Catalytic system for treating exhaust gases from an internal combustion engine

JP2023543607A5Inactive Publication Date: 2024-10-23BASF CORPORATON
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023519842
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-09-30
Filing Date
2021-09-29
Publication Date
2024-10-23
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing systems for treating exhaust gases from diesel internal combustion engines struggle to effectively reduce NOx emissions, particularly during cold start periods when temperatures are low, and fail to adequately address the adsorption and conversion of NOx, CO, and total hydrocarbons (THC).

Method used

A system comprising a NOx adsorbent component, diesel oxidation catalyst (DOC) component, selective catalytic reduction (SCR) component, and a gas heating component, arranged in a specific order within the exhaust gas flow, where the NOx adsorbent is upstream of the gas heating component, and the reductant injector is upstream of the SCR component, with the DOC component and gas heating component in direct succession, utilizing specific catalyst materials and coatings to enhance NOx adsorption and conversion.

Benefits of technology

The system significantly reduces NOx emissions, especially during cold start periods, achieving low NOx, CO, and THC emissions when tested under the World Harmonized Fuel Economy and Emissions Test Cycle (WLTC) and in urban areas, demonstrating improved catalytic activity and performance compared to prior art systems.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a system for treating the exhaust gases of a diesel internal combustion engine, the system comprising a specific NOx adsorbent component, a diesel oxidation catalyst (DOC) component, a selective catalytic reduction (SCR) component, a gas heating component, and a reductant injector, wherein the specific NOx adsorbent component is located upstream of the gas heating component, the reductant injector is located upstream of the SCR component, the gas heating component is located upstream of the reductant injector, and the DOC component is located upstream of the reductant injector, with the DOC component and the gas heating component in direct series. Furthermore, the present invention relates to a method for preparing such a system and its use.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a system for treating exhaust gas from a diesel internal combustion engine, a method for preparing such a system, a method for treating exhaust gas from a diesel internal combustion engine using the system, and the use of the system. [Background technology]

[0002] In the automotive industry, there is a continuous need to reduce engine NOx emissions because NOx emitted from engines is harmful. Therefore, there is interest in avoiding NOx emissions and addressing current regulations. In particular, removing NOx emissions immediately after the cold start period is difficult because the temperature required for NOx conversion in catalytic systems is typically relatively low.

[0003] DE102018101929 discloses a system for reducing cold start emissions that includes a first selective catalytic reduction (SCR) catalytic converter which may contain a NOx adsorbent, a heating element located downstream of the first SCR catalytic converter, and a second SCR catalytic converter located downstream of the heating element. US2017 / 0284250A1 discloses a system that includes a NOx storage catalyst located upstream of the heating element and an SCR catalyst located downstream of the heating element. Furthermore, US10480369B1 discloses a system that includes an electric heating element downstream of the engine, a diesel oxidation catalyst (DOC) which can be combined with a NOx adsorbent or diesel particulate filter located downstream of the electric heating element, and a selective catalytic reduction catalyst (SCRoF) on the filter located downstream of the DOC. WO2019 / 077111A1 relates to an exhaust gas purification system comprising a catalyst and a first SCR catalyst, the catalyst comprising a carrier substrate of length L, a passive nitrogen oxide adsorbent, and means for controlling the temperature of the carrier substrate, wherein the carrier substrate can support an oxidation catalyst in addition to the passive nitrogen oxide adsorbent. [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] -DE102018101929 [Patent Document 2] -US2017 / 0284250A1 [Patent Document 3] -US10480369B1 [Overview of the project] [Problems that the invention aims to solve]

[0005] The object of the present invention is to provide a system that can significantly reduce overall NOx emissions. In particular, the object of the present invention is to improve NOx adsorption and / or conversion of the system, especially during the cold start period, i.e., at temperatures below 300°C, thereby significantly reducing overall NOx emissions. Furthermore, the object of the present invention is to ensure NOx adsorption during the subsequent cold start. Therefore, the object of the present invention is to provide a system that exhibits a low NOx desorption temperature, in particular a low NOx desorption temperature for conditions after a cold start where downstream SCR conversion is high. It is also an object of the present invention to provide a system that adsorbs NOx during a cold start when downstream SCR conversion is low.

[0006] Therefore, surprisingly, it has been found that a system for treating exhaust gases from a diesel internal combustion engine can solve the above problems, particularly with respect to improving performance in adsorption and / or conversion of one or more of NOx, CO, and total hydrocarbons (THC), wherein the system particularly includes a specific NOx adsorbent component, a diesel oxidation catalyst (DOC) component, a selective catalytic reduction (SCR) component, and a gas heating component, wherein the components are particularly arranged in a specific order with respect to the direction of the exhaust gas flow.

[0007] Remarkably, the system of the present invention thus enables improved catalytic activity. Furthermore, the system of the present invention exhibits excellent behavior with respect to NOx emission and NOx adsorption, particularly during cold start periods, and especially when tested in the World Harmonized Fuel Economy and Exhaust Gas Test Cycle (WLTC) for passenger cars and the like. Accordingly, the system of the present invention exhibits relatively low NOx emissions compared to prior art systems, and particularly low NOx emissions after short periods of driving. Moreover, surprisingly, it has been found that systems using an electrically heated element, particularly between the NA catalyst and the DOC, can achieve relatively low NOx, CO, and THC emissions. In particular, when tested in the WLTC, surprisingly, the system of the present invention has been found to achieve relatively low emissions in both the WLTC overall and the WLTC urban section. [Means for solving the problem]

[0008] Exhaust gas treatment system Accordingly, the present invention relates to a system for treating exhaust gas of a diesel internal combustion engine, the system comprising a NOx adsorbent component, a diesel oxidation catalyst (DOC) component, a selective catalytic reduction (SCR) component, a gas heating component, and a reducing agent injector, wherein the NOx adsorbent component is located upstream of the gas heating component, the reducing agent injector is located upstream of the SCR component, the gas heating component is located upstream of the reducing agent injector, the DOC component is located upstream of the reducing agent injector, and the DOC component and the gas heating component are in a direct continuous configuration. The aforementioned NOx adsorbent component is (i) A catalyst, (i.1) A first substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the first substrate, and the inner wall of the first substrate extending therethrough; (i.2) NOx adsorbent coating which is the NOx adsorbent component, wherein the coating is disposed on the surface of the inner wall of the first substrate over at least 50% of the substrate axial length of the first substrate, and the NOx adsorbent coating comprises a platinum group metal component and a 10-membered ring-pore zeolite material having a framework type selected from the group consisting of FER, TON, MTT, SZR, MWW, AEL, HEU, AFO, two or more mixtures thereof and two or more mixed types thereof, It is included in catalysts that contain [this substance].

[0009] Preferably, no other components for treating the exhaust gas are placed between the DOC component and the gas heating component.

[0010] Preferably, the components are arranged in a conduit for exhaust gases, preferably in a continuous sequence, and the upstream end of the conduit is preferably located downstream of the diesel internal combustion engine, and more preferably, the upstream end of the conduit is located downstream of the diesel internal combustion engine.

[0011] Preferably, the reducing agent injector comprises one or more of a hydrocarbon injector, a hydrocarbon cylinder post-injector, and a urea injector, preferably a urea injector, and preferably consists of one or more of a hydrocarbon injector, a hydrocarbon cylinder post-injector, and a urea injector, preferably a urea injector, and the reducing agent injector is preferably positioned downstream of the DOC component. First alternative arrangement Preferably, the DOC component is placed upstream of the gas heating component, and preferably, the DOC component and the NOx adsorbent component are placed upstream of the gas heating component.

[0012] Preferably, the catalyst according to (i.3) (i) has a diesel oxidation catalyst (DOC) coating which is the DOC component, the DOC coating is at least partially placed on the NOx adsorbent coating over at least 70% of the substrate axial length of the first substrate, the DOC coating comprises a platinum group metal component and a non-zeolite oxide material which comprises one or more alumina, silica, zirconia and titania, and the DOC coating is preferably placed from the outlet end to the inlet end of the first substrate.

[0013] Preferably, the NOx adsorbent coating according to (i.2) is placed on the surface of the inner wall of the first substrate over 70-100%, preferably 80-100%, more preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the first substrate, and the first NOx adsorbent coating according to (i.2) is preferably placed on the surface of the inner wall of the first substrate from the inlet end to the outlet end of the first substrate.

[0014] Preferably, the platinum group metal component of the NOx adsorbent coating according to (i.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the platinum group metal component more preferably comprises palladium, and more preferably palladium, where the first NOx adsorbent coating according to (i.2) comprises a platinum group metal component, preferably calculated as a Pd element, preferably palladium, in a concentration of 30 to 300 g / ft 3 The range is more preferably 45-200 g / ft 3 A comfortable range of 60-150 g / ft 3 A comfortable range of 60-100 g / ft 3 range or 100-150g / ft 3 In the range of 60-80 g / ft, more preferably 60-80 g / ft 3 The range is 100-140g / ft 3 Includes filling amounts within the range.

[0015] Preferably, the platinum group metal component of the NOx adsorbent coating according to (i.2) is contained in the 10-membered ring-pore zeolite material of the NOx adsorbent coating according to (i.2), where the platinum group metal component is preferably present in the zeolite material in an amount ranging from 0.5 to 10% by mass, more preferably from 1 to 6% by mass, more preferably from 1.25 to 4% by mass, and more preferably from 1.5 to 3% by mass, based on the total mass of the 10-membered ring-pore zeolite material of the NOx adsorbent coating according to (i.2).

[0016] Preferably, the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (i.2) has a framework type selected from the group consisting of FER, TON, mixtures thereof, and mixed forms thereof, more preferably the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (i.2) has a framework type FER, where the framework structure of the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (i.2) preferably comprises a tetravalent element Y, a trivalent element X, and oxygen, more preferably a tetravalent element It consists of element Y, a trivalent element X, and oxygen, where Y is preferably one or more of Si, Sn, Ti, Zr, and Ge, more preferably Si, and X is preferably one or more of Al, B, In, and Ga, more preferably Al, and the molar ratio of Y:X calculated as YO2:X2O3 is preferably in the range of 2:1 to 100:1, more preferably in the range of 10:1 to 55:1, more preferably in the range of 12:1 to 40:1, more preferably in the range of 15:1 to 28:1, and more preferably in the range of 18:1 to 25:1.

[0017] Preferably, the NOx adsorbent coating according to (i.2) contains a 10-membered ring-pore zeolite material in an amount ranging from 80 to 99.75% by mass, preferably 85 to 99.5% by mass, more preferably 90 to 99.25% by mass, and more preferably 95 to 99% by mass, based on the mass of the NOx adsorbent coating.

[0018] Preferably, the catalyst according to (i) has a filling amount in the range of 0.5 to 8 g / in 3 Preferably in the range of 1 to 5 g / in 3 More preferably in the range of 1.5 to 4.5 g / in 3 More preferably in the range of 2 to 4 g / in 3 and includes the NOx adsorbent coating according to (i.2) with a filling amount in the range thereof.

[0019] Preferably, 95 to 100% by mass, preferably 98 to 100% by mass, more preferably 99 to 100% by mass, and more preferably 99.5 to 100% by mass of the NOx adsorbent coating according to (i.2) consists of a platinum group metal component and a 10-membered ring pore zeolite material.

[0020] Preferably, the DOC coating according to (i.3) is at least partially disposed on the NOx adsorbent coating according to (i.2), extends over 80 to 100% of the substrate axial length of the first substrate, preferably 95 to 100%, more preferably 98 to 100%, and more preferably 99 to 100%, and the DOC according to (i.3) is preferably at least partially disposed on the NOx adsorbent coating according to (i.2) from the inlet end to the outlet end of the first substrate.

[0021] Preferably, the platinum group metal component of the DOC coating according to (i.3) includes one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, more preferably includes platinum, and more preferably is platinum. Here, the DOC coating according to (i.3) includes the platinum group metal component, preferably platinum calculated as elemental Pt as the platinum group metal element, preferably platinum, preferably in the range of 15 to 200 g / ft 3 More preferably in the range of 20 to 150 g / ft 3 More preferably in the range of 30 to 100 g / ft 3 More preferably in the range of 40 to 90 g / ft 3 More preferably in the range of 50 to 80 g / ft 3 and includes it with a filling amount in the range thereof. Here, the platinum group metal component of the DOC coating according to (i.3) more preferably includes platinum and palladium, and the mass ratio of platinum to palladium, Pt:Pd, calculated as elements, is more preferably in the range of 1:1 to 11:1, more preferably in the range of 2:1 to 10:1, more preferably in the range of 3:1 to 5:1, and the mass ratio is more preferably about 4:1. Here, the platinum group metal components of the DOC coating according to (i.3) are more preferably calculated as elements or components based on the total mass of the non-zeolite oxide material according to (i.3) and supported on the non-zeolite oxide material according to (i.3) in a packing amount more preferably in the range of 1 to 5 mass%, more preferably in the range of 2 to 4 mass%.

[0022] Preferably, the non-zeolite oxide material of the DOC coating according to (i.3) comprises one or more of alumina, silica, and zirconia, preferably one or more of alumina and silica, more preferably alumina, more preferably gamma-alumina, the non-zeolite oxide material preferably further comprises one or more of manganese, silicon, and zirconium, the non-zeolite oxide material more preferably comprises alumina and manganese, the non-zeolite oxide material of the DOC coating according to (i.3) more preferably comprises alumina in an amount in the range of 80-99% by mass, more preferably 85-98% by mass, and more preferably 90-97% by mass, based on the mass of the non-zeolite oxide material, the non-zeolite oxide material of the DOC coating according to (i.3) more preferably 75m 2 More than / g, more preferably 100m 2 The non-zeolite oxide material exhibiting a BET specific surface area greater than / g and DOC coating according to (i.3) is more preferably 0.04 cm². 3 More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g.

[0023] Preferably, the DOC coating according to (i.3) further comprises a zeolite material, preferably a 12-membered ring-pore zeolite material, the 12-membered ring-pore zeolite material preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type BEA for the 12-membered ring-pore zeolite material, the framework structure of the zeolite material preferably comprises Si, Al, and O, more preferably consisting of Si, Al, and O, the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1. The zeolite material contains, preferably at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, copper calculated as CuO.

[0024] Preferably, the zeolite material contains iron calculated as Fe2O3 in an amount of at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass; or the zeolite material contains iron calculated as Fe2O3 in an amount preferably in the range of 0.5 to 8% by mass, and more preferably in the range of 1 to 5% by mass.

[0025] Preferably, the mass ratio of the non-zeolite oxide material in the DOC coating by (i.3) to the zeolite material in the DOC coating by (i.3) is in the range of 1:1 to 10:1, preferably in the range of 1.5:1 to 8:1, and more preferably in the range of 2:1 to 4.5:1.

[0026] Preferably, the catalyst according to (i) is coated with DOC according to (i.3) at a rate of 0.5 to 5 g / in 3 The range is preferably 0.75 to 4 g / in.3 In the range of 1-3 g / in, more preferably 1-3 g / in 3 The range, more preferably 1.25 to 2.5 g / in 3 Includes filling amounts within the range.

[0027] Preferably, 95-100% by mass, preferably 98-100% by mass, more preferably 99-100% by mass, and more preferably 99.5-100% by mass of the DOC coating according to (i.3) consist of platinum group metal components, the non-zeolite oxide material of the DOC coating according to (i.3) preferably comprises one or more of alumina, silica, and zirconia, preferably one or more of alumina and silica, more preferably alumina, and more preferably gamma-alumina, the non-zeolite oxide material further preferably comprises one or more of manganese, silicon, and zirconium, and the non-zeolite oxide material more preferably comprises alumina and manganese, where the non-zeolite oxide material of the DOC coating according to (i.3) more preferably contains alumina in an amount in the range of 80-99% by mass, more preferably 85-98% by mass, and more preferably 90-97% by mass, based on the mass of the non-zeolite oxide material, and the non-zeolite oxide material of the DOC coating according to (i.3) more preferably comprises 75m 2 More than / g, more preferably 100m 2 The non-zeolite oxide material exhibiting a BET specific surface area greater than / g and DOC coating according to (i.3) is more preferably 0.04 cm². 3 More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g, The zeolite material is preferably a 12-membered ring-pore zeolite material, which preferably has a framework type selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed types thereof, more preferably a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed types thereof, and more preferably a framework type BEA for the 12-membered ring-pore zeolite material, which preferably has a framework type BEA, and the framework structure of the zeolite material preferably contains Si, Al, and O, more preferably consists of Si, Al, and O, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1. The ratio is preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1, and the zeolite material contains copper calculated as CuO, preferably at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, and the zeolite material contains iron calculated as Fe2O3, preferably at most 0.001% by mass, more preferably 0 to 0.0001% by mass, or the zeolite material contains iron calculated as Fe2O3 in an amount preferably in the range of 0.5 to 8% by mass, more preferably in the range of 1 to 5% by mass.

[0028] Preferably, the first substrate according to (i.1) is a flow-through substrate or a wall-flow filter substrate, preferably a flow-through substrate, the flow-through substrate preferably one or more of cordierite flow-through substrates and metal flow-through substrates, more preferably a metal flow-through substrate, the first substrate is preferably cylindrical, the diameter of the first substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and the first substrate has an axial length preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches.

[0029] Preferably, the catalyst according to (i) consists of (i.1), (i.2), and (i.3). Gas heating component Preferably, (ii) the gas heating component is (ii.1) A second substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the second substrate, and the inner wall of the second substrate extending therethrough; Here, the inlet end of the second substrate according to (ii.1) and the outlet end of the first substrate according to (i.1) are coupled so that the exhaust gas exiting the passage of the first substrate enters the passage of the second substrate; The inner wall of the second substrate is thermally conductive to allow heating in order to heat the exhaust gas flowing through the passage of the second substrate.

[0030] Preferably, the second substrate according to (ii.1) is a flow-through substrate, preferably a metal flow-through substrate, and more preferably a metal electrically and / or thermally conductive flow-through substrate.

[0031] Preferably, the second substrate according to (ii.1) is cylindrical in shape, and the diameter of the second substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, more preferably the diameter of the second substrate is in the range of 90 to 110% of the diameter of the first substrate, preferably in the range of 95 to 105%, more preferably in the range of 98 to 102%, the diameter of the first substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, the first substrate has an axial length preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and the second substrate according to (ii.1) has an axial length preferably in the range of 0.15 to 2 inches, more preferably in the range of 0.20 to 1.5 inches, more preferably in the range of 0.30 to 1 inch.

[0032] Preferably, the gas heating component according to (ii) consists of a second substrate according to (ii.1), the substrate being an uncoated substrate.

[0033] Preferably, the gas heating component according to (ii) is (ii.2) Optionally, a NOx adsorbent coating disposed on the surface of the inner wall of the second substrate over at least 50% of the substrate axial length of the second substrate, wherein the NOx adsorbent coating comprises a platinum group metal component and a 10-membered ring-pore zeolite material having a framework type selected from the group consisting of FER, TON, MTT, SZR, MWW, AEL, HEU, AFO, two or more mixtures thereof and two or more mixed types thereof, (ii.3) A diesel oxidation catalyst (DOC) coating that is at least partially disposed on the surface of the inner wall of the second substrate and / or at least partially disposed on any NOx adsorbent coating according to (ii.2), and extending over at least 70% of the substrate axis length of the second substrate, wherein the DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania, It also includes.

[0034] Preferably, the NOx adsorbent coating according to (ii.2) is applied to the surface of the inner wall of the second substrate over an area of ​​70-100%, preferably 80-100%, more preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the second substrate. The NOx adsorbent coating according to (ii.2) is preferably placed on the surface of the inner wall of the second substrate from the exit end to the entrance end of the second substrate.

[0035] Preferably, the platinum group metal component of the NOx adsorbent coating according to (ii.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the platinum group metal component more preferably comprises palladium, and more preferably palladium, where the NOx adsorbent coating according to (ii.2) comprises a platinum group metal component calculated as a platinum group metal element, preferably as a Pd element, preferably palladium, preferably in a quantity of 30 to 300 g / ft 3 The range is more preferably 45-200 g / ft 3 A comfortable range of 60-150 g / ft 3 A comfortable range of 60-100 g / ft 3 range or 100-150g / ft 3 In the range of 60-80 g / ft, more preferably 60-80 g / ft 3 The range is 100-140g / ft 3 Includes filling amounts within the range.

[0036] Preferably, the platinum group metal component of the NOx adsorbent coating according to (ii.2) is contained in the 10-membered ring-pore zeolite material of the NOx adsorbent coating according to (ii.2), where the platinum group metal component is preferably present in the zeolite material in an amount ranging from 0.5 to 10% by mass, more preferably from 1 to 6% by mass, more preferably from 1.25 to 4% by mass, and more preferably from 1.5 to 3% by mass, based on the total mass of the 10-membered ring-pore zeolite material of the NOx adsorbent coating according to (ii.2).

[0037] Preferably, the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (ii.2) has a framework type selected from the group consisting of FER, TON, mixtures thereof, and mixed forms thereof, and more preferably, the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (ii.2) has a framework type FER, where the framework structure of the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (ii.2) preferably comprises a tetravalent element Y, a trivalent element X, and oxygen, and more preferably a tetravalent element. It consists of element Y, a trivalent element X, and oxygen, where Y is preferably one or more of Si, Sn, Ti, Zr, and Ge, more preferably Si, and X is preferably one or more of Al, B, In, and Ga, more preferably Al, and the molar ratio of Y:X calculated as YO2:X2O3 is preferably in the range of 2:1 to 100:1, more preferably in the range of 10:1 to 55:1, more preferably in the range of 12:1 to 40:1, more preferably in the range of 15:1 to 28:1, and more preferably in the range of 18:1 to 25:1.

[0038] Preferably, the NOx adsorbent coating according to (ii.2) contains a 10-membered ring-pore zeolite material in an amount based on the mass of the NOx adsorbent coating according to (ii.2), preferably in the range of 80 to 99.75% by mass, more preferably in the range of 85 to 99.5% by mass, more preferably in the range of 90 to 99.25% by mass, and more preferably in the range of 95 to 99% by mass.

[0039] Preferably, the gas heating component according to (ii) is preferably 0.5 to 8 g / in 3 The range is more preferably 1-5 g / in 3 The range is, more preferably 1.5 to 4.5 g / in 3 In the range of 2-4 g / in 3 The filling amount includes a NOx adsorbent coating according to (ii.2) within the range of [specified range].

[0040] Preferably, 95 to 100% by mass, more preferably 98 to 100% by mass, more preferably 99 to 100% by mass, and more preferably 99.5 to 100% by mass of the NOx adsorbent coating according to (ii.2) consist of a platinum group metal component and a 10-membered ring pore zeolite material.

[0041] Preferably, the DOC coating according to (ii.3) is at least partially distributed on the inner wall surface of the second substrate and / or at least partially distributed on the NOx adsorbent coating according to (ii.2), extending over 80-100%, preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axial length of the first substrate, and the DOC according to (ii.3) is preferably at least partially distributed on the inner wall surface of the second substrate and / or at least partially distributed on any NOx adsorbent coating according to (ii.2) from the inlet end to the outlet end of the first substrate.

[0042] Preferably, the platinum group metal component of the DOC coating according to (ii.3) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, the platinum group metal component more preferably comprises platinum, and more preferably is platinum, and the DOC coating according to (ii.3) comprises a platinum group metal component, preferably calculated as element Pt, preferably platinum, in a quantity of 15 to 200 g / ft 3 A comfortable range is 20-150 g / ft 3 Comfortably within the range of 30-100g / ft 3 In the range of 40-90 g / ft, more preferably 40-90 g / ft 3 In the range of 50-80 g / ft, more preferably 50-80 g / ft 3The platinum group metal components of the DOC coating according to (ii.3) are more preferably calculated as elements based on the total mass of the non-zeolite oxide material according to (ii.3) and supported on the non-zeolite oxide material according to (ii.3) in a packing amount more preferably in the range of 1 to 5 mass%, more preferably in the range of 2 to 4 mass%.

[0043] Preferably, the platinum group metal component of the DOC coating according to (ii.3) includes platinum and palladium, where the mass ratio of platinum to palladium, Pt:Pd, calculated as elements, is more preferably in the range of 1:1 to 11:1, more preferably in the range of 2:1 to 10:1, more preferably in the range of 3:1 to 5:1, and the mass ratio is more preferably about 4:1.

[0044] Preferably, the non-zeolite oxide material of the DOC coating according to (ii.3) preferably comprises one or more of alumina, silica and zirconia, more preferably one or more of alumina and silica, more preferably alumina, more preferably gamma-alumina, the non-zeolite oxide material preferably further comprises one or more of manganese, silicon and zirconium, the non-zeolite oxide material more preferably comprises alumina and manganese, and the non-zeolite oxide material of the DOC coating according to (ii.3) more preferably comprises alumina in an amount in the range of 80 to 99% by mass, more preferably 85 to 98% by mass, and more preferably 90 to 97% by mass, based on the mass of the non-zeolite oxide material.

[0045] Preferably, the non-zeolite oxide material for the DOC coating according to (ii.3) is 75m 2 More than / g, more preferably 100m 2 The non-zeolite oxide material exhibiting a BET specific surface area greater than / g and DOC coating according to (ii.3) is more preferably 0.04 cm². 3 More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g.

[0046] Preferably, the DOC coating according to (ii.3) further comprises a zeolite material, more preferably a 12-membered ring-pore zeolite material, the 12-membered ring-pore zeolite material is preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type BEA for the 12-membered ring-pore zeolite material, the framework structure of the zeolite material preferably consists of Si, Al and O, more preferably Si, Al and O, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably The ratio is in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1, and the zeolite material contains copper calculated as CuO, preferably at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass; the zeolite material contains iron calculated as Fe2O3, preferably at most 0.001% by mass, more preferably 0 to 0.00001% by mass; or the zeolite material contains iron calculated as Fe2O3 in an amount preferably in the range of 0.5 to 8% by mass, more preferably in the range of 1 to 5% by mass.

[0047] Preferably, the mass ratio of the non-zeolite oxide material of the DOC coating according to (ii.3) to the zeolite material of the DOC coating according to (ii.3) is preferably in the range of 1:1 to 10:1, more preferably in the range of 1.5:1 to 8:1, and more preferably in the range of 2:1 to 4.5:1.

[0048] Preferably, the gas heating component according to (ii) is coated with DOC according to (ii.3), preferably 0.5 to 5 g / in 3 The range is, more preferably 0.75 to 4 g / in 3In the range of 1-3 g / in, more preferably 1-3 g / in 3 The range, more preferably 1.25 to 2.5 g / in 3 Includes filling amounts within the range.

[0049] Preferably, 95-100% by mass, more preferably 98-100% by mass, more preferably 99-100% by mass, and more preferably 99.5-100% by mass of the DOC coating according to (ii.3) consist of a platinum group metal component and a non-zeolite oxide material which preferably contains one or more of alumina, silica, and zirconia, preferably one or more of alumina and silica, more preferably alumina, and more preferably gamma-alumina, the non-zeolite oxide material which preferably further contains one or more of manganese, silicon, and zirconium, and the non-zeolite oxide material which more preferably contains alumina and manganese, where the non-zeolite oxide material which more preferably contains alumina in the range of 80-99% by mass, more preferably 85-98% by mass, and more preferably 90-97% by mass, based on the mass of the non-zeolite oxide material, and the non-zeolite oxide material which more preferably contains 75m 2 More than / g, more preferably 100m 2 The non-zeolite oxide material exhibits a BET specific surface area greater than / g, and more preferably 0.04 cm². 3 More than 0.06 cm² / g 3The zeolite material exhibits a pore volume exceeding / g, and is preferably a 12-membered ring pore zeolite material, which is preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed types thereof, more preferably has a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed types thereof, and more preferably the 12-membered ring pore zeolite material has a framework type BEA, and the framework structure of the zeolite material is preferred The zeolite material contains Si, Al, and O, more preferably Si, Al, and O, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1, and the zeolite material contains copper calculated as CuO, preferably at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass.

[0050] Preferably, the non-zeolite oxide material of the DOC coating according to (ii.3) comprises one or more of alumina, silica, and zirconia, preferably one or more of alumina and silica, more preferably alumina, more preferably gamma-alumina, the non-zeolite oxide material preferably further comprises one or more of manganese, silicon, and zirconium, the non-zeolite oxide material more preferably comprises alumina and manganese, the non-zeolite oxide material of the DOC coating according to (ii.3) more preferably comprises alumina in an amount in the range of 80-99% by mass, more preferably 85-98% by mass, and more preferably 90-97% by mass, based on the mass of the non-zeolite oxide material, and the non-zeolite oxide material of the DOC coating according to (ii.3) more preferably comprises 75m 2 More than / g, more preferably 100m 2The non-zeolite oxide material exhibiting a BET specific surface area greater than / g and DOC coating according to (ii.3) is more preferably 0.04 cm². 3 More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g, The zeolite material is preferably a 12-membered ring-pore zeolite material, which is preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed types thereof, and more preferably has a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed types thereof, and more preferably the 12-membered ring-pore zeolite material has a framework type BEA, and the framework structure of the zeolite material preferably contains Si, Al, and O, more preferably consists of Si, Al, and O, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1. The zeolite material preferably contains at least 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, copper calculated as CuO, and the zeolite material preferably contains at least 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, iron calculated as Fe2O3; or the zeolite material preferably contains iron calculated as Fe2O3 in an amount in the range of 0.5 to 8% by mass, and more preferably 1 to 5% by mass.

