Weather-resistant and durable coating composition

JP2023504239A5Active Publication Date: 2024-11-13DOW GLOBAL TECHNOLOGIES LLC +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022529100
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-12-05
Filing Date
2020-11-12
Publication Date
2024-11-13
Estimated Expiration
2040-11-12

AI Technical Summary

Technical Problem

Existing coatings, such as isocyanate-containing polyurethane-based and epoxy coatings, face issues with moisture stability, brittleness, and the need for humidity-dependent curing, which affects their performance and durability, especially in applications requiring UV protection, corrosion resistance, and chemical resistance.

Method used

A curable coating composition comprising amino-functional silicone resin with aryl groups connected via Si-O-C bonds and acrylic copolymers with epoxy functional groups, providing a balanced molar ratio of amine to epoxy groups, ensuring stability and compatibility, and incorporating cure-compatible groups for improved performance.

Benefits of technology

The composition achieves enhanced moisture stability, UV protection, corrosion resistance, and chemical resistance while maintaining good dry time and appearance, offering a cost-effective alternative to traditional coatings.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A curable coating composition is provided that includes a multifunctionalized acrylic copolymer and an amino-functional silicone resin curing agent. The acrylic copolymer of the curable coating composition has, in polymerized form, epoxy-functionalized groups and curing-compatible groups, and the amino-functional silicone resin is an aryloxy-containing amino-functional siloxane, which optionally derives from a sterically hindered alcohol-amine precursor moiety. The coating composition is useful in the field of superior weather resistance and durability coatings and as an alternative to isocyanate-containing polyurethane-based coatings. Coated articles made from the curable composition are also provided.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a curable coating composition comprising a polyfunctionalized acrylic copolymer and an amino-functionalized silicone resin curing agent. More specifically, the acrylic copolymer has epoxy-functionalized groups and curing-compatible groups in its polymerized form, and the amino-functionalized silicone resin is an aryloxy-containing amino-functionalized siloxane, which is also optionally derived from a sterically hindered alcohol-amine precursor moiety. The coating composition is useful in the field of coatings with excellent weather resistance and durability, and is useful as an alternative to isocyanate-containing polyurethane-based coatings.

[0002] Isocyanate-containing polyurethane coatings are used in applications where excellent weather resistance and durability are required. However, manufacturers and consumers are moving towards isocyanate-free coatings that offer weather resistance in addition to chemical and corrosion resistance, in order to limit exposure to such materials. Epoxy coatings are used to protect metals, but in applications where good color and gloss retention is required, epoxy coatings are further coated with a topcoat (usually polyurethane). Other coatings derived from epoxy resins, such as polysiloxane-epoxy coatings, are humidity-dependent in terms of curing and often become brittle as the coating continues to cure.

[0003] Some amino-functionalized polysiloxanes with amine functional groups also incorporate aryl-containing groups, such as phenyl groups, to improve the performance attributes of the coating and the compatibility of the coating components. While amine functional groups can be linked via Si-C and / or Si-OC bonds, linkages via Si-OC bonds typically present stability concerns in the presence of moisture, as the SiOC bonds are susceptible to hydrolysis, regenerating the original amine alcohols and silanols. Hydrolysis affects both the appearance of the protective coating, as the alcohol amines typically do not mesh well with the host siloxane resin and organic epoxy curing agents, and the performance of the protective coating, as the level of chemical crosslinking is greatly limited when the SiOC bonds are cleaved. Aryl-containing groups, such as phenyl groups, typically link to polysiloxanes via high-cost Si-C bonds.

[0004] U.S. Patent Publication 2005 / 0148752 A1 discloses an amino-functional polysiloxane having a Si-OC bond between the polymer backbone and the functional group, and includes an epoxypolysiloxane composition. U.S.2005 / 0148752 A1 fails to distinguish coatings containing acrylic copolymers. Furthermore, U.S.2005 / 0148752 A1 fails to distinguish the advantages associated with the use of siloxanes derived from sterically hindered alcohol-amine precursor moieties from those of non-sterically hindered moieties.

[0005] U.S. Patent No. 8,012,543 discloses the use of polyorganosiloxanes modified with amino alcohols to reduce corrosion of reinforcing bars in concrete structures, wherein the polyorganosiloxanes may contain alkyl or aryl radicals, including phenyloxy radicals. U.S. Patent No. 8,012,543 does not identify coatings containing acrylic copolymers.

[0006] U.S. Patent Publication 2017 / 0174938 A1 discloses the use of a coating layer composition containing a silsesquioxane composite polymer to prevent warping of a substrate, and some embodiments of the silsesquioxane composite polymer contain an OSiOC amine and an OSiOC aryl group. U.S.2017 / 0174938 A1 does not identify coatings containing an acrylic copolymer.

[0007] U.S. Patent No. 8,193,293 discloses a low-temperature ambient curable coating composition comprising an amino-functionalized polysiloxane, a polysiloxane resin which is a reaction product of a hydroxyl-functionalized material having two or more unsaturated bonds that can undergo a hydrosilylation reaction with a silicon-hydrogenated polysiloxane, and a polyepoxide.

[0008] U.S. Patent No. 8,871,888 discloses a high solids content, one-component, and storage-stable coating composition comprising an epoxy resin containing two or more 1,2-epoxy groups per molecule, a hydrocarbon compound having a softening point of 50°C to 140°C, an alkoxy-functionalized and / or silanol-functionalized silicone, and a ketimine curing agent containing a reaction product of a reaction mixture comprising a polyalkyldiamine component and a ketone component.

[0009] International Patent Publication No. 01 / 51575 A1 discloses an ambient temperature curing coating composition comprising a polysiloxane having alkyl, aryl, alkoxy, reactive glycidoxy, and OSi(OR)3 groups, a glycidyl-functionalized acrylic polymer, and a curing agent. The polysiloxane does not contain amine functional groups.

[0010] Japanese Patent Publication No. 2002-167546 A discloses a corrosion-resistant coating material composition for a single coating finish, comprising (A) an acrylic resin, (B) an epoxy resin having at least two epoxy groups, (C) an organosilane compound, and (D) an aminosilane-containing amine curing agent. As the mixing ratios of the acrylic resin (A), the epoxy resin (B), and the organosilane compound (C), based on the total solid content of these resins respectively, component (A) is 5 to 65% by weight, component (B) is 30 to 90% by weight, and component (C) is 5 to 65% by weight.

[0011] What is needed is a cost-effective coating composition that exhibits good stability in the presence of moisture and provides a good balance of properties including UV protection, corrosion resistance, good drying time, and chemical resistance, all using a minimum amount of materials.

