Austenitic stainless steel and its manufacturing method
Patent Information
- Application Number
- JP2023512141
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-09-03
- Filing Date
- 2021-08-26
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2041-08-26
AI Technical Summary
【0016】 本発明によれば、高強度と高延性を同時に満足する超細粒300系ステンレス鋼を提供することができる。 また、本発明は、高強度-高延性を同時に満足するオーステナイト系ステンレス鋼を提供すると共に、高価の合金元素であるNi、Crの含量を低減して経済的である。 さらに、本発明は、高強度-高延性を同時に満足すると共に、優れた耐食性を確保可能なオーステナイト系ステンレス鋼を提供することができる。
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to austenitic stainless steel and a method for manufacturing the same, and more particularly, to austenitic stainless steel that can be utilized as various materials such as for automotive outer panels and building components, and a method for manufacturing the same.
Background Art
[0002] Austenitic stainless steel is applied in various uses such as transportation parts and building parts due to its excellent formability, work hardening ability, and weldability. However, typical general-purpose austenitic stainless steels such as 304 series stainless steel and 301 series stainless steel have a yield strength in the range of 200 to 350 MPa, and thus have limitations in application to structures due to their low strength.
[0003] As a measure to increase the yield strength of austenitic stainless steel, temper rolling may be additionally performed. However, such a measure has problems in that the cost increases due to additional processes, and the elongation rate of the material deteriorates extremely.
[0004] Patent Document 1 discloses a method for manufacturing 300 series stainless steel with a small warp even after half etching by stress relief (SR) heat treatment twice after temper rolling a cold-rolled annealed material for a laser metal mask for photoetching. However, Patent Document 1 relates to a manufacturing technique for controlling etching properties and warp after etching, and the Austenitic Stability Parameter (ASP) value of the austenite phase stability is 30 to 50, and there is a risk that the transformation of deformed organic martensite occurs rapidly during forming and the elongation rate decreases.
[0005] Patent Document 2 relates to components for nuclear power plants, and describes a method for producing austenitic stainless steel with an average grain size of 10 μm or less, which involves long-term heat treatment at 600-700°C for 48 hours or more. However, according to Patent Document 2, since long-term heat treatment is required, there are problems in implementing it in an actual production line, such as reduced productivity and increased manufacturing costs. [Prior art documents] [Patent Documents]
[0006] [Patent Document 1] International Publication No. 2016 / 043125 [Patent Document 2] Japanese Patent Publication No. 2020-50940 [Overview of the project] [Problems that the invention aims to solve]
[0007] The objective of this invention is to provide an ultrafine-grained 300 series stainless steel that simultaneously satisfies high yield strength and excellent elongation. [Means for solving the problem]
[0008] The austenitic stainless steel of the present invention is characterized by containing, by weight percent, C: 0.005~0.03%, Si: 0.1~1%, Mn: 0.1~2%, Ni: 6~9%, Cr: 16~19%, N: 0.2% or less, with the remainder being Fe and unavoidable impurities, and having an average crystal grain size d value of 5 μm or less for a thickness of 1 / 4t to 3 / 4t when the total thickness of the steel material is t, having an ASP value expressed by the following formula (1) of 10 to 25, having a value of 435 or more in the following formula (2), and having a value of 6000 or more in the following formula (3). (1)551-462*([C]+[N])-9.2*[Si]-8.1*[Mn]-13.7*[Cr]-29*([Ni]+[Cu])-18.5*[Mo]-68*([Nb]+[V]) (2)(1600*[N])+(700 / )+(4*ASP)-(20*[Ni])+100 (3) YS*EL-500*([Ni]+[Cr]) In the above formulas (1), (2), and (3), [C], [N], [Si], [Mn], [Cr], [Ni], [Cu], [Mo], [Nb], and [V] represent the weight percentage of each element, YS represents the yield strength (MPa), and EL represents the elongation (%).
[0009] Furthermore, each austenitic stainless steel according to the present invention may have a value of 200 or more in the following formula (4). (4) Hv-([Ni]+[Cr]) In equation (4) above, Hv represents the Vickers hardness (Hv), and [Ni] and [Cr] represent the weight percentage of each element.
