Consolidation of a fibrous preform
A novel process for consolidating fibrous preforms using a fugitive material and blowing agents simplifies the manufacturing of CMC parts, addressing the limitations of conventional tooling and improving turbomachine efficiency and fuel consumption.
Patent Information
- Application Number
- FR2023003630
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-18
AI Technical Summary
Conventional conformation tooling for consolidating fibrous preforms in the production of ceramic matrix composite (CMC) materials is costly, fragile, has a limited lifespan, and requires frequent replacement, complicating the manufacturing process and increasing the bulk of turbomachines.
A process involving shaping a fibrous preform with a fugitive material, coating it with a slip containing blowing agents, heat treating to form a shell, and eliminating the blowing agent and fugitive material, followed by chemical vapor infiltration, allows for a simpler and more cost-effective consolidation without the need for complex tooling.
This process enables the production of CMC parts with reduced porosity and improved homogeneity, reducing manufacturing costs and tooling complexity while maintaining mechanical properties at high temperatures, enhancing turbomachine efficiency and reducing fuel consumption.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Title of the invention: Consolidation of a fibrous preform Technical field
[0001] The present disclosure relates to processes for consolidating fiber preforms, and the manufacture of composite materials, in particular with a ceramic matrix. Prior art
[0002] A field of application of the invention is the production of parts intended to be exposed in service to high temperatures, in particular in the aeronautical and space fields, in particular parts of hot parts of aeronautical turbomachines, it being noted that the invention can be applied in other fields, for example the field of industrial gas turbines.
[0003] CMC composite materials have good thermostructural properties, i.e. high mechanical properties which make them suitable for forming structural parts and the ability to retain these properties at high temperatures.
[0004] Due to their better resistance to high temperatures, CMCs require less cooling. This cooling traditionally comes from a sample in the compressor which impacts the efficiency of the turbomachine, CMC materials therefore make it possible to improve engine efficiency which reduces fuel consumption.
[0005] Furthermore, the use of ceramic matrix composite materials contributes to optimizing the performance of turbomachines, in particular by reducing the overall mass of the turbomachine, which further contributes to a reduction in fuel consumption and therefore to a significant reduction in pollutant emissions.
[0006] A well-known method for manufacturing parts from CMC material comprises the following steps: - weaving of a fibrous preform from fibrous layers of carbon or silicon carbide (SiC) fibers, - consolidation of a fiber preform by depositing an interphase on the surface of the fibers of the preform produced by chemical gas infiltration (CVI), the fiber preform being held in a shaping tool during the CVI, - injection of a slip into the fiber preform (“Slurry Cast” or “Slurry Transfer Molding”), - infiltration of the preform with a molten silicon-based composition so as to form a ceramic matrix, a densification process known as the MI process ("Melt Infiltration"). The method may optionally further comprise one or more of the steps of following finishing: - machining, - formation of a coating.
[0007] This method of manufacturing parts in CMC material requires the use of shaping tooling during the deposition of the interphase. This type of tooling corresponds to a multi-perforated mold whose internal shape makes it possible to shape the fiber preform and fix it in its geometry, and the perforations allow the gas phase used during the deposition of the interphase to penetrate into the preform and consolidate it. The shaping tooling is made, for example, of graphite because it is a material compatible with the reactive atmosphere used during the deposition of the interphase while being harmless with respect to carbon or silicon carbide fibers.
[0008] This type of shaping tooling, however, has the following disadvantages: - high cost (machining of refined graphite blocks), - fragility (risk of breakage when tightening the graphite blocks, poor mechanical resistance to stress), - limited lifespan (clogging of multi-perforations and clamping systems), - need to frequently replace the tool clamping elements, - significant bulk due to the clamping devices used to assemble and tighten the tools.
[0009] Improvements to conformers have already been proposed, in particular to improve their lifespan or reduce their production costs.
[0010] For example, application WO2018 / 162827 envisages forming conformers with a slip coated around a preform filled with a fugitive material.
[0011] This method is not, however, fully satisfactory, in particular since porosities must be pierced in the formed conformer to allow the passage of the gas phase enabling the conformation of the preform.
[0012] However, it has been found that drilling into the conformer is likely to cause deterioration of the preform contained in the conformer.
[0013] Alternatively, document WO2018 / 162827 proposes the production of channels at means of local fusible growths which are removed after sintering of the shell.
[0014] The positioning of these protrusions also involves additional complexity in the manufacturing process of the conformer which is incompatible with the desired industrial rate.
[0015] Therefore, there remains a need for improvement of the conformers used for the consolidation of fiber preforms used for the manufacture of materials composites. Statement of the invention
[0016] The invention aims to address the problems set out above, and for this purpose proposes a method for consolidating a fiber preform without the disadvantages of the prior art.
