Junction structure of vacuum valve and vacuum valve

A multi-stage brazing process with distinct liquidus temperature layers in vacuum valves addresses the challenge of maintaining electrical conductivity and cost-effectiveness by using non-noble metals, ensuring durability and efficiency.

JP2024134360APending Publication Date: 2024-10-03KK TOSHIBA +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023044619
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing vacuum valve manufacturing processes face challenges in achieving low-cost bonding while maintaining electrical conductivity, as high melting point brazing filler metals without noble metals often have poor electrical conductivity, leading to issues in environments where electricity is applied.

Method used

A multi-stage brazing process using a first bonding layer with a first liquidus temperature and a second bonding layer with a higher liquidus temperature, composed of different brazing filler metals, to prevent melt-through and resistance increase, without using expensive noble metals like palladium.

Benefits of technology

This approach maintains electrical conductivity at a lower cost by preventing melt-through and resistance increase in vacuum valves, even under high temperatures, without relying on costly noble metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134360000001_ABST
    Figure 2024134360000001_ABST
Patent Text Reader

Abstract

To provide a junction structure of a vacuum valve using a junction layer at a low cost.SOLUTION: According to an embodiment, a junction structure of a vacuum valve includes: a first base material in which a first junction region is provided; a second base material in which a second junction region arranged so as to be faced to the first junction region is arranged; and a junction layer that bonds the first junction region and the second junction region. The first base material is a contact point, and the second base material is a current-carrying shaft. The junction layer includes: a first junction part that has a first liquid phase line temperature, and bonds a first part of the first junction region and a second part of the second junction region; and a second junction part that has a second liquid phase line temperature that is higher than the first liquid phase line temperature, and bonds a third part that is different from the first part of the first junction region and a fourth part that is different from the second part of the second junction region.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] An embodiment of the present invention relates to a joining structure of a vacuum interrupter and a vacuum interrupter. [Background technology]

[0002] A brazing process is used to join metals together in the manufacture of vacuum vessels. In some vacuum vessels, a multi-stage brazing process is used to realize complex internal structures. The multi-stage brazing process is characterized by the use of two brazing materials with different melting points. First, a brazing material with a higher melting point is used to join components inside the vacuum vessel, such as the contacts and the current-carrying shaft, and in a later process, a brazing material with a lower melting point is used to seal, for example, the ceramic vessel and the sealing metal fittings. In addition, in vacuum equipment that involves electrical current, the brazing material generally uses precious metal brazing materials with low electrical resistance, and in particular, brazing materials containing palladium are often used as high-melting point brazing materials. On the other hand, there is a demand to reduce the amount of these precious metals used in order to reduce costs. High-melting point brazing materials that do not contain precious metals generally have poor electrical conductivity, and electrical loss can be an issue in environments where electricity is constantly being passed. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 5668123 [Patent Document 2] Patent No. 5350317 [Patent Document 3] Patent No. 6187189 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a bonding structure for a vacuum interrupter using a low-cost bonding layer. [Means for solving the problem]

[0005] According to an embodiment, a first base material having a first bonding region provided thereon; a second base material provided with a second bonding region disposed opposite the first bonding region; a first bonding layer that bonds the first bonding region and the second bonding region; The first base material is a contact point, and the second base material is a current-carrying shaft, A joining structure for a vacuum valve is provided, characterized in that the first joining layer includes a first joining portion having a first liquidus temperature and joining a first portion of the first joining region and a second portion of the second joining region, and a second joining portion having a second liquidus temperature higher than the first liquidus temperature and joining a third portion different from the first portion of the first joining region and a fourth portion different from the second portion of the second joining region. [Brief description of the drawings]

[0006] [Figure 1] 1 is a schematic cross-sectional view showing an example of a joining structure of a vacuum interrupter according to an embodiment of the present invention. [Diagram 2] 1 is a vertical cross-sectional view showing the configuration of a vacuum interrupter according to an embodiment of the present invention. [Diagram 3] 4 is a schematic cross-sectional view showing another example of a joining structure of a vacuum interrupter according to an embodiment of the present invention. FIG. [Figure 4] 1 is a schematic cross-sectional view showing a joining structure of a vacuum interrupter according to a first embodiment. [Diagram 5] 6 is a schematic cross-sectional view showing a joining structure of a vacuum interrupter according to a second embodiment. FIG. [Figure 6] 11 is a schematic cross-sectional view showing a joining structure of a vacuum interrupter according to Example 3. FIG. [Figure 7] 7 is an electron microscope photograph of a portion of FIG. 6. [Figure 8] 7 is an electron microscope photograph of another part of FIG. 6. [Figure 9] This is a Cu-Ag equilibrium phase diagram. [Figure 10] 11 is a schematic cross-sectional view showing a joining structure of a vacuum interrupter according to Example 4. FIG. [Figure 11]11 is a schematic enlarged cross-sectional view of a portion of FIG. 10. FIG. [Figure 12] This is a Cu-Bi equilibrium phase diagram. [Figure 13] This is a Cu-Zn equilibrium phase diagram. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The joining structure of the vacuum interrupter according to the first embodiment includes a first base material having a first joining region, a second base material having a second joining region arranged opposite to the first joining region, and a first joining layer joining the first joining region and the second joining region. The first base material can be a contact, and the second base material can be a current-carrying shaft. The first bonding layer includes a first bonding portion having a first liquidus temperature and a second bonding portion having a second liquidus temperature higher than the first liquidus temperature. The first bonding portion bonds a first portion of the first bonding region and a second portion of the second bonding region. The second bonding portion bonds a third portion of the first bonding region different from the first portion and a fourth portion of the second bonding region different from the second portion.