[0051] Preferably, the gas heating component according to (ii) consists of (ii.1), (ii.2), and (ii.3).

[0052] Preferably, the gas heating component according to (ii) consists of (ii.1) and (ii.3), and the gas heating component according to (ii) preferably consists of (ii.1), (ii.2), and (ii.3).

[0053] Preferably, the DOC coating according to (ii.3) exhibits essentially the same, preferably the same, chemical and physical properties as the DOC coating according to (i.3), and preferably the coating of the gas heating component according to (ii) exhibits essentially the same, preferably the same, chemical and physical properties as the coating of the catalyst according to (i).

[0054] Preferably, the exit end of the first substrate and the inlet end of the second substrate are arranged opposite each other, and the angle between the surface normal of the surface defined by the exit end of the first substrate and the surface normal of the surface defined by the inlet end of the second substrate is preferably in the range of 0 to 5°, more preferably in the range of 0 to 3°, and more preferably in the range of 0 to 1°.

[0055] Preferably, the exit end of the first substrate and the inlet end of the second substrate are spaced apart from each other by a distance of preferably 2 to 20 mm, preferably 5 to 15 mm, and more preferably 8 to 12 mm, and the exit end of the first substrate and the inlet end of the second substrate are spaced apart from each other preferably by one or more spacer means, preferably by one or more spacer rods, and the given spacer rod is preferably fixed to either the exit end of the first substrate, the inlet end of the second substrate, or the exit end of the first substrate and the inlet end of the second substrate, and the one or more spacer means, preferably one or more spacer rods, are preferably electrically insulating.

[0056] Preferably, the first and second substrates together form a single substrate including an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the single substrate, and a plurality of passages defined therethrough by the inner wall of the single substrate, the DOC coating according to (i.3) and the DOC coating according to (ii.3) together form a single DOC coating, the single DOC coating preferably at least partially disposed on the NOx adsorbent coating according to (i.2), and the single DOC coating preferably extends over at least 90%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the single substrate; Preferably, the first substrate and the second substrate together form a single substrate including an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the single substrate, and a plurality of passages defined therethrough by the inner wall of the single substrate; the NOx adsorbent coating by (i.2) and the NOx adsorbent coating by (ii.2) together form a single NOx adsorbent coating; and the DOC coating by (i.3) and the DOC coating by (ii.3) together form a single DOC coating; The single NOx adsorbent coating preferably extends over at least 50% of the substrate axial length of the single substrate, more preferably over 70% to 100%, more preferably over 80% to 100%, more preferably over 95% to 100%, more preferably over 98% to 100%, more preferably over 99% to 100%, and / or A single DOC coating is preferably at least partially placed on a single NOx adsorbent coating, and preferably extends over at least 90% of the substrate axial length of a single substrate, more preferably over 95-100%, more preferably over 98-100%, and more preferably over 99-100%.

[0057] Preferably, the system further includes a jacket surrounding a first substrate according to (i) and a second substrate according to (ii), wherein preferably 95-100%, more preferably 98-100%, more preferably 99-100% of the inlet end face of the first substrate and preferably 95-100%, more preferably 98-100%, more preferably 99-100% of the outlet end face of the second substrate are not covered by the jacket, where the jacket preferably includes one or more means for connecting the second substrate to a power source. Second alternative arrangement Preferably, the DOC component is located downstream of the gas heating component.

[0058] Preferably, the NOx adsorbent component is (i) A catalyst, (i.1) A first substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the first substrate, and the inner wall of the first substrate extending therethrough; (i.2) A NOx adsorbent coating disposed on the surface of the inner wall of the first substrate over at least 50% of the substrate shaft length of the first substrate, wherein the NOx adsorbent coating comprises a platinum group metal component and a 10-membered ring-pore zeolite material having a framework type selected from the group consisting of FER, TON, MTT, SZR, MWW, AEL, HEU, AFO, two or more mixtures thereof and two or more mixed types thereof, It is included in catalysts that contain [this ingredient].

[0059] Preferably, the NOx adsorbent coating according to (i.2) is placed on the surface of the inner wall of the first substrate over 70-100%, preferably 80-100%, more preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the first substrate, and the first NOx adsorbent coating according to (i.2) is preferably placed on the surface of the inner wall of the first substrate from the inlet end to the outlet end of the first substrate.

[0060] Preferably, the platinum group metal component of the NOx adsorbent coating according to (i.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the platinum group metal component more preferably comprises palladium, and more preferably palladium, where the first NOx adsorbent coating according to (i.2) comprises a platinum group metal component, preferably calculated as a Pd element, preferably palladium, in a concentration of 30 to 300 g / ft 3 The range is more preferably 45-200 g / ft 3 A comfortable range of 60-150 g / ft 3 A comfortable range of 60-100 g / ft 3 range or 100-150g / ft 3 In the range of 60-80 g / ft, more preferably 60-80 g / ft 3 The range is 100-140g / ft 3 Includes filling amounts within the range.

[0061] Preferably, the platinum group metal component of the NOx adsorbent coating according to (i.2) is contained in the 10-membered ring-pore zeolite material of the NOx adsorbent coating according to (i.2), where the platinum group metal component is preferably present in the zeolite material in an amount ranging from 0.5 to 10% by mass, more preferably from 1 to 6% by mass, more preferably from 1.25 to 4% by mass, and more preferably from 1.5 to 3% by mass, based on the total mass of the 10-membered ring-pore zeolite material of the NOx adsorbent coating according to (i.2).

[0062] Preferably, the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (i.2) has a framework type selected from the group consisting of FER, TON, mixtures thereof, and mixed forms thereof, more preferably the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (i.2) has a framework type FER, where the framework structure of the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (i.2) preferably comprises a tetravalent element Y, a trivalent element X, and oxygen, more preferably a tetravalent element It consists of element Y, a trivalent element X, and oxygen, where Y is preferably one or more of Si, Sn, Ti, Zr, and Ge, more preferably Si, and X is preferably one or more of Al, B, In, and Ga, more preferably Al, and the molar ratio of Y:X calculated as YO2:X2O3 is preferably in the range of 2:1 to 100:1, more preferably in the range of 10:1 to 55:1, more preferably in the range of 12:1 to 40:1, more preferably in the range of 15:1 to 28:1, and more preferably in the range of 18:1 to 25:1.

[0063] Preferably, the NOx adsorbent coating according to (i.2) contains a 10-membered ring-pore zeolite material in an amount ranging from 80 to 99.75% by mass, preferably 85 to 99.5% by mass, more preferably 90 to 99.25% by mass, and more preferably 95 to 99% by mass, based on the mass of the NOx adsorbent coating.

[0064] Preferably, the catalyst according to (i) is coated with NOx adsorbent according to (i.2) at a rate of 0.5 to 8 g / in 3 In the range of 1 to 5 g / in 3 The range is, more preferably 1.5 to 4.5 g / in 3 In the range of 2-4 g / in 3 Includes filling amounts within the range.

[0065] Preferably, 95 to 100% by mass, preferably 98 to 100% by mass, more preferably 99 to 100% by mass, and more preferably 99.5 to 100% by mass of the NOx adsorbent coating according to (i.2) consist of a platinum group metal component and a 10-membered ring pore zeolite material.

[0066] Preferably, the first substrate according to (i.1) is a flow-through substrate or a wall-flow filter substrate, preferably a flow-through substrate, the flow-through substrate is preferably one or more of a cordierite flow-through substrate and a metal flow-through substrate, the first substrate according to (i.1) is preferably cylindrical, the diameter of the first substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and the first substrate according to (i.1) has an axial length preferably in the range of 0.5 to 8 inches, more preferably in the range of 1 to 5 inches, more preferably in the range of 1.25 to 3 inches.

[0067] Preferably, the catalyst according to (i) consists of a first substrate according to (i.1) and a NOx adsorbent coating according to (i.2).

[0068] Preferably, the DOC component is (iii) A catalyst, (iii.1) A third substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the third substrate, and the inner wall of the third substrate extending through therethe; (iii.2) A first DOC coating disposed on the surface of the inner wall of the third substrate over at least 70% of the substrate axial length of the third substrate, wherein the first DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania, (iii.3) Optionally, a second DOC coating, at least partially disposed on the first DOC coating and extending over at least 20% of the substrate axial length of the third substrate, wherein the second DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania, and the second DOC coating is preferably disposed from the exit end to the inlet end of the third substrate, It is included in catalysts that contain [this ingredient].

[0069] Preferably, the platinum group metal component of the first DOC coating according to (iii.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, wherein the second platinum group metal component more preferably comprises platinum and palladium, more preferably platinum and palladium, and the mass ratio of Pt to Pd, Pt:Pd, calculated as elements Pt and Pd, is preferably in the range of 0.5:1 to 5:1, more preferably in the range of 0.75:1 to 4.5:1, more preferably in the range of 1:1 to 4:1, and more preferably in the range of 1.5:1 to 3:1.

[0070] Preferably, the non-zeolite oxide material according to (iii.2) comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably silica-doped gamma-alumina, and the non-zeolite oxide material preferably comprises an amount of alumina in the range of 80-99% by mass, more preferably 85-95% by mass, and more preferably 88-90% by mass, based on the mass of the non-zeolite oxide material, and the non-zeolite oxide material preferably comprises 75m 2 More than / g, more preferably 100m 2 The non-zeolite oxide material exhibits a BET specific surface area greater than / g, and more preferably 0.04 cm². 3More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g.

[0071] Preferably, the first DOC coating according to (iii.2) further comprises a zeolite material, preferably a 12-membered ring-pore zeolite material, the 12-membered ring-pore zeolite material preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof and two or more mixed forms thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof and two or more mixed forms thereof, more preferably having a framework type BEA for the 12-membered ring-pore zeolite material. The zeolite material preferably contains Si, Al, and oxygen, more preferably Si, Al, and oxygen, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1, and the zeolite material preferably contains copper calculated as CuO in an amount of at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass.

[0072] Preferably, the zeolite material contains iron calculated as Fe2O3 in an amount of at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass; or the zeolite material contains iron calculated as Fe2O3 in an amount preferably in the range of 0.5 to 8% by mass, and more preferably in the range of 1 to 5% by mass.

[0073] Preferably, the mass ratio of the non-zeolite oxide material of the first DOC coating according to (iii.2) to the zeolite material of the first DOC coating according to (iii.2) is in the range of 1:1 to 10:1, preferably in the range of 1.5:1 to 8:1, and more preferably in the range of 2:1 to 4.5:1.

[0074] Preferably, the catalyst according to (iii) is coated with a first DOC coating according to (iii.2) at a rate of 0.5 to 5 g / in 3 The range is preferably 0.75 to 4 g / in. 3 In the range of 1-3 g / in, more preferably 1-3 g / in 3 The range, more preferably 1.25 to 2.5 g / in 3 Includes filling amounts within the range.

[0075] Preferably, 98-100% by mass, preferably 99-100% by mass, more preferably 99.5-100% by mass of the first DOC coating according to (iii.2) consists of platinum group metal components, preferably Pt and Pd, the non-zeolite oxide material preferably comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, more preferably silica-doped gamma-alumina, the non-zeolite oxide material more preferably contains alumina in the range of 80-99% by mass, more preferably 85-95% by mass, and more preferably 88-90% by mass, based on the mass of the non-zeolite oxide material, the non-zeolite oxide material is more preferably 75m 2 More than / g, more preferably 100m 2 The non-zeolite oxide material exhibits a BET specific surface area greater than / g, and more preferably 0.04 cm². 3 More than 0.06 cm² / g 3The zeolite material exhibits a pore volume greater than / g, and is preferably a 12-membered ring pore zeolite material, the 12-membered ring pore zeolite material is preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed types thereof, more preferably has a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed types thereof, more preferably the 12-membered ring pore zeolite material has a framework type BEA, the framework structure of the zeolite material preferably contains Si, Al, and oxygen, more preferably consists of Si, Al, and oxygen, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably 2: The ratio is in the range of 1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1, wherein the zeolite material preferably contains at least 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, copper calculated as CuO, and the zeolite material contains at least 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, iron calculated as Fe2O3; or the zeolite material contains iron calculated as Fe2O3 in an amount preferably in the range of 0.5 to 8% by mass, more preferably in the range of 1 to 5% by mass.

[0076] Preferably, the first DOC coating according to (iii.2) extends over 80-100% of the substrate axial length of the third substrate according to (iii.1), preferably over 90-100%, more preferably over 95-100%, more preferably over 98-100%, and more preferably over 99-100%.

[0077] Preferably, the catalyst according to (iii) includes a second DOC coating according to (iii.3).

[0078] Preferably, the platinum group metal component of the second DOC coating according to (iii.3) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the second platinum group metal component more preferably comprises platinum and palladium, more preferably platinum and palladium, and the mass ratio of Pt to Pd, Pt:Pd, calculated as elements Pt and Pd, is preferably in the range of 2:1 to 20:1, more preferably in the range of 3:1 to 8:1, more preferably in the range of 4:1 to 7.5:1, and more preferably in the range of 5:1 to 7:1; Here, the platinum group metal component of the second DOC coating according to (iii.3) more preferably comprises platinum, where the second DOC coating according to (iii.3) contains platinum calculated as element Pt, preferably in an amount of 15 to 200 g / ft. 3 A comfortable range is 20-150 g / ft 3 Comfortably within the range of 30-100g / ft 3 In the range of 40-90 g / ft, more preferably 40-90 g / ft 3 In the range of 50-80 g / ft, more preferably 50-80 g / ft 3 The platinum group metal components of the second DOC coating according to (iii.3) are more preferably calculated as elements based on the total mass of the non-zeolite oxide material according to (ii.3) and supported on the non-zeolite oxide material according to (iii.3) in a packing amount more preferably in the range of 1 to 5 mass%, more preferably in the range of 2 to 4 mass%.

[0079] Preferably, the non-zeolite oxide material of the second DOC coating according to (iii.3) includes one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and even more preferably gamma-alumina doped with silica. The non-zeolite oxide material of the second DOC coating according to (iii.3) preferably contains alumina in an amount in the range of 80 to 99% by mass, more preferably in the range of 85 to 95% by mass, and even more preferably in the range of 88 to 90% by mass, based on the mass of the non-zeolite oxide material. The non-zeolite oxide material of the second DOC coating according to (iii.3) more preferably has a BET specific surface area exceeding 75 m 2 / g, and even more preferably exceeding 100 m 2 / g, and the non-zeolite oxide material of the second DOC coating according to (iii.3) more preferably has a pore volume exceeding 0.04 cm 3 / g, and even more preferably exceeding 0.06 cm 3 / g.

[0080] Preferably, the catalyst according to (iii) contains the second DOC coating according to (iii.3) in a filling amount in the range of 0.5 to 5 g / in 3 , preferably in the range of 0.75 to 4 g / in 3 , more preferably in the range of 0.75 to 3 g / in 3 , and even more preferably in the range of 1.25 to 2.5 g / in 3 .

[0081] Preferably, 98 to 100% by mass, preferably 99 to 100% by mass, and more preferably 99.5 to 100% by mass of the second DOC coating according to (iii.3) consists of a platinum group metal component, preferably Pt and Pd, and a non-zeolite oxide material.

[0082] Preferably, the second DOC coating according to (iii.3) extends over 30-100% of the substrate axial length of the third substrate according to (iii.1), preferably over 35-80%, more preferably over 40-60%, and more preferably over 45-55%.

[0083] Preferably, the third substrate according to (iii.1) is a flow-through substrate, preferably one or more of a cordierite flow-through substrate and a metal flow-through substrate, the third substrate according to (iii.1) is preferably cylindrical, the diameter of the third substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, and more preferably in the range of 4 to 6 inches, and the third substrate according to (iii.1) has an axial length preferably in the range of 1 to 10 inches, more preferably in the range of 1.5 to 7 inches, and more preferably in the range of 2 to 5 inches.

[0084] Preferably, the catalyst according to (iii) consists of a third substrate according to (iii.1), a first DOC coating according to (iii.2), and preferably a second DOC coating according to (iii.3). Gas heating component Preferably, (ii) the gas heating component is (ii.1) A second substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the second substrate, and the inner wall of the second substrate extending therethrough; Here, the inlet end of the second substrate according to (ii.1) and the outlet end of the first substrate according to (i.1) are coupled so that the gas exiting from the passage of the first substrate according to (i.1) can enter the passage of the second substrate according to (ii.1); Here, the inlet end of the third substrate according to (iii.1) and the outlet end of the second substrate according to (ii.1) are coupled so that the gas exiting the passage of the second substrate can enter the passage of the third substrate according to (iii.1); The inner wall of the second substrate according to (ii.1) is thermally conductive to allow heating in order to heat the exhaust gas flowing through the passage of the second substrate.

[0085] Preferably, the second substrate according to (ii.1) is a flow-through substrate, preferably a metal flow-through substrate, and more preferably a metal electrically and / or thermally conductive flow-through substrate.

[0086] Preferably, the second substrate according to (ii.1) is cylindrical in shape, and the diameter of the second substrate is preferably in the range of 3 to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, more preferably the diameter of the second substrate is in the range of 90 to 110% of the diameter of the first substrate, preferably in the range of 95 to 105%, more preferably in the range of 98 to 102%, and the first substrate according to (i.1) is a flow-through substrate or a wall flow filter substrate, preferably a flow-through substrate, and the flow-through substrate is preferably a cordierite flow-through substrate and a metal flow-through One or more base materials, wherein the first base material according to (i.1) is preferably cylindrical in shape, the diameter of the first base material is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, and more preferably in the range of 4 to 6 inches, the first base material according to (i.1) has an axial length preferably in the range of 0.5 to 8 inches, more preferably in the range of 1 to 5 inches, and more preferably in the range of 1.25 to 3 inches, and the second base material according to (ii.1) has an axial length preferably in the range of 0.15 to 2 inches, more preferably in the range of 0.20 to 1.5 inches, and more preferably in the range of 0.30 to 1 inch.

[0087] Preferably, the gas heating component according to (ii) consists of a second substrate according to (ii.1), the substrate being an uncoated substrate.

[0088] Preferably, the gas heating component according to (ii) is (ii.2) A first DOC coating disposed on the surface of the inner wall of the second substrate according to (ii.1) over at least 50% of the substrate axial length of the second substrate according to (ii.1), wherein the first DOC coating comprises a platinum group metal component and a non-zeolite oxide material containing one or more of alumina, silica, zirconia and titania, the first DOC coating; (ii.3) Optionally, a second DOC coating disposed at least partially on the first DOC coating according to (ii.2) and extending over at least 50% of the substrate axial length of the second substrate according to (ii.1), wherein the second DOC coating comprises a platinum group metal component and a non-zeolite oxide material containing one or more of alumina, silica, zirconia and titania, the second DOC coating; Further comprising.

[0089] Preferably, the platinum group metal component of the first DOC coating according to (ii.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium and ruthenium, preferably one or more of palladium, platinum and rhodium, more preferably one or more of palladium and platinum, wherein the second platinum group metal component preferably comprises platinum and palladium, more preferably platinum and palladium, and the mass ratio of Pt to Pd calculated as elements Pt and Pd, Pt:Pd, is preferably in the range of 0.5:1 to 5:1, more preferably in the range of 0.75:1 to 4.5:1, more preferably in the range of 1:1 to 4:1, more preferably in the range of 1.5:1 to 3:1.

[0090] Preferably, the platinum group metal component of the first DOC coating according to (ii.2) comprises platinum, and the first DOC coating according to (ii.2) contains platinum calculated as element Pt, preferably in the range of 15 - 200 g / ft 3 range, more preferably in the range of 20 - 150 g / ft 3 range, more preferably in the range of 30 - 100 g / ft 3 range, more preferably in the range of 40 - 90 g / ft 3 range, more preferably in the range of 50 - 80 g / ft3 The platinum group metal components of the first DOC coating according to (ii.2) are more preferably calculated as elements based on the total mass of the non-zeolite oxide material according to (ii.2) and supported on the non-zeolite oxide material according to (ii.2) in a packing amount more preferably in the range of 1 to 5 mass%, more preferably in the range of 2 to 4 mass%.

[0091] Preferably, the non-zeolite oxide material according to (ii.2) comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably silica-doped gamma-alumina, and the non-zeolite oxide material preferably contains an amount of alumina in the range of 80 to 99% by mass, more preferably 85 to 95% by mass, and more preferably 88 to 90% by mass, based on the mass of the non-zeolite oxide material.

[0092] Preferably, the non-zeolite oxide material is 75m 2 More than / g, more preferably 100m 2 It exhibits a BET specific surface area exceeding / g.

[0093] Preferably, the non-zeolite oxide material is 0.04 cm 3 More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g.

[0094] Preferably, the first DOC coating according to (ii.2) further comprises preferably a zeolite material, preferably a 12-membered ring-pore zeolite material, the 12-membered ring-pore zeolite material preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof and two or more mixed forms thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof and two or more mixed forms thereof, more preferably having a framework type 12-membered ring-pore zeolite material having framework type BEA, and the zeolite material The framework structure preferably contains Si, Al, and oxygen, more preferably consisting of Si, Al, and oxygen, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1, and the zeolite material preferably contains copper calculated as CuO in an amount of at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass; The zeolite material preferably contains iron calculated as Fe2O3 in an amount of at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass; or the zeolite material preferably contains iron calculated as Fe2O3 in an amount in the range of 0.5 to 8% by mass, more preferably 1 to 5% by mass; The mass ratio of the non-zeolite oxide material of the first DOC coating according to (ii.2) to the zeolite material of the first DOC coating according to (ii.2) is preferably in the range of 1:1 to 10:1, more preferably in the range of 1.5:1 to 8:1, and more preferably in the range of 2:1 to 4.5:1.

[0095] Preferably, the gas heating component according to (ii) is coated with a first DOC coating according to (ii.2) at a rate of 0.5 to 5 g / in 3 The range is preferably 0.75 to 4 g / in. 3 In the range of 1-3 g / in, more preferably 1-3 g / in3 The range, more preferably 1.25 to 2.5 g / in 3 Includes filling amounts within the range.

[0096] Preferably, 98 to 100% by mass, more preferably 99 to 100% by mass, and more preferably 99.5 to 100% by mass of the first DOC coating according to (ii.2) consist of a platinum group metal component, preferably Pt and Pd, a non-zeolite oxide material, and preferably a zeolite material.

[0097] Preferably, the first DOC coating according to (ii.2) extends over 80-100% of the substrate axial length of the second substrate according to (ii.1), more preferably over 90-100%, more preferably over 95-100%, more preferably over 98-100%, and more preferably over 99-100%.

[0098] Optionally, the gas heating component according to (ii) includes a second DOC coating according to (ii.3).

[0099] Preferably, the platinum group metal component of the second DOC coating according to (ii.3) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the second platinum group metal component more preferably comprises platinum and palladium, and more preferably platinum and palladium, and the mass ratio of Pt to Pd, Pt:Pd, calculated as elements Pt and Pd, is preferably in the range of 2:1 to 20:1, more preferably in the range of 3:1 to 8:1, more preferably in the range of 4:1 to 7.5:1, and more preferably in the range of 5:1 to 7:1.

[0100] Preferably, the non-zeolite oxide material of the second DOC coating according to (ii.3) comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably silica-doped gamma-alumina, and the non-zeolite oxide material of the second DOC coating according to (iii.3) preferably comprises alumina in an amount in the range of 80 to 99% by mass, more preferably 85 to 95% by mass, and more preferably 88 to 90% by mass, based on the mass of the non-zeolite oxide material.

[0101] Preferably, the non-zeolite oxide material is 75m 2 More than / g, more preferably 100m 2 It exhibits a BET specific surface area exceeding / g.

[0102] Preferably, the non-zeolite oxide material is 0.04 cm 3 More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g.

[0103] Preferably, the gas heating component according to (ii) is coated with a second DOC coating according to (ii.3) at a rate of 0.5 to 5 g / in 3 The range is, more preferably 0.75 to 4 g / in 3 The range is, more preferably 0.75 to 3 g / in 3 The range is, more preferably 1 to 2.5 g / in 3 Includes filling amounts within the range.

[0104] Preferably, 98 to 100% by mass, more preferably 99 to 100% by mass, and more preferably 99.5 to 100% by mass of the second DOC coating according to (ii.3) consist of platinum group metal components, preferably Pt and Pd, and non-zeolite oxide materials.

[0105] Preferably, the second DOC coating according to (ii.3) extends over 30-100% of the substrate axial length of the second substrate according to (ii.1), preferably over 35-80%, more preferably over 40-60%, and more preferably over 45-55%.

[0106] Preferably, the gas heating component according to (ii) comprises a second substrate according to (ii.1), a first DOC coating according to (ii.2), and preferably a second DOC coating according to (ii.3).

[0107] Preferably, the coating of the gas heating component according to (ii) exhibits essentially the same, preferably the same, chemical and physical properties as the coating of the catalyst according to (iii).

[0108] Preferably, the second substrate according to (ii.1) and the third substrate according to (iii.1) together form a single substrate including an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the single substrate, and a plurality of passages defined by the inner wall of the single substrate extending therethrough, the first DOC coating according to (ii.2) and the first DOC coating according to (iii.2) together form a single first DOC coating, preferably the second DOC coating according to (ii.3) and the second DOC coating according to (iii.3) The coatings combine to form a single second DOC coating; the single first DOC coating preferably extends over at least 90% of the substrate axial length of the single substrate, more preferably over 95-100%, more preferably over 98-100%, and more preferably over 99-100%, and preferably over the single second DOC coating preferably extends over at least 40% of the substrate axial length of the single substrate, more preferably over 45-100%, and more preferably over 50-80%.

[0109] Preferably, the exit end of the second substrate and the inlet end of the third substrate are arranged opposite each other, and the angle between the surface normal of the surface defined by the exit end of the second substrate and the surface normal of the surface defined by the inlet end of the third substrate is preferably in the range of 0 to 5°, more preferably in the range of 0 to 3°, and more preferably in the range of 0 to 1°.

[0110] Preferably, the exit end of the second substrate and the inlet end of the third substrate are spaced apart from each other by a distance preferably in the range of 2 to 20 mm, preferably in the range of 5 to 15 mm, and more preferably in the range of 8 to 12 mm, and the exit end of the second substrate and the inlet end of the third substrate are spaced apart from each other preferably by one or more spacer means, preferably by one or more spacer rods, and the given spacer rod is preferably fixed to either the exit end of the second substrate or the inlet end of the third substrate, or the exit end of the second substrate and the inlet end of the third substrate, and the one or more spacer means, preferably one or more spacer rods, is preferably electrically insulating. SCR component Preferably, the SCR component is (iv) A selective catalytic reduction (SCR) catalyst, (iv.1) A fourth substrate, preferably a wall flow filter substrate, comprising an inlet end, an outlet end, and a substrate axis length extending from the inlet end to the outlet end of the fourth substrate; (iv.2) A selective catalytic reduction (SCR) coating is applied to the surface of the inner wall of the fourth substrate according to (iv.1), It is included in selective catalytic reduction (SCR) catalysts; Here, the inlet end of the fourth substrate according to (iv.1) and the outlet end of the second substrate according to (ii.1) as defined in any one of the embodiments disclosed herein, or the outlet end of the third substrate according to (iii.1) as defined in any one of the embodiments disclosed herein, are coupled so that exhaust gas is introduced into the fourth substrate by exhaust gas exiting the passage of the second substrate or exhaust gas exiting the passage of the third substrate.

[0111] Preferably, the SCR coating according to (iv.2) comprises an 8-membered ring-pore zeolite material containing one or more copper and iron, preferably copper, and the amount of one or more copper and iron calculated as CuO and Fe2O3, more preferably the amount of copper calculated as CuO, is in the range of 1 to 10% by mass, preferably 2 to 8% by mass, more preferably 3 to 6% by mass, based on the mass of the 8-membered ring-pore zeolite material containing one or more copper and iron.

[0112] Preferably, the 8-membered ring-pore zeolite material of the selective catalytic reduction coating is selected from the group consisting of CHA, AEI, RTH, LEV, DDR, KFI, ERI, AFX, two or more mixtures thereof, and two or more mixed forms thereof, more preferably selected from the group consisting of CHA, AEI, RTH, two or more mixtures thereof, and two or more mixed forms thereof, and more preferably selected from the group consisting of CHA and AEI, and more preferably the 8-membered ring-pore zeolite material of the selective catalytic reduction coating has a framework type CHA.

[0113] Preferably, the framework structure of the 8-membered ring-pore zeolite material comprises a tetravalent element Y, a trivalent element X, and O, and more preferably consists of a tetravalent element Y, a trivalent element X, and O, where Y is one or more of Si, Sn, Ti, Zr, and Ge, and X is one or more of Al, B, In, and Ga, and the molar ratio of Y:X calculated as YO2:X2O3 is in the range of 2:1 to 45:1, preferably in the range of 10:1 to 40:1, more preferably in the range of 15:1 to 30:1, where Y preferably comprises Si, more preferably Si, and X preferably comprises one or more of Al and B, more preferably Al and B, and more preferably Al.