[0010] Furthermore, each austenitic stainless steel according to the present invention may further contain one or more of the following in weight percent: Cu: 0.4% or less, Mo: 0.2% or less, Nb: 0.25% or less, and V: 0.25% or less.
[0011] Furthermore, in each austenitic stainless steel according to the present invention, the thickness t may be 0.4 to 2.0 mm.
[0012] Furthermore, each austenitic stainless steel according to the present invention may have a formal potential value of 250 mV or higher, measured by immersion in a 3.5% NaCl solution at 30°C.
[0013] The present invention relates to a method for producing austenitic stainless steel, which may include the steps of hot-rolling a slab containing, by weight %, C: 0.005-0.03%, Si: 0.1-1%, Mn: 0.1-2%, Ni: 6-9%, Cr: 16-19%, N: 0.2% or less, with the remainder being Fe and unavoidable impurities, followed by cold-rolling at room temperature with a reduction ratio of 40% or more, and annealing at 700-850°C.
[0014] Furthermore, the method for producing each austenitic stainless steel according to the present invention can be characterized by performing cold rolling without annealing after hot rolling.
[0015] In addition, the method for manufacturing each austenitic stainless steel according to the present invention may further include a step of temper rolling with a reduction rate of 60% or more.
Advantages of the Invention
[0016] According to the present invention, it is possible to provide an ultrafine grain 300 series stainless steel that simultaneously satisfies high strength and high ductility. In addition, the present invention provides an austenitic stainless steel that simultaneously satisfies high strength and high ductility, and is economical by reducing the contents of expensive alloy elements Ni and Cr. Furthermore, the present invention can provide an austenitic stainless steel that simultaneously satisfies high strength and high ductility and can ensure excellent corrosion resistance.
Brief Description of the Drawings
[0017] [Figure 1] It is a diagram showing the ranges of the invention examples and the comparative examples by the values of formula (2) and the values of formula (3). [Figure 2(a)] It is a diagram for comparing the average grain size d of the invention examples and the comparative examples. [Figure 2(b)] It is a diagram for comparing the average grain size d of the invention examples and the comparative examples. [Figure 2(c)] It is a diagram for comparing the average grain size d of the invention examples and the comparative examples. [Figure 3] (a) to (c) are graphs showing the Strain (%) - Stress (MPa) curves of the invention examples. [Figure 4] (a) to (c) are graphs showing the Strain (%) - Stress (MPa) curves of the comparative examples.
Embodiments for Carrying Out the Invention
[0018] The austenitic stainless steel of the present invention is characterized by containing, by weight percent, C: 0.005~0.03%, Si: 0.1~1%, Mn: 0.1~2%, Ni: 6~9%, Cr: 16~19%, N: 0.2% or less, with the remainder being Fe and unavoidable impurities, and having an average crystal grain size d value of 5 μm or less for a thickness of 1 / 4t to 3 / 4t when the total thickness of the steel material is t, having an ASP value expressed by the following formula (1) of 10 to 25, having a value of 435 or more in the following formula (2), and having a value of 6000 or more in the following formula (3). (1)551-462*([C]+[N])-9.2*[Si]-8.1*[Mn]-13.7*[Cr]-29*([Ni]+[Cu])-18.5*[Mo]-68*([Nb]+[V]) (2)(1600*[N])+(700 / )+(4*ASP)-(20*[Ni])+100 (3) YS*EL-500*([Ni]+[Cr]) In the above formulas (1), (2), and (3), [C], [N], [Si], [Mn], [Cr], [Ni], [Cu], [Mo], [Nb], and [V] represent the weight percentage of each element, YS represents the yield strength (MPa), and EL represents the elongation (%).