[0012] The present invention is a curable coating composition, (1) in a polymerized form (i) (R3SiO a , (4-z) / 2 , , b , d ) a , (ii) (R2Si(OR’) x O (2-x) / 2 ) b , (iii) (RSi(OR’) y ,O (3-y) / 2 ) c 、and (iv) (Si(OR’) z O (4-z) / 2 ) d , an amino-functional silicone resin containing structural units of, wherein each R’ is independently hydrogen, an alkyl group, a functionalized alkyl group, an aryl group or a functionalized aryl group, provided that at least 10 mole percent of all R’ groups are aryl groups or functionalized aryl groups, wherein each R is independently hydrogen, an alkyl group, or a functionalized alkyl group, and wherein at least 10 mole percent of the combination of R and R’ groups is of the formula: -R a -NHR bIt is an amine-containing group, in the formula R a R is an alkyl or aryl-containing group derived from an amino alcohol, b The present invention provides a coating composition comprising: (2) an amino-functional silicone resin, wherein a+b+c+d=1.00 (100 mole percent), x is either 0 or 1, y is either 0, 1 or 2, z is either 0, 1, 2 or 3, and the -NH- equivalent mass of the amino-functional silicone resin is 50 to 750; and (2) an acrylic copolymer having epoxy-functionalized groups and curing-compatible groups in its polymerization form, wherein the coating composition has a molar ratio of amine-NH functional groups to epoxy functional groups in the range of 0.5 to 1.3. The present invention further provides a coated article comprising one or more layers of the cured coating composition.

[0013] The term “mole percent” can also be expressed as “mole fraction,” where 1 mole percent is equal to a mole fraction of 0.01. The terms “mole percent” and “mole fraction” are based on the Si content in the material totaling 100 mol% (i.e., 1.00 mole fraction). For each range presented in this invention, the lower and upper limits of the range can be separated and combined in any way with other lower or upper limits, including combinations of lower and upper limits of the range for additional components identified in this invention. All individual values ​​and subranges are included and disclosed herein.

[0014] Amino-functional silicone resin The amino-functionalized silicone resin of the present invention can be described as a siloxane structure having a siloxane bond (-Si-O-Si-) having an aryl functional group connected to a Si unit on the siloxane structure via a Si-OC bond, and an amine functional group connected to a Si unit on the siloxane structure via a Si-OC bond, a Si-C bond, or one of several combinations thereof, and in polymerization form, (i)(R3SiO 1 / 2 ) a , (ii)(R2Si(OR') x O (2-x) / 2 ) b , (iii)(RSi(OR') y ,O (3-y) / 2 ) c , and (iv)(Si(OR') z O (4-z) / 2 ) d The structural unit comprises the formula, where each R' is independently hydrogen, alkyl group, functionalized alkyl group, aryl group, or functionalized aryl group, provided that at least 10 mole percent of all R' groups are aryl groups or functionalized aryl groups. In the formula, each R is independently hydrogen, an alkyl group, or a functionalized alkyl group. In the formula, at least 10 mole percent of the combination of R and R' groups is represented by formula:-R a -NHR b It is an amine-containing group, in the formula R a R is an alkyl or aryl-containing group derived from an amino alcohol, b is hydrogen or alkyl group, In the equation, a + b + c + d = 1.00 (100 mole percent), x is either 0 or 1, y is either 0, 1, or 2, and z is either 0, 1, 2, or 3. The -NH-equivalent mass of the amino-functionalized silicone resin is 50 to 1000, preferably 50 to 750, more preferably 80 to 900, even more preferably 100 to 800, and most preferably 100 to 700.

[0015] The R and / or R' group is represented by the formula: -R a -NHR b It may be an amine-containing group. Formula: -R a -NHR bThe amounts of all R and R' groups, which are amine-containing groups, can be as low as 10 mole percent or 20 mole percent, and independently as high as 90 mole percent, 50 mole percent or 30 mole percent, with preferred ranges being 10-42 mole percent and 20-30 mole percent, provided that the -NH- equivalent mass of the amino-functionalized silicone resin is within the specified range. a is, formula HO-R a -NHR b It is derived from an amino alcohol represented by the formula, where R a is an alkyl group or an aryl-containing group. Preferably, R a It is derived from an amino alcohol selected from the group consisting of (a) an amino alcohol having steric hindrance around the COH moiety, (b) an amino alcohol that is a secondary or tertiary alcohol, or (c) a mixture thereof.

[0016] The amount of all R' groups, which are aryl groups or functionalized aryl groups, can be as low as 10 mole percent or 20 mole percent, and independently as high as 100 mole percent, 50 mole percent or 30 mole percent, with preferred ranges being 10-60 mole percent and 20-50 mole percent.

[0017] In the description of silicone resin, R3SiO 1 / 2 It is also called M, R2SiO 2 / 2 It is also called D, RSiO 3 / 2 It is also called T, SiO 4 / 2 It is also referred to as Q. When a superscript is used next to the M, D, T, or Q symbol, it refers to the type of R base that exists. For example, D Ph This means that one of the two R groups is a phenyl group. Any R group(s) that are not superscripted should be understood to those skilled in the art as a methyl group unless otherwise indicated by a specific description of the polymer. The -NH-equivalent mass of an amino-functionalized silicone resin is the -NH equivalent mass of a known amount of solution or neat sample of the amino-functionalized silicone resin. 13The 13C-NMR spectrum is obtained, and the peaks associated with the amino-functional Si units of the amino-functional silicone resin are quantified against the peaks associated with a known amount of internal standard (typically 1,4-dioxane), and the solvent content present in the sample, if determined by gas chromatography, is adjusted for. The amino-functional silicone resin exists in the form of a neat liquid, solution, or fusible solid. Each subscript a, b, c, or d represents the mean value of the overall distribution of units constituting the material, and the NMR spectral data (typically, 29 Si-NMR and 13 CNMR, or 29 Si-NMR and 1 This can be determined for any given material by using calculations based on 1H-NMR.

[0018] The amino-functional silicone resins of the present invention can be produced by reacting (1) a silicone resin having a hydroxy or alkoxy functional group with (2) an amino alcohol and an aryl alcohol. The silicone resin having a hydroxy or alkoxy functional group may be derived from polysiloxane, alkoxysilane, or chlorosilane. The hydroxy or alkoxy functional group of the silicone resin (1) composition is sometimes referred to as the "OZ" content and is expressed in mole percent. Non-limiting examples of suitable silicone resins include DOWSIL® 2403, DOWSIL® 3074 and DOWSIL® 3037 available from The Dow Chemical Company, Shin-Etsu Silicone KR-213 and KR-510 available from Shin-Etsu Chemical Co., Ltd., and SILRES® IC232 and SILRES® SY231 available from Wacker Chemie AG.

