Electrically insulated wires and cables
A polyimide film with a corona-resistant composite filler and fluoropolymer coatings for stranded conductors enhances mechanical strength and reduces bulk, addressing void space issues in aerospace cables.
Patent Information
- Application Number
- FR2024003438
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-04
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-11
AI Technical Summary
Existing electrically insulated wires and cables used in aerospace applications face challenges with corona-resistant films that compromise mechanical properties due to the presence of void spaces, leading to unpredictable performance in high-voltage environments, and thicker layers to address this issue increase bulk and weight.
A stranded conductor is wrapped with an inner casing of a polyimide film containing a corona-resistant composite filler, bonded with fluoropolymer coatings, and an outer fluoropolymer strip, minimizing void spaces and enhancing mechanical properties while maintaining electrical insulation.
The solution provides improved mechanical strength, corona resistance, and reduced bulk and weight, achieving superior performance in high-voltage applications with a thinner form factor.
Abstract
Description
Title of the invention: ELECTRICALLY INSULATED WIRES and CABLES Technical field
[0001] The field of this invention is that of electrically insulated wires and cables. STATE OF THE ART
[0002] Modern aerospace applications demand ever-increasing performance for electrically insulated wires and cables. As systems are designed to operate at higher voltages for extended periods of time, the need for corona-resistant films arises. These films, when used as wire insulation material, must maintain both good electrical properties (e.g., voltage endurance) and mechanical properties (e.g., scrape abrasion and dynamic cutting). Typically, a wire will be bent into various shapes or directions, and the corona-resistant film covering the wire or cable must have the ability to do the same. Adding filler to corona-resistant films can negatively impact their mechanical properties, and the films may become more brittle (lower tensile strength and elongation).
[0003] Corona resistant films have previously been used in magnet wire constructions for traction motors, i.e. wires consisting of a singular copper strand, the surface of which is covered with an insulating film material. Since only a single strand wire is used, the insulating film is in very close contact with the conductor of the wire, thus providing a uniform interface throughout the construction, and the resulting construction is essentially free of any substantial void space between the side of the film facing the wire and the surface of the wire itself. Furthermore, there is no significant void space beneath the insulating material since the space beneath the insulating material is entirely occupied by the conductor.However, in aerospace applications, single stranded conductors are preferentially used instead of single stranded wire to take advantage of the greater flexibility and lower resistance of such constructions. As can be seen in a cross-section of an insulated stranded wire, covering a single stranded conductor with a film-based insulation material leaves significant amounts of void space within the resulting construction, unlike the construction obtained using single stranded wire. The presence of such void space can adversely affect the results of performance tests such as PDIV (partial discharge onset voltage) tests or voltage endurance tests. Due to the existence of additional void space inside the single multi-stranded film-insulated conductor, the performance of corona-resistant insulating films usually used in magnet wire constructions can be expected to be adversely affected because the insulating material is attacked simultaneously by corona from two opposite sides instead of just one side, and thus the function, behavior, and benefit of such corona-resistant insulating films are difficult to predict in such a construction.
[0004] Crosslinked ethylene-tetrafluoroethylene (XL-ETFE, where ETFE is a copolymer of ethylene (E) and tetrafluoroethylene (TFE), such as Tefzel® ETFE) is commonly used as an electrical cable jacketing material in aircraft wire insulation due to its resistance to heat, fining, and arc tracking. Compared to polytetrafluoroethylene (PTFE), it has improved impact, abrasion, and cut resistance. ETFE is radiation resistant and has higher mechanical strength than other fluoropolymers and is free from fining problems noticed in improperly sintered PTFE. XL-ETFE can be used continuously at 200°C and has improved tensile strength and anti-aging resistance compared to uncrosslinked ETFE.However, XL-ETFE does not meet flammability criteria in 30+% oxygen (unless additional additives are added), releases fluorine over time which can cause corrosion of unprotected metals in sealed or confined environments, and is susceptible to degradation by ultraviolet radiation, and is less flexible and more difficult to strip.
[0005] In higher voltage applications, the performance deficiencies of the insulating material can be overcome by using thicker layers of insulating wrap, but this adds unwanted bulk and weight to the wrapped wire. There is a need for corona-resistant, electrically insulating films that can withstand the demands of high voltage aerospace applications and can do so while limiting the film form factor. DETAILED DESCRIPTION
[0006] In a first aspect, an electrically insulated wire or cable comprises a stranded conductor, an inner jacket around the stranded conductor, and an outer jacket around the inner jacket. The inner jacket comprises a base film strip, the base film strip comprising a polyimide film having an electrically insulating and corona-resistant composite filler, a first fluoropolymer coating adhered to a first side of the polyimide film, and a second fluoropolymer coating adhered to a second side of the polyimide film. The outer jacket comprises a fluoropolymer strip. The wire or Electrically insulated cable has a void space in the range of 2 to 43%, based on the total space available within the inner jacket.
[0007] The stranded conductor may comprise a copper or copper alloy wire, the copper or copper alloy being coated with a metal selected from tin, silver, nickel or being coated with an alloy of these metals or a mixture of these metals.
[0008] A polyimide film having an electrically insulating and corona resistant composite filler may be formed from a substantially chemically converted polyimide or a thermally converted polyimide. Polyimide films having an electrically insulating and corona resistant composite filler may be made by carefully selecting the dianhydride and diamine monomers used for the polyimide backbone. In one embodiment, a polyimide film having a chemically converted polyimide has a more uniform dispersion of corona resistant composite filler than a polyimide film having a thermally converted polyimide.In addition, the polyimide film having a chemically converted polyimide has better dielectric strength, tensile strength, elongation and corona resistance than a polyimide film having a thermally converted polyimide.
[0009] As used herein, the terms "substantially chemically converted" mean that a polyimide is 75% or more, 80% or more, 85% or more, 90% or more, or 95% or more imidized by means of a process incorporating conversion chemicals (i.e., catalysts and dehydrating agents) in which a solvated mixture (a polyamic acid casting solution) may be cast or coated onto a support to give a partially imidized gel film, and then heated in an oven, using convective and radiant heat, to remove the solvent and complete the imidization.The percentage of imidization can be measured by comparing a ratio of intensities at 1365 cm 1 (polyimide CN) versus 1492 cm 1 (aromatic stretching used as an internal standard) in attenuated total reflectance Fourier transform infrared spectroscopy (ATR-FTIR) and comparing the ratio to that of a sample prepared with standard curing processes which is defined as 100% cured.
[0010] Depending on the context, "diamine" as used herein is intended to mean: (i) the unreacted form (i.e., a diamine monomer); (ii) a partially reacted form (i.e., the portion or portions of an oligomer or other polymer precursor derived from or otherwise attributable to the diamine monomer); or (iii) a fully reacted form (the portion or portions of the polymer derived from or otherwise attributable to the diamine monomer). diamine may be functionalized with one or more groups, depending on the particular embodiment chosen in implementing the present invention.
[0011] Indeed, the term "diamine" is not intended to be limiting (or interpreted literally) as to the number of amine groups in the diamine component. For example, (ii) and (iii) above include polymeric materials that may have two, one, or zero amine groups. Alternatively, the diamine may be functionalized with additional amine groups (in addition to the amine groups at the ends of the monomer that react with the dianhydride to propagate a polymer chain). Such additional amine groups may be used to crosslink the polymer or to provide other functionality to the polymer.
