Phase modulator and manufacturing method for the same

By using transparent electrodes within cavities in the cladding layer to reduce light absorption, the phase modulator achieves a wider scan angle and smaller optical phased array design with reduced optical loss, enhancing LiDAR performance.

JP2024134350APending Publication Date: 2024-10-03KK TOYOTA CHUO KENKYUSHO +3
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023044608
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Reducing the pitch distance between adjacent optical waveguides in a phase modulator to widen the scan angle of a light beam leads to increased optical loss due to light absorption by electrodes.

Method used

Employing transparent electrodes filled in cavities within the cladding layer to minimize light absorption, with a manufacturing process that includes forming cavities and planarizing the electrodes to ensure they are flush with the cladding layer surface, thereby reducing optical loss.

Benefits of technology

The use of transparent electrodes allows for a wider scan angle and smaller optical phased array design while maintaining light intensity, suitable for applications like LiDAR devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134350000001_ABST
    Figure 2024134350000001_ABST
Patent Text Reader

Abstract

To provide a technique of suppressing the absorption of propagation light in an electrode in a phase modulator.SOLUTION: A phase modulator includes a semiconductor layer including an optical waveguide, a clad layer provided on the semiconductor layer and including a first cavity and a second cavity, a first electrode in contact with an upper surface of the semiconductor layer through the first cavity, and a second electrode in contact with the upper surface of the semiconductor layer through the second cavity. The first electrode includes a first transparent electrode filling the first cavity. The second electrode includes a second transparent electrode filling the second cavity. An upper surface of the first transparent electrode is the same plane as an upper surface of the clad layer. An upper surface of the second transparent electrode is the same plane as the upper surface of the clad layer.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The technology disclosed in this specification relates to a phase modulator used in an optical phased array (OPA). [Background technology]

[0002] Patent Documents 1 to 3 disclose an example of a phase modulator used in an optical phased array. This type of phase modulator includes a semiconductor layer including an optical waveguide and an electrode in contact with the semiconductor layer. The electrode includes a first electrode in contact with the semiconductor layer and a second electrode in contact with the semiconductor layer and disposed away from the first electrode. The optical waveguide is configured such that its refractive index or optical absorptance changes when a voltage is applied between the first electrode and the second electrode. When the refractive index or optical absorptance changes, the phase of the propagating light propagating through the optical waveguide changes.

[0003] The optical phased array is configured to generate a plurality of propagating lights having a phase difference between each other by using such a phase modulator, and to output each of the plurality of propagating lights from a corresponding transmitting antenna. The plurality of propagating lights output from the transmitting antenna become a light beam having a specific deflection angle. The deflection angle of the light beam depends on the phase difference of the plurality of propagating lights. For this reason, the optical phased array having the phase modulator can scan the output light beam by controlling the voltage applied between the first electrode and the second electrode. In this way, the optical phased array having the phase modulator has a feature that the deflection angle of the light beam can be changed without using, for example, a mechanical mirror structure. Such an optical phased array can be mounted on, for example, a LiDAR (Light Detection and Ranging) device. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] U.S. Patent Publication No. 2021 / 0026216 [Patent Document 2] Patent Publication No. 2021-103147 [Patent Document 3] JP 2020-166061 A Summary of the Invention [Problem to be solved by the invention]

[0005] In order to widen the scan angle of the light beam emitted from the transmitting antenna, the pitch distance between adjacent optical waveguides must be reduced. However, according to the study by the present inventors, it has been found that when the pitch distance between adjacent optical waveguides is reduced, a problem occurs in which a part of the propagating light propagating through the optical waveguide is absorbed by the electrodes, resulting in increased optical loss. This specification provides a technology for suppressing the absorption of propagating light by the electrodes in a phase modulator. [Means for solving the problem]

[0006] The phase modulator disclosed in the present specification may include a semiconductor layer including an optical waveguide, a cladding layer provided on the semiconductor layer, the cladding layer including a first cavity exposing a part of the upper surface of the semiconductor layer and a second cavity exposing another part of the upper surface of the semiconductor layer, a first electrode contacting the upper surface of the semiconductor layer through the first cavity, and a second electrode contacting the upper surface of the semiconductor layer through the second cavity. The optical waveguide may be disposed between a position where the first electrode contacts the upper surface of the semiconductor layer and a position where the second electrode contacts the upper surface of the semiconductor layer, and may be configured such that a phase of propagating light changes when a voltage is applied between the first electrode and the second electrode. The first electrode may include a first transparent electrode filled in the first cavity. The second electrode may include a second transparent electrode filled in the second cavity. The upper surface of the first transparent electrode may be flush with the upper surface of the cladding layer. An upper surface of the second transparent electrode may be flush with an upper surface of the cladding layer. According to this phase modulator, since at least a portion of each of the first electrode and the second electrode includes a transparent electrode, it is possible to suppress absorption of propagating light by the first electrode and the second electrode.