[0019] Preferred embodiments of the present invention are described below. However, embodiments of the present invention can be modified into various other forms, and the technical concept of the present invention is not limited to the embodiments described below. Furthermore, embodiments of the present invention are provided to give a more complete explanation of the present invention to a person with average skill in the art. The terminology used in this application is for illustrative purposes only. For example, singular expressions include plural expressions unless the context clearly requires them to be singular. In addition, it should be noted that terms such as “includes” or “comprising” used in this application are used to explicitly indicate the existence of features, stages, functions, components, or combinations thereof described in the specification, and are not used to provisionally exclude the existence of other features, stages, functions, components, or combinations thereof.
[0020] On the other hand, unless otherwise defined, all terms used herein should be considered to have the same meaning as that generally understood by a person of ordinary skill in the art to which this invention pertains. Therefore, unless explicitly defined herein, no particular term should be interpreted in an overly idealistic or formal sense. For example, in this specification, singular expressions include plural expressions unless there is an obvious exception in the context. Furthermore, the terms “approximately,” “substantially,” and similar terms used herein are used in the sense of or close to the numerical tolerances of manufacture and materials inherent to the meaning referred to, when such tolerances are presented, and are used to prevent unscrupulous infringers from unfairly exploiting disclosures that refer to precise or absolute numerical values in order to aid in understanding the invention.
[0021] Austenitic stainless steel is used in a variety of applications due to its excellent formability, work hardening ability, and weldability. However, it has the disadvantage of low yield strength, and when temper rolling is performed to increase yield strength, there is a problem of inferior elongation. The inventors of this invention focused on ultrafine-grained austenitic stainless steel as a steel material that simultaneously satisfies high yield strength and excellent elongation. However, even ultrafine-grained steel does not simultaneously satisfy high yield strength and excellent elongation. The Ni and Cr content differs for each steel type, the amount of martensite transformation during cold working differs depending on the degree of austenite phase stabilization, and the tensile curve characteristics differ depending on the TRIP (Transformation Induced Plasticity) transformation behavior. Therefore, even among ultrafine-grained austenitic stainless steels, the yield strength and elongation also differ greatly from steel to steel. Taking these effects into consideration, the inventors of this invention have devised an ultrafine-grained austenitic stainless steel that can simultaneously achieve high strength and high ductility.
[0022] The austenitic stainless steel of the present invention contains, by weight percent, C: 0.005-0.03%, Si: 0.1-1%, Mn: 0.1-2%, Ni: 6-9%, Cr: 16-19%, and N: 0.2% or less, with the remainder being Fe and unavoidable impurities. Furthermore, it may selectively contain one or more of the following: Cu: 0.4% or less, Mo: 0.2% or less, Nb: 0.25% or less, and V: 0.25% or less.
[0023] The reasons for limiting the alloy composition will be explained in detail below. The carbon (C) content is 0.005 to 0.03% by weight. Carbon (C) is a stabilizing element of the austenite phase. Considering this, C is added in an amount of 0.005% by weight or more in this invention. However, if the C content is excessive, it can lead to the formation of chromium carbides during low-temperature annealing, reducing grain boundary corrosion resistance. Therefore, in this invention, the C content is limited to 0.03% by weight or less. The silicon (Si) content is 0.1 to 1% by weight. Si is an ingredient added as a deoxidizing agent during steelmaking. When performing a bright annealing process, it forms Si oxides in the passivation film, improving the corrosion resistance of the steel. Considering this, Si is added at a concentration of 0.1% by weight or more in this invention. However, if the Si content is excessive, it can reduce ductility, so in this invention, the Si content is limited to 1.0% by weight or less.
[0024] The manganese (Mn) content is 0.1 to 1.0% by weight. Mn is a stabilizing element of the austenite phase. Considering this, in this invention, Mn is added at a concentration of 0.1% by weight or more. However, excessive Mn content can reduce corrosion resistance; therefore, in this invention, the Mn content is limited to 1.0% by weight or less. The nickel (Ni) content is 6.0-9.0% by weight. Ni is a stabilizing element of the austenite phase and has the effect of softening steel. Taking this into consideration, Ni is added in an amount of 6.0% by weight or more in this invention. However, if the Ni content is too high, the cost will increase, so in this invention, the Ni content is limited to 9.0% by weight or less.