[0114] Preferably, a system according to any one of the embodiments disclosed above comprises a NOx adsorbent component, a DOC component, an SCR component, and a gas heating component.

[0115] Accordingly, according to the first alternative configuration of the present invention, it is particularly preferable that the NOx adsorbent coating, which is the NOx adsorbent component, is disposed on a first substrate, and the diesel oxidation catalyst (DOC) coating, which is the DOC component, is at least partially disposed on the NOx adsorbent coating as defined herein. Furthermore, according to the first alternative configuration, the gas heating component comprises a second substrate as defined herein.

[0116] Furthermore, according to the second alternative configuration of the present invention, it is particularly preferable that the NOx adsorbent coating, which is the NOx adsorbent component, is placed on a first substrate, the gas heating component includes a second substrate, and the DOC coating, which is the DOC component, is placed on a third substrate. More preferably, the gas heating component includes a first DOC coating and optionally a second DOC coating.

[0117] As defined above, the DOC component is positioned downstream of the gas heating component according to the second alternative arrangement of the present invention. Alternatively, the DOC component, which is a DOC coating, may be positioned on a third substrate upstream of the gas heating component, which includes a second substrate. System preparation method Furthermore, the present invention relates to a method for preparing a system for treating exhaust gases of a diesel internal combustion engine, preferably a method for preparing a system for treating exhaust gases of a diesel internal combustion engine according to any one of the embodiments disclosed herein, wherein the method is (1) To provide NOx adsorbent components, diesel oxidation catalyst (DOC) components, selective catalytic reduction (SCR) components, gas heating components, and reducing agent injectors, NOx adsorbent components are (i) A catalyst, (i.1) A first substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the first substrate, and the inner wall of the first substrate extending therethrough; (i.2) NOx adsorbent coating which is the NOx adsorbent component, wherein the coating is disposed on the surface of the inner wall of the first substrate over at least 50% of the substrate axial length of the first substrate, and the NOx adsorbent coating comprises a platinum group metal component and a 10-membered ring-pore zeolite material having a framework type selected from the group consisting of FER, TON, MTT, SZR, MWW, AEL, HEU, AFO, two or more mixtures thereof and two or more mixed types thereof, It is included in catalysts that contain, (2) Placing the NOx adsorbent component upstream of the gas heating component, (3) The reducing agent injector is placed upstream of the SCR component, (4) The gas heating component is placed upstream of the reducing agent injector, (5) The DOC component is placed upstream of the reducing agent injector, (6) Arranging the DOC component and the gas heating component in a direct and continuous order, Includes.

[0118] Preferably, no other components for treating the exhaust gas are placed between the DOC component according to (1) and the gas heating component according to (1).

[0119] Preferably, the components are arranged in a conduit for exhaust gases, more preferably in a continuous sequence, and the upstream end of the conduit is preferably designed to be located downstream of the diesel internal combustion engine, and more preferably, the upstream end of the conduit is located downstream of the diesel internal combustion engine.

[0120] Preferably, the DOC component is placed upstream of the gas heating component, and the DOC component and NOx adsorbent component are preferably placed upstream of the gas heating component.

[0121] Preferably, the reducing agent injector comprises one or more of a hydrocarbon injector, a hydrocarbon cylinder post-injector, and a urea injector, and more preferably consists of one or more of a hydrocarbon injector, a hydrocarbon cylinder post-injector, and a urea injector.

[0122] Preferably, when the catalyst contains a DOC component and a NOx adsorbent component, the catalyst is prepared by and / or by the method described below. (a) To provide a first substrate and a NOx adsorbent mixture comprising a source of water and platinum group metal components and a 10-membered ring pore zeolite material, (b) The NOx adsorbent mixture obtained in (a) is placed on the surface of the inner wall of a first substrate, which has an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the first substrate, and a plurality of passages defined by the inner wall of the first substrate extending through thereto over at least 50% of the substrate axis length of the first substrate. (c) Optionally, the coated substrate obtained in (b) is fired in a gas atmosphere having a temperature preferably in the range of 400 to 800°C, preferably in the range of 450 to 700°C, more preferably in the range of 550 to 650°C, wherein the gas atmosphere is preferably air. Here, prior to firing in (c), the first NOx adsorbent mixture placed on the first substrate is dried in a gas atmosphere having a temperature in the range of 90 to 150°C, preferably in the range of 100 to 120°C, the gas atmosphere is preferably air, and the drying period is preferably in the range of 0.5 to 4 hours, more preferably in the range of 0.75 to 2 hours; here, prior to firing in (c), the coated substrate obtained in (b) is dried in a gas atmosphere having a temperature in the range of 90 to 150°C, more preferably in the range of 100 to 120°C, the gas atmosphere is more preferably air, (d) To provide a diesel oxidation catalyst (DOC) mixture comprising water, a source of platinum group metal components, and a non-zeolite oxide material containing one or more of alumina, silica, zirconia, and titania, and preferably a zeolite material, The diesel oxide mixture obtained in (e)(d) is placed on a first substrate containing a NOx adsorbent coating obtained by (b) or (c) and placed thereon, over at least 70% of the substrate axial length of the first substrate, where the coated substrate is dried in a gas atmosphere having a temperature preferably in the range of 90 to 150°C, more preferably in the range of 100 to 120°C, the gas atmosphere is preferably air, and the dried substrate is fired in a gas atmosphere having a temperature preferably in the range of 400 to 800°C, more preferably in the range of 450 to 700°C, more preferably in the range of 550 to 650°C for preferably 0.25 to 5 hours; to obtain a first substrate containing a NOx adsorbent coating and a diesel oxide coating placed thereon, It also includes.

[0123] Preferably, the NOx adsorbent mixture is arranged on the surface of the inner wall of the first substrate in (b) over a length of 70-100%, preferably 80-100%, more preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the first substrate, and preferably the first NOx adsorbent mixture is arranged on the surface of the inner wall of the first substrate from the inlet end to the outlet end of the first substrate in (b).

[0124] Preferably, the platinum group metal component of the NOx adsorbent mixture according to (a) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the platinum group metal component more preferably comprises palladium, and more preferably palladium.

[0125] Preferably, the 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (a) is impregnated with a source of platinum group metal components of the NOx adsorbent mixture according to (a), the impregnation of which is preferably carried out by mixing the 10-membered ring-pore zeolite material with a source of platinum group metal components, preferably a palladium source, more preferably an aqueous solution of palladium nitrate, and the impregnated 10-membered ring-pore zeolite material is preferably dispersed in water.

[0126] Preferably, the 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (a) has a framework type selected from the group consisting of FER, TON, mixtures thereof, and mixed types thereof; more preferably, the 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (a) has a framework type FER; and the framework structure of the 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (a) preferably contains a tetravalent element Y, a trivalent element X, and oxygen; more preferably, contains a tetravalent element Y and a trivalent element X The material consists of oxygen and oxygen, where Y is preferably one or more of Si, Sn, Ti, Zr, and Ge, more preferably Si, and X is preferably one or more of Al, B, In, and Ga, more preferably Al, and the molar ratio of Y:X calculated as YO2:X2O3 is preferably in the range of 2:1 to 100:1, more preferably in the range of 10:1 to 55:1, more preferably in the range of 12:1 to 40:1, more preferably in the range of 15:1 to 28:1, and more preferably in the range of 18:1 to 25:1.

[0127] Preferably, the DOC mixture according to (d) is distributed over 80-100%, preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the first substrate, which includes a NOx adsorbent coating obtained by (b) or (c) and placed thereon, and preferably the DOC according to (d) is distributed over the first substrate, which includes a NOx adsorbent coating obtained by (b) or (c) and placed thereon, from the inlet end to the outlet end of the first substrate.

[0128] Preferably, the platinum group metal component of the DOC mixture according to (d) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, more preferably platinum, and the non-zeolite oxide material according to (d) is more preferably impregnated with the platinum group metal component of the DOC mixture according to (d).

[0129] Preferably, the non-zeolite oxide material of the DOC mixture according to (d) comprises one or more of alumina, silica, and zirconia, preferably one or more of alumina and silica, more preferably alumina, more preferably gamma-alumina, the non-zeolite oxide material preferably further comprises one or more of manganese, silicon, and zirconium, the non-zeolite oxide material more preferably comprises alumina and manganese, and the non-zeolite oxide material of the DOC mixture according to (d) preferably contains alumina in an amount in the range of 80 to 99% by mass, more preferably 85 to 98% by mass, and more preferably 90 to 97% by mass, based on the mass of the non-zeolite oxide material.

[0130] Preferably, the DOC mixture according to (d) further comprises a zeolite material, preferably a 12-membered ring-pore zeolite material, the 12-membered ring-pore zeolite material preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed types thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed types thereof, more preferably having a framework type BEA for the 12-membered ring-pore zeolite material, and the framework of the zeolite material The structure preferably comprises Si, Al, and O, more preferably Si, Al, and O, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1, and the zeolite material preferably contains copper calculated as CuO in an amount of at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass.

[0131] Preferably, the first substrate according to (a) is a flow-through substrate or a wall-flow filter substrate, preferably a flow-through substrate, the flow-through substrate preferably one or more of cordierite flow-through substrates and metal flow-through substrates, more preferably a metal flow-through substrate, the first substrate is preferably cylindrical, the diameter of the first substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and the first substrate has an axial length preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches.

[0132] Preferably, the gas heating component according to (1) comprises a second substrate having an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the second substrate, and a plurality of passages defined by the inner wall of the second substrate extending therethrough; The inlet end of the second substrate and the outlet end of the first substrate are coupled together according to (a) so that exhaust gas from the passage of the first substrate enters the passage of the second substrate; The inner wall of the second substrate is thermally conductive to allow heating in order to heat the exhaust gas flowing through the passage of the second substrate.

[0133] Preferably, the second substrate is a flow-through substrate, preferably a metal flow-through substrate, and more preferably a metal electrically and / or thermally conductive flow-through substrate.

[0134] Preferably, the second substrate is cylindrical in shape, and the diameter of the second substrate is preferably in the range of 3 to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, more preferably in the range of 90 to 110% of the diameter of the first substrate, preferably in the range of 95 to 105%, more preferably in the range of 98 to 102%, the diameter of the first substrate is preferably in the range of 3 to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, the first substrate has an axial length preferably in the range of 3 to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and the second substrate has an axial length preferably in the range of 0.15 to 2 inches, more preferably in the range of 0.20 to 1.5 inches, more preferably in the range of 0.30 to 1 inch.

[0135] Preferably, the gas heating component according to (1) is prepared by and / or the method is (g.1) Optionally, a NOx adsorbent mixture is placed on the surface of the inner wall of the second substrate over at least 50% of the substrate axial length of the second substrate, wherein the NOx adsorbent mixture comprises a source of platinum group metal components and a 10-membered ring-pore zeolite material having a framework type selected from the group consisting of FER, TON, MTT, SZR, MWW, AEL, HEU, AFO, two or more mixtures thereof and two or more mixed types thereof. (g.2) Distributing a diesel oxidation catalyst (DOC) mixture on the surface of the inner wall of the second substrate and / or on the NOx adsorbent coating of the substrate obtained from (g.1) over at least 70% of the substrate axial length of the second substrate, wherein the DOC mixture comprises a source of platinum group metal components and a source of non-zeolite oxide material containing one or more of alumina, silica, zirconia and titania. It also includes.

[0136] Preferably, the NOx adsorbent mixture according to (g.1) is distributed on the surface of the inner wall of the second substrate over an area of ​​70-100%, preferably 80-100%, more preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the second substrate. Here, the NOx adsorbent mixture according to (g.1) is preferably placed on the surface of the inner wall of the second substrate, from the outlet end to the inlet end of the second substrate.

[0137] Preferably, the platinum group metal component of the NOx adsorbent mixture according to (g.1) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the platinum group metal component more preferably comprises palladium, and more preferably palladium.

[0138] Preferably, the 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (g.1) is impregnated with a source of platinum group metal components of the NOx adsorbent mixture according to (g.1).

[0139] Preferably, the 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (g.1) has a framework type selected from the group consisting of FER, TON, mixtures thereof, and mixed types thereof, and more preferably, the 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (g.1) has a framework type FER, where the framework structure of the 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (g.1) preferably comprises a tetravalent element Y, a trivalent element X, and oxygen, and more preferably, a tetravalent element Y, 3 It consists of a valence element X and oxygen, Y is preferably one or more of Si, Sn, Ti, Zr, and Ge, more preferably Si, and X is preferably one or more of Al, B, In, and Ga, more preferably Al, and the molar ratio of Y:X calculated as YO2:X2O3 is preferably in the range of 2:1 to 100:1, more preferably in the range of 10:1 to 55:1, more preferably in the range of 12:1 to 40:1, more preferably in the range of 15:1 to 28:1, and more preferably in the range of 18:1 to 25:1.

[0140] Preferably, the DOC mixture according to (g.2) is distributed over 80-100%, preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the first substrate, on the surface of the inner wall of the second substrate and / or on the NOx adsorbent coating of the substrate obtained by (g.1), and preferably, the DOC mixture according to (g.2) is distributed over the surface of the inner wall of the second substrate and / or on the NOx adsorbent coating of the substrate obtained by (g.1), from the inlet end to the outlet end of the first substrate.

[0141] Preferably, the DOC mixture according to (g.2) is distributed over 80-100%, preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the first substrate, on the surface of the inner wall of the second substrate and / or on the NOx adsorbent coating of the substrate obtained by (g.1), and preferably, the DOC mixture according to (g.2) is distributed over the surface of the inner wall of the second substrate and / or on the NOx adsorbent coating of the substrate obtained by (g.1), from the inlet end to the outlet end of the first substrate.

[0142] Preferably, the platinum group metal component of the DOC mixture according to (g.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, more preferably platinum, and more preferably platinum.

[0143] Preferably, the non-zeolite oxide material according to (g.2) is impregnated with a source of platinum group metal components of the DOC mixture according to (g.2); Here, the source of the non-zeolite oxide material for the DOC coating according to (g.2) preferably comprises one or more of alumina, silica, and zirconia, preferably one or more of alumina and silica, more preferably alumina, more preferably gamma-alumina; the source of the non-zeolite oxide material preferably further comprises one or more of manganese, silicon, and zirconium; the source of the non-zeolite oxide material more preferably comprises alumina and manganese; and the source of the non-zeolite oxide material for the DOC mixture according to (g.2) more preferably comprises alumina in an amount in the range of 80-99% by mass, more preferably 85-98% by mass, and more preferably 90-97% by mass, based on the mass of the non-zeolite oxide material; The DOC mixture according to (g.2) preferably further comprises a zeolite material, more preferably a 12-membered ring-pore zeolite material, the 12-membered ring-pore zeolite material preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type BEA for the 12-membered ring-pore zeolite material, the framework structure of the zeolite material preferably consists of Si, Al, and O, more preferably Si, Al, and O, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably 2 The ratio is in the range of 1 to 1200:1, more preferably in the range of 10 to 400:1, more preferably in the range of 15 to 100:1, more preferably in the range of 18 to 30:1, and more preferably in the range of 20 to 26:1, wherein the zeolite material contains copper calculated as CuO, preferably at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass; or the zeolite material contains iron calculated as Fe2O3, preferably in an amount in the range of 0.5 to 8% by mass, more preferably 1 to 5% by mass.

[0144] Preferably, the exit end of the first substrate and the inlet end of the second substrate are arranged opposite each other, and the angle between the surface normal of the surface defined by the exit end of the first substrate and the surface normal of the surface defined by the inlet end of the second substrate is preferably in the range of 0 to 5°, more preferably in the range of 0 to 3°, and more preferably in the range of 0 to 1°.

[0145] Preferably, the exit end of the first substrate and the inlet end of the second substrate are spaced apart from each other by a distance of preferably 2 to 20 mm, preferably 5 to 15 mm, and more preferably 8 to 12 mm, and the exit end of the first substrate and the inlet end of the second substrate are spaced apart from each other preferably by one or more spacer means, preferably by one or more spacer rods, and the given spacer rod is preferably fixed to either the exit end of the first substrate, the inlet end of the second substrate, or the exit end of the first substrate and the inlet end of the second substrate, and the one or more spacer means, preferably one or more spacer rods, are preferably electrically insulating.

[0146] Preferably, one single substrate is used together as a first substrate and a second substrate, and the single substrate includes a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the single substrate, and an inner wall of the single substrate extending therethrough, wherein the NOx adsorbent mixture according to (b) is placed on the surface of the inner wall of the single substrate, wherein the coated substrate is dried in a gas atmosphere having a temperature preferably in the range of 90 to 150°C, more preferably in the range of 100 to 120°C, for a period preferably in the range of 0.5 to 4 hours, more preferably in the range of 0.75 to 2 hours, the gas atmosphere is preferably air, and the dried substrate is fired in a gas atmosphere having a temperature preferably in the range of 400 to 800°C, more preferably in the range of 450 to 700°C, more preferably in the range of 550 to 650°C, for a period preferably in the range of 0.25 to 5 hours, more preferably in the range of 0.5 to 2 hours, the gas atmosphere is preferably air. Here, the DOC mixture according to (d) and the DOC mixture according to (g.2) are at least partially placed on a single substrate coated with a single NOx adsorbent coating to form a single DOC coating; Here, the NOx adsorbent coating is preferably distributed over at least 50% of the substrate axial length of a single substrate, more preferably over 70-100%, more preferably over 80-100%, more preferably over 95-100%, more preferably over 98-100%, more preferably over 99-100%, and / or Here, the single DOC coating is preferably placed at least partially on the inner wall surface and / or NOx adsorbent coating of the single substrate over at least 90%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axial length of the single substrate, wherein the coated substrate is preferably dried in a gas atmosphere having a temperature in the range of 90-150°C, more preferably 100-120°C, for a period of preferably 0.5-4 hours, more preferably 0.75-2 hours, where the gas atmosphere is preferably air; and the dried substrate is preferably fired in a gas atmosphere having a temperature in the range of 400-800°C, more preferably 450-700°C, more preferably 550-650°C, for a period of preferably 0.25-5 hours, more preferably 0.5-2 hours, where the gas atmosphere is preferably air; More preferably, one single substrate is used together as a first substrate and a second substrate, and the single substrate includes a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the single substrate, and an inner wall of the single substrate extending therethrough, wherein the NOx adsorbent mixture according to (b) and the NOx adsorbent mixture according to (g.1) are placed on the inner wall of the single substrate to form a single NOx adsorbent coating, wherein the coated substrate is preferably heated in a gas atmosphere having a temperature in the range of 90 to 150°C, more preferably in the range of 100 to 120°C, for a range of 0.5 to 4 hours, The substrate is preferably dried for a period of 0.75 to 2 hours, with the gas atmosphere preferably being air, and the dried substrate is preferably calcined for a period of 0.25 to 5 hours, preferably being 0.5 to 2 hours, in a gas atmosphere having a temperature preferably in the range of 400 to 800°C, preferably in the range of 450 to 700°C, more preferably in the range of 550 to 650°C, with the gas atmosphere preferably being air, where the DOC mixture according to (d) and the DOC mixture according to (g.2) are at least partially placed on a single substrate coated with a single NOx adsorbent coating to form a single DOC coating; Here, a single NOx adsorbent coating is preferably positioned over at least 50% of the substrate axial length of a single substrate, more preferably over 70-100%, more preferably over 80-100%, more preferably over 95-100%, more preferably over 98-100%, more preferably over 99-100%, and / or A single DOC coating is preferably applied at least partially to the surface of the inner wall of a single substrate and / or a single NOx adsorbent coating over at least 90%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axial length of the single substrate, wherein the coated substrate is dried in a gas atmosphere having a temperature preferably in the range of 90-150°C, more preferably in the range of 100-120°C, for a period preferably in the range of 0.5-4 hours, more preferably in the range of 0.75-2 hours, where the gas atmosphere is preferably air. The dried substrate is then fired in a gas atmosphere having a temperature preferably in the range of 400-800°C, more preferably in the range of 450-700°C, more preferably in the range of 550-650°C, for a period preferably in the range of 0.25-5 hours, more preferably in the range of 0.5-2 hours, where the gas atmosphere is preferably air.

[0147] Preferably, the first and second substrates according to (a) are surrounded by a jacket, with preferably 95-100%, more preferably 98-100%, more preferably 99-100% of the inlet end face of the first substrate and preferably 95-100%, more preferably 98-100%, more preferably 99-100% of the outlet end face of the second substrate not covered by the jacket, where the jacket preferably includes one or more means for connecting the second substrate to a power source.

[0148] Preferably, the DOC component is located downstream of the gas heating component.

[0149] Preferably, when the catalyst contains a NOx adsorbent component, the catalyst is prepared by and / or the method is (n.1) To provide a first substrate including an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the first substrate, and a plurality of passages defined by the inner wall of the first substrate extending therethrough; (n.2) Placing a NOx adsorbent mixture on the surface of the inner wall of a first substrate over at least 50% of the substrate axial length of the first substrate, wherein the NOx adsorbent mixture comprises a source of platinum group metal components and a 10-membered ring-pore zeolite material, wherein the coated substrate is dried in a gas atmosphere having a temperature preferably in the range of 90 to 150°C, more preferably in the range of 100 to 120°C, for a period preferably in the range of 0.5 to 4 hours, more preferably in the range of 0.75 to 2 hours, where the gas atmosphere is preferably air; and placing the NOx adsorbent mixture in a gas atmosphere having a temperature preferably in the range of 400 to 800°C, more preferably in the range of 450 to 700°C, more preferably in the range of 550 to 650°C, for a period preferably in the range of 0.25 to 5 hours, more preferably in the range of 0.5 to 2 hours, where the gas atmosphere is preferably air; It also includes.

[0150] Preferably, the NOx adsorbent mixture according to (n.2) is placed on the surface of the inner wall of the first substrate over a length of 70-100%, preferably 80-100%, more preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the first substrate, and the first NOx adsorbent mixture according to (n.2) is preferably placed on the surface of the inner wall of the first substrate from the inlet end to the outlet end of the first substrate.

[0151] Preferably, the platinum group metal component of the NOx adsorbent coating according to (n.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the platinum group metal component more preferably comprises palladium, and more preferably palladium, where the platinum group metal component of the NOx adsorbent coating according to (n.2) is preferably impregnated into a 10-membered ring-pore zeolite material.

[0152] Preferably, the 10-membered ring-pore zeolite material coated with (n.2) has a framework type selected from the group consisting of FER, TON, mixtures thereof, and mixed types thereof, more preferably the 10-membered ring-pore zeolite material coated with (n.2) has a framework type FER, and the framework structure of the 10-membered ring-pore zeolite material coated with (n.2) preferably contains a tetravalent element Y, a trivalent element X, and oxygen, more preferably a tetravalent element The material consists of Y, a trivalent element X, and oxygen, where Y is preferably one or more of Si, Sn, Ti, Zr, and Ge, more preferably Si, and X is preferably one or more of Al, B, In, and Ga, more preferably Al, and the molar ratio of Y:X calculated as YO2:X2O3 is preferably in the range of 2:1 to 100:1, more preferably in the range of 10:1 to 55:1, more preferably in the range of 12:1 to 40:1, more preferably in the range of 15:1 to 28:1, and more preferably in the range of 18:1 to 25:1.

[0153] Preferably, the first substrate according to (n.1) is a flow-through substrate or a wall-flow filter substrate, preferably a flow-through substrate, the flow-through substrate is preferably one or more of a cordierite flow-through substrate and a metal flow-through substrate, the first substrate according to (n.1) is preferably cylindrical, the diameter of the first substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and the first substrate according to (n.1) has an axial length preferably in the range of 0.5 to 8 inches, more preferably in the range of 1 to 5 inches, more preferably in the range of 1.25 to 3 inches.

[0154] Preferably, if the catalyst contains a DOC component, the catalyst is prepared by and / or the method is (d.1) To provide a third substrate, which includes an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the third substrate, and a plurality of passages defined by the inner wall of the third substrate extending therethrough; (d.2) Placing the first DOC mixture on the surface of the inner wall of the third substrate over at least 70% of the substrate axial length of the third substrate, wherein the first DOC mixture comprises a source of platinum group metal components and a source of non-zeolite oxide material containing one or more of alumina, silica, zirconia and titania; (d.3) Optionally, a second DOC mixture is placed on a third substrate coated with a first DOC mixture over at least 20% of the substrate axial length of the third substrate, wherein the second DOC mixture comprises a source of platinum group metal components and a source of non-zeolite oxide material comprising one or more of alumina, silica, zirconia, and titania, and the second DOC coating preferably comprises the placement of the second DOC mixture from the exit end to the inlet end of the third substrate. It also includes.

[0155] Preferably, the platinum group metal component of the first DOC mixture according to (d.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the second platinum group metal component more preferably comprises platinum and palladium, and more preferably platinum and palladium.

[0156] Preferably, the source of the non-zeolite oxide material according to (d.2) comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably silica-doped gamma-alumina, and the non-zeolite oxide material preferably comprises an amount of alumina in the range of 80-99% by mass, more preferably 85-95% by mass, and more preferably 88-90% by mass, based on the mass of the non-zeolite oxide material, and the non-zeolite oxide material preferably comprises 75m 2 More than / g, more preferably 100m 2 The non-zeolite oxide material exhibits a BET specific surface area greater than / g, and more preferably 0.04 cm². 3 More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g.

[0157] Preferably, the first DOC coating according to (d.2) further comprises a zeolite material, preferably a 12-membered ring-pore zeolite material, the 12-membered ring-pore zeolite material preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof and two or more mixed forms thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof and two or more mixed forms thereof, more preferably having a framework type BEA for the 12-membered ring-pore zeolite material, and the frame of the zeolite material The workpiece structure preferably contains Si, Al, and oxygen, more preferably consists of Si, Al, and oxygen, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1, and the zeolite material preferably contains copper calculated as CuO, preferably at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass.

[0158] Preferably, the first DOC mixture according to (d.2) is distributed over 80-100% of the substrate axis length of the third substrate according to (d.1), preferably over 90-100%, more preferably over 95-100%, more preferably over 98-100%, and more preferably over 99-100%.

[0159] Preferably, the second DOC mixture is placed on a third substrate coated with the first DOC mixture according to (d.3).

[0160] Preferably, the source of the platinum group metal component of the second DOC mixture according to (d.3) contains one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the source of the second platinum group metal component more preferably contains platinum and palladium, and more preferably is platinum and palladium.

[0161] Preferably, the non-zeolite oxide material of the second DOC mixture according to (d.3) contains one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably gamma-alumina doped with silica, where the non-zeolite oxide material of the second DOC mixture according to (d.3) preferably contains alumina in an amount in the range of 80 to 99% by mass, more preferably in the range of 85 to 95% by mass, and more preferably in the range of 88 to 90% by mass based on the mass of the non-zeolite oxide material, and the non-zeolite oxide material more preferably has a BET specific surface area exceeding 75 m 2 / g, and more preferably exceeding 100 m 2 / g.

[0162] Preferably, the second DOC mixture according to (d.3) is disposed over 30 to 100% of the substrate axial length of the third substrate according to (d.1), preferably over 35 to 80%, more preferably over 40 to 60%, and more preferably over 45 to 55%.

[0163] Preferably, the third substrate according to (d.1) is a flow-through substrate, preferably one or more of a cordierite flow-through substrate and a metal flow-through substrate, the third substrate according to (d.1) is preferably cylindrical, the diameter of the third substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, and more preferably in the range of 4 to 6 inches, and the third substrate according to (d.1) has an axial length preferably in the range of 1 to 10 inches, more preferably in the range of 1.5 to 7 inches, and more preferably in the range of 2 to 5 inches.

[0164] Preferably, the gas heating component is (g.1') A second substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the second substrate, and the inner wall of the second substrate extending through thereto; Here, the inlet end of the second substrate by (g.1') and the outlet end of the first substrate by (n.1) are coupled such that the gas exiting the passage of the first substrate by (n.1) enters the passage of the second substrate by (g.1'); Here, the inlet end of the third substrate according to (d.1) and the outlet end of the second substrate according to (g.1') are coupled so that the gas exiting the passage of the second substrate can enter the passage of the third substrate according to (d.1); The inner wall of the second substrate according to (g.1') is thermally conductive to allow heating therein in order to heat the exhaust gas flowing through the passage of the second substrate.

[0165] Preferably, the second substrate according to (g.1') is a flow-through substrate, preferably a metal flow-through substrate, and more preferably a metal electrically and / or thermally conductive flow-through substrate.

[0166] Preferably, the second substrate according to (g.1') is cylindrical in shape, and the diameter of the second substrate is preferably in the range of 3 to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, more preferably in the range of 90 to 110% of the diameter of the first substrate as defined in Embodiment 48, and the second substrate according to (g.1') has an axial length preferably in the range of 0.15 to 2 inches, more preferably in the range of 0.20 to 1.5 inches, more preferably in the range of 0.30 to 1 inch.

