3D printable dual-cure resin nanocomposite for high-performance thermal shielding

IN606767BActive Publication Date: 2026-10-23NAT INST OF TECH WARANGAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202641020767
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Filing Date
2026-02-23
Publication Date
2026-10-23
Estimated Expiration
2046-02-23

AI Technical Summary

Technical Problem

Existing additive manufacturing methods for high-temperature applications face challenges such as defects, uneven material distribution, and inconsistent mechanical and thermal performance due to lack of precise composition and optimized printing parameters, particularly in dual-cure thermosetting resins with nanofillers.

Method used

A dual-cure resin hybrid nanocomposite formulation with UV-curable epoxy acrylate oligomer, glycidyl methacrylate crosslinker, and thermally curable resole phenolic resin, incorporating nano silica and boron nitride nanofillers, optimized for Direct Ink Writing (DIW) 3D printing, with controlled rheology and curing parameters to ensure smooth deposition and complete crosslinking.

Benefits of technology

The formulation achieves enhanced mechanical strength, thermal stability, and ablation resistance, with improved tensile, flexural, and compressive strengths, reduced erosion rates, and superior thermal protection, suitable for aerospace and high-temperature applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000015_0000
    Figure 00000015_0000
  • Figure 00000015_0001
    Figure 00000015_0001
  • Figure 00000015_0002
    Figure 00000015_0002
Patent Text Reader

Abstract

TITLE: 3D PRINTABLE DUAL-CURE RESIN NANOCOMPOSITE FOR HIGH-PERFORMANCE THERMAL SHIELDING A dual-cure resin hybrid nanocomposite for additive manufacturing through direct ink writing (DIW) 3D printing, has been proposed in the present invention. The formulation combines a UV-curable epoxy acrylate oligomer (10–25 %), glycidyl methacrylate crosslinker (1–10 %), a phosphine-oxide photoinitiator (1-4 %), and a thermally curable resole phenolic resin (73–88 %), reinforced with 5 wt% nano silica and 1–5 wt% boron nitride nano powder. UV curing provides immediate green strength during layer deposition, while thermal post-curing ensures full crosslinking, high mechanical performance, and strong interlayer adhesion. Optimized printing parameters corresponding to different filler loadings, and the related representative images are provided below for each condition is depicted in figure-2. Nano silica improves rheology, shape retention, and erosion resistance, whereas boron nitride enhances ablation resistance. The composite is suitable for aerospace and high-temperature structural applications, offering efficient, mould-free fabrication of thermally resistant components.
Need to check novelty before this filing date? Find Prior Art

Description

FIELD OF THE INVENTION

[0001] The present invention is related to dual-cure resin hybrid nanocomposite designed foradditive manufacturing more particularly using direct ink writing (DIW) 3D printing aimed atproducing high-performance, thermally resistant composite structures for aerospace and hightemperature applications.BACKGROUND

[0002] The ability of materials to withstand rapid thermal changes is critical for heat shields in reentry vehicles. Traditional fabrication methods like hand lay-up, hot pressing, and resin infusionoften produce defects such as voids, uneven material distribution, and inconsistent fiber volume,reducing mechanical and thermal performance. Additive manufacturing (3D printing) offersprecise layer-by-layer control, improved geometry, and automated material placement, addressingmany conventional challenges. While most additive manufacturing (AM) focuses onthermoplastics or single-cure photopolymers, dual-cure thermosetting resins with nanofillers showpromise for high-temperature applications. These systems improve rheology, crosslinking, andshape stability but have rarely been tailored for extreme TPS environments (~2500°C). Therefore,there is a clear need for 3D-printable dual-cure hybrid nano filled composites optimized for thermalprotection and mechanical reliability.

[0003] The existing invention discloses a dual-cure epoxy resin composition for additivemanufacturing of three-dimensional objects. The composition comprises a photoinitiator and oneor more monomers and prepolymers that are polymerizable upon exposure to actinic radiation orlight. An optional light-absorbing pigment or dye is included to control curing characteristics. Thecomposition comprises an epoxy resin and, preferably, an organic hardener co-polymerizable withthe epoxy resin. In addition, the formulation may include a dual-reactive compound having a firstreactive group compatible with the light-curable monomers or prepolymers and a second reactivegroup reactive with the epoxy resin, such as an epoxy acrylate. The resulting dual-cure systemenables light-induced curing followed by epoxy curing, making it suitable for additivemanufacturing applications.