[0025] The chromium (Cr) content is 16.0-19.0% by weight. Cr is a key element for improving the corrosion resistance of stainless steel. Considering this, in this invention, 16.0% by weight or more of Cr is added. However, if the Cr content is excessive, the steel hardens, which can suppress the transformation of deformed organic martensite during cold rolling. Therefore, in this invention, the Cr content is limited to 19.0% by weight or less. The nitrogen (N) content is 0.2% by weight or less. N is a stabilizing element of the austenite phase and improves the strength of steel. However, if the N content is excessive, the steel becomes hardened and its hot workability decreases. Therefore, in this invention, the N content is limited to 0.2% by weight or less.
[0026] The following section provides a detailed explanation of the reasons for limiting the content of the selective alloying components: Cu, Mo, Nb, and V. The copper (Cu) content may be 0.4% by weight or less. Cu is a stabilizing element of the austenite phase. However, if the Cu content is too high, the corrosion resistance of the steel decreases and costs increase. Therefore, in this invention, the Cu content is limited to 0.4% by weight or less. The molybdenum (Mo) content may be 0.2% by weight or less. Mo has the effect of improving corrosion resistance and processability. However, if the Mo content is too high, the cost increases, so in this invention, the Mo content is limited to 0.2% by weight or less. The content of Nb (niobium) or V (vanadium) may be 0.25% by weight or less. Nb and V have the effect of suppressing grain growth by forming (Nb,V)(C,N) precipitates when added. However, if the content of Nb and V is excessive, the cost increases, so in this invention, the content of Nb and V is limited to 0.25% by weight or less each.
[0027] The remaining component of this invention is iron (Fe). However, in the normal manufacturing process, unintended impurities may inevitably be introduced from the raw materials or the surrounding environment, and therefore cannot be eliminated. Since such impurities are easily recognizable to any technician in the normal manufacturing process, their details are not specifically mentioned herein.
[0028] In addition to limiting the content of each alloying element under the conditions described above, the stainless steel of the present invention can be further limited as follows. The ASP (Austenitic Stability Parameter) value expressed by formula (1) may be between 10 and 25. (1)551-462*([C]+[N])-9.2*[Si]-8.1*[Mn]-13.7*[Cr]-29*([Ni]+[Cu])-18.5*[Mo]-68*([Nb]+[V]) In equation (1), [C], [N], [Si], [Mn], [Cr], [Ni], [Cu], [Mo], [Nb], and [V] represent the weight percentage of each element. Elements that are not added are derived by substituting 0 weight% into equation (1). Equation (1) represents the temperature at which 50% of austenite transforms into martensite when stainless steel is deformed at a true strain of 0.3, and is used as an indicator of the degree of austenite phase stabilization. A lower value of Equation (1) indicates a higher degree of austenite phase stabilization, and a smaller amount of processed organic martensite is transformed during deformation. If the value of equation (1) is less than 10, the amount of TRIP transformation from the austenite phase to the martensite phase due to cold rolling is low, resulting in a low fraction of martensite in the cold-rolled material and a high fraction of retained austenite. As the amount of processed organic martensite decreases, the proportion that becomes the reverted austenite phase due to low-temperature annealing decreases, and the fraction of retained austenite that does not transform into martensite is high, making it difficult to secure ultrafine grains. If the value of equation (1) exceeds 25, the TRIP transformation due to cold rolling is activated, but there is a problem in that the excessively fast TRIP transformation rate results in a low elongation value.
[0029] The value of equation (2) may be 435 or greater. (2)(1600*[N])+(700 / )+(4*ASP)-(20*[Ni])+100 In equation (2), [N] and [Ni] represent the weight percentage of each element. ASP represents the ASP value in equation (1). d represents the average grain size at thicknesses from 1 / 4t to 3 / 4t, where t is the total thickness of the steel. In this invention, t may be 0.4 to 2.0 mm. Structural components often use materials with a thickness of 0.4 to 2.0 mm, and according to the present invention, it is possible to provide austenitic stainless steel having high strength and high ductility within this thickness range. In one example of the present invention, d may be 5 μm or less. If d exceeds 5 μm, the Hall-Petch equation indicates a low yield strength, which causes a lower YS*El value. Equation (2) is a parameter for ensuring high strength, taking into account factors that affect strength, such as N, Ni content, grain size, and the degree of austenite phase stabilization. If the value of Equation (2) is less than 435, it becomes impossible to ensure sufficient high strength.