[0012] Similarly, the term "dianhydride," as used herein, is intended to refer to the component that reacts with (is complementary to) the diamine and in combination is capable of reacting to form an intermediate (which can then be cured into a polymer). Depending on the context, "anhydride," as used herein, may refer not only to an anhydride moiety per se, but also to a precursor to an anhydride moiety, such as: (i) a pair of carboxylic acid groups (which can be converted to an anhydride by dehydration or a reaction of a similar type); or (ii) an acid halide (e.g., chloride) ester functionality (or any other functionality presently known or developed in the future that is) capable of conversion to an anhydride functionality.
[0013] Depending on the context, "dianhydride" may refer to: (i) the unreacted form (i.e., a dianhydride monomer, whether the anhydride functionality is in true anhydride form or in anhydride precursor form, as indicated in the preceding paragraph); (ii) a partially reacted form (i.e., the portion(s) of a precursor or partially reacted oligomer or other polymer composition reacted from or otherwise attributable to a dianhydride monomer); or (iii) a fully reacted form (the portion(s) of the polymer derived from or attributable to a dianhydride monomer).
[0014] The dianhydride may be functionalized with one or more groups, depending on the particular embodiment chosen in practicing the present invention. Indeed, the term "dianhydride" is not intended to limit (or be interpreted literally) the number of anhydride groups in the dianhydride component. For example, (i), (ii) and (iii) (in the paragraph above) include organic substances that may have two, one or zero anhydride groups, depending on whether the anhydride is in the precursor state or in the reacted state. Alternatively, the dianhydride component may be functionalized with anhydride-like groups additional (in addition to the anhydride groups that react with the diamine to provide a polymer). Such additional anhydride groups may be used to crosslink the polymer or to provide other functionality to the polymer.
[0015] Any of a number of polymer manufacturing processes can be used to prepare polyimide films. It would be impossible to discuss or describe all possible manufacturing processes useful in practicing the present invention. It should be noted that the monomer systems of the present invention are capable of providing the advantageous properties described above in a variety of manufacturing processes. The compositions of the present invention can be manufactured as described herein and can be readily manufactured in any of the many (perhaps countless) ways known to those skilled in the art, using any conventional or unconventional manufacturing technology.
[0016] Although methods and materials similar or equivalent to those described herein may be used in practicing or testing the present invention, suitable methods and materials are described herein.
[0017] Where a quantity, concentration or other value or parameter is given as a range, preferred range or list of upper preferable values and lower preferable values, this is to be understood as specifically disclosing all ranges formed from any pair of upper limits or preferred values and lower limits or preferred values, whether or not the ranges are separately disclosed. Where a range of numerical values is cited herein, unless otherwise indicated, the range is intended to include its endpoints, and all integers and fractions within the range. It is not intended that the scope of the invention be limited to the specific values cited when defining a range.
[0018] In describing certain polymers, it should be understood that sometimes applicants refer to polymers by the monomers used to make them or the amounts of the monomers used to make them. Although such a description may not include the particular nomenclature used to describe the final polymer or contain product-by-process terminology, any reference to monomers and amounts should be interpreted to mean that the polymer is made from those monomers or that amount of the monomers, and the corresponding polymers and their compositions.
[0019] The materials, methods and examples of the invention are given for illustrative purposes only and, unless otherwise indicated, are not intended to be limiting.
[0020] As used herein, the terms "comprises," "comprising," "includes," "including," "has," "having," or any other variation thereof are intended to cover non-exclusive inclusion. For example, a method, article, or apparatus that includes a list of elements is not necessarily limited to only those elements, but may include other elements not expressly listed or inherent in that method, article, or apparatus. Further, unless expressly stated otherwise, "or" means an inclusive or and not an exclusive or. For example, a condition A or B is satisfied by any of the following: A is true (or present) and B is false (or not present), A is false (or not present) and B is true (or present), and both A and B are true (or present).
[0021] It is understood that although the terms first, second, third, etc. may be used herein to describe various elements, components, regions, layers and / or sections, such elements, components, regions, layers and / or sections are not to be limited by such terms. Such terms are used only to distinguish one element, component, region, layer and / or section from another element, component, region, layer and / or section. Thus, a first element, first component, first region, first layer and / or first section could be referred to as a second element, component, region, layer and / or section without departing from the teachings of the present invention. Similarly, the terms "top" and "bottom" are relative only to each other.It will be appreciated that when an element, component, layer or the like is inverted, what is the "bottom" before being inverted would be the "top" after being inverted, and vice versa. When an element is referred to as being "on" or "arranged upon" another element, this refers to a positioning on or under the object part, but does not essentially refer to a positioning on top of the object part in terms of a direction of gravity, and it may be directly upon the other element or intermediate elements may be present between them. On the other hand, when an element is said to be "directly upon" or "arranged directly upon" another element, there are no intermediate elements present.
[0022] Furthermore, it will also be understood that when an element, component, region, layer and / or section is referred to as being “between” two elements, components, regions, layers and / or sections, it may be the only element, component, region, layer and / or section between the two elements, components, regions, layers and / or sections, or one or more intermediate elements, components, regions, layers and / or sections may also be present. Stranded conductors
[0023] In one embodiment, a stranded conductor may be a high temperature stranded conductor wire with individual strands in a range of 19 to 5 000, designed for temperatures up to 260°C. Stranded conductor, as used herein, means a conductive wire in which several strands of uninsulated wire are bundled together to form a single-conductor wire, as opposed to "Litz" wire in which each strand of a multi-strand is individually insulated. In one embodiment, the individual strands may comprise copper. In one embodiment, the copper may comprise oxygen-free copper. In one embodiment, individual strands of copper may be coated with a metal or metal alloy plating, such as tin, silver, nickel, and mixtures and alloys thereof. In one embodiment, a high-strength copper alloy may be used that is resistant to corrosion and oxidation at elevated temperatures, as well as chemical compounds, alkalis, hydraulic fluids, and fuel.In one embodiment, the size of the multi-stranded conductive wire may be in a range of AWG (American Wire Gauge) 0000 to AWG 26 (a diameter of the conductive wire in the range of 0.0175 to 0.6050 inches (0.445 to 15.4 mm)). The size of the individual strands of a given wire may be in a range of AWG 24 to AWG 40 (a diameter in the range of 0.0031 to 0.0201 inches (78.7 to 511 µm)).
[0024] The stranded conductor can be manufactured in a variety of configurations, the most common being concentric (true concentric, equilay concentric, unidirectional concentric, and unilay concentric), bundled, and roped, with concentric being defined as a center strand surrounded by one or more layers of helical strands laid in a geometric pattern. The geometric pattern requires that concentric constructions can only be made with 7, 19, 37, 61, (etc.) strands or elements, following the pattern that each successive layer has 6 more strands than the layer below it. In all types of concentric constructions, the geometric pattern of the strands is consistent throughout the length of the conductor. That is, the center strand and the strands in each layer remain in their respective positions from the beginning to the end of its length. In one embodiment, a concentric stranded conductor is used. Organic solvents
[0025] Organic solvents useful for the synthesis of the polyimides of the present invention are preferably capable of dissolving the polyimide precursor materials. Such a solvent should also have a relatively low boiling point, e.g., less than 225°C, so that the polymer can be dried at moderate (i.e., more convenient and less expensive) temperatures. A boiling point less than 210, 205, 200, 195, 190, or 180°C is preferred.