[0167] Preferably, the gas heating component is prepared by and / or the method is (g.2') Placing the first DOC mixture on the surface of the inner wall of the second substrate according to (g.1') over at least 70% of the substrate axis length of the second substrate according to (g.1'), wherein the first DOC mixture comprises a source of platinum group metal components and a source of non-zeolite oxide material containing one or more of alumina, silica, zirconia, and titania. (g.3') Optionally, a second DOC mixture is placed on a second substrate coated with the first DOC mixture according to (g.2') over at least 70% of the substrate axial length of the second substrate according to (g.1'), wherein the second DOC mixture contains a source of platinum group metal components and a non-zeolite oxide material containing one or more of alumina, silica, zirconia, and titania. It also includes.

[0168] Preferably, the second substrate according to (g.1') is a flow-through substrate, preferably a metal flow-through substrate, and more preferably a metal electrically and / or thermally conductive flow-through substrate.

[0169] Preferably, the second substrate according to (g.1') is cylindrical in shape, and the diameter of the second substrate is preferably in the range of 3 to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and more preferably the diameter of the second substrate is in the range of 90 to 110% of the diameter of the first substrate, preferably in the range of 95 to 105%, more preferably in the range of 98 to 102%, and the first substrate is preferably a flow-through substrate or a wall-flow filter substrate, preferably a flow-through substrate, and the flow-through substrate is preferably a cordierite flow-through substrate and a metal One or more flow-through substrates, the first substrate is preferably cylindrical in shape, the diameter of the first substrate is preferably in the range of 3 to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, the first substrate has an axial length preferably in the range of 0.5 to 8 inches, more preferably in the range of 1 to 5 inches, more preferably in the range of 1.25 to 3 inches, and the second substrate according to (g.1') has an axial length preferably in the range of 0.15 to 2 inches, more preferably in the range of 0.20 to 1.5 inches, more preferably in the range of 0.30 to 1 inch.

[0170] Preferably, the gas heating component is prepared by the following method, and / or the method is (g.2') Placing the first DOC mixture on the surface of the inner wall of the second substrate according to (g.1') over at least 70% of the substrate axis length of the second substrate according to (g.1'), wherein the first DOC mixture comprises a source of platinum group metal components and a source of non-zeolite oxide material containing one or more of alumina, silica, zirconia, and titania. (g.3') Preferably, the second DOC mixture is placed on a second substrate coated with the first DOC mixture according to (g.2') over at least 70% of the substrate axial length of the second substrate according to (g.1'), wherein the second DOC mixture includes a source of platinum group metal components and a source of non-zeolite oxide material containing one or more of alumina, silica, zirconia, and titania. It also includes.

[0171] Preferably, the source of the platinum group metal component in the first DOC mixture according to (g.2') includes one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the source of the metal group metal component more preferably includes platinum and palladium, and more preferably platinum and palladium.

[0172] Preferably, the source of the non-zeolite oxide material according to (g.2') comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably silica-doped gamma-alumina, where the source of the non-zeolite oxide material preferably contains alumina in an amount in the range of 80-99% by mass, more preferably 85-95% by mass, and more preferably 88-90% by mass, based on the mass of the non-zeolite oxide material.

[0173] Preferably, the source of the non-zeolite oxide material is 75m 2 More than / g, more preferably 100m 2 It exhibits a BET specific surface area exceeding / g.

[0174] Preferably, the source of the non-zeolite oxide material is more preferably 0.04 cm 3 More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g.

[0175] Preferably, the first DOC mixture according to (g.2') further comprises a zeolite material, preferably a 12-membered ring-pore zeolite material, the 12-membered ring-pore zeolite material preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof and two or more mixed forms thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof and two or more mixed forms thereof, more preferably having a framework type 12-membered ring-pore zeolite material having a framework type BEA, and the framework of the zeolite material The zeolite structure preferably contains Si, Al, and oxygen, more preferably consisting of Si, Al, and oxygen, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1, and the zeolite material preferably contains copper calculated as CuO in an amount of at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass; The first DOC mixture according to (g.2') is distributed over 80-100% of the substrate axis length of the second substrate according to (g.1'), preferably over 90-100%, more preferably over 95-100%, more preferably over 98-100%, and more preferably over 99-100%.

[0176] Preferably, the gas heating component includes a second DOC coating by (g.3').

[0177] Preferably, the source of the platinum group metal component of the second DOC mixture according to (g.3') comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum. The source of the non-zeolite oxide material of the second DOC mixture according to (g.3’) preferably includes one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, more preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably gamma-alumina doped with silica, where the non-zeolite oxide material of the second DOC mixture according to (g.3’) preferably contains alumina in an amount in the range of 80 to 99% by mass, more preferably in the range of 85 to 95% by mass, and more preferably in the range of 88 to 90% by mass based on the mass of the non-zeolite oxide material; where the source of the non-zeolite oxide material more preferably has a BET specific surface area exceeding 75 m 2 / g, and more preferably exceeding 100 m 2 / g; where the source of the non-zeolite oxide material more preferably has a pore volume exceeding 0.04 cm 3 / g, and more preferably exceeding 0.06 cm 3 / g; The second DOC mixture according to (g.3’) is preferably arranged over 30 to 100% of the substrate axial length of the second substrate according to (g.1’), preferably over 35 to 80%, more preferably over 40 to 60%, and more preferably over 45 to 55%.

[0178] Preferably, the coating of the gas heating component exhibits essentially the same, preferably the same chemical and physical properties as the coating of the catalyst defined in any one of the embodiments disclosed herein.

[0179] Preferably, one single substrate is used to form a second substrate according to (g.1') and a third substrate according to (d.1), the single substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the single substrate, and the inner wall of the single substrate extending therethrough, the first DOC mixture according to (g.2') and the first DOC mixture according to (d.2) being arranged together to form one single first DOC coating, preferably the second DOC mixture according to (g.3') and (d.3) The second DOC mixture is arranged together to form a single second DOC coating; the single first DOC mixture is preferably arranged over at least 90% of the substrate axial length of the single substrate, more preferably over 95-100%, more preferably over 98-100%, and more preferably over 99-100%; the single second DOC mixture is preferably arranged over at least 40% of the substrate axial length of the single substrate, more preferably over 45-100%, and more preferably over 50-80%.

[0180] Preferably, the exit end of the second substrate and the inlet end of the third substrate are positioned opposite each other, and the angle between the surface normal of the surface defined by the exit end of the second substrate and the surface normal of the surface defined by the inlet end of the third substrate is preferably in the range of 0 to 5°, more preferably in the range of 0 to 3°, and more preferably in the range of 0 to 1°.

[0181] Preferably, the exit end of the second substrate and the inlet end of the third substrate are spaced apart from each other by a distance preferably in the range of 2 to 20 mm, preferably in the range of 5 to 15 mm, and more preferably in the range of 8 to 12 mm, and the exit end of the second substrate and the inlet end of the third substrate are spaced apart from each other preferably by one or more spacer means, preferably by one or more spacer rods, and the given spacer rod is preferably fixed to either the exit end of the second substrate or the inlet end of the third substrate, or the exit end of the second substrate and the inlet end of the third substrate, and the one or more spacer means, preferably one or more spacer rods, is preferably electrically insulating.

[0182] Preferably, a selective catalytic reduction (SCR) catalyst is provided as the SCR component, and the selective catalytic reduction (SCR) catalyst is (s.1) To provide a fourth substrate, preferably a wall flow filter substrate, which includes an inlet end, an outlet end, and a substrate axis length extending from the inlet end to the outlet end of the third substrate; (s.2) Placing a selective catalytic reduction (SCR) mixture on the fourth substrate according to (s.1); The mixture is prepared by (s.1), where the inlet end of the fourth substrate according to (s.1) and either the outlet end of the second substrate according to (s.1) or the outlet end of the third substrate according to (d.1) are coupled so that the exhaust gas from the passage of the second substrate enters the third substrate.

[0183] Preferably, the SCR mixture according to (s.2) comprises one or more copper and iron, preferably copper, in an 8-membered ring porous zeolite material, where the amount of one or more copper and iron calculated as CuO and Fe2O3, and more preferably the amount of copper calculated as CuO, is in the range of 1 to 10% by mass, preferably 2 to 8% by mass, and more preferably 3 to 6% by mass, based on the mass of the 8-membered ring porous zeolite material containing one or more copper and iron.

[0184] Preferably, the 8-membered ring-pore zeolite material of the selective catalytic reduction coating is selected from the group consisting of CHA, AEI, RTH, LEV, DDR, KFI, ERI, AFX, two or more mixtures thereof, and two or more mixed forms thereof, more preferably selected from the group consisting of CHA, AEI, RTH, two or more mixtures thereof, and two or more mixed forms thereof, and more preferably selected from the group consisting of CHA and AEI, and more preferably the 8-membered ring-pore zeolite material of the selective catalytic reduction coating has a framework type CHA.

[0185] Preferably, the framework structure of the 8-membered ring-pore zeolite material comprises a tetravalent element Y, a trivalent element X, and O, and more preferably consists of a tetravalent element Y, a trivalent element X, and O, where Y is one or more of Si, Sn, Ti, Zr, and Ge, and X is one or more of Al, B, In, and Ga, and the molar ratio of Y:X calculated as YO2:X2O3 is in the range of 2:1 to 45:1, preferably in the range of 10:1 to 40:1, more preferably in the range of 15:1 to 30:1, where Y preferably comprises Si, more preferably Si, and X preferably comprises one or more of Al and B, more preferably Al and B, and more preferably Al.

[0186] Preferably, the reducing agent injector comprises one or more of a hydrocarbon injector, a hydrocarbon cylinder post-injector, and a urea injector, preferably one or more of a hydrocarbon injector, a hydrocarbon cylinder post-injector, and a urea injector, preferably a urea injector, and the reducing agent injector is preferably positioned downstream of the DOC component.

[0187] Product-by-process The present invention further relates to a system for treating exhaust gases of a diesel internal combustion engine, preferably a system for treating exhaust gases of a diesel internal combustion engine according to any one of the embodiments disclosed herein, which can be obtained or obtained by a method according to any one of the embodiments disclosed herein.

[0188] Exhaust gas treatment methods The present invention further relates to a method for processing exhaust gases from a diesel internal combustion engine, comprising providing exhaust gases from the diesel internal combustion engine and passing the exhaust gases through a system according to any one of the embodiments disclosed herein.

[0189] Preferably, one or more of a reducing agent, more preferably a hydrocarbon and urea, is injected into the exhaust gas passing through the system via a reducing agent injector.

[0190] Preferably, the exhaust gas is heated through a gas heating component included in the system for heating one or more of the SCR component, DOC component, and NA adsorbent component included in the system.

[0191] The present invention further relates to the use of a system according to any one of the embodiments disclosed herein for treating exhaust gases of a diesel internal combustion engine, wherein the use includes passing the exhaust gases through the system.

[0192] For example, a reducing agent injector may include a pump mechanism and / or valves for introducing one or more reducing agents into the exhaust gas, the pump mechanism and / or valves being connected to a control device, which is preferably integrated into a monitoring system that allows for precise control of the amount of one or more reducing agents introduced into the exhaust gas, depending on the desired composition of the exhaust gas when the exhaust gas comes into contact with at least a portion of the catalyst bed. [Modes for carrying out the invention]

[0193] In the context of this invention, the term “interior wall surface” is understood as the “bare,” “exposed,” or “blank” surface of the wall, that is, the untreated surface of the wall made of the wall material, apart from unavoidable impurities that may contaminate the surface.

[0194] In the context of the present invention, the term "consisting of" with respect to the mass percentage of one or more components indicates the mass percentage amount of the component based on 100 mass percent of the specified entity. For example, the phrase "0 to 0.001 mass percent of the first coating consists of X" indicates that 0 to 0.01 mass percent of 100 mass percent of the components constituting the coating is X.

[0195] In the context of the present invention, the platinum group metal component preferably comprises one or more platinum group metals, or one or more oxides of one or more platinum group metals, and more preferably comprises one or more platinum group metals, or one or more oxides of one or more platinum group metals.

[0196] In the context of this invention, the mass / filling amount of a platinum group metal component is calculated as the mass / filling amount of each platinum group metal as an element, or as the sum of the mass / filling amounts of each platinum group metal as an element. For example, if the platinum group metal component is Rh, the mass of the platinum group metal component is calculated as element Rh. As a further example, if the platinum group metal component consists of Pt and Pd, the mass of the platinum group metal component is calculated as elements Pt and Pd.

[0197] In the context of this invention, "amount of filling of a given component / coating" (g / in 3 or g / ft 3 The term refers to the mass of the component / coating per unit volume of the substrate, where the volume of the substrate is defined by multiplying the substrate axial length over which the component / coating exists in the cross-section of the substrate. For example, extending over x% of the substrate axial length, X g / in 3 When referring to the filling amount of a first coating having a filling amount of , the filling amount is the total volume of the substrate (in units in 3 This refers to X grams of the first coating per x% of ).

[0198] Furthermore, in the context of the present invention, the phrase "X is one or more of A, B, and C" (where X is a given feature and each of A, B, and C represents a specific realization of the feature) is understood to disclose that X is either A, or B, or C, or A and B, or A and C, or B and C, or A, B, and C. In this regard, it should be noted that those skilled in the art can translate the above abstract terms into specific examples, for example, if X is a chemical element and A, B, and C are specific elements such as Li, Na, and K, or if X is a temperature and A, B, and C are specific temperatures such as 10°C, 20°C, and 30°C. In this regard, those skilled in the art should further note that the above terms can be expanded to less specific realizations of the features, for example, "X is one or more of A and B" to "X is A, or B, or A and B," or to more specific relationships, for example, "X is one or more of A, B, C, and D" to "X is A, or B, or C, or D, or A and B, or A and C, or A and D, or B and C, or B and D, or C and D, or A and B and C, or A and B and D, or B and C and D, or A and B and C and D.

[0199] In the context of the present invention, the mass / filling ratio of non-zeolite oxide materials is calculated as the mass / filling ratio of each non-zeolite oxide material as an oxide, or as the sum of the mass / filling ratios of each non-zeolite oxide material as an oxide. For example, if the non-zeolite oxide material is silica, the mass of the non-zeolite oxide material is calculated as SiO2. As a further example, if the non-zeolite oxide material consists of a mixed oxide containing TiO2 and Al2O3, the mass of the non-zeolite oxide material is calculated as the sum of TiO2 and Al2O3.

[0200] In the context of this invention, the term "based on the mass of the zeolite material" refers to the mass of the zeolite material alone, i.e., it does not include platinum group metal components.

[0201] The present invention is further described by the following series of embodiments and combinations of dependent embodiments and backreferences indicated. In particular, it should be noted that in each example where the scope of an embodiment is referred to, for example, in the context of terms such as "any one of Embodiments 1 to 4", all embodiments within this scope are expressly disclosed to those skilled in the art, i.e., the expression of this term should be understood by those skilled in the art as synonymous with "any one of Embodiments 1, 2, 3 and 4". Furthermore, it should be clearly noted that the subsequent series of embodiments represent a well-structured portion of the description directed toward general and preferred embodiments of the invention, rather than a series of claims that determine the scope of protection.

[0202] A system for treating exhaust gases from diesel engines 1. A system for treating exhaust gas from a diesel internal combustion engine, the system comprising a NOx adsorbent component, a diesel oxidation catalyst (DOC) component, a selective catalytic reduction (SCR) component, a gas heating component, and a reducing agent injector, wherein the NOx adsorbent component is located upstream of the gas heating component, the reducing agent injector is located upstream of the SCR component, the gas heating component is located upstream of the reducing agent injector, the DOC component is located upstream of the reducing agent injector, and the DOC component and the gas heating component are in a direct continuous configuration. The aforementioned NOx adsorbent component is (i) A catalyst, (i.1) A first substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the first substrate, and the inner wall of the first substrate extending therethrough; (i.2) NOx adsorbent coating which is the NOx adsorbent component, wherein the coating is disposed on the surface of the inner wall of the first substrate over at least 50% of the substrate axial length of the first substrate, and the NOx adsorbent coating comprises a platinum group metal component and a 10-membered ring-pore zeolite material having a framework type selected from the group consisting of FER, TON, MTT, SZR, MWW, AEL, HEU, AFO, two or more mixtures thereof and two or more mixed types thereof, A system that includes a catalyst containing [this].

[0203] 2. The system according to Embodiment 1, wherein no other components for treating exhaust gas are placed between the DOC component and the gas heating component.

[0204] 3. The system according to Embodiment 1 or 2, wherein the components are preferably arranged in a continuous sequence in an exhaust gas conduit, the upstream end of the conduit is preferably designed to be located downstream of a diesel internal combustion engine, and more preferably the upstream end of the conduit is located downstream of a diesel internal combustion engine.

[0205] 4. The system according to any one of Embodiments 1 to 3, wherein the reducing agent injector comprises one or more of a hydrocarbon injector, a hydrocarbon cylinder post-injector, and a urea injector, preferably a urea injector, and preferably consists of one or more of a hydrocarbon injector, a hydrocarbon cylinder post-injector, and a urea injector, preferably a urea injector, and the reducing agent injector is preferably positioned downstream of the DOC component.

[0206] First alternative arrangement 5. The system according to any one of Embodiments 1 to 4, wherein the DOC component is located upstream of the gas heating component, and preferably the DOC component and the NOx adsorbent component are located upstream of the gas heating component.

[0207] 6. The catalyst according to (i) is (i.3) a diesel oxidation catalyst (DOC) coating which is the DOC component, wherein the DOC coating is at least partially disposed on the NOx adsorbent coating over at least 70% of the substrate axial length of the first substrate, the DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania, and the DOC coating is preferably disposed from the outlet end to the inlet end of the first substrate, the system according to any one of Embodiments 1 to 5, preferably Embodiment 5.

[0208] 7. The NOx adsorbent coating according to (i.2) is distributed on the surface of the inner wall of the first substrate over 70-100%, preferably 80-100%, more preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the first substrate, and the first NOx adsorbent coating according to (i.2) is preferably distributed on the surface of the inner wall of the first substrate from the inlet end to the outlet end of the first substrate, the system according to Embodiment 6.

[0209] 8. The platinum group metal component of the NOx adsorbent coating according to (i.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the platinum group metal component more preferably comprises palladium, and more preferably palladium, where the first NOx adsorbent coating according to (i.2) comprises a calculated platinum group metal component, preferably palladium, preferably 30 to 300 g / ft, where the platinum group metal element is preferably the Pd element. 3 The range is more preferably 45-200 g / ft 3 A comfortable range of 60-150 g / ft 3 A comfortable range of 60-100 g / ft 3 range or 100-150g / ft 3 In the range of 60-80 g / ft, more preferably 60-80 g / ft3 The range is 100-140g / ft 3 The system according to embodiment 6 or 7, including a filling amount within the range of [amount].

[0210] 9. The system according to any one of Embodiments 6 to 8, wherein the platinum group metal component of the NOx adsorbent coating according to (i.2) is contained in the 10-membered ring-pore zeolite material of the NOx adsorbent coating according to (i.2), where the platinum group metal component is preferably present in the zeolite material in an amount ranging from 0.5 to 10% by mass, more preferably from 1 to 6% by mass, more preferably from 1.25 to 4% by mass, and more preferably from 1.5 to 3% by mass, based on the total mass of the 10-membered ring-pore zeolite material of the NOx adsorbent coating according to (i.2).

[0211] 10. The 10-membered ring-pore zeolite material coated with NOx adsorbent according to (i.2) has a framework type selected from the group consisting of FER, TON, mixtures thereof, and mixed forms thereof, more preferably the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (i.2) has a framework type FER, where the framework structure of the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (i.2) preferably comprises a tetravalent element Y, a trivalent element X, and oxygen, more preferably a tetravalent element Y, a trivalent element X, and oxygen A system according to any one of Embodiments 6 to 9, comprising, where Y is preferably one or more of Si, Sn, Ti, Zr, and Ge, more preferably Si, and X is preferably one or more of Al, B, In, and Ga, more preferably Al, and the molar ratio of Y:X calculated as YO2:X2O3 is preferably in the range of 2:1 to 100:1, more preferably in the range of 10:1 to 55:1, more preferably in the range of 12:1 to 40:1, more preferably in the range of 15:1 to 28:1, and more preferably in the range of 18:1 to 25:1.

[0212] The NOx adsorbent coating according to 11.(i.2) comprises a 10-membered ring-pore zeolite material in an amount ranging from 80 to 99.75% by mass, preferably 85 to 99.5% by mass, more preferably 90 to 99.25% by mass, and more preferably 95 to 99% by mass, based on the mass of the NOx adsorbent coating, according to any one of Embodiments 6 to 10.

[0213] The catalyst according to 12.(i) is 0.5-8 g / in 3 In the range of 1 to 5 g / in 3 The range is, more preferably 1.5 to 4.5 g / in 3 In the range of 2-4 g / in 3 A system according to any one of embodiments 6 to 11, comprising a NOx adsorbent coating by (i.2) in a filling amount within the range of .

[0214] The system according to any one of Embodiments 6 to 12, wherein 95 to 100% by mass, preferably 98 to 100% by mass, more preferably 99 to 100% by mass, and more preferably 99.5 to 100% by mass of the NOx adsorbent coating according to 13.(i.2) consists of a platinum group metal component and a 10-membered ring pore zeolite material.

[0215] 14. The system according to any one of Embodiments 6 to 13, wherein the DOC coating according to (i.3) is at least partially disposed on the NOx adsorbent coating according to (i.2) and extends over 80-100%, preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axial length of the first substrate, and the DOC according to (i.3) is preferably at least partially disposed on the NOx adsorbent coating according to (i.2) from the inlet end to the outlet end of the first substrate.

[0216] 15. The platinum group metal component of the DOC coating according to (i.3) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, more preferably platinum, and the DOC coating according to (i.3) comprises a calculated platinum group metal component, preferably platinum, preferably 15 to 200 g / ft, with the platinum group metal element preferably Pt. 3 A comfortable range is 20-150 g / ft 3 Comfortably within the range of 30-100g / ft 3 In the range of 40-90 g / ft, more preferably 40-90 g / ft 3 In the range of 50-80 g / ft, more preferably 50-80 g / ft 3 It contains in a filling amount within the range, Here, the platinum group metal component of the DOC coating according to (i.3) more preferably comprises platinum and palladium, where the mass ratio of platinum to palladium, Pt:Pd, calculated as elements, is more preferably in the range of 1:1 to 11:1, more preferably in the range of 2:1 to 10:1, more preferably in the range of 3:1 to 5:1, and the mass ratio is more preferably about 4:1. Herein, the platinum group metal components of the DOC coating according to (i.3) are more preferably calculated as elements based on the total mass of the non-zeolite oxide material according to (i.3) and supported on the non-zeolite oxide material according to (i.3) in a packing amount more preferably in the range of 1 to 5 mass%, more preferably in the range of 2 to 4 mass%, according to any one of embodiments 6 to 14 of the system.

[0217] 16. The non-zeolite oxide material of the DOC coating according to (i.3) comprises one or more of alumina, silica, and zirconia, preferably one or more of alumina and silica, more preferably alumina, more preferably gamma-alumina, the non-zeolite oxide material preferably further comprises one or more of manganese, silicon, and zirconium, the non-zeolite oxide material more preferably comprises alumina and manganese, the non-zeolite oxide material of the DOC coating according to (i.3) more preferably comprises alumina in an amount in the range of 80-99% by mass, more preferably 85-98% by mass, more preferably 90-97% by mass, based on the mass of the non-zeolite oxide material, and the non-zeolite oxide material of the DOC coating according to (i.3) more preferably 75m 2 More than / g, more preferably 100m 2 The non-zeolite oxide material exhibiting a BET specific surface area greater than / g and DOC coating according to (i.3) is more preferably 0.04 cm². 3 More than 0.06 cm² / g 3 The system according to any one of embodiments 6 to 15, exhibiting a pore volume greater than / g.

[0218] The DOC coating according to 17.(i.3) further comprises a zeolite material, preferably a 12-membered ring-pore zeolite material, wherein the 12-membered ring-pore zeolite material is preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type BEA, wherein the 12-membered ring-pore zeolite material has a framework type BEA, wherein the framework structure of the zeolite material preferably comprises Si, Al, and O, more preferably consisting of Si, Al, and O, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1. The system according to any one of Embodiments 6 to 16, wherein the zeolite material preferably contains at least 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, copper calculated as CuO.

[0219] 18. The system of Embodiment 17, wherein the zeolite material contains at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, iron calculated as Fe2O3; or the zeolite material contains iron calculated as Fe2O3 in an amount preferably in the range of 0.5 to 8% by mass, and more preferably in the range of 1 to 5% by mass.

[0220] The system according to Embodiment 17 or 18, wherein the mass ratio of the non-zeolite oxide material of the DOC coating according to (i.3) to the zeolite material of the DOC coating according to (i.3) is in the range of 1:1 to 10:1, preferably in the range of 1.5:1 to 8:1, and more preferably in the range of 2:1 to 4.5:1.

[0221] 20. The catalyst according to (i) is coated with DOC according to (i.3) at a rate of 0.5-5 g / in 3 The range is preferably 0.75 to 4 g / in. 3 In the range of 1-3 g / in, more preferably 1-3 g / in 3 The range, more preferably 1.25 to 2.5 g / in 3 The system according to any one of embodiments 6 to 19, including a filling amount in the range of .

[0222] The system according to any one of Embodiments 6 to 20, wherein 95 to 100% by mass, preferably 98 to 100% by mass, more preferably 99 to 100% by mass, and more preferably 99.5 to 100% by mass of the DOC coating according to 21.(i.3) consists of a platinum group metal component, preferably a non-zeolite oxide material as defined in Embodiment 16, and preferably a zeolite material as defined in Embodiment 17 or 18.

[0223] The system according to any one of Embodiments 6 to 21, wherein the first substrate according to 22.(i.1) is a flow-through substrate or a wall-flow filter substrate, preferably a flow-through substrate, the flow-through substrate is preferably one or more of cordierite flow-through substrates and metal flow-through substrates, more preferably a metal flow-through substrate, the first substrate is preferably cylindrical, the diameter of the first substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and the first substrate has an axial length preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches. The catalyst according to 23.(i) is the system according to any one of Embodiments 6 to 22, comprising (i.1), (i.2), and (i.3).

[0224] Gas heating component 24. (ii) Gas heating components are, (ii.1) A second substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the second substrate, and an inner wall of the second substrate extending therethrough; Here, the inlet end of the second substrate according to (ii.1) and the outlet end of the first substrate according to (i.1) are coupled so that the exhaust gas exiting the passage of the first substrate enters the passage of the second substrate; The system according to any one of Embodiments 1 to 23, preferably any one of Embodiments 4 to 23, more preferably any one of Embodiments 6 to 23, wherein the inner wall of the second substrate is thermally conductive to allow heating therein in order to heat the exhaust gas flowing through the passage of the second substrate.

[0225] The system according to Embodiment 24, wherein the second substrate according to 25.(ii.1) is a flow-through substrate, preferably a metal flow-through substrate, and more preferably a metal electrically and / or thermally conductive flow-through substrate.

[0226] The system according to Embodiment 24 or 25, wherein the second substrate according to 26.(ii.1) is cylindrical in shape, and the diameter of the second substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and more preferably the diameter of the second substrate is in the range of 90 to 110% of the diameter of the first substrate as defined in Embodiment 23, preferably in the range of 95 to 105%, more preferably in the range of 98 to 102%, and the second substrate according to (ii.1) has an axial length preferably in the range of 0.15 to 2 inches, more preferably in the range of 0.20 to 1.5 inches, more preferably in the range of 0.30 to 1 inch.

[0227] The system according to any one of embodiments 24 to 26, wherein the gas heating component according to 27.(ii) consists of a second substrate according to (ii.1), and the substrate is an uncoated substrate.

[0228] The gas heating component according to 28.(ii) is (ii.2) Optionally, a NOx adsorbent coating disposed on the surface of the inner wall of the second substrate over at least 50% of the substrate axial length of the second substrate, wherein the NOx adsorbent coating comprises a platinum group metal component and a 10-membered ring-pore zeolite material having a framework type selected from the group consisting of FER, TON, MTT, SZR, MWW, AEL, HEU, AFO, two or more mixtures thereof and two or more mixed types thereof, (ii.3) A diesel oxidation catalyst (DOC) coating that is at least partially disposed on the surface of the inner wall of the second substrate and / or at least partially disposed on any NOx adsorbent coating according to (ii.2), and extending over at least 70% of the substrate axis length of the second substrate, wherein the DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania, The system according to any one of embodiments 24 to 26, further including the following.

[0229] The NOx adsorbent coating according to 29.(ii.2) is applied to the surface of the inner wall of the second substrate over an area of ​​70-100%, preferably 80-100%, more preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axial length of the second substrate. The NOx adsorbent coating according to (ii.2) is preferably placed on the surface of the inner wall of the second substrate from the outlet end to the inlet of the second substrate, in the system according to Embodiment 28.