[0008] A vacuum interrupter according to a second embodiment is a vacuum interrupter using the above-mentioned joining structure, The vacuum vessel includes an insulating vessel having open ends at both ends, a vacuum vessel having a pair of sealing fittings joined to the open ends by a second bonding layer, and a pair of electrodes detachably provided on the vacuum vessel, at least one of the electrodes including the bonding structure of the vacuum valve according to the first embodiment described above. The first bonding layer is provided by a first stage of bonding (brazing) in the process of producing the vacuum interrupter bonding structure according to the first embodiment. The second bonding layer is provided by a second stage of bonding (brazing) in the process of encapsulating the vacuum interrupter bonding structure including the first bonding layer and sealing the open end of the insulating container with a sealing metal fitting. In this way, the first bonding layer is subjected to at least two stages of bonding (multi-stage brazing) and exposed to high temperatures when producing the vacuum interrupter. A brazing material can be used for the first and second bonding parts of the first bonding layer. The first bonding part, which has a low liquidus temperature, tends to have high electrical conductivity but melts easily at high temperatures. On the other hand, the second bonding part, which has a high liquidus temperature, tends to melt less easily at high temperatures but has high electrical resistance. .

[0009] According to the first and second embodiments, a first bonding layer including a first bonding portion having a first liquidus temperature and a second bonding portion having a second liquidus temperature higher than the first liquidus temperature is used to bond a first portion of the first bonding region to a second portion of the second bonding region, and a second bonding portion is used to bond a third portion different from the first portion of the first bonding region to a fourth portion different from the second portion of the second bonding region. This makes it possible to prevent the second bonding portion from melting through the first bonding layer at high temperatures, such as the temperature of the second stage bonding, and to prevent an increase in the resistance value of the first bonding layer at the first bonding portion.

[0010] Thus, according to the embodiment, by using a combination of a first bonding part having a first liquidus temperature in the first bonding layer and a second bonding part having a second liquidus temperature higher than the first liquidus temperature, it is possible to maintain electrical conductivity at low cost in the bonding structure of a vacuum valve without using a brazing material containing an expensive precious metal such as palladium in the first bonding layer.

[0011] Hereinafter, embodiments will be described with reference to the drawings. The disclosure is merely an example, and appropriate modifications that are within the spirit of the invention and that can be easily conceived by a person skilled in the art are naturally included in the scope of the present invention. In addition, in order to make the explanation clearer, the width, thickness, shape, etc. of each part may be shown diagrammatically compared to the actual embodiment, but these are merely examples and do not limit the interpretation of the present invention. In this specification and each figure, elements similar to those described above with respect to the previous figures may be given the same reference numerals, and detailed explanations may be omitted as appropriate.

[0012] FIG. 1 is a schematic cross-sectional view showing an example of a joining structure of a vacuum interrupter according to a first embodiment. Reference numeral 21 denotes an example of a part used in the vacuum valve according to the first embodiment, and denotes one of the electrodes for the vacuum valve, for example, a fixed electrode. The fixed electrode 21 includes a contact 6 as a first base material having a first joint region 6a on its end face, a current-carrying shaft 4 as a second base material having a second joint region 4a disposed opposite the first joint region 6a, and a joint structure 121 including a first joint layer 5 that joins the first joint region 6a of the contact 6 to the second joint region 4a of the current-carrying shaft 4.

[0013] The first bonding layer 5 includes a first bonding portion 5-1 having a first liquidus temperature and a second bonding portion 5-2 having a second liquidus temperature higher than the first liquidus temperature. Here, as an example, the first bonding portion 5-1 is provided near the center of the first bonding layer 5, and the second bonding portion 5-2 is provided around the first bonding portion 5-1. The first bonding portion 5-1 bonds a first portion 6a-1 near the center of the first bonding region 6a and a second portion 4a-1 near the center of the second bonding region 4a. The second bonding portion 5-2 bonds a third portion 6a-2 provided around the first portion 6a-1 of the first bonding region 6a and a fourth portion 4a-2 provided around the second portion 4a-1 of the second bonding region. The first bonding layer 5 can be made of a metal. The first bonding portion 5-1 and the second bonding portion 5-2 can be made of metals having different compositions. As the metal, various brazing materials can be used. Examples of the brazing material include a CuAg alloy, a BiCu alloy, and a CuZn alloy.