[0026] Useful organic solvents include: N-methylpyrrolidone (NMP), N,N-dimethylacetamide (DMAc), methyl ethyl ketone (MEK), N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), tetramethylurea (TMU), glycol ethyl ether, diethylene glycol diethyl ether, 1,2-dimethoxyethane (monoglyme), diethylene glycol dimethyl ether (diglyme), 1,2-bis-(2-methoxyethoxy)ethane (triglyme), gamma-butyrolactone, and bis-(2-methoxyethyl) ether, tetrahydrofuran (THF), ethyl acetate, hydroxyethyl acetate, glycol monoacetate, acetone, and mixtures thereof. In one embodiment, preferred solvents include N-methylpyrrolidone (NMP) and N,N-dimethylacetamide (DMAc). Diamines
[0027] In one embodiment, any number of suitable diamines may be used for the monomers to form the polymer backbone. Aromatic diamines may include fluorinated aromatic diamines, such as 2,2'-bis(trifluoromethyl)benzidine (TFMB), 2,2'-bis-(4-aminophenyl)hexafluoropropane, 4,4'-diamino-2,2'-trifluoromethyldiphenyloxide, 3,3'-diamino-5,5'-trifluoromethyldiphenyloxide, 9,9'-bis(4-aminophenyl)fluorene, 4,4'-trifluoromethyl-2,2'-diaminobiphenyl, 4,4'-oxy-bis[2-trifluoromethyl)benzeneamine] (1,2,4-OBABTF), 4,4'-oxy-bis[3-trifluoromethyl)benzeneamine], 4,4'-thiobis[(2-trifluoromethyl)benzeneamine], 4,4'-thiobis[(3-trifluoromethyl)benzeneamine], 4,4'-sulfoxyl-bis[(2-trifluoromethyl)benzeneamine, 4,4'-sulfoxyl-bis[(3-trifluoromethyl)b enzeneamine], 4,4'-keto-bis[(2-trifluoromethyl)benzeneamine], 1,1 -bis[4'-(4”-amino-2”-trifluoromethylphenoxy)phenyl]cyclopentane, 1,1-bis[4'-(4”-amino-2”-trifluoromethylphenoxy)phenyl]cyclohexane,2-trifluoromethyl-4,4'-diaminodiphenyl ether; l,4-(2'-trifluoromethyl-4',4”-diaminodiphenoxy)benzene, l,4-bis(4'-aminophenoxy)-2-[(3',5'-ditrifluoromethyl)phenyl]benzene (6F-amine), l,4-bis[2'-cyano-3'(“4-amino phenoxy)phenoxy]-2-[(3',5'-ditrifluoro-methyl)phenyl]benzene (6FC-diamine), 3,5-diamino-4-methyl-2',3',5',6'-tetrafluoro-4'-tri-fluoromethyldiphenyloxide, 2,2-bis[4(4-aminophenoxy)phenyl]phthalein-3',5'-bis(trifluoromethyl)anilide (6FADAP) and 3,3',5,5'-tetrafluoro-4,4'-diamino-diphenylmethane (TFDAM). ,
[0028] Other useful aromatic diamines may include 4,4'-diaminobiphenyl, 4,4'-diaminoterphenyl, 4,4'-diaminobenzanilide (DABA), 4,4'-diaminophenylbenz oate, 4,4'-diaminobenzophenone, 4,4'-diaminodiphenylmethane (MDA), 4,4'-diaminodiphenylsulfide, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), 4,4'-bis(4-aminophenoxy)biph enyl (BAPB), 4,4'-diaminodiphenyl ether (ODA), 3,4'-diaminodiphenyl ether, 4,4'-isopropylidenedianiline, 2,2'-bis(3-aminophenyl)propane, 2,2-bis(4-aminophenyl)propane, 3,3'-dimethyl-4,4'-diaminobiphenyl, 4-aminophenyl-3-aminobenzoate, bis(p-beta-amino-t-butylphenyl)ether, p-bis-2-(2-methyl-4-aminopentyl)benzene. In one embodiment, the diamine is a triamine, such as N,N-bis(4-aminophenyl)-n-butylamine, N,N-bis(4-aminophenyl)methylamine or N,N-bis(4-aminophenyl) aniline.
[0029] Other useful aromatic diamines may include l,2-bis(4-aminophenoxy)benzene, l,3-bis(4-aminophenoxy)benzene (RODA), l,2-bis(3-aminophenoxy)benzene, l,3-bis(3-aminophenoxy)benzene, l-(4-aminophenoxy)-3-(3-aminophenoxy)benzene, l,4-bis-(4-aminophenoxy)benzene, l,4-bis(3-aminophenoxy)benzene, l-(4-aminophenoxy)-4-(3-aminophenoxy)benzene, 2,2-bis(4-[4-aminophenoxy]phen yl)propane (BAPP), 2,2'-bis(4-phenoxyaniline)isopropylidene.
[0030] Other useful aromatic diamines may include p-phenylenediamine (PPD), m-phenylenediamine (MPD), 2,5-dimethyl-1,4-diaminobenzene, 2,5-dimethyl-1,4-phenylenediamine (DPX), 1,4-naphthalenediamine, 1,5-naphthalenediamine, 1,5-diaminonaphthalene, m-xylylenediamine and p-xylylenediamine.
[0031] In one embodiment, other diamines useful for forming the polyimide may include an aliphatic diamine, such as 1,2-diaminoethane, 1,6-diaminohexane (HMD), 1,4-diaminobutane, 1,5-diaminopentane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane (DMD), 1,11-diaminoundecane, 1,12-diaminododecane (DDD), 1,16-hexadecamethylenediamine, 1,3-bis(3-aminopropyl)-tetramethyldisiloxane, trans-1,4-diaminocyclohexane (CHDA), isophoronediamine (IPDA), bicyclo[2.2.2]octane-1,4-diamine and combinations thereof. Other aliphatic diamines suitable for practicing the invention include those having six to twelve carbon atoms or a combination of longer and shorter chain diamines as long as the expandability and flexibility of the polymer are maintained. Long chain aliphatic diamines can increase flexibility.
[0032] Other additional diamines useful for forming the polyimide may include an alicyclic diamine (which may be fully or partially saturated), such as a cyclobutane diamine (e.g., cA- and trans-1,3-diaminocyclobutane, 6-amino-3-azaspiro[3,3]heptane, and 3,6-diaminospiro[3,3]heptane), bicyclo[2,2.1]heptane-1,4-diamine, isophoronediamine, and bicyclo[2,2.2]octane-1,4-diamine. Other alicyclic diamines include cis-1,4-cyclohexanediamine, trans-1,4-cyclohexanediamine, 1,4-bis(aminomethyl)cyclohexane, 4,4'-methylenebis(cyclohexylamine), 4,4'-methylenebis(2-methylcyclohexylamine), bis(aminomethyl)norbornane. Dianhydrides
[0033] In one embodiment, any number of suitable dianhydrides may be used for the monomers to form the polymer backbone. The dianhydrides may be used in their tetraacid form (or as mono, di, tri, or tetraesters of the tetraacid), or as their diester acid halides (chlorides). However, in some embodiments, the dianhydride form may be preferred, as it is generally more reactive than the acid or ester.