[0230] 30. - The platinum group metal component of the NOx adsorbent coating according to (ii.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the platinum group metal component more preferably comprises palladium, and more preferably palladium, where the NOx adsorbent coating according to (ii.2) comprises a platinum group metal component, preferably calculated as a Pd element, preferably palladium, in a concentration of 30 to 300 g / ft 3 The range is more preferably 45-200 g / ft 3 A comfortable range of 60-150 g / ft 3 A comfortable range of 60-100 g / ft 3 range or 100-150g / ft 3 In the range of 60-80 g / ft, more preferably 60-80 g / ft 3 The range is 100-140g / ft 3 Contains within the range of filling amounts; - The platinum group metal component of the NOx adsorbent coating according to (ii.2) is preferably contained in the 10-membered ring-pore zeolite material of the NOx adsorbent coating according to (ii.2), where the platinum group metal component is preferably present in the zeolite material in an amount ranging from 0.5 to 10% by mass, more preferably from 1 to 6% by mass, more preferably from 1.25 to 4% by mass, and more preferably from 1.5 to 3% by mass, based on the total mass of the 10-membered ring-pore zeolite material of the NOx adsorbent coating according to (ii.2); - The 10-membered ring-pore zeolite material coated with NOx adsorbent according to (ii.2) preferably has a framework type selected from the group consisting of FER, TON, mixtures thereof, and mixed forms thereof, and more preferably the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (ii.2) has a framework type FER, where the framework structure of the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (ii.2) preferably contains a tetravalent element Y, a trivalent element X, and oxygen, and more preferably a tetravalent element It consists of element Y, trivalent element X, and oxygen, where Y is preferably one or more of Si, Sn, Ti, Zr, and Ge, more preferably Si, and X is preferably one or more of Al, B, In, and Ga, more preferably Al, and the molar ratio of Y:X calculated as YO2:X2O3 is preferably in the range of 2:1 to 100:1, more preferably in the range of 10:1 to 55:1, more preferably in the range of 12:1 to 40:1, more preferably in the range of 15:1 to 28:1, and more preferably in the range of 18:1 to 25:1; - The NOx adsorbent coating according to (ii.2) comprises a 10-membered ring-pore zeolite material in an amount based on the mass of the NOx adsorbent coating according to (ii.2), preferably in the range of 80 to 99.75% by mass, more preferably in the range of 85 to 99.5% by mass, more preferably in the range of 90 to 99.25% by mass, and more preferably in the range of 95 to 99% by mass; - The gas heating component according to (ii) is preferably 0.5 to 8 g / in 3 The range is more preferably 1-5 g / in 3 The range is, more preferably 1.5 to 4.5 g / in 3 In the range of 2-4 g / in 3 The NOx adsorbent coating is included in the packing amount within the range of (ii.2); - 95-100% by mass, more preferably 98-100% by mass, more preferably 99-100% by mass, and more preferably 99.5-100% by mass of the NOx adsorbent coating according to (ii.2) consist of a platinum group metal component and a 10-membered ring pore zeolite material. The system according to Embodiment 28 or 29.

[0231] 31. The DOC coating according to (ii.3) is at least partially disposed on the inner wall surface of the second substrate and / or at least partially disposed on any NOx adsorbent coating according to (ii.2), extending over 80 to 100%, preferably 95 to 100%, more preferably 98 to 100%, more preferably 99 to 100% of the substrate axial length of the first substrate, and the DOC according to (ii.3) is preferably at least partially disposed on the inner wall surface of the second substrate and / or at least partially disposed on the NOx adsorbent coating according to (ii.2) from the inlet end to the outlet end of the first substrate, the system according to any one of embodiments 28 to 30.

[0232] 32. - The platinum group metal component of the DOC coating according to (ii.3) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, more preferably platinum, and the DOC coating according to (ii.3) comprises a platinum group metal component, preferably calculated as element Pt, preferably platinum, in a quantity of 15 to 200 g / ft 3 A comfortable range is 20-150 g / ft 3 Comfortably within the range of 30-100g / ft 3 In the range of 40-90 g / ft, more preferably 40-90 g / ft 3 In the range of 50-80 g / ft, more preferably 50-80 g / ft 3 The platinum group metal components of the DOC coating according to (ii.3) are more preferably supported on the non-zeolite oxide material according to (ii.3) in a filling amount in the range of 1 to 5 mass%, more preferably in the range of 2 to 4 mass%, based on the total mass of the non-zeolite oxide material according to (ii.3); The platinum group metal component of the DOC coating according to (ii.3) more preferably comprises platinum and palladium, where the mass ratio of platinum to palladium, Pt:Pd, calculated as elements, is more preferably in the range of 1:1 to 11:1, more preferably in the range of 2:1 to 10:1, more preferably in the range of 3:1 to 5:1, and the mass ratio is more preferably about 4:1; - The non-zeolite oxide material of the DOC coating according to (ii.3) preferably comprises one or more of alumina, silica, and zirconia, more preferably one or more of alumina and silica, more preferably alumina, more preferably gamma-alumina, the non-zeolite oxide material preferably further comprises one or more of manganese, silicon, and zirconium, the non-zeolite oxide material more preferably comprises alumina and manganese, and the non-zeolite oxide material of the DOC coating according to (ii.3) preferably comprises alumina in an amount in the range of 80 to 99% by mass, more preferably 85 to 98% by mass, and more preferably 90 to 97% by mass, based on the mass of the non-zeolite oxide material; (ii.3) The non-zeolite oxide material for the DOC coating is more preferably 75m 2 More than / g, more preferably 100m 2 The non-zeolite oxide material exhibiting a BET specific surface area greater than / g and DOC coating according to (ii.3) is more preferably 0.04 cm². 3 More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g; - The DOC coating according to (ii.3) preferably further comprises a zeolite material, more preferably a 12-membered ring-pore zeolite material, wherein the 12-membered ring-pore zeolite material is preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed forms thereof, more preferably has a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed forms thereof, more preferably the 12-membered ring-pore zeolite material has a framework type BEA, the framework structure of the zeolite material preferably comprises Si, Al, and O, more preferably consists of Si, Al, and O, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably Or the ratio is in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, more preferably in the range of 20:1 to 26:1, and the zeolite material preferably contains at least 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, copper calculated as CuO; the zeolite material preferably contains at least 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, iron calculated as Fe2O3; or the zeolite material preferably contains an amount of iron calculated as Fe2O3 in the range of 0.5 to 8% by mass, and more preferably 1 to 5% by mass; - The mass ratio of the non-zeolite oxide material in the DOC coating according to (ii.3) to the zeolite material in the DOC coating according to (ii.3) is preferably in the range of 1:1 to 10:1, more preferably in the range of 1.5:1 to 8:1, and more preferably in the range of 2:1 to 4.5:1; - The gas heating component according to (ii) applies the DOC coating according to (ii.3), preferably at a rate of 0.5 to 5 g / in 3 The range is, more preferably 0.75 to 4 g / in 3 In the range of 1-3 g / in, more preferably 1-3 g / in 3 The range, more preferably 1.25 to 2.5 g / in3 Contains within the range of filling amounts; - The system according to any one of Embodiments 28 to 31, wherein preferably 95 to 100% by mass, more preferably 98 to 100% by mass, more preferably 99 to 100% by mass, and more preferably 99.5 to 100% by mass of the DOC coating according to (ii.3) consists of a platinum group metal component, a non-zeolite oxide material, and preferably a zeolite material as defined in Embodiment 17 or 18.

[0233] The system according to any one of Embodiments 28 to 32, wherein the gas heating component according to 33.(ii) consists of (ii.1) and (ii.3), and the gas heating component according to (ii) preferably consists of (ii.1), (ii.2), and (ii.3).

[0234] A system according to any one of Embodiments 28 to 33, wherein the DOC coating according to 34.(ii.3) exhibits essentially the same, preferably the same, chemical and physical properties as the DOC coating according to (i.3), and preferably the coating of the gas heating component according to (ii) exhibits essentially the same, preferably the same, chemical and physical properties as the coating of the catalyst according to (i).

[0235] 35. The system according to any one of embodiments 24 to 34, wherein the exit end of the first substrate and the inlet end of the second substrate are located on opposite sides of each other, and the angle between the surface normal defined by the exit end of the first substrate and the surface normal defined by the inlet end of the second substrate is preferably in the range of 0 to 5°, more preferably in the range of 0 to 3°, and more preferably in the range of 0 to 1°.

[0236] 36. The system according to Embodiment 35, wherein the exit end of the first substrate and the inlet end of the second substrate are spaced apart from each other, preferably in the range of 2 to 20 mm, preferably in the range of 5 to 15 mm, more preferably in the range of 8 to 12 mm, and the exit end of the first substrate and the inlet end of the second substrate are spaced apart from each other, preferably by one or more spacer means, preferably by one or more spacer rods, the given spacer rod is preferably fixed to either the exit end of the first substrate or the inlet end of the second substrate, or the exit end of the first substrate and the inlet end of the second substrate, and the one or more spacer means, preferably the one or more spacer rods, are preferably electrically insulating.

[0237] 37. The first substrate and the second substrate together form a single substrate including an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the single substrate, and a plurality of passages defined therethrough by the inner wall of the single substrate, wherein the DOC coating according to (i.3) and the DOC coating according to (ii.3) together form a single DOC coating, the single DOC coating preferably at least partially disposed on the NOx adsorbent coating according to (i.2), and the single DOC coating preferably extends over at least 90%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the single substrate; The first substrate and the second substrate together form a single substrate including an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the single substrate, and a plurality of passages defined therethrough by the inner wall of the single substrate; the NOx adsorbent coating according to (i.2) and the NOx adsorbent coating according to (ii.2) together form a single NOx adsorbent coating; and the DOC coating according to (i.3) and the DOC coating according to (ii.3) together form a single DOC coating; The single NOx adsorbent coating preferably extends over at least 50% of the substrate axial length of the single substrate, more preferably over 70% to 100%, more preferably over 80% to 100%, more preferably over 95% to 100%, more preferably over 98% to 100%, more preferably over 99% to 100%, and / or The system according to any one of embodiments 24 to 34, wherein the single DOC coating is preferably disposed at least partially on the single NOx adsorbent coating and preferably extends over at least 90% of the substrate axial length of the single substrate, more preferably over 95-100%, more preferably over 98-100%, and more preferably over 99-100%.

[0238] 38. The system according to any one of embodiments 24 to 37, further comprising a jacket surrounding a first substrate according to (i) and a second substrate according to (ii), wherein preferably 95 to 100%, more preferably 98 to 100%, more preferably 99 to 100% of the inlet end face of the first substrate and preferably 95 to 100%, more preferably 98 to 100%, more preferably 99 to 100% of the outlet end face of the second substrate are not covered by the jacket, wherein the jacket preferably includes one or more means for connecting the second substrate to a power source.

[0239] Second alternative arrangement 39. The system according to any one of Embodiments 1 to 3, wherein the DOC component is located downstream of the gas heating component.

[0240] 40. NOx adsorbent components, (i) A catalyst, (i.1) A first substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the first substrate, and the inner wall of the first substrate extending therethrough; (i.2) A NOx adsorbent coating disposed on the surface of the inner wall of the first substrate over at least 50% of the substrate axial length of the first substrate, wherein the NOx adsorbent coating comprises a platinum group metal component and a 10-membered ring-pore zeolite material having a framework type selected from the group consisting of FER, TON, MTT, SZR, MWW, AEL, HEU, AFO, two or more mixtures thereof and two or more mixed types thereof, The system according to embodiment 39, comprising a catalyst containing the following.

[0241] The NOx adsorbent coating according to 41.(i.2) is distributed on the surface of the inner wall of the first substrate over 70-100%, preferably 80-100%, more preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the first substrate, and the first NOx adsorbent coating according to (i.2) is preferably distributed on the surface of the inner wall of the first substrate from the inlet end to the outlet end of the first substrate, the system according to Embodiment 40.

[0242] The platinum group metal component of the NOx adsorbent coating according to 42.(i.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, wherein the platinum group metal component more preferably comprises palladium, and more preferably palladium, wherein the first NOx adsorbent coating according to (i.2) comprises a platinum group metal component calculated as a platinum group metal element, preferably as a Pd element, preferably palladium, in a concentration of 30 to 300 g / ft 3 The range is more preferably 45-200 g / ft 3 A comfortable range of 60-150 g / ft 3 A comfortable range of 60-100 g / ft 3 range or 100-150g / ft 3 In the range of 60-80 g / ft, more preferably 60-80 g / ft 3The range is 100-140g / ft 3 The system according to embodiment 40 or 41, including a filling amount within the range of [amount].

[0243] 43. The system according to any one of embodiments 40 to 42, wherein the platinum group metal component of the NOx adsorbent coating according to (i.2) is contained in the 10-membered ring-pore zeolite material of the NOx adsorbent coating according to (i.2), where the platinum group metal component is preferably present in the zeolite material in an amount ranging from 0.5 to 10% by mass, more preferably from 1 to 6% by mass, more preferably from 1.25 to 4% by mass, and more preferably from 1.5 to 3% by mass, based on the total mass of the 10-membered ring-pore zeolite material of the NOx adsorbent coating according to (i.2).

[0244] 44. The 10-membered ring-pore zeolite material coated with NOx adsorbent according to (i.2) has a framework type selected from the group consisting of FER, TON, mixtures thereof, and mixed forms thereof, more preferably the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (i.2) has a framework type FER, where the framework structure of the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (i.2) preferably comprises a tetravalent element Y, a trivalent element X, and oxygen, more preferably a tetravalent element Y, a trivalent element X, and oxygen The system according to any one of embodiments 40 to 43, wherein Y is preferably one or more of Si, Sn, Ti, Zr, and Ge, more preferably Si, and X is preferably one or more of Al, B, In, and Ga, more preferably Al, and the molar ratio of Y:X calculated as YO2:X2O3 is preferably in the range of 2:1 to 100:1, more preferably in the range of 10:1 to 55:1, more preferably in the range of 12:1 to 40:1, more preferably in the range of 15:1 to 28:1, and more preferably in the range of 18:1 to 25:1.

[0245] The NOx adsorbent coating according to 45.(i.2) comprises a 10-membered ring-pore zeolite material in an amount ranging from 80 to 99.75% by mass, preferably 85 to 99.5% by mass, more preferably 90 to 99.25% by mass, and more preferably 95 to 99% by mass, based on the mass of the NOx adsorbent coating, according to any one of Embodiments 40 to 44.

[0246] 46. ​​The catalyst according to (i) is coated with NOx adsorbent according to (i.2) at a rate of 0.5-8 g / in 3 In the range of 1 to 5 g / in 3 The range is, more preferably 1.5 to 4.5 g / in 3 In the range of 2-4 g / in 3 The system according to any one of embodiments 40 to 45, including a filling amount in the range of .

[0247] The system according to any one of Embodiments 40 to 46, wherein 95 to 100% by mass, preferably 98 to 100% by mass, more preferably 99 to 100% by mass, and more preferably 99.5 to 100% by mass of the NOx adsorbent coating according to 47.(i.2) consists of a platinum group metal component and a 10-membered ring pore zeolite material.

[0248] The system according to any one of Embodiments 40 to 47, wherein the first substrate according to 48.(i.1) is a flow-through substrate or a wall-flow filter substrate, preferably a flow-through substrate, wherein the flow-through substrate is preferably one or more of a cordierite flow-through substrate and a metal flow-through substrate, the first substrate according to (i.1) is preferably cylindrical, the diameter of the first substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and the first substrate according to (i.1) has an axial length preferably in the range of 0.5 to 8 inches, more preferably in the range of 1 to 5 inches, more preferably in the range of 1.25 to 3 inches.

[0249] The catalyst according to 49.(i) is a system according to any one of Embodiments 40 to 48, comprising a first substrate according to (i.1) and a NOx adsorbent coating according to (i.2).

[0250] 50. The DOC component is, (iii) A catalyst, (iii.1) A third substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the third substrate, and the inner wall of the third substrate extending therethrough; (iii.2) A first DOC coating disposed on the surface of the inner wall of the third substrate over at least 70% of the substrate axial length of the third substrate, wherein the first DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania, (iii.3) Optionally, a second DOC coating, at least partially disposed on the first DOC coating and extending over at least 20% of the substrate axial length of the third substrate, wherein the second DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania, and the second DOC coating preferably extends from the exit end to the inlet end of the third substrate. A system according to any one of embodiments 39 to 49, comprising a catalyst containing the following.

[0251] The system according to Embodiment 50, wherein the platinum group metal component of the first DOC coating according to 51.(iii.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, wherein the second platinum group metal component more preferably comprises platinum and palladium, more preferably platinum and palladium, and the mass ratio Pt:Pd of Pt to Pd calculated as elements Pt and Pd is preferably in the range of 0.5:1 to 5:1, more preferably in the range of 0.75:1 to 4.5:1, more preferably in the range of 1:1 to 4:1, and more preferably in the range of 1.5:1 to 3:1.

[0252] The non-zeolite oxide material according to 52.(iii.2) comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably silica-doped gamma-alumina, wherein the non-zeolite oxide material more preferably contains an amount of alumina in the range of 80-99% by mass, more preferably 85-95% by mass, and more preferably 88-90% by mass, based on the mass of the non-zeolite oxide material, and wherein the non-zeolite oxide material is more preferably 75m 2 More than / g, more preferably 100m 2 The non-zeolite oxide material exhibits a BET specific surface area greater than / g, and more preferably 0.04 cm². 3 More than 0.06 cm² / g 3 The system according to embodiment 50 or 51, exhibiting a pore volume exceeding / g.

[0253] The first DOC coating according to 53.(iii.2) further comprises a zeolite material, preferably a 12-membered ring-pore zeolite material, the 12-membered ring-pore zeolite material preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type BEA, and the framework structure of the zeolite material is preferably The system according to any one of Embodiments 50 to 52, comprising Si, Al and oxygen, more preferably consisting of Si, Al and oxygen, wherein the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1, and the zeolite material preferably contains copper calculated as CuO, preferably at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass.

[0254] 54. The system according to Embodiment 53, wherein the zeolite material contains at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, iron calculated as Fe2O3; or the zeolite material contains iron calculated as Fe2O3 in an amount preferably in the range of 0.5 to 8% by mass, and more preferably in the range of 1 to 5% by mass.

[0255] The system according to Embodiment 53 or 54, wherein the mass ratio of the non-zeolite oxide material of the first DOC coating according to 55.(iii.2) to the zeolite material of the first DOC coating according to (iii.2) is in the range of 1:1 to 10:1, preferably in the range of 1.5:1 to 8:1, and more preferably in the range of 2:1 to 4.5:1.

[0256] The catalyst according to 56.(iii) is used to coat the first DOC coating according to (iii.2) at a rate of 0.5-5 g / in. 3 The range is preferably 0.75 to 4 g / in. 3 In the range of 1-3 g / in, more preferably 1-3 g / in 3 The range, more preferably 1.25 to 2.5 g / in 3 The system according to any one of embodiments 50 to 55, including a filling amount in the range of .

[0257] The system according to any one of Embodiments 50 to 56, wherein 98 to 100% by mass, preferably 99 to 100% by mass, more preferably 99.5 to 100% by mass of the first DOC coating according to 57.(iii.2) consists of a platinum group metal component, preferably Pt and Pd, preferably a non-zeolite oxide material as defined in Embodiment 52, and preferably a zeolite material as defined in Embodiment 53 or 54.

[0258] The system according to any one of Embodiments 50 to 57, wherein the first DOC coating according to 58.(iii.2) extends over 80 to 100% of the substrate axial length of the third substrate according to (iii.1), preferably over 90 to 100%, more preferably over 95 to 100%, more preferably over 98 to 100%, and more preferably over 99 to 100%.

[0259] The catalyst according to 59.(iii) is a system according to any one of Embodiments 50 to 58, comprising a second DOC coating according to (iii.3).

[0260] The platinum group metal component of the second DOC coating according to 60.(iii.3) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the second platinum group metal component more preferably comprises platinum and palladium, more preferably platinum and palladium, and the mass ratio of Pt to Pd calculated as elements Pt and Pd, Pt:Pd, is preferably in the range of 2:1 to 20:1, more preferably in the range of 3:1 to 8:1, more preferably in the range of 4:1 to 7.5:1, and more preferably in the range of 5:1 to 7:1; Here, the platinum group metal component of the second DOC coating according to (iii.3) more preferably comprises platinum, where the second DOC coating according to (iii.3) contains platinum calculated as element Pt, preferably in an amount of 15 to 200 g / ft. 3 A comfortable range is 20-150 g / ft 3 Comfortably within the range of 30-100g / ft 3 In the range of 40-90 g / ft, more preferably 40-90 g / ft 3 In the range of 50-80 g / ft, more preferably 50-80 g / ft 3 The system according to Embodiment 59, comprising a filling amount in the range, where the platinum group metal component of the second DOC coating according to (iii.3) is more preferably calculated as an element based on the total mass of the non-zeolite oxide material according to (ii.3) and supported on the non-zeolite oxide material according to (iii.3) in a filling amount more preferably in the range of 1 to 5 mass%, more preferably in the range of 2 to 4 mass%.

[0261] The non-zeolite oxide material for the second DOC coating according to 61.(iii.3) comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably silica-doped gamma-alumina, and the non-zeolite oxide material for the second DOC coating according to (iii.3) preferably comprises an amount of alumina in the range of 80-99% by mass, more preferably 85-95% by mass, and more preferably 88-90% by mass, based on the mass of the non-zeolite oxide material, and the non-zeolite oxide material for the second DOC coating according to (iii.3) preferably comprises 75m 2 More than / g, more preferably 100m 2 The non-zeolite oxide material of the second DOC coating according to (iii.3) exhibits a BET specific surface area greater than / g, and is more preferably 0.04 cm². 3 More than 0.06 cm² / g 3 The system according to embodiment 59 or 60, exhibiting a pore volume exceeding / g.

[0262] The catalyst according to 62.(iii) is used for the second DOC coating according to (iii.3), with a concentration of 0.5-5 g / in. 3 The range is preferably 0.75 to 4 g / in. 3 The range is, more preferably 0.75 to 3 g / in 3 The range, more preferably 1.25 to 2.5 g / in 3 The system according to any one of embodiments 59 to 61, including a filling amount in the range of .

[0263] The system according to any one of Embodiments 59 to 62, wherein 98 to 100% by mass, preferably 99 to 100% by mass, more preferably 99.5 to 100% by mass of the second DOC coating according to 63.(iii.3) consists of platinum group metal components, preferably Pt and Pd, and a non-zeolite oxide material.

[0264] The second DOC coating according to 64.(iii.3) extends over 30 to 100% of the substrate axial length of the third substrate according to (iii.1), preferably over 35 to 80%, more preferably over 40 to 60%, and more preferably over 45 to 55%, as described in any one of Embodiments 59 to 63.

[0265] The system according to any one of embodiments 50 to 64, wherein the third substrate according to 65.(iii.1) is a flow-through substrate, preferably one or more of a cordierite flow-through substrate and a metal flow-through substrate, the third substrate according to (iii.1) is preferably cylindrical, the diameter of the third substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and the third substrate according to (iii.1) has an axial length preferably in the range of 1 to 10 inches, more preferably in the range of 1.5 to 7 inches, more preferably in the range of 2 to 5 inches.

[0266] The catalyst according to 66.(iii) comprises a third substrate according to (iii.1), a first DOC coating according to (iii.2), and preferably a second DOC coating according to (iii.3), as described in any one of Embodiments 50 to 65, preferably Embodiments 59 to 65.

[0267] Gas heating component 67. (ii) The gas heating component (ii.1) A second substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the second substrate, and an inner wall of the second substrate extending therethrough; Here, the inlet end of the second substrate according to (ii.1) and the outlet end of the first substrate according to (i.1) are coupled so that the gas exiting from the passage of the first substrate according to (i.1) can enter the passage of the second substrate according to (ii.1); Here, the inlet end of the third substrate according to (iii.1) and the outlet end of the second substrate according to (ii.1) are coupled so that the gas exiting the passage of the second substrate can enter the passage of the third substrate according to (iii.1); The system according to any one of embodiments 39 to 66, wherein the inner wall of the second substrate according to (ii.1) is thermally conductive to allow heating therein in order to heat the exhaust gas flowing through the passage of the second substrate.

[0268] The system according to Embodiment 67, wherein the second substrate according to 68.(ii.1) is a flow-through substrate, preferably a metal flow-through substrate, and more preferably a metal electrically and / or thermally conductive flow-through substrate.

[0269] The system according to Embodiment 67 or 68, wherein the second substrate according to 69.(ii.1) is cylindrical in shape, and the diameter of the second substrate is preferably in the range of 3 to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and more preferably the diameter of the second substrate is in the range of 90 to 110% of the diameter of the first substrate as defined in Embodiment 48, preferably in the range of 95 to 105%, more preferably in the range of 98 to 102%, and the second substrate according to (ii.1) has an axial length preferably in the range of 0.15 to 2 inches, more preferably in the range of 0.20 to 1.5 inches, more preferably in the range of 0.30 to 1 inch.

[0270] The system according to any one of embodiments 67 to 69, wherein the gas heating component according to 70.(ii) consists of a second substrate according to (ii.1), and the substrate is an uncoated substrate.

[0271] The gas heating component according to 71.(ii) is (ii.2) A first DOC coating disposed on the surface of the inner wall of the second substrate according to (ii.1) over at least 50% of the substrate axis length of the second substrate according to (ii.1), wherein the first DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania, (ii.3) A second DOC coating optionally disposed at least partially on the first DOC coating according to (ii.2) and extending over at least 50% of the substrate axis length of the second substrate according to (ii.1), wherein the second DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania, The system according to any one of embodiments 67 to 69, further including the following.

[0272] The platinum group metal component of the first DOC coating according to 72.(ii.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the second platinum group metal component more preferably comprises platinum and palladium, more preferably platinum and palladium, and the mass ratio Pt:Pd calculated as elements Pt and Pd is preferably in the range of 0.5:1 to 5:1, more preferably in the range of 0.75:1 to 4.5:1, more preferably in the range of 1:1 to 4:1, and more preferably in the range of 1.5:1 to 3:1. The platinum group metal component of the first DOC coating according to (ii.2) more preferably includes platinum, and the first DOC coating according to (ii.2) contains platinum calculated as element Pt, preferably in a quantity of 15 to 200 g / ft. 3 A comfortable range is 20-150 g / ft 3 Comfortably within the range of 30-100g / ft 3 In the range of 40-90 g / ft, more preferably 40-90 g / ft 3 In the range of 50-80 g / ft, more preferably 50-80 g / ft3 The platinum group metal components of the first DOC coating according to (ii.2) are more preferably calculated as elements based on the total mass of the non-zeolite oxide material according to (ii.2) and supported on the non-zeolite oxide material according to (ii.2) in a packing amount more preferably in the range of 1 to 5 mass%, more preferably in the range of 2 to 4 mass%, The non-zeolite oxide material according to (ii.2) preferably comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, more preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably silica-doped gamma-alumina, and the non-zeolite oxide material preferably comprises an amount of alumina in the range of 80 to 99% by mass, more preferably 85 to 95% by mass, and more preferably 88 to 90% by mass, based on the mass of the non-zeolite oxide material. The non-zeolite oxide material is more preferably 75m 2 More than / g, more preferably 100m 2 It exhibits a BET specific surface area exceeding / g, The non-zeolite oxide material is more preferably 0.04 cm 3 More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g, The first DOC coating according to (ii.2) preferably further comprises a zeolite material, preferably a 12-membered ring-pore zeolite material, wherein the 12-membered ring-pore zeolite material is preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed forms thereof, more preferably has a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed forms thereof, more preferably has a framework type BEA, and the zeolite material The framework structure preferably contains Si, Al, and oxygen, more preferably consisting of Si, Al, and oxygen, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1, and the zeolite material preferably contains copper calculated as CuO in an amount of at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass; The zeolite material preferably contains iron calculated as Fe2O3 in an amount of at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass; or the zeolite material preferably contains iron calculated as Fe2O3 in an amount in the range of 0.5 to 8% by mass, more preferably 1 to 5% by mass; The mass ratio of the non-zeolite oxide material of the first DOC coating according to (ii.2) to the zeolite material of the first DOC coating according to (ii.2) is preferably in the range of 1:1 to 10:1, more preferably in the range of 1.5:1 to 8:1, and more preferably in the range of 2:1 to 4.5:1. The gas heating component according to (ii) is coated with the first DOC coating according to (ii.2), preferably 0.5 to 5 g / in 3 The range is, more preferably 0.75 to 4 g / in 3 In the range of 1-3 g / in, more preferably 1-3 g / in 3The range, more preferably 1.25 to 2.5 g / in 3 It contains in a filling amount within the range, Preferably 98-100% by mass, more preferably 99-100% by mass, and more preferably 99.5-100% by mass of the first DOC coating according to (ii.2) consist of a platinum group metal component, preferably Pt and Pd, a non-zeolite oxide material, and preferably a zeolite material; The system according to Embodiment 71, wherein the first DOC coating according to (ii.2) extends over preferably 80-100%, more preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axial length of the second substrate according to (ii.1).