[0014] FIG. 2 is a vertical cross-sectional view showing the configuration of a vacuum interrupter according to the second embodiment. As shown in the figure, the vacuum valve 100 includes a cylindrical ceramic container 1 having openings at both ends and made of, for example, alumina porcelain, a fixed sealing metal fitting 2 bonded and sealed to one opening by a second bonding layer 15, a movable sealing metal fitting 3 bonded and sealed to the other opening by a second bonding layer 15', and a pair of electrodes, a fixed electrode 21 and a movable electrode 22. A vacuum is maintained inside the vacuum valve 100. The fixed sealing metal fitting 2 has a central opening, through which a fixed current-carrying shaft 4, which serves as one of the electric paths, is fixed. A fixed contact 6 is fixed to the end of the fixed current-carrying shaft 4 inside the ceramic container 1 via a first bonding layer 5, thereby obtaining a bonding structure for the fixed electrode 21 as one of the pair of electrodes of the vacuum valve 100. As the bonding structure for the fixed electrode 21, a bonding structure 121 for a vacuum valve according to the first embodiment shown in FIG. 1 can be applied.

[0015] In addition, the movable contact 7, which faces the fixed contact 6 and forms a pair of separable contacts, is fixed to the end face of the movable current-carrying shaft 9 via a first bonding layer 8, thereby forming a bonding structure of the movable electrode 22. The movable current-carrying shaft 9 serves as another electric path that movably passes through a central opening provided in the movable sealing metal fitting 3.

[0016] The part of the movable current-carrying shaft 9 on the movable sealing metal fitting 3 side from the center part is the part that is led out of the ceramic container 1, and a bellows cover 10 for airtight sealing is provided at that part, and one end of a cylindrical bellows 11 that can expand and contract is disposed on the bellows cover 10. The other end of the bellows 11 is sealed to the central opening of the movable sealing metal fitting 3. This allows the movable current-carrying shaft 9 to move in the axial direction while maintaining the vacuum of the insulating container 1. A cylindrical arc shield 12 is provided around the fixed contact 6 and the movable contact 7 to prevent metal vapor and molten metal generated during opening and closing from adhering to the inner wall of the insulating container 1 and reducing the insulation resistance. As the joint structure of the movable side electrode 22, the joint structure 122 of the vacuum interrupter according to the first embodiment can be applied.

[0017] FIG. 3 is a schematic cross-sectional view showing an example of a joining structure of the movable electrode. Reference numeral 22 denotes a movable electrode which is the other of the vacuum valve electrodes used in the vacuum valve 100 shown in Fig. 2. The movable electrode 22 is provided with a joint structure 122 including a contact 7 as a first base material having a first joint region 7a provided on an end face thereof, a current-carrying shaft 9 as a second base material having a second joint region 9a disposed opposite to the first joint region 7a, and a first joint layer 8 which joins the first joint region 7a of the contact 7 and the second joint region 9a of the current-carrying shaft 4.

[0018] The above-mentioned joint structure 122 has the same structure as that shown in FIG. 1, except that a first joint 8-1 is provided instead of the first joint 5-1, a second joint 8-2 is provided instead of the second joint 5-2, a first portion 7a-1 is provided instead of the first portion 6a-1, a second portion 9a-1 is provided instead of the second portion 4a-1, a third portion 7a-2 is provided instead of the third portion 6a-2, and a fourth portion 9a-2 is provided instead of the fourth portion 4a-2. Here, in the vacuum valve of the second embodiment, the joint structure of the vacuum valve of the first embodiment is applied to both the joint structure of the fixed side electrode 21 and the joint structure of the movable side electrode 22, but it is sufficient to apply it to at least one of them.

[0019] In the joint structure of the vacuum interrupter according to the first embodiment, the ratio of the first joint portions 5-1, 8-1 to the second joint portions 5-2, 8-2 can be set to, for example, 1:2 to 1:10 in terms of area ratio. The diameter of the end 4b or end 9b of the current-carrying shaft 4, 9 can be, for example, 10 mm to 150 mm, and the thickness in the axial direction can be, for example, 1 mm to 30 mm. The diameter of the contacts can be, for example, 15 mm to 150 mm, and the thickness can be, for example, 3 mm to 10 mm. The first bonding layer may have a diameter of, for example, 10 mm to 150 mm and a thickness of, for example, 0.1 mm to 1 mm. The joint structure of the vacuum interrupter according to the first embodiment may further include a structure for shielding at least a portion between the first joint portion and the second joint portion. The shielding structure refers to a structure that prevents the diffusion of elements from the first bonding part to the second bonding part, or the diffusion of elements from the second bonding part to the first bonding part. As the shielding structure, for example, a slit provided in at least one of the first and second bonding regions can be used. Also, for example, a ring-shaped shielding material having a composition different from the composition of the first bonding parts 5-1, 8-1 and the second bonding parts 5-2, 8-2 can be applied to the slit. As the shielding material, it is possible to use a material in which the alloy used in the first bonding layer is unlikely to diffuse into the shielding material, or in which the alloy used in the first bonding layer is unlikely to chemically react with the shielding material, for example, alumina, graphite, calcia, zirconia, magnesia, silica, etc. can be used.