[0019] As mentioned earlier, amino alcohols are given by formula HO-R a -NHR bIt can be expressed by: Non-limiting examples of preferred amino alcohols include: 2-amino-1-ethanol, 1-amino-2-propanol, 1-amino-2-methylpropan-2-ol, 2-amino-1-propanol, 3-amino-1-propanol, 2-amino-1-butanol, 3-amino-1-butanol, neopentanolamine (3-amino-2,2-dimethyl-1-propanol), 2-amino-1-methyl-1-propanol, 2-amino-2-methyl-1-propanol, 2-amino-2-ethylpropan-1,3-diol, 2-amino -2-methylpropane-1,3-diol, 5-amino-1-pentanol, 1,2-dimethylethanolamine, 3-alloxy-2-hydroxypropylamine, 1-amino-2-methylpentanol, N-methylethanolamine, N-hydroxyethylpropanediamine, N-cyclohexylethanolamine, p-(beta-hydroxyethyl)-aniline, N-(beta-hydroxypropyl)-N'-(beta-aminoethyl)piperazine, 2-hydroxy-3-(m-ethylphenoxy)propyl Amine, 2-hydroxy-2-phenylethylamine, tris(hydroxymethyl)aminomethane, 2-aminobenzyl alcohol, 3-aminobenzyl alcohol, 3-amino-o-cresol, 4-amino-o-cresol, 5-amino-o-cresol, 2-amino-p-cresol, 4-amino-m-cresol, 6-amino-m-cresol, 1-amino-1-cyclopentanemethanol, 2-(2-aminoethoxy)ethanol, 2-(2-aminoethylamino)ethanol, 6-amino-1-hexanol, 3-(1 This includes (alpha-hydroxyethyl)aniline, 2-amino-1-phenylethanol, 1-aminomethyl-1-cyclohexanol, 8-amino-2-naphthol, 2-amino-phenethyl alcohol, 4-aminophenethyl alcohol, 3-(alpha-hydroxyethyl)aniline, Mannich bases, products from the reaction of amino alcohols with cis-2-pentennitrile, followed by a hydrogenation step, aminophenols such as p-aminophenol, tyrosine, tyramine, epoxyamine adducts, and mixtures thereof.Preferred amino alcohols include, but are not limited to, 1-amino-2-propanol and 1-amino-2-methylpropan-2-ol.

[0020] NMR: The composition of various aryloxy-containing amino-functional silicone resin compositions is determined using NMR. Nuclear magnetic resonance (NMR) analysis is performed using a Mercury 400 MHz superconducting spectrometer. This instrument uses silicon-free probes.

[0021] Aryloxy content - The aryloxy content is calculated from the 13C NMR data using deuterated chloroform as an internal standard. The weight % of aryloxy is determined using the weight of the resin and chloroform added to the NMR sample. This information 29 The molar amount of aryloxy is calculated by using this in combination with the composition obtained from Si NMR.

[0022] Molecular weight-molecular weight (Mn and Mw) analysis of resins is performed using gel permeation chromatography. Samples are prepared in 0.5% THF, capped with acetic anhydride, filtered, and analyzed against a polystyrene standard using RI detection. The columns are two 300 mm 5 micrometer Mixed C columns with 50 mm guard columns. The flow rate is 1 ml / min.

[0023] Alkyl groups are exemplified by, but are not limited to, methyl, ethyl, propyl, butyl, hexyl, octyl, decyl, dodecyl, hexadecyl, and octadecyl; alkyl groups are typically methyl. Aryl groups are exemplified by, but are not limited to, phenyl, naphthyl, benzyl, tolyl, xylyl, xenyl, methylphenyl, 2-phenylethyl, 2-phenyl-2-methylethyl, chlorophenyl, bromophenyl, and fluorophenyl; aryl groups are typically phenyl.

[0024] Silicone resins having hydroxy, alkoxy, or aryloxy functional groups are synthesized according to polymerization methods known in the art. Non-limiting and exemplary polymerization methods are disclosed in U.S. Patent Publication 2005 / 0148752 A1.

[0025] Description of polyfunctionalized acrylic copolymers A polyfunctionalized acrylic copolymer means a copolymer comprising a majority copolymerized (meth)acrylic ester, including polymerization forms via acrylate bonds, epoxy functionalizing groups, and curing compatibility groups that retain functional groups on the main chain of the acrylic copolymer. Preferably, polyfunctionalized acrylic copolymers are polar materials, partly due to the presence of curing compatibility groups, which, while not bound by any theory, are considered to aid compatibility with polar aryl-containing, amino-functionalized silicone resins. This compatibility is best seen in the reduction of haze in cured coating compositions. As used herein, the use of the term "(meth)" followed by another term such as acrylate refers to both acrylate and methacrylate. For example, the term "(meth)acrylate" refers to either acrylate or methacrylate. Similarly, the term "(meth)acrylic acid" refers to methacrylic acid or acrylic acid. Acrylic copolymers are prepared by free radical polymerization in a solvent such as xylene, where monomers, initiators, optionally chain transfer agents, and solvents are packed into a container and reacted at approximately 60° to 175°C for approximately 1 to 6 hours to form the polymer. Typical solvents that can be used to prepare acrylic copolymers include toluene, ethyl acetate, butyl acetate, acetone, methyl isobutyl ketone, methyl ethyl ketone, ethyl alcohol, mineral spirits, ethylene glycol monoethyl ether acetate, and other aliphatic, alicyclic, and aromatic hydrocarbons, esters, ethers, ketones, and alcohols, which are conveniently used. Alternatively, acrylic copolymers can be prepared via free radical emulsification or suspension addition polymerization, or by dispersing a preformed polymer under shear in an aqueous medium. Preferably, the acrylic copolymers of the present invention are solvent-type.

[0026] Suitable monomers for the preparation of acrylic copolymers include (meth)acrylates, such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and combinations thereof. Additional monomers, including carboxylic acid monomers such as (meth)acrylic acid and itaconic acid and their salts, sulfonic acid monomers such as sodium styrenesulfonate and sulfonic acid acrylamide-methyl-propane and their salts, and phosphoric acid monomers such as phosphoethyl methacrylate and its salts, may be used to prepare acrylic copolymers. Monomers such as styrene, acrylonitrile, acetoacetoxyethyl methacrylate (AAEM), and alkoxysilane-functionalized (meth)acrylates, as well as monomers that can impart co-curing functional groups such as glycidyl (meth)acrylate and hydroxyalkyl (meth)acrylate, may also be used in the preparation of acrylic copolymers. In certain embodiments, it may be advantageous to incorporate small amounts of copolymerized polyethylenically unsaturated monomer groups into the acrylic copolymer, including allyl (meth)acrylate, diallyl phthalate, 1,4-butylene glycol di(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and divinylbenzene. It may also be advantageous to heterogeneously incorporate such monomer groups into the polymer to form multiphase polymer particles and create core-shell, hemispherical, or occluded morphologies. Chain transfer agents may be used to prepare these acrylic copolymers, examples of which include dodecyl mercaptan, 2-mercaptoethanol, mercaptotrialkoxysilane, butyl mercaptopropionate, methyl mercaptopropionate, and mercaptopropionic acid. Initiators may be used to prepare these acrylic copolymers, examples of which include peroxy and azo compounds.

