Over-cooling coagulation method of preparation of noncrystalline nanocrystal soft magnetic alloy of high iron content
By employing glass purification and electromagnetic suspension melting for supercooling solidification, the method addresses the limitations of existing alloys by increasing ferromagnetic iron content and enhancing saturation magnetization strength while maintaining low coercive force, optimizing the microstructure of iron-based amorphous nanocrystalline soft magnetic alloys.
Patent Information
- Application Number
- JP2023201698
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-16
- Filing Date
- 2023-11-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-11-29
AI Technical Summary
Existing methods for preparing iron-based amorphous nanocrystalline soft magnetic alloys face limitations in increasing saturation magnetization strength due to the need for non-magnetic elements, which reduce the ferromagnetic element content and hinder high output and miniaturization.
A method combining glass purification with cyclic superheating or electromagnetic suspension melting to achieve supercooling solidification, reducing non-magnetic elements and increasing the ferromagnetic iron content, thereby enhancing saturation magnetization strength and maintaining low coercive force.
The method results in amorphous nanocrystalline soft magnetic alloys with high saturation magnetization strength and low coercive force by optimizing the microstructure and reducing heterogeneous nucleation points, thus expanding the design range and performance of these alloys.
Smart Images

Figure 2024132846000001 
Figure 2024132846000002 
Figure 2024132846000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for preparing an amorphous nanocrystalline soft magnetic alloy with high iron content by undercooling solidification, which belongs to the field of metallic soft magnetic materials. [Background technology]
[0002] Due to its special microstructure, iron-based amorphous nanocrystalline soft magnetic alloys have great advantages over crystalline soft magnetic alloys, such as low coercivity and high resistivity. However, the presence of a large amount of amorphous forming elements in iron-based amorphous nanocrystalline soft magnetic alloys leads to a decrease in saturation magnetization strength, which limits the development of high power and miniaturization of related soft magnetic components. The saturation magnetization strength of a typical amorphous soft magnetic alloy (international symbol Metglas 2605SA1, Chinese symbol 1K101) is about 1.55 T, and the saturation magnetization strength of a typical nanocrystalline soft magnetic alloy (international symbol Finemet, Chinese symbol 1K107) is about 1.24 T, both of which are much lower than the saturation magnetization strength of silicon steel (about 2.12 T).
[0003] For amorphous nanocrystalline soft magnetic alloys, in order to fully expand the potential applications in various electronic devices, it is urgent to increase the Fe-based magnetic element content and saturation magnetization strength in the iron-based amorphous nanocrystalline soft magnetic alloys. The difficulty in preparing amorphous nanocrystalline soft magnetic alloys with high iron content lies in the strict requirement for obtaining an amorphous matrix, i.e., the cooling rate of the molten alloy must be 10 5 ℃ / S or more. According to the Inoue amorphous principle, it is always necessary to add about 20 at% of non-magnetic elements to the alloy to promote the formation of amorphous structure. Nanocrystalline soft magnetic alloys are formed by crystallizing and tempering amorphous alloys, and often require the addition of non-magnetic elements to form crystal nuclei and inhibit grain growth. The introduction of these elements greatly limits the content of ferromagnetic elements in amorphous nanocrystalline soft magnetic alloys, making it difficult to obtain high saturation magnetization strength.
[0004] At present, methods for increasing the saturation magnetization strength of iron-based amorphous nanocrystalline soft magnetic alloys mainly focus on controlling the components. On the one hand, the saturation magnetization strength of the alloy can be increased by adding Co element to increase the ferromagnetic exchange strength in the alloy. For example, patent ZL201410728540.1 claims that adding 6-20at%Co increases the saturation magnetization strength of nanocrystalline alloys to 1.80T, and the coercive force falls in the range of 10-35A / m. TIFF2024132846000001.tif1062 alloys. On the other hand, the amount of metalloid elements such as Si, B, C, and P is adjusted. For example, patent ZL200510066862.5 discloses alloys in which c is in the range of 12-18 at% and b≦(0.5×a-36)×d 1 / 3 If the above conditions are met, the saturation magnetization strength of the iron-based amorphous material may reach 1.60 T or more. TIFF2024132846000002.tif1044 alloy. In addition, patent ZL201410285976.8 discloses alloys obtained by adjusting the addition ratio of semi-metallic elements. TIFF2024132846000003.tif1084 alloy has the highest saturation magnetization strength of 1.69T. TIFF2024132846000004.tif952 alloys. On the one hand, these methods, according to the Inoue amorphous principle, adjust the addition ratio of metalloid elements to affect the mixing enthalpy and atomic size difference of the alloy, thereby improving the amorphous forming ability of the alloy, and thus increasing the content of ferromagnetic elements. On the other hand, the 2p electrons of metalloid elements can affect the 3d electrons of Fe, and thus affect the magnitude of the magnetic moment of Fe atoms to adjust the saturation magnetization strength of the alloy. From the above patents, it can be seen that the method of adjusting the content of metalloid elements requires accurate control of the proportional relationship of different elements, and the increase in the amount of ferromagnetic elements added is still limited, which limits the further improvement of the saturation magnetization strength.