[0017] Thus, according to a first of its aspects, the invention relates to a method for consolidating a fiber preform intended for the manufacture of a part made of composite material comprising at least the following steps: a- shaping a fiber preform in a mold, the fiber preform being previously impregnated with a fugitive or fugitive material, or shaping a fiber preform in a mold and injecting a fugitive or fugitive material into the fiber preform held in shape in the mold; b- demolding of the frozen fiber preform; c- coating the fixed fibrous preform with a slip, said slip comprising one or more pore-forming agents, the mass content of pore-forming agent being between 25% and 75% relative to the total mass of the slip; d- heat treatment of the coated fibrous preform to form a shell by consolidation of the slip; e- a step of eliminating the pore-forming agent; f- a step of eliminating the fugitive or fugitive material; and g- consolidation of the fiber preform by a chemical vapor infiltration process.
[0018] The consolidation of a fiber preform is understood as a partial densification thereof. The consolidation of a fiber preform is generally carried out with the aim of obtaining a self-supporting fiber preform, that is to say one which no longer needs another element to hold its shape.
[0019] The consolidation of a fiber preform corresponds to a deposition of an interphase and / or a first matrix phase in the internal porosity of the fiber preform, but up to a porosity filling rate less significant than that which will be reached during the densification of the preform, which densification will make it possible to obtain the final composite material part.
[0020] In one embodiment, step d- of consolidation of the slip is carried out before step e- of elimination of the pore-forming agents and before step f- of elimination of the fugitive or fugitive material.
[0021] This embodiment makes it possible to ensure that the fiber preform retains the desired shape during step e- of removing the pore-forming agents and step f- of removing the fugitive or fugitive material.
[0022] It should be noted, however, that the slip, once dried, can allow the fiber preform to retain the desired shape. It is then possible to carry out step d- of consolidating the slip during or after step f- of removing the fugitive or fugitive material.
[0023] In one embodiment, step e- of removing the pore-forming agents is carried out before step f- of removing the fugitive or fugitive material. Such an embodiment makes it possible to ensure excellent removal of the fugitive or fugitive material.
[0024] For example, the fiber preform initially comprises an internal porosity of between 55% and 70% by volume.
[0025] In one embodiment, the consolidation process allows filling of the internal porosity of the fiber preform such that the internal porosity after the consolidation process is between 40% and 60%.
[0026] In one embodiment, the final part, after densification, will have a residual porosity less than or equal to 1%.
[0027] The consolidation can be carried out by a chemical vapor infiltration process in a manner known per se. The method of the invention, however, allows a consolidation process in which the former, i.e. the part in which the preform will be during consolidation, is obtained in a simpler manner, regardless of the geometry of the fiber preform, while presenting a reduced cost compared to the formers of the prior art.
[0028] Indeed, unlike the consolidation methods of the prior art, the method of the invention makes it possible to obtain the conformer directly around the fiber preform, thus ensuring a conformer adapted to the geometry of the preform. In addition, the conformer used in the method of the invention has an open porosity much higher than that of the conformers of the prior art, thus ensuring a more homogeneous distribution of the matrix formed in the internal porosity of the fiber preform during the consolidation step.
[0029] The particular choice of a slip comprising one or more pore-forming agents makes it possible to very finely control the porosity of the shaper, without requiring drilling of the fiber preform.
[0030] Throughout the present description, and unless otherwise stated, it will be understood that the term "pore-forming agent" may refer to a plurality of pore-forming agents and that the "pore-forming agent content" is understood, in the case where several pore-forming agents are present, as the sum of the contents for all of the pore-forming agents.
[0031] In one embodiment, the pore-forming agent(s) is(are) chosen from: polyvinyl alcohols, polystyrenes, wax, carbon fibers or a mixture of two or more of these compounds.
[0032] In one embodiment, step c- of coating the set fiber preform comprises one or more times the repetition of at least the following sub-steps: cl- dipping the set fiber preform in a slip comprising one or more pore-forming agents, the mass content being between 25% and 75% relative to the total mass of the slip; c2- drying of the fiber preform obtained at the end of step cl; then c3- possibly, sandblasting the surface of the fiber preform obtained at the end of step c2.
[0033] The possible repetition of the sub-steps described must be understood as the realization of several cycles each comprising the sub-steps described.
[0034] In this case, the possible repetition is understood as the possible repetition of a sub-step cl, followed by a sub-step c2 and possibly a sub-step c3 then a new sub-step cl, then c2 ... and so on.
[0035] In one embodiment, it is possible to pre-arrange masks that do not allow slip to adhere to the parts of the preform that are not to be coated with slip.
[0036] In one embodiment, these masks can be removed between two repetitions of step c-.
[0037] Such portions will be a function of the particular geometry of the preform, but the ability to achieve different pore-forming agent contents on different portions of the preform is a particular advantage of this embodiment as it allows the particular geometry of the preform to be taken into account in defining the porosity of the former.