[0020] The slit may have, for example, a ring shape or a lattice shape. For example, in the case of a ring shape, the depth can be 1 mm to 5 mm, and the width can be 1 mm to 30 mm. Furthermore, for example, in the case of a lattice shape, the depth can be 1 mm to 5 mm, and the width can be 1 mm to 5 mm. If the slit depth is less than 1.5 mm, the components constituting the joint tend to flow from the joint to the slit, and if the slit width is less than 3 mm, the components of one joint tend to mix with the components of the other joint.

[0021] The first bonding layer may further include a third bonding portion between the first bonding portion and the second bonding portion, the third bonding portion having a composition different from the compositions of the first bonding portion and the second bonding portion. In this case, the first bonding layer may further include a third bonding portion having a third liquidus temperature different from the first liquidus temperature and the second liquidus temperature, and bonding a fifth portion different from the first portion and the third portion of the first bonding region and a sixth portion different from the second portion and the fourth portion of the second bonding region. The third junction may have a gradient composition that changes continuously from the composition of the first junction to the composition of the second junction. Here, when the first bonding layer 5, 8 has a first solidus temperature and the second bonding layer has a first liquidus temperature, the first liquidus temperature of the second bonding layer can be set to be equal to or lower than the first solidus temperature. If the first liquidus temperature of the second bonding layer exceeds the first solidus temperature of the first bonding layer, a part of the first bonding layer bonded in the first stage tends to melt during the second stage bonding. Here, the first solidus temperature of the first bonding layer refers to the lowest solidus temperature when the first bonding layer has multiple solidus temperatures, and the first liquidus temperature of the second bonding layer refers to the highest liquidus temperature when the second bonding layer has multiple liquidus temperatures.

[0022] The methods for manufacturing the joining structure of the vacuum interrupter used in the first and second embodiments can be divided into the following two methods. First, in the first forming method, two or more brazing filler metals having different liquidus temperatures, for example, a first brazing filler metal having a first liquidus temperature and a second brazing filler metal having a second liquidus temperature higher than the first liquidus temperature, are applied to the joint region of the current-carrying shaft, the joint region of the contacts is placed thereon, and brazing is performed at an atmospheric pressure equal to or lower than normal pressure and at a temperature equal to or higher than the liquidus temperature, thereby obtaining a first joint structure consisting of the current-carrying shaft, the contacts, and a first joint layer provided between the current-carrying shaft and the contacts. In the first joint layer of the first joint structure, for example, a first joint portion corresponding to the first brazing filler metal and a second joint portion corresponding to the second brazing filler metal can be created in accordance with the applied brazing filler metals.

[0023] In the second forming method, one or more brazing materials, for example, a first brazing material having a first liquidus temperature, is applied to the joint area of ​​the current-carrying shaft, and the joint area of ​​the contact is placed thereon. Brazing is performed in a vacuum atmosphere at a temperature between the first liquidus temperature and a temperature at which the current-carrying shaft and the contact do not melt, thereby obtaining a second joint structure consisting of the current-carrying shaft, the contact, and a first joint layer provided between the current-carrying shaft and the contact. In the first joint layer of the second joint structure, brazing is performed in a vacuum atmosphere, so that the side surface becomes a second joint portion having a composition rich in another part of the metal components, as a result of a part of the metal components contained in the first brazing material evaporating, changing the metal composition ratio. The center portion becomes a first joint portion having a composition similar to the metal composition of the first brazing material. Between the side surface and the center portion, a third joint portion can be formed having a gradient composition that changes continuously from the composition of the second joint portion to the composition of the first joint portion.

[0024] In the second forming method, the brazing temperature in a vacuum atmosphere can be set to a temperature equal to or higher than the liquidus temperature of the brazing material and equal to or lower than a temperature at which the current-carrying shaft and the contacts do not melt. -5 Pa~10 -3 It can be made Pa. In the first forming method, the brazing temperature can be set to a temperature equal to or higher than the liquidus temperature of the brazing material and equal to or lower than a temperature at which the current-carrying shaft and the contacts do not melt. -5 It can be adjusted to Pa~101300 (atmospheric pressure) Pa.