[0005] The present invention combines glass purification with cyclic heating or utilizes electromagnetic suspension melting to realize supercooling solidification of an iron-based amorphous nanocrystalline soft magnetic alloy, thereby reducing the amount of non-magnetic elements added to the alloy and effectively increasing the amount of ferromagnetic elements added to the alloy, thereby enhancing the saturation magnetization strength of the alloy and maintaining a low coercive force. Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention aims to overcome the shortcomings of the existing techniques for preparing iron-based amorphous nanocrystalline soft magnetic alloys, and to use the supercooling non-equilibrium solidification method to reduce the amount of amorphous-forming elements added to the alloy, thereby realizing the preparation of amorphous nanocrystalline soft magnetic alloys with high iron content, thereby broadening the design range of iron-based amorphous nanocrystalline soft magnetic alloys, and increasing the saturation magnetization strength of the alloys. [Means for solving the problem]
[0007] The technical solutions adopted by the present invention are as follows: A method of combining glass purification with cyclic superheating or electromagnetic suspension melting to make the alloy supercooled solidified, thereby reducing the amount of non-magnetic elements added to the iron-based amorphous nanocrystalline soft magnetic alloy and increasing the proportion of Fe element, thereby achieving the goals of increasing the saturation magnetization strength and decreasing the coercivity, and thus a supercooled solidification method for preparing a high iron content amorphous nanocrystalline soft magnetic alloy.
[0008] Preferably, the method for combining glass purification with cyclic heating comprises the steps of: S1, the chemical formula of the amorphous nanocrystalline alloy is FeSiBM, where M is one or more elements of P, C, Nb, Mo, Zr, Hf, Mo, Y, Cu and Co; removing oxide film from the alloy raw materials and cleaning them, weighing the raw materials according to a specific mass ratio, and loading the weighed raw materials into a vacuum sensitive melting furnace or a vacuum arc melting furnace, and evacuating the raw materials for 10 minutes. -3 After the pressure reaches 1 Pa, inert gas is introduced to protect the melting process, and the melting is repeated 4 to 6 times to obtain an alloy ingot. S2, placing the alloy ingot into a crucible, and covering its upper and lower surfaces with a glass purifier in a specific mass ratio, so as to completely enclose the alloy ingot in the glass purifier; S3, vacuum 10 -2 After the pressure reaches 1 Pa, inert gas is introduced to heat and melt the alloy under its protection, then the temperature is raised to 1200-1500°C, kept at that temperature for 1-10 minutes, and the heating power is turned off to allow the alloy to cool naturally. S4, "heating-warming-solidifying" cyclic treatment is carried out 3 to 6 times to make the alloy obtain the desired degree of supercooling; S5. Rapidly solidifying the alloy that has been undercooled and solidified into a strip or powder by rapid cooling of the melt or spraying; S6, the obtained strip or powder is annealed to remove internal stress to obtain an iron-based amorphous alloy, or crystallization annealed to obtain an iron-based nanocrystalline alloy.
[0009] Preferably, the inert gas is argon or nitrogen having a purity of 99.9 vol.% or more. Preferably, the crucible has a heat-resistant temperature of 1400° C. or higher. Preferably, the process for preparing the glass purification agent comprises using a powder having a purity of 98% or more. TIFF2024132846000005.tif1052 were weighed and placed in high-purity corundum crucibles, respectively, and fired at 400-600°C for 1-8 hours, and then melted and fired at 800-1000°C for 2-16 hours. TIFF2024132846000006.tif1052 was mixed to obtain the purification agent, and the mass ratio of both was 1:1-20. Preferably, the mass ratio of the glass purifying agent to the alloy ingot is 1:1-5.
[0010] Preferably, the method of electromagnetic suspension melting comprises: S1, the chemical formula of the amorphous nanocrystalline alloy is FeSiBM, where M is one or more elements of P, C, Nb, Mo, Zr, Hf, Mo, Y, Cu and Co; removing oxide film from the alloy raw materials and cleaning them, weighing the raw materials according to a specific mass ratio, and loading the weighed raw materials into a vacuum sensitive melting furnace or a vacuum arc melting furnace, and evacuating the raw materials for 10 minutes. -3 After the pressure reaches 1 Pa, inert gas is introduced to protect the melting process, and the melting is repeated 4 to 6 times to obtain an alloy ingot. S2, vacuum 10 -3 After the pressure reaches 1 Pa, inert gas is introduced for protection, and the alloy ingot is sent under the hanging coil, so that the master alloy is stably suspended in the center of the heating coil under the action of the Lorentz force formed by the interaction between the electromagnetic field and the induced current; S3, the alloy is heated and melted by the heating coil, and the temperature is raised to 1200-1500°C, and the temperature is kept for 1-10 minutes, after which the heating power is turned off and the alloy is allowed to cool naturally; S4, "heating-warming-solidifying" cyclic treatment is carried out 3 to 6 times to make the alloy obtain the desired degree of supercooling; S5, the alloy that has been supercooled and solidified is solidified into a strip-shaped member or powder by a melt rapid cooling method or a spraying method; S6, tempering the obtained strip or powder for stress relief or crystallization to obtain an iron-based nanocrystalline alloy.
