Consolidation of a fibrous preform

The described process simplifies the consolidation of fibrous preforms by using a porosity mask and fugitive material, addressing the limitations of conventional tooling in ceramic matrix composite production, achieving efficient and cost-effective manufacturing with controlled porosity.

FR3147804A1Pending Publication Date: 2024-10-18SAFRAN CERAMICS SA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
FR2023003632
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Conventional conformation tooling for consolidating fibrous preforms in the production of ceramic matrix composites is costly, fragile, has a limited lifespan, and requires frequent replacement, complicating the manufacturing process.

Method used

A process involving shaping a fibrous preform in a mold with a fugitive material, applying a porosity mask, coating with a slip, heat treating to form a shell, and eliminating the mask and fugitive material, followed by chemical vapor infiltration, allowing for controlled porosity and simplified tooling.

Benefits of technology

Enables cost-effective and homogeneous consolidation of fibrous preforms with controlled porosity, reducing manufacturing complexity and tooling costs while maintaining mechanical properties at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Consolidation of a fibrous preform The invention relates to a process for consolidating a fibrous preform comprising at least the following steps: a- shaping a fibrous preform (10) in a mold (S5), the fibrous preform being previously impregnated (S4) with a fugitive or fugitive material (30), or shaping a preform in a mold (S2) and injecting a fugitive or fugitive material into the fibrous preform held in shape in the mold (S3); b- demolding (S6) the solidified fibrous preform (40); c- deposition (S8) of one or more porosity masks (50); d- coating (S9) with a slip (60); e- heat treatment (S11) to consolidate the slip; f- removal of the porosity mask; g- removal of the fugitive or fugitive material; and h- consolidation (S12) by a chemical vapor-phase infiltration process. Figure for the abstract: Fig. 1.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Consolidation of a fibrous preform Technical field

[0001] The present disclosure relates to methods for consolidating fiber preforms, and the manufacture of composite materials, in particular ceramic matrix composite materials (also known as “CMC materials” or more simply “CMC”). Prior art

[0002] A field of application of the invention is the production of parts intended to be exposed in service to high temperatures, in particular in the aeronautical and space fields, in particular parts of hot parts of aeronautical turbomachines, it being noted that the invention can be applied in other fields, for example the field of industrial gas turbines.

[0003] CMC materials have good thermostructural properties, i.e. high mechanical properties which make them suitable for forming structural parts and the ability to retain these properties at high temperatures.

[0004] Due to their better resistance to high temperatures, CMCs require less cooling. This cooling traditionally comes from a sample in the compressor which impacts the efficiency of the turbomachine, CMC materials therefore make it possible to improve engine efficiency which reduces fuel consumption.

[0005] Furthermore, the use of ceramic matrix composite materials contributes to optimizing the performance of turbomachines, in particular by reducing the overall mass of the turbomachine, which further contributes to a reduction in fuel consumption and therefore to a significant reduction in pollutant emissions.

[0006] A well-known method for manufacturing parts from CMC material comprises the following steps: - weaving of a fibrous preform from fibrous layers of carbon or silicon carbide (SiC) fibers, - consolidation of a fiber preform by depositing an interphase on the surface of the fibers of the preform produced by chemical gas infiltration (CVI), the fiber preform being held in a shaping tool during the CVI, - injection of a slip into the fiber preform (“Slurry Cast” or “Slurry Transfer Molding”), - infiltration of the preform with a molten silicon-based composition so as to form a ceramic matrix, a densification process known as the MI process ("Melt Infiltration"). The process may optionally also include one or more of the following finishing steps: - machining, - formation of a coating.

[0007] This method of manufacturing parts in CMC material requires the use of shaping tooling during the deposition of the interphase. This type of tooling corresponds to a multi-perforated mold whose internal shape makes it possible to shape the fiber preform and fix it in its geometry and whose multi-perforations allow the gas phase used during the deposition of the interphase to penetrate into the preform and consolidate it. The shaping tooling is made, for example, of graphite because it is a material compatible with the reactive atmosphere used during the deposition of the interphase while being harmless with respect to carbon or silicon carbide fibers.

[0008] This type of shaping tooling, however, has the following disadvantages: - high cost (machining of refined graphite blocks), - fragility (risk of breakage when tightening the graphite blocks, poor mechanical resistance to stress), - limited lifespan (clogging of multi-perforations and clamping systems), - need to frequently replace the tool clamping elements, - significant bulk due to the clamping devices used to assemble and tighten the tools.

[0009] Improvements to conformers have already been proposed, in particular to improve their lifespan or reduce their production costs.