[0273] The gas heating component according to 73.(ii) is the system according to Embodiment 71 or 72, which includes a second DOC coating according to (ii.3).

[0274] The platinum group metal component of the second DOC coating according to 74.(ii.3) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the second platinum group metal component more preferably comprises platinum and palladium, and more preferably platinum and palladium, and the mass ratio Pt:Pd calculated as elements Pt and Pd is preferably in the range of 2:1 to 20:1, more preferably in the range of 3:1 to 8:1, more preferably in the range of 4:1 to 7.5:1, and more preferably in the range of 5:1 to 7:1; The non-zeolite oxide material of the second DOC coating according to (ii.3) preferably comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably silica-doped gamma-alumina; the non-zeolite oxide material of the second DOC coating according to (iii.3) preferably comprises alumina in an amount in the range of 80 to 99% by mass, more preferably 85 to 95% by mass, and more preferably 88 to 90% by mass, based on the mass of the non-zeolite oxide material; The non-zeolite oxide material is more preferably 75m 2 More than / g, more preferably 100m 2 It exhibits a BET specific surface area exceeding / g; The non-zeolite oxide material is more preferably 0.04 cm 3 More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g; The gas heating component according to (ii) is coated with a second DOC coating according to (ii.3), preferably 0.5 to 5 g / in 3 The range is, more preferably 0.75 to 4 g / in 3 The range is, more preferably 0.75 to 3 g / in 3 The range is, more preferably 1 to 2.5 g / in 3 Contains within the range of filling amounts; Preferably 98-100% by mass, more preferably 99-100% by mass, and more preferably 99.5-100% by mass of the second DOC coating according to (ii.3) consist of platinum group metal components, preferably Pt and Pd, and a non-zeolite oxide material; The system according to Embodiment 73, wherein the second DOC coating according to (ii.3) extends over preferably 30-100%, preferably 35-80%, more preferably 40-60%, and more preferably 45-55% of the substrate axial length of the second substrate according to (ii.1).

[0275] The gas heating component according to 75.(ii) comprises a second substrate according to (ii.1), a first DOC coating according to (ii.2), and preferably a second DOC coating according to (ii.3), as described in any one of embodiments 67 to 74, preferably embodiments 72 to 74.

[0276] The system according to any one of Embodiments 67 to 75, wherein the coating of the gas heating component according to 76.(ii) exhibits essentially the same, preferably the same, chemical and physical properties as the coating of the catalyst according to (iii).

[0277] 77. The second substrate according to (ii.1) and the third substrate according to (iii.1) together form one single substrate including an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the single substrate, and a plurality of passages defined by the inner wall of the single substrate extending therethrough; the first DOC coating according to (ii.2) and the first DOC coating according to (iii.2) together form one single first DOC coating; preferably the second DOC coating according to (ii.3) and the second DOC coating according to (iii.3) together form one A system according to any one of embodiments 67 to 76, which forms a single second DOC coating; the single first DOC coating preferably extends over at least 90% of the substrate axial length of the single substrate, more preferably over 95-100%, more preferably over 98-100%, and more preferably over 99-100%, and preferably the single second DOC coating preferably extends over at least 40% of the substrate axial length of the single substrate, more preferably over 45-100%, and more preferably over 50-80%.

[0278] 78. The system according to any one of embodiments 67 to 77, wherein the exit end of the second substrate and the inlet end of the third substrate are arranged opposite to each other, and the angle between the surface normal of the surface defined by the exit end of the second substrate and the surface normal of the surface defined by the inlet end of the third substrate is preferably in the range of 0 to 5°, more preferably in the range of 0 to 3°, and more preferably in the range of 0 to 1°.

[0279] 79. The system according to Embodiment 78, wherein the exit end of the second substrate and the inlet end of the third substrate are spaced apart from each other, preferably by a distance of 2 to 20 mm, preferably by a distance of 5 to 15 mm, more preferably by a distance of 8 to 12 mm, and the exit end of the second substrate and the inlet end of the third substrate are spaced apart from each other, preferably by one or more spacer means, preferably by one or more spacer rods, and the given spacer rod is preferably fixed to either the exit end of the second substrate or the inlet end of the third substrate, or the exit end of the second substrate and the inlet end of the third substrate, and the one or more spacer means, preferably the one or more spacer rods, are preferably electrically insulating.

[0280] SCR component 80. The SCR component is, (iv) A selective catalytic reduction (SCR) catalyst, (iv.1) A fourth substrate, which includes an inlet end, an outlet end, and a substrate axis length extending from the inlet end to the outlet end of the fourth substrate, preferably a wall flow filter substrate; (iv.2) A selective catalytic reduction (SCR) coating is applied to the surface of the inner wall of the fourth substrate according to (iv.1), It is included in selective catalytic reduction (SCR) catalysts; The system according to any one of Embodiments 1 to 79, wherein the inlet end of a fourth substrate according to (iv.1) and the outlet end of a second substrate according to (ii.1) in the range in which Embodiment 80 refers to any one of Embodiments 24 to 38, or the outlet end of a third substrate according to (iii.1) in the range in which Embodiment 80 refers to any one of Embodiments 50 to 79, are coupled so that exhaust gases exiting the passage of the second substrate or exhaust gases exiting the passage of the third substrate enter the fourth substrate.

[0281] The system according to Embodiment 80, wherein the SCR coating according to 81(iv.2) comprises an 8-membered ring-pore zeolite material containing one or more copper and iron, preferably copper, and the amount of one or more copper and iron calculated as CuO and Fe2O3, respectively, more preferably the amount of copper calculated as CuO, is in the range of 1 to 10 mass%, preferably in the range of 2 to 8 mass%, more preferably in the range of 3 to 6 mass%, based on the mass of the 8-membered ring-pore zeolite material containing one or more copper and iron.

[0282] 82. The system according to Embodiment 81, wherein the 8-membered ring-pore zeolite material of the selective catalytic reduction coating is selected from the group consisting of CHA, AEI, RTH, LEV, DDR, KFI, ERI, AFX, two or more mixtures thereof, and two or more mixed forms thereof, preferably selected from the group consisting of CHA, AEI, RTH, two or more mixtures thereof, and two or more mixed forms thereof, more preferably selected from the group consisting of CHA and AEI, and more preferably the 8-membered ring-pore zeolite material of the selective catalytic reduction coating has a framework type CHA.

[0283] 83. The framework structure of the eight-membered ring-pore zeolite material comprises a tetravalent element Y, a trivalent element X and O, preferably consisting of a tetravalent element Y, a trivalent element X and O, where Y is one or more of Si, Sn, Ti, Zr and Ge, and X is one or more of Al, B, In and Ga, and the molar ratio of Y:X calculated as YO2:X2O3 is in the range of 2:1 to 45:1, preferably in the range of 10:1 to 40:1, more preferably in the range of 15:1 to 30:1, where Y preferably comprises Si, more preferably Si, and X preferably comprises one or more of Al and B, more preferably Al and B, and preferably Al, the system of Embodiment 81 or 82.

[0284] 84. A system according to any one of Embodiments 1 to 83, comprising a NOx adsorbent component, a DOC component, an SCR component, and a gas heating component.

[0285] System preparation method 85. A method for preparing a system for treating exhaust gases of a diesel internal combustion engine, preferably a method for preparing a system for treating exhaust gases of a diesel internal combustion engine according to any one of Embodiments 1 to 84, wherein the method is (1) To provide NOx adsorbent components, diesel oxidation catalyst (DOC) components, selective catalytic reduction (SCR) components, gas heating components, and reducing agent injectors, The aforementioned NOx adsorbent component is (i) A catalyst, (i.1) A first substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the first substrate, and the inner wall of the first substrate extending therethrough; (i.2) NOx adsorbent coating which is the NOx adsorbent component, wherein the coating is disposed on the surface of the inner wall of the first substrate over at least 50% of the substrate axial length of the first substrate, and the NOx adsorbent coating comprises a platinum group metal component and a 10-membered ring-pore zeolite material having a framework type selected from the group consisting of FER, TON, MTT, SZR, MWW, AEL, HEU, AFO, two or more mixtures thereof and two or more mixed types thereof, It is included in catalysts containing, (2) Placing the NOx adsorbent component upstream of the gas heating component, (3) The reducing agent injector is placed upstream of the SCR component, (4) The gas heating component is placed upstream of the reducing agent injector, (5) The DOC component is placed upstream of the reducing agent injector, (6) Arranging the DOC component and the gas heating component in a direct and continuous order, Methods that include...

[0286] The method according to Embodiment 85, wherein no other components for treating exhaust gas are placed between the DOC component according to 86.(1) and the gas heating component according to (1).

[0287] 87. The method according to Embodiment 85 or 86, wherein the components are preferably arranged in a continuous sequence in an exhaust gas conduit, and the upstream end of the conduit is preferably designed to be located downstream of a diesel internal combustion engine, and more preferably the upstream end of the conduit is located downstream of a diesel internal combustion engine.

[0288] 88. The method according to any one of embodiments 85 to 87, wherein the DOC component is located upstream of the gas heating component, and the DOC component and the NOx adsorbent component are preferably located upstream of the gas heating component.

[0289] 89. The DOC component and the NOx adsorbent component are contained in the catalyst, and the catalyst is prepared by the following method and / or method, (a) To provide a NOx adsorbent mixture comprising a first substrate, water, a source of platinum group metal components, and a 10-membered ring-pore zeolite material, (b) The NOx adsorbent mixture obtained in (a) is placed on the surface of the inner wall of a first substrate, which has an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the first substrate, and a plurality of passages defined by the inner wall of the first substrate extending through thereto over at least 50% of the substrate axis length of the first substrate. (c) Optionally, the coated substrate obtained in (b) is fired in a gas atmosphere having a temperature preferably in the range of 400 to 800°C, preferably in the range of 450 to 700°C, more preferably in the range of 550 to 650°C, wherein the gas atmosphere is preferably air. Here, prior to firing in (c), the first NOx adsorbent mixture placed on the first substrate is dried in a gas atmosphere having a temperature in the range of 90 to 150°C, preferably in the range of 100 to 120°C, for a period of preferably 0.5 to 4 hours, more preferably in the range of 0.75 to 2 hours, wherein the gas atmosphere is preferably air; and here, prior to firing in (c), the coated substrate obtained in (b) is dried in a gas atmosphere having a temperature in the range of 90 to 150°C, more preferably in the range of 100 to 120°C, wherein the gas atmosphere is more preferably air. (d) To provide a diesel oxidation catalyst (DOC) mixture comprising water, a source of platinum group metal components, and a non-zeolite oxide material containing one or more of alumina, silica, zirconia, and titania, and preferably a zeolite material, The diesel oxide mixture obtained in (e)(d) is placed on the first substrate, which includes a NOx adsorbent coating obtained by (b) or (c) and placed thereon, over at least 70% of the substrate axial length of the first substrate, where the coated substrate is dried in a gas atmosphere having a temperature preferably in the range of 90 to 150°C, more preferably in the range of 100 to 120°C, the gas atmosphere is preferably air, and the dried substrate is fired in a gas atmosphere having a temperature preferably in the range of 400 to 800°C, more preferably in the range of 450 to 700°C, more preferably in the range of 550 to 650°C, for preferably 0.25 to 5 hours; to obtain a first substrate including a NOx adsorbent coating and a diesel oxide coating placed thereon, The method according to any one of embodiments 85 to 88, further including the method described above.

[0290] 90. The method according to Embodiment 89, wherein the NOx adsorbent mixture is disposed on the surface of the inner wall of the first substrate in (b) over a length of 70-100%, preferably 80-100%, more preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the first substrate, and the first NOx adsorbent mixture is preferably disposed on the surface of the inner wall of the first substrate from the inlet end to the outlet end of the first substrate in (b).

[0291] The method according to Embodiment 89 or 90, wherein the platinum group metal component of the NOx adsorbent mixture according to 91.(a) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, wherein the platinum group metal component more preferably comprises palladium, and more preferably palladium.

[0292] The method according to any one of Embodiments 89 to 90, wherein a 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to 92(a) is impregnated with a source of platinum group metal components of the NOx adsorbent mixture according to (a), the impregnation of which is preferably carried out by mixing the 10-membered ring-pore zeolite material with a source of platinum group metal components, preferably a palladium source, more preferably an aqueous solution of palladium nitrate, and the impregnated 10-membered ring-pore zeolite material is preferably dispersed in water.

[0293] The 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to 93.(a) has a framework type selected from the group consisting of FER, TON, mixtures thereof, and mixed types thereof, more preferably the 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (a) has a framework type FER, and the framework structure of the 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (a) preferably comprises a tetravalent element Y, a trivalent element X, and oxygen, more preferably consisting of a tetravalent element Y, a trivalent element X, and oxygen, where Y is preferred The method according to any one of embodiments 89 to 92, wherein Mashi is one or more of Si, Sn, Ti, Zr, and Ge, more preferably Si, X is one or more of Al, B, In, and Ga, more preferably Al, and the molar ratio of Y:X calculated as YO2:X2O3 is preferably in the range of 2:1 to 100:1, more preferably in the range of 10:1 to 55:1, more preferably in the range of 12:1 to 40:1, more preferably in the range of 15:1 to 28:1, and more preferably in the range of 18:1 to 25:1.

[0294] The method according to any one of embodiments 89 to 93, wherein the DOC mixture according to 94.(d) is obtained by (b) or (c) and is distributed on the first substrate including a NOx adsorbent coating placed thereon over 80 to 100%, preferably 90 to 100%, more preferably 95 to 100%, more preferably 98 to 100%, more preferably 99 to 100% of the substrate axis length of the first substrate, and the DOC according to (d) is preferably obtained by (b) or (c) and is distributed on the first substrate including a NOx adsorbent coating placed thereon from the inlet end to the outlet end of the first substrate.

[0295] The method according to any one of Embodiments 89 to 94, wherein the platinum group metal component of the DOC mixture according to 95.(d) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, more preferably platinum, and the non-zeolite oxide material according to (d) is more preferably impregnated with the platinum group metal component of the DOC mixture according to (d).

[0296] The method according to any one of Embodiments 89 to 95, wherein the non-zeolite oxide material of the DOC mixture according to 96.(d) comprises one or more of alumina, silica and zirconia, preferably one or more of alumina and silica, more preferably alumina, more preferably gamma-alumina, the non-zeolite oxide material preferably further comprises one or more of manganese, silicon and zirconium, the non-zeolite oxide material more preferably comprises alumina and manganese, and the non-zeolite oxide material of the DOC mixture according to (d) more preferably comprises alumina in an amount in the range of 80 to 99% by mass, more preferably in the range of 85 to 98% by mass, and more preferably in the range of 90 to 97% by mass, based on the mass of the non-zeolite oxide material.

[0297] The DOC mixture according to 97.(d) further comprises a zeolite material, preferably a 12-membered ring-pore zeolite material, wherein the 12-membered ring-pore zeolite material is preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type BEA, wherein the 12-membered ring-pore zeolite material has a framework type BEA, wherein the framework structure of the zeolite material preferably comprises Si, Al, and O, more preferably consisting of Si, Al, and O, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1. The method according to any one of Embodiments 89 to 96, wherein the zeolite material preferably contains at least 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, copper calculated as CuO.

[0298] The method according to any one of embodiments 89 to 97, wherein the first substrate according to 98.(a) is a flow-through substrate or a wall-flow filter substrate, preferably a flow-through substrate, wherein the flow-through substrate is preferably one or more of cordierite flow-through substrates and metal flow-through substrates, more preferably a metal flow-through substrate, wherein the first substrate is preferably cylindrical, the diameter of the first substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and the first substrate has an axial length preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches.

[0299] A gas heating component according to 99.(1) comprises a second substrate, which includes a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the second substrate, and an inner wall of the second substrate extending through therethe The inlet end of the second substrate and the outlet end of the first substrate are coupled according to (a) so that exhaust gas exiting the passage of the first substrate enters the passage of the second substrate; The method according to any one of embodiments 89 to 98, wherein the inner wall of the second substrate is thermally conductive to allow heating therein in order to heat the exhaust gas flowing through the passage of the second substrate.

[0300] 100. The method according to Embodiment 99, wherein the second substrate is a flow-through substrate, preferably a metal flow-through substrate, and more preferably a metal electrically and / or thermally conductive flow-through substrate.

[0301] 101. The method according to Embodiment 99 or 100, wherein the second substrate is preferably cylindrical in shape, the diameter of the second substrate is preferably in the range of 3 to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, more preferably the diameter of the second substrate is in the range of 90 to 110% of the diameter of the first substrate as defined in Embodiment 23, preferably in the range of 95 to 105%, more preferably in the range of 98 to 102%, and the second substrate has an axial length preferably in the range of 0.15 to 2 inches, more preferably in the range of 0.20 to 1.5 inches, more preferably in the range of 0.30 to 1 inch.

[0302] The gas heating component according to 102.(1) is prepared by and / or the method is (g.1) Optionally, a NOx adsorbent mixture is placed on the surface of the inner wall of the second substrate over at least 50% of the substrate axial length of the second substrate, wherein the NOx adsorbent mixture comprises a source of platinum group metal components and a 10-membered ring-pore zeolite material having a framework type selected from the group consisting of FER, TON, MTT, SZR, MWW, AEL, HEU, AFO, two or more mixtures thereof and two or more mixed types thereof; (g.2) Placing a diesel oxidation catalyst (DOC) mixture over at least 70% of the substrate shaft length of the second substrate on the surface of the inner wall of the second substrate and / or on the NOx adsorbent coating of the substrate obtained from (g.1), wherein the DOC mixture comprises a source of platinum group metal components and a source of non-zeolite oxide material containing one or more of alumina, silica, zirconia and titania, The method according to any one of embodiments 99 to 101, further including the method described above.

[0303] The NOx adsorbent mixture according to 103.(g.1) is distributed on the surface of the inner wall of the second substrate over an area of ​​70-100%, preferably 80-100%, more preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the second substrate. Herein, the NOx adsorbent mixture according to (g.1) is preferably placed on the surface of the inner wall of the second substrate from the outlet end to the inlet end of the second substrate, according to the method of Embodiment 102.

[0304] 104. - The platinum group metal component of the NOx adsorbent mixture according to (g.1) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, wherein the platinum group metal component more preferably comprises palladium, and more preferably palladium; - The 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (g.1) is preferably impregnated with a source of platinum group metal components of the NOx adsorbent mixture according to (g.1); - The 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (g.1) preferably has a framework type selected from the group consisting of FER, TON, mixtures thereof and mixed types thereof, and more preferably the 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (g.1) has a framework type FER, where the framework structure of the 10-membered ring-pore zeolite material of the NOx adsorbent mixture according to (g.1) preferably comprises a tetravalent element Y, a trivalent element X and oxygen, and more preferably from a tetravalent element Y, a trivalent element X and oxygen. The method according to Embodiment 102 or 103, wherein Y is preferably one or more of Si, Sn, Ti, Zr, and Ge, more preferably Si, and X is preferably one or more of Al, B, In, and Ga, more preferably Al, and the molar ratio of Y:X calculated as YO2:X2O3 is preferably in the range of 2:1 to 100:1, more preferably in the range of 10:1 to 55:1, more preferably in the range of 12:1 to 40:1, more preferably in the range of 15:1 to 28:1, and more preferably in the range of 18:1 to 25:1.

[0305] The method according to any one of embodiments 102 to 104, wherein the DOC mixture according to 105.(g.2) is distributed on the surface of the inner wall of the second substrate and / or on the NOx adsorbent coating of the substrate obtained by (g.1) over 80 to 100%, preferably 90 to 100%, more preferably 95 to 100%, more preferably 98 to 100%, and more preferably 99 to 100% of the substrate axis length of the first substrate, and the DOC mixture according to (g.2) is preferably distributed from the inlet end to the outlet end of the first substrate on the surface of the inner wall of the second substrate and / or on the NOx adsorbent coating of the substrate obtained by (g.1). The method according to any one of embodiments 102 to 105, wherein the DOC mixture according to 106.(g.2) is placed on the surface of the inner wall of the second substrate and / or on the NOx adsorbent coating of the substrate obtained by (g.1) over 80 to 100%, preferably 90 to 100%, more preferably 95 to 100%, more preferably 98 to 100%, and more preferably 99 to 100% of the substrate axis length of the first substrate, and the DOC mixture according to (g.2) is preferably placed on the surface of the inner wall of the second substrate and / or on the NOx adsorbent coating of the substrate obtained by (g.1) from the inlet end to the outlet end of the first substrate.

[0306] 107. - The platinum group metal component of the DOC mixture according to (g.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, more preferably platinum, and the non-zeolite oxide material according to (g.2) is more preferably impregnated with a source of platinum group metal component of the DOC mixture according to (g.2); - The source of the non-zeolite oxide material for the DOC coating according to (g.2) preferably comprises one or more of alumina, silica, and zirconia, preferably one or more of alumina and silica, more preferably alumina, more preferably gamma-alumina, the source of the non-zeolite oxide material preferably further comprises one or more of manganese, silicon, and zirconium, the source of the non-zeolite oxide material more preferably comprises alumina and manganese, and the source of the non-zeolite oxide material for the DOC mixture according to (g.2) more preferably comprises alumina in an amount in the range of 80-99% by mass, more preferably 85-98% by mass, and more preferably 90-97% by mass, based on the mass of the non-zeolite oxide material; - The DOC mixture according to (g.2) preferably further comprises a zeolite material, more preferably a 12-membered ring-pore zeolite material, the 12-membered ring-pore zeolite material preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type BEA for the 12-membered ring-pore zeolite material, the framework structure of the zeolite material preferably comprises Si, Al, and O, more preferably consisting of Si, Al, and O, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1 The range is, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1; the zeolite material preferably contains at least 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, copper calculated as CuO; the zeolite material preferably contains at least 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass, iron calculated as Fe2O3; or the method according to any one of embodiments 102 to 106, wherein the zeolite material contains iron calculated as Fe2O3 in an amount preferably in the range of 0.5 to 8% by mass, and more preferably in the range of 1 to 5% by mass.

[0307] 108. The method according to any one of embodiments 99 to 107, wherein the exit end of the first substrate and the inlet end of the second substrate are arranged facing each other, and the angle between the surface normal of the surface defined by the exit end of the first substrate and the surface normal of the surface defined by the inlet end of the second substrate is preferably in the range of 0 to 5°, more preferably in the range of 0 to 3°, and more preferably in the range of 0 to 1°.

[0308] 109. The method according to Embodiment 108, wherein the exit end of the first substrate and the inlet end of the second substrate are spaced apart from each other, preferably by a distance of 2 to 20 mm, preferably by a distance of 5 to 15 mm, more preferably by a distance of 8 to 12 mm, the exit end of the first substrate and the inlet end of the second substrate are spaced apart from each other, preferably by one or more spacer means, preferably by one or more spacer rods, the given spacer rod is preferably fixed to either the exit end of the first substrate or the inlet end of the second substrate, or the exit end of the first substrate and the inlet end of the second substrate, and the one or more spacer means, preferably the one or more spacer rods, are preferably electrically insulating.

[0309] 110. A single substrate is used together as the first substrate and the second substrate, and the single substrate includes a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the single substrate, and an inner wall of the single substrate extending therethrough, wherein the NOx adsorbent mixture according to (b) is placed on the surface of the inner wall of the single substrate, and the coated substrate is subjected to a gas atmosphere having a temperature preferably in the range of 90 to 150°C, more preferably in the range of 100 to 120°C, for a period preferably in the range of 0.5 to 4 hours, more preferably in the range of 0.75 to 2 hours. The substrate is dried, the gas atmosphere is preferably air, the dried substrate is fired in a gas atmosphere having a temperature preferably in the range of 400 to 800°C, preferably in the range of 450 to 700°C, more preferably in the range of 550 to 650°C for a period of preferably in the range of 0.25 to 5 hours, preferably in the range of 0.5 to 2 hours, the gas atmosphere is preferably air, and the DOC mixture according to (d) and the DOC mixture according to (g.2) are at least partially placed on the single substrate coated with a single NOx adsorbent coating to form a single DOC coating; Here, the NOx adsorbent coating is preferably distributed over at least 50% of the substrate axis length of the single substrate, more preferably over 70-100%, more preferably over 80-100%, more preferably over 95-100%, more preferably over 98-100%, more preferably over 99-100%, and / or The single DOC coating is preferably applied at least partially to the surface of the inner wall of the single substrate and / or the NOx adsorbent coating over at least 90%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axial length of the single substrate; the coated substrate is preferably dried in a gas atmosphere having a temperature in the range of 90-150°C, more preferably 100-120°C, for a period of preferably 0.5-4 hours, and preferably 0.75-2 hours, wherein the gas atmosphere is preferably air; the dried substrate is preferably fired in a gas atmosphere having a temperature in the range of 400-800°C, more preferably 450-700°C, and more preferably 550-650°C, for a period of preferably 0.25-5 hours, and preferably 0.5-2 hours, wherein the gas atmosphere is preferably air; More preferably, one single substrate is used together as the first substrate and the second substrate, and the single substrate includes an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the single substrate, and a plurality of passages defined therethrough by the inner wall of the single substrate, wherein the NOx adsorbent mixture according to (b) and the NOx adsorbent mixture according to (g.1) are placed on the inner wall of the single substrate to form a single NOx adsorbent coating, and the coated substrate is preferably heated in a gas atmosphere having a temperature in the range of 90 to 150°C, more preferably in the range of 100 to 120°C, for a range of 0.5 to 4 hours. The substrate is dried for a period of preferably 0.75 to 2 hours, the gas atmosphere being preferably air, the dried substrate is calcined for a period of preferably 0.25 to 5 hours, preferably 0.5 to 2 hours, in a gas atmosphere having a temperature of preferably 400 to 800°C, preferably 450 to 700°C, more preferably 550 to 650°C, the gas atmosphere being preferably air, and the DOC mixture according to (d) and the DOC mixture according to (g.2) are at least partially placed on the single substrate coated with a single NOx adsorbent coating to form a single DOC coating; A single NOx adsorbent coating is preferably distributed over at least 50% of the substrate axial length of the single substrate, more preferably over 70-100%, more preferably over 80-100%, more preferably over 95-100%, more preferably over 98-100%, more preferably over 99-100%, and / or The single DOC coating is preferably placed at least partially on the surface of the inner wall of the single substrate and / or on the single NOx adsorbent coating over at least 90%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axial length of the single substrate, the coated substrate is preferably dried in a gas atmosphere having a temperature in the range of 90-150°C, more preferably 100-120°C for a period of preferably 0.5-4 hours, more preferably 0.75-2 hours, wherein the gas atmosphere is preferably air, and the dried substrate is preferably fired in a gas atmosphere having a temperature in the range of 400-800°C, more preferably 450-700°C, more preferably 550-650°C for a period of preferably 0.25-5 hours, more preferably 0.5-2 hours, wherein the gas atmosphere is preferably air, according to any one of embodiments 99 to 109.

[0310] The method according to any one of embodiments 99 to 110, wherein the first substrate and the second substrate according to 111.(a) are surrounded by a jacket, and preferably 95 to 100%, more preferably 98 to 100%, more preferably 99 to 100% of the inlet end face of the first substrate and preferably 95 to 100%, more preferably 98 to 100%, more preferably 99 to 100% of the outlet end face of the second substrate are not covered by the jacket, wherein the jacket preferably includes one or more means for connecting the second substrate to a power source.

[0311] 112. The method according to any one of embodiments 85 to 87, wherein the DOC component is located downstream of the gas heating component.

[0312] 113. The catalyst contains the NOx adsorbent component, and the catalyst is prepared by the following, and / or the method is (n.1) To provide a first substrate, which includes an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the first substrate, and a plurality of passages defined by the inner wall of the first substrate extending therethrough; (n.2) Placing a NOx adsorbent mixture on the surface of the inner wall of the first substrate over at least 50% of the substrate axial length of the first substrate, wherein the NOx adsorbent mixture comprises a source of platinum group metal components and a 10-membered ring-pore zeolite material, the coated substrate is dried in a gas atmosphere having a temperature preferably in the range of 90 to 150°C, more preferably in the range of 100 to 120°C, for a period preferably in the range of 0.5 to 4 hours, more preferably in the range of 0.75 to 2 hours, the gas atmosphere is preferably air, and the dried substrate is calcined in a gas atmosphere having a temperature preferably in the range of 400 to 800°C, more preferably in the range of 450 to 700°C, more preferably in the range of 550 to 650°C, for a period preferably in the range of 0.25 to 5 hours, more preferably in the range of 0.5 to 2 hours, the gas atmosphere is preferably air; The method according to embodiment 112, further comprising:

[0313] The method according to Embodiment 113, wherein the NOx adsorbent mixture according to 114.(n.2) is disposed on the surface of the inner wall of the first substrate over a length of 70-100%, preferably 80-100%, more preferably 90-100%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axis length of the first substrate, and the first NOx adsorbent mixture according to (n.2) is preferably disposed on the surface of the inner wall of the first substrate from the inlet end to the outlet end of the first substrate.