[0007] A method for manufacturing a phase modulator disclosed in the present specification may include an optical waveguide forming step of forming an optical waveguide in a semiconductor layer, a transparent electrode film forming step of forming a transparent electrode film on the semiconductor layer, the transparent electrode film having a first transparent electrode and a second transparent electrode arranged apart from each other, a cladding layer forming step of forming a cladding layer on the semiconductor layer so as to cover the first transparent electrode and the second transparent electrode, and a planarizing step of planarizing the cladding layer until an upper surface of the first transparent electrode filled in the first cavity of the cladding layer and an upper surface of the second transparent electrode filled in the second cavity of the cladding layer are exposed. According to this manufacturing method, a phase modulator in which absorption of propagating light is suppressed can be manufactured.

[0008] Another method for manufacturing a phase modulator disclosed in the present specification may include an optical waveguide forming step of forming an optical waveguide in a semiconductor layer, a cladding layer forming step of forming a cladding layer on the semiconductor layer, the cladding layer having a first cavity exposing a part of the upper surface of the semiconductor layer and a second cavity exposing another part of the upper surface of the semiconductor layer, a transparent electrode film forming step of forming a transparent electrode film on the cladding layer, the transparent electrode film having a first transparent electrode filling the first cavity and a second transparent electrode filling the second cavity, and a planarizing step of planarizing the transparent electrode film until the first transparent electrode filling the first cavity of the cladding layer and the second transparent electrode filling the second cavity of the cladding layer are exposed. According to this manufacturing method, a phase modulator in which absorption of propagating light is suppressed can be manufactured. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic perspective view of a main part of an optical phased array. [Diagram 2] FIG. 1 is a schematic cross-sectional view of a main portion of an embodiment of a phase modulator. [Diagram 3] 3A to 3C are schematic cross-sectional views of a main part of the phase modulator shown in FIG. 2 during a manufacturing process according to a first manufacturing method. [Figure 4] 3A to 3C are schematic cross-sectional views of a main part of the phase modulator shown in FIG. 2 during a manufacturing process according to a first manufacturing method. [Diagram 5] 3A to 3C are schematic cross-sectional views of a main part of the phase modulator shown in FIG. 2 during a manufacturing process according to a first manufacturing method. [Figure 6] 3A to 3C are schematic cross-sectional views of a main part of the phase modulator shown in FIG. 2 during a manufacturing process according to a first manufacturing method. [Figure 7] 3A to 3C are schematic cross-sectional views of a main part of the phase modulator shown in FIG. 2 during a manufacturing process according to a first manufacturing method. [Figure 8] 3A to 3C are schematic cross-sectional views of a main part of the phase modulator shown in FIG. 2 during a manufacturing process according to a first manufacturing method. [Figure 9] 3A to 3C are schematic cross-sectional views of a main part of the phase modulator shown in FIG. 2 during a manufacturing process according to a first manufacturing method. [Figure 10] 3A to 3C are schematic cross-sectional views of a main part of the phase modulator shown in FIG. 2 during a manufacturing process according to a second manufacturing method. [Figure 11] 3A to 3C are schematic cross-sectional views of a main part of the phase modulator shown in FIG. 2 during a manufacturing process according to a second manufacturing method. [Figure 12] 3A to 3C are schematic cross-sectional views of a main part of the phase modulator shown in FIG. 2 during a manufacturing process according to a second manufacturing method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] (Configuration of optical phased array) 1, the optical phased array 1 includes an optical waveguide 4, a distributor 6, a phase modulator 8, and a transmitting antenna 9. The optical waveguide 4, distributor 6, phase modulator 8, and transmitting antenna 9 are configured on a substrate 2 as an optical integrated circuit.

[0011] The distributor 6 is configured to split the optical waveguide 4 into a plurality of beams, and splits the propagating light input to the optical waveguide 4 into a plurality of propagating lights of the same phase. Each of the split propagating lights is phase-modulated by the phase modulator 8. The phase-modulated propagating lights are input to the transmitting antenna 9. The transmitting antenna 9 includes a diffraction grating provided corresponding to each of the optical waveguides 4, and outputs the phase-modulated propagating lights as a light beam toward the outside. The phase modulator 8 of the optical phased array 1 can control the phase difference between the propagating lights and adjust the deflection angle of the output light beam. Such an optical phased array 1 is mounted, for example, in a LiDAR device, although it is not particularly limited thereto.

[0012] (Structure of phase modulator) Hereinafter, the phase modulator 8 will be described with reference to the drawings. For clarity of illustration, reference numerals may be attached only to some of the repeatedly arranged structures.