[0010] For example, application WO2018 / 162827 envisages forming conformers around a preform filled with a fugitive material with a slip.

[0011] This method is not, however, fully satisfactory, in particular since porosities must be pierced in the formed conformer to allow the passage of the gas phase allowing the consolidation of the preform.

[0012] However, it was found that drilling was likely to cause deterioration of the preform contained in the conformer and did not offer an optimal solution.

[0013] Alternatively, document WO2018 / 162827 proposes the production of channels at means of local fusible growths which are removed after sintering of the shell.

[0014] The positioning of these protrusions nevertheless implies an additional complexity of the manufacturing process of the conformer which is incompatible with the desired industrial rate.

[0015] Therefore, there remains a need for improvement of the conformers used for the consolidation of fiber preforms used for the manufacture of composite materials. Statement of the invention

[0016] The invention aims to address the problems set out above, and for this purpose proposes a method for consolidating a fiber preform without the disadvantages of the prior art.

[0017] Thus, according to a first of its aspects, the invention relates to a method for consolidating a fiber preform intended for the manufacture of a part made of composite material comprising at least the following steps: a- shaping a fiber preform in a mold, the fiber preform being previously impregnated with a fugitive or fugitive material, or shaping a preform in a mold and injecting a fugitive or fugitive material into the fiber preform held in shape in the mold; b- demolding of the frozen fiber preform; c- the deposition on one or more surfaces of the frozen fiber preform of one or more porosity masks; d- coating of the fiber preform covered with the porosity mask by a slip; e- heat treatment of the coated fibrous preform to form a shell by consolidation of the slip; f- a step of removing the porosity mask; g- a step of eliminating the fugitive or fugitive material; and h- consolidation of the fiber preform by a chemical vapor infiltration process.

[0018] The consolidation of a fiber preform is understood as a partial densification thereof. The consolidation of a fiber preform is generally carried out with the aim of obtaining a self-supporting fiber preform, that is to say one which no longer needs another element to hold its shape.

[0019] The consolidation of a fiber preform corresponds to a deposition of an interphase and / or a first matrix phase in the internal porosity of the fiber preform, but up to a porosity filling rate less significant than that which will be reached during the densification of the preform, which densification will make it possible to obtain the final composite material part. For example, the fiber preform initially comprises an internal porosity of between 55% and 70% by volume.

[0020] In one embodiment, the consolidation process allows filling of the internal porosity of the fiber preform such that the internal porosity after the consolidation process is between 40% and 60%.

[0021] The final part, after densification, will have a residual porosity less than or equal to 1%.

[0022] The consolidation can be carried out by a chemical vapor infiltration process in a manner known per se. The method of the invention, however, allows a consolidation process in which the former, i.e. the part in which the preform will be during consolidation, is obtained in a simpler manner, regardless of the geometry of the fiber preform, while presenting a reduced cost compared to the formers of the prior art.

[0023] Indeed, unlike the consolidation methods of the prior art, the method of the invention makes it possible to obtain the conformer directly around the fiber preform, thus ensuring a conformer adapted to the geometry of the preform. In addition, the conformer used in the method of the invention has an open porosity that is much better controlled than that of the conformers of the prior art, thus ensuring a more homogeneous distribution of the matrix formed in the internal porosity of the fiber preform during the consolidation step.

[0024] The particular choice of a porosity mask in fact makes it possible to precisely define the desired geometry for the porosity of the shaper, and the specificities of the geometry of the fiber preform can thus be taken into account from the manufacture of the shaper.

[0025] Indeed, it is the elimination of the porosity mask which ensures the creation of a porosity network in the conformer, formed by consolidation of the shell.

[0026] In one embodiment, the mask may be a regular mesh composed of parallel guide lines extending in two intersecting directions, intersecting and forming after elimination a continuous two-dimensional network of porosity, for example the mask may be composed of vertical and horizontal lines.

[0027] In one embodiment, the mask comprises lines in a horizontal or vertical dimension, but the thickness is variable so as to form greater porosities in certain locations after removal of the mask.

[0028] The shape of the mask is not limiting and makes it possible to precisely define the desired porosity for the shell because it is the elimination of the mask which will be at the origin of the porosity network created in the shell.

[0029] In one embodiment, step e- of consolidation of the slip is carried out before step f- of elimination of the porosity mask and before step g- of elimination of the fugitive or fugitive material.

[0030] This embodiment makes it possible to ensure that the fiber preform retains the desired shape during step f- of removing the porosity mask and step g- of removing the fugitive or fugitive material.