[0011] Preferably, the chemical formula of the high iron content amorphous nanocrystalline soft magnetic alloy is FeSiBM, where M is one or more of P, C, Nb, Mo, Zr, Hf, Mo, Y, Cu and Co, and the atomic percentages of each alloying element are as follows: Fe: 80.0-89.0 at%, Si: 1.0-9.0 at%, B: 3.0-12.0 at%, P: 0-5.0 at%, C: 0-5.0 at%, Nb: 0-3.0 at%, Zr: 0-3.0 at%, Hf: 0-3.0 at%, Mo: 0-3.0 at%, Y: 0-5.0 at%, Cu: 0-2.0 at%, Co: 0-16.0 at%, and the total is 100%.
[0012] Preferably, the inert gas is argon or nitrogen having a purity of 99.9 vol.% or more. Preferably, the tempering temperature of the amorphous alloy is within a temperature range of 50-100° C. below the crystallization temperature, and the tempering temperature of the nanocrystal is within a temperature range of 0-100° C. above the crystallization temperature. Preferably, the tempering is carried out in an inert gas atmosphere or in a 10 -1 The process is carried out in a vacuum atmosphere of less than 1 Pa. Effect of the Invention
[0013] The amorphous nanocrystalline soft magnetic alloy prepared by the above non-equilibrium solidification method has high amorphous forming ability, which helps to reduce the amount of amorphous forming elements added in the alloy and increase the content of ferromagnetic element Fe. The amorphous nanocrystalline soft magnetic alloy with high iron content prepared by the above method has soft magnetic properties of high saturation magnetization strength and low coercivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] We now turn to a detailed description of an embodiment of the present invention, in which an amorphous nanocrystalline soft magnetic alloy with high iron content and high saturation magnetization strength is obtained by adjusting the alloy composition and the degree of supercooling. EXAMPLES
[0015] Example 1 Preparation of FeSiB amorphous alloy by supercooling solidification method The FeSiB-based alloys were prepared: alloy 1 had an Fe content of 83.0 at%, Si content of 8.0 at%, and B content of 9.0 at%; alloy 2 had an Fe content of 85.0 at%, Si content of 7.0 at%, and B content of 8.0 at%; and alloy 3 had an Fe content of 88.0 at%, Si content of 3.0 at%, and B content of 9.0 at%. S1, remove the oxide film of the alloy raw materials, wash them, and weigh the raw materials according to a specific mass ratio. The weighed raw materials are loaded into a vacuum arc melting furnace, and the vacuum is 8×10 -4After the pressure reaches 1 Pa, argon gas with a purity of 99.9 vol% is introduced to protect the melting process. The melting process is repeated five times to obtain an alloy ingot. S2, put the alloy ingot into the crucible and heat the top and bottom of it. The alloy ingot is covered with a mixture of purifying glass (TIFF2024132846000007.tif1052) in a mass ratio of 1:5, so that the glass purifying agent completely envelops the alloy ingot. S3, vacuum 5×10 -3 After the pressure reaches 1 Pa, argon gas with a purity of 99.9 vol% is poured in to heat and melt the alloy under its protection, and then the temperature is raised to 1350°C and kept for 2 minutes, after which the heating power is turned off and the alloy is allowed to cool naturally. S4. The "heating-warming-solidification" cyclic treatment is carried out four and six times respectively, so that the alloy achieves a supercooling degree of about 190℃ and 260℃. S5, the alloy that has undergone undercooling solidification is rapidly cooled through the melt and solidified into a strip-shaped member. S6, the obtained strip-shaped member is tempered at 300°C to relieve stress, to obtain an iron-based amorphous alloy.