[0013] As shown in FIG. 1 and FIG. 2, the phase modulator 8 includes a plurality of optical waveguides 4 formed on a substrate 2. The optical waveguides 4 are arranged adjacent to each other in the x direction. Each of the optical waveguides 4 extends between the distributor 6 and the transmitting antenna 9 along the y direction. The x direction indicates one direction parallel to the main surface 2S of the substrate 2, the y direction indicates a direction parallel to the main surface 2S of the substrate 2 and perpendicular to the x direction, and the z direction indicates a direction perpendicular to the main surface 2S of the substrate 2 (perpendicular to each of the x direction and the y direction). As shown in FIG. 2, the portion surrounded by the dashed line is a unit 10 constituting the phase modulator 8. The distance between adjacent optical waveguides 4 is referred to as a pitch distance 10D. Hereinafter, the unit 10 will be described as a phase modulator 8.

[0014] The phase modulator 8 includes a substrate 2, a cladding layer 16 provided on the substrate 2, a first electrode 40, and a second electrode 50. The substrate 2 includes an insulating layer 12 and a semiconductor layer 14 laminated on the insulating layer 12. The material of the insulating layer 12 is not particularly limited, but may be, for example, silicon oxide (SiO2). The material of the semiconductor layer 14 is not particularly limited, but may be, for example, silicon. The semiconductor layer 14 includes an optical waveguide 4, a p-type semiconductor region 22, and an n-type semiconductor region 32.

[0015] The optical waveguide 4 is provided at a position exposed to one of the principal surfaces 2S of the semiconductor layer 14. In this example, the optical waveguide 4 is a non-doped region formed as a part of the semiconductor layer 14. Alternatively, the optical waveguide 4 may be formed of a semiconductor material different from that of the semiconductor layer 14, for example, silicon nitride. The optical waveguide 4 is disposed between the first electrode 40 and the second electrode 50 when viewed from the z-axis direction (hereinafter, referred to as "when viewed in plan"). The optical waveguide 4 is also provided between the p-type semiconductor region 22 and the n-type semiconductor region 32 when the substrate 2 is viewed in plan. The optical waveguide 4 has a protruding portion 4A protruding from the principal surface 2S of the semiconductor layer 14. When the optical waveguide 4 has the protruding portion 4A, the protruding portion 4A is covered with the cladding layer 16, and the propagating light is effectively confined within the optical waveguide 4. The protruding portion 4A may not be formed as necessary.

[0016] The p-type semiconductor region 22 is provided at a position exposed on one main surface 2S of the semiconductor layer 14, and is disposed between the first electrode 40 and the optical waveguide 4. The p-type semiconductor region 22 contacts both the first electrode 40 and the optical waveguide 4. When viewed in a plan view, the p-type semiconductor region 22 extends along the direction in which the optical waveguide 4 extends, i.e., the y direction. The p-type semiconductor region 22 may have a high concentration region in which the p-type impurity concentration is adjusted to be high in a portion in contact with the first electrode 40.

[0017] The n-type semiconductor region 32 is provided at a position exposed to one main surface 2S of the semiconductor layer 14, and is disposed between the second electrode 50 and the optical waveguide 4. The n-type semiconductor region 32 contacts both the second electrode 50 and the optical waveguide 4. When viewed in a plan view, the n-type semiconductor region 32 extends along the direction in which the optical waveguide 4 extends, i.e., the y direction. The n-type semiconductor region 32 may have a high concentration region in which the n-type impurity concentration is adjusted to be high in a portion in contact with the second electrode 50.

[0018] The cladding layer 16 is provided so as to cover one of the principal surfaces 2S of the semiconductor layer 14. The cladding layer 16 is made of a material having a smaller refractive index than the optical waveguide 4. The material of the cladding layer 16 is not particularly limited, and may be, for example, silicon oxide (SiO2). A first cavity 24 and a second cavity 34 are formed in the cladding layer 16. The first cavity 24 penetrates the cladding layer 16 and is formed so as to expose a part of the range of one of the principal surfaces 2S of the semiconductor layer 14 in which the p-type semiconductor region 22 is formed. The first cavity 24 extends in a plan view in the direction in which the optical waveguide 4 extends, that is, along the y direction. The second cavity 34 penetrates the cladding layer 16 and is formed so as to expose a part of the range of one of the principal surfaces 2S of the semiconductor layer 14 in which the n-type semiconductor region 32 is formed. The second cavity 34 extends in the direction in which the optical waveguide 4 extends, i.e., the y direction, when viewed in a plan view. Both the first cavity 24 and the second cavity 34 are formed approximately vertically from the upper surface of the cladding layer 16 toward one main surface 2S of the semiconductor layer 14. Alternatively, both the first cavity 24 and the second cavity 34 may be formed in a tapered shape from the upper surface of the cladding layer 16 toward one main surface 2S of the semiconductor layer 14.

[0019] The first electrode 40 and the second electrode 50 are disposed apart in the x-axis direction with the optical waveguide 4 therebetween, and are electrically insulated. The first electrode 40 extends in the direction in which the optical waveguide 4 extends, i.e., along the y-axis direction, when viewed in a plan view. Similarly, the second electrode 50 extends in the direction in which the optical waveguide 4 extends, i.e., along the y-axis direction, when viewed in a plan view.

