Reflective mask blank, reflective mask, method for producing reflective mask blank, and method for producing reflective mask

A composite phase shift film with Ag and Ru improves etching selectivity and processability, addressing the limitations of Ag-based films in EUV lithography masks by promoting vertical etching and inhibiting horizontal etching, thereby enhancing pattern precision.

JP2024134752AActive Publication Date: 2024-10-04AGC INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023045100
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

Conventional phase shift films made of Ag have slow etching rates and low selectivity ratios during dry etching, making it difficult to form precise opening patterns for EUV lithography masks.

Method used

A phase shift film composed of a compound containing elements such as Ag and Ru, which enhances optical properties and processability by promoting vertical etching in dry etching and inhibiting horizontal etching in wet etching.

Benefits of technology

The composite phase shift film achieves improved etching selectivity and processability, allowing for precise pattern formation with reduced shadowing effects, enhancing the accuracy of EUV lithography masks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134752000001_ABST
    Figure 2024134752000001_ABST
Patent Text Reader

Abstract

To provide a phase shift film with superior optical properties and superior processability.SOLUTION: A reflective mask blank includes a substrate, a multilayer reflection film that reflects EUV light, a protective film that protects the multilayer reflection film, and a phase shift film that shifts the phase of the EUV light, in the stated order. The phase shift film has a layer composed of a compound. The compound contains at least one element X1 selected from Ag, Pd, In, Co, Ni, Pt, Cu and Au and at least one element X2 selected from Ru, Ta, Os, Si and Cr.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a reflective mask blank, a reflective mask, a method for manufacturing a reflective mask blank, and a method for manufacturing a reflective mask. [Background technology]

[0002] In recent years, with the miniaturization of semiconductor devices, EUV lithography (EUVL), an exposure technology using extreme ultraviolet (EUV) light, has been developed. EUV includes soft X-rays and vacuum ultraviolet light, and specifically refers to light with a wavelength of about 0.2 nm to 100 nm. At present, EUV with a wavelength of about 13.5 nm is mainly being considered.

[0003] In EUVL, a reflective mask is used. The reflective mask has, in this order, a substrate such as a glass substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light. An opening pattern is formed in the phase shift film. In EUVL, the opening pattern in the phase shift film is transferred to a target substrate such as a semiconductor substrate. Transferring includes reducing and transferring.

[0004] Patent Document 1 describes that the phase shift film contains at least one element selected from a first material group at a total content of at least 50 atomic %, and that the first material group contains Te, Co, Ni, Sn, Pt, In, Ag, Cu, Zn, and Bi. Patent Document 2 describes that the phase shift film is a multilayer film containing a first layer and a second layer, that the second layer contains any one of metal materials selected from Ru, Pt, Pd, Ag, and Au, that the material containing Ag may be an Ag alloy, and that the Ag alloy contains Ag as a main component and may also contain Nb, Zr, Y, B, Ti, La, Mo, Co, or Re. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2022 / 172916 [Patent Document 2] Patent No. 6441012 Summary of the Invention [Problem to be solved by the invention]

[0006] Traditionally, Ag and other materials have been considered as materials for phase shift films. Ag has a small refractive index and a large extinction coefficient, and has excellent optical properties. However, a film made only of Ag has a slow etching rate when dry-etched (anisotropic etching), and the etching rate ratio (selectivity) between the phase shift film and the protective film is small, making it difficult to form an opening pattern.

[0007] One aspect of the present disclosure provides a phase shift film having excellent optical properties and processability. [Means for solving the problem]

[0008] A reflective mask blank according to one embodiment of the present disclosure includes, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light. The phase shift film includes a layer made of a compound. The compound includes at least one element X1 selected from Ag, Pd, In, Co, Ni, Pt, Cu, and Au, and at least one element X2 selected from Ru, Ta, Os, Si, and Cr. Effect of the Invention