[0025] The following examples are provided to more specifically explain the embodiments. Working Example Example 1 FIG. 4 is a schematic cross-sectional view showing a joint structure of the vacuum interrupter according to the first embodiment. As shown in Fig. 4, a current-carrying shaft 34 made of oxygen-free copper having a joint surface 34a with a diameter of 50 mm and a contact 36 made of a Cu alloy (Cu 75% by weight-Cr 25% by weight) with a joint surface 36a with a diameter of 50 mm were prepared. As a pair of slits 31, a concentric slit 31-1 was provided on the joint surface 36a, and a concentric slit 31-2 was provided on the joint surface 34a opposite to the slit 31-1. A cylindrical Al2O3 (alumina) material 33 was placed in the slit 31-2 of the oxygen-free copper joint surface 34a. A eutectic Ag brazing foil 35-2 (0.1 mm) made of a CuAg alloy (Cu 28% by weight-Ag 72% by weight) was placed on the oxygen-free copper joint surface 34a inside the alumina material 33 as the brazing material 1, and a Ni-P brazing foil 35-1 (0.1 mm) made of a Ni-P alloy was placed on the smooth surface outside the alumina material 33 as the brazing material 2. The solidus temperature and liquidus temperature of the eutectic Ag brazing foil 35-2 are both 780°C, and the solidus temperature and liquidus temperature of the Ni-P brazing foil 35-1 are both 875°C. The alumina material 33 on the oxygen-free copper side was placed in the slit 31-1 provided on the joint surface 36a of the Cu alloy so as to fit therein, and brazing was performed in a vacuum atmosphere at a temperature of 900°C for a holding time of 10 minutes to obtain an electrode 23 having a joint structure 123 including a current-carrying shaft 34, a contact 36, and a first joint layer 35 provided between the current-carrying shaft 34 and the contact 36. When the resistance between the contact 36 and the current-carrying shaft 34 was measured after the brazing was completed, the obtained resistance was about 1.7 times the resistance value of a joint structure in which the same joint surface as the joint surface of the contact 36 and the current-carrying shaft 34 was brazed entirely with eutectic Ag brazing, which was taken as the reference resistance value. In addition, when the joint structure of Example 1 was heated at 800°C for 10 minutes, the Cu alloy did not fall off from the oxygen-free copper. Note that such a heat treatment at 800°C for 10 minutes is similar to the treatment used for the second stage joining using, for example, eutectic Ag brazing foil. The results obtained are shown in Table 1 below.

[0026] Example 2 FIG. 5 is a schematic cross-sectional view showing a joint structure of a vacuum interrupter according to a second embodiment. A current-carrying shaft 44 made of oxygen-free copper having a joint surface 44a with a diameter of 50 mm and a contact 46 made of a Cu alloy (Cu 75% by weight-Cr 25% by weight) having a joint surface 46a with a diameter of 50 mm were prepared. As shown in FIG. 5, a pair of slits 41 were provided, a concentric slit 41-1 on the joint surface 46a, and a concentric slit 41-2 on the joint surface 44a facing the slit 41-1. A eutectic Ag brazing foil 45-2 (0.1 mm) similar to that in Example 1 was placed as the brazing material 1 on the inner side of the slit 41 on the oxygen-free copper joint surface 44a, and a Ni-P brazing foil 45-1 (0.1 mm) was placed as the brazing material 2 on the outer side of the slit 41 on the joint surface 44a. The solidus temperature and liquidus temperature of the eutectic silver brazing foil 45-2 were both 780°C, and the solidus temperature and liquidus temperature of the Ni-P brazing foil 45-1 were both 875°C. The joining surfaces 46a, 44a were placed facing each other so that the slit 41-1 provided in the Cu alloy 46 and the slit 41-2 on the oxygen-free copper 44 side were aligned, and brazing was performed in a vacuum atmosphere at a temperature of 900°C for a holding time of 10 minutes to obtain an electrode 24 having a joining structure 124 including a current-carrying shaft 44, a contact 46, and a first joining layer 45 provided between the current-carrying shaft 44 and the contact 46. When the resistance between the contact 46 and the current-carrying shaft 44 was measured after the brazing was completed, it was about 1.7 times the reference value of the resistance in Example 1. In addition, when the joining structure in Example 2 was heated at 800°C for 10 minutes, the Cu alloy did not fall off from the oxygen-free copper. The results obtained are shown in Table 1 below.

[0027] Example 3 FIG. 6 is a schematic cross-sectional view showing a joint structure of a vacuum interrupter according to a third embodiment. A current-carrying shaft 54 ​​made of oxygen-free copper having a joint surface 54a of 50 mm in diameter, and a contact 56 made of a Cu alloy (Cu 75% by weight-Cr 25% by weight) having a joint surface 56a of 50 mm in diameter were prepared. As shown in FIG. 6, a eutectic Ag brazing foil similar to that in Example 1 was placed as a brazing material on the joint surface 54a, and a joint surface 56a made of a Cu alloy 56 (Cu 75% by weight-Cr 25% by weight) was placed thereon, and the brazing process was performed by heating at a temperature of 1050° C. for 30 minutes in a vacuum atmosphere to obtain an electrode 26 having a joint structure 126 including the current-carrying shaft 54, the contact 56, and a first joint layer 55 provided between the current-carrying shaft 54 ​​and the contact 56. The cross section of the brazed portion was observed with an electron microscope.

