Sliding member

A laminated coating structure with a hard first layer and soft self-lubricating second layer addresses seizure and galling in scroll compressors, enhancing wear resistance and lubrication, thus reducing friction and manufacturing costs.

JP2024132595AInactive Publication Date: 2024-10-01SANDEN CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023043430
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing sliding members in scroll compressors face issues with seizure and galling due to the lack of self-lubricating properties in poor lubrication environments during initial operation, despite having improved wear resistance through electroless Ni-P plating.

Method used

A laminated structure is introduced with a first coating layer harder than the second coating layer, composed of electroless Ni-P plating, and a second coating layer with self-lubricating properties, such as polytetrafluoroethylene (PTFE), to facilitate transfer and maintain lubrication, reducing friction and preventing seizure.

Benefits of technology

The laminated structure provides wear resistance and self-lubricating properties, reducing friction and preventing galling, especially in initial operation, while maintaining lubrication performance and reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132595000001_ABST
    Figure 2024132595000001_ABST
Patent Text Reader

Abstract

To provide a sliding member further imparting even self lubricity while holding a wear-resistant improvement effect by plating.SOLUTION: A slide member includes a first sliding body and a second sliding body sliding the surface of the first sliding body. The second sliding body has a structure obtained by laminating a base material, a first coating layer and a second coating layer in this order; the first sliding body surface slides on the second coating layer; and the first coating layer is harder than the first sliding body surface and the second coating layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sliding member, and more particularly to a sliding member that is used in a scroll compressor or the like and that can suppress the occurrence of seizure and scoring under a poor lubrication environment such as at the time of initial movement. [Background technology]

[0002] A scroll compressor is equipped with a scroll unit that compresses a refrigerant, and has a fixed scroll body and a movable scroll body that are installed facing each other. As the movable scroll body revolves, the refrigerant moves toward the center of the scroll body while being compressed.

[0003] In order to prevent wear caused by the operation of the movable scroll, it has been considered to form a plating layer such as electroless nickel-phosphorus (Ni-P) plating on the surface of one or both of the two scrolls (see, for example, Patent Documents 1 and 2).

[0004] Providing a plating layer on the sliding surface is effective in preventing sliding between base materials such as aluminum alloys in sliding components that require wear resistance. In order to improve wear resistance, hardness and toughness against impact are also required, so the above-mentioned Ni-P-based hard plating is generally used. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2001-304151 A [Patent Document 2] JP 2019-60259 A Summary of the Invention [Problem to be solved by the invention]

[0006] Electroless Ni-P plating is relatively hard and therefore effective in improving the wear resistance of sliding surfaces. However, unlike electroless Sn plating and the like, it does not have self-lubricating properties, and so there is a risk of seizure or scoring occurring in a poor lubrication environment, for example, at the initial start.

[0007] An object of the present invention is to provide a sliding member which retains the wear resistance improving effect achieved by plating and further has self-lubricating properties. [Means for solving the problem]

[0008] A slide member according to one embodiment of the present invention includes a first slide body and a second slide body sliding against a surface of the first slide body. The second slide body has a structure in which a base material, a first coating layer, and a second coating layer are laminated in this order. The first slide body surface and the second coating layer slide against each other. The first coating layer is harder than the first slide body surface and the second coating layer.

[0009] By adjusting the hardness of the first coating layer, the first slide body surface, and the second coating layer as described above, some of the components from the second coating layer and the first slide body surface are easily transferred to the other surface during sliding, which results in the development of lubricity on the sliding surfaces and improves the conformability and seizure resistance.

[0010] More preferably, the surface roughness Rz of the first coating layer is 0.1 μm or more and 7.0 μm or less, and the thickness of the second coating layer is 15 μm or less. This facilitates transfer from the second coating layer to the first sliding body surface due to sliding, and the components of the second coating layer are present on both sliding body surfaces, thereby further improving the lubricating performance. Furthermore, even if a part of the first coating layer is exposed due to the transfer of the second coating layer, the lubricating performance is maintained.