[0314] The method according to Embodiment 113 or 114, wherein the platinum group metal component of the NOx adsorbent coating according to 115(n.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, wherein the platinum group metal component more preferably comprises palladium, and more preferably palladium, and wherein the platinum group metal component of the NOx adsorbent coating according to (n.2) is preferably impregnated into a 10-membered ring-pore zeolite material.

[0315] 116. The 10-membered ring-pore zeolite material coated with NOx adsorbent according to (n.2) has a framework type selected from the group consisting of FER, TON, mixtures thereof, and mixed forms thereof, more preferably the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (n.2) has a framework type FER, and the framework structure of the 10-membered ring-pore zeolite material coated with NOx adsorbent according to (n.2) preferably comprises a tetravalent element Y, a trivalent element X, and oxygen, more preferably from a tetravalent element Y, a trivalent element X, and oxygen. The method according to any one of embodiments 113 to 115, wherein Y is preferably one or more of Si, Sn, Ti, Zr, and Ge, more preferably Si, and X is preferably one or more of Al, B, In, and Ga, more preferably Al, and the molar ratio of Y:X calculated as YO2:X2O3 is preferably in the range of 2:1 to 100:1, more preferably in the range of 10:1 to 55:1, more preferably in the range of 12:1 to 40:1, more preferably in the range of 15:1 to 28:1, and more preferably in the range of 18:1 to 25:1.

[0316] The method according to any one of embodiments 113 to 116, wherein the first substrate according to 117(n.1) is a flow-through substrate or a wall-flow filter substrate, preferably a flow-through substrate, wherein the flow-through substrate is preferably one or more of a cordierite flow-through substrate and a metal flow-through substrate, the first substrate according to (n.1) is preferably cylindrical, the diameter of the first substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and the first substrate according to (n.1) has an axial length preferably in the range of 0.5 to 8 inches, more preferably in the range of 1 to 5 inches, more preferably in the range of 1.25 to 3 inches.

[0317] 118. The DOC component is contained in the catalyst, the catalyst is prepared by and / or the method is (d.1) To provide a third substrate, comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the third substrate, and the inner wall of the third substrate extending through thereto; (d.2) Placing a first DOC mixture on the surface of the inner wall of the third substrate over at least 70% of the substrate axial length of the third substrate, wherein the first DOC mixture comprises a source of platinum group metal components and a source of non-zeolite oxide material containing one or more of alumina, silica, zirconia and titania; (d.3) Optionally, a second DOC mixture is placed on the third substrate coated with the first DOC mixture over at least 20% of the substrate axial length of the third substrate, wherein the second DOC mixture comprises a source of platinum group metal components and a source of non-zeolite oxide material comprising one or more of alumina, silica, zirconia, and titania, and the second DOC coating preferably comprises the placement of the second DOC mixture from the exit end to the inlet end of the third substrate. The method according to any one of embodiments 113 to 117, further including the method described above.

[0318] The method according to Embodiment 118, wherein the platinum group metal component of the first DOC mixture according to 119.(d.2) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the second platinum group metal component more preferably comprises platinum and palladium, and more preferably platinum and palladium.

[0319] The source of the non-zeolite oxide material according to 120.(d.2) comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably silica-doped gamma-alumina, wherein the non-zeolite oxide material more preferably contains an amount of alumina in the range of 80-99% by mass, more preferably 85-95% by mass, and more preferably 88-90% by mass, based on the mass of the non-zeolite oxide material, and wherein the non-zeolite oxide material is more preferably 75m 2 More than / g, more preferably 100m 2 The non-zeolite oxide material exhibits a BET specific surface area greater than / g, and more preferably 0.04 cm². 3 More than 0.06 cm² / g 3 The method according to Embodiment 118 or 119, which exhibits a pore volume exceeding / g.

[0320] The first DOC coating according to 121.(d.2) further comprises a zeolite material, preferably a 12-membered ring-pore zeolite material, the 12-membered ring-pore zeolite material preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof, and two or more mixed forms thereof, more preferably having a framework type BEA, and the framework structure of the zeolite material is preferably The method according to any one of Embodiments 118 to 120, wherein the zeolite material contains Si, Al, and oxygen, more preferably consisting of Si, Al, and oxygen, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1, and the zeolite material contains copper calculated as CuO, preferably at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass.

[0321] The method according to any one of Embodiments 118 to 121, wherein the first DOC mixture according to 122.(d.2) is distributed over 80-100% of the substrate axial length of the third substrate according to (d.1), preferably over 90-100%, more preferably over 95-100%, more preferably over 98-100%, and more preferably over 99-100%.

[0322] 123. The method according to any one of embodiments 118 to 122, wherein the second DOC mixture is placed on the third substrate coated with the first DOC mixture according to (d.3).

[0323] The method according to Embodiment 123, wherein the source of the platinum group metal component of the second DOC mixture according to 124.(d.3) comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, where the source of the second platinum group metal component more preferably comprises platinum and palladium, and more preferably platinum and palladium.

[0324] The non-zeolite oxide material of the second DOC mixture according to 125.(d.3) comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably silica-doped gamma-alumina, wherein the non-zeolite oxide material of the second DOC mixture according to (d.3) preferably contains alumina in an amount in the range of 80-99% by mass, more preferably 85-95% by mass, and more preferably 88-90% by mass, based on the mass of the non-zeolite oxide material, and the non-zeolite oxide material is more preferably 75m 2 More than / g, more preferably 100m 2 The method according to Embodiment 123 or 124, which exhibits a BET specific surface area greater than / g.

[0325] The method according to any one of Embodiments 123 to 125, wherein the second DOC mixture according to 126.(d.3) is distributed over 30 to 100%, preferably over 35 to 80%, more preferably over 40 to 60%, and more preferably over 45 to 55% of the substrate axial length of the third substrate according to (d.1).

[0326] The method according to any one of embodiments 123 to 126, wherein the third substrate according to 127.(d.1) is a flow-through substrate, preferably one or more of a cordierite flow-through substrate and a metal flow-through substrate, the third substrate according to (d.1) is preferably cylindrical, the diameter of the third substrate is preferably in the range of 3 inches to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and the third substrate according to (d.1) has an axial length preferably in the range of 1 to 10 inches, more preferably in the range of 1.5 to 7 inches, more preferably in the range of 2 to 5 inches.

[0327] 128. The gas heating component is (g.1') A second substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the second substrate, and the inner wall of the second substrate extending therethrough; Here, the inlet end of the second substrate by (g.1') and the outlet end of the first substrate by (n.1) are coupled such that the gas exiting the passage of the first substrate by (n.1) enters the passage of the second substrate by (g.1'); The inlet end of the third substrate according to (d.1) and the outlet end of the second substrate according to (g.1') are coupled so that the gas exiting the passage of the second substrate can enter the passage of the third substrate according to (d.1); The method according to any one of embodiments 113 to 127, wherein the inner wall of the second substrate according to (g.1') is thermally conductive to allow heating therein in order to heat the exhaust gas flowing through the passage of the second substrate.

[0328] The method according to Embodiment 128, wherein the second substrate according to 129.(g.1') is a flow-through substrate, preferably a metal flow-through substrate, and more preferably a metal electrically and / or thermally conductive flow-through substrate.

[0329] The method according to Embodiment 128 or 129, wherein the second substrate according to 130.(g.1') is cylindrical in shape, and the diameter of the second substrate is preferably in the range of 3 to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and more preferably the diameter of the second substrate is in the range of 90 to 110% of the diameter of the first substrate as defined in Embodiment 48, preferably in the range of 95 to 105%, more preferably in the range of 98 to 102%, and the second substrate according to (g.1') has an axial length preferably in the range of 0.15 to 2 inches, more preferably in the range of 0.20 to 1.5 inches, more preferably in the range of 0.30 to 1 inch.

[0330] 131. (g.2') The first DOC mixture is placed on the surface of the inner wall of the second substrate according to (g.1') over at least 70% of the substrate shaft length of the second substrate according to (g.1'), wherein the first DOC mixture comprises a source of platinum group metal components and a source of non-zeolite oxide material containing one or more of alumina, silica, zirconia, and titania. (g.3') Optionally, placing a second DOC mixture on a second substrate coated with the first DOC mixture according to (g.2') over at least 70% of the substrate axial length of the second substrate according to (g.1'), wherein the second DOC mixture comprises a source of platinum group metal components and a source of non-zeolite oxide material containing one or more of alumina, silica, zirconia, and titania. The method according to any one of embodiments 128 to 130, further including the method described above.

[0331] The method according to Embodiment 131, wherein the second substrate according to 132.(g.1') is a flow-through substrate, preferably a metal flow-through substrate, and more preferably a metal electrically and / or thermally conductive flow-through substrate.

[0332] The method according to Embodiment 131 or 132, wherein the second substrate according to 133.(g.1') is cylindrical in shape, and the diameter of the second substrate is preferably in the range of 3 to 10 inches, more preferably in the range of 3.5 to 8 inches, more preferably in the range of 4 to 6 inches, and more preferably the diameter of the second substrate is in the range of 90 to 110% of the diameter of the first substrate as defined in Embodiment 48, preferably in the range of 95 to 105%, more preferably in the range of 98 to 102%, and the second substrate according to (g.1') has an axial length preferably in the range of 0.15 to 2 inches, more preferably in the range of 0.20 to 1.5 inches, more preferably in the range of 0.30 to 1 inch.

[0333] 134. The gas heating component is prepared by and / or the method is (g.2') The first DOC mixture is placed on the surface of the inner wall of the second substrate according to (g.1') over at least 70% of the substrate shaft length of the second substrate according to (g.1'), wherein the first DOC mixture comprises a source of platinum group metal components and a source of non-zeolite oxide material containing one or more of alumina, silica, zirconia, and titania. (g.3') Preferably, the second DOC mixture is placed on a second substrate coated with the first DOC mixture according to (g.2') over at least 70% of the substrate axial length of the second substrate according to (g.1'), wherein the second DOC mixture comprises a source of platinum group metal components and a source of non-zeolite oxide material containing one or more of alumina, silica, zirconia, and titania. The method according to any one of embodiments 131 to 133, further including the method described above.

[0334] The source of the platinum group metal component in the first DOC mixture according to 135.(g.2') comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum, and the source of the platinum group metal component comprises more preferably platinum and palladium, and more preferably platinum and palladium; The source of the non-zeolite oxide material according to (g.2') preferably comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, more preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably silica-doped gamma-alumina, and the source of the non-zeolite oxide material preferably comprises an amount of alumina in the range of 80-99% by mass, more preferably 85-95% by mass, and more preferably 88-90% by mass, based on the mass of the non-zeolite oxide material. The source of the non-zeolite oxide material is more preferably 75m 2 More than / g, more preferably 100m 2 It exhibits a BET specific surface area exceeding / g; The source of the non-zeolite oxide material is more preferably 0.04 cm 3 More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g; The first DOC mixture according to (g.2') further preferably comprises a zeolite material, more preferably a 12-membered ring-pore zeolite material, the 12-membered ring-pore zeolite material preferably selected from the group consisting of BEA, FAU, USY, GME, MOR, OFF, two or more mixtures thereof and two or more mixed forms thereof, more preferably having a framework type selected from the group consisting of BEA, USY, FAU, two or more mixtures thereof and two or more mixed forms thereof, more preferably having a framework type BEA of the 12-membered ring-pore zeolite material, and the frame of the zeolite material The zeolite material preferably contains Si, Al, and oxygen, more preferably consisting of Si, Al, and oxygen, and the molar ratio of Si:Al calculated as SiO2:Al2O3 is preferably in the range of 2:1 to 1200:1, more preferably in the range of 10:1 to 400:1, more preferably in the range of 15:1 to 100:1, more preferably in the range of 18:1 to 30:1, and more preferably in the range of 20:1 to 26:1, and the zeolite material preferably contains copper calculated as CuO in an amount of at most 0.001% by mass, more preferably 0 to 0.0001% by mass, and more preferably 0 to 0.00001% by mass; The method according to Embodiment 134, wherein the first DOC mixture according to (g.2') is distributed over 80-100% of the substrate axial length of the second substrate according to (g.1'), preferably over 90-100%, more preferably over 95-100%, more preferably over 98-100%, and more preferably over 99-100%.

[0335] 136. The gas heating component comprises a second DOC coating by (g.3') as described in Embodiment 135.

[0336] The source of the platinum group metal component of the second DOC mixture according to 137.(g.3') comprises one or more of palladium, platinum, rhodium, iridium, osmium, and ruthenium, preferably one or more of palladium, platinum, and rhodium, more preferably one or more of palladium and platinum. The source of the non-zeolite oxide material for the second DOC mixture according to (g.3') preferably comprises one or more of alumina, silica, zirconia, silica-alumina, alumina-zirconia, and silica-zirconia, more preferably one or more of alumina, silica, and silica-alumina, more preferably silica-alumina, and more preferably silica-doped gamma-alumina; the non-zeolite oxide material for the second DOC coating according to (g.3') preferably comprises alumina in an amount in the range of 80-99% by mass, more preferably 85-95% by mass, and more preferably 88-90% by mass, based on the mass of the non-zeolite oxide material; The source of the non-zeolite oxide material is more preferably 75m 2 More than / g, more preferably 100m 2 It exhibits a BET specific surface area exceeding / g; The source of the non-zeolite oxide material is more preferably 0.04 cm 3 More than 0.06 cm² / g 3 It exhibits a pore volume exceeding / g; The second DOC mixture according to (g.3') is preferably distributed over 30-100% of the substrate shaft length of the second substrate according to (g.1'), preferably over 35-80%, more preferably over 40-60%, and more preferably over 45-55%. The method according to Embodiment 136.

[0337] 138. The method according to any one of embodiments 128 to 137, wherein the coating of the gas heating component exhibits essentially the same, preferably the same, chemical and physical properties as the coating of the catalyst defined in any one of embodiments 118 to 127.

[0338] 139. A single substrate is used to form a second substrate according to (g.1') and a third substrate according to (d.1), wherein the single substrate includes a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the single substrate, and an inner wall of the single substrate extending therethrough, wherein a first DOC mixture according to (g.2') and a first DOC mixture according to (d.2) are arranged together to form a single first DOC coating, and preferably a second DOC mixture according to (g.3') and a second DOC mixture according to (d.3) are arranged together The method according to any one of embodiments 128 to 138, wherein a single second DOC coating is formed by being arranged on a single substrate; a single first DOC mixture is arranged over preferably at least 90%, more preferably 95-100%, more preferably 98-100%, and more preferably 99-100% of the substrate axial length of the single substrate; and preferably, a single second DOC mixture is arranged over preferably at least 40%, more preferably 45-100%, and more preferably 50-80% of the substrate axial length of the single substrate.

[0339] 140. The method according to any one of embodiments 128 to 139, wherein the exit end of the second substrate and the inlet end of the third substrate are arranged opposite to each other, and the angle between the surface normal of the surface defined by the exit end of the second substrate and the surface normal of the surface defined by the inlet end of the third substrate is preferably in the range of 0 to 5°, more preferably in the range of 0 to 3°, and more preferably in the range of 0 to 1°.

[0340] 141. The method according to Embodiment 140, wherein the exit end of the second substrate and the inlet end of the third substrate are spaced apart from each other, preferably in the range of 2 to 20 mm, preferably in the range of 5 to 15 mm, more preferably in the range of 8 to 12 mm, and the exit end of the second substrate and the inlet end of the third substrate are spaced apart from each other, preferably by one or more spacer means, preferably by one or more spacer rods, the given spacer rod is preferably fixed to either the exit end of the second substrate or the inlet end of the third substrate, or the exit end of the second substrate and the inlet end of the third substrate, and the one or more spacer means, preferably the one or more spacer rods, are preferably electrically insulating.

[0341] 142. A selective catalytic reduction (SCR) catalyst is provided as the SCR component, and the selective catalytic reduction (SCR) catalyst is, (s.1) To provide a fourth substrate, preferably a wall flow filter substrate, which includes an inlet end, an outlet end, and a substrate axis length extending from the inlet end to the outlet end of the third substrate; (s.2) A selective catalytic reduction (SCR) mixture is placed on the fourth substrate according to (s.1); Prepared by, The method according to any one of embodiments 85 to 141, wherein the inlet end of the fourth substrate according to (s.1), the outlet end of the second substrate according to (s.1) in the range in which Embodiment 142 refers to any one of embodiments 99 to 111, or the outlet end of the third substrate according to (d.1) in the range in which Embodiment 142 refers to any one of embodiments 118 to 141 is coupled so that exhaust gases exiting the passage of the second substrate enter the third substrate.

[0342] The method according to Embodiment 142, wherein the SCR mixture according to 143.(s.2) comprises an 8-membered ring porous zeolite material containing one or more of copper and iron, preferably copper, and the amount of one or more of copper and iron calculated as CuO and Fe2O3, respectively, more preferably the amount of copper calculated as CuO, is in the range of 1 to 10% by mass, preferably 2 to 8% by mass, more preferably 3 to 6% by mass, based on the mass of the 8-membered ring porous zeolite material containing one or more of copper and iron.

[0343] 144. The method according to Embodiment 143, wherein the 8-membered ring-pore zeolite material of the selective catalytic reduction coating is selected from the group consisting of CHA, AEI, RTH, LEV, DDR, KFI, ERI, AFX, two or more mixtures thereof, and two or more mixed forms thereof, preferably selected from the group consisting of CHA, AEI, RTH, two or more mixtures thereof, and two or more mixed forms thereof, more preferably selected from the group consisting of CHA and AEI, and more preferably the 8-membered ring-pore zeolite material of the selective catalytic reduction coating has framework-type CHA.

[0344] The framework structure of the 145.8-membered ring-pore zeolite material comprises a tetravalent element Y, a trivalent element X and O, preferably consisting of a tetravalent element Y, a trivalent element X and O, where Y is one or more of Si, Sn, Ti, Zr and Ge, and X is one or more of Al, B, In and Ga, and the molar ratio of Y:X calculated as YO2:X2O3 is in the range of 2:1 to 45:1, preferably in the range of 10:1 to 40:1, more preferably in the range of 15:1 to 30:1, where Y preferably comprises Si, more preferably Si, and X preferably comprises one or more of Al and B, more preferably Al and B, preferably Al, according to Embodiment 142 or 143.

[0345] 146. The method according to any one of embodiments 85 to 145, wherein the reducing agent injector comprises one or more of a hydrocarbon injector, a hydrocarbon cylinder post-injector, and a urea injector, preferably a urea injector, and preferably consists of one or more of a hydrocarbon injector, a hydrocarbon cylinder post-injector, and a urea injector, preferably a urea injector, and the reducing agent injector is preferably positioned downstream of the DOC component.

[0346] 147. A system for treating exhaust gases of a diesel internal combustion engine, preferably a system for treating exhaust gases of a diesel internal combustion engine as described in any one of embodiments 1 to 84, which can be obtained or obtained by the method described in any one of embodiments 85 to 146.

[0347] 148. A method for treating exhaust gases from a diesel internal combustion engine, comprising providing exhaust gases from a diesel internal combustion engine and passing the exhaust gases through a system described in any one of embodiments 1 to 84 or 147.

[0348] 149. The method according to Embodiment 148, wherein one or more reducing agents, more preferably hydrocarbons and urea, are injected into the exhaust gas passing through the system via a reducing agent injector.

[0349] 150. The method according to Embodiment 148 or 149, wherein the exhaust gas is heated via a gas heating component included in the system for heating one or more of the SCR component, DOC component, and NA adsorbent component included in the system. 151. Use of a system according to any one of embodiments 1 to 84 or 147 for treating exhaust gases of a diesel internal combustion engine, wherein the use includes passing the exhaust gases through the system. [Examples]

[0350] The present invention is further illustrated by the following reference examples, comparative examples, and embodiments. Examples Reference example 1 1.1 Volume-based particle size distribution, especially Dv 10 Dv 50 Dv 90 Determining the value The volume-based particle size distribution was determined by static light scattering using state-of-the-art equipment, where the optical density of the sample was in the range of 5–10 mass%.

[0351] 1.2 Measurement of BET Specific Surface Area The BET specific surface area was determined using liquid nitrogen in accordance with DIN 66131 or DIN ISO 9277.

[0352] 1.3 Determination of Crystallinity The relative crystallinity of the zeolite was measured by X-ray diffraction using a test method under the jurisdiction of ASTM Committee D32 on Catalysts, and specifically Subcommittee D32.05 on Zeolites. The current version was approved on March 10, 2001, and published in May 2001, originally published as D 5758-95.

[0353] Reference Example 2: Preparation of NOx adsorbent using DOC functional catalyst (layered catalyst-FER) Bottom coating: Ammonium ferrielite (framework structure type FER, SiO2:Al2O3 molar ratio of 21, crystallinity versus standard (XRD) greater than 80%) zeolite material was wet-impregnated with an aqueous palladium nitrate solution, achieving a 2.31 mass% Pd loading based on the mass of the final material (zeolite material + palladium) dispersed in water. An uncoated flow-through metal substrate (total volume 1.81 L, 400 cpsi, wall thickness 40 micrometers, cylindrical, diameter 5.2 inches × length 5.3 inches) was immersed in the resulting slurry over 100% of the substrate's axial length to form a bottom coating. The coated substrate was dried in air at 110°C for 1 hour, and then calcined in air at 590°C for 2 hours to form a bottom coating. The palladium loading of the bottom coating was 120 g / ft. 3 The total bottom coating load is 3g / in 3 That was the case.

[0354] Top coat: A highly porous gamma-alumina support material containing 5% by mass MnO2 (calculated as MnO2, 95% by mass Al2O3, 5% by mass Mn) was impregnated with a stabilized platinum complex solution by wet impregnation, achieving a 3.2% by mass Pt loading based on the mass of the final material (Mn-alumina + platinum). Ammonium beta-zeolite material (BEA, SiO2:Al2O3 molar ratio of 23, crystallinity versus standard (XRD) greater than 90%) was added to the Pt-alumina mixture. The mass ratio of Mn-doped alumina to beta-zeolite material was 3.14:1. The substrate coated with the bottom coating was coated with the obtained slurry over 100% of the substrate axial length. The coated substrate was dried in air at a temperature of 110°C for 1 hour, and then calcined in air at 590°C for 2 hours to form a top coating. The platinum loading in the top coat was 60 g / ft 3 The total top coat load is 1.45 g / in. 3 The catalyst for Reference Example 1 is shown in Figure 3 (including any SCRoF(2)).

[0355] Example 3: Gas heating component As the electrically heated substrate, and therefore as the gas heated component, an uncoated flow-through metal substrate with a total capacity of 0.164 L, a diameter of 5.66 inches × length of 0.4 inches, a pressure of 130 cpsi, and a wall thickness of 50 micrometers was used. The substrate was electrically heatable, and a voltage of 48 V was used in Examples 1 and Comparative Example 1, and a voltage of 12 V was used in Examples 4 and 5 and Comparative Examples 2 and 3.

[0356] Comparative Example 1: Preparation of NOx adsorbent (NA-) having a DOC functional catalyst (layered catalyst-FER on a substrate including an upstream heating substrate) The catalyst of Comparative Example 1, which is not according to the present invention, was prepared by applying a Pd-FER slurry upstream to a substrate made of an uncoated electrically heated substrate (total volume 0.164 L, 48 volts, diameter: 5.7 inches × length: 0.4 inches, 130 cpsi, wall thickness 50 micrometers) electrically connected to an uncoated flow-through metal substrate (total volume 1.85 L, 400 cpsi, wall thickness 40 micrometers, diameter: 5.7 inches × length: 4.45 inches) downstream, similar to the one prepared in Reference Example 2 for bottom coating. The coated substrate was dried in air at a temperature of 110°C for 1 hour, and then calcined in air at 590°C for 2 hours to form a bottom coating. The bottom coating covered 100% of the substrate shaft length. Furthermore, a Pt / Mn-alumina / BEA slurry similar to that prepared in Reference Example 2 was applied to the substrate coated with the bottom coating, covering 100% of the substrate shaft length. The coated substrate was dried in air at a temperature of 110°C for 1 hour, and then fired in air at a temperature of 590°C for 2 hours to form a top coat. The catalyst for Comparative Example 1 is shown in Figure 3 (where an arbitrary SCRoF2 is present).

[0357] Example 1: Preparation of NOx adsorbent (NA-) having a DOC functional catalyst (layered catalyst-FER on a substrate including a downstream heating substrate) The catalyst of Example 1 according to the present invention was prepared by applying a Pd-FER slurry upstream to a substrate made of an uncoated flow-through metal substrate (total volume 1.81 L, 400 cpsi, wall thickness 40 micrometers, diameter 5.7 inches × length 4.45 inches) connected downstream to an uncoated electrically heated flow-through metal substrate (total volume 0.164 L, 48 volts, diameter: 5.7 inches × length: 0.4 inches, 130 cpsi, wall thickness 50 micrometers), similar to the one prepared in Reference Example 2 for the bottom coating. The coated substrate was dried in air at a temperature of 110°C for 1 hour, and then calcined in air at 590°C for 2 hours to form a bottom coating. The bottom coating covered 100% of the substrate shaft length. Furthermore, a Pt / Mn-alumina / BEA slurry similar to the one prepared in Reference Example 2 was applied to the substrate coated with the bottom coating, covering 100% of the substrate shaft length. The coated substrate was dried in air at a temperature of 110°C for 1 hour, and then fired in air at a temperature of 590°C for 2 hours to form a top coat. The catalyst for Example 1 is shown in Figure 3 (where an arbitrary SCRoF2 is present).

[0358] Example 2: Testing of the NA-DOC catalyst from Reference Example 2 - Simulated low-temperature city driving cycle, NOx adsorption evaluation The catalyst from Reference Example 2 was aged at 800°C for 16 hours in 10% vapor / air, and then tested in a 2L diesel engine under a simulated low-temperature city driving mode. The driving cycle was compiled from the city driving mode of the New European Driving Cycle (NEDC). The average temperature of the cycle was approximately 170°C. The cycle was driven twice for 1880 seconds. This test was performed using the SCR catalyst article downstream of the NOx adsorbent-DOC sample from Reference Example 2 described above. The SCR catalyst article contains Cu-CHA coated on a filter substrate. An injector for urea administration was applied between the NOx adsorbent-DOC article and the SCR catalyst article to deliver the reducing agent for the SCR reaction. The test system is shown in Figure 3. Prior to the first test, the temperature of the NOx adsorbent-DOC sample was raised to 650°C for 10 minutes.

[0359] Figure 1 shows the test results from the initial test run. All formulations were observed in the NO emissions from the engine for approximately 500 seconds. x It is adsorbing. Figure 2 shows the test results of the second driving test. The second test drive showed that the exhaust of the test system had insufficient NOx handshake in the downstream SCR of the NA-DOC in Reference Example 2, meaning that the NOx desorbed from the NA-DOC was not completely converted by the downstream SC.

[0360] Example 3: Testing of catalysts from Reference Example 2, Comparative Example 1, and Example 1 in a system - WLTC evaluation in a diesel engine The catalysts of Reference Example 2, Comparative Example 1, and Example 1 were aged at 800°C for 16 hours in 10% vapor / air, and then tested in a 3L diesel engine using the Worldwide Harmonized Fuel Economy and Exhaust Gas Test Cycle (WLTC) for passenger cars, etc. Prior to the first test, the temperature of the NOx adsorbent sample was raised to 650°C for 10 minutes to remove pre-adsorbed NOx.

[0361] The catalysts of Reference Example 2, Comparative Example 1, and Example 1 were evaluated using a downstream SCR catalyst. The SCR catalyst article contained Cu-CHA (SCRoF) coated on a filter substrate. A urea injector was applied between the sample (components including NOx adsorbent and DOC functions) and the SCR catalyst article to deliver the reducing agent for the SCR reaction. The test system is shown in Figure 3.

[0362] In Comparative Example 1 and Example 1, the electric heating element was turned on for 450 seconds immediately after the start of WLTC. After another 50 seconds, the heating element was started again for 400 seconds. The temperature of the heating element rose to a maximum of 350°C.

[0363] Figure 4 shows the test results. The thick line represents emissions from the sample before SCRoF. The thin line represents NOx emissions after the SCR catalyst article. The catalysts of Reference Example 1 and Example 1 showed NOx emissions in the exhaust gases leaving the engine for approximately 800 seconds. x It adsorbs NOx. The catalyst in Comparative Example 1 does not show NOx adsorption due to the inlet temperature from the heating element being too high. The catalysts in Reference Example 1 and Example 1 show high NOx emission after approximately 800 seconds. In the case of Example 1 of the present invention, the downstream SCRoF, which is directly heated by the heating element, completely converts the emitted NOx.

[0364] Table 1 shows the system NOx emissions (mg / km) for the entire WLTC cycle (23km) and for the urban driving portion only after 600 seconds (3km). Only Example 1 (the present invention) achieved the lowest emissions in both the entire WLTC and the urban driving portion of the WLTC. The values ​​were measured at the SCRoF outlet.

[0365] [Table 1]

[0366] Table 2 shows the CO and THC emissions (g / km) of the catalyst / system for Reference Example 1, Comparative Example 1, and Example 1 over the entire WLTC cycle.