[0034] Examples of suitable aromatic dianhydrides include 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2-(3',4'-dicarboxyphenyl)-5,6-dicarboxybenzimidazole dianhydride, 2-(3',4'-dicarboxyphenyl)-5,6-dicarboxybenzoxazole dianhydride, 2-(3',4'-dicarboxyphenyl)-5,6-dicarboxybenzothiazole dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), 2,2',3,3'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 4,4'-thio-diphthalic anhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, bis(3,4-dicarboxyphenyl)sulfoxide dianhydride (DSDA), bis(3,4-dicarboxyphenyloxadiazole-1,3,4)-p-phenylene dianhydride, bis(3,4-dicarboxyphenyl)-2,5-oxadiazole-1,3,4-dianhydride, bis(3',4'-dicarboxydiphenyl ether)-2,5-oxadiazole-1,3,4-dianhydride, 4,4'-oxydiphthalic anhydride (ODPA),bis(3,4-dicarboxyphenyl)t hioether dianhydride, bisphenol A dianhydride (BPADA), bisphenol S dianhydride, bis-1,3-isobenzofurandione, l,4-bis(4,4'-oxyphthalic anhydride)benzene, bis(3,4-dicarboxyphenyl)methane dianhydride, perylene-3,4,9,10-tetracarboxylic dianhydride, l,3-bis-(4,4'-oxydiphthalic anhydride)benzene, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA) and 9,9-bis(trifluoromethyl)-2,3,6,7-xanthenetetracarboxylic dianhydride. ,
[0035] In one embodiment, additional dianhydrides to form the polyimide may include 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, bicyclo-[2,2,2]-octene-(7)-2,3,5,6-tetracarboxylic dianhydride, cyclopentadienyltetracarboxylic dianhydride, ethylenetetracarboxylic dianhydride, pyromellitic dianhydride (PMDA), tetrahydrofurantetracarboxylic dianhydride, 2,6-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,7-Dichloronaphthalene-1,4,5,8-tetracarboxylic acid, 2,3,6,7-tetrachloronaphthalene-1,4,5,8-tetracarboxylic acid dianhydride, phenanthrene-1,8,9,10-tetracarboxylic acid dianhydride, pyrazine-2,3,5,6-tetracarboxylic acid dianhydride, benzene-1,2,3,4-tetracarboxylic acid dianhydride and thiophene-2,3,4,5-tetracarboxylic acid dianhydride.
[0036] In one embodiment, additional dianhydrides to form the polyimide may include an alicyclic dianhydride, such as cyclobutane-1,2,3,4-tetracarboxylic dianhydride (CBDA), 1,2,4,5-cyclohexanetetrac arboxylic dianhydride, 1,2,3,4-cyclohexanetetracarboxylic dianhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,3,4- cyclopentanetetracarboxylic acid (CPDA), hexahydro-4,8-ethano-1H,3H-benzo[1,2-c:4,5-c']difuran-1,3,5,7-tetrone (BODA), 1,4:2,3-dianhydride 3-(carboxymethyl)-1,2,4-cyclopentanetricarboxylic acid (TCA) and meso-butane-1,2,3,4-tetracarboxylic acid.
[0037] In one embodiment, a polyimide is derived from 100 mol% pyromellitic dianhydride (PMDA) and 100 mol% 4,4'-diaminodiphenyl ether (ODA). In one embodiment, a polyimide may have a weight average molecular weight (Mw) of 100,000 daltons or more, 150,000 daltons or more, 200,000 daltons or more, or 250,000 daltons or more. Imidization catalysts
[0038] In one embodiment, an imidization catalyst (sometimes referred to as an "imidization accelerator") may be used as a conversion chemical that may help lower the imidization temperature to form the polyimide and shorten the imidization time. The polyamic acid casting solutions of the present invention comprise both a polyamic acid solution combined with an amount of conversion chemical compounds. Conversion chemical compounds that are useful in the present invention include, among others, (i) one or more dehydrating agents and / or cocatalysts, such as aliphatic acid anhydrides (acetic anhydride, trifluoroacetic anhydride, propionic anhydride, monochloroacetic anhydride, bromoadipic anhydride, etc.) and aromatic acid anhydrides; and (ii) one or more imidization catalysts, such as aliphatic tertiary amines (triethylamine, etc.), aromatic tertiary amines (dimethylaniline, N,N-dimethylbenzylamine, etc.) and heterocyclic tertiary amines (pyridine, alpha-, beta-, gamma-picoline, 3,5-lutidine, 3,4-lutidine, isoquinoline, etc.) and guanidines (e.g., tetramethylguanidine). In one embodiment, an imidization catalyst does not comprise a diazole. Other useful dehydrating agents may include diacetyl ether, butyryl ether, benzoyl ether, 1,3-dichlorohexyl carbodiimide, N,N-dicyclohexylcarbodiimide, benzenesulfonyl chloride, thionyl chloride, and phosphorus pentachloride. In some embodiments, the dehydrating agent may also serve as a catalyst to improve the reaction kinetics for imidization. The anhydride dehydrating material is generally used in a slight molar excess of the amount of amide acid groups present in the polyamic acid solution.In one embodiment, the amount of dehydrating agent used is typically about 2.0 to 4.0 moles per equivalent of the polyamic acid formula unit. Generally, a comparable amount of tertiary amine catalyst is used. The ratio of these catalysts and their concentration in the . polyamic acid solution will influence imidization kinetics and film properties. Polyimide films having substantially chemically converted polyimide may have imidization catalysts present in the polyimide film in an amount ranging from 1 part per billion (ppb) to 1% by weight, 10 ppb to 0.1% by weight, or 100 ppb to 0.01% by weight. Corona resistant composite fillers
[0039] The polyimide film of the present disclosure comprises an electrically insulating and corona resistant composite filler. In one embodiment, a corona resistant composite filler may comprise an organic component and an inorganic ceramic oxide component, wherein a weight ratio of the organic component to the inorganic ceramic oxide component is from 0.01:1 to 1:1. In some embodiments, the weight ratio of the organic component to the inorganic ceramic oxide component may be in a range between (and optionally include) any two of the following numbers: 0.01:1, 0.05:1, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1 and 1:1. In one embodiment, at least a portion of the organic component may comprise an organosiloxane moiety or an organometaloxane moiety (e.g., organozirconate, organotitanate, organoaluminate).
[0040] In one embodiment, the inorganic ceramic oxide component may comprise silica, alumina, titanium dioxide, zirconia, or mixtures thereof. In one embodiment, the inorganic ceramic oxide component comprises silica, alumina, or a mixture thereof. In one embodiment, the inorganic ceramic oxide component is fumed alumina.
[0041] In one embodiment, the organic component of the corona resistant composite filler material is selected primarily to impart or enhance the dispersibility of the corona resistant composite filler material in a particulate solvated polymer matrix or polymer matrix precursor. In some embodiments, the organic component of the corona resistant composite filler material is selected to reduce moisture absorption onto the inorganic ceramic oxide component. Ordinary skill and experience may be required to optimize the organic component for any particular solvent system selected. In some embodiments, the organosiloxane moiety is n-octylsilane, or any of its structural isomers. In some embodiments, the corona resistant composite filler is an inorganic ceramic oxide without an organic component.In another embodiment, the organic component is a coating on the component. inorganic ceramic oxide. The organic component may or may not cover the entire surface of the inorganic ceramic oxide component.
[0042] In one embodiment, the electrically insulating and corona resistant composite filler is present in an amount between and including any two of the following numbers: 5, 10, 15, 20, 25 and 30% by weight, based on the total weight of the polyimide film. In one embodiment, the corona resistant composite filler is present in an amount in a range of 5 to 30, 5 to 25 or 5 to 20% by weight, based on the total weight of the polyimide film.
[0043] In one embodiment, the corona resistant composite filler may have a median particle size in a range of 0.1 to 5 μm, wherein at least 80, 85, 90, 92, 94, 95, 96, 98, 99, or 100 percent of the dispersed corona resistant composite filler falls within the size range defined above. The median particle size may be measured using a Horiba LA-930 particle size analyzer (Horiba Instruments, Inc., Irvine, CA). DMAc may be used as a carrier fluid. In some embodiments, the corona resistant composite filler is a nanofiller. By nanofiller, is meant a filler with at least one dimension less than 1000 nm, i.e., less than 1 μm.