[0011] More preferably, the surface roughness Rz of the first slide body surface is 0.1 μm or more and 5.0 μm or less, which makes it possible to achieve both the prevention of transfer of components and the durability of the second coating layer.

[0012] More preferably, the first coating layer and the second coating layer are both electroless nickel-phosphorus (Ni-P) plating. The first coating layer and the second coating layer are made of the same components, which can improve the adhesion between the first coating layer and the second coating layer.

[0013] More preferably, the first coating layer has a Vickers hardness of 600 HV or more, the second coating layer has a Vickers hardness of 150 HV or more and 600 HV or less, and the first slide body surface has a Vickers hardness of 150 HV or more and 500 HV or less.

[0014] More preferably, the phosphorus concentration of the first coating layer is from 1% by mass to 4% by mass, which can improve the wear resistance and heat resistance of the sliding member.

[0015] More preferably, the second coating layer is an electroless Ni-P plating containing polytetrafluoroethylene (PTFE). The presence of the highly lubricating second coating layer on the surface of the second slide body can realize high lubrication performance on the sliding surfaces between the slide bodies.

[0016] More preferably, the phosphorus concentration of the second coating layer is higher than that of the first coating layer, thereby improving the adhesion between the second coating layer and the first coating layer while realizing a difference in hardness between the two layers.

[0017] More preferably, at least one of the base materials of the first slide body and the second slide body is made of aluminum, an aluminum alloy, or iron. This is suitable for use in compressors because it is possible to achieve weight reduction while ensuring strength. Effect of the Invention

[0018] According to the present invention, it is possible to provide a sliding member having wear resistance and self-lubricating properties. [Brief description of the drawings]

[0019] [Figure 1]1 is a schematic cross-sectional view of a sliding member according to an embodiment of the present invention. [Diagram 2] FIG. 13 is a diagram showing the results of friction coefficient evaluation. [Figure 3A] 4 is a microscope photograph of the sliding surface of the second slide body of Example 1. [Figure 3B] 3 is a microscope photograph of the sliding surface of the first slide body of Example 1. [Figure 4A] 1 is a microscope photograph of the sliding surface of the second slide body of Comparative Example 1. [Figure 4B] 4 is a microscope photograph of the sliding surface of the first slide body of Comparative Example 1. [Diagram 5] 1A is a component mapping of the sliding surface of the first slide body of Example 1, and FIG. 1B is a component mapping of the sliding surface of the first slide body of Comparative Example 1. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] 1 is a schematic cross-sectional view of a slide member according to one embodiment of the present invention. The slide member 1 has a first slide body 10 and a second slide body 20 facing each other. The second slide body 20 includes a substrate 21, a first coating layer 22 formed on the surface of the substrate 21, and a second coating layer 23 formed on the surface of the first coating layer 22. Thus, the second slide body 20 has a structure in which the substrate 21, the first coating layer 22, and the second coating layer 23 are laminated in this order.

[0021] With the above-mentioned configuration, the first slide body surface 11 slides against the surface of the second coating layer 23 of the second slide body 20. For example, when the sliding member 1 of the present embodiment is applied to a scroll compressor, the fixed scroll forming a scroll unit is the first slide body 10, and the movable scroll is the second slide body 20. The fixed scroll may be the second slide body 20, and the movable scroll may be the first slide body 10. As the movable scroll makes an orbital motion, the refrigerant moves toward the center of the scroll while being compressed.

[0022] Examples of the material for the first slide body 10 include aluminum, aluminum alloys, iron, etc. Aluminum alloys are lightweight and therefore are suitably used in applications that require weight reduction, such as automobile parts.

[0023] From the viewpoint of manufacturing costs, it is preferable that the first slide body surface 11 does not have a coating layer, but this is not limitative, and the first slide body surface 11 may be coated with plating or the like.

[0024] The specific hardness of the first slide body surface 11 is preferably 150 HV or more and 500 HV or less in Vickers hardness. By using the above-mentioned components, a surface having an appropriate hardness can be obtained.