[0004] Furthermore, the other invention discloses an advanced ink formulation for additivemanufacturing comprising imide-extended bismaleimide (IE-BMI) and / or extended bismaleimide(E-BMI), cyanate ester, and optionally one or more additives, including reactive or non-reactivematerials. The formulation incorporate carbonaceous or functional materials, sol-gel or inorganicprecursors, and epoxy or bismaleimide triazine resins to enhance mechanical, thermal, andchemical performance. The IE-BMI and E-BMI components feature tunable molecular structures,enabling control over viscosity, crosslinking, and processability for layer-by-layer deposition viavat polymerization techniques such as stereolithography (SLA) or digital light processing (DLP).The disclosed formulation allows for the fabrication of high-performance polymeric objects withprecise dimensional fidelity and enhanced structural and thermal properties suitable for aerospace,automotive, electronic packaging, medical devices, and other advanced applications. Methods ofprinting and curing the formulation to produce three-dimensional objects with tailored propertiesare also described.

[0005] The existing inventions have limitations: lack precise quantitative composition, includingspecific % of epoxy acrylate oligomer, glycidyl methacrylate, photoinitiator, phenolic resin, andnanofillers such as nano silica and boron nitride. They do not provide details on dual-curingmechanisms combining UV-induced in-situ gelation with thermal post-curing, nor optimization ofDIW printing parameters such as nozzle diameter, extrusion pressure, or bed temperature.Rheological control, shear-thinning behaviour and viscosity stability during extrusion are absent,as are experimental data on mechanical and thermal properties including tensile, flexural,compressive strength, char yield, and ablation resistance. The prior art also fails to disclose thesynergistic effect of hybrid nanofillers on shape retention, thermal conductivity, and erosionresistance. Hence, the proposed invention addresses these gaps by providing a precisely formulateddual-cure resin hybrid nanocomposite, optimized DIW 3D printing parameters, and improvedmechanical, thermal, and ablative properties compared to the prior art.SUMMARY

[0006] The invention presents a dual-cure resin hybrid nanocomposite for additive manufacturingusing Direct Ink Writing (DIW) 3D printing. It contains a UV-curable epoxy acrylate oligomer(10-25 %), glycidyl methacrylate crosslinker (1-10%), a phosphine-oxide photoinitiator (1-4 %),and a thermally curable resole phenolic resin (73-88 %). The UV-curable components providegreen strength during printing, while thermal curing completes crosslinking for high mechanicalperformance.

[0007] Nanofillers include 5wt% nano silica for rheology control and 1-5wt% boron nitride toenhance ablation resistance.

[0008] Printing is performed through a 1.37mm DIW nozzle under UV light and bed temperaturesof 80-100°C to ensure layer adhesion and dimensional stability. Optimized parameters, includingprint speed, extrusion pressure, and UV exposure, allow smooth, defect-free deposition and in-situstructural reinforcement.

[0009] Mechanical and thermal performance improves significantly with nanofiller incorporation.Adding 5wt% nanosilica enhances tensile strength (15-20MPa), flexural strength (35-40MPa),and compressive strength (55-60MPa), along with better shape retention and lower heat flux.

[0010] A hybrid system of 5 wt% nanosilica and 5 wt% boron nitrides increases tensile strength(31-35MPa), flexural strength (51-55MPa), compressive strength (75-80MPa), and char yield(65-70 %).

[0011] Erosion rates decrease from 0.3-0.4mm / s to 0.1-0.15mm / s, and back-face temperaturesdrop, indicating superior thermal protection. The dual-cure photo-thermal process ensures fullpolymerization, strong interlayer adhesion, and dimensional stability for high-temperatureapplications.

[0012] The optimized formulation and printing method enable cost-effective, high-performance3D-printed composite structures for aerospace and other thermal-protection applications.OBJECTIVES OF THE INVENTION

[0013] The main objective of the proposed invention is to develop a dual-cure resin hybridnanocomposite suitable for DIW 3D printing that combines UV- and thermally curablecomponents for rapid in-situ stabilization and complete post-print crosslinking.