[0009] According to one embodiment of the present disclosure, the phase shift film has a layer made of a compound containing X1 and X2. By adding X2 to X1, it is possible to provide a phase shift film having excellent optical properties and processability. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view showing a reflective mask blank according to one embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a reflective mask according to an embodiment. [Diagram 3] FIG. 3 is a cross-sectional view showing an example of EUV light reflected by the reflective mask of FIG. [Figure 4] FIG. 4 is a flowchart showing a method for manufacturing a reflective mask blank according to one embodiment. [Diagram 5] FIG. 5 is a flowchart showing a method for manufacturing a reflective mask according to an embodiment. [Figure 6] FIG. 6 is a diagram showing an example of the refractive index and extinction coefficient of each element. [Figure 7] FIG. 7 is a flowchart showing an example of S203 in FIG. [Figure 8] FIG. 8 is a cross-sectional view showing an example of S203 in FIG. [Figure 9] FIG. 9 is a SEM photograph showing an example of S203 in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In each drawing, the same or corresponding components are denoted by the same reference numerals, and the description may be omitted. In the specification, the symbol "~" indicating a range of values ​​means that the values ​​before and after the symbol are included as the lower and upper limits.

[0012] 1 to 3, the X-axis direction, the Y-axis direction, and the Z-axis direction are perpendicular to each other. The Z-axis direction is perpendicular to the first main surface 10a of the substrate 10. The X-axis direction is perpendicular to the incidence surface of the EUV light (the surface including the incident light beam and the reflected light beam). As shown in FIG. 3, the incident light beam is inclined toward the positive Y-axis direction as it moves toward the negative Z-axis direction, and the reflected light beam is inclined toward the positive Y-axis direction as it moves toward the positive Z-axis direction.

[0013] A reflective mask blank 1 according to one embodiment will be described with reference to Fig. 1. The reflective mask blank 1 has, for example, a substrate 10, a multilayer reflective film 11, a protective film 12, a phase shift film 13, and an etching mask film 14, in this order. The multilayer reflective film 11, the protective film 12, the phase shift film 13, and the etching mask film 14 are formed, in this order, on a first main surface 10a of the substrate 10. It should be noted that the reflective mask blank 1 only needs to have at least the substrate 10, the multilayer reflective film 11, the protective film 12, and the phase shift film 13.

[0014] The reflective mask blank 1 may further have a functional film not shown in FIG. 1. For example, the reflective mask blank 1 may have a conductive film on the opposite side of the multilayer reflective film 11 with respect to the substrate 10. The conductive film is formed on the second main surface 10b of the substrate 10. The second main surface 10b is the surface facing opposite to the first main surface 10a. The conductive film is used, for example, to attach the reflective mask 2 to an electrostatic chuck of an exposure tool. The reflective mask blank 1 may have a diffusion barrier film (not shown) between the multilayer reflective film 11 and the protective film 12. The diffusion barrier film suppresses diffusion of metal elements contained in the protective film 12 into the multilayer reflective film 11.

[0015] Although not shown, the reflective mask blank 1 may have a buffer film between the protective film 12 and the phase shift film 13. The buffer film protects the protective film 12 from an etching gas that forms an opening pattern 13a in the phase shift film 13. The buffer film is etched more slowly than the phase shift film 13. Unlike the protective film 12, the buffer film will ultimately have the same opening pattern as the opening pattern 13a of the phase shift film 13.

[0016] Next, a reflective mask 2 according to one embodiment will be described with reference to Figures 2 and 3. The reflective mask 2 is produced, for example, by using the reflective mask blank 1 shown in Figure 1, and includes an opening pattern 13a in a phase shift film 13. Note that the etching mask film 14 shown in Figure 1 is removed after the opening pattern 13a is formed in the phase shift film 13.

[0017] In EUVL, the opening pattern 13a of the phase shift film 13 is transferred to a target substrate such as a semiconductor substrate. The transfer includes reducing and transferring. The substrate 10, the multilayer reflective film 11, the protective film 12, the phase shift film 13, and the etching mask film 14 will be described below in this order.

[0018] The substrate 10 is, for example, a glass substrate. The material of the substrate 10 is preferably quartz glass containing TiO2. Quartz glass has a smaller linear expansion coefficient and a smaller dimensional change due to temperature change than general soda-lime glass. Quartz glass may contain 80% to 95% by mass of SiO2 and 4% to 17% by mass of TiO2. When the TiO2 content is 4% to 17% by mass, the linear expansion coefficient is approximately zero near room temperature, and there is almost no dimensional change near room temperature. Quartz glass may contain a third component or impurity other than SiO2 and TiO2. The material of the substrate 10 may be crystallized glass in which a β-quartz solid solution is precipitated, silicon, metal, or the like.