[0016] The saturation magnetization strength and coercivity of the alloys at various degrees of undercooling are given in the following table. Table 1 Saturation magnetization and coercivity of FeSiB-based amorphous alloys at various degrees of supercooling JPEG2024132846000008.jpg191135 EXAMPLES
[0017] Example 2 Preparation of FeSiBPC amorphous alloy by supercooling solidification method The FeSiBPC alloys were prepared, with alloy 1 having an Fe content of 84.0 at%, Si content of 2.0 at%, B content of 8.0 at%, P content of 5.0 at%, and C content of 1.0 at%; alloy 2 having an Fe content of 84.0 at%, Si content of 2.0 at%, B content of 8.0 at%, P content of 1.0 at%, and C content of 5.0 at%; and alloy 3 having an Fe content of 89.0 at%, Si content of 2.0 at%, B content of 8.0 at%, P content of 0.5 at%, and C content of 0.5 at%. S1, remove the oxide film of the alloy raw materials, wash them, and weigh the raw materials according to a specific mass ratio. The weighed raw materials are loaded into a vacuum arc melting furnace, and the vacuum is 7×10 -4 After the pressure reaches 1 Pa, melting is performed under the protection of nitrogen gas with a purity of 99.9 vol%. Melting is repeated six times to obtain an alloy ingot. S2, put the alloy ingot into the crucible and heat the top and bottom of it. The alloy ingot is then covered with a mixture of purifying glass (TIFF2024132846000009.tif1052) in a mass ratio of 1:4, so that the glass purifying agent completely envelops the alloy ingot. S3, vacuuming is 4x10 -3 After the pressure reaches 1 Pa, nitrogen gas with a purity of 99.9 vol% is poured in to protect the alloy and heat it to melt, then the temperature is raised to 1400°C and kept for 3 minutes, after which the heating power is turned off and the alloy is allowed to cool naturally. S4. The "heating-warming-solidification" cyclic treatment is carried out four and six times respectively, so that the alloy achieves a supercooling degree of about 160℃ and 255℃. S5, the alloy that has undergone undercooling solidification is rapidly cooled through the melt and solidified into a strip-shaped member. S6, the obtained strip-shaped member is tempered at 300°C to relieve stress, to obtain an iron-based amorphous alloy.
[0018] The saturation magnetization strength and coercivity of the alloys at various degrees of undercooling are given in the following table. Table 2 Saturation magnetization and coercivity of FeSiBPC amorphous alloys at various degrees of undercooling JPEG2024132846000010.jpg191135 EXAMPLES
[0019] Example 3 Preparation of FeSiBC amorphous alloy by supercooling solidification method The FeSiBC-based alloys were prepared, with alloy 1 having an Fe content of 84.0 at%, Si content of 2.0 at%, B content of 8.0 at%, and C content of 6.0 at%; alloy 2 having an Fe content of 85.0 at%, Si content of 2.0 at%, B content of 8.0 at%, and C content of 5.0 at%; and alloy 3 having an Fe content of 89.0 at%, Si content of 2.0 at%, B content of 8.0 at%, and C content of 1.0 at%. S1, remove the oxide film of the alloy raw materials, wash them, and weigh the raw materials according to a specific mass ratio. The weighed raw materials are loaded into a vacuum sensitive melting furnace or a vacuum arc melting furnace, and the vacuum is 8×10 -4 After the pressure reaches 1 Pa, inert gas is introduced to protect the melting process, and the melting is repeated six times to obtain an alloy ingot. S2, vacuuming is 4x10 -3 After the pressure reaches 1 Pa, nitrogen gas with a purity of 99.9 vol% is injected for protection, and the alloy ingot is sent under the hanging coil, and the master alloy is stably suspended in the center of the heating coil under the action of the Lorentz force formed by the interaction between the electromagnetic field and the induced current. S3, the heating coil heats and melts the alloy, thus raising the temperature to 1500°C, keeping it at that temperature for 5 minutes, and then turning off the heating power to allow the alloy to cool naturally. S4. The "heating-warming-solidification" cyclic treatment is carried out three and five times respectively, so that the alloy achieves a supercooling degree of about 150℃ and 225℃. S5, the alloy that has undergone undercooling solidification is rapidly cooled through the melt and solidified into a strip-shaped member. S6, the obtained strip-shaped member is tempered at 300°C to crystallize, to obtain an iron-based amorphous alloy.
[0020] The saturation magnetization strength and coercivity of the alloys at various degrees of undercooling are given in the following table. Table 3. Saturation magnetization and coercivity of FeSiBC amorphous alloys at various degrees of supercooling JPEG2024132846000011.jpg191135 EXAMPLES
[0021] Example 4 Preparation of nanocrystalline FeSiBCu alloys by undercooling solidification method The FeSiBCu alloys were prepared, with alloy 1 having an Fe content of 80.5 at%, Si content of 7.0 at%, B content of 12.0 at%, and Cu content of 0.5 at%, alloy 2 having an Fe content of 85.0 at%, Si content of 2.5 at%, B content of 12.0 at%, and Cu content of 0.5 at%, and alloy 3 having an Fe content of 85.0 at%, Si content of 1.2 at%, B content of 12.0 at%, and Cu content of 1.8 at%, respectively. S1, remove the oxide film of the alloy raw materials, wash them, and weigh the raw materials according to a specific mass ratio. The weighed raw materials are loaded into a vacuum sensitive melting furnace, and the vacuum is 9×10 -4 After the pressure reaches 1 Pa, argon gas with a purity of 99.9 vol% is introduced to protect the melting process. The melting process is repeated four times to obtain an alloy ingot. S2, put the alloy ingot into the crucible and heat the top and bottom of it. The alloy ingot is then covered with a mixture of purifying glass (TIFF2024132846000012.tif1052) in a mass ratio of 1:20, so that the glass purifying agent completely envelops the alloy ingot. S3, vacuum 5×10 -3 After the pressure reaches 1 Pa, argon gas with a purity of 99.9 vol% is poured in to heat and melt the alloy under its protection, and then the temperature is raised to 1320°C and kept for 5 minutes, after which the heating power is turned off and the alloy is allowed to cool naturally. S4. The "heating-warming-solidification" cyclic treatment is carried out three and four times respectively, so that the alloy achieves a supercooling degree of about 205℃ and 255℃. S5, the alloy that has undergone undercooling solidification is rapidly cooled through the melt and solidified into a strip-shaped member. S6, the obtained strip is tempered at 450°C to relieve stress, to obtain an iron-based nanocrystalline alloy.