[0031] It should be noted, however, that the slip, once dried, can allow the preform fibrous to maintain the desired shape.

[0032] It is then possible in one embodiment to carry out step e- of consolidation of the slip during or after step g- of elimination of the fugitive or fugitive material.

[0033] In one embodiment, step f- of removing the porosity mask is carried out before step g- of removing the fugitive or fugitive material. Such an embodiment makes it possible to ensure excellent removal of the fugitive or fugitive material.

[0034] Alternatively or additionally, step f- of removing the porosity mask and step e- of heat treatment of the coated fiber preform to form a shell by consolidation of the slip are both carried out during a single heat treatment.

[0035] For example, the method comprises a heat treatment step, which can be broken down into a first heating step f- comprising maintaining at a first temperature, the first temperature making it possible to eliminate the porosity mask.

[0036] The heat treatment step then comprises, and without returning to room temperature, a second heating step e- comprising maintaining at a sintering temperature, higher than the first temperature, this second heating step making it possible to form a shell by consolidation of the preform.

[0037] Similarly, in one embodiment, step g- of removing the fugitive or fugitive material and step e- of heat treatment of the coated fiber preform to form a shell by consolidation of the slip are both carried out during a single heat treatment.

[0038] For example, the method comprises a heat treatment step, which can be broken down into a first heating step g- comprising maintaining at a second temperature, the second temperature making it possible to eliminate the fugitive or fugitive material.

[0039] The heat treatment step then comprises, and without returning to room temperature, a second heating step e- comprising maintaining at a sintering temperature, higher than the second temperature, this second heating step making it possible to form a shell by consolidation of the preform.

[0040] In one embodiment, the method comprises a single heat treatment step which comprises a step f- of maintaining at a first temperature allowing the porosity mask to be eliminated, a step g- of maintaining at a second temperature higher than the first temperature allowing the elimination of the fugitive or fugitive material, then a step e- of maintaining at a sintering temperature, higher than the second temperature, allowing a shell to be formed by consolidation of the preform.

[0041] This embodiment is particularly applicable when using wax as a component of the porosity mask, due to its melting point being lower than that of the material that can be used to pre-consolidate a fiber preform, for example polyvinyl alcohol (PVA) or poly(methyl methacrylate) (PMMA) or PVA).

[0042] For example, step f- may be a step of maintaining at a temperature between 40 and 50°C for a duration between 1 hour and 3 hours.

[0043] For example, step g- may be a step of maintaining at a temperature between 50 and 450°C for a duration between 1 hour and 5 hours.

[0044] For example, step e- may be a step of maintaining at a temperature between 700 and 1300°C for a duration between 1 hour and 10 hours.

[0045] In one embodiment, steps f- and g- are carried out simultaneously during a single heating step at a temperature jointly allowing the elimination of the porosity mask and the fugitive or fugitive material.

[0046] In one embodiment, the porosity mask comprises one or more compounds chosen from: wax, for example foundry wax, a polyvinyl alcohol (PVA) or any other hydrodegradable or solvent-soluble or thermodegradable polymers with a low residue level, for example chosen from polystyrene, polymethylmethacrylate, polyethylene, polyvinylbutyral, naphthalene, starch, petroleum coke, sawdust or a mixture of two or more of the aforementioned compounds.

[0047] In one embodiment, the method may comprise, prior to step c-, a step of manufacturing the porosity mask by additive manufacturing.

[0048] For example, the porosity mask can be manufactured by fused deposition method (FDM), stereolithography or selective laser sintering (SLS).

[0049] Additive manufacturing of the porosity mask makes it possible to precisely define the geometry of the mask and therefore to more precisely define the geometry of the porosities in the conformer.

[0050] In one embodiment, the porosity mask can be formed by additive manufacturing directly on the surface of the preform, whether consolidated or not.

[0051] Alternatively, the porosity mask can be formed by injection, for example by means of a stencil placed on the consolidated or unconsolidated preform, the hollows of the stencil forming the geometry of the desired porosity mask.

[0052] The term “porosity” of the mask only means that the mask will be removed during a step of the process, and that it will leave room for a network of pores in the conformer.

[0053] Furthermore, the additive manufacturing of the porosity mask makes it possible to reduce the manufacturing cost of the porosity mask and therefore the cost of the entire process.

[0054] Throughout the application, the use of the singular for porosity mask should not be interpreted as the presence of a single porosity mask. It is understood that several porosity masks may be present.

[0055] In one embodiment, the fiber preform is covered with several porosity masks. Indeed, it is generally preferable for the consolidation to be homogeneous in the preform, and in one embodiment, a porosity mask covers each of the external surfaces of the fiber preform.