[0019] The substrate 10 has a first main surface 10a and a second main surface 10b facing opposite to the first main surface 10a. A multilayer reflective film 11 and the like are formed on the first main surface 10a. The size of the substrate 10 in plan view (viewed in the Z-axis direction) is, for example, 152 mm long and 152 mm wide. The vertical and horizontal dimensions may be 152 mm or more. The first main surface 10a and the second main surface 10b each have, for example, a square quality assurance area in the center. The size of the quality assurance area is, for example, 142 mm long and 142 mm wide. The quality assurance area of ​​the first main surface 10a preferably has a root-mean-square roughness (Rq) of 0.15 nm or less and a flatness of 100 nm or less. In addition, it is preferable that the quality assurance area of ​​the first main surface 10a does not have a defect that causes a phase defect.

[0020] The multilayer reflective film 11 reflects EUV light. The multilayer reflective film 11 is, for example, formed by alternately laminating a high refractive index layer and a low refractive index layer. The material of the high refractive index layer is, for example, silicon (Si), and the material of the low refractive index layer is, for example, molybdenum (Mo), and a Mo / Si multilayer reflective film is used. Note that a Ru / Si multilayer reflective film, a Mo / Be multilayer reflective film, a Mo compound / Si compound multilayer reflective film, a Si / Mo / Ru multilayer reflective film, a Si / Mo / Ru / Mo multilayer reflective film, a Si / Ru / Mo / Ru multilayer reflective film, a Si / Ru / Mo multilayer reflective film, etc. can also be used as the multilayer reflective film 11.

[0021] The film thickness of each layer constituting the multilayer reflective film 11 and the number of repeating units of the layer can be appropriately selected according to the material of each layer and the reflectivity with respect to EUV light. When the multilayer reflective film 11 is a Mo / Si multilayer reflective film, in order to achieve a reflectivity of 60% or more with respect to EUV light with an incident angle θ (see FIG. 3) of 6°, a Mo layer with a film thickness of 2.3 ± 0.1 nm and a Si layer with a film thickness of 4.5 ± 0.1 nm may be laminated so that the number of repeating units is 30 or more and 60 or less. The multilayer reflective film 11 preferably has a reflectivity of 60% or more with respect to EUV light with an incident angle θ of 6°. More preferably, the reflectivity is 65% or more.

[0022] The film formation method of each layer constituting the multilayer reflective film 11 is, for example, a DC sputtering method, a magnetron sputtering method, or an ion beam sputtering method. When forming a Mo / Si multilayer reflective film using the ion beam sputtering method, an example of the film formation conditions for each of the Mo layer and the Si layer is as follows. <Film formation conditions for Si layer> Target: Si target, Sputtering gas: Ar gas, Gas pressure: 1.3×10 -2 Pa~2.7×10 -2 Pa, Ion acceleration voltage: 300V~1500V, Film formation speed: 0.030 nm / sec~0.300 nm / sec, Film thickness of Si layer: 4.5 ± 0.1 nm, <Film formation conditions for Mo layer> Target: Mo target, Sputtering gas: Ar gas, Gas pressure: 1.3×10 -2 Pa to 2.7×10 -2 Pa, Ion acceleration voltage: 300 V to 1500 V, Film deposition rate: 0.030 nm / sec to 0.300 nm / sec, Thickness of Mo layer: 2.3 ± 0.1 nm, <Repeating unit of Si layer and Mo layer> Number of repeating units: 30 to 60 (preferably 40 to 50).

[0023] The protective film 12 is formed between the multilayer reflection film 11 and the phase shift film 13 and protects the multilayer reflection film 11. The protective film 12 protects the multilayer reflection film 11 from the etching gas that forms the opening pattern 13a (see FIG. 2) in the phase shift film 13. The protective film 12 remains on the multilayer reflection film 11 without being removed even when exposed to the etching gas.