[0027] The epoxy functionalized groups of the acrylic copolymer include glycidyl groups such as glycidyl methacrylate (GMA) or glycidyl acrylate, with GMA being preferred. The curing-compatible groups of the acrylic copolymer include, in polymer form, monomer groups containing one or more of the following: alcohol (OH) functional groups, phenolic groups, silicone groups, tertiary amines such as 3-(trimethoxysilyl)propyl methacrylate (MATS) in the monomer, or acidic groups that are either attached to the main chain (as in the case of acrylic monomers) or linked as terminal groups, for example, in this case an OH functionalized chain transfer agent is used for polymerization. Preferably, the curing-compatible groups are hydroxyethyl (meth)acrylate (HEMA or HEA). Preferably, the acrylic copolymer is synthesized from monomers including GMA, HEMA, methyl methacrylate (MMA), and 2-ethylhexyl acrylate (EHA).

[0028] The acrylic copolymer contains 30-80% by weight of glycidyl (meth)acrylate monomer units, preferably 40-60% by weight of glycidyl (meth)acrylate monomers, and most preferably more than 30% by weight of glycidyl (meth)acrylate monomers, based on the weight of the total monomer units added to produce the copolymer. The acrylic copolymer contains up to 20% by weight of curing-compatible group monomer units, preferably up to 10% by weight of curing-compatible group monomer units, preferably up to 8% by weight of curing-compatible group monomer units, and preferably more than 2% by weight of curing-compatible group monomer units, based on the weight of the total monomer units added to produce the copolymer, with a preferred range of 5-10% by weight. The upper limit of curing-compatible groups is mainly determined by the viscosity of the copolymer when HEMA is combined with GMA functional groups. Theoretically, when using other monomers, such as a combination of HEA and glycidyl acrylate, it is possible to have a higher content of curing-compatible groups. When determined according to ASTM D1652, the acrylic copolymer contains epoxy equivalents (EEW) in the range of 200 to 600 g / mol epoxy, preferably greater than 250 g / mol epoxy, more preferably greater than 275 g / mol epoxy, more preferably less than 500 g / mol epoxy, and more preferably less than 450 g / mol epoxy, with a preferred range of 300 to 400 g / mol epoxy.

[0029] Acrylic copolymers have a calculated glass transition temperature ("Tg") of 80 degrees Celsius (80°C) or less, preferably 30°C or less, most preferably 15°C or less, with a preferred range of -40°C to 10°C. The Tg is achieved by selecting monomers and amounts of monomers to achieve the desired polymer Tg, as is well known in the art. The Tg of a polymer is measured using dynamic scanning calorimetry.

[0030] The acrylic copolymer solution is a viscous liquid with a viscosity in the range of 500 centipoise (cP) to 8,000 cP at room temperature (25°C) with a solid content of approximately 70%. The acrylic copolymer of the present invention has a number average molecular weight of 500 to 10,000 g / mol, preferably 1,000 to 5,000 g / mol or more, or more preferably 4,000 g / mol or less, as measured by gel permeation chromatography using a polystyrene standard.

[0031] Description of the coating composition The coating composition of the present invention comprises an acrylic copolymer and an amino-functionalized silicone resin. The molar ratio of amine NH functional groups to epoxy functional groups is in the range of 0.5 to 1.3, preferably 0.8 to 1. Preferably, an excess of amine groups is best avoided, as it can lead to amine blush, which adversely affects external durability. Amine blush results in loss of gloss when exposed to water. The coating composition can be accelerated to cure, but typically undergoes ambient curing.

[0032] The coating composition of the present invention may contain additional compositions including, but not limited to, accelerators / plasticizers such as benzyl alcohol, salicylic acid, and tris-2,4,6-dimethylaminomethylphenol; fillers such as finely divided minerals including silica, alumina, zirconia, talc, sulfate, TiO2, carbon black, graphite, silicate, etc.; other curing agents; other epoxy resins; reinforcing agents; rheology modifiers; solvents; accelerators; surfactants; ultraviolet (UV) stabilizers; antioxidants; wetting agents; solvents; defoaming agents; strengthening agents; and colorants including pigments, dyes, and colorants.

[0033] The curable coating compositions of the present invention may be uncolored, transparent clear coats, or colored systems for primer, base coat, and top coat applications. The pigments may be any typical organic or inorganic pigments. Several different pigments may be required to achieve the desired color for a particular application. Examples of suitable pigments include, but are not limited to, titanium dioxide, opaque polymers, barite, clay, calcium carbonate, red iron oxide, CI Pigment Yellow 42, CI Pigment Blue 15, 15:1, 15:2, 15:3, 15:4 (copper phthalocyanine), CI Pigment Red 49:1, CI Pigment Red 57:1, and carbon black.

[0034] The resulting coating composition can be applied to a substrate using techniques known in the art, such as spraying, brushing, swiping, and roll coating. The nominal dry film thickness (DFT) of the coating is 1 mil or more, preferably 2 mil or more, preferably 2.5 mil or more, and more preferably 3 mil or more. 1 mil corresponds to 1 / 1000 of an inch. Examples of substrates that can be coated include, but are not limited to, plastics, wood, metals (such as aluminum, steel, or galvanized sheets), tinned steel, concrete, glass, composite materials, urethane elastomers, and primer (painted) substrates. The coating can be cured at room temperature or at high temperatures using a forced-air oven or other type of heat source.

[0035] The following examples illustrate the present invention.