[0038] Dipping the frozen fiber preform into a slip makes it possible to deposit slip on the external surface of the preform, where appropriate on the external surface of the preform which is not covered by the mask.
[0039] Drying c2- ensures that the slip adheres well to the fiber preform, and is not eliminated by gravity.
[0040] In one embodiment, there is more than one repetition of sub-steps c1-, c2- and optionally c3-, and the content of pore-forming agent varies in the slip of the different steps c1.
[0041] This embodiment makes it possible to vary the porosity in the thickness of the shaper precisely and in a chosen manner.
[0042] In an alternative embodiment, the arrangement of the masks can be varied between two iterations of step c1, which offers the possibility of achieving different porogenic agent contents on different parts of the preform. This is a particular advantage of this embodiment because it makes it possible to take into account the particular geometry of the preform in defining the porosity of the conformer.
[0043] In one embodiment, step c- of coating the frozen fiber preform comprises one or more times the repetition of at least the following sub-steps: c' 1- dipping the preform in a slip not comprising any pore-forming agent; c'2- the projection of one or more pore-forming agents onto the preform obtained at the end of step c' 1,; c'3- drying of the fiber preform obtained at the end of step c'2; then c'4- possibly sanding of the preform obtained at the end of step c'3; the total quantity of blowing agent projected representing between 25% and 75% of the total mass of the slip.
[0044] This embodiment makes it possible to precisely choose the quantity of pore-forming agent present as well as its distribution. In particular, this embodiment makes it possible to take into account the geometry of the preform and to adjust the quantity of pore-forming agent according to the precise location of the preform which is being covered.
[0045] Alternatively, it is possible to spray a pore-forming agent onto the entire preform, but to first place masks impermeable to said pore-forming agent on the parts of the preform which are not to be coated.
[0046] Such portions will be a function of the particular geometry of the preform, but the ability to achieve different pore-forming agent contents on different portions of the preform is a particular advantage of this embodiment as it allows the particular geometry of the preform to be taken into account in defining the porosity of the former.
[0047] It is also possible to carry out steps c'1, c'2, c'3 and possibly c'4 a plurality of times, and it is possible either to change the projected pore-forming agent between two iterations of step c'2, or to remove masks impermeable to the pore-forming agent between two iterations of step c'2. This makes it possible to define the distribution of the pore-forming agent very precisely, and therefore to define the porosity of the conformer very precisely.
[0048] In one embodiment, step c- of coating the frozen fiber preform comprises at least the following sub-steps: c” 1- the arrangement of the fixed fiber preform in an injection tool formed of a mold and a counter-mold; c”2- the injection into the mold of a slip comprising one or more pore-forming agents, the mass content of pore-forming agent being between 25% and 75% relative to the total mass of the slip.
[0049] This embodiment makes it possible to precisely control the thickness of the slip introduced onto the preform. Indeed, this thickness is controlled by the dimensioning of the injection tool.
[0050] In one embodiment, step c”2- is followed by a drying step, for allow good adhesion of the slip to the surface of the preform.
[0051] In one embodiment, the drying can be carried out by passing through an oven or a hot air dryer, at a temperature between 50°C and 80°C and for a duration between 5 minutes and 30 minutes.
[0052] In one embodiment, step c- may allow coating with a slip thickness greater than or equal to 2 mm.
[0053] In one embodiment, and regardless of the embodiment chosen for step c-, the slip may comprise alumina A12O3, silica SiO2, carbon C, silicon carbide SiC, oxides including zirconia ZrO2 or mullite, or nitrides including silicon nitride Si3N4 or a mixture of two or more of these compounds.
[0054] In one embodiment, the slip may further comprise one or more sintering agents, for example chosen from Na2B4O7, B2O3, alumina A12O3, mullite or a mixture of two or more of these compounds.
[0055] In one embodiment, the mass content of pore-forming agent in the slip coating the preform is between 35% and 50% relative to the total mass of the slip. This preferred content is a compromise considered optimal between excellent strength of the former and sufficient porosity thereof to facilitate consolidation of the fiber preform.
[0056] Furthermore, this content allows a suspension with excellent homogeneity.
[0057] In one embodiment, step e- of removing the pore-forming agent is carried out by chemical degradation.
[0058] During such a step, the preform coated and coated with slip comprising the pore-forming agent may be brought into contact with an element reactive with the pore-forming agent, but inert with respect to the preform and the slip.
[0059] This reactive element makes it possible to degrade the porogenic agent, in order to generate porosity in the shell.
[0060] In one embodiment, this step can be carried out by soaking the fiber preform obtained at the end of step c- in a solution of water or ethanol comprising a polyvinyl alcohol (PVA) or poly(methyl methacrylate) (PMMA). For example, the concentration of the solution is between 10 gL 1 and 20 gL *.