[0024] The etching gas is, for example, a halogen-based gas, an oxygen-based gas, or a mixed gas thereof. Examples of the halogen-based gas include a chlorine-based gas and a fluorine-based gas. Examples of the chlorine-based gas include Cl2 gas, SiCl4 gas, CHCl3 gas, CCl4 gas, BCl3 gas, or a mixed gas thereof. Examples of the fluorine-based gas include CF4 gas, CHF3 gas, SF6 gas, BF3 gas, XeF2 gas, or a mixed gas thereof. Examples of the oxygen-based gas include O2 gas, O3 gas, or a mixed gas thereof.

[0025] The ratio (ER1 / ER2) of the etching rate ER1 of the phase shift film 13 by the etching gas to the etching rate ER2 of the protective film 12 by the etching gas is also called the selection ratio. The larger the selection ratio, the better the processability of the phase shift film 13. The selection ratio is preferably 10 or more, more preferably 30 or more. The selection ratio is preferably 200 or less, more preferably 100 or less.

[0026] The protective film 12 contains at least one element selected from, for example, Ru, Rh, and Si. When the protective film 12 contains Rh, the protective film 12 may contain only Rh, or may contain an Rh compound. The Rh compound may contain, in addition to Rh, at least one element Z1 selected from the group consisting of Ru, Nb, Mo, Ta, Ir, Pd, Zr, Y, and Ti.

[0027] By adding Ru, Nb, Mo, Zr, Y or Ti to Rh, the extinction coefficient can be reduced while suppressing an increase in the refractive index, and the reflectance to EUV light can be improved. Furthermore, by adding Ta, Ir, Pd or Y to Rh, the durability to etching gas and / or sulfuric acid / hydrogen peroxide can be improved. Sulfuric acid / hydrogen peroxide is used for removing a resist film or cleaning a reflective mask 2, which will be described later.

[0028] The element ratio (Z1:Rh) of Z1 (all Z1) to Rh is preferably 1:99 to 1:1. In this specification, the element ratio means a molar ratio. If the ratio value (Z1 / Rh) is 1 / 99 or more, the reflectance to EUV light is good. If the ratio value (Z1 / Rh) is 1 or less, the durability of the protective film 12 to the etching gas is good. The element ratio (Z1:Rh) of Z1 to Rh is more preferably 3:10 to 1:1.

[0029] When Z1 is Ru, the element ratio of Ru to Rh (Ru / Rh) is preferably greater than 0.0 and less than 1.0 (0.0<(Ru / Rh)<1.0), and more preferably greater than 0.3 and less than 0.5 (0.3<(Ru / Rh)<0.5). When the element ratio (Ru / Rh) is greater than 0.0, the reflectance to EUV light is good. When the element ratio (Ru / Rh) is less than 1.0, the etching resistance is good.

[0030] When Z1 is Pd, the element ratio of Pd to Rh (Pd / Rh) is preferably more than 0.00 and less than 1.0 (0.00<(Pd / Rh)<1.0), and more preferably more than 0.01 and less than 0.1 (0.01<(Pd / Rh)<0.1). When the element ratio (Pd / Rh) is more than 0.00, the etching resistance is good. When the element ratio (Pd / Rh) is less than 1.0, the reflectance to EUV light is good.

[0031] The Rh compound may contain, in addition to Rh, at least one element Z2 selected from the group consisting of N, O, C, and B. The element Z2 reduces the durability of the protective film 12 against etching gas, but improves the smoothness of the protective film 12 by reducing the crystallinity of the protective film 12. The Rh compound containing the element Z2 has an amorphous structure or a microcrystalline structure. When the Rh compound has an amorphous structure or a microcrystalline structure, the X-ray diffraction profile of the Rh compound does not have a clear peak.

[0032] When the Rh compound contains Z2 in addition to Rh, the content of Rh or the total content of Rh and Z1 is preferably 40 at% to 99 at% and the total content of Z2 is preferably 1 at% to 60 at%. When the Rh compound contains Z2 in addition to Rh, the content of Rh or the total content of Rh and Z1 is more preferably 80 at% to 99 at% and the total content of Z2 is more preferably 1 at% to 20 at%.

[0033] The Rh compound contains 90 at % or more of Rh, contains at least one of Z1 and Z2, and has a density of 10.0 g / cm 3 ~14.0g / cm 3 The Rh compound has an amorphous or microcrystalline structure when it has a density of 11.0 g / cm. 3 ~13.0g / cm 3 It is.