[0044] In one embodiment, the polyimide film further comprises a dispersing agent. In some embodiments, the polyimide film further comprises a dispersing agent in an amount ranging from 1 to 100 weight percent based on the weight of the inorganic ceramic oxide component. In some embodiments, the dispersing agent is selected from the group consisting of phosphated polyethers, phosphated polyesters, and mixtures thereof. In another embodiment, the dispersing agent is an alkylolammonium salt of a polyglycol ester. In another embodiment, the dispersing agent is selected from the group consisting of Disperbyk 180, an alkylolammonium salt of a polyglycol ester, Disperbyk 111, a phosphated polyester, BYK W-9010, a phosphated polyester, or mixtures thereof (all available from ByK-Chemie GmBH, Wesel, Germany).In another embodiment, the dispersing agent is Solplus D540, a phosphated ethylene oxide / propylene oxide copolymer available from Lubrizol, Inc., Cleveland, OH. In yet another embodiment, the dispersing agent is a mixture of any of the above dispersing agents. In some embodiments, the dispersing agent is an aromatic polyamic acid or an aromatic polyimide. In another embodiment, the dispersing agent is a polyalkylene ether such as polytetramethylene glycol and polyethylene glycol. Typically, the aromatic polyamic acid or aromatic polyimide have high temperature stability and therefore would remain primarily in the polyimide. Whereas dispersing agents such as ethers . Polyalkylene films have low temperature stability and would decompose or burn primarily at the temperatures used in the imidization process. Polyimide films
[0045] In one embodiment, a polyimide film may be produced by combining a diamine and a dianhydride (monomer or other precursor form of polyimide) with a solvent to form a polyamic acid (also referred to as polyamide acid) solution. The dianhydride and diamine may be combined in a molar ratio of about 0.90 to 1.10. The molecular weight of the polyamic acid formed therefrom may be adjusted by adjusting the molar ratio of the dianhydride and diamine.
[0046] In one embodiment, a polyamic acid molding solution is derived from the polyamic acid solution. The polyamic acid molding solution and / or the polyamic acid solution are combined with conversion chemicals such as: (i) one or more dehydrating agents, such as aliphatic acid anhydrides (acetic anhydride, etc.) and / or aromatic acid anhydrides; and (ii) one or more catalysts, such as aliphatic tertiary amines (triethylamine, etc.), aromatic tertiary amines (dimethylaniline, etc.), and heterocyclic tertiary amines (pyridine, picoline, isoquinoline, etc.). The anhydride dehydration material is often used in molar excess relative to the amount of amide acid groups in the polyamic acid. The amount of acetic anhydride used is typically in the range of about 2.0 to 4.0 moles per equivalent (repeating unit) of polyamic acid.Typically, a comparable amount of tertiary amine catalyst is used. Dispersed or solvent-suspended fillers are then added to the polyamic acid solution as described above.
[0047] In one embodiment, the polyamic acid solution is dissolved in an organic solvent at a concentration of about 5.0 or 10 percent to 15, 20, 25, 30, 35, or 40 percent by weight. In one embodiment, a slurry is prepared comprising a filler, the slurry having a solids content in a range of 0.1 to 70, 0.5 to 60, 1 to 55, 5 to 50, or 10 to 45 percent by weight. The slurries may or may not be ball milled to achieve the desired particle size. The slurries may or may not be filtered to remove any residual large particles. A polyamic acid solution may be made by methods well known in the art. The polyamic acid solution may or may not be filtered. In some embodiments, the solution is mixed in a high shear mixer with the feed suspension.When a polyamic acid solution is made with a slight excess of diamine, an additional dianhydride solution may or may not be added to increase the viscosity. of the mixture to the desired level for casting the film. The amount of the polyamic acid solution and filler suspension can be adjusted to achieve the desired filler levels in the cured film. In some embodiments, the mixture is cooled to a temperature below 10°C and mixed with conversion chemicals prior to casting.
[0048] The solvated mixture (polyamic acid casting solution) may then be cast or coated onto a support, such as an endless belt or rotating drum, to yield a partially imidized gel film. Alternatively, it may be cast onto a polymeric support such as PET, other forms of Kapton® polyimide film (e.g., Kapton® HN or Kapton® E films), or other polymeric supports. The gel film may be removed from the drum or belt, placed on a stretching frame, and cured in an oven, using convective and radiant heat to remove the solvent and complete imidization to a solids level greater than 98%. The film may then be separated from the support, oriented as by stretching, with continued heating (drying and curing) to yield a substantially chemically converted polyimide film.
[0049] Useful methods for producing polyimide films can be found in U.S. Patent Nos. 5,166,308 and 5,298,331, which are incorporated by reference into this specification for all the teachings contained therein. Many variations are also possible, such as, (a) a method in which the diamine and dianhydride components are premixed together, and then the mixture is added portionwise to a solvent while stirring. (b) a process in which a solvent is added to a stirred mixture of diamine and dianhydride components. (unlike (a) above) (c) a process in which the diamines are dissolved exclusively in a solvent, and then dianhydrides are added thereto in a ratio which allows the reaction rate to be controlled. (d) a process in which the dianhydride components are dissolved exclusively in a solvent, and then amine components are added thereto in a ratio enabling the reaction rate to be controlled. (e) a process in which the diamine components and the dianhydride components are dissolved separately in solvents, and then these solutions are mixed in a reactor. (f) a process in which polyamic acid having an excess of amine component and another polyamic acid having an excess of dianhydride component are preformed and then reacted with each other in a reactor, particularly so as to create a non-random or block copolymer. (g) a process in which a specific portion of the amine components and dianhydride components are reacted first, and then the residual diamine components are reacted, or vice versa. (h) a process in which the conversion chemicals (catalysts) are mixed with the polyamic acid to form a polyamic acid casting solution and then cast to form a gel film. (i) a process in which the components are added in part or in whole in any order to part or all of the solvent, also in which part or all of any component may be added as a solution in part or all of the solvent. (j) a process wherein one of the dianhydride components is first reacted with one of the diamine components to give a first polyamic acid. Then another dianhydride component is reacted with another amine component to give a second polyamic acid. Then the amic acids are combined in any of several ways before the film is formed.
[0050] In one embodiment, the filler is first dispersed in a solvent to form a suspension. The suspension is then dispersed in the polyamic acid solution. In one embodiment, the filler concentration relative to the polyimide (in the final film) is in a range of 10 to 50% by volume, 15 to 45% by volume, 15 to 40% by volume, 20 to 35% by volume, or 25 to 30% by volume. In one embodiment, the filler concentration relative to the polyimide (in the final film) is at least 10, at least 15, at least 20, or at least 25% by volume. The composition of the cured film can be calculated from the composition of the components in the mixtures, excluding the DMAc solvent (which is removed during curing) and taking into account the removal of water during the conversion of polyamic acid to polyimide.
[0051] In one embodiment, the loaded polyamic acid casting solution is a mixture of a polyamic acid solution and a filler. In this casting solution, the filler is present in a concentration range of 0.1 to 70% by volume, 1 to 60% by volume, 2 to 50% by volume, 5 to 45% by volume, or 5 to 40% by volume. In one embodiment, the filler is first dispersed in the same polar aprotic solvent used to make the polyamic acid solution (e.g., DMAc). Optionally, a small amount of polyamic acid solution may be added to the filler slurry to increase the viscosity of the slurry. Optionally, a dispersant or dispersing agent may be added to aid dispersion or alter the rheology of the slurry.
[0052] The filler may be mixed with a particulate solvated polymer matrix or polymer matrix precursor using any commonly used technique used, such as batch mixing using solvent(s), dry mixing, or continuous mixing using solvent(s). Parameters such as order of raw material addition, mixing speed, shear rate, type of mixing blade (e.g., shear blade), mixing time, temperature, and pressure are known to affect the final degree of mixing between the filler and matrix material.