[0061] In this embodiment, the pore-forming agent is completely removed by chemical degradation. However, it is possible, according to other embodiments, to partially or completely remove the pore-forming agent by heat treatment.
[0062] In particular, in one embodiment, the method may comprise, before step e- of eliminating the pore-forming agent, a step e'- of chemical degradation of the pore-forming agent.
[0063] For example, step e'- makes it possible to degrade the properties of the pore-forming agent, the pore-forming agent only being completely eliminated during the subsequent step e-.
[0064] In one embodiment, step e- of removing the pore-forming agent can be carried out entirely during a heat treatment step.
[0065] Similarly, in one embodiment, step f- of removing the fugitive or fugitive material may be carried out by chemical degradation.
[0066] This step f- can in particular be carried out by soaking the fiber preform obtained at the end of step c- in a solution of water or ethanol comprising a polyvinyl alcohol (PVA) or even poly(methyl methacrylate) (PMMA). For example, the concentration of the solution is between 10 gL 1 and 20 gL *.
[0067] In this embodiment, the fugitive or fugitive material is completely removed by chemical degradation. However, it is possible, according to other embodiments, to partially or completely remove the fugitive or fugitive material by heat treatment.
[0068] In particular, in one embodiment, the method may comprise, before step f- of eliminating the fugitive or fugitive material, a step f' - of chemical degradation of the fugitive or fugitive material.
[0069] For example, step f'- makes it possible to degrade the properties of the fugitive or fugitive material, the fugitive or fugitive material only being completely eliminated during the subsequent step f-.
[0070] In one embodiment, step f- of removing the fugitive or fugitive material may be carried out entirely during a heat treatment step.
[0071] Furthermore, in one embodiment, step e- of removing the pore-forming agent and step d- of heat treatment of the coated fiber preform to form a shell by consolidation of the slip are both carried out during a single heat treatment.
[0072] For example, the method comprises a heat treatment step, which can be broken down into a first heating step e- comprising maintaining at a first temperature, the first temperature making it possible to eliminate the pore-forming agent.
[0073] The heat treatment step then comprises, and without returning to room temperature, a second heating step d- comprising maintaining it at a sintering temperature, higher than the first temperature, this second heating step making it possible to form a shell by consolidating the preform.
[0074] Similarly, in one embodiment, step f- of removing the fugitive or fugitive material and step d- of heat treatment of the coated fiber preform to form a shell by consolidation of the slip are both carried out during a single heat treatment.
[0075] For example, the method comprises a heat treatment step, which may be decomposed in a first heating step f- comprising maintenance at a second temperature, the second temperature making it possible to eliminate the fugitive or fugitive material.
[0076] The heat treatment step then comprises, and without returning to room temperature, a second heating step d- comprising maintaining at a sintering temperature, higher than the second temperature, this second heating step making it possible to form a shell by consolidation of the preform.
[0077] In one embodiment, the method comprises a single heat treatment step which comprises a step e- of maintaining at a first temperature allowing the elimination of the pore-forming agent, a step f- of maintaining at a second temperature, higher than the first temperature, allowing the elimination of the fugitive or fugitive material, then a step d- of maintaining at a sintering temperature, higher than the second temperature, allowing a shell to be formed by consolidation of the preform.
[0078] This embodiment is particularly applicable when using wax as a pore-forming agent, due to its melting point being lower than that of the material which can be used to pre-consolidate a fibrous preform, for example polyvinyl alcohol (PVA) or poly(methyl methacrylate) (PMMA) or PVA).
[0079] For example, step e- may be a step of maintaining at a temperature between 40°C and 50°C for a duration between 1 hour and 3 hours.
[0080] For example, step f- may be a step of maintaining at a temperature between 50 and 450°C for a duration between 1 hour and 5 hours.
[0081] For example, step d- may be a step of maintaining at a temperature between 700°C and 1300°C for a period of between 1 hour and 10 hours.
[0082] In one embodiment, steps e- and f- are carried out simultaneously during a single heating step at a temperature jointly allowing the elimination of the pore-forming agent and the fugitive or fugitive material.
[0083] In one embodiment, the pore-forming agents may have a form factor of between 1 and 10.
[0084] The form factor is here understood for an object as the ratio between its longest dimension and its smallest dimension. Thus, a perfectly spherical particle has a form factor of 1.
[0085] In one embodiment, the pore-forming agents are such that their smallest dimension is between 0.2 mm and 0.5 mm, and their largest dimension is between 0.2 mm and 2.0 mm.
[0086] For example, the pore-forming agents may have a form factor of between 1 and 2, and they will then be said to be substantially spherical.