[0022] The saturation magnetization strength and coercivity of the alloys at various degrees of undercooling are given in the following table. Table 4. Saturation magnetization and coercivity of FeSiBCu nanocrystalline alloys at various degrees of undercooling JPEG2024132846000013.jpg191135 EXAMPLES
[0023] Example 5 Preparation of nanocrystalline FeSiBNbCu alloys by undercooling solidification method The FeSiBNbCu alloys were prepared, with alloy 1 having an Fe content of 80.0 at%, Si content of 7.0 at%, B content of 9.0 at%, Nb content of 3.0 at%, and Cu content of 1.0 at%, alloy 2 having an Fe content of 82.0 at%, Si content of 6.0 at%, B content of 9.0 at%, Nb content of 2.0 at%, and Cu content of 1.0 at%, and alloy 3 having an Fe content of 85.0 at%, Si content of 4.5 at%, B content of 9.0 at%, Nb content of 0.5 at%, and Cu content of 1.0 at%,. S1, remove the oxide film of the alloy raw materials, wash them, and weigh the raw materials according to a specific mass ratio. The weighed raw materials are loaded into a vacuum arc melting furnace, and the vacuum is 8×10 -4 After the pressure reaches 1 Pa, argon gas with a purity of 99.9 vol% is introduced to protect the melting process. The melting process is repeated six times to obtain an alloy ingot. S2, put the alloy ingot into the crucible and heat the top and bottom of it. The alloy ingot is then covered with a mixture of purifying glass (TIFF2024132846000014.tif1052) in a mass ratio of 1:10, so that the glass purifying agent completely envelops the alloy ingot. S3, vacuuming is 8x10 -3After the pressure reaches 1 Pa, nitrogen gas with a purity of 99.9 vol% is poured in to protect the alloy and heat it to melt, then the temperature is raised to 1380°C and kept for 1 minute, after which the heating power is turned off and the alloy is allowed to cool naturally. S4. The "heating-warming-solidification" cyclic treatment is carried out five and six times respectively, so that the alloy achieves a supercooling degree of about 190℃ and 225℃. S5, the alloy that has undergone undercooling solidification is rapidly cooled through the melt and solidified into a strip-shaped member. S6, the obtained strip is tempered at 550°C to relieve stress, to obtain an iron-based nanocrystalline alloy.
[0024] The saturation magnetization strength and coercivity of the alloys at various degrees of undercooling are given in the following table. Table 5. Saturation magnetization and coercivity of FeSiBNbCu nanocrystalline alloys at various degrees of undercooling JPEG2024132846000015.jpg191135 EXAMPLES
[0025] Example 6 Preparation of FeSiBMoCu nanocrystalline alloys by supercooling solidification method The FeSiBMoCu alloys were prepared, with alloy 1 having an Fe content of 80.0 at%, Si content of 7.0 at%, B content of 9.0 at%, Mo content of 3.0 at%, and Cu content of 1.0 at%; alloy 2 having an Fe content of 82.0 at%, Si content of 6.0 at%, B content of 9.0 at%, Mo content of 2.0 at%, and Cu content of 1.0 at%; and alloy 3 having an Fe content of 83.3 at%, Si content of 5.0 at%, B content of 9.0 at%, Mo content of 0.7 at%, and Cu content of 1.0 at%. S1, remove the oxide film of the alloy raw materials, clean them, and weigh the raw materials according to a specific mass ratio. The weighed raw materials are loaded into a vacuum sensitive melting furnace, and the vacuum is 8×10 -4After the pressure reaches 1 Pa, argon gas with a purity of 99.9 vol% is introduced to protect the melting process. The melting process is repeated four times to obtain an alloy ingot. S2, put the alloy ingot into the crucible and heat the top and bottom of it. The alloy ingot is then covered with a mixture of purifying glass (TIFF2024132846000016.tif1052) in a mass ratio of 1:1, so that the glass purifying agent completely envelops the alloy ingot. S3, vacuuming is 1×10 -2 After the pressure reaches 1 Pa, argon gas with a purity of 99.9 vol% is poured in to heat and melt the alloy under its protection, and then the temperature is raised to 1370°C and kept for 6 minutes, after which the heating power is turned off and the alloy is allowed to cool naturally. S4. The "heating-warming-solidification" cyclic treatment is carried out three and five times respectively, so that the alloy achieves a supercooling degree of about 175℃ and 255℃. S5, the alloy that has undergone undercooling solidification is rapidly cooled through the melt and solidified into a strip-shaped member. S6, the obtained strip is tempered at 500°C to relieve stress, to obtain an iron-based nanocrystalline alloy.