[0030] The value of equation (3) may be 6000 or greater. (3) YS*EL-500*([Ni]+[Cr]) In equation (3), YS represents the yield strength (MPa), EL represents the elongation (%), and [Ni] and [Cr] represent the weight percentage of each element. The YS*EL value in equation (3) is heavily influenced by the Cr and Ni content. For example, when the Cr and Ni content is low, TRIP transformation occurs easily, and there is a tendency for the YS*EL value to be high. If the value of equation (3) is less than 6000, there is a problem in that high strength and high ductility cannot be satisfied simultaneously.
[0031] The value of equation (4) may be 200 or greater. (4) Hv-([Ni]+[Cr]) In equation (4), Hv represents the Vickers hardness (Hv), and [Ni] and [Cr] represent the weight percentage of each element. The Hv value in equation (4) is more influenced by the Cr and Ni content. For example, if the Cr and Ni content is low, TRIP transformation occurs easily, which increases the amount of transformation of the processed organic martensite during cold deformation. As a result, the hardness of the steel increases. If the value of equation (4) is less than 200, there is a problem in that sufficient hardness cannot be ensured.
[0032] The austenitic stainless steel according to the present invention not only satisfies high strength and high ductility simultaneously, but also exhibits excellent corrosion resistance. An example of austenitic stainless steel may have a formal potential value of 250 mV or higher, measured by immersion in a 3.5% NaCl solution at 30°C. An example of the present invention may be an austenitic stainless steel having a tensile strength of 1750 MPa or more after temper rolling. An example of a method for producing austenitic stainless steel according to the present invention may include the steps of hot-rolling a slab containing, by weight %, C: 0.005-0.03%, Si: 0.1-1%, Mn: 0.1-2%, Ni: 6-9%, Cr: 16-19%, N: 0.2% or less, with the remainder being Fe and unavoidable impurities, followed by cold-rolling at room temperature with a reduction ratio of 40% or more, and annealing at 700-850°C. If the reduction ratio during cold rolling is less than 40%, the amount of TRIP transformation in the austenitic stainless steel of the present invention having an ASP range of 10 to 25 is excessively low, resulting in a low martensite fraction in the cold-rolled material and a high fraction of retained austenite phase. As the amount of processed organic martensite decreases, the proportion that becomes the reverse-transformed austenite phase through subsequent low-temperature annealing decreases, and the fraction of retained austenite phase that does not transform into martensite remains high, making it difficult to secure ultrafine grains.
[0033] According to the present invention, a hot-rolled material can be cold-rolled and then annealed at a low temperature of 700 to 850°C. If the low-temperature annealing temperature is below 700°C, there is a problem that recrystallization from the processed organic martensite phase to the reverse-transformed austenite phase does not occur. On the other hand, if the low-temperature annealing temperature exceeds 850°C, the grain size of the reverse-transformed austenite becomes coarser, which may lead to a decrease in yield strength. According to one example of the present invention, after hot rolling, cold rolling can be performed without annealing. Furthermore, the manufacturing process may include a step of temper rolling at a reduction ratio of 60% or more in order to further increase the strength following the manufacturing stage described above.
[0034] The present invention will be described more specifically below through examples. However, it should be noted that the following examples are merely illustrative and intended to explain the present invention in more detail, and are not intended to limit the scope of the rights of the present invention. This is because the scope of the rights of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom. <Examples> Slabs having the components shown in Table 1 were hot-rolled and then cold-rolled at room temperature with a total reduction ratio of 40% or more, without annealing. Subsequently, they were annealed at 700-850°C to produce cold-rolled and annealed materials with a thickness of 0.4-2.0 mm.