[0053] In one embodiment, mixing the filler slurry with a polyamic acid solution to form the filled polyamic acid casting solution is carried out using high shear mixing. In this embodiment, if the filler is present above 50 volume percent in the final film, the film may be too brittle and not be sufficiently flexible to form a flexible, self-supporting, mechanically strong sheet.
[0054] In one embodiment, the casting solution may also include any of a number of additives, such as processing aids (e.g., oligomers), antioxidants, light stabilizers, flame retardant additives, antistatic agents, heat stabilizers, ultraviolet absorbers, or various reinforcing agents.
[0055] In some embodiments, a coextrusion process may be used to form a multilayer polyimide film having an inner core layer sandwiched between two outer layers. In this process, a finished polyamic acid solution is filtered and pumped to a slot die, where the stream is split to form the first outer layer and the second outer layer of a three-layer coextruded film. In some embodiments, a second polyimide stream is filtered and then pumped to a casting die, such that the central polyimide core layer of a three-layer coextruded film is formed. The flow rates of the solutions may be adjusted to achieve the desired layer thickness.
[0056] In some embodiments, the multilayer film is prepared by simultaneous extrusion of the first outer layer, the core layer, and the second outer layer. In some embodiments, the layers are extruded through a single-cavity or multi-cavity extrusion die. In another embodiment, the multilayer film is produced using a single-cavity die. If a single-cavity die is used, the laminar flow of the streams must be of a sufficiently high viscosity to prevent mixing of the streams and provide uniform lamination. In some embodiments, the multilayer film is prepared by casting from the slotted die onto a moving stainless steel belt. In one embodiment, the belt is then passed through a convection oven, to evaporate the solvent and partially imidize the polymer, to produce a "green" film. The green film may be removed from the casting belt and wound. The green film may then be passed through a stretching oven to produce a fully cured polyimide film. In some embodiments, during stretching, shrinkage may be minimized by constraining the film along the edges (i.e., using clamps or pins).
[0057] In one embodiment, the outer layers of the present invention may also be applied to the core layer during an intermediate step of polyimide film manufacturing, for example on a gel film or on a green film.
[0058] When forming a polyimide film, the term "gel film" refers to a sheet of polyamic acid, which is loaded with volatile compounds, primarily solvents, to such an extent that the polyamic acid is in a swollen or rubbery gel state, and can be formed in a chemical conversion process. The volatile content is usually in a range of 70 to 90% by weight and the polymer content is usually in a range of 10 to 30% by weight of the gel film. The final film becomes "self-supporting" at the gel film stage. It can be removed from the support on which it was cast and heated to a final curing temperature. The gel film generally has an amic acid to imide ratio of between 10:90 and 50:50, most commonly 30:70.
[0059] The gel film structure may be prepared by the method described in U.S. Patent No. 3,410,826. The invention relates to mixing a chemical conversion agent and a catalyst, such as a lower fatty acid anhydride and a tertiary amine, into the polyamic acid solution at a low temperature. This is followed by casting the polyamic acid solution as a film onto a casting drum. The film is slightly heated after casting, for example to 100°C, to activate the conversion agent and catalyst to transform the cast film into a polyamic acid / polyimide gel film.
[0060] Another type of polymer film is a "green film" which, for a polyimide film, is partly polyamic acid and partly polyimide, and may be formed in a thermal conversion process. A green film typically contains about 50 to 75% by weight of polymer and 25 to 50% by weight of solvent. In general, it should be strong enough to be substantially self-supporting. The green film may be prepared by casting the polyamic acid solution as a film onto a suitable support such as a drum or casting belt and removing the solvent by gentle heating to a temperature of up to 150°C. A small proportion of amic acid units in the polymer, for example up to 25%, may be converted to imide units.
[0061] The application of the polyimide films of the present invention can be carried out in several ways. Such methods include the use of a slot die, dip coating or transfer roller coating on a film followed by addition using a doctor's knife, doctor rollers, compression rollers, or an air knife. The coating can also be applied by brushing or spraying. Using such techniques, it is possible to prepare laminates coated on both sides. In preparing double-sided coated structures, coatings can be applied to both sides of a polymer either simultaneously or consecutively before proceeding to the polymer curing and drying step.
[0062] The electrically insulating and corona-resistant composite filler (a dispersion or colloid thereof) may be added at several points in the preparation of the polyimide film. In one embodiment, the colloid or dispersion is incorporated into a prepolymer having a Brookfield solution viscosity in the range of about 50-100 poise at 25°C. By "prepolymer" is meant a lower molecular weight polymer, typically made with a small stoichiometric excess (in the order of 2-4%) of diamine monomer (or an excess of dianhydride monomer). In an alternative embodiment, the colloid or dispersion may be combined directly with the monomers, in which case polymerization occurs with the filler present during the reaction. In another embodiment, the colloid or dispersion may be combined with the "finished" high viscosity polyimide.The monomers may have an excess of either monomer (diamine or dianhydride) during this "in situ" polymerization. The monomers may also be added in a 1:1 ratio. In the case where the monomers are added with either the amine (case i) or the dianhydride (case ii) in excess, the increase in molecular weight (and solution viscosity) can be achieved, if necessary, by adding additional amounts of dianhydride (case i) or diamine (case ii) to approach the 1:1 stoichiometric ratio of dianhydride to amine.
[0063] The thickness of the polyimide film may be adjusted, depending on the intended use of the film or the specifications of the end application. In one embodiment, the polyimide film has a total thickness in a range of 2 to 300 μm, 5 to 200 μm, 10 to 150 μm, 20 to 100 μm, or 20 to 80 μm. Fluoropolymer coatings
[0064] In one embodiment, the polyimide film having an electrically insulating and corona-resistant composite filler has a first fluoropolymer coating adhered to a first side of the polyimide film and a second fluoropolymer coating adhered to a second side of the polyimide film. One fluoropolymer coating is used to bond the polyimide film to a metal layer or wire, such as a stranded conductor. The other fluoropolymer coating is used to bond the polyimide film to an outer shell, such as a fluoropolymer tape.
[0065] In one embodiment, a base film strip comprises the polyimide film having a first and a second fluoropolymer coating. In one embodiment, the base film strip may be used as an inner wrap for an electrically insulated wire or cable comprising a stranded conductor. In one embodiment, the base film strip has a thickness in a range of 25 µm to 40 µm as measured in the unwrapped state.
[0066] In one embodiment, the fluoropolymer coatings comprise fluoropolymers selected from the group consisting of tetrafluoroethylene-hexafluoropropylene (FEP) copolymer, perfluoroalkoxy (PFA) resin, polytetrafluoroethylene (PTFE), or mixtures thereof. In one embodiment, a fluoropolymer coating comprises FEP in an amount in a range of 65 to 100 weight percent based on the total weight of the fluoropolymer coating. In one embodiment, the fluoropolymer coating comprises FEP in an amount in a range of (and optionally including) any two of the following: 65, 70, 75, 80, 85, 90, 95, and 100 weight percent based on the total weight of the fluoropolymer coating.In one embodiment, the first fluoropolymer coating, the second fluoropolymer coating, or both are in direct contact with the polyimide film, such that there are no interlayers between the fluoropolymer coatings and the polyimide film. In one embodiment, the fluoropolymer coating comprises 100 weight percent FEP. In one embodiment, the fluoropolymer of the first fluoropolymer coating and the fluoropolymer of the second fluoropolymer coating are not individually crosslinked. In one embodiment, the first fluoropolymer coating and the second fluoropolymer coating are the same or different.