[0034] The protective film 12 contains 100 at % Rh and has a density of 11.0 g / cm 3 ~12.0g / cm 3When having a density, it has an amorphous structure or a microcrystalline structure. Note that the density of the protective film 12 is measured using the X-ray reflectivity method.

[0035] The thickness of the protective film 12 is preferably 1.0 nm to 4.0 nm, more preferably 2.0 nm to 3.5 nm, and even more preferably 2.5 nm to 3.0 nm. If the thickness of the protective film 12 is 1.0 nm or more, the etching resistance is good. Also, if the thickness of the protective film 12 is 4.0 nm or less, the reflectivity to EUV light is good.

[0036] The density of the protective film 12 is preferably 10.0 g / cm 3 ~14.0 g / cm 3 It is. If the density of the protective film 12 is 10.0 g / cm 3 or more, the etching resistance is good. Also, if the density of the protective film 12 is 14.0 g / cm 3 or less, a decrease in the reflectivity to EUV light can be suppressed.

[0037] The upper surface of the protective film 12, that is, the surface on which the phase shift film 13 of the protective film 12 is formed, preferably has a root mean square roughness Rq of 0.20 nm or less, more preferably 0.17 nm or less. If the root mean square roughness Rq is 0.20 nm or less, a phase shift film 13 or the like can be smoothly formed on the protective film 12. Also, scattering of EUV light can be suppressed, and the reflectivity to EUV light can be improved. The root mean square roughness Rq is preferably 0.05 nm or more.

[0038] The film formation method of the protective film 12 is, for example, a DC sputtering method, a magnetron sputtering method, or an ion beam sputtering method. When forming a Rh film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of Rh film> Target: Rh target, Sputtering gas: Ar gas, Gas pressure: 1.0×10 -2 Pa~1.0×10 0 Pa, Output density of target: 1.0 W / cm 2 ~8.5 W / cm 2 , Film formation rate: 0.020 nm / sec to 1.000 nm / sec, Film thickness: 1 nm to 10 nm.

[0039] When forming the Rh film, as the sputtering gas, N2 gas, or a mixed gas of Ar gas and N2 may be used. The volume ratio of N2 gas in the sputtering gas (N2 / (Ar + N2)) is 0.05 or more and 1.0 or less.

[0040] When forming the RhO film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of RhO film> Target: Rh target, Sputtering gas: O2 gas, or a mixed gas of Ar gas and O2, Volume ratio of O2 gas in the sputtering gas (O2 / (Ar + O2)): 0.05 to 1.0, Gas pressure: 1.0×10 -2 Pa to 1.0×10 0 Pa, Output density of target: 1.0 W / cm 2 ~8.5 W / cm 2 , Film formation rate: 0.020 nm / sec to 1.000 nm / sec, Film thickness: 1 nm to 10 nm.

[0041] When forming the RhRu film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of RhRu film> Target: Rh target and Ru target (or RhRu target), Sputtering gas: Ar gas, Gas pressure: 1.0×10 -2 Pa to 1.0×10 0 Pa, Output density of target: 1.0 W / cm 2 ~8.5 W / cm 2 , Film formation rate: 0.020nm / sec~1.000nm / sec, Film thickness: 1nm~10nm.

[0042] The phase shift film 13 is a film in which an opening pattern 13a is to be formed. The opening pattern 13a is not formed in the manufacturing process of the reflective mask blank 1, but is formed in the manufacturing process of the reflective mask 2. The phase shift film 13 shifts the phase of the second EUV light L2 with respect to the first EUV light L1 shown in FIG.

[0043] The first EUV light L1 is light that passes through the opening pattern 13a without passing through the phase shift film 13, is reflected by the multilayer reflective film 11, and passes through the opening pattern 13a without passing through the phase shift film 13 again. The second EUV light L2 is light that passes through the phase shift film 13 while being absorbed by the phase shift film 13, is reflected by the multilayer reflective film 11, and passes through the phase shift film 13 while being absorbed by the phase shift film 13 again.