[0056] In one embodiment, the coating of the fiber preform carried out in step d-can be carried out so that the slip does not completely cover the porosity mask.

[0057] Thus, it is ensured that the shell formed by consolidation of the slip and elimination of the porosity mask has porosities emerging at the locations where the porosity mask was initially present.

[0058] In one embodiment, step d- of coating the frozen fiber preform and the porosity mask may comprise one or more times the repetition of at least the following sub-steps: dl-dipping the frozen fiber preform covered with the porosity mask into a slip; d2- drying of the fiber preform and the porosity mask obtained at the end of step dl; then d3- possibly, sandblasting the surface of the fiber preform obtained at the end of step d2.

[0059] The presence of a step d3 is preferable, to ensure that the porosity mask deposited on the surface of the frozen preform is exposed.

[0060] The choice of sandblasting parameters and in particular the choices of media, pressure, distance or even pass time are determined so as to allow the mask to be exposed without damaging it.

[0061] This will in fact be degraded during the subsequent step f-.

[0062] The possible repetition of the sub-steps described must be understood as the performance of several cycles each comprising a sub-step d1, followed by a sub-step d2 and possibly a sub-step d3.

[0063] Dipping the frozen fiber preform and the porosity mask into a slip makes it possible to deposit slip on the external surface of the preform which is not covered by the mask.

[0064] Drying ensures that the slip adheres well to the fiber preform and is not removed by gravity.

[0065] In one embodiment, the drying can be carried out by passing through an oven or a hot air dryer, at a temperature between 50 and 80°C and for a duration between 5 and 30 minutes.

[0066] In one embodiment, step d- may allow coating with a slip thickness greater than or equal to 4 mm.

[0067] For example, steps d1, d2 and possibly d3 are repeated until the desired slip thickness is obtained.

[0068] In one embodiment, the slip may comprise carbon C, silicon carbide SiC, oxides including zirconia ZrO2 or mullite, nitrides including silicon nitride Si3N4 or a mixture of two or more of these compounds.

[0069] In one embodiment, the slip may further comprise one or more sintering agents, for example chosen from Na2B4O7, B2O3, alumina A12O3, mullite or a mixture of two or more of these compounds.

[0070] In one embodiment, step d- of coating the fiber preform can be carried out by means of the following sub-steps: 1- the arrangement of the fiber preform covered with the porosity mask in an injection device, between an injection mold and an injection counter-mold; then 2- the injection of the slip into said injection device.

[0071] In such an embodiment, the mold and the injection counter-mold may be arranged on the porosity mask such that a space exists between the mold and the preform and between the counter-mold and the preform.

[0072] It is precisely in this space that the slip is injected during step 2.

[0073] In this way, it is ensured that the slip thickness is defined precisely, and it can be ensured, if necessary, that the slip does not cover the porosity mask at the end of step d-.

[0074] In one embodiment, step f- may be a step of chemical removal of the porosity mask.

[0075] For example, an alcohol or ketone in which the porosity mask is soluble can be used for chemical removal.

[0076] In one embodiment, this step can be carried out by soaking the fiber preform obtained at the end of step d- in a solution comprising butanone or an alcohol chosen from ethanol or isopropanol.

[0077] Preferably, a solution comprising butanone may be used when the mask comprises poly(methyl methacrylate) and a solution comprising an alcohol selected from ethanol or isopropanol may be used when the mask is made of wax.

[0078] In one embodiment, the method further comprises an additional step f'- chemical degradation of the porosity mask carried out after step d- and before step f-.

[0079] During such a step f'-, the preform coated with the mask and coated with slip is brought into contact with an element reactive with the mask, but inert with respect to the preform and the slip.

[0080] In one embodiment, step f' - can be carried out using the same reagents as those envisaged for carrying out a step f- by chemical elimination.

[0081] Step f' - can in particular be carried out by soaking the fibrous preform obtained at the end of step d- in a solution comprising butanone or an alcohol chosen from ethanol or isopropanol.

[0082] The reactive element makes it possible to degrade the porosity mask. This step f' - makes it possible to facilitate the subsequent step f- of removing the mask, for example by lowering the temperature necessary for its removal.

[0083] In one embodiment, the fibrous preform may comprise silicon carbide SiC fibers, silicon nitride Si3N4 fibers, or carbon fibers.

[0084] In one embodiment, the fiber preform may be a preform intended to form a ring sector, a turbine blade, a distributor (singlet, doublet or triplet) or any other component of a turbomachine subjected to temperatures above 900°C.