[0025] The base material 21 of the second slide body 20 is a constituent material of the slide body, and like the first slide body 10, examples of the material include aluminum, an aluminum alloy, and iron.

[0026] The first coating layer 22 is a layer harder than the second coating layer 23, and is formed to improve the wear resistance of the substrate 21. The first coating layer 22 is harder than the substrate 21. For example, the first coating layer 22 may be a hard electroless Ni-P plating layer. Specifically, a so-called low phosphorus electroless Ni-P plating layer having a phosphorus content of 1 mass% or more and 4 mass% or less is preferable. Electroless nickel-boron (Ni-B) plating may also be used. The first coating layer 22 is not limited to the above as long as it is a layer harder than the second coating layer 23, and may be a layer hardened by surface modification such as a thermal spray coating, a carbon-based hard coating, a resin-based coating, an oxide coating, plating other than the above, or carburizing and quenching.

[0027] Specifically, the first coating layer 22 preferably has a Vickers hardness of 600 HV or more when formed by Ni-P plating. When the first coating layer is formed by a low phosphorus electroless Ni-P plating layer or an electroless Ni-B plating layer, the Vickers hardness is 800 HV or less.

[0028] The second coating layer 23 is a coating layer softer than the first coating layer 22 and is a layer that imparts self-lubrication to the first coating layer 22. The second coating layer 23 is not particularly limited as long as it is a layer softer than the first coating layer 22, and may be a thermal spray coating, a carbon-based hard coating, a resin-based coating, an oxide coating, plating other than those mentioned above, or a layer hardened by surface modification such as carburizing and quenching.

[0029] As the second coating layer 23, for example, so-called medium phosphorus or high phosphorus electroless Ni-P plating having a phosphorus content of 8 mass% or more and 12 mass% or less is preferable. The phosphorus concentration of the second coating layer 23 is preferably higher than that of the first coating layer 22. This makes it possible to improve the adhesion between the second coating layer 23 and the first coating layer 22 while realizing a difference in hardness between the two layers.

[0030] When the second covering layer 23 is made of Ni-P plating, the Vickers hardness of the second covering layer 23 is preferably 150 HV or more and 600 HV or less.

[0031] Also preferred is electroless Ni-P plating containing a fluororesin as the second coating layer 23. Examples of the fluororesin include polytetrafluoroethylene (PTFE). The lubricating component such as PTFE contained in the second coating layer 23 is transferred to the first slide body surface 11, whereby the lubricating component is present on the sliding surface, thereby further improving the slidability.

[0032] In the slide member 1 of the present embodiment, the hardness of the first coating layer 22 of the second slide body 20 is higher than the hardness of the first slide body surface 11 and the second coating layer of the second slide body 20. In a poor lubrication environment, the hard first coating layer 22 exists on the base of the relatively soft second coating layer 23, so that the second coating layer 23 is likely to transfer to the first slide body surface 11. A part of the second coating layer 23 is transferred to the first slide body surface 11, thereby providing lubricity to the sliding part. At this time, depending on the relationship between the hardness of the first slide body surface 11 and the second coating layer 23, a part of the first slide body surface 11 may be transferred to the surface of the second coating layer 23.

[0033] As described above, in this embodiment, the second coating layer 23, which is softer than the first coating layer 22, is formed on the surface of the harder first coating layer 22, and therefore the second coating layer 23 is more likely to transfer to the first slide body surface 11. This makes it possible to reduce the static friction coefficient of the sliding surface in a poor lubrication environment such as at the initial movement. In addition, a part of the second coating layer 23 is transferred by sliding with the first slide body 10, thereby exerting the effect of reducing the friction coefficient of the sliding surface. In addition, even if the first coating layer 22 is partially exposed due to the transfer of the second coating layer 23, the self-lubricating performance can be maintained.