[0026] The saturation magnetization strength and coercivity of the alloys at various degrees of undercooling are given in the following table. Table 6. Saturation magnetization and coercivity of FeSiBMoCu nanocrystalline alloys at various degrees of undercooling JPEG2024132846000017.jpg191135 EXAMPLES
[0027] Example 7 Preparation of FeCoSiBCCu nanocrystalline alloys by supercooling solidification method The FeCoSiBCu alloys were prepared, with alloy 1 having an Fe content of 80.0 at%, Co content of 5.0 at%, Si content of 1.5 at%, B content of 9.0 at%, C content of 3.0 at%, and Cu content of 1.5 at%; alloy 2 having an Fe content of 80.0 at%, Co content of 5.0 at%, Si content of 1.5 at%, B content of 9.0 at%, C content of 3.0 at%, and Cu content of 1.5 at%; alloy 3 having an Fe content of 80.0 at%, Co content of 5.0 at%, Si content of 1.5 at%, B content of 9.0 at%, C content of 3.0 at%, and Cu content of 1.5 at%. S1, remove the oxide film of the alloy raw materials, wash them, and weigh the raw materials according to a specific mass ratio. The weighed raw materials are loaded into a vacuum arc melting furnace, and the vacuum is 8×10 -4 After the pressure reaches 1 Pa, argon gas with a purity of 99.9 vol% is introduced to protect the melting process. The melting process is repeated five times to obtain an alloy ingot. S2, put the alloy ingot into the crucible and heat the top and bottom of it. The alloy ingot is then covered with a mixture of purifying glass (TIFF2024132846000018.tif1052) in a mass ratio of 1:3, so that the glass purifying agent completely envelops the alloy ingot. S3, vacuuming is 8x10 -3 After the pressure reaches 1 Pa, nitrogen gas with a purity of 99.9 vol% is poured in to heat and melt the alloy under its protection, then the temperature is raised to 1350°C and kept for 8 minutes, after which the heating power is turned off and the alloy is allowed to cool naturally. S4. The "heating-warming-solidification" cyclic treatment is carried out three and six times respectively, so that the alloy achieves a supercooling degree of about 150℃ and 265℃. S5, the alloy that has undergone undercooling solidification is rapidly cooled through the melt and solidified into a strip-shaped member. S6, the obtained strip is tempered at 400°C to relieve stress, to obtain an iron-based nanocrystalline alloy.
[0028] The saturation magnetization strength and coercivity of the alloys at various degrees of undercooling are given in the following table. Table 7. Saturation magnetization and coercivity of FeCoSiBCCu nanocrystalline alloys at various degrees of undercooling JPEG2024132846000019.jpg191135 EXAMPLES
[0029] Example 8 Preparation of nanocrystalline FeSiBZrHfCu alloys by undercooling solidification method The FeSiBZrHfCu alloys were prepared, with alloy 1 having an Fe content of 80.0 at%, Si content of 6.0 at%, B content of 9.0 at%, Zr content of 3.0 at%, Hf content of 1.0 at%, and Cu content of 1.0 at%; alloy 2 having an Fe content of 80.0 at%, Si content of 6.0 at%, B content of 9.0 at%, Zr content of 1.0 at%, Hf content of 3.0 at%, and Cu content of 1.0 at%; and alloy 3 having an Fe content of 87.0 at%, Si content of 2.0 at%, B content of 9.0 at%, Zr content of 0.5 at%, Hf content of 0.5 at%, and Cu content of 1.0 at%. S1, remove the oxide film of the alloy raw materials, wash them, and weigh the raw materials according to a specific mass ratio. The weighed raw materials are loaded into a vacuum sensitive melting furnace or a vacuum arc melting furnace, and the vacuum is 8×10 -4 After the pressure reaches 1 Pa, inert gas is introduced to protect the melting process, and the melting is repeated six times to obtain an alloy ingot. S2, vacuuming is 4x10 -3 After the pressure reaches 1 Pa, nitrogen gas with a purity of 99.9 vol% is injected for protection, and the alloy ingot is sent under the hanging coil, and the master alloy is stably suspended in the center of the heating coil under the action of the Lorentz force formed by the interaction between the electromagnetic field and the induced current. S3. The heating coil heats and melts the alloy, thus raising the temperature to 1400°C, keeping it at that temperature for 10 minutes, and then turning off the heating power to allow the alloy to cool naturally. S4. The "heating-warming-solidification" cyclic treatment is carried out four and six times respectively, so that the alloy achieves a supercooling degree of about 210℃ and 270℃. S5, the alloy that has undergone undercooling solidification is rapidly cooled through the melt and solidified into a strip-shaped member. S6, the obtained strip is tempered at 550°C to crystallize, to obtain an iron-based nanocrystalline alloy.