[0028] FIG. 7 shows an electron microscope photograph of a part of the cross section of the brazed portion of FIG. FIG. 8 shows an electron microscope photograph of another part of the cross section of the brazed portion of FIG. As shown in Fig. 7, by performing brazing in a vacuum atmosphere, part of the Ag contained in the eutectic Ag braze evaporated, and the sides became a region 55-1 (joining material 3) with a Cu-rich composition, and as shown in Fig. 8, near the center was a region 55-2 (joining material 1) with a composition close to the eutectic Ag braze, and between them was a region 55-3 (joining material 2) with an intermediate composition whose composition changed continuously from that of joining material 1 to that of joining material 3. As a result of elemental analysis, the average composition of joining material 2 was Ag 5 wt%-Cu 95 wt%, the average composition of joining material 3 was Ag 20 wt%-Cu 80 wt%, and joining material 1 was a eutectic composition (Ag 28 wt%-Cu 72 wt%).

[0029] FIG. 9 shows the equilibrium phase diagram of the Cu-Ag system. In the figure, 131 indicates the liquidus line. From the phase diagram, it was confirmed that the solidus temperatures of the bonding materials 1 and 3 were 780°C, and that of the bonding material 2 was about 900°C, and that the liquidus temperatures of the bonding materials 1, 3, and 2 were 780°C, 960°C, and 1050°C, respectively. This bonded structure was heated at 800°C for 10 minutes, but the Cu alloy did not fall off from the oxygen-free copper. The resistance between the current-carrying shaft 54 ​​and the contact 56 was measured and found to be equivalent to the reference value of Example 1. The results obtained are shown in Table 1 below.

[0030] Example 4 FIG. 10 is a schematic cross-sectional view showing a joint structure of a vacuum interrupter according to a fourth embodiment. A current-carrying shaft 64 made of oxygen-free copper and having a joint surface 64a with a diameter of 50 mm, and a contact 66 made of a Cu alloy (Cu 75% by weight-Cr 25% by weight) and having a joint surface 66a with a diameter of 50 mm were prepared. As shown in Fig. 10, a lattice-shaped slit 61-2 was provided on the joining surface 64a, and a lattice-shaped slit 61-1 was provided on the joining surface 66a opposite the slit 61-2, as a pair of slits 61. As shown in Fig. 10, lattice-shaped slits were provided on the oxygen-free copper joining surface and the Cu alloy (Cu 75 wt%-Cr 25 wt%) joining surface, both of which had a diameter of 50 mm.

[0031] The same eutectic Ag brazing foil as in Example 1 was placed in the region 62-2 of the joining surface 64a other than the slit 61-2, and the region 62-1 of the joining surface 66a of the Cu alloy other than the slit 61-1 was placed on the region 62-2 in a positioning manner. Brazing was performed by heating at 1050°C for 30 minutes in a vacuum atmosphere, and an electrode 27 having a joining structure 127 was obtained. The cross section of the brazed portion was observed with an electron microscope.

[0032] FIG. 11 is an enlarged schematic cross-sectional view of a portion of FIG. In the eutectic Ag brazing foil 25 between region 62-2 which is the part other than slit 61-2 and region 62-1 which is the part other than slit 61-1, some of the Ag contained in the eutectic Ag brazing foil evaporated, and the sides became Cu-rich region 25-1 (joining material 2), region 25-3 near the center had a composition close to the eutectic Ag brazing foil (joining material 1), and region 25-2 in between had an intermediate composition (joining material 3) in which the composition changed continuously from the composition of joining material 1 to the composition of joining material 2. As a result of elemental analysis, the average composition of bonding material 2 was 5 wt % Ag-95 wt % Cu, the average composition of bonding material 3 was 20 wt % Ag-80 wt % Cu, and the average composition of bonding material 1 was a eutectic composition.

[0033] In addition, from the phase diagram in Figure 9, it was confirmed that the solidus temperatures were approximately 780°C for joining material 2 and joining material 3 and 900°C for joining material 1, and the liquidus temperatures were approximately 780°C for joining material 1, 960°C for joining material 3 and 1050°C for joining material 2. This joined body was heated at 800°C for 10 minutes, but the Cu alloy did not fall off from the oxygen-free copper. The resistance between the contact 66 and the current-carrying shaft 64 was measured and found to be equal to the reference resistance value of Example 1. The results obtained are shown in Table 1 below.