[0020] The first electrode 40 has a first transparent electrode 42 and a first wiring electrode 44. The first transparent electrode 42 is provided so as to completely fill the first cavity 24 of the cladding layer 16, and is in contact with the p-type semiconductor region 22. As will be described later in the manufacturing method, the upper surface of the first transparent electrode 42 is flush with the upper surface of the cladding layer 16 due to a planarization process. The first wiring electrode 44 is provided outside the first cavity 24 of the cladding layer 16, and is provided on the first transparent electrode 42. The first wiring electrode 44 is electrically connected to the p-type semiconductor region 22 via the first transparent electrode 42. In this way, the first wiring electrode 44 is located away from the protrusion 4A of the optical waveguide 4 in the stacking direction (z-axis direction).

[0021] The second electrode 50 has a second transparent electrode 52 and a second wiring electrode 54. The second transparent electrode 52 is provided so as to completely fill the second cavity 34 of the cladding layer 16, and is in contact with the n-type semiconductor region 32. As will be described later in the manufacturing method, the upper surface of the second transparent electrode 52 is flush with the upper surface of the cladding layer 16 due to the planarization process. The second wiring electrode 54 is provided outside the second cavity 34 of the cladding layer 16, and is provided on the second transparent electrode 52. The second wiring electrode 54 is electrically connected to the n-type semiconductor region 32 via the second transparent electrode 52. In this way, the second wiring electrode 54 is located away from the protrusion 4A of the optical waveguide 4 in the stacking direction (z-axis direction).

[0022] The first transparent electrode 42 of the first electrode 40 and the second transparent electrode 52 of the second electrode 50 are made of a material that is transparent to the light propagating through the optical waveguide 4. The material of the transparent electrodes 42, 52 may be a transparent conductive oxide (TCO). The transparent conductive oxide (TCO) is not particularly limited, and may be, for example, an indium oxide (InO)-based, tin oxide (SnO)-based, or zinc oxide (ZnO)-based material. The impurities doped into these oxide semiconductors may include at least one selected from the group consisting of indium (In), gallium (Ga), aluminum (Al), antimony (Sb), fluorine (F), tin (Sn), yttrium (Y), cadmium (Cd), arsenic (As), niobium (Nb), tantalum (Ta), germanium (Ge), molybdenum (Mo), titanium (Ti), zirconium (Zr), hafnium (Hf), tungsten (W), tellurium (Te), boron (B), scandium (Sc), vanadium (V), and silicon (Si).

[0023] The first wiring electrode 44 of the first electrode 40 is connected to a wiring for electrically connecting a control terminal (not shown) provided in the optical phased array 1 and the first transparent electrode 42. The material of the first wiring electrode 44 is not particularly limited, and may be, for example, aluminum (Al). The first wiring electrode 44 may be formed to extend from one end to the other end of the first transparent electrode 42 along the y-axis direction in a planar view. Alternatively, the first wiring electrode 44 may be formed to contact only a part of the first transparent electrode 42 in the y-axis direction in a planar view.

[0024] The second wiring electrode 54 of the second electrode 50 is connected to a wiring for electrically connecting a control terminal (not shown) provided in the optical phased array 1 and the second transparent electrode 52. The material of the second wiring electrode 54 is not particularly limited, and may be, for example, aluminum (Al). The second wiring electrode 54 may be formed to extend from one end to the other end of the second transparent electrode 52 along the y-axis direction in a planar view. The second wiring electrode 54 may be formed to contact only a part of the second transparent electrode 52 in the y-axis direction in a planar view.

[0025] (Operation of phase modulator) When a voltage that is more positive than the second electrode 50 is applied to the first electrode 40, a current flows from the first electrode 40 to the second electrode 50 via the p-type semiconductor region 22, the optical waveguide 4, and the n-type semiconductor region 32. This increases the carrier concentration in the optical waveguide 4, and changes the phase of the propagating light propagating through the optical waveguide 4. The phase modulator 8 adjusts the phase of the propagating light propagating through the optical waveguide 4, and outputs the phase-modulated propagating light to the transmitting antenna 9 (see FIG. 1).

[0026] The distribution of the propagating light propagating through the optical waveguide 4 is a range including the periphery of the optical waveguide 4. A part of the propagating light propagating through the optical waveguide 4 contacts the first transparent electrode 42 of the first electrode 40 and the second transparent electrode 52 of the second electrode 50. For example, if these contacting parts are opaque metal electrodes, a part of the propagating light is absorbed by the metal electrodes, and the optical loss increases. On the other hand, in the phase modulator 8, since these contacting parts are composed of the transparent electrodes 42 and 52, such optical loss is suppressed. Therefore, the phase modulator 8 can output the propagating light to the transmitting antenna 9 (see FIG. 1) while maintaining the intensity of the propagating light. As a result, when the optical phased array 1 (see FIG. 1) is mounted on a LiDAR device, the LiDAR device can measure long distances.