[0087] In such an embodiment, the pore-forming agents may have a diameter, or in any case their largest dimension, between 0.2 mm and 2.0 mm.
[0088] In another embodiment, the form factor may be between 2 and 10.
[0089] In such an embodiment, the pore-forming agents may be such that their smallest dimension is between 0.2 mm and 0.5 mm, and their largest dimension is between 0.5 mm and 2.0 mm.
[0090] The inventors have found that these dimensions of the pore-forming agents make it possible to ensure in the shaper an excellent network of macropores which allows optimal consolidation of the fiber preform.
[0091] In one embodiment, the fibrous preform comprises silicon carbide SiC fibers, silicon nitride Si3N4 fibers, or carbon fibers.
[0092] In one embodiment, the fiber preform may be a preform intended to form a ring sector, a turbine blade, a distributor (singlet, doublet or triplet) or any other component of a turbomachine subjected to temperatures above 900°C.
[0093] In one embodiment, the fugitive or fugitive material has the same chemical composition as the pore-forming agent.
[0094] According to another of its aspects, the invention relates to a method for manufacturing a part made of composite material, the method comprising at least the steps of: - the consolidation of a fibrous preform produced using a process described above; - a step of unsticking the porous shell, - a step of densification of the porous preform.
[0095] In one embodiment, such a part may be a ring sector, a turbine blade, a distributor (singlet, doublet or triplet) or any other component of a turbomachine subjected to temperatures above 900°C. Brief description of the drawings
[0096] [Fig.l] [Fig.l] schematically represents a flowchart for carrying out a method in one embodiment of the invention.
[0097] [Fig.2] [Fig.2] represents a fiber preform useful for carrying out the method of the invention, in one of its embodiments.
[0098] [Fig.3] [Fig.3] represents a fiber preform useful for carrying out the method of the invention, in one of its embodiments.
[0099] [Fig.4] [Fig.4] represents a fiber preform subsequent to the performance of a step S5 of an embodiment of the method.
[0100] [Fig.5] [Fig.5] represents a fiber preform subsequent to the performance of a step S6 of an embodiment of the method.
[0101] [Fig.6] [Fig.6] schematically represents an embodiment of step S7 of the process.
[0102] [Fig.7] [Fig.7] schematically represents an embodiment of step S7 of the process.
[0103] [Fig.8] [Fig.8] represents a fiber preform after the production of a step S7 of an embodiment of the method.
[0104] [Fig.9] [Fig.9] represents a fiber preform after the production of a step S8 of an embodiment of the method.
[0105] [Fig. 10] [Fig. 10] schematically represents an embodiment of the step S9 of the process. Description of the embodiments
[0106] The invention is now described by means of figures, present for descriptive purposes to illustrate certain embodiments of the invention and which should not be interpreted as limiting the latter. In particular, the figures are not presented to scale.
[0107] [Fig.l] illustrates a method in one embodiment of the invention.
[0108] Figures 2 to 10 are described hereinafter with reference to certain steps of the process.
[0109] A first step SI consists of producing a fiber preform 10 from which a fiber preform having a shape close to that of a part to be manufactured will be produced ([Fig.2]). Such a fiber preform 10 can be obtained by multilayer or three-dimensional weaving from yarns or cables. It is also possible to start from two-dimensional fiber preforms such as fabrics or sheets of yarns or cables to form layers which will then be draped over a form and possibly linked together for example by sewing or implantation of yarns. In the example described in [Fig.2], the fiber preform 10 is intended to form a turbine ring sector made of CMC material having an inverted Pi or ir shape with an annular base from which two attachment tabs extend.For this purpose, the fiber preform 10 is produced by three-dimensional weaving of silicon carbide or carbon threads with the provision of decoupling zones 11 and 12 making it possible to separate parts of the preforms 13 and 14 corresponding to the attachment flanges of the ring sector.
[0110] The effect of the debonding zones 11 and 12 is visible in [Fig.3] which represents the fiber preform in its final form.
[0111] The weave may be of the interlock type. Other three-dimensional or multi-layer weave weaves may be used, such as multi-plain or multi-satin weaves. Reference may be made in particular to document WO 2006 / 136755.
[0112] The fibers constituting the fiber preform are preferably ceramic fibers, for example fibers formed essentially from silicon carbide SiC (hereinafter referred to as SiC fibers) or silicon nitride Si3N4. It is possible in particular to use SiC fibers marketed under the names “Tyranno ZMI”, “Tyranno Lox-M” and “Tyranno S A3” by the Japanese company Ube Industries, Ltd or “Nicalon”, “Hi-Nicalon” and “Hi-Nicalon(S)” by the Japanese company Nippon Carbon. It is possible, as a variant, to use carbon fibers.