[0034] Example 5 A current-carrying shaft made of oxygen-free copper and having a joint surface of 50 mm in diameter, and a contact point made of a Cu alloy (Cu 75% by weight-Cr 25% by weight) and having a joint surface of 50 mm in diameter, were prepared. A brazing foil of Cu50wt%-Bi50wt% was placed on the oxygen-free copper joint surface as a brazing material, and the Cu alloy of the contact was placed on top of it, and brazing was performed by heating at 900℃ for 30 minutes in a vacuum atmosphere to obtain a joint structure. When the cross section of the brazed part was observed with an electron microscope, it was found that, as in the joint structure shown in Figure 6, part of the Bi contained in the Cu50wt%-Bi50wt% alloy had evaporated, and the side had become a Cu-rich region (joining material 2), the center area had a composition close to the initial composition (joining material 1), and between them was an intermediate composition region (joining material 3) whose composition changed continuously from that of joining material 1 to that of joining material 3. Elemental analysis showed that joining material 2 was almost a single phase of Cu, joining material 3 had an average composition of Cu80wt%-Bi20wt%, and joining material 1 had the initial composition of Cu50wt%-Bi50wt%.

[0035] FIG. 12 shows an example of a Cu-Bi system equilibrium phase diagram. In the figure, 132 indicates the liquidus line. From the phase diagram, it was confirmed that the solidus temperatures were 300°C for joining material 1 and joining material 3, and approximately 1080°C for joining material 2, and the liquidus temperatures were 900°C for joining material 1, 1000°C for joining material 3, and approximately 1080°C for joining material 2. In addition, when the resistance between the contact and the current-carrying shaft was measured, it was approximately the same as when a similar contact and current-carrying shaft were fully brazed with eutectic silver solder. This joint structure was heated at 800°C for 10 minutes, but the Cu alloy did not fall off from the oxygen-free copper. The results obtained are shown in Table 1 below.

[0036] Example 6 A brazing process was carried out in the same manner as in Example 5, except that a brazing foil of Cu50%-Zn50% was used instead of a brazing foil of Cu50%-Bi50% as the brazing material, and a joint structure was obtained by brazing a current-carrying shaft made of oxygen-free copper to a contact made of a Cu alloy (Cu75%-Cr25% by weight). When the cross section of the brazed portion was observed with an electron microscope, it was found that, as in the joint structure shown in FIG. 6, part of the Zn contained in the Cu50%-Zn50% alloy evaporated, and the side became a Cu-rich region (joining material 2), the center had a composition close to the initial composition (joining material 1), and the intermediate composition (joining material 3) in between changed continuously from the composition of joining material 1 to the composition of joining material 3. As a result of elemental analysis, joining material 2 was Cu90%-Zn10% by weight, joining material 3 had an average composition of Cu60%-Zn40% by weight, and joining material 1 had the initial composition.

[0037] FIG. 13 shows an example of a Cu-Zn system equilibrium phase diagram. In the figure, 133 indicates the liquidus line. From the phase diagram, it was confirmed that the solidus temperatures were approximately 1030°C for joining material 2, 890°C for joining material 3, and 870°C for joining material 1, and that the liquidus temperatures were approximately 1050°C for joining material 2, 900°C for joining material 3, and 850°C for joining material 1. In addition, when the resistance between the contact and the current-carrying shaft was measured, it was approximately the same as when a similar contact and current-carrying shaft were fully brazed with eutectic silver solder. This joint structure was heated at 800°C for 10 minutes, but the Cu alloy did not fall off from the oxygen-free copper. The results obtained are shown in Table 1 below.

[0038] Comparative Example 1 A 50 mm diameter oxygen-free copper current-carrying shaft and a 50 mm diameter Cu alloy (Cu 75 wt %-Cr 25 wt %) contact were joined via Ni-P brazing paste. A brazing process was performed in a vacuum atmosphere with a temperature of 900°C and a holding time of 10 minutes to obtain a joint structure. When the resistance between the contact and the current-carrying shaft was measured after the brazing was completed, it was about 20 times the reference resistance value of Example 1. In addition, this joint structure was heated at 800°C for 10 minutes, but the Cu alloy did not fall off from the oxygen-free copper.

[0039] Comparative Example 2 A 50 mm diameter oxygen-free copper current-carrying shaft and a 50 mm diameter Cu alloy (Cu 75 wt %-Cr 25 wt %) contact were joined via eutectic silver brazing foil. Brazing was performed in a vacuum atmosphere at a temperature of 900°C and a holding time of 10 minutes to obtain a joint structure. When the resistance between the contact and the current-carrying shaft was measured after brazing was completed, a sufficient resistance value was obtained. Note that in each example, the resistance value was compared using this resistance value as the reference value. When this joint structure was heated at 800°C for 10 minutes, the Cu alloy fell off from the oxygen-free copper. The results obtained are shown in Table 1 below.

