transmission factor measured during the fourth step (E4).
9. Method according to the preceding claim, characterized in that the corrected power (Ptc) is calculated as a function of the proportion of the power (Pnir) of the heating electromagnetic radiation extending into the near infrared range.
10. Installation (10) for implementing the method according to any one of the preceding claims, the installation comprising means (36) for conveying preforms (12) in a row along a predetermined production path (34) passing successively through a zone (42) for heating a body (14) of the preforms (12) and through a station (32) for forming the preforms (12) into a container (11), in particular by stretch-blow molding, characterized in that the installation comprises a measuring device (56) of the absorption spectrum (o(Xl)) in the visible light range of at least one wall (16) of the preforms (12) during their passage through an associated measurement zone (Z).
11. Installation (10) according to the preceding claim, characterized in that the device (56) for measuring the absorption spectrum (o(Xl)) comprises: - a first light source (58) which emits a first light beam (55) according to a continuous spectrum (oO) which extends at least in the visible range, - a spectrometer (62, 70) measuring the intensity (I) and the wavelength (XI) of the first light beam (55) after having passed through at least one thickness of the wall (16) of the preform (12).
12. Installation according to any one of claims 10 or 11, characterized in that it comprises a device (64) for measuring the infrared transmission factor (T(X2)) of at least one wall (16) of the preforms (12) during their passage through an associated measurement zone (Z).
13. Installation according to the preceding claim, characterized in that the device (64) for measuring a value representative of the infrared transmission factor (T(X2)) comprises: - a light source (58, 68) which emits a light beam (55, 66) having at least a second wavelength (X2) in the near infrared range, - a measuring member measuring the intensity (I) for the at least one second wavelength (X2) of said light beam (55, 66) after having passed through at least one thickness of the wall (16) of the preform (12).
14. Installation (10) according to the preceding claim, characterized in that the first light beam (55) emitted by the first light source (58) has a continuous spectrum which includes said at least one second wavelength (X2).
15. Installation (10) according to claim 13, characterized in that the device (64) for measuring a value representative of the infrared transmission factor (T(X2)) comprises a second light source (68) which is distinct from the first light source (58) and which emits a second light beam (66) having at least a second wavelength (X2) in the near infrared range.
16. Installation (10) according to the preceding claim, characterized in that the first light beam (55) and the second light beam (66) pass through the wall (16) of the preform (12) at the same height (h).
17. Installation (10) according to the preceding claim, characterized in that the first light beam (55) and the second light beam (66) are merged into a common beam (72) before reaching the preform (12).
18. Installation (10) according to any one of claims 13 to 17, characterized in that the measurement of the infrared transmission factor (T(X2)) and the measurement of the absorption spectrum (o(Xl)) are carried out simultaneously in the same measurement zone (Z) of the production path (34).
19. Installation (10) according to any one of claims 13 to 18 taken in combination with claim 11, characterized in that the measuring member of the device (64) for measuring the infrared transmission factor (T(X2)) and the spectrometer (62) of the device for measuring the absorption spectrum (o(Xl)) are formed by a single spectrometer (70) common to the two devices (56, 64).