[0014] It aims to enhance printability, shape retention, and mechanical performance through theincorporation of nano silica and boron nitride nanofillers.

[0015] Another objective is to achieve superior thermal stability and ablation resistance, makingthe printed composites suitable for high-temperature applications such as aerospace thermalshields and nozzle liners.

[0016] Furthermore, the present invention seeks to optimize rheology, extrusion, and curingparameters to enable smooth, defect-free printing without requiring large moulds or extendedthermal curing cycles.BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Table 1 illustrates the optimized dual-cure resin formulation for DIW 3D printing and UVphotocuring.

[0018] Figure-1 illustrates the photo-DSC of neat and nano-filled dual-cure resole phenoliccomposites under 405Nm UV.

[0019] Table-2: illustrates the optimization of 3D printing parameters based on filler content.

[0020] Figure-2. illustrates the optimized printing parameters corresponding to different fillerloadings, and the related representative images are provided below for each condition.

[0021] Figure-3 (a-d) illustrates the curing process of 3D-printed composite thermal shields.

[0022] Figure-4 (a) illustrates the varying shear rate from 0 to 100 (s-1) and (b) constant shear rate at 50 (s-1).

[0023] Figure-5 (a) illustrates the tensile strength vs. strain for dual-cure 3D printable resin with 5wt% nano silica and varying boron nitride content (1-5 wt %).

[0024] Figure-5 (b) illustrates the flexural strength vs. displacement for dual-cure 3D printableresin with 5 wt% nano silica and varying boron nitride content (1-5 wt %).

[0025] Figure-5 (c) illustrates the compressive strength vs. strain for dual-cure 3D printable resinwith 5 wt% nano silica and varying boron nitride content (1-5 wt %).

[0026] Figure-6 (a) illustrates the thermogravimetric analysis (TGA) for dual-cure 3D printableresin with 5 wt% nano silica and varying boron nitride content (1-5 wt %).

[0027] Figure-6 (b) illustrates the OAT test on the 3D printed sample.

[0028] Table-3 illustrates the OAT for dual-cure 3D printable resin with 5 wt% nanosilica andvarying boron nitride content (1-5 wt %).DETAILED DESCRIPTION OF THE INVENTION:

[0029] A dual-cure resin hybrid nanocomposite for additive manufacturing (3D printing) has beenproposed in the present invention. The proposed invention discloses (a) a UV-curable Bis-Adiglycidyl ether diacrylate oligomer in an amount of 10-25 % part of the base resin, (b) a glycidylmethacrylate crosslinker in an amount of 1-10 % part of the base resin, (c) a Diphenyl (2, 4, 6trimethylbenzoyl) phosphine oxide (TPO) photoinitiator in an amount of 1-4 % part of the baseresin, (d) a thermally curable resole ABRON PR 100 WS resin in an amount of 73-88 % part ofthe base resin, (e) the nanofillers comprise a nano silica in an amount of 5 wt% and a boron nitridenano powder in an amount of 1-5 wt% of the base resin as shown in table-1.

[0030] The nanosilica functions as a rheology modifier exhibiting enhanced shape retention duringprinting and enhanced thermal-erosive resistance. The boron nitride nano powder enhances theheat flux through the printed structure and increases ablation resistance. The nanofillers are addedinto the reactive base resin under mechanical stirring to form a nanocomposite ink. The nanofillersexhibit thixotropic recovery enabling stable extrusion without nozzle clogging. Thenanocomposite ink is loaded into the direct ink writing (DIW) 3D printer is equipped with the 405Nm UV light source. The nanocomposite ink is extruded through the nozzle to deposit layers whileexposing each layer to UV radiation to induce in-situ gelation and green-strength formation alongwith bed temperature of 80-100°C to form a printed structure. The UV exposure per printed layeris between 10-60 seconds at a wavelength of 405 Nm.

[0031] The direct ink writing (DIW) 3D printer nozzle has a diameter of 1.37 mm and extrusionpressure corresponds to a pulse rate of 20-40 as shown in table-2. The print speed is between 5-25 mm / s. The printed structure is thermally cured at 80-120 °C in a staged heating cycle to forma dual-cure resin hybrid nanocomposite. The thermal post-curing comprises sequential holding at80 °C-100 °C and 120 °C for 2-4 hours each to complete phenolic crosslinking and enhancethermal stability.