[0027] In addition, when the optical phased array 1 (see FIG. 1) is mounted on a LiDAR device, in order to widen the scan angle of the light beam emitted from the transmitting antenna 9, the pitch distance 10D between adjacent optical waveguides 4 must be reduced. For example, in order to emit a light beam with a wavelength of 1550 nm at a scan angle of 60°, the pitch distance 10D between adjacent optical waveguides 4 must be 1.55 μm or less. However, when the pitch distance 10D between the optical waveguides 4 is reduced, the above-mentioned problem of a part of the propagating light being absorbed by the metal electrode and increasing the light loss becomes apparent. The phase modulator 8 having the transparent electrodes 42 and 52 can suppress such an increase in light loss. As a result, the LiDAR device mounted with the optical phased array 1 including the phase modulator 8 can reduce the pitch distance 10D between adjacent optical waveguides 4 while suppressing the increase in light loss, and therefore the scan angle can be widened. Furthermore, since the pitch distance 10D of the optical waveguides 4 can be reduced, the optical phased array 1 can also be made smaller.

[0028] In the phase modulator 8, the upper surface of the first transparent electrode 42 and the upper surface of the clad layer 16 are configured to be in the same plane, so the first wiring electrode 44 is arranged by being laminated on the first transparent electrode 42. Similarly, the upper surface of the second transparent electrode 52 and the upper surface of the clad layer 16 are configured to be in the same plane, so the second wiring electrode 54 is arranged by being laminated on the second transparent electrode 52. With this configuration, it is not necessary to secure a large space for disposing the wiring electrodes 44, 54 outside the cavities 24, 34, so the pitch distance 10D of the optical waveguides 4 is reduced, and the optical phased array 1 can be made smaller.

[0029] (First manufacturing method of phase modulator) Hereinafter, a first manufacturing method of the phase modulator 8 will be described with reference to Fig. 3 to Fig. 9. First, as shown in Fig. 3, a substrate 2 on which an insulating layer 12 and a semiconductor layer 14 are laminated is prepared.

[0030] 4, a part of the semiconductor layer 14 is removed by etching to form a convex portion 4A of the optical waveguide 4. Next, p-type impurities and n-type impurities are introduced into a part of the semiconductor layer 14 by ion implantation, and the introduced impurities are activated to form a p-type semiconductor region 22 and an n-type semiconductor region 32.

[0031] 5, a transparent electrode film 70 is formed on the semiconductor layer 14 by using a sputtering technique. Since the sputtering technique has good step coverage, the transparent electrode film 70 is formed conformally. Instead of the sputtering technique, the transparent electrode film 70 may be formed by using a CVD (Chemical Vapor Deposition) technique or an ALD (Atomic Layer Deposition) technique.

[0032] Next, a heat treatment process is performed to adjust the extinction coefficient and electrical resistance of the transparent electrode film 70. This heat treatment process is composed of a combination of heating in an oxygen atmosphere and heating in a non-oxygen atmosphere. In this example, heating is performed first in an oxygen (O2) atmosphere, and then heating is performed in a nitrogen (N2) atmosphere. The heating in the oxygen (O2) atmosphere is performed under conditions of, but not limited to, 400°C and 20 minutes, for example. The heating in the nitrogen (N2) atmosphere is performed under conditions of, but not limited to, 500°C and 60 minutes.

[0033] The properties required for the transparent electrode film 70 are a low extinction coefficient and a low electrical resistance. In the transparent conductive oxide (TCO), which is the material of the transparent electrode film 70, its oxygen defects (oxygen vacancies and interstitial oxygen) act as carriers. The carriers in the transparent conductive oxide (TCO) have electrical conductivity and inhibit light transmission. When the transparent conductive oxide (TCO) is heated in an oxygen atmosphere, the oxygen defects are filled, and the electrical resistance increases and the extinction coefficient decreases due to the disappearance of carriers. On the other hand, when the transparent conductive oxide (TCO) is heated in a non-oxygen atmosphere, oxygen is removed and the electrical resistance decreases and the extinction coefficient increases due to the generation of carriers. The upper and lower limits of the extinction coefficient and the upper and lower limits of the electrical resistance depend on the conditions of heating in an oxygen atmosphere and heating in a non-oxygen atmosphere. In this way, the extinction coefficient and electrical resistance of the transparent conductive oxide (TCO) can be adjusted by combining heating in an oxygen atmosphere and heating in a non-oxygen atmosphere. In this example, the conditions of heating in an oxygen atmosphere and heating in a non-oxygen atmosphere are adjusted so that the electrical resistance value ensures the necessary electrical conductivity while suppressing an increase in the extinction coefficient due to oxygen defects. In addition to adjusting the extinction coefficient and electrical resistance value, this heat treatment can also eliminate other types of defects other than oxygen defects formed in the transparent electrode film 70 during film formation. The order of performing heating in an oxygen atmosphere and heating in a non-oxygen atmosphere is not particularly limited.