[0085] According to another of its aspects, the invention relates to a method for manufacturing a part made of composite material, the method comprising at least the steps of: - the consolidation of a fibrous preform produced using a process described above; - a step of unsticking the shell, - a step of densification of the porous preform.

[0086] For example, such a part may be a ring sector, a turbine blade, a distributor (singlet, doublet or triplet) or any other component of a turbomachine subjected to temperatures above 900°C. Brief description of the drawings

[0087] [Fig.l] [Fig.l] schematically represents a flowchart for carrying out a method in one embodiment of the invention.

[0088] [Fig.2] [Fig.2] represents a fiber preform useful for carrying out the method of the invention, in one of its embodiments.

[0089] [Fig.3] [Fig.3] represents a fiber preform useful for carrying out the method of the invention, in one of its embodiments.

[0090] [Fig.4] [Fig.4] represents a fiber preform after the production of a step S5 of an embodiment of the method.

[0091] [Fig.5] [Fig.5] represents a fiber preform after the production of a step S6 of an embodiment of the method.

[0092] [Fig.6] [Fig.6] schematically represents an embodiment of step S8 of the process.

[0093] [Fig.7] [Fig.7] represents a fiber preform after the production of a step S9 of an embodiment of the method.

[0094] [Fig.8] [Fig.8] schematically represents an embodiment of step S9 of the process.

[0095] [Fig.9] [Fig.9] shows a fiber preform in one embodiment of step SI 1 of the process.

[0096] [Fig. 10] [Fig. 10] schematically represents an embodiment of step S12 of the method. Description of the embodiments

[0097] The invention is now described by means of figures, present for descriptive purposes to illustrate certain embodiments of the invention and which should not be interpreted as limiting the latter. In particular, the figures are not presented to scale.

[0098] [Fig.l] illustrates a method in one embodiment of the invention.

[0099] Figures 2 to 10 are described hereinafter with reference to certain steps of the process.

[0100] A first step SI consists of producing a fiber preform 10 from which a fiber preform having a shape close to that of a part to be manufactured will be produced ([Fig.2]). Such a fiber preform 10 can be obtained by multi-layer or three-dimensional weaving from yarns or cables. It is also possible to start from two-dimensional fiber preforms such as fabrics or sheets of yarns or cables to form layers which will then be draped over a form and possibly linked together for example by sewing or implantation of yarns. In the example described in [Fig.2], the fiber preform 10 is intended to form a turbine ring sector made of CMC material having an inverted Pi or ir shape with an annular base from which two attachment tabs extend.For this purpose, the fiber preform 10 is produced by three-dimensional weaving of silicon carbide or carbon threads with the provision of decoupling zones 11 and 12 making it possible to separate parts of the preform 13 and 14 corresponding to the attachment flanges of the ring sector.

[0101] The effect of the debonding zones 11 and 12 is visible in [Fig.3] which represents the fiber preform in its final form.

[0102] The weave may be of the interlock type. Other three-dimensional or multi-layer weave weaves may be used, such as multi-plain or multi-satin weaves. Reference may be made in particular to document WO 2006 / 136755.

[0103] The fibers constituting the fiber preform are preferably ceramic fibers, for example fibers formed essentially from silicon carbide SiC (hereinafter referred to as SiC fibers) or silicon nitride Si3N4. It is possible in particular to use SiC fibers marketed under the names “Tyranno ZMI”, “Tyranno Lox-M” and “Tyranno S A3” by the Japanese company Ube Industries, Ltd or “Nicalon”, “Hi-Nicalon” and “Hi-Nicalon(S)” by the Japanese company Nippon Carbon. It is possible, as a variant, to use carbon fibers.

[0104] In a known manner, in the case of ceramic fibers, in particular SiC fibers, a surface treatment of these prior to the formation of an interphase deposit is preferably carried out to eliminate the sizing and a surface layer of oxide such as silica SiO2 present on the fibers.

[0105] Steps S2 and S3 or S4 and S5 together form step a- of a method of the invention. Together, these steps aim to maintain the shape of the fiber preform in a mold 20 and to freeze it to obtain a preform having a shape close to that of the part to be manufactured ([Fig.4]).

[0106] For this purpose, and as described in connection with [Fig. 4], the fiber preform is placed in a mold 20 whose molding cavity 21 corresponds to the shape of the part to be manufactured (step S2), a fugitive or fugitive material 30 being injected into the preform thus maintained in shape (step S3). According to an alternative implementation, the fiber preform 10 can be impregnated with a fugitive or fugitive material (step S4) before it is shaped in the mold (step S5).