[0030] The saturation magnetization strength and coercivity of the alloys at various degrees of undercooling are given in the following table. Table 8. Saturation magnetization and coercivity of nanocrystalline FeSiBZrHfCu alloys at various degrees of undercooling JPEG2024132846000020.jpg191135 EXAMPLES
[0031] Example 9 Preparation of FeSiBYCu nanocrystalline alloys by supercooling solidification method The FeSiBYCu alloys were prepared, with alloy 1 having an Fe content of 81.0 at%, Si content of 4.0 at%, B content of 9.0 at%, Y content of 5.0 at%, and Cu content of 1.0 at%, alloy 2 having an Fe content of 84.0 at%, Si content of 4.0 at%, B content of 9.0 at%, Y content of 2.0 at%, and Cu content of 1.0 at%, and alloy 3 having an Fe content of 87.0 at%, Si content of 2.0 at%, B content of 9.0 at%, Y content of 1.0 at%, and Cu content of 1.0 at%,. S1, remove the oxide film of the alloy raw materials, wash them, and weigh the raw materials according to a specific mass ratio. The weighed raw materials are loaded into a vacuum arc melting furnace, and the vacuum is 8×10 -4 After the pressure reaches Pa, inert gas is introduced to protect the melting process, and the melting is repeated four times to obtain an alloy ingot. S2, vacuum 5×10 -3After the pressure reaches 1 Pa, argon gas with a purity of 99.9 vol% is introduced for protection, and the alloy ingot is sent under the hanging coil, where the master alloy is stably suspended in the center of the heating coil under the action of the Lorentz force formed by the interaction between the electromagnetic field and the induced current. S3. The heating coil heats and melts the alloy, thus raising the temperature to 1500°C, keeping it at that temperature for 3 minutes, and then turning off the heating power to allow the alloy to cool naturally. S4. The "heating-warming-solidification" cyclic treatment is carried out three and six times respectively, so that the alloy achieves a supercooling degree of about 180℃ and 255℃. S5, the alloy that has undergone undercooling solidification is rapidly cooled through the melt and solidified into a strip-shaped member. S6, the obtained strip is tempered at 500°C to crystallize, to obtain an iron-based nanocrystalline alloy.
[0032] The saturation magnetization strength and coercivity of the alloys at various degrees of undercooling are given in the following table. Table 9. Saturation magnetization and coercivity of nanocrystalline FeSiBYCu alloys at various degrees of undercooling JPEG2024132846000021.jpg191135
[0033] In summary, the technical effect of the present invention is to improve the amorphous forming ability of iron-based alloys by combining glass purification with cyclic heating or by using electromagnetic suspension melting, to achieve the goal of reducing the content of amorphous forming elements and increasing the content of ferromagnetic elements, and to obtain an amorphous nanocrystalline soft magnetic alloy with both high saturation magnetization strength and low coercivity. The principle of achieving this technical effect is that in the process of combining glass purification with cyclic heating, not only can the molten glass adsorb the heterogeneous nucleation points of the molten alloy, but also the superheating and heating-warming-cooling cold and hot cycles can thermally decompose the heterogeneous nucleation points at high temperatures, and cause material exchange in the process of thermal convection inside and on the surface, effectively reducing the heterogeneous nucleation points inside the alloy. In the process of electromagnetic suspension melting, the introduction of impurities into the alloy during the melting process is effectively avoided by containerless melting, and the heterogeneous nucleation points inside the alloy are thermally decomposed by high temperature superheating. Both methods can reduce or avoid crystallization and improve the amorphous forming ability. On the one hand, reducing the number of heterogeneous nucleation sites can optimize the microstructure of the alloy, weaken the destructive effect on the magnetic exchange coupling effect, and increase the saturation magnetization strength of the alloy. On the other hand, improving the amorphous forming ability of the alloy promotes the formation of more disordered amorphous structures, effectively eliminating the magnetocrystalline anisotropy, and also reduces or avoids the obstacle of heterogeneous nucleation sites to magnetic reversal, resulting in low coercivity.
Claims
1. By combining glass purification with cyclic heating or electromagnetic suspension melting, the alloy is supercooled and solidified, the amount of non-magnetic elements added to the iron-based amorphous nanocrystalline soft magnetic alloy is reduced, and the proportion of Fe element is increased, thereby achieving the goal of increasing the saturation magnetization strength and decreasing the coercive force. A supercooling solidification method for preparing an amorphous nanocrystalline soft magnetic alloy with a high iron content, characterized in that
2. The method of combining the above-mentioned glass purification with cyclic heating comprises the steps of: S1, the chemical formula of the amorphous nanocrystalline alloy is FeSiBM, where M is one or more elements of P, C, Nb, Mo, Zr, Hf, Mo, Y, Cu and Co; The oxide film of the alloy raw materials is removed and washed, the raw materials are weighed according to a specific mass ratio, and the weighed raw materials are loaded into a vacuum sensitive melting furnace or a vacuum arc melting furnace, and the vacuum is maintained for 10 minutes. -3 After the pressure reaches Pa, melting is performed under the protection of an inert gas, and melting is repeated 4 to 6 times to obtain an alloy ingot. S2. Putting the alloy ingot into a crucible, and covering its upper and lower surfaces with a glass purifier in a specific mass ratio, so as to completely enclose the alloy ingot in the glass purifier; S3, vacuum 10 -2 After the pressure reaches Pa, inert gas is introduced to heat and melt the alloy under its protection, and then the temperature is raised to 1200-1500°C, kept at that temperature for 1-10 minutes, and the heating power is turned off to allow the alloy to cool naturally; S4. Carry out the "heating-warming-solidification" cyclic process 3 to 6 times to allow the alloy to obtain a desired degree of undercooling; S5. Rapidly solidifying the alloy that has been supercooled and solidified into a strip-shaped member or powder by a melt rapid cooling method or a spraying method; S6, annealing the obtained strip or powder to remove internal stress to obtain an iron-based amorphous alloy, or crystallization annealing to obtain an iron-based nanocrystalline alloy; 2. The supercooling solidification method according to claim 1 .