[0036] Examples and experimental methods: Acrylic copolymer Xylene was added to a 500 mL four-necked round-bottom flask equipped with a stirring shaft, condenser, thermocouple port, and additional port. The temperature of the xylene was raised to reflux (140°C) using a heating mantle. A monomer blend consisting of glycidyl methacrylate (GMA), methyl methacrylate (MMA), 2-ethylhexyl acrylate (EHA), and 2-hydroxyethyl methacrylate (HEMA) was weighed, mixed in a 500 mL glass jar, and then evenly divided into 50 mL plastic feed syringes with Luer lock connectors. The initiator, tert-butyl peroxyacetate (TBPA, 50% in mineral spirits), was added to a single 50 mL plastic syringe and connected to a feed tube via a Luer lock connector with a long feed needle attachment. The monomer mixture was added at a constant feed rate using a dual syringe pump, and the initiator was fed using a single feed syringe pump. Feeding was initiated when the solvent was refluxing. The feed rate, time, and temperature depend on the half-lives of the solvent and initiator. Once the feed was depleted, the line was flushed with a small amount of solvent. The run was continued for another hour to reduce residual monomers and initiators to acceptable levels. Table 1 shows the acrylic copolymers prepared. [Table 1]

[0037] Characterization of acrylic copolymers GPC A 2 mg / mL sample was dissolved in tetrahydrofuran (THF), and the solution was filtered through a 0.2 μm PTFE syringe filter before injection. Molecular weight measurements were performed using GPC measured on an Agilent 1100 series with a MIXED-D column (300 x 7.5 mm) at a flow rate of 1.0 mL / min at 35°C. An Agilent refractive index detector was used with Agilent's GPC / SEC software. Calibration was performed using 17 narrow PS standards from Polymer labs, and a cubic polynomial curve was fitted over the range of 3,742 kg / mol to 0.580 kg / mol.

[0038] EEW EEW was measured according to ASTM D1652. Epoxy resin was dissolved in methylene chloride and titrated with standardized 0.1N perchloric acid (HClO4) in glacial acetic acid in the presence of excess tetraethylammonium bromide (TEAB) in acetic acid. Measurements were performed using a Metrohm905 titrator and associated Tiamo titration software configured for EEW determination.

[0039] Solids content percentage Label the bottom of a small aluminum pot, place the pot on a scale, and record its weight to the nearest 0.0001 grams. Using a pipette, evenly distribute approximately 0.5g to 1.5g of sample into the pot. Record this weight as the initial weight (pot + sample). Before placing the sample in the oven, place it on a baking tray, clip it with a binder clip, use a pipette to coat the resin with approximately 2 grams of toluene, and then carefully place it in a preheated Class A oven. After 2 hours, remove the baking tray and sample from the oven. Set the balance to zero, place the sample (and pot) on the balance, record the final weight, and calculate the solids content using the following formula. Solids %=(Final weight - Pot weight) / (Initial weight - Pot weight)*100

[0040] glass transition temperature T g Samples of approximately 5-10 mg were measured using differential scanning calorimetry (DSC Q2000 V24.10) according to ASTM D7426. Temperature profiles were obtained as follows: isotherm at 10°C for 5 minutes; isotherm at 10°C / min ramp down to -50°C for 5 minutes; isotherm at 10°C / min ramp up to 150°C for 5 minutes; and Tg was analyzed using TA software.

[0041] viscosity Viscosity measurements were performed using a Brookfield DV-III Ultra Viscometer with a Small Sample Adapter (SSA). The rheologically accurate cylindrical shape of the Small Sample Adapter provides highly accurate viscosity measurements and shear rate determinations. For these samples, 9 mL of material was deposited into the cylinder, and the rate was varied using a spindle #31 or #34 to achieve a torque of approximately 25 Newton meters (N*m). Measurements were reported in centipoise (cP).

[0042] Amino-functional silicone resin The amino-functionalized silicone resins S1 to S6 are shown in Table 2. Resins S1 to S4 incorporate aryl groups by SiC grafting, resin S5 incorporates aryl groups by SiC grafting, and resin S6 does not incorporate aryl groups. Resins S1, S3, and S4 incorporate amine functional groups via SiC bonds, while resins S2, S5, and S6 incorporate amine functional groups via SiC bonds. The procedure for producing resins S1 to S6 is provided after Table 2. [Table 2]

[0043] S1:D 0.14 T NH2 0.22 T Me 0.64 (OBz) 0.21 , amine equivalent 261g / eq NH, 37mol% OMe, 20mol% OEt Test material: ● Methyltrimethoxysilane (MTM) - Mw = 136.22 ●Dimethyldimethoxysilane - Mw=120.22 ● Aminopropyltriethoxysilane - Mw = 221.37 ● Benzyl alcohol - Mw = 108.14 g / mol, bp = 205℃

[0044] procedure: The following was packed into a 250 mL two-necked round-bottom flask. -MTM (80.96g, 0.594mols, 1.783mols OMe) -Dimethyldimethoxysilane (21.88g, 0.182mols, 0.364mols OMe) -3-aminopropyltriethoxysilane, available from The Dow Chemical Company as Dowsil® Z-6011 (48.78g, 0.220mols, 0.660mols OEt) - Benzyl alcohol (22.25g, 0.206mols)

[0045] The flask was equipped with a Dean Stark apparatus attached to a magnetic stirring rod and a water-cooled condenser. The mixture was miscible at room temperature. Starting at room temperature, deionized water (16.73 g, 0.929 mols) was slowly added. After heating to 46°C, the mixture was heated in an aluminum block at a pot temperature of 65°C for 1 hour. Next, the temperature was increased and the alcohol was removed by distillation to a pot temperature of 150°C. Amount of volatile substances removed: 73.65 g. Heating was continued at 150°C for 5 hours. 1.65 g of volatile substances were removed within the first hour. No further was collected after this time. The product was stripped using a rotary evaporator (rotovapor) at an oil bath temperature of 120°C and a pressure of approximately 1.5–2 mmHg. The product was a clear, colorless, viscous liquid at room temperature. Isolation yield: 100.5 g. 13 Amine equivalent calculated from ¹³C NMR spectrum: 261 g / mol NH₄. NMR analysis of product: D 0.136 T PrNH2 0.219 T Me 0.645 , OZ content: 79.1 mol% (OMe=36.6 mol%; OEt=19.7 mol%; OBz=21.2 mol%; OH=1.6 mol%).

[0046] S2:T Me 0.99 (OBz) 0.2 (OCH(CH3)CH2NH2) 0.18, amine equivalent 297g / eq NH, 32.5mol% OZ) Test material: ● Methyl-T resin (described below): D 0.01 T Me 0.99 FW=83.52g / mol Si;OZ=71.77mol%(OMe=70.30mol%, OH=1.47mol%) ●1-Amino-2-propanol - Mw=75.11, bp=160℃ ● Benzyl alcohol - Mw = 108.14 g / mol, bp = 205℃ ●Xylene-ACS grade

[0047] procedure: ●The following was filled into a 250 mL two-necked round-bottom flask. -Methyl-T resin (84.89g, 1.016 mols Si, 0.729 mols OZ) -1-amino-2-propanol (16.52g, 0.220mols) - Benzyl alcohol (22.21g, 0.205mols) - Xylene (36.67g)

[0048] The flask was equipped with a Dean Stark apparatus attached to a magnetic stirring rod and a water-cooled condenser. The amount of xylene added yielded a theoretical yield of 75 wt% in xylene. The reaction mixture was initially cloudy at room temperature but became clear within 5 minutes at room temperature. Theoretical amount of methanol that could be produced when 100% BzOH reacted with the amine: 13.62 g. The mixture was heated to a pot temperature of 135°C using an aluminum block. The start time was measured from when volatile substances first began to be collected in the Dean Stark apparatus corresponding to a pot temperature of 127°C. The reactants were heated to 135°C and then held at this temperature. Total time: 12 hours. Volatile substances removed: 30 minutes - 3.81 g, 1 hour - 6.28 g, 2 hours - 8.39 g, 3 hours - 10.06 g, 4 hours - 10.55 g, 5 hours - 10.77 g. No volatile substances were collected after 5 hours. Analysis of the sample after 12 hours by 13C NMR showed that approximately 89% of 1-amino-2-propanol reacted with silicon. Approximately 93% of benzyl alcohol also reacted with silicon.