[0107] The fugitive or fugitive material preferably has a melting and evaporation temperature significantly higher than room temperature (20°C ± 5°C), for example at least 50°C higher than room temperature (20°C ± 5°C). The fugitive or fugitive material may consist in particular of an injection wax or a fugitive resin, for example a PPMA acrylic resin or polyvinyl alcohol (PVA).

[0108] In one embodiment, the fugitive or fugitive material has the same composition as the porosity mask.

[0109] In one embodiment, the porosity mask is formed of wax beads, and the fugitive or fugitive material is wax of the same composition.

[0110] This embodiment makes it possible to simplify the method by carrying out steps f- and g- simultaneously.

[0111] At the end of step S3 or S5, a fiber preform 40 is demolded during step S6. The preform 40, shown in [Fig. 5], is then fixed and self-supporting thanks to the presence of the fugitive or fugitive material in the solid state therein.

[0112] Furthermore, the fugitive or fugitive material helps prevent slip particles from the subsequent step from penetrating the fiber preform.

[0113] In one embodiment, the mold may be heated for steps S2 to S5, which allows for easier circulation of the fugitive or fugitive material. If necessary, demolding S6 may be carried out after cooling of the mold.

[0114] The fibrous preform 40 thus formed is covered on one or more surfaces by a porosity mask 50.

[0115] For example, such a porosity mask 50 can be manufactured during an independent step of the method (step S7).

[0116] In one embodiment, visible in the figure, the porosity mask may be a regular mask formed of guidelines extending in two directions, here vertical and horizontal, and shaped to correspond to the surface of the preform.

[0117] Depending on the desired porosity, the mask can have a more or less dense regular mesh, or even an irregular mesh for certain areas which require lower or higher porosity.

[0118] For example, the manufacture of the porosity mask 50 is carried out by 3D printing.

[0119] This embodiment makes it possible to precisely define the desired mask according to of the porosity that we wish to obtain.

[0120] [Fig.6] represents step S8 of placing the porosity mask 50 on the fiber preform 40.

[0121] In the embodiment of [Fig.6], a porosity mask 50 is deposited on each of the external surfaces of the preform.

[0122] Once the porosity mask 50 has been deposited on the fiber preform 40, the assembly is coated with a slip 60 (step S9).

[0123] For example, the slip 60 comprises a powder of ceramic or carbon particles dispersed in a fluid, for example water.

[0124] In one embodiment, the particles may comprise oxide-type particles (silica, alumina, aluminosilicate, etc.), silicon carbide particles with or without colloidal silica, carbon particles, or a mixture of these particles.

[0125] A cluster assembly of several preforms 40 covered with the porosity mask 50 can be envisaged to increase production rates and reduce the unit manufacturing cost of the parts.

[0126] In one embodiment, step S9 can be carried out by several cycles of soaking in a slip bath and drying, for example in an oven.

[0127] This allows a progressive thickening of the slip layer 60 deposited at the surface of the fiber preform 40 and better control of its thickness.

[0128] In one embodiment, the slip 60 thus deposited does not exceed the porosity mask. In other words, starting from the surface of the preform, the slip 60 is present over a height smaller than or equal to the height of the porosity mask 50. Thus, the slip 60 does not cover the porosity mask 50 and it is ensured that the subsequent removal of the porosity mask allows direct access to the underlying fiber preform 40.

[0129] The preform obtained at the end of step S9 is shown in [Fig.7].

[0130] As an alternative to dipping in a slip bath, the coating step S9 of the preform 40 by a layer of slip 60 can take place by slip injection. Such an embodiment is shown in [Fig.8].

[0131] The preform 40 coated with a porosity mask 50 is arranged in an injection element comprising a mold 25 and a counter-mold 26. Slip 60 is introduced into the injection element formed from the mold 25 and the counter-mold 26.

[0132] Once the injection has been carried out, the slip 60 is dried, for example in an oven and the assembly is removed from the mold. This gives a preform 40 covered with a mask of porosity 50 and slip 60, identical to that shown in [Fig.7].

[0133] Optionally, this step may be followed by a step S10 of chemical degradation of the porosity mask 50, not shown.

[0134] The optional nature of step S10 is represented by the dotted lines in [Fig.l].

[0135] Such chemical degradation S10 of the porosity mask 50 can make it possible to completely eliminate the porosity mask 50 present on the surface of the fiber preform 40.

[0136] Alternatively, a step S10 of chemical degradation of the porosity mask 50 may have the objective of facilitating the subsequent decomposition thereof, in particular during the subsequent step SI 1 of heat treatment.