[0113] In a known manner, in the case of ceramic fibers, in particular SiC fibers, a surface treatment of these prior to the formation of an interphase deposit is preferably carried out to eliminate the sizing and a surface layer of oxide such as silica SiO2 present on the fibers.
[0114] Steps S2 and S3 or S4 and S5 together form step a- of a method of the invention. Together, these steps aim to maintain the shape of the fiber preform in a mold 20 and to freeze it to obtain a preform having a shape close to that of the part to be manufactured ([Fig.4]).
[0115] For this purpose, and as described in connection with [Fig. 4], the fiber preform is placed in a mold 20 whose molding cavity 21 corresponds to the shape of the part to be manufactured (step S2), a fugitive or fugitive material 30 being injected into the preform thus maintained in shape (step S3). According to an alternative implementation, the fiber preform 10 can be impregnated with a fugitive or fugitive material (step S4) before it is shaped in the mold (step S5).
[0116] The fugitive or fugitive material preferably has a melting and evaporation temperature significantly higher than room temperature (20°C ± 5°C), for example at least 50°C higher than room temperature (20°C ± 5°C). The fugitive or fugitive material may consist in particular of an injection wax or a fugitive resin, for example a PPMA acrylic resin or polyvinyl alcohol (PVA).
[0117] In one embodiment, the fugitive or fugitive material has the same composition as the pore-forming agent.
[0118] In one embodiment, the pore-forming agent consists of wax beads, and the fugitive or fugitive material consists of wax of the same composition.
[0119] This embodiment makes it possible to simplify the method by carrying out steps e- and f- simultaneously,
[0120] At the end of step S3 or S5, a fiber preform 40 is demolded during step S6. The preform 40, shown in [Fig.5], is then fixed and self-supporting thanks to the presence of the fugitive or fugitive material in the solid state therein.
[0121] Furthermore, the fugitive or fugitive material helps prevent slip particles from the subsequent step from penetrating the fiber preform.
[0122] In one embodiment, the mold may be heated for steps S2 to S5, which allows for easier circulation of the fugitive or fugitive material. If necessary, demolding S6 may be carried out after cooling of the mold.
[0123] The self-supporting preform 40 is then coated with slip during a step S7.
[0124] Figures 6 and 7 show two distinct embodiments of such a step S7.
[0125] [Fig.6] illustrates a step of coating the preform 40 by dipping it in a bath slip comprising pore-forming agents.
[0126] As described above, the soaking step can be followed by a drying step and then possibly a sanding step.
[0127] For example, drying is carried out in an oven.
[0128] For example, sandblasting can be achieved by using a granular powder. lometry between 0.1 mm and 0.5 mm with an ejection pressure between 2 bars and 6 bars. The sandblasting media may be of the same nature as that used for the production of the shell (mullite or alumina), the stripping factor then being linked to the kinetics of the powder more than to the hardness of the projected material.
[0129] Optionally, all of these steps can be carried out several times, and the thickening of the slip layer is then progressive, by deposition, drying and possibly sandblasting of several elementary layers.
[0130] [Fig.8] illustrates a preform obtained at the end of step S7 and there is found a fibrous preform 40 coated with a slip 60 comprising pore-forming agents 50.
[0131] As shown in [Fig. 6] and as described above, the pore-forming agents may all be identical, or have a single composition but different form factors and dimensions, be of different compositions but identical dimensions, or even be of different composition and dimensions.
[0132] The particular choice of porogenic agents, their shapes and their compositions makes it possible to precisely define the porosity of the conformer and will be chosen according to what is desired.
[0133] Alternatively to the embodiment of [Fig.6], step S7 of coating the preform 40 with a layer of slip 60 can take place by slip injection. Such an embodiment is shown in [Fig.7].
[0134] The preform 40 is arranged in an injection element comprising a mold 25 and a counter-mold 26. Slip 60 comprising the pore-forming agents 50 is introduced into the injection element formed from the mold 25 and the counter-mold 26.
[0135] Once the injection has been carried out, the slip 60 is dried, for example in an oven and the assembly is removed from the mold. This gives a preform 40 covered with a slip 60 comprising pore-forming agents 50, identical to that of [Fig.8].
[0136] Alternatively, but not shown, the preform may be covered of a slip not including a pore-forming agent, then pore-forming agents are sprayed onto the coated preform.
[0137] For example, the projection can be done by means of a powder projection method known as such.
[0138] This embodiment is advantageous because it makes it possible to precisely define the quantity of pore-forming agent 50 projected, and makes it possible to modify the quantity according to the surface area of the preform considered.
[0139] The fiber preform 40 covered with a slip 60 comprising pore-forming agents 50 is subjected to a heat treatment during step S8. This heat treatment step S8 makes it possible to sinter the particles present in the slip so as to consolidate the slip layer coating the surface of the preform 40 and form a shell 61 around the preform 40. The shell 61 will play the usual role of the shaper in the remainder of the process.