[0049] Preparation of methyl-T resin: T resin with a target of 75 mol% OMe Me 1 resin Test material: ● Methyltrimethoxysilane - Mw = 136.22 ● Deionized water ● Trifluoromethanesulfonic acid, available from 3M as Fluorad(trademark) FC-24 - Mw = 150.08 g / mol, density = 1.696 g / ml ● Calcium carbonate powder, particle size ≤50um, Mw = 100.09 g / mol

[0050] procedure: A 1 L four-necked round-bottom flask was packed with methyltrimethoxysilane (650.0 g, 4.772 mols Si, 14.315 mols OMe). FC24 (0.33 g, 192 uL) was added, which corresponds to 500 ppm. Starting at room temperature, deionized water (96.71 g, 5.368 mols) was slowly added. The mixture was heated to 64°C. Theoretical amount of methanol that could be produced: 344.0 g (assuming 100% hydrolysis and condensation). The mixture was heated at 65°C for 2 hours. 320.88 g of methanol was removed by distillation to a pot temperature of 75°C. Calcium carbonate (1.32 g) was added to neutralize the FC24, which corresponds to four times the amount of FC24 added (based on weight). The mixture was mixed for 2 hours while cooling to room temperature. The resin was stripped using a rotary evaporator. Oil bath temperature = 50°C, approximately 50-60 mmHg. Pressure filtration was performed at room temperature through a 142 mm diameter Magna, Nylon, Supported, Plain, 0.45 Micron filter. Isolation yield: 394.0 g. The product was a clear, low-viscosity liquid at room temperature. Molecular weight: Mn = 1,837; Mw = 2,838 (compared to polystyrene standard in THF). 29Si NMR analysis of the product: D Me2 0.010 T Me 0.990 OZ = 71.77 mol% (70.30 mol% OMe, 1.47 mol% OH), FW = 83.52 g / mol Si. Methoxy content was calculated from 13C NMR using CDCl3 as an internal standard.

[0051] S3: Amine siloxane resin having an aryl group added via SiC using a secondary alcohol and an amine functional group added via a SiC bond. Test material: ● Methyltrimethoxysilane (MTM) - Mw = 136.22 ●Dimethyldimethoxysilane - Mw=120.22 ● Aminopropyltriethoxysilane - Mw = 221.37 ●DL-sec-phenethyl alcohol (sPhEtOH)-Mw=122.17g / mol, bp=203~205℃

[0052] procedure: The following was packed into a 250 mL two-necked round-bottom flask. -MTM (77.25g, 0.567mols, 1.701mols OMe) -Dimethyldimethoxysilane (20.88g, 0.174mols, 0.347mols OMe) -Z-6011 (48.76g, 0.220mols, 0.660mols OEt) -sec-phenethyl alcohol (25.10g, 0.205mols)

[0053] The flask was equipped with a Dean-Stark apparatus attached to a magnetic stirring rod and a water-cooled condenser. The mixture was miscible at room temperature. Starting at room temperature, deionized water (16.17 g, 0.898 mols) was slowly added. The mixture was heated to 43°C. The mixture was heated for 1 hour at a pot temperature of 65°C using an aluminum block. The temperature was increased, and the alcohol was removed by distillation to a pot temperature of 150°C. Amount of volatile substances removed: 67.98 g. Heating was continued at 150°C for 10 hours. Volatile substances removed: 1 hour - 2.22 g, 2 hours - 3.57 g, 3 hours - 4.02 g, 4 hours - 4.22 g, 5 hours - 4.42 g. No volatile substances were collected after 5 hours. The product was stripped using a rotary evaporator at an oil bath temperature of 120°C and at approximately 1.5-2 mmHg.

[0054] Results: The product was a slightly yellowish, clear, viscous liquid at room temperature. Isolation yield: 98.4 g. 13 Amine equivalent calculated from ¹³C NMR spectrum: 258 g / mol NH₄. NMR analysis of product: D 0.135 T PrNH2 0.227 T Me 0.638OZ content: 78.5 mol% (OMe=32.1 mol%; OEt=23.9 mol%; sec-PhEtO=20.1 mol%; OH=2.4 mol%); 8.52 wt% OMe; 9.18 wt% OEt; 20.8 wt% sec-PhEtO; 13.3 wt% phenyl (from sec-PhEtO). OR values ​​calculated from 13C NMR data using CDCl3 as an internal standard. PrNH2 and T Me The Si mole fraction for this was derived from 13C NMR data.

[0055] S4: Aminesiloxane resin having an aryl group added via SiC using a tertiary alcohol and an amine functional group added via a SiC bond. Test material: ● Methyltrimethoxysilane (MTM) - Mw = 136.22 g / mol ● Aminopropyltrimethoxysilane - Mw = 179.29 ● 2-methyl-1-phenyl-2-propanol - Mw=150.22, bp=215℃ ●Xylene-ACS grade ●KOH (45% in water)-Mw=56.1g / mol ●HCl solution - 8.0N HCl in water was diluted with methanol to obtain a solution containing 0.000742 mols HCl / gram.