[0367] [Table 2]

[0368] As can be seen from these tables and Figure 4, the system according to Example 1 of the present invention can significantly reduce NOx emissions as well as CO and THC (total hydrocarbons) compared to an NA-DOC catalyst not coupled with a gas heating component (Reference Example 1). Surprisingly, it was found that the gas heating component should be placed downstream of the NA-DOC catalyst to obtain the optimal balance for reducing NOx, CO, and THC emissions.

[0369] Reference Example 4: Preparation of NOx adsorbent (NA) catalyst (FER) Ammonium ferrielite (framework structure type FER, SiO2:Al2O3 molar ratio of 21, crystallinity-to-standard (XRD) greater than 90%) zeolite material was wet-impregnated with an aqueous palladium nitrate solution to achieve a 2.7 mass% palladium loading based on the mass of the zeolite material. An uncoated flow-through honeycomb cordierite substrate (total volume 0.6 L, 400 cpsi, wall thickness 4 mil, diameter: 5.66 inches × length: 1.6 inches) was coated with the obtained slurry over 100% of the substrate shaft length. The coated substrate was dried in air at a temperature of 110°C for 1 hour, and then calcined in air at 590°C for 2 hours. The palladium loading was 140 g / ft. 3 The total coating load is 3g / in 3 That was the case.

[0370] Reference Example 5: Preparation of DOC Catalyst Bottom coating: It contains 95% by mass of Al, calculated as Al2O3, and 5% by mass of Si, calculated as SiO2, and 100m 2 BET specific surface area exceeding / g and 0.06 cm² 3A highly porous gamma-alumina support material having a pore volume exceeding 1 / g was impregnated with a stabilized platinum complex solution and an aqueous palladium nitrate solution by a simple wetting method. The Pd / Pt-alumina powder was slurryed in water by adding ammonium beta-zeolite material (BEA, SiO2:Al2O3 molar ratio of 23, crystallinity greater than 90% vs standard (XRD)). The mass ratio of Si-doped alumina to beta-zeolite material was 4.3:1. An uncoated flow-through honeycomb cordierite substrate (total volume 1.24 L, 400 cpsi, wall thickness 4 mil, diameter: 5.66 inches × length: 3 inches) was coated with the obtained slurry over 100% of the substrate shaft length. The coated substrate was dried in air at a temperature of 110°C for 1 hour, and then calcined in air at 590°C for 2 hours to form a bottom coating. The palladium and platinum loadings in the bottom coating were 20 g / ft, respectively. 3 and 40g / ft 3 The total bottom coating load is 1.9g / in. 3 That was the case.

[0371] Top coat: It contains 95% by mass of Al, calculated as Al2O3, and 5% by mass of Si, calculated as SiO2, and 100m 2 BET specific surface area exceeding / g and 0.06 cm² 3 A highly porous gamma-alumina support material having a pore volume exceeding 17 g / ft was impregnated with a stabilized platinum complex solution and an aqueous palladium nitrate solution by a simple wetting method. The Pd / Pt-alumina powder was made into a slurry in water. The substrate coated with the bottom coating was coated with the obtained slurry over 50% of the substrate axis length, from the outlet end to the inlet end. The coated substrate was dried in air at 110°C for 1 hour, and then calcined in air at 590°C for 2 hours to form a top coat. The loading amounts of palladium and platinum in the top coating (over 50% of the substrate length) were 17 g / ft, respectively. 3 and 103g / ft 3Therefore, the total top coating load (50% of the base material volume) is 1.5 g / in. 3 The total coating load (bottom coating and top coating) was 2.65 g / in. 3 The palladium load is 28.5 g / ft 3 The platinum load is 91.5 g / ft 3 (Total PGM load is 120g / ft) 3 ) was. Comparative Example 2: Preparation of DOC, an electric heating substrate, and a system containing DOC The system of Comparative Example 2, which does not conform to the present invention, was prepared by combining two diesel oxidation catalysts according to Reference Example 5 with an electric heating substrate from Reference Example 3, wherein the first DOC of Reference Example 5 is placed upstream of the electric heating substrate of Reference Example 3, and the electric heating substrate of Reference Example 3 is placed upstream of the second DOC of Reference Example 5.

[0372] Example 4: Preparation of a system containing NOx adsorbent (NA-) catalyst, electroheating substrate, and DOC catalyst In particular, Example 4, which is very similar to Example 2, was prepared for testing zeolite materials with a framework structure type FER and relatively low Pd loading.

[0373] The system of Example 4 according to the present invention was prepared by combining the NOx adsorption catalyst of Reference Example 4, the diesel oxidation catalyst (DOC) of Reference Example 5, and the electrically heated substrate of Reference Example 3, with the NOx adsorbent catalyst of Reference Example 4 positioned upstream of the electrically heated substrate of Reference Example 3, and the electrically heated substrate of Reference Example 3 positioned upstream of the DOC of Reference Example 5.

[0374] Reference Example 6: Preparation of NOx adsorbent (NA) catalyst (FER) Ammonium ferrielite (framework structure FER, SiO2:Al2O3 molar ratio of 21, crystallinity-to-standard (XRD) greater than 90%) zeolite material was wet-impregnated with an aqueous palladium nitrate solution, dried in air at 110°C for 1 hour, and calcined in air at 590°C for 2 hours to achieve a 2.7 mass% Pd loading based on the mass of the zeolite material. This Pd-FER powder was slurryed with water. An uncoated flow-through metal substrate (total volume 0.6 L, 400 cpsi, wall thickness 4 mil, diameter: 5.66 inches × length: 1.6 inches) was coated with the obtained slurry over 100% of the substrate shaft length. The coated substrate was dried in air at 110°C for 1 hour, and then calcined in air at 590°C for 2 hours. The palladium loading was 120 g / ft. 3 The total coating load is 3g / in 3 That was the case.

[0375] Reference Example 7: Preparation of DOC catalyst Bottom coating: It contains 95% by mass of Al, calculated as Al2O3, and 5% by mass of Si, calculated as SiO2, and 100m 2 BET specific surface area exceeding / g and 0.06 cm² 3 A highly porous gamma-alumina support material having a pore volume exceeding 1 / g was impregnated with a stabilized platinum complex solution and an aqueous palladium nitrate solution by a simple wetting method. The Pd / Pt-alumina powder was made into a slurry in water. An uncoated flow-through honeycomb cordierite substrate (total volume 1.24 L, 400 cpsi, wall thickness 4 mil, diameter: 5.66 inches × length: 3 inches) was coated with the obtained slurry over 100% of the substrate shaft length. The coated substrate was dried in air at 110°C for 1 hour, and then calcined in air at 590°C for 2 hours to form a bottom coating. The palladium and platinum loadings in the bottom coating were 32.75 g / ft, respectively. 3 and 65.5g / ft 3 The total bottom coating load is 1.5g / in. 3 That was the case.

[0376] Top coat: It contains 95% by mass of Al, calculated as Al2O3, and 5% by mass of Si, calculated as SiO2, and 100m 2 BET specific surface area exceeding / g and 0.06 cm² 3 A highly porous gamma-alumina support material having a pore volume exceeding 1 / g was impregnated with an aqueous palladium nitrate solution by a simple wetting method. The Pd / Pt-alumina powder was made into a slurry in water by adding ammonium beta zeolite material (BEA, SiO2:Al2O3 molar ratio of 23, crystallinity greater than 90% versus standard (XRD)). A substrate coated with a bottom coating was coated with the obtained slurry over 100% of the substrate shaft length. The coated substrate was dried in air at a temperature of 110°C for 1 hour, and then calcined in air at a temperature of 590°C for 2 hours to form a top coat. The amount of palladium supported in the top coating was 32.7 g / ft 3 The total top coating load is 1.5g / in. 3 That was the case.

[0377] Comparative Example 3: Preparation of DOC, an electric heating substrate, and a system containing DOC The system of Comparative Example 3, which does not conform to the present invention, is prepared by combining the diesel oxidation catalyst of Reference Example 7, the diesel oxidation catalyst of Reference Example 5, and the electric heating substrate of Reference Example 3, with the DOC of Reference Example 7 positioned upstream of the electric heating substrate of Reference Example 3, and the electric heating substrate of Reference Example 3 positioned upstream of the DOC of Reference Example 5.

[0378] Example 5: Preparation of a system containing NOx adsorbent (NA-) catalyst, electroheating substrate, and DOC catalyst The system of Example 5 according to the present invention is prepared by combining the NOx adsorbent catalyst of Reference Example 6, the diesel oxidation catalyst (DOC) of Reference Example 5, and the gas heating component of Reference Example 3, wherein the NOx adsorbent catalyst of Reference Example 6 is located upstream of the gas heating component of Reference Example 3, and the electrically heated substrate of Reference Example 3 is located upstream of the DOC of Reference Example 5.

[0379] Example 6: Testing of the systems of Comparative Examples 2 and 3 and Examples 4 and 5 - WLTC evaluation in a diesel engine - NOx emissions The systems of Comparative Examples 2 and 3, and Examples 4 and 5, were aged at 800°C for 16 hours in 10% vapor / air, and then tested in a 2L diesel engine using the Worldwide Harmonized Fuel Economy and Exhaust Gas Test Cycle (WLTC). Prior to the first test, the temperature of the NOx adsorbent samples (Examples 4 and 5) was raised to 650°C for 10 minutes to remove any pre-adsorbed NOx.

[0380] The systems of Comparative Examples 2 and 3 and Examples 4 and 5 were evaluated with a downstream SCR catalyst. The SCR catalyst article contained Cu-CHA(SCRoF) coated on a filter substrate. A urea injector was applied between the NOx adsorbent, the DOC article, and the SCR catalyst article to deliver the reducing agent for the SCR reaction. The test systems of Comparative Example 2 and Example 4 are shown in Figure 3.

[0381] All electric heating elements were switched on immediately after the start of WLTC. The temperature in front of the SCR article was adjusted between 200 and 250°C. The temperature immediately behind the heating elements was raised to a maximum of 380°C.

[0382] Table 3 shows the system NOx emissions (mg / km) for the entire WLTC cycle (23km) and for the urban driving section only after 600 seconds (3km). The system of Example 4 achieves the lowest emissions for both the entire WLTC and the urban driving section of the WLTC. The system of Example 5 achieves lower emissions for both the entire WLTC compared to the systems of Comparative Examples 2 and 3.

[0383] [Table 3]

[0384] Table 4 shows the CO and THC emissions (g / km) of the systems in Comparative Example 2 and Example 4 in the WLTC cycle. Both examples show very low CO and THC emissions from the high temperature of the DOC after the heating element. CO and THC emissions are lower compared to the emissions obtained in the system of Comparative Example 1. The system of Example 5 shows similar results for CO emissions.

[0385] [Table 4]

[0386] As can be seen from these tables, the system of Example 4 provides the lowest emissions for all three components: CO, THC, and NOx. Therefore, surprisingly, a further processing system using an electric heating element between the NA catalyst and DOC (the system of the present invention) was found to obtain the lowest NOx, CO, and THC emissions.

[0387] Even more surprisingly, both types of substrates for supporting the NA catalyst, namely cordierite and metal, were found to significantly reduce NOx, CO, and THC emissions compared to the emissions obtained in the comparative example.

[0388] Example 7: Testing of the systems of Comparative Example 2 and Example 4 - WLTC evaluation in a diesel engine - N2O formation The systems of Comparative Examples 2 and 4 were aged at 800°C for 16 hours in 10% steam / air, and then tested with a 2L diesel engine using the Worldwide Harmonized Fuel Economy and Exhaust Gas Test Cycle (WLTC) for passenger cars. A urea injector was placed between the DOC component of the system and the SCR catalyst to deliver the reducing agent for the SCR reaction.

[0389] Figure 5 shows the NOx emissions divided by the WLTC distance, displayed relative to the WLTC distance. From this data plot, the system in Example 4 achieves NOx emissions of less than 30 mg / km after driving 2 km. In Comparative Example 2, NOx emissions of less than 30 mg / km are achieved after four times longer operation, i.e., 8 km. Figure 6 shows greenhouse gas N2O emissions at the WLTC. The system in Comparative Example 2 shows higher N2O emissions compared to the system in Example 4.

[0390] Reference Example 8: Preparation of a NOx adsorbent apparatus (NA) having a DOC functional catalyst (layered catalyst-FER on a substrate including a downstream heating substrate) Bottom coating (NOx adsorbent coating): Ammonium ferrielite zeolite material (framework structure type FER, SiO2:Al2O3 molar ratio of 21, zeolite material with crystallinity versus standard (XRD) greater than 80%) was wet-impregnated with an aqueous palladium nitrate solution to achieve a Pd load of 1.48 mass% based on the mass of the final material (zeolite material + palladium). A zirconium acetate mixture was added to the resulting slurry. The amount of zirconium acetate was calculated to be 5 mass% based on the mass of the zeolite material, with the amount of zirconia in the bottom coat calculated as ZrO2.

[0391] A porous, uncoated, round, flow-through honeycomb cordierite substrate (total volume 1.85 L, 400 cpsi, wall thickness 4 mil, diameter: 5.66 inches, length: 4.5 inches) was coated with the obtained slurry over 100% of the substrate's axial length. The coated substrate was dried in air at 110°C for 1 hour, and then calcined in air at 590°C for 2 hours to form a bottom coating. The palladium loading in the bottom coating was 70 g / ft 3 The amount of FER loaded in the bottom coating is 2.7g / in. 3 The amount of ZrO2 loaded is 0.135 g / in. 3 The load capacity of the bottom coating was 2.9 g / in. 3 That was the case.

[0392] Top coating (DOC coating): The exit top coating consists of an Al2O carrier material containing 5% by mass of MnO2 (95% by mass of Al2O3 with 5% by mass of Mn calculated as MnO2, 100m 2 BET specific surface area exceeding / g and 0.06 cm² 3 A material with a pore volume exceeding 1 / g was impregnated with platinum by a wet impregnation method. The slurry containing the obtained material was coated over 50% of the substrate shaft length, from the outlet end to the inlet end, on a cordierite substrate supporting a Pd-FER bottom coating. The outlet top coating was 80 g / ft 3 It contains platinum, and the load capacity of the outlet coating is 1.3 g / in. 3 That was the case.

[0393] For the inlet top coating, an alumina support material containing 5% by mass of SiO2 was impregnated with platinum and palladium in a 2:1 mass ratio by a wet impregnation method. Fe-beta zeolite material (framework structure type BEA, SiO2:Al2O3 molar ratio 23:1, crystallinity versus standard (XRD) greater than 90%, zeolite material with a Fe content of 4.3% by mass calculated as Fe2O3 based on the mass of the zeolite material) was added to the Pd / Pt-alumina slurry. The mass ratio of Si-doped alumina to beta zeolite material was 1:1. The resulting slurry was coated over 50% of the substrate axis length from the inlet end to the outlet end of a cordierite substrate coated with a Pd-FER bottom layer and an outlet top coating. The inlet top coating contained 13.3 g / ft 3 Platinum and 6.7g / ft 3 It contained Pd. The filling amount of the inlet top coating was 1.41 g / in. 3 That was the case.

[0394] The total load capacity of the top coating (exit top coat + inlet top coat) is 1.355 g / in. 3 That was the case.

[0395] Reference Example 9: Preparation of NOx adsorbent catalyst (NA) H-chabazite zeolite material (framework structure type CHA, SiO2:Al2O3 molar ratio of 14, crystallinity against standard (XRD) greater than 90%) was wet-impregnated with an aqueous palladium nitrate solution and calcined in air at 590°C for 2 hours. The resulting Pd-impregnated chabazite had a Pd load of 1.22% by mass based on the mass of the final material (zeolite material + palladium). The Pd-impregnated chabazite was dispersed in water to obtain a slurry.

[0396] A porous, uncoated flow-through honeycomb cordierite substrate (total volume 1.85 L, 400 cpsi, wall thickness 4 mil, diameter: 5.66 inches × length: 4.5 inches) was coated with the slurry over 100% of the substrate's axial length. The coated substrate was dried in air at 110°C for 1 hour, and then calcined in air at 590°C for 2 hours. The amount of palladium loaded onto the coated substrate was 60 g / ft 3 The total wash coat load is 2.85g / in. 3 That was the case.

[0397] Example 8: Preparation of a system comprising a catalyst having NOx adsorbent (Pd-FER) component and a DOC component, and an electroheating substrate. The system of Example 8 according to the present invention was prepared by combining the catalyst of Reference Example 8, which includes a NOx adsorbent component and a diesel oxidation catalyst (DOC) component, with the gas heating component of Reference Example 3, wherein the catalyst of Reference Example 8 was placed upstream of the gas heating component of Reference Example 3. Comparative Example 4: Preparation of a system containing a NOx adsorbent (Pd-CHA) catalyst and an electroheating substrate The system of Comparative Example 4 according to the present invention was prepared by combining the catalyst of Reference Example 9, which contains an NOx adsorbent component, with the gas heating component of Reference Example 3, wherein the catalyst of Reference Example 9 was placed upstream of the gas heating component of Reference Example 3.

[0398] Example 9: Test-simulated low-temperature city driving cycle and NOx adsorption evaluation of the embodiment and comparative example of the present invention. The systems according to Example 8 and Comparative Example 4 were aged for 16 hours at 800°C in 10% steam (water) / air, and then tested, respectively, in a 2L diesel engine under simulated low-temperature city driving conditions. The systems according to Example 8 and Comparative Example 4 were tested independently of each other, using a selective catalytic reduction (SCR) catalyst located downstream. The SCR catalyst contained Cu-CHA zeolite coated on a 3L filter substrate. A urea injector was applied between the system and the SCR catalyst to deliver the reducing agent for the SCR reaction.

[0399] The driving cycle was compiled from the city driving mode of the New European Driving Cycle (NEDC). The average temperature of the cycle was approximately 170°C. The cycle was run twice for 1880 seconds each. Prior to the first test, the temperature of the NOx adsorbent catalyst was raised to 650°C for 10 minutes to purge any pre-adsorbed NOx.

[0400] The test results from the first test run are shown in Figure 7. Both systems showed NO emissions from the engine for up to approximately 500 seconds. x It adsorbs NOx. The NOx catalyst containing Pd-CHA zeolite in the system of Comparative Example 4 showed lower NOx adsorption during the first 500 seconds, and also showed lower NOx emissions at the end of the first test run compared to the NOx adsorbent catalyst in the system of Example 8.

[0401] Prior to the second test run, the system was cooled to room temperature, and no high-temperature pretreatment was performed. The test results of the second test run are shown in Figure 8. In the second test run, the system according to Comparative Example 4 (which thus includes a NOx adsorbent catalyst having Pd-CHA zeolite) did not show NOx adsorption because no NOx was released during the first cold urban cycle, and instead showed strong NOx emission. Therefore, the system according to Comparative Example 4 requires undesirable heat treatment to release stored NOx when running in such a cold urban cycle. The system according to Example 8 (which thus includes a NOx adsorbent catalyst having Pd-FER zeolite) still shows good NOx adsorption even in the second cold urban cycle. [Brief explanation of the drawing]

[0402] [Figure 1] Reference Example 2 shows the simulated low-temperature urban driving cycle and NOx adsorption evaluation (first test run). [Figure 2] Reference Example 2 shows the simulated low-temperature city driving cycle and NOx adsorption evaluation (second test run). [Figure 3]This figure shows a schematic diagram of a system for treating NOx, CO, and THC emissions. In particular, this figure first shows a first system not according to the present invention, which includes an NA-DOC catalyst 1 comprising a substrate coated with an NA (NOx adsorbent) coating and a DOC (diesel oxidation catalyst) coating on the NA coating of Reference Example 2, and a selective catalytic reduction catalyst (SCRoF) 2 on a filter substrate downstream of the NA-DOC catalyst 1 (coatings are not shown). Furthermore, a urea injector can be added between the NA-DOC 1 and the SCRoF 2. Furthermore, this figure shows a second system not according to the present invention, which includes an NA-DOC catalyst according to Comparative Example 1, which includes an NA coating and a DOC coating (coatings are not shown) placed on the NA coating, wherein the NA coating is placed on a single substrate including a gas heating component 3 (coatings are not shown) located upstream of the flow-through substrate 4 and a selective catalytic reduction catalyst (SCRoF) 2 on a filter substrate downstream of the NA-DOC catalyst (3+4+coating). Furthermore, a urea injector can be added, positioned between the NA-DOC catalyst and the SCRoF2. The figure also shows a system according to the present invention, including an NA-DOC catalyst according to Example 1, which includes an NA coating and a DOC coating (coating not shown) placed on the NA coating, wherein the NA coating is positioned on a single substrate including a flow-through substrate 4 located upstream of a gas heating component 3 (coating not shown) and an optional selective catalytic reduction catalyst on a filter substrate (SCRoF) 2 downstream of the NA-DOC catalyst (4+3+coating). Furthermore, a urea injector can be added, positioned between the NA-DOC catalyst and any SCRoF2. [Figure 4] The WLTC evaluation (NOx emissions) of NOx adsorbent DOC for Reference Example 2, Example 1, and Comparative Example 1, which have electric heating in a diesel engine, is shown. [Figure 5] The WLTC evaluation (N2O emissions) of the systems of Comparative Example 2 and Example 4, which have electric heating in a diesel engine, is shown. [Figure 6]The WLTC evaluation (N2O emissions) of the systems of Comparative Example 2 and Example 4, which have electric heating in a diesel engine, is shown. [Figure 7] The simulated low-temperature city driving cycle and NOx adsorption evaluation of the system according to Example 8 and the system according to Comparative Example 4 are shown (First Test Drive). [Figure 8] The simulated low-temperature city driving cycle and NOx adsorption evaluation of the system according to Example 8 and the system according to Comparative Example 4 are shown (Second Test Drive).

[0403] References -DE102018101929 -US2017 / 0284250A1 -US10480369B1

Claims

1. A system for processing exhaust gases from a diesel internal combustion engine, The system comprises a NOx adsorbent component, a diesel oxidation catalyst (DOC) component, a selective catalytic reduction (SCR) component, a gas heating component, and a reducing agent injector, wherein the NOx adsorbent component is located upstream of the gas heating component, the reducing agent injector is located upstream of the SCR component, the gas heating component is located upstream of the reducing agent injector, the DOC component is located upstream of the reducing agent injector, and the DOC component and the gas heating component are in a direct continuous configuration. The aforementioned NOx adsorbent component is contained in the catalyst. (i) The catalyst is (i.1) A first substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the first substrate, and the inner wall of the first substrate extending therethrough; (i.2) NOx adsorbent coating which is the NOx adsorbent component, wherein the coating is disposed on the surface of the inner wall of the first substrate over at least 50% of the substrate axial length of the first substrate, and the NOx adsorbent coating comprises a platinum group metal component and a 10-membered ring-pore zeolite material having a framework type selected from the group consisting of FER, TON, MTT, SZR, MWW, AEL, HEU, AFO, two or more mixtures thereof and two or more mixed types thereof, A system that includes this.

2. The system according to claim 1, wherein the platinum group metal component of the NOx adsorbent coating according to (i.2) is contained in the 10-membered ring-pore zeolite material of the NOx adsorbent coating according to (i.2).

3. The system according to claim 1 or 2, wherein the DOC component is located upstream of the gas heating component.

4. The catalyst produced by (i) is (i.3) A diesel oxidation catalyst (DOC) coating which is the DOC component, wherein the DOC coating is at least partially disposed on the NOx adsorbent coating over at least 70% of the substrate axial length of the first substrate, and the DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania. The system according to any one of claims 1 to 3, further comprising:

5. (ii) The gas heating component is (ii.1) A second substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the second substrate, and an inner wall of the second substrate extending through thereto; The inlet end of the second substrate according to (ii.1) and the outlet end of the first substrate according to (i.1) are coupled so that exhaust gas exiting the passage of the first substrate enters the passage of the second substrate; The system according to any one of claims 1 to 4, wherein the inner wall of the second substrate is thermally conductive to allow heating therein in order to heat the exhaust gas flowing through the passage of the second substrate.

6. The gas heating component according to (ii) is (ii.2) Optionally, a NOx adsorbent coating disposed on the surface of the inner wall of the second substrate over at least 50% of the substrate axial length of the second substrate, wherein the NOx adsorbent coating comprises a platinum group metal component and a 10-membered ring-pore zeolite material having a framework type selected from the group consisting of FER, TON, MTT, SZR, MWW, AEL, HEU, AFO, two or more mixtures thereof and two or more mixed types thereof, (ii.3) A diesel oxidation catalyst (DOC) coating that is at least partially disposed on the surface of the inner wall of the second substrate and / or at least partially disposed on any NOx adsorbent coating according to (ii.2), and extending over at least 70% of the substrate axis length of the second substrate, wherein the DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania, The system according to claim 5, further comprising:

7. The system according to claim 1, wherein the DOC component is located downstream of the gas heating component.

8. The aforementioned DOC component is contained in the catalyst, (iii) The catalyst is, (iii.1) A third substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the third substrate, and the inner wall of the third substrate extending through therefor; (iii.2) A first DOC coating disposed on the surface of the inner wall of the third substrate over at least 70% of the substrate axial length of the third substrate, wherein the first DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania; (iii.3) Optionally, a second DOC coating, at least partially disposed on the first DOC coating and extending over at least 20% of the substrate axial length of the third substrate, wherein the second DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania, The system according to claim 7, including the above.

9. (ii) The gas heating component is (ii.1) A second substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the second substrate, and an inner wall of the second substrate extending through thereto; Includes, The inlet end of the second substrate according to (ii.1) and the outlet end of the first substrate according to (i.1) are coupled so that the gas exiting from the passage of the first substrate according to (i.1) enters the passage of the second substrate according to (ii.1); The inlet end of the third substrate according to (iii.1) and the outlet end of the second substrate according to (iii.1) are coupled so that the gas exiting the passage of the second substrate enters the passage of the third substrate according to (iii.1); The system according to claim 7 or 8, wherein the inner wall of the second substrate according to (ii.1) is thermally conductive to allow heating therein in order to heat the exhaust gas flowing through the passage of the second substrate.

10. The gas heating component according to (ii) is (ii.2) A first DOC coating disposed on the surface of the inner wall of the second substrate according to (ii.1) over at least 50% of the substrate axial length of the second substrate according to (ii.1), wherein the first DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania; (ii.3) A second DOC coating optionally disposed at least partially on the first DOC coating according to (ii.2) and extending over at least 50% of the substrate axis length of the second substrate according to (ii.1), wherein the second DOC coating comprises a platinum group metal component and a non-zeolite oxide material comprising one or more of alumina, silica, zirconia and titania, The system according to claim 9, further comprising:

11. The aforementioned SCR component is contained in a selective catalytic reduction (SCR) catalyst. (iv) The selective catalytic reduction (SCR) catalyst is (iv. 1) A fourth substrate, comprising an inlet end, an outlet end, and a substrate axis length extending from the inlet end to the outlet end of the fourth substrate; (iv.2) A selective catalytic reduction (SCR) coating placed on a fourth substrate according to (iv.1), Including; The system according to any one of claims 1 to 10, wherein the inlet end of a fourth substrate according to (iv. 1), the outlet end of a second substrate according to (ii. 1) within the scope of claim 11 referring to any one of claims 5 or 6, or the outlet end of a third substrate according to (iii. 1) within the scope of claim 11 referring to any one of claims 7 to 10, is coupled such that exhaust gas from the passage of the second substrate or exhaust gas from the passage of the third substrate enters the fourth substrate.

12. A method for preparing a system for treating exhaust gases of a diesel internal combustion engine, wherein the method is (1) To provide NOx adsorbent components, diesel oxidation catalyst (DOC) components, selective catalytic reduction (SCR) components, gas heating components, and reducing agent injectors, The aforementioned NOx adsorbent component is contained in the catalyst. (i) The catalyst is (i.1) A first substrate comprising a plurality of passages defined by an inlet end, an outlet end, a substrate axis length extending from the inlet end to the outlet end of the first substrate, and the inner wall of the first substrate extending therethrough; (i.2) NOx adsorbent coating which is the NOx adsorbent component, wherein the coating is disposed on the surface of the inner wall of the first substrate over at least 50% of the substrate axial length of the first substrate, and the NOx adsorbent coating comprises a platinum group metal component and a 10-membered ring-pore zeolite material having a framework type selected from the group consisting of FER, TON, MTT, SZR, MWW, AEL, HEU, AFO, two or more mixtures thereof and two or more mixed types thereof, Including the provision of the foregoing, (2) Placing the NOx adsorbent component upstream of the gas heating component, (3) The reducing agent injector is placed upstream of the SCR component, (4) Placing the gas heating component upstream of the reducing agent injector, (5) Placing the DOC component upstream of the reducing agent injector, (6) Arranging the DOC component and the gas heating component in a direct and continuous order, Methods that include...

13. A system for treating exhaust gases of a diesel internal combustion engine that can be obtained or obtained by the method of claim 12.

14. A method for treating exhaust gases from a diesel internal combustion engine, comprising providing exhaust gases from a diesel internal combustion engine and passing the exhaust gases through a system according to any one of claims 1 to 11 or 13.

15. A use of the system according to any one of claims 1 to 11 or 13 for treating exhaust gases of a diesel internal combustion engine, wherein the use includes passing the exhaust gases through the system.