[0034] Next, as shown in Fig. 6, the transparent electrode film 70 is processed using photolithography and reactive ion etching techniques so that parts of the transparent electrode film 70 on the p-type semiconductor region 22 and the n-type semiconductor region 32 remain, forming the first transparent electrode 42 and the second transparent electrode 52. In this specification, the steps shown in Figs. 5 and 6 are referred to as a transparent electrode film forming step.

[0035] 7, a film formation technique is used to form the cladding layer 16 on the semiconductor layer 14 so as to cover the first transparent electrode 42 and the second transparent electrode 52. On the upper surface of the cladding layer 16, projections and recesses corresponding to the first transparent electrode 42, the second transparent electrode 52, and the projections 4A of the optical waveguide 4 are formed.

[0036] 8, the upper surface of the cladding layer 16 is planarized using a chemical mechanical polishing (CMP) technique until the first transparent electrode 42 and the second transparent electrode 52 are exposed. As a result, the upper surfaces of the transparent electrodes 42 and 52 and the upper surface of the cladding layer 16 become flush with each other.

[0037] 9, an aluminum electrode film 72 is formed on the first transparent electrode 42, the second transparent electrode 52, and the cladding layer 16 using a sputtering technique. Thereafter, the electrode film 72 is processed using a photolithography technique and a wet etching technique to form the first wiring electrode 44 and the second wiring electrode 54. Through these steps, the phase modulator 8 can be manufactured.

[0038] In the above manufacturing method, the heat treatment step is performed to adjust the extinction coefficient and electrical resistance value of the transparent electrode film 70 immediately after the transparent electrode film 70 is formed on the semiconductor layer 14. Instead of this example, the heat treatment step may be performed to adjust the extinction coefficient and electrical resistance value of the transparent electrode film 70 (i.e., the first transparent electrode 42 and the second transparent electrode 52) after the planarization step shown in FIG.

[0039] In the above manufacturing method, the transparent electrode film 70 is formed over the entire semiconductor layer 14, and then the transparent electrode film 70 is processed to form the first transparent electrode 42 and the second transparent electrode 52. Therefore, the transparent electrode film 70 is formed in one direction (i.e., the vertical direction). The transparent electrode film 70 thus formed has good film quality. As a result, the first transparent electrode 42 and the second transparent electrode 52 have good film quality.

[0040] (Second manufacturing method of phase modulator) 3 and 4 are performed. Next, as shown in Fig. 10, a cladding layer 16 is formed on the semiconductor layer 14 using a film formation technique. On the upper surface of the cladding layer 16, projections and recesses corresponding to the projections 4A of the optical waveguide 4 are formed.

[0041] Next, as shown in Fig. 11, a first cavity 24 and a second cavity 34 are formed in the cladding layer 16 using photolithography and reactive ion etching techniques. Both the first cavity 24 and the second cavity 34 are formed approximately vertically from the upper surface of the cladding layer 16 toward one main surface 2S of the semiconductor layer 14. In this specification, the process shown in Figs. 10 and 11 is referred to as a cladding layer formation process.

[0042] 12, a transparent electrode film 70 is formed in the cavities 24, 34 and on the cladding layer 16 using a sputtering technique. The transparent electrode film 70 is formed thick enough to completely fill the cavities 24, 34. Next, a heat treatment consisting of a combination of heating in an oxygen atmosphere and heating in a non-oxygen atmosphere is performed to adjust the extinction coefficient and electrical resistance of the transparent electrode film 70.

[0043] Next, the upper surface of the transparent electrode film 70 is planarized using CMP technology until the first transparent electrode 42 filled in the first cavity 24 of the cladding layer 16 and the second transparent electrode 52 filled in the second cavity 34 of the cladding layer 16 are exposed. This makes the upper surfaces of the transparent electrodes 42, 52 flush with the upper surface of the cladding layer 16. As a result, as described in the first manufacturing method, a structure identical to that shown in FIG. 8 is formed. The subsequent steps are identical to those in the first manufacturing method.

[0044] In the above manufacturing method, the heat treatment step is performed to adjust the extinction coefficient and electrical resistance value of the transparent electrode film 70 immediately after the transparent electrode film 70 is formed on the cladding layer 16. Instead of this example, the heat treatment step may be performed to adjust the extinction coefficient and electrical resistance value of the transparent electrode film 70 (i.e., the first transparent electrode 42 and the second transparent electrode 52) after the planarization step is performed.

[0045] The features of the technology disclosed in this specification are summarized below. Note that the technical elements described below are independent technical elements that exhibit technical usefulness alone or in various combinations, and are not limited to the combinations described in the claims at the time of filing.