[0140] In addition, this step S8 degrades the pore-forming agents present in the slip, for example by calcination.
[0141] Furthermore, during step S8, the fugitive or fugitive material contained in the fiber preform 40 is also removed. For this, the heat treatment of step S8 is carried out at a temperature higher than the melting and / or evaporation temperature of the fugitive or fugitive material.
[0142] At the end of the heat treatment step S8, the porous preform 80 is obtained, surrounded by the shaper 61 obtained by consolidation of the slip 60.
[0143] As shown in [Fig.9], the shaper 61 comprises pores 51, a consequence of the elimination of the pore-forming material.
[0144] The method of the invention allows a simplification of the methods of the prior art. Indeed, usually, vents making it possible to facilitate the evacuation of the fugitive or fugitive material must be provided in the shell surrounding the preform 40. However, in the method of the invention, since the elimination of the pore-forming agent 50 takes place during the same step S8 as the evacuation of the fugitive or fugitive material, such vents are not necessary.
[0145] The method further comprises a step g- of consolidating the fiber preform by chemical infiltration in the gas phase (step S9). For this purpose and as illustrated in [Fig. 10], the preform 80 held inside the former 61 is placed in a chemical infiltration installation or furnace in the gas phase 200.
[0146] In a manner known per se, the gas phase chemical infiltration installation 200 comprises a cylindrical enclosure 201 delimiting a reaction chamber 210 closed in its upper part by a removable cover 220 provided with a gas inlet pipe 221 which opens into a preheating zone 222 making it possible to heat the gas before its diffusion into the reaction chamber 210 containing the or the preforms to be consolidated. The residual gases are extracted at the bottom 230 of the installation by an evacuation pipe 231 which is connected to suction means (not shown). The bottom 230 comprises a support 232 on which the preform 80 surrounded by the shell 61 is intended to be deposited.
[0147] The heating in the preheating zone as well as inside the reaction chamber 210 is produced by a graphite susceptor 211 forming an armature electromagnetically coupled with an inductor (not shown). The heating can also be implemented by a resistive system. In this case, a resistor forming a cage is crossed by a current, heats by the Joule effect and radiates the generated heat towards the useful zone.
[0148] The preform 80 is consolidated by chemical gas infiltration. In order to ensure the consolidation of the preform, a reactive gas containing at least one or more precursors of the material of a consolidation interphase is introduced into the reaction chamber 210.
[0149] Alternatively or additionally, it is also possible to consolidate the preform by adding an additional layer of matrix before detaching the shell.
[0150] The interphase deposited in the preform may in particular be made of pyrolytic carbon or PyC, boron nitride (BN), boron-doped carbon or BC (with 5% at to 20% at boron, the remainder being carbon), silicon carbide or a mixture of two or more of these compounds.
[0151] The thickness of the deposited interphase is preferably between 100 nm and 1500 nm. The total thickness of the interphase and the first matrix phase is chosen to be sufficient to consolidate the fiber preform, i.e. to bind the fibers of the preform together sufficiently so that the preform can be handled while retaining its shape without the assistance of holding tools. This thickness may be at least 300 nm. After consolidation, the preform remains porous, the initial porosity being filled, for example, only a minor part by the interphase and the first matrix phase.
[0152] The production of deposits of PyC, BC, B4C, Si-BC, Si3N4, BN and SiC by CVI is known. Reference may in particular be made to documents US 5,246,736, US 5,738,951, US 5,965,266, US 6,068,930 and US 6,284,358.
[0153] Once the consolidation is complete, the shell can be unstuck (step S10) and is mechanically destroyed in order to release a preform corresponding to the consolidated preform 80. The preform thus obtained is self-supporting and does not require any shape-holding tools for subsequent operations.
[0154] The preform may in particular be subjected to one or more of the following subsequent steps in the manufacture of a part made of CMC material:
[0155] - Additional densification, outside of shaping tools, with the materials mentioned for the interphase deposition step, including: PyC, BC, B4C, Si-BC, Si3N4, BN and SiC by CVI,
[0156] - an injection of a densification slip into the fiber preform ("Slurry Cast” or “Slurry Transfer Molding”),
[0157] - an infiltration of the preform with a composition based on molten silicon of in order to form a ceramic matrix, a densification process known as the MI process (for the English acronym "Melt Infiltration"),
[0158] - one or more machining operations,
[0159] - the formation of a coating.
[0160] Such steps are known per se and are not described in further detail here.
[0161] In an alternative implementation, the shell 61 can be preserved during the operations of injecting a slip and infiltration with a composition based on molten silicon.