[0067] The fluoropolymer coating will generally have a thickness in a range between (and optionally including) two of the following numbers: 0.25, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.25, 1.5, 1.75, 2, 3, 4, 5, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24 and 25 µm. A useful thickness range is often in the range of about 0.75 µm to 2.5 µm (generally in the range of about 0.03 to about 0.10 mil). In practice, the desired thickness may depend on specifications, particularly for military or commercial aircraft applications.
[0068] In some embodiments, the fluoropolymer coating may be applied to the polyimide film by, but not limited to, solution coating, colloidal dispersion coating, or lamination.
[0069] The surface of the polyimide film may be modified to improve adhesion to other layers, such as the fluoropolymer coating. Examples of useful surface modification include, but are not limited to, corona treatment, atmospheric pressure plasma treatment, reduced pressure plasma treatment, treatment with coupling agents such as silanes and titanates, sandblasting, alkali treatment, and acid treatment.
[0070] The fluoropolymer coating of the present disclosure may include flame retardants and thermally conductive fillers, as well as fillers to tailor the opacity, color, and rheology of the fluoropolymer coating.
[0071] In some embodiments, the fluoropolymer coating may contain a silane of the structure R^SifOR2^ m, wherein m is 0, 1, 2, or 3. R2 is a C1-C4 alkyl group or a C1-C4 acyl group. RI is a C1-C20 alkyl, a C6-C30 aryl group, or a C5-C20 aliphatic group, each of which may optionally contain one or more heteroatoms as substituents. The term "one or more heteroatoms," as used herein, refers to one or more of the following: (1) halogen, such as fluorine; (2) an ester group, such as an acrylate group, a methacrylate group, an amine group, an imine group, a fumarate group, and a maleate group; (3) a urethane group; and (4) a vinyl ether group.
[0072] In some embodiments, the fluoropolymer coating may contain an inorganic filler such as silica, alumina, titanium dioxide, and / or zirconia. The filler may be the same as or different from that present in the polyimide film. The filler may be present in a range of 1 to 10% by weight based on the dry weight of the coating. If more than one fluoropolymer coating is present on a polyimide film, each fluoropolymer coating may be independently filled or unfilled.
[0073] In some embodiments, the thickness of a fluoropolymer coating does not exceed the thickness of the polyimide film. In one embodiment, the thickness ratios of the fluoropolymer coatings to the polyimide film are each individually less than 0.5:1, or less than 0.4:1, or less than 0.3:1, or less than 0.2:1. In one embodiment, a thickness ratio of the first fluoropolymer coating to the polyimide film and a thickness ratio of the second fluoropolymer coating to the polyimide film are each individually in a range of from 0.01:1 to 0.5:1, or from 0.03:1 to 0.3:1, or from 0.05:1 to 0.2:1. Fluoropolymer strips
[0074] In one embodiment, a fluoropolymer tape comprises polytetrafluoroethylene (PTFE). In one embodiment, a fluoropolymer tape comprises a blend of FEP and perfluoroalkoxy (PFA) resin, a blend of FEP and PTFE, or a blend of FEP, PFA, and PTFE. Electrically insulated wires and cables
[0075] In one embodiment, an electrically insulated wire or cable having an electrically insulating and corona resistant composite filler is useful as a wire wrap. In some embodiments, the wire wrap may contain additional layers, such as adhesive layers or scrape abrasion resistant layers. The wire wrap films or sheets may be slit into narrow widths to provide strips. These strips may then be wrapped around an electrical conductor in a spiral manner or in an overlapped manner. The overlap rate may vary depending on the angle of the wrap. In one embodiment, the overlap rate does not exceed 66%.The tension employed during the wrapping operation can also vary widely, ranging from just enough tension to prevent wrinkling, to tension high enough to stretch and tighten the tape. Even when the tension is low, a tight wrap is possible since the tape often shrinks under the influence of heat during any subsequent heat sealing operation. Heat sealing of the tape can be accomplished by treating the tape-wrapped conductor at a temperature and for a time sufficient to fuse the bonding layer to the other layers in the composite. The required heat sealing temperature is typically in the range of 240, 250, 275, 300, 325 or 350°C to 375, 400, 425, 450, 475 or 500°C, depending on the insulation thickness, metallic conductor gauge, production line speed and seal length.In one embodiment, the wound wire is designed for voltages up to 600 V and has properties meeting or exceeding those listed in SAE AS22579™, particularly AS22579™ / 80-82 and AS22579™ / 86-92.
[0076] In one embodiment, a cross-section of a wound wire generally has a certain contact length between insulation, such as an inner jacket, and individual strands of the wire. The term "contact length," as used herein, refers to the percentage of the length of the inner jacket that is in intimate contact with the outer surface of the stranded conductor. In the case of a solid (i.e., non-stranded) wire, the contact length is essentially 100%. For a stranded conductor having fewer than 100 strands, the contact length will be in a range of 15 to 69%, while for a stranded conductor having more than 100 strands, the contact length will be in a range of 15 to 79%. For a concentric stranded conductor, the contact length will be in the range of 10-70% or 12-60%. The specific contact length will depend on a variety of factors, such as the nominal size of the stranded wire and the nominal wire size of the individual strands, the chemical nature of the polyimide as well as the fluoropolymer applied to the polyimide film and facing the individual strands, the temperature and pressure profiles applied during the wire wrapping process, the line speed, as well as the overlap rate and tension applied to the tape during the wrapping process. The specific mechanical properties of the polyimide, such as its mechanical response under compressive loads, are expected to influence the resulting contact length under a given set of specific processing values (temperature, line speed, pressure, etc.).It is known that the incorporation of fillers into a polyimide film can modify its mechanical response under compressive loads.
[0077] In one embodiment, a wound stranded conductor will contain void space within the wound wire that can be viewed in a cross-section of the construction. By "void space" is meant the space within the boundary formed by the jacket, such as an inner jacket, that is not occupied by the conductive material, such as a stranded conductor, or any other solid material. In one embodiment, the void space is occupied by air. The percentage of void space within a wound wire having a stranded conductor is in a range of 2 to 43%, based on the total space available within the jacket. The specific amount of void space present will depend on a variety of factors similar to those that affect contact length.
[0078] One of the advantages of using a corona resistant insulating film on a single stranded conductor is that the resulting construction has a significantly thinner overall diameter compared to similar performance solutions that use a non-corona resistant insulating film, thereby providing overall savings in space occupied and weight in any given application.