[0032] The neat resin, which is not printable, shows no layer retention during composite printingand exhibits a Photo-DSC peak exotherm of about 2.2 W / g at 920 seconds. Incorporating 5 wt%nano silica into the resin significantly improves processing behaviour, resulting in smoothprintability and stable shape retention. The formulation displays a reduced Photo-DSC peakexotherm of roughly 1.7 W / g with a peak time near 970 seconds. Its mechanical performance risesto tensile strengths of 15-20 MPa, flexural strengths of 35-40 MPa, and compressive strengths of55-60 MPa. Thermogravimetric analysis shows a char yield of 55-60 %, while ablation testingindicates an erosion rate of 0.3-0.4 mm / s and a back-face temperature of about 160-165 °C.

[0033] Further enhancement is achieved with a hybrid system containing 5 wt% nano silica and 5wt% boron nitrides, which delivers the best overall performance. The composite records the lowestPhoto-DSC exotherm at 1.05 W / g with a peak near 880 seconds. Mechanical strengths increasesubstantially, reaching tensile values of 31-35 MPa, flexural strengths of 51-55 MPa, andcompressive strengths of 75-80 MPa. It also exhibits a higher char yield of 65-70 % and superiorablation resistance, with erosion rates of just 0.1-0.15 mm / s and back-face temperatures of only35-40 °C.

[0034] The dual-cure mechanism promotes deep and complete curing, high crosslink density, andstrong interlayer adhesion. This translates to significant mechanical improvements including gainsof 75-100 % in tensile strength, 45-48 % in flexural strength, and 33-36 % in compressive strengthalong with increased char formation (about 18 % higher) and more than 1.5-times better ablationresistance. The approach also supports cost-effective manufacturing by removing the need forlarge-mold tooling and lengthy thermal curing cycles. Potential applications include aerospace androcketry components such as thermal-protection shields, nozzle liners, and other high-temperaturecomposite structures.

[0035] Development of 3D printable composite thermal shield ink formulation: A dual-cure resinformulation was created for Direct Ink Writing (DIW)-based 3D printing by combining UV-reactive epoxy acrylate oligomers with a thermally curable resole-type phenolic resin. This systemutilized both photo- and thermal-initiated polymerization to provide immediate structural integrityduring printing and complete crosslinking during subsequent thermal curing. Epoxy acrylate (10-25%) contributed UV reactivity and green strength, while 1-10 % glycidyl methacrylateintroduced additional crosslinking sites to enhance stiffness. A phosphine-oxide-typephotoinitiator (1-4 %) supported uniform curing in the filled system. The concentration of thethermal-curable base resin was controlled to maintain appropriate flowability and nanofillers suchas nanosilica and boron nitride (BN) powder (1-5 wt% of the dual cure base resin) wereincorporated to enhance and thixotropic behavior, mechanical and thermal performance.

[0036] Optimal dispersion was achieved through mechanical agitation, ensuring a viscositybalance conducive to smooth, clog-free extrusion. The resulting formulation demonstrated strongcuring response, low shrinkage, and uniform surface quality following post-thermal treatment.Characterization of peak exothermic behaviour of neat and particulate-filled dual-cure resins usingphoto-DSC analysis: Photo-DSC measurements illustrate the heat-flow response (W / g) of the dualcure resin hybrid nanocomposite during UV curing at 405 Nm for various nanofiller compositions.The neat resin displays the highest peak exothermic heat flow of 2.2 W / g and the fastest cure, witha peak near 920 s, reflecting rapid photopolymerization.

[0037] Incorporating 5 wt% nano silica reduces the peak heat flow to about 1.7 W / g and shifts thepeak to roughly 970 s, indicating that the presence of nano silica restricts radical mobility andslows the cure rate. Hybrid nanocomposites containing both nano silica and boron nitride (BN)follow a consistent trend of decreasing peak exotherm and shifted peak time as BN contentincreases. Formulations with 5 wt% NS + 1 wt% BN show a moderate reduction to 1.5 W / g witha peak at about 950 s, while 5 wt% NS + 3 wt% BN decreases the exotherm to around 1.3 W / gwith a peak near 930 s. The 5 wt% NS + 5 wt% BN formulation produces the lowest exothermicheat flow, roughly 1.05 W / g, with a peak at 880s. The progressive decline in photopolymerizationreactivity with increasing BN content, in the presence of nano silica, is attributed to enhanced lightscattering and higher viscosity, both of which hinder the diffusion of reactive species.