[0034] In one embodiment, it is preferable that the surface roughness Rz of the first coating layer 22 is 0.1 μm or more and 7.0 μm or less, and the thickness of the second coating layer 23 is 15 μm or less. The thickness of the second coating layer 23 is related to the surface roughness (unevenness) of the first coating layer 22 on which the second coating layer 23 is formed. In the initial state, it is preferable that the entire surface of the first coating layer 22 is coated with the second coating layer 23. On the other hand, the second coating layer 23 is transferred to the first sliding body surface 22 by being worn by sliding, but if there is too much wear material, it floats between the sliding surfaces and, for example, when the sliding member is used in a compressor, it will be mixed as foreign matter in the refrigeration oil and refrigerant. Since the amount of foreign matter in the refrigeration oil and refrigerant needs to be minimized, it is preferable that the second coating layer 23 is minimal. Considering the surface roughness Rz of the first coating layer 22 adopted in this embodiment, the thickness of the second coating layer 23 is preferably 15 μm or less, and may be 10 μm or less. It is usually 0.1 μm or more, and preferably 5 μm or more. The thickness of the second coating layer 23 used here is the average value of a plurality of locations. The number of locations to be measured is preferably 10 or more arbitrarily selected points.

[0035] The second coating layer 23 of the present invention does not necessarily have to be present on the entire surface of the first coating layer 22 to achieve the desired effect of the present invention. Even if the components constituting the second coating layer 23 are transferred to the first sliding body 11 through repeated sliding with the first sliding body 11 and the first coating layer 22 formed below the second coating layer 23 is partially exposed, the desired effect of the present invention is achieved.

[0036] The surface roughness Rz of the first slide body surface 11 is preferably 0.1 μm or more and 5.0 μm or less. If the first slide body surface 11 is too smooth, the second coating layer 23 and the transfer from the first slide body surface 11 are unlikely to occur. On the other hand, if the surface is too rough, the durability of the second coating layer 23 is significantly reduced. By adjusting the surface roughness Rz of the first slide body surface 11 to the above range, it is possible to achieve both the transfer of the components and the durability of the second coating layer 23.

[0037] The thickness of the first coating layer 22 is preferably 10 μm or more. The first coating layer 22 needs to be sufficiently thick to protect the substrate 21 and improve the abrasion resistance, and to serve as a hard base to support the second coating layer 23. There are no particular limitations on the thickness of the first coating layer 22, but it is preferably 20 μm or less in consideration of the manufacturing cost.

[0038] In one embodiment, it is preferable that both the first coating layer 22 and the second coating layer 23 are electroless Ni-P plating. By making the first coating layer 22 and the second coating layer 23 from the same components, the adhesion between the first coating layer 22 and the second coating layer 23 can be improved.

[0039] There is no particular limitation on the method for forming the first coating layer 22 and the second coating layer 23, and known electroless plating methods and conditions can be used. For the hard plating layer, a commercially available plating solution such as SEK-797 manufactured by Nippon Kanigen Co., Ltd. can be used. For the PTFE-containing electroless Ni-P plating solution, Kaniflon 4S manufactured by Nippon Kanigen Co., Ltd. can be used.

[0040] For example, an electroless Ni-P plating layer can be obtained by immersing an object to be plated for a predetermined time in a plating bath kept at 88° C. to 94° C., rinsing with water, and drying. It is preferable to pretreat the object to be plated by a known method such as degreasing, washing, desmutting, or zincating.

[0041] The sliding member of this embodiment is suitable for compressors equipped with sliding members, such as scroll compressors and piston-type compressors. When the sliding member of this embodiment is used in a scroll compressor, it can be used for either the fixed scroll or the movable scroll of a scroll unit that compresses a refrigerant. By using the sliding member of this embodiment in a scroll unit, it is possible to prevent galling and seizure. In addition, the sliding member of this embodiment is effective when a second coating layer is formed on either the fixed scroll or the movable scroll, so that one of the members does not require a plating layer. Furthermore, a chip seal made of fluororesin is not required. Therefore, the manufacturing cost of the scroll compressor can be reduced.