[0056] procedure: The following was packed into a 250 mL two-necked round-bottom flask. -MTM (97.01g, 0.712mols, 2.136mols OMe) - Aminopropyltrimethoxysilane (39.40 g, 0.22 mols, 0.659 mols OMe) -2-methyl-1-phenyl-2-propanol (39.85g, 0.265mols)

[0057] The flask was equipped with a Dean Stark apparatus attached to a magnetic stirring rod and a water-cooled condenser. 1.8 times MePhPrOH was added. Starting at room temperature, deionized water (17.14 g, 0.951 mols) was slowly added. The mixture was heated to 50°C. It was heated for 1 hour at a pot temperature of 65°C using an aluminum block. It remained cloudy throughout. The temperature was increased, and methanol was removed by distillation to a pot temperature of 95°C. Amount of volatile substances removed: 53.9 g. Diluted to approximately 75% with xylene (36.67 g). Clear. While mixing, a solution containing (45% KOH (aq) of 0.122 g in 1 g methanol) was added at room temperature. This amount of KOH corresponds to approximately 500 ppm based on the theoretical yield. It was heated using an aluminum block. The start time was measured from when volatile substances first began to be collected in the Dean Stark apparatus corresponding to a pot temperature of 91°C. The mixture was heated to 115°C and then left to stand at this temperature. Volatile substances removed: 30 minutes = 9.32 g, 1 hour = 10.72 g, 2 hours = 11.86 g. No volatile substances were collected after 2 hours. Total time = 12 hours. 13C NMR analysis of the 5-hour sample showed that approximately 35% of the MePhPrOH reacted with silicon. 13C NMR analysis of the 12-hour sample showed that approximately 46% of the MePhPrOH reacted with silicon. An additional HCl solution (1.38 g solution) was added at room temperature. Stoichiometric 1.05 mols HCl:1.0 mols KOH. Mixed overnight at room temperature. The product was stripped using a rotary evaporator at an oil bath temperature of 120°C and approximately 2 mmHg. Pressure filtration was performed at room temperature through an Osmonics MAGNA Nylon Supported Plain 0.45 μm filter (47 mm diameter). The filtration rate was slow. Only 80-90% of the material was filtered out.

[0058] Results: The product was a clear, pale yellow, viscous liquid at room temperature. Isolation yield: 91.3 g. 13 Amine equivalent calculated from ¹³C NMR spectrum: 229 g / mol NH₄. NMR analysis of the product: T PrNH2 0.233 T Me0.767 ; OZ content: 63.8 mol%; (51.3 mol% OMe, 12.5 mol% MePhPrO); 17.5 wt% MePhPrO; 9.1 wt% phenyl (from MePhPrO); Si molar ratio and OR value derived from 13C NMR data.

[0059] S5: DTPh resin reacted with amino - propanol Reagents: ● Dowsil (trademark) 3074 - D available from The Dow Chemical Company 0.337 T シクロヘキシル 0.010 T Ph 0.653 ; OZ = 68.64 mol%; FW approximately 126.5 g / mol Si ● 1 - Amino - 2 - propanol - Mw = 75.11, bp = 160 °C

[0060] Procedure: A 250 mL one - neck round - bottom flask was charged with Dowsil (trademark) 3074 (94.19 g, 0.745 mols Si, 0.511 mols OZ) and 1 - amino - 2 - propanol (16.52 g, 0.220 mols, 0.440 mols NH). The flask was equipped with a Dean Stark apparatus attached to a magnetic stir bar and a water - cooled condenser. The mixture was not compatible at room temperature. It was heated at an aluminum block temperature of 140 °C for 2 hours. The amount of volatile substances collected at the first hour was 3.35 g, and at the second hour was 0.31 g. While heating at 140 °C, the reaction mixture became transparent. The block temperature was raised to 180 °C. It was held at this temperature for 2 hours. The amount of volatile substances collected at the first hour was 1.85 g, and at the second hour was 0.13 g. The product was stripped on a rotary evaporator at an oil bath temperature of 115 °C and approximately 1 mmHg.

[0061] Results: The product was a clear viscous liquid at room temperature. Isolated yield: 100.9 g. 13 Amine equivalent calculated from 13C NMR spectrum: 256 g / mol NH. NMR analysis of the product: D0.333 T シクロヘキシル 0.007 T Ph 0.660 ; OZ content: 61.95 mol% 26.9 mol% OR; 33.5 mol% OMe. The above two OR values were calculated from 13C NMR by taking the ratio of the OR integral values and dividing it by the integral value of the phenyl group.

[0062] S6: Me-T resin reacted with 1-amino-2-propanol without aryl functional groups Reagents: ● Dowsil™ CF-2403 methyl-T resin-D available from The Dow Chemical Company 0.015 T Me 0.985 FW = 93.4 g / mol Si; OMe = 113.6 mol% ● 1-amino-2-propanol - Mw = 75.11, bp = 160 °C

[0063] Procedure: A 250 mL two-neck round-bottom flask was charged with Dowsil™ CF-2403 (80.0 g, 0.857 mols Si, 0.973 mols OMe) and 1-amino-2-propanol (14.47 g, 0.193 mols). The flask was equipped with a magnetic stir bar, nitrogen, an applied nitrogen blanket, and a Dean Stark apparatus attached to a water-cooled condenser. The reaction mixture was turbid at room temperature. It was heated using an aluminum block. The start time was measured when volatile substances began to be collected in the Dean Stark apparatus corresponding to a pot temperature of 101 °C. It was heated to 125 °C and then held at this temperature. Total time = 4 hours. During heating, at about 60 °C, the reaction mixture became transparent. Volatile substances removed: 30 minutes - 5.97 g; 1 hour - 6.00 g. No volatile substances were collected after 1 hour. The product was stripped on a rotary evaporator at an oil bath temperature of 70 °C and about 2 mmHg.

[0064] Results: The product was a clear, low-viscosity liquid at room temperature. Yield: 76.4 g.13 Amine equivalents calculated from the 13C NMR spectrum: 241 g / mol NH₃. The amine equivalents were calculated from the 13C NMR data using the average of two carbon atoms in the 13C NMR spectrum (approximately 20 ppm and 70 ppm), with CDCl3 as the internal reference. Integrated values ​​(9.38 and 8.62). NMR analysis of the product: D 0.010 T Me 0.990 Total OZ content: 100.3 mol% (20.6 mol% OR; 79.7 mol% OMe) OR = 1-amino-2-propanol reacted with silicon.

[0065] Coating composition: Clear coating The clear coating compositions shown in Table 3 were prepared by the following method: Acrylic copolymer was placed in a MAX 40 SpeedMixer® cup, an amino-functional silicone resin was added, and the mixture was combined in a FlackTek® DAC150 SpeedMixer® at 2000 rpm for 2 minutes. In the formulation of the coating compositions, the acrylic copolymer and amino-functional silicone resin were added in amounts that provided a 1:1 epoxy / NH molar ratio. [Table 3]

[0066] The coating's Tg was measured using DSC (first heating at 20°C / min) and determined after 10 days of moisture curing.

[0067] The comparison of CTG1, CTG2, and CTG5 in Table 2 illustrates the advantages of the present invention. CTG1 contains 21 mol% of phenyl groups, CTG2 contains 22 mol% of phenyl groups, and CTG5 contains 66 mol% of phenyl groups. Comparatively, CTG5 contains a higher mol% of phenyl groups than CTG1 or CTG2, and incorporates these groups via SiC bonds, but the coating becomes cloudy and exhibits inferior properties. CTG1 and CTG2 demonstrate that the incorporation of phenyl groups via SiC bonds can provide a high-quality, optically transparent coating even when the incorporation of aryl groups via SiC bonds is less than that of the SiC bonded version. The industrial applicability of the present invention should not be underestimated, considering the lower cost of SiC-based resins compared to SiC-based resins.