Claims
Claims
1. A method for consolidating a fiber preform intended for the manufacture of a composite material part comprising at least the following steps: a- shaping a fiber preform (10) in a mold (S5), the fiber preform being previously impregnated (S4) with a fugitive or fugitive material (30), or shaping a fiber preform in a mold (S2) and injecting a fugitive or fugitive material into the fiber preform held in shape in the mold (S3); b- demolding (S6) the set fiber preform (40); c- coating (S7) the set fiber preform with a slip (60), said slip comprising one or more pore-forming agents (50), the mass content of pore-forming agent being between 25% and 75% relative to the total mass of the slip; d- a heat treatment (S8) of the coated fibrous preform to form a shell (61) by consolidation of the slip; e- a step of eliminating the pore-forming agent;f- a step of removing the fugitive or fugitive material; and g- consolidation (S9) of the fibrous preform by a chemical vapor infiltration process.;
2. A method of consolidating a fibrous preform according to claim 1, wherein the pore-forming agent(s) (50) is chosen from: polyvinyl alcohols, polystyrenes, wax, carbon fibers or a mixture of two or more of these compounds.
3. A method of consolidating a fibrous preform according to claim 1 or 2, wherein the pore-forming agents are such that their smallest dimension is between 0.2 mm and 0.5 mm, and their largest dimension is between 0.2 mm and 2.0 mm.
4. Method for consolidating a fibrous preform according to any one of claims 1 to 3, in which step c- of coating the set fibrous preform (40) comprises one or more times the repetition of at least the following sub-steps: cl- soaking the set fibrous preform in a slip (60) comprising one or more pore-forming agents (50), the mass content being between 25% and 75% relative to the total mass of the slip; c2- drying the fibrous preform obtained at the end of step cl; then c3- possibly, sandblasting the surface of the fiber preform obtained at the end of step c2.
5. A method of consolidating a fiber preform according to claim 4, wherein there is more than one repetition of sub-steps c1-, c2- and optionally c3-, and wherein the content of pore-forming agent (50) varies in the slip of the different steps c1.
6. Method for consolidating a fiber preform according to one of claims 1 to 3, in which step c- of coating the frozen fiber preform (40) comprises one or more times the repetition of at least the following sub-steps: c' 1- dipping the preform in a slip (60) comprising no pore-forming agent; c'2- spraying one or more pore-forming agents (50) onto the preform obtained at the end of step c' 1; c'3- drying the fiber preform obtained at the end of step c'2; then c'4- optionally sanding the preform obtained at the end of step c'3; the total quantity of pore-forming agent sprayed representing between 25% and 75% of the total mass of the slip.
7. Method for consolidating a fiber preform according to one of claims 1 to 4, in which step c- of coating the frozen fiber preform (40) comprises at least the following sub-steps: c” 1- the arrangement of the frozen fiber preform in an injection tool formed of a mold (25) and a counter-mold (26); c”2- the injection into the injection tool of a slip comprising one (or more) pore-forming agent, the mass content of pore-forming agent being between 25% and 75% relative to the total mass of the slip.
8. Method for consolidating a fibrous preform according to any one of claims 1 to 7, in which the mass content of pore-forming agent (50) in the slip (60) coating the preform is between 35% and 50% relative to the total mass of the slip.
9. A method of consolidating a fiber preform according to one of claims 1 to 8, wherein said fiber preform comprises silicon carbide SiC fibers, silicon nitride Si3N4 fibers, or carbon fibers.
10. Method for consolidating a fiber preform according to any one of claims 1 to 9, which comprises a single heat treatment step which comprises a step e- of maintaining at a first temperature allowing the elimination of the pore-forming agent, a step f- of maintaining at a second temperature, higher than the first temperature, allowing the elimination of the fugitive or fugitive material, then a step d- of maintaining at a sintering temperature, higher than the second temperature, allowing a shell to be formed by consolidation of the slip.
11. Method for consolidating a fibrous preform according to any one of claims 1 to 10, which further comprises, before step e-, a step e'- of chemical degradation of the pore-forming agent.
12. A method of consolidating a fibrous preform according to any one of claims 1 to 11, wherein the fugitive or fugitive material has the same chemical composition as the pore-forming agent.
13. Method for manufacturing a part made of composite material, the method comprising at least the steps of: - the consolidation of a fibrous preform produced by means of a method according to any one of claims 1 to 12; - a step of detaching the porous shell, - a step of densifying the porous preform.
Citation Information
Patent Citations
Process for the manufacture of a refractory composite material protected against corrosion
US5246736A
Method of manufacturing a composite material with lamellar interphase between reinforcing fibers and matrix, and material obtained
US5738951A
Composite material protected against oxidation by a self-healing matrix, and a method of manufacturing it
US5965266A
High-temperature composite materials with carbon or carbon-coated fibre reinforcements and enhanced oxidation resistance
US6068930A
Textile preforms sheathed in a boron nitride coating, composites incorporating them and their preparation
US6284358B1