[0040] [Table 1]

[0041] As shown in Table 1, in the joint structures of Examples 1 to 6, it is possible to prevent the joint layer from burning through at high temperatures and to prevent an increase in the resistance value of the joint layer. As the Cu alloy used as the contacts in Examples 1 to 6, other combinations are applicable, such as Cu-50% by weight W-1% by weight Sb, Cu-60% by weight Mo-2% by weight Cr, Cu-40% by weight Mo-1% by weight Cr, Cu-25% by weight Cr, Cu-50% by weight Cr, or Cu-65% by weight Cr, etc. In addition, any other material can be used as the base material. In addition, in relation to Examples 1 and 2, the combinations shown in Table 2 below are also applicable as combinations of brazing filler metal 1 and brazing filler metal 2. In addition to the following, any joining material can be used as long as it satisfies the claims.

[0042] [Table 2]

[0043] In Table 2, Bal. indicates the balance. In the above embodiment, a joining structure for a vacuum interrupter is shown in which the first base material is the electrode and the second base material is the conductive shaft, but the joining structure between the first base material and the second base material can also be used for devices other than vacuum interrupters.

[0044] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]

[0045] 1...Insulating container, 4, 9, 34, 44, 54, 64...Electrifying shaft, 4a,9a...Second bonding area, 5, 25, 35, 45, 55...First bonding layer, 4a-1, 9a-1...Second part, 4a-2, 9a-2...Fourth part, 5-1, 8-1...First bonding part, 5-2, 8-2...Second Joint, 6, 7, 36, 46, 56, 66...Contact, 6a,7a...First bonding area, 6a-1, 7a-1...First part, 6a-2, 7a-2...Third part, 21, 22, 24, 26, 27...Electrode, 100...Vacuum valve, 121, 122, 126, 127...Joint structure

Claims

1. a first base material provided with a first bonding region; a second base material provided with a second bonding region disposed opposite the first bonding region; a first bonding layer that bonds the first bonding region and the second bonding region; The first base material is a contact point, and the second base material is a current-carrying shaft, A joining structure for a vacuum valve, characterized in that the first joining layer includes a first joining portion having a first liquidus temperature and joining a first portion of the first joining region and a second portion of the second joining region, and a second joining portion having a second liquidus temperature higher than the first liquidus temperature and joining a third portion different from the first portion of the first joining region and a fourth portion different from the second portion of the second joining region.

2. The joining structure of the vacuum valve according to claim 1 , further comprising a structure for shielding at least a portion between the first joining portion and the second joining portion.

3. 3. The joining structure of a vacuum valve according to claim 2, wherein the shielding structure is a slit provided in at least one of the first joining region and the second joining region.

4. The vacuum valve joint structure according to claim 1 , wherein the joint layer further includes a third joint portion between the first joint portion and the second joint portion, the third joint portion having a composition different from the compositions of the first joint portion and the second joint portion.

5. 5. The joining structure of a vacuum valve according to claim 4, wherein the third joining portion has a gradient composition, the composition of which changes continuously from the composition of the first joining portion to the composition of the second joining portion.

6. an insulating container having open ends at both ends; a vacuum vessel having a pair of sealing fittings joined to the open end; A vacuum valve comprising a pair of electrodes detachably provided on the vacuum vessel, At least one of the electrodes is a first base material provided with a first bonding region; a second base material provided with a second bonding region disposed opposite the first bonding region; a first bonding layer having a first solidus temperature bonding the first bonding region and the second bonding region, The first base material is a contact point, and the second base material is a current-carrying shaft, A vacuum valve characterized in that the first bonding layer includes a first bonding portion having a first liquidus temperature and bonding a first portion of the first bonding region and a second portion of the second bonding region, and a second bonding portion having a second liquidus temperature higher than the first liquidus temperature and bonding a third portion different from the first portion of the first bonding region and a fourth portion different from the second portion of the second bonding region.

7. 7. The vacuum valve as described in claim 6, wherein the first bonding layer has a first solidus temperature, the vacuum container includes a second bonding layer having a first liquidus temperature between both ends of the insulating container and a pair of sealing fittings, and the first liquidus temperature of the second bonding layer is lower than the first solidus temperature of the first bonding layer.

8. The vacuum valve according to claim 6 , further comprising a structure for shielding at least a portion between the first joint portion and the second joint portion.

9. 9. The vacuum valve according to claim 8, wherein the shielding structure is a slit provided in at least one of the first bonding region and the second bonding region.

10. The vacuum valve according to claim 6, wherein the first bonding layer further includes a third bonding portion between the first bonding portion and the second bonding portion, the third bonding portion having a composition different from the compositions of the first bonding portion and the second bonding portion.

11. 11. The vacuum valve according to claim 10, wherein the third joint has a gradient composition, the composition of which changes continuously from the composition of the first joint to the composition of the second joint.

Citation Information

Patent Citations

  • Method of treating contaminated and polluted waste liquids by magnetite

    JP1978032870A

  • Production of airtight ceramic vessel

    JP1989111784A

  • Vacuum valve and manufacture thereof

    JP1996031279A

  • Joining material for vacuum valve

    JP2013025870A

  • Substance for controllably releasing active substance

    JP1978050317A