[0046] (First feature) 1. A phase modulator comprising: a semiconductor layer including an optical waveguide; a cladding layer provided on the semiconductor layer, the cladding layer having a first cavity exposing a portion of an upper surface of the semiconductor layer and a second cavity exposing another portion of the upper surface of the semiconductor layer; a first electrode in contact with the top surface of the semiconductor layer via the first cavity; a second electrode in contact with the top surface of the semiconductor layer through the second cavity, the optical waveguide is disposed between a position where the first electrode contacts the upper surface of the semiconductor layer and a position where the second electrode contacts the upper surface of the semiconductor layer, and is configured such that a phase of propagating light changes when a voltage is applied between the first electrode and the second electrode; the first electrode includes a first transparent electrode filling the first cavity; the second electrode includes a second transparent electrode filling the second cavity; an upper surface of the first transparent electrode is flush with an upper surface of the cladding layer; A phase modulator, wherein an upper surface of the second transparent electrode is flush with an upper surface of the cladding layer.

[0047] (Second feature) The semiconductor layer is a first semiconductor region of a first conductivity type in contact with the first electrode; a second semiconductor region of a second conductivity type in contact with the second electrode, 2. The phase modulator of claim 1, wherein the optical waveguide is disposed between the first semiconductor region and the second semiconductor region.

[0048] (Third feature) the first electrode includes a first wiring electrode electrically connected to the first semiconductor region via the first transparent electrode; the first wiring electrode is provided outside the first cavity, the second electrode includes a second wiring electrode electrically connected to the second semiconductor region via the second transparent electrode, 3. The phase modulator according to claim 1, wherein the second wiring electrode is provided outside the second cavity.

[0049] (Fourth feature) 4. The phase modulator according to any one of Features 1 to 3, wherein the first transparent electrode and the second transparent electrode are made of a transparent conductive oxide (TCO).

[0050] (Fifth feature) A method for manufacturing a phase modulator, comprising the steps of: an optical waveguide forming step of forming an optical waveguide in the semiconductor layer; a transparent electrode film forming step of forming a transparent electrode film on the semiconductor layer, the transparent electrode film having a first transparent electrode and a second transparent electrode disposed apart from each other; a cladding layer forming step of forming a cladding layer on the semiconductor layer so as to cover the first transparent electrode and the second transparent electrode; and a planarizing step of planarizing the upper surface of the cladding layer until the upper surfaces of the first transparent electrode and the second transparent electrode are exposed.

[0051] (6th feature) The method further includes a heat treatment step of heat treating the transparent electrode film, The transparent electrode film is a transparent conductive oxide (TCO), 6. The method for manufacturing a phase modulator according to claim 5, wherein the heat treatment includes heating in an oxygen atmosphere and heating in a non-oxygen atmosphere.

[0052] (7th feature) The transparent electrode film forming step includes: forming the transparent electrode film on the semiconductor layer; removing a portion of the transparent electrode film to form the first transparent electrode and the second transparent electrode; 7. The method for producing a phase modulator according to claim 6, wherein the heat treatment is performed before removing a portion of the transparent electrode film.

[0053] (8th feature) 7. The method for manufacturing a phase modulator according to claim 6, wherein the heat treatment is performed after the planarization step.

[0054] (9th feature) A method for manufacturing a phase modulator, comprising the steps of: an optical waveguide forming step of forming an optical waveguide in the semiconductor layer; a cladding layer forming step of forming a cladding layer on the semiconductor layer, the cladding layer having a first cavity exposing a portion of an upper surface of the semiconductor layer and a second cavity exposing another portion of the upper surface of the semiconductor layer; a transparent electrode film forming step of forming a transparent electrode film on the cladding layer, the transparent electrode film having a first transparent electrode filling the first cavity and a second transparent electrode filling the second cavity; and a planarization process of planarizing the transparent electrode film until the first transparent electrode filled in the first cavity of the cladding layer and the second transparent electrode filled in the second cavity of the cladding layer are exposed.

[0055] (10th Feature) The method further includes a heat treatment step of heat treating the transparent electrode film, The transparent electrode film is a transparent conductive oxide (TCO), 10. The method for manufacturing a phase modulator according to claim 9, wherein the heat treatment includes heating in an oxygen atmosphere and heating in a non-oxygen atmosphere.

[0056] (11th Feature) 11. The method for manufacturing a phase modulator according to claim 10, wherein the heat treatment is performed before the planarization step or after the planarization step.