[0042] As examples of scroll compressors, reference can be made to Japanese Patent Application Laid-Open No. 2013-170516 and Japanese Patent Application Laid-Open No. 2020-33987. EXAMPLES

[0043] The present invention will now be described in detail with reference to examples, in which the evaluation methods are as follows. (1) Plating thickness A fluorescent X-ray coating thickness gauge (Fisher Instruments XDLM-C4-PCD) was used. If necessary, cross-sections were cut, filled with resin, polished, and cross-sectional observations were performed (for example, Keyence VHX-7000). The thickness was measured at 10 randomly selected points, and the average value was taken as the plating thickness.

[0044] (2) Surface roughness Rz (ten-point average roughness) A shape measuring machine (SV-3000S CNC manufactured by Mitutoyo Corporation) was used, and measurements were performed under conditions (reference length 0.8 mm, evaluation length 4 mm) in accordance with JIS B 0633:2001 (ISO4288:1996).

[0045] (3) Vickers hardness A micro Vickers hardness tester (Mitutoyo HM-220D) was used, and the measurement conditions were partially in accordance with JIS Z 2244-1. The measurement conditions were changed depending on the plating thickness, and as an example, the test force (test load) was 0.2943N (30gf), the loading time was 5[s], the holding time was 15[s], the unloading time was 4[s], and the indenter approach speed was 60.0[μm / s].

[0046] Example 1 (1) First sliding body An aluminum alloy (A4032) was used as the substrate of the sliding member. No coating layer was provided on the surface of the first sliding body, and the surface was smoothed by end mill processing. The surface roughness Rz of the first sliding body was 1.0 μm. The Vickers hardness of the surface of the first sliding body was 170 HV.

[0047] (2) Second sliding body (A) Formation of the first coating layer An electroless Ni-P plating layer was formed on the surface of a substrate (aluminum alloy) that had been processed in the same way as the first sliding body. The plating solution used was SEK-797 manufactured by Japan Kanigen Co., Ltd. The plating solution temperature was set to between 85°C and 95°C, and plating was formed for between 1 hour and 2 hours, although this varied depending on the turnover of the plating solution.

[0048] The first coating layer had a thickness of 11.0 μm, a surface roughness Rz of 3.0 μm, and a Vickers hardness of 680 HV. The phosphorus concentration of the first coating layer was 2.0 mass %.

[0049] (B) Formation of the second coating layer A PTFE-containing electroless Ni-P plating layer was formed on the surface of the first coating layer to form a second coating layer. Kaniflon 4S manufactured by Japan Kanigen Co., Ltd. was used as the plating solution. Although it varies depending on the turnover of the plating solution, the temperature of the plating solution was set to 85°C or more and 95°C or less, and plating was formed for 30 minutes to 1 hour.

[0050] The second coating layer had a thickness of 5.6 μm, a surface roughness Rz of 3.0 μm, and a Vickers hardness of 200 HV. The phosphorus concentration of the second coating layer was 6.7 mass %. This value was calculated including PTFE.

[0051] Example 2 Except for changing the second coating layer of the second slide body to an electroless Ni-P plating layer having a phosphorus concentration of 9.3 mass%, a slide member was produced in the same manner as in Example 1. In forming the second coating layer, SE-200 manufactured by Nippon Kangen Co., Ltd. was used as the plating solution.

[0052] The second coating layer had a thickness of 5.9 μm, a surface roughness Rz of 2.8 μm, and a Vickers hardness of 500 HV.

[0053] Comparative Example 1 A slide member was produced in the same manner as in Example 1, except that the second coating layer of the second slide body was not formed.

[0054] [Evaluation of friction coefficient] In order to confirm the change in the coefficient of friction between the first slide body and the second slide body when the second coating layer is formed on the surface of the second slide body, the following experiment was carried out. The samples used had a pin-shaped first slide body and a plate-shaped second slide body.