[0038] Optimization of 3D printing process: Optimization of printability was performed byadjusting nozzle diameters (0.2, 0.53, 0.63, 0.86, 1.37, and 1.52 mm) as shown in table-2 and fillerconcentrations to assess the flow behaviour and structural integrity of the dual-cure resin system.A nozzle diameter of 1.37 mm was identified as optimal, providing stable extrusion, uniform layerdeposition, and defect-free printing. The neat phenolic resin displayed excessive fluidity, extrudinglike a liquid without retaining its shape.

[0039] 1-2 wt% nano silica offered slight improvements but still resulted in unstable flow andmerged layers. Increasing nano silica to 3-4 wt% produced more consistent extrusion with onlyminor irregularities. The best printability occurred at 5 wt% nano silica, where the resin exhibitedcontinuous flow, reliable layer stacking, and strong shape retention. Loadings above 6 % led toexcessive viscosity, causing nozzle clogging and diminished print quality. When 5 wt% nano silicawas combined with varying boron nitride (BN) concentrations, viscosity gradually increased withhigher BN content as shown in the figure 2.

[0040] Formulations containing up to 5 wt% BN maintained smooth, uninterrupted extrusionwithout void formation, whereas BN levels of 6 wt% or more resulted in intermittent flow andprint defects due to overly high viscosity. Overall, the formulation consisting of 5 wt% nanosilicaand up to 5 wt% BN provided the best compromise between flowability, layer adhesion, anddimensional accuracy, making it the most suitable composition for defect-free 3D printing of dualcure resin hybrid composites.

[0041] Curing process of in-situ photo- and thermally partially cured 3D printed composite thermalshields at 405 Nm is shown in figure-3 (a-d) with different bed temperatures: The printedcomposites were cured using simultaneous UV irradiation at 405 Nm and controlled bed heating,enabling uniform polymerization and crosslinking throughout the printed layers. Sequentialphoto-thermal curing ensured consistent material consolidation, with specimens cured at theoptimized bed temperature of 80 °C exhibiting superior dimensional stability, reduced warpage,and improved quality of product compared to samples partially cured solely by UV or by combinedUV and lower-temperature thermal treatments (40-60 °C).

[0042] Rheology of the reaction mixture through viscometry: Rheological evaluation of the resinformulations showed that the neat resin possessed the lowest viscosity (~100-20 Pa.s across shearrates of 1-100 s-1), resulting in inadequate shape retention after extrusion. Adding fillers increasedviscosity significantly: 5 wt% nano silica raised the viscosity to 135-30 Pa.s, improving shapestability during printing, while incorporating 1-5 wt% boron nitride (BN) alongside nano silicacaused a slight additional rise in low-shear viscosity (~140-40 Pa.s), strengthening structuralintegrity of the deposited material as shown in the figure 4(a). All formulations displayed shear-thinning behaviour, which is advantageous for extrusion based 3D printing.

[0043] Time-dependent viscosity measurements at a constant shear rate (50 s-1, 0-300 s)demonstrated that filled formulations retained viscosity more consistently than the neat resin asshown in figure-4(a). The combination of 5 wt% nano silica and 5 wt% BN showed the highestviscosity stability, providing an optimal balance for DIW printing by supporting smooth extrusion,minimal sagging, and high dimensional fidelity as shown in figure-4(b).

[0044] Mechanical characterization: Tensile strength-The incorporation of 5 wt% nanosilica (NS)into the 3D-printable composite resin enhances mechanical performance, which is improved withthe addition of boron nitride (BN) nanopowder at 1, 3, and 5 wt%. The base resin containing only5 wt% NS exhibits the lowest tensile strength (~19 MPa) and the highest strain (~4.4 %) as shownin figure-5 (a), indicating good ductility but limited reinforcement. Increasing BN contentprogressively improves tensile strength: 1 % BN achieves ~25 MPa (31 % increase), 3 % BNreaches ~29 MPa (52 % increase), and 5 % BN attains ~35 MPa (84 % increase), while the straindecreases to 3 %. This behaviour reflects increased stiffness and effective load transfer, as BNrestricts polymer chain mobility, limiting deformation under load. As a result, stiffness and strengthare enhanced at the expense of ductility.