[0035] In Table 1, ASP is a value derived by substituting the alloy composition in Table 1 into equation (1) below, which indicates the degree of austenite phase stabilization. (1)551-462*([C]+[N])-9.2*[Si]-8.1*[Mn]-13.7*[Cr]-29*([Ni]+[Cu])-18.5*[Mo]-68*([Nb]+[V]) In equation (1), [C], [N], [Si], [Mn], [Cr], [Ni], [Cu], [Mo], [Nb], and [V] represent the weight percentage of each element.
[0036] [Table 1]
[0037] In Table 2, 'd' represents the average grain size (μm) for thicknesses from 1 / 4t to 3 / 4t, where t is the total thickness of the cold-rolled and annealed material in Table 1. Equation (2) in Table 2 represents the value derived by the following equation (2). (2)(1600*[N])+(700 / )+(4*ASP)-(20*[Ni])+100 The value in equation (2) was derived by substituting the weight percentages of [N] and [Ni] from Table 1, the ASP value, and the d value from Table 2. Equation (3) in Table 2 represents the value derived from equation (3) below. (3) YS*EL-500*([Ni]+[Cr])
[0038] The value in equation (3) was derived by substituting the yield strength (YS, MPa) and elongation (EL, %) measured under the conditions described below, along with the weight percentages of [Ni] and [Cr] from Table 1. Yield strength (YS, MPa) and elongation (EL, %) were measured after tensile testing of the manufactured cold-rolled and annealed material using test specimens according to JIS 13B standard at room temperature with a crosshead range of 10 mm / min to 20 mm / min. Equation (4) in Table 2 represents the value derived from equation (4) below. (4) Hv-([Ni]+[Cr]) The value of equation (4) above was derived by substituting the Vickers hardness (Hv) measured under the conditions described later, and the weight percent of [Ni] and [Cr] from Table 1. Vickers hardness (Hv) is a value measured using a Vickers hardness tester with a load of 2 kgf. The official potentials (mV) in Table 2 were measured by immersing cold-rolled and annealed material in a 3.5% NaCl solution at 30°C.
[0039] [Table 2]
[0040] As shown in Tables 1 and 2, Invention Examples 1 to 8 satisfied the requirements of an ASP value of 10 to 25, a d value of 5 μm or less, a value of 435 or more in formula (2), and a value of 6000 or more in formula (3), thereby ensuring high strength, high ductility, and excellent corrosion resistance. Furthermore, as shown in Table 2, the value of formula (4) for Invention Examples 1 to 8 was 200 or more, and the official potential was 250 mV or more. Comparative Examples 6 to 18 fell outside the range of ASP values limited by the present invention. Comparative Examples 6 to 13 and 18, whose ASP values exceeded 25, showed low elongation due to an excessively fast TRIP transformation rate during molding. Comparative Examples 14 to 17, whose ASP values were less than 10, could not secure ultrafine grains due to a high fraction of the retained austenite phase. Comparative Examples 1-5, 7, 10, and 13-17 showed coarse grain formation outside the d-value range defined by the present invention. As a result, they failed to simultaneously satisfy high strength and high ductility. Comparative Examples 3-5 and 13-17 did not satisfy the range of values of formula (2) limited by the present invention. As a result, they did not simultaneously satisfy high strength and high ductility. Comparative Examples 2, 5-17 did not satisfy the range of values of formula (3) limited by the present invention. As a result, they did not simultaneously satisfy high strength and high ductility. Comparative Examples 1, 3-5, 7, 10, 12, and 14-17 did not satisfy the range of values of formula (4) limited by the present invention. As a result, sufficient hardness was not achieved. Comparative Example 18 contained a large amount of Mn, resulting in reduced corrosion resistance, and its official potential was low at 30 mV.