[0137] Whether or not step S10 of chemical degradation of the porosity mask 50 is carried out, the porosity mask 50 is, at the latest, eliminated by the heat treatment of step S11. For example, step S11 allows calcination of the material constituting the porosity mask 50.

[0138] The fiber preform 40 covered with the porosity mask 50, possibly degraded as just described, and coated with a layer of slip 60 is subjected to a heat treatment during step SI 1. This heat treatment step SI 1 makes it possible to sinter the particles present in the slip so as to consolidate the layer of slip coating the surface of the preform 40 and form a shell 61 around the preform 40.

[0139] Furthermore, during step S1 1, the fugitive or fugitive material contained in the fiber preform 40 is also removed. For this, the heat treatment of step SI 1 is carried out at a temperature above the melting and / or evaporation temperature of the fugitive or fugitive material.

[0140] The method of the invention allows a simplification of the methods of the prior art. Indeed, usually, vents making it possible to facilitate the evacuation of the fugitive or fugitive material must be provided in the shell surrounding the preform 40. However, in the method of the invention, since the elimination of the porosity mask 50 takes place during the same step SI 1 as the evacuation of the fugitive or fugitive material, such vents are not necessary.

[0141] [Fig.9] describes an example of the assembly formed by the fiber preform and the shaper obtained at the end of the heat treatment SI 1. In [Fig.9], the porous fiber preform 80 no longer comprises any fugitive or fugitive material and it is covered with a shaper formed by the shell 61, and which has open passages 51 making it possible to ensure the consolidation of the preform.

[0142] As can be seen in [Fig.9], the open passages 51 testify to the disappearance of the porosity mask 50.

[0143] The method further comprises a step of consolidating the fiber preform by chemical gas infiltration (step S12). For this purpose and as illustrated in [Fig. 10], the preform 80 held inside the shell 61 is placed in a chemical gas infiltration installation or furnace 200.

[0144] In a manner known per se, the gas phase chemical infiltration installation 200 comprises a cylindrical enclosure 201 delimiting a reaction chamber 210 closed in its upper part by a removable cover 220 provided with a gas inlet pipe 221 which opens into a preheating zone 222 making it possible to heat the gas before its diffusion into the reaction chamber 210 containing the preform(s) to be consolidated. The residual gases are extracted at the bottom 230 of the installation by an evacuation pipe 231 which is connected to suction means (not shown). The bottom 230 comprises a support 232 on which the preform 80 surrounded by the shell 61 is intended to be deposited.

[0145] The heating in the preheating zone as well as inside the reaction chamber 210 is produced by a graphite susceptor 211 forming an armature electromagnetically coupled with an inductor (not shown). The heating can also be implemented by a resistive system. In this case, a resistor forming a cage is crossed by a current, heats by the Joule effect and radiates the generated heat towards the useful zone.

[0146] The preform 80 is consolidated by chemical gas infiltration. In order to ensure the consolidation of the preform, a reactive gas containing at least one or more precursors of the material of a consolidation interphase is introduced into the reaction chamber 210.

[0147] Alternatively or additionally, it is also possible to consolidate the preform by adding an additional layer of matrix before detaching the shell.

[0148] The interphase deposited in the preform may be in particular pyrolytic carbon PyC, boron nitride BN, boron-doped carbon BC with 5 atomic% to 20 atomic% boron, the remainder being carbon, silicon carbide or a mixture of two or more of these compounds.

[0149] The thickness of the deposited interphase is preferably between 100 nm and 1500 nm. The total thickness of the interphase and the first matrix phase is chosen to be sufficient to consolidate the fiber preform, i.e. to bind the fibers of the preform together sufficiently so that the preform can be handled while retaining its shape without the assistance of holding tools. This thickness may be at least 300 nm. After consolidation, the preform remains porous, the initial porosity being filled, for example, only a minor part by the interphase and the first matrix phase.

[0150] The production of deposits of PyC, BC, B4C, Si-BC, Si3N4, BN and SiC by CVI is known. Reference may in particular be made to documents US 5,246,736, US 5,738,951, US 5,965,266, US 6,068,930 and US 6,284,358.

[0151] Once the consolidation is complete, the shell can be unstuck (step S13) and is mechanically destroyed in order to release a preform corresponding to the consolidated preform 80. The preform thus obtained is self-supporting and does not require any shape-holding tools for subsequent operations.