[0045] Flexural strength follows a similar trend for the dual-cure 3D-printable resin containing 5wt% NS with varying BN content. The base resin with only 5 wt% NS exhibits the lowest flexuralstrength (~38 MPa) and the highest displacement, indicative of higher ductility but reduced load bearing capacity. The addition of BN significantly enhances flexural performance: ~45 MPa at 1 %BN (18.4 % increase), ~51 MPa at 3 wt% BN (34.2% increase), and ~55 MPa at 5 wt% BN (44 %increase) as shown in figure-5 (b). The improvement arises from more efficient stress transfer,stronger matrix-filler interactions, and the inherent stiffness of BN, which restricts polymer chainmobility. Consequently, displacement at failure decreases. The combination of 5 wt% NS and 5wt% BN provides an optimized balance of flexural strength and structural integrity.

[0046] Compressive strength: The compressive strength of the dual-cure 3D-printable resin hybridcomposite thermal shields improves with increasing boron nitride (BN) content in formulationscontaining 5 wt% nanosilica (NS). The base resin with only 5 wt% NS exhibits the lowestcompressive strength (~57 MPa) and the highest strain (~7 %), reflecting good ductility but limitedload-bearing capacity as shown in figure-5 (c). Addition of 1 wt% boron nitride (BN) increasesstrength by ~5.2 % to ~60 MPa, accompanied by a reduced strain. Further increases in BN contentresult in 3 wt% BN achieving ~69 MPa (21 % increase) and 5 wt% boron nitride (BN) reaching~75 MPa (31.5 % increase), while the strain at failure decreases to ~4.5 %. This enhancement isattributed to BN's intrinsic stiffness and high aspect ratio, which improve load-bearing capacityand restrict polymer chain mobility, albeit with a slight trade-off in ductility.

[0047] Thermal characterization of 3D-printed composite thermal shields: Thermogravimetricanalysis (TGA)-TGA was performed to evaluate the thermal stability of dual-cure 3D-printableresin hybrid nanocomposite thermal shields containing 5 wt% nanosilica (NS) with varying boronnitride (BN) content as shown in figure-6 (a). The resin with only 5 wt% NS exhibits the highestweight loss and the lowest char yield (~57 %), indicating limited thermal stability. Incorporationof boron nitride (BN) progressively enhances thermal resistance, with char yields increasing to~59 %, 62 %, and 65 % for 1 wt%, 3 wt%, and 5 wt% boron nitride (BN), respectively. Theimproved thermal stability is attributed to BN's heat-resistant nature and its ability to form barrierlayers, making the composites more suitable for high-temperature shielding applications.

[0048] Oxyacetylene Test (OAT): Figure 6 (b) illustrates the OAT test on the 3D printed sample.Oxyacetylene ablation testing confirms the thermal protection performance of the DIW 3D-printeddual-cure resin composite shields. The silica-only resin (5 wt% NS) exhibits the highest erosionrate (~0.327 mm / s) and back-face temperature (~162 °C) as shown, indicating limited thermalresistance. Increasing boron nitride (BN) content (1-5 %) substantially reduces both erosion ratesand back-face temperatures, reaching 0.110 mm / s and 36 °C for the formulation containing 5 wt%NS + 5 wt% boron nitrides (BN) as shown in table-3. The improvement is due to the formation ofa denser, thermally insulating char layer. boron nitride (BN) also enhances lateral heat dissipationand maintains structural integrity under high heat, reducing thickness loss (from 1.11 mm to 0.86mm) and improving mass retention. These results highlight BN's critical role in enhancing theablative and thermal protection performance of the composite shields.