[0057] Although specific examples of the present invention have been described above in detail, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and variations of the specific examples exemplified above. Furthermore, the technical elements described in this specification or drawings exhibit technical utility alone or in various combinations, and are not limited to the combinations described in the claims at the time of filing. Furthermore, the technology exemplified in this specification or drawings can achieve multiple objectives simultaneously, and achieving one of these objectives is itself technically useful. [Explanation of symbols]

[0058] 2: substrate, 4: optical waveguide, 4A: convex portion, 8: phase modulator, 10: unit, 10D: pitch distance, 12: insulating layer, 14: semiconductor layer, 16: cladding layer, 22: p-type semiconductor region, 24: first cavity, 32: n-type semiconductor region, 34: second cavity, 40: first electrode, 42: first transparent electrode, 44: first wiring electrode, 50: second electrode, 52: second transparent electrode, 54: second wiring electrode,

Claims

1. 1. A phase modulator comprising: a semiconductor layer including an optical waveguide; a cladding layer provided on the semiconductor layer, the cladding layer having a first cavity exposing a portion of an upper surface of the semiconductor layer and a second cavity exposing another portion of the upper surface of the semiconductor layer; a first electrode in contact with the top surface of the semiconductor layer through the first cavity; a second electrode in contact with the top surface of the semiconductor layer through the second cavity, the optical waveguide is disposed between a position where the first electrode contacts the upper surface of the semiconductor layer and a position where the second electrode contacts the upper surface of the semiconductor layer, and is configured such that a phase of propagating light changes when a voltage is applied between the first electrode and the second electrode; the first electrode includes a first transparent electrode filling the first cavity; the second electrode includes a second transparent electrode filling the second cavity; an upper surface of the first transparent electrode is flush with an upper surface of the cladding layer; A phase modulator, wherein an upper surface of the second transparent electrode is flush with an upper surface of the cladding layer.

2. The semiconductor layer is a first semiconductor region of a first conductivity type in contact with the first electrode; a second semiconductor region of a second conductivity type in contact with the second electrode, The phase modulator according to claim 1 , wherein the optical waveguide is disposed between the first semiconductor region and the second semiconductor region.

3. the first electrode includes a first wiring electrode electrically connected to the first semiconductor region via the first transparent electrode; the first wiring electrode is provided outside the first cavity, the second electrode includes a second wiring electrode electrically connected to the second semiconductor region via the second transparent electrode, The phase modulator according to claim 2 , wherein the second wiring electrode is provided outside the second cavity.

4. 4. The phase modulator according to claim 1, wherein the first transparent electrode and the second transparent electrode are transparent conductive oxides (TCOs).

5. A method for manufacturing a phase modulator, comprising the steps of: an optical waveguide forming step of forming an optical waveguide in the semiconductor layer; a transparent electrode film forming step of forming a transparent electrode film on the semiconductor layer, the transparent electrode film having a first transparent electrode and a second transparent electrode disposed apart from each other; a cladding layer forming step of forming a cladding layer on the semiconductor layer so as to cover the first transparent electrode and the second transparent electrode; and a planarizing step of planarizing the cladding layer until an upper surface of the first transparent electrode and an upper surface of the second transparent electrode are exposed.

6. The method further includes a heat treatment step of heat treating the transparent electrode film, the transparent electrode film is a transparent conductive oxide (TCO); The method for manufacturing a phase modulator according to claim 5 , wherein the heat treatment includes heating in an oxygen atmosphere and heating in a non-oxygen atmosphere.

7. The transparent electrode film forming step includes: forming the transparent electrode film on the semiconductor layer; removing a portion of the transparent electrode film to form the first transparent electrode and the second transparent electrode; The method for manufacturing a phase modulator according to claim 6 , wherein the heat treatment is performed before removing a portion of the transparent electrode film.

8. The method for manufacturing a phase modulator according to claim 6 , wherein the heat treatment is performed after the planarization step.

9. A method for manufacturing a phase modulator, comprising the steps of: an optical waveguide forming step of forming an optical waveguide in the semiconductor layer; a cladding layer forming step of forming a cladding layer on the semiconductor layer, the cladding layer having a first cavity exposing a portion of an upper surface of the semiconductor layer and a second cavity exposing another portion of the upper surface of the semiconductor layer; a transparent electrode film forming step of forming a transparent electrode film, the transparent electrode film having a first transparent electrode filling the first cavity and a second transparent electrode filling the second cavity; and a planarization process of planarizing the transparent electrode film until the first transparent electrode filled in the first cavity of the clad layer and the second transparent electrode filled in the second cavity of the clad layer are exposed.

10. The method further includes a heat treatment step of heat treating the transparent electrode film, the transparent electrode film is a transparent conductive oxide (TCO); The method for manufacturing a phase modulator according to claim 9 , wherein the heat treatment includes heating in an oxygen atmosphere and heating in a non-oxygen atmosphere.

11. The method for manufacturing a phase modulator according to claim 10 , wherein the heat treatment is performed before the planarizing step or after the planarizing step.

Citation Information

Patent Citations

  • Optical scanning device

    JP2020166061A

  • Optical antenna

    JP2021103147A

  • Optical Phase Shifter Device

    US20210026216A1