[0055] The first sliding body and the second sliding body were slid against each other, and the change in the friction coefficient was observed. Specifically, using a load-varying friction and wear tester (HHS-2000S manufactured by Shinto Scientific Co., Ltd.), both sliding bodies were repeatedly slid at a load and speed that did not significantly damage the surfaces of both sliding bodies, and the change in the friction coefficient was measured. The measurement results are shown in Figure 2. It was confirmed that, compared to Comparative Example 1, Examples 1 and 2 had smaller dynamic friction coefficients at the initial movement (static friction coefficient) and in the region with fewer sliding movements.

[0056] [Surface observation] A pin-shaped first sliding body (aluminum alloy: A4032) was pressed against the second sliding body and slid back and forth using a load-varying friction and wear tester, and then the sliding surfaces of the first sliding body and the second sliding body were observed under a microscope at a magnification of 500 times.

[0057] Fig. 3A is a micrograph of the sliding surface of the second sliding body of Example 1, and Fig. 3B is a micrograph of the sliding surface of the first sliding body of Example 1. Fig. 4A is a micrograph of the sliding surface of the second sliding body of Comparative Example 1, and Fig. 4B is a micrograph of the sliding surface of the first sliding body of Comparative Example 1. From the micrographs, it can be seen that the sliding surface of the sliding member of Comparative Example 1 is deeply worn over a wide area. On the other hand, it can be seen that the wear range of the sliding member of Example 1 is reduced due to the lubricating effect of the second coating layer.

[0058] [Transfer of the second coating layer] The presence of fluorine atoms on the sliding surface of the first sliding body after repeated sliding using the load-varying friction and wear tester was observed by component mapping. Fig. 5 shows component mapping of fluorine atoms, where (a) is the component mapping of the sliding surface of the first sliding body of Example 1, and (b) is the component mapping of the sliding surface of the first sliding body of Comparative Example 1. The component mapping of Example 1 confirmed the presence of fluorine atoms (white dots), confirming that PTFE, a component of the second coating layer, had been transferred and scattered. [Industrial Applicability]

[0059] The sliding member of the present invention can be suitably used in devices equipped with a sliding member, such as scroll compressors and piston-type compressors. [Explanation of symbols]

[0060] 1 Sliding member 10 First sliding body 11 First sliding body surface 20 Second sliding body 21 Base material 22 First coating layer 23 Second coating layer

Claims

1. A first sliding body; a second slide body that slides on the first slide body surface, the second slide body has a structure in which a base material, a first coating layer, and a second coating layer are laminated in this order; the first slide body surface and the second coating layer slide against each other, A sliding member, wherein the first coating layer is harder than the first sliding body surface and the second coating layer.

2. The surface roughness Rz of the first coating layer is 0.1 μm or more and 7.0 μm or less, 2. The sliding member according to claim 1, wherein the second coating layer has a thickness of 15 μm or less.

3. 3. The sliding member according to claim 1, wherein the surface roughness Rz of the first slide body surface is 0.1 μm or more and 5.0 μm or less.

4. 3. The sliding member according to claim 1, wherein the first coating layer and the second coating layer are both electroless nickel-phosphorus (Ni-P) plating.

5. The first coating layer has a Vickers hardness of 600 HV or more, The second coating layer has a Vickers hardness of 150 HV or more and 600 HV or less, 5. The sliding member according to claim 4, wherein the Vickers hardness of the surface of the first slide body is 150 HV or more and 500 HV or less.

6. 5. The sliding member according to claim 4, wherein the first coating layer has a phosphorus concentration of 1% by mass or more and 4% by mass or less.

7. 5. The sliding member according to claim 4, wherein the second coating layer is an electroless Ni-P plating containing polytetrafluoroethylene (PTFE).

8. 5. The slide member according to claim 4, wherein the second coating layer has a higher phosphorus concentration than the first coating layer.

9. 3. The slide member according to claim 1, wherein at least one of the base materials of the first slide body and the second slide body is made of aluminum, an aluminum alloy, or iron.

10. 3. The sliding member according to claim 1, which is for a compressor.

Citation Information

Patent Citations

  • Scroll compressor

    JP2001304151A

  • Slide member for compressor

    JP2019060259A