[0068] Method of applying direct debit for clear coat application Coatings were applied to Q-Panel R-412-I (phosphated cold-rolled steel) and AL412 (chromated aluminum) panels according to ASTM D4147. The panels were secured to a firm, horizontal surface using magnetic chucks or clamps. The coatings were applied to the panels using a multi-clearance square applicator, achieving a desired dry film thickness of approximately 2.5 mils with a target wet thickness of 5-6 mils.

[0069] Application and testing methods for coatings Withdrawal procedure The coating was applied to the metal panel according to ASTM D4147-99 (2007). The panel was secured to a firm, horizontal surface using a magnetic chuck. A sufficient amount of coating was poured over the entire upper edge of the panel, and a uniform film was applied by using a 5-mil gap wet film applicator to pull the coating down along the length of the panel towards the operator with uniform pressure and speed. The panel was cured in a controlled temperature and humidity laboratory at 72°F and 50% relative humidity.

[0070] Drying time: The coating was dropped onto a 1" × 12" glass substrate with a 76 micrometer (μm) thick wet film, and a BYK drying time recorder was set up. Using a BYK drying time recorder compliant with ASTM D5895-03, touch-dry time, non-stick time, and dry hardness were measured by dragging a needle through the coating.

[0071] Pendulum hardness: Pendulum hardness was measured using a BYK Gardner pendulum hardness tester equipped with a König pendulum. The tester was operated according to ISO 1522 and set to measure hardness in seconds.

[0072] pencil hardness The pencil hardness of the coating film is measured according to the ASTM D3363 method. The coating composition is applied to a glass panel to form a wet film with a thickness of 120 microns, which is cured at room temperature for 7 days. The resulting film is then tested with Zhonghua pencils. The pencil hardnesses used are 9H, 8H, 7H, 6H, 5H, 4H, 3H, 2H, H, F, HB, B, 2B, 3B, 4B, 5B, and 6B, where 9H is the hardest and 6B is the softest.

[0073] Gloss: The gloss of the coating at 20°, 60°, and 85° was measured according to ASTM D-523-89 using a BYK Gardner microTRI gloss meter.

[0074] Methyl ethyl ketone double friction test: A double friction test of methyl ethyl ketone (MEK) was performed according to ASTM D5402 using a semi-automatic MEK friction tester manufactured by DJH DESIGNS INC. The test continued until the coating was removed to the substrate by friction or until up to 200 double friction cycles were completed without breakage.

[0075] The performance characteristics of the coating compositions are shown in Section 4. Compared to Ctg7 and Ctg8, Ctg1 and Ctg2 exemplify the importance of curing compatibility groups (e.g., HEMA) in the acrylic copolymer, providing improved pencil hardness, improved drying time, improved gloss readings, improved hardness, and improved MEK resistance. [Table 4]

Claims

1. 1. A curable coating composition comprising: (1) In polymerized form (i)(R 3 SiO 1/2 ) a 、 (fm)(R 2 Si(OR') x O (2-x)/2 ) b 、 (iii) (RSi(OR') y , O (3-y)/2 ) c , and (iv)(Si(OR') z O (4-z)/2 ) d wherein each R′ is independently hydrogen, an alkyl group, a functionalized alkyl group, an aryl group, or a functionalized aryl group, provided that at least 10 mole percent of all R′ groups are aryl groups or functionalized aryl groups; wherein each R is independently hydrogen, an alkyl group, or a functionalized alkyl group; wherein at least 10 mole percent of the combined R and R′ groups have the formula: —R a -NHR b is an amine-containing group of the formula a is an alkyl or aryl-containing group derived from an amino alcohol, and R b is hydrogen or an alkyl group, wherein a+b+c+d=1.00 (100 mole percent), x is either 0 or 1, y is either 0, 1, or 2, and z is either 0, 1, 2, or 3; an amino-functional silicone resin having an —NH— equivalent weight of 50 to 750; (2) an acrylic copolymer having, in polymerized form, epoxy-functionalized groups and cure-compatible groups; A curable coating composition, wherein said coating composition has a molar ratio of amine NH functional groups to epoxy functional groups in the range of 0.5 to 1.

3.

2. 10. The coating composition of claim 1 having a molar ratio of amine NH functional groups to epoxy functional groups in the range of 0.8 to 1.

3. At least 20 mole percent of the combined R and R′ groups of the amino-functional silicone resin are of the formula: a -NHR b 2. The coating composition of claim 1, wherein the amine-containing group is

4. From 5 to 42 mole percent of the combination of R and R′ groups of the amino-functional silicone resin are of the formula: a -NHR b 2. The coating composition of claim 1, wherein the amine-containing group is

5. 10. The coating composition of claim 1, wherein the amino alcohol is selected from the group of: (a) sterically hindered around the COH moiety, (b) a secondary or tertiary alcohol, or (c) a mixture thereof.

6. The coating composition of claim 1, wherein the amino alcohol is 1-amino-2-propanol or 1-amino-2-methylpropan-2-ol.

7. 10. The coating composition of claim 1, wherein 20 to 50 mole percent of all R' groups are aryl groups or functionalized aryl groups.

8. 10. The coating composition of claim 1, wherein the epoxy-functionalized groups of the acrylic copolymer are derived from one or more monomers selected from the group of glycidyl methacrylate (GMA), glycidyl acrylate, and mixtures thereof, and the acrylic copolymer has an epoxy equivalent weight (EEW) in the range of 200 to 600.

9. 9. The coating composition of claim 8, wherein the acrylic copolymer comprises 30 to 60 weight percent glycidyl (meth)acrylate monomer units in polymerized form, based on the weight of total monomer units of the acrylic copolymer.

10. 10. The coating composition of claim 1, wherein the acrylic copolymer comprises from 2% to 20% by weight of cure compatible group monomer units in polymerized form, based on the weight of the total monomer units of the acrylic copolymer.

11. 10. The coating composition of claim 1, wherein the cure compatible groups of the acrylic copolymer comprise, in polymerized form, monomeric groups containing one or more of an alcohol (OH) functional group, a phenolic group, a tertiary amine, or an acid group either pendant to the backbone or attached as an end group.

12. The coating composition of claim 1 , wherein the cure compatible group is derived from hydroxyethyl methacrylate (HEMA).

13. A coated article comprising one or more layers of the cured coating composition of claim 1.