[0041] Figure 1 shows the range of the inventive examples and comparative examples based on the values of formula (2) and formula (3). Referring to Figure 1, it can be confirmed that all inventive examples are included within the range of values of formula (2) and formula (3) that the present invention limits, and that austenitic stainless steel that simultaneously satisfies high strength and high ductility properties can be provided within this range. On the other hand, in the case of the comparative examples, the range of values of formula (2) and / or the range of values of formula (3) are not satisfied, and in this case, it is difficult to simultaneously satisfy high strength and high ductility properties. Figures 2(a) to 2(c) are diagrams for comparing the average grain size d of the inventive example and the comparative example. Figures 2(a) and 2(b) are drawings according to the present invention, and Figure 2(c) is a drawing according to the comparative example. Comparing Figures 2(a), 2(b), and 2(c), it can be confirmed that the austenitic stainless steel according to the present invention has an ultrafine grain with a d value of 5 μm or less. Figures 3(a) to 3(c) are graphs showing the Strain (%)-Stress (MPa) curves of the inventive example. Figures 4(a) to 4(c) show the Strain (%)-Stress (MPa) curves of the comparative example.
[0042] Although exemplary embodiments of the present invention have been described above, the present invention is not limited thereto, and a person with ordinary skill in the art should understand that various modifications and variations are possible without departing from the concepts and scope of the claims described below. [Industrial applicability]
[0043] The austenitic stainless steel according to the present invention simultaneously satisfies high strength and high ductility, is economical due to the reduced content of expensive alloying elements Ni and Cr, and ensures excellent corrosion resistance. Therefore, it can be used as a material for a variety of applications, such as automotive body panels and building components.
Claims
1. In weight percent, it contains C: 0.005-0.03%, Si: 0.1-1%, Mn: 0.1-2%, Ni: 6-9%, Cr: 16-19%, N: 0.2% or less, with the remainder being Fe and unavoidable impurities. An austenitic stainless steel characterized in that, when the total thickness of the steel material is t, the average grain size d value is 5 μm or less for thicknesses from 1 / 4 t to 3 / 4 t, the ASP value expressed by formula (1) is 10 to 25, the value of formula (2) is 435 or more, and the value of formula (3) is 6000 or more. (1) 551-462*([C]+[N])-9.2*[Si]-8.1*[Mn]-13.7*[Cr]-29*([Ni]+[Cu])-18.5*[Mo]-68*([Nb]+[V]) (2) (1600*[N])+(700 / )+(4*ASP)-(20*[Ni])+100 (3) YS*EL-500*([Ni]+[Cr]) (In formulas (1), (2), and (3), [C], [N], [Si], [Mn], [Cr], [Ni], [Cu], [Mo], [Nb], and [V] represent the weight percentage of each element, YS represents the yield strength (MPa), and EL represents the elongation rate (%).)
2. The austenitic stainless steel according to claim 1, characterized in that the value of formula (4) is 200 or more. (4) Hv-([Ni]+[Cr]) (In equation (4), Hv represents the Vickers hardness (Hv), and [Ni] and [Cr] represent the weight percentage of each element.)
3. The austenitic stainless steel according to claim 1, further comprising one or more of the following in weight percent: Cu: 0.4% or less, Mo: 0.2% or less, Nb: 0.25% or less, and V: 0.25% or less.
4. The austenitic stainless steel according to claim 1, characterized in that t is 0.4 to 2.0 mm.
5. The austenitic stainless steel according to claim 1, characterized in that the official potential value measured by immersion in a 3.5% NaCl solution at 30°C is 250 mV or higher.
6. A method for producing austenitic stainless steel according to claim 1, The process involves hot-rolling a slab containing, by weight percent, C: 0.005-0.03%, Si: 0.1-1%, Mn: 0.1-2%, Ni: 6-9%, Cr: 16-19%, N: 0.2% or less, with the remainder being Fe and unavoidable impurities, followed by cold-rolling at room temperature to a reduction ratio of 40% or more, and A method for producing austenitic stainless steel, characterized by including a step of annealing at 700 to 850°C.
7. A method for producing austenitic stainless steel according to claim 6, characterized by performing hot rolling followed by cold rolling without annealing.
8. The method for producing austenitic stainless steel according to claim 6, further comprising the step of temper rolling with a reduction ratio of 60% or more.