[0079] The advantageous properties of this invention can be observed by reference to the following examples which illustrate, but are not limited to, the invention. All parts and percentages are by weight unless otherwise indicated. Examples Testing methods Thickness
[0080] The thickness of the film samples was determined according to ASTM D374 using a pressure setting of 25 psi and an anvil size of 0.25 in. diameter. Endurance under tension
[0081] Voltage endurance was determined in accordance with ASTM D2275 using 0.5 in. diameter electrodes and reporting the median failure time from a sample set of 9 specimens. Test conditions included an applied voltage of 1.4 kV at 1 kHz. The specimens were wound with 10 turns and had a 1 1b weight attached to them. Scraping abrasion
[0082] A GE Repeated Scraper Abrasion Tester, Wellman Thermal Systems Catalog No. 158L238G1 was used with a stainless steel scraper having a 0.6 mm radial edge. A 1000 g weight rested on the scraper (including the weight of the arm). The test specimen was clamped in the tester to prevent lengthwise movement. A travel distance of 9.8 mm was used at a rate of 56 cycles per minute. The test was stopped when electrical contact was made between the weighted scraper and the bare conductor contained in the specimen, and the number of cycles achieved was noted. The average number of cycles for 5 locations tested on the same specimen is reported per specimen. The wire was moved 100 mm lengthwise and rotated 90 degrees between test locations. Dynamic cutoff
[0083] Determined in accordance with ASTM D-3032. The mean of 8 independent samples is reported. Example 1
[0084] For Example 1 (E1), a 1 mil (25.4 pm) polyimide film derived from pyromellitic dianhydride (PMDA) and 4,4'-diaminodiphenyl ether (ODA) and having 17 wt% Al2O3 filler was dispersion coated on both sides with a fluoropolymer coating of tetrafluoroethylene-hexafluoropropylene copolymer (FEP) containing 5.6 wt% TiO2 and 0.4 wt% silane (both based on the dry weight of the coating). The dry thickness of the FEP coating is 0.1 mil (2.54 pm) on each side of the polyimide film. The 1.2 mil (30.5 μm) coated film was slit to form a 5.5 mm wide base film strip and wrapped around a 20 gauge unilay nickel-plated copper alloy stranded conductor (Fisk Alloy Inc., Hawthome, NJ). The 19 / 32 unilay stranded conductor had a diameter of 37.6 mil (0.955 mm), and the base film strip was wrapped with a 53% overlap to form an inner jacket around the stranded conductor.A 2 mil (50.8 μm) thick PTFE fluoropolymer tape (available from 3M, St. Paul, MN), 6.35 mm wide, was used as the outer cover and had a 53% overlap. Comparative example 1
[0085] For Comparative Examples 1 (CEI), a 0.65 mil (16.5 pm) polyimide film derived from pyromellitic dianhydride (PMDA) and 4,4'-diaminodiphenyl ether (ODA) and paraphenylenediamine (PPD) (ODA to PPD weight ratio 2.777:1) was dispersion coated on both sides with a fluoropolymer coating mixture of tetrafluoroethylene-hexafluoropropylene copolymer (FEP) and PTFE (25:75 w / w) containing 6.5 wt% TiO2 and 0.4 wt% silane (both based on the dry weight of the coating). The dry thickness of the fluoropolymer coating was 0.1 mil (2.54 pm) on the first side of the polyimide film and 0.5 mil on the second side of the polyimide film. The 1.2 mil (30.5 pm) coated film was slit to form a 5.5 mm wide base film strip and wrapped around a 20 gauge unilay nickel-plated copper alloy stranded conductor.The base film tape was wrapped with a 53% overlap to form an inner jacket around the stranded conductor and the same 2 mil (50.8 pm) thick PTFE fluoropolymer tape of El was used as the outer jacket and also had a 53% overlap. Comparative example 2
[0086] For Comparative Examples 2 (CE2), a 0.65 mil (16.5 pm) polyimide film derived from pyromellitic dianhydride (PMDA) and biphenyltetracarboxylic acid dianhydride (BPDA) (weight ratio of PMDA to BPDA 1.074:1) and 4,4'-diaminodiphenyl ether (ODA) and paraphenylenediamine (PPD) (weight ratio of ODA to PPD 1.24:1) was dispersion coated on the first side with a fluoropolymer coating of tetrafluoroethylene-hexafluoropropylene copolymer (FEP) with a dry thickness of 0.1 mil, and then dispersion coated on the second side with a mixture of tetrafluoroethylene-hexafluoropropylene copolymer (FEP) and PTFE (25:75 w / w) fluoropolymer coating containing 6.5 wt% TiO2. The dry thickness of the fluoropolymer coating was 0.1 mil (2.54 pm) on the first side of the polyimide film and 0.5 mil on the second side of the polyimide film.The 1.2 mil (30.5 pm) coated film was slit to form a 5.5 mm wide base film strip and wrapped around a 20 gauge unilay nickel-plated copper alloy stranded conductor. The base film strip was wrapped with a 53% overlap to form an inner jacket around the stranded conductor and the same 2 mil (50.8 pm) thick PTFE fluoropolymer strip of El was used as the outer jacket and also had a 53% overlap. Comparative example 3
[0087] For Comparative Examples 3 (CE3), a 20 gauge unilay nickel-plated copper alloy stranded conductor carrying a 48.8 µm thick crosslinked ETFE insulating layer was used. XL-ETFE is processed using the same techniques used to develop other thermoplastics (e.g., heat sealing, thermoforming, laminating, and cutting). XL-ETFE, when applied as wire insulation, has typical properties as described in SAE AS22759™, particularly AS22759™ / 32-35 and AS22759™ / 41-46. Insulated stranded wire incorporating XL-ETFE is available from Allied Wire and Cable (Collegeville, PA), Mouser Electronics (Mansfield, TX), Marmon Aerospace & Defense, LLC (Naples, FL), and TE Connectivity (Switzerland). Most grades of ETFE are designed for continuous use at 150°C.
[0088] The examples are summarized in Table 1 below. The electrically insulated wire of El is far superior to those made using a typical envelope structure (CE1-CE3) of comparable thicknesses. [Tables 1] Example Scraping Abrasion (Number of Cycles) Dynamic Cutting (Newtons) Tensile Endurance (Hours to Failure) El 702 91.8 147.6 IEC 150 58.9 7.1 CE2 206 77.5 5.4 CE3 491 71.6 58.2
Claims
Claims
1. An electrically insulated wire or cable comprising: a stranded conductor; an inner jacket around the stranded conductor, the inner jacket comprising a base film strip, the base film strip comprising: a polyimide film having an electrically insulating and corona-resistant composite filler; a first fluoropolymer coating adhered to a first side of the polyimide film; and a second fluoropolymer coating adhered to a second side of the polyimide film; and an outer jacket surrounding the inner jacket, the outer jacket comprising a fluoropolymer strip, the electrically insulated wire or cable having a void space in a range of 2 to 43%, based on the total space available within the inner jacket.
2. An electrically insulated wire or cable according to claim 1, wherein the stranded conductor comprises a copper or copper alloy wire, the copper or copper alloy being coated with a metal selected from tin, silver, nickel or being coated with an alloy of these metals or a mixture of these metals.
3. An electrically insulated wire or cable according to claim 1, wherein the electrically insulating and corona resistant composite filler is present in an amount in a range of 5 to 30 weight percent, based on the total weight of the polyimide film.
4. The electrically insulated wire or cable of claim 1, wherein the first fluoropolymer coating and the second fluoropolymer coating each individually comprise a fluoropolymer selected from the group consisting of a tetrafluoroethylene-hexafluoropropylene copolymer, a perfluoroalkoxy resin, a polytetrafluoroethylene, or a mixture thereof.
5. An electrically insulated wire or cable according to claim 1, wherein the stranded conductor has less than 100 strands and a contact length between the inner sheath and the stranded conductor is in a range of 15 to 69%.
6. An electrically insulated wire or cable according to claim 1, wherein the stranded conductor has more than 100 strands and a contact length between the inner sheath and the stranded conductor is in a range of 15 to 79%.
7. An electrically insulated wire or cable according to claim 1, wherein the stranded conductor is a concentric multi-strand conductor and has a contact length between the inner jacket and the stranded conductor in a range of 10 to 70%.
8. An electrically insulated wire or cable according to claim 1, wherein the electrically insulating and corona resistant composite filler comprises an organic component and an inorganic ceramic oxide component.
9. An electrically insulated wire or cable according to claim 8, wherein a weight ratio of the organic component to the inorganic ceramic oxide component is in a range of from 0.01:1 to 1-1
10. An electrically insulated wire or cable according to claim 1, wherein a thickness ratio of the first fluoropolymer coating to the polyimide film and a thickness ratio of the second fluoropolymer coating to the polyimide film are each individually in a range of 0.01:1 to 0.5:1.