3. 3. The method according to claim 2, wherein the inert gas is argon or nitrogen having a purity of 99.9 vol % or more.
4. 3. The method according to claim 2, wherein the crucible has a heat-resistant temperature of 1400° C. or higher.
5. The preparation process of the glass purification agent is a powder with a purity of 98% or more. Weighed and placed in a high purity steel crucible, each was fired at 400-600°C for 1-8 hours, and then melted and fired at 800-1000°C for 2-16 hours. and mixing the two to obtain a purification agent, and the mass ratio of the two is 1:1-20.
3. The supercooling solidification method according to claim 2 .
6. 3. The method according to claim 2, wherein a mass ratio of the glass purifying agent to the alloy ingot is 1:1-5.
7. The method of electromagnetic suspension melting is as follows: S1, the chemical formula of the amorphous nanocrystalline alloy is FeSiBM, where M is one or more elements of P, C, Nb, Mo, Zr, Hf, Mo, Y, Cu and Co; The oxide film of the alloy raw materials is removed and washed, the raw materials are weighed according to a specific mass ratio, and the weighed raw materials are loaded into a vacuum sensitive melting furnace or a vacuum arc melting furnace, and the vacuum is maintained for 10 minutes. -3 After the pressure reaches Pa, melting is performed under the protection of an inert gas, and melting is repeated 4 to 6 times to obtain an alloy ingot. S2, vacuum 10 -3 After the pressure reaches 1 Pa, inert gas is introduced for protection, and the alloy ingot is sent under the hanging coil, so that the master alloy is stably suspended in the center of the heating coil under the action of the Lorentz force formed by the interaction between the electromagnetic field and the induced current; S3, the alloy is heated and melted by the induction of the heating coil, and the temperature is raised to 1200-1500°C, and the temperature is kept for 1-10 minutes, after which the heating power supply is turned off and the alloy is allowed to cool naturally; S4. Carry out the "heating-warming-solidification" cyclic process 3 to 6 times to allow the alloy to obtain a desired degree of undercooling; S5. Solidifying the alloy that has been supercooled and solidified into a strip-shaped member or powder by a melt rapid cooling method or a spraying method; S6. Tempering the obtained strip or powder to relieve stress or crystallize to obtain an iron-based nanocrystalline alloy.
2. The supercooling solidification method according to claim 1 .
8. The high iron content amorphous nanocrystalline soft magnetic alloy has a chemical formula of FeSiBM, where M is one or more of P, C, Nb, Mo, Zr, Hf, Mo, Y, Cu and Co, and the atomic percentages of each alloying element are as follows: Fe: 80.0-89.0 at%, Si: 1.0-9.0 at%, B: 3.0-12.0 at%, P: 0-5.0 at%, C: 0-5.0 at%, Nb: 0-3.0 at%, Zr: 0-3.0 at%, Hf: 0-3.0 at%, Mo: 0-3.0 at%, Y: 0-5.0 at%, Cu: 0-2.0 at%, Co: 0-16.0 at%, and the total is 100%.
8. The supercooling solidification method according to claim 2 or 7.
9. 8. The method according to claim 7, wherein the inert gas is argon or nitrogen having a purity of 99.9 vol % or more.
10. The supercooling solidification method according to claim 7, characterized in that the tempering temperature of the amorphous alloy is within a temperature range of 50 to 100°C below the crystallization temperature, and the tempering temperature of the nanocrystal is within a temperature range of 0 to 100°C above the crystallization temperature.
11. Tempering is done in an inert gas atmosphere or 10 -1 11. The supercooling solidification method according to claim 10, wherein the method is carried out in an atmosphere with a degree of vacuum of 0.1 Pa or less.
Citation Information
Patent Citations
Preparation method of Fe-B block nano soft magnetic material
CN103898394A
Iron-based amorphous alloys with high saturation magnetic induction and strong amorphous forming ability
CN105088107B
Manufacturing method of block Fe-B directional nano soft magnetic material
CN108611542A
Manufacture of metal powder from molten metal material
JP1984208003A
Magnetic alloy, amorphous alloy thin band, and magnetic component