[0049] The dual-cure resin hybrid nanofilled composite thermal shields for DIW 3D printing areformulated within carefully optimized parameter ranges to ensure processability, in-situstabilization, and enhanced final performance. The resin formulation consists of 10-25 % epoxyacrylate (Bis-A diglycidyl ether diacrylate), 1-10 % glycidyl methacrylate (GMA), 1-4 %photoinitiator (diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, TPO), and 73-88 % phenolicresin (ABRON PR100 WS), with 5 wt% nanosilica for rheological control and reinforcement, and1-5 wt% boron nitride nano powder to enhance thermal erosion resistance.

[0050] Rheological and printing parameters are also carefully controlled, with viscosities rangingfrom 160-10 Pa.s at shear rates of 1-100 s-1, nozzle diameters ≥1.37 mm, pneumatic extrusionpressures of 20-40 pulse rate, print speeds of 5-25 mm / s, and layer heights between 1 and 1.2 mm.Curing is performed using UV exposure at 405 Nm for 10-60 seconds per layer, followed bythermal post-curing at temperatures up to 120°C in stepwise increments of 80°C, 100°C, and120°C for 30-90 minutes. These optimized conditions allow for smooth extrusion, reliable layerstacking, in-situ structural stabilization, and final composites with improved mechanical andthermal performance, while offering tunability to accommodate specific part geometries andperformance requirements.

Claims

1. A A dual-cure resin hybrid nanocomposite for additive manufacturing, comprising: (a) a UV-curable epoxy acrylate oligomer in an amount of 10-25 % of the total weight; (b) a glycidyl methacrylate crosslinker in an amount of 1-10 % of the total weight; (c) a phosphine-oxide photoinitiator in an amount of 1-4 % of the total weight; (d) a thermally curable resole phenolic resin in an amount of 73-88 % of the total weight; (e) the nanofillers comprise a nano silica in an amount of 5 wt% and a boron nitride nano powder in an amount of 1-5 wt% of the total weight; (f) a direct ink writing (DIW) 3D printer with a nozzle; (g) a UV light source; characterized in that: the UV-curable epoxy acrylate oligomer in (a), the glycidyl methacrylate crosslinker in (b), the phosphine-oxide photoinitiator in (c) and the thermally curable resole phenolic resin in (d) are mixed to form a reactive base resin; the nanofillers in (e) are added into the reactive base resin under mechanical stirring to form a nanocomposite ink; the nanocomposite ink is loaded into the direct ink writing (DIW) 3D printer in (f), is equipped with the UV light source in (g); wherein the nanocomposite ink is extruded through the nozzle to deposit layers while exposing each layer to UV radiation to induce in-situ gelation and green-strength formation to form a printed structure; and whereby the printed structure is thermally cured at 80-120 °C in a staged heating cycle to form a dual-cure resin hybrid nanocomposite; and the thermal post-curing comprises sequential holding at 80 °C, 100 °C and 120 °C for 2-4 hours to complete phenolic crosslinking and to enhance thermal stability.

2. The dual-cure resin hybrid nanocomposite as claimed in claim 1, wherein the UV-curable epoxy acrylate oligomer in (a) is a Bis-A diglycidyl ether diacrylate.

3. The dual-cure resin hybrid nanocomposite as claimed in claim 1, wherein the phosphine-oxide photoinitiator in (c) is a Diphenyl (2, 4, 6 trimethylbenzoyl) phosphine oxide (TPO).

4. The dual-cure resin hybrid nanocomposite as claimed in claim 1, wherein the nano silica in (d) functions as a rheology modifier exhibiting enhanced shape retention during printing and enhanced thermal-erosive resistance.

5. The dual-cure resin hybrid nanocomposite as claimed in claim 1, wherein the boron nitride nano powder in (d) enhances the ablation resistance.

6. The dual-cure resin hybrid nanocomposite as claimed in claim 1, wherein the nanofillers in (d) exhibit thixotropic recovery enabling stable extrusion without nozzle clogging.

7. The dual-cure resin hybrid nanocomposite as claimed in claim 1, wherein the UV exposure per printed layer is between 10-60 seconds at a wavelength of 405 Nm.

8. The dual-cure resin hybrid nanocomposite as claimed in claim 1, wherein the direct ink writing (DIW) 3D printer in (f) nozzle have a diameter of 1.37 mm and extrusion pressure corresponds to a pulse rate of 20-40.

9. The dual-cure resin hybrid nanocomposite as claimed in claim 1, wherein the print speed is between 5-25 mm / s.