[0152] The preform may in particular be subjected to one or more of the following subsequent steps in the manufacture of a part made of CMC material:

[0153] - Additional densification, outside of shaping tools, with the materials mentioned for the interphase deposition step, including: PyC, BC, B4C, Si-BC, Si3N4, BN and SiC by CVI,

[0154] - an injection of a densification slip into the fiber preform ("Slurry Cast” or “Slurry Transfer Molding”),

[0155] - an infiltration of the preform with a composition based on molten silicon of in order to form a ceramic matrix, a densification process known as the MI process (for the English acronym of "Melt Infiltration"),

[0156] - one or more machining operations,

[0157] - the formation of a coating.

[0158] Such steps are known per se and are not described in further detail herein.

[0159] In an alternative implementation, the shell 61 can be preserved during the operations of injecting a slip and infiltration with a composition based on molten silicon.

Claims

Claims

1. Method for consolidating a fiber preform intended for the manufacture of a part made of composite material comprising at least the following steps: a- shaping a fiber preform (10) in a mold (S5), the fiber preform being previously impregnated (S4) with a fugitive or fugitive material (30), or shaping a preform in a mold (S2) and injecting a fugitive or fugitive material into the fiber preform held in shape in the mold (S3); b- demolding (S6) the set fiber preform (40); c- depositing (S8) on one or more surfaces of the set fiber preform one or more porosity masks (50); d- coating (S9) the fiber preform covered with the porosity mask with a slip (60); e- the heat treatment (SI 1) of the coated fibrous preform to form a shell (61) by consolidation of the slip; f- a step of eliminating the porosity mask;g- a step of removing the fugitive or fugitive material; and h- the consolidation (S 12) of the fibrous preform by a chemical vapor infiltration process.;

2. A method of consolidating a fiber preform according to claim 1, wherein the porosity mask (50) comprises one or more compounds chosen from: wax, for example foundry wax, polyvinyl alcohol (PVA) or any other hydrodegradable or solvent-soluble or thermodegradable polymers with a low residue level, for example chosen from polystyrene, polymethylmethacrylate, polyethylene, polyvinylbutyral, naphthalene, starch, petroleum coke, sawdust or a mixture of two or more of the above-mentioned compounds.

3. Method for consolidating a fiber preform according to claim 1 or 2, comprising a step (S7), prior to step c-, of manufacturing the porosity mask (50) by additive manufacturing.

4. Method for consolidating a fibrous preform according to any one of claims 1 to 3, in which step d- of coating the frozen fibrous preform (40) and the porosity mask (50) comprises one or more times the repetition of at least the following sub-steps: dl- soaking the frozen fiber preform covered with the porosity mask in a slip (60); d2- drying the fiber preform and the porosity mask obtained at the end of step dl; then d3- possibly, sandblasting the surface of the fiber preform obtained at the end of step d2.

5. Method for consolidating a fiber preform according to any one of claims 1 to 3, in which step d- of coating the preform is carried out by means of the following sub-steps: d' 1- the arrangement of the fiber preform (40) covered with the porosity mask (50) in an injection device, between an injection mold (25) and an injection counter-mold (26); then d' 2- the injection of the slip (60) into said injection device.

6. A method of consolidating a fiber preform according to any one of claims 1 to 5, wherein an additional step f - (S 10) of chemical degradation of the porosity mask (50) is carried out after step d- and before step f-.

7. Method for consolidating a fibrous preform according to claim 6, in which step f'- (S10) of chemical degradation of the porosity mask (50) prior to step f- is carried out by soaking the fibrous preform obtained at the end of step d- in a solution comprising butanone or an alcohol chosen from ethanol or isopropanol.

8. A method of consolidating a fiber preform according to one of claims 1 to 7, wherein said fiber preform (40, 80) comprises silicon carbide SiC fibers, silicon nitride Si 3N4 fibers, or carbon fibers.

9. Method for manufacturing a part made of composite material, the method comprising at least the steps of: - the consolidation of a fibrous preform (40, 80) produced by means of a method according to any one of claims 1 to 8; - a step of unsticking the shell (61), - a step of densifying the porous preform.

Citation Information

Patent Citations

  • Process for the manufacture of a refractory composite material protected against corrosion

    US5246736A

  • Method of manufacturing a composite material with lamellar interphase between reinforcing fibers and matrix, and material obtained

    US5738951A

  • Composite material protected against oxidation by a self-healing matrix, and a method of manufacturing it

    US5965266A

  • High-temperature composite materials with carbon or carbon-coated fibre reinforcements and enhanced oxidation resistance

    US6068930A

  • Textile preforms sheathed in a boron nitride coating, composites incorporating them and their preparation

    US6284358B1