[0044] The phase difference (≧0) between the first EUV light L1 and the second EUV light L2 is, for example, 170° to 250°. The phase of the first EUV light L1 may be ahead of or behind the phase of the second EUV light L2. The phase shift film 13 improves the contrast of the transferred image by utilizing the interference between the first EUV light L1 and the second EUV light L2. The transferred image is an image obtained by transferring the opening pattern 13a of the phase shift film 13 onto the target substrate.

[0045] In EUVL, a so-called projection effect (shadowing effect) occurs. The shadowing effect refers to a region in which the sidewall of the opening pattern 13a blocks the EUV light due to the incident angle θ of the EUV light being not 0° (for example, 6°), resulting in a positional or dimensional shift of the transferred image. In order to reduce the shadowing effect, it is effective to reduce the height of the sidewall of the opening pattern 13a, and it is also effective to thin the phase shift film 13.

[0046] The thickness of the phase shift film 13 is, for example, 60 nm or less, and preferably 50 nm or less, in order to reduce the shadowing effect. The thickness of the phase shift film 13 is preferably 20 nm or more, and more preferably 30 nm or more, in order to ensure a phase difference between the first EUV light L1 and the second EUV light L2.

[0047] In order to reduce the thickness of the phase shift film 13 so as to reduce the shadowing effect while maintaining the phase difference between the first EUV light L1 and the second EUV light L2, it is effective to reduce the refractive index n of the phase shift film 13. Also, in order to reduce the reflectance for EUV light, it is effective to increase the extinction coefficient k of the phase shift film 13. Thus, the phase shift film 13 is required to have excellent optical properties.

[0048] The phase shift film 13 is required to have excellent processability in addition to optical properties. The opening pattern 13a is usually formed by dry etching. Since dry etching is anisotropic etching, etching proceeds only in the vertical direction (Z-axis direction), and the opening pattern 13a has good accuracy.

[0049] The phase shift film 13 of this embodiment has a layer made of a compound containing the following elements X1 and X2 in order to achieve both optical properties and processability. Note that the phase shift film 13 is a single layer in this embodiment, but may be a multi-layer film. In any case, it is sufficient that at least one layer constituting the phase shift film 13 is formed of a compound containing the following elements X1 and X2.

[0050] The element X1 is at least one element selected from Ag, Pd, In, Co, Ni, Pt, Cu, and Au. Ag, Pt, Pd, and Au are excellent in that they have a small refractive index as shown in Figure 6. Ag, Pd, In, Co, Ni, Pt, Cu, and Au are also excellent in that they have a large extinction coefficient k as shown in Figure 6.

[0051] Although the element X1 has excellent optical properties, it reduces the etching rate ER1 by dry etching. A film consisting of only X1 has a small selection ratio (ER1 / ER2), making it difficult to form the opening pattern 13a. Therefore, by adding X2 to X1, the processability of the phase shift film 13 is improved.

[0052] The element X2 is at least one element selected from Ru, Ta, Os, Si, and Cr. Ru, Ta, Os, Si, and Cr react with the etching gas used in dry etching to generate volatile substances, which are desorbed. By adding X2 to X1, a phase shift film 13 having excellent optical properties and processability can be obtained.

[0053] The formation of the opening pattern 13a of the phase shift film 13 in this embodiment (Step S203) will be described with reference to Figures 7 to 9. As shown in Figure 7, Step S203 is different from the usual process and includes dry etching (Step S203a) and wet etching (Step S203b) in this order.

[0054] 8, the etching mask film 14 has an opening 14a exposing the phase shift film 13 and a covering portion 14b covering the phase shift film 13. The etching mask film 14 is used in both steps S203a and S203b in this embodiment, but may be removed before or during step S203b.

[0055] In the dry etching (step S203a), the phase shift film 13 is exposed to an etching gas at the openings 14a of the etching mask film 14. In the openings 14a, the element X2 is desorbed, and the element X1 remains. The dry etching residue 13R mainly contains the element X1. The residue 13R is clump-like in FIG. 8, but is actually granular as shown in FIG. 9. The granular residue 13R is scattered in the openings 14a.

[0056] Dry etching is anisotropic etching. The removal of element X2 proceeds only in the vertical direction (Z-axis direction) and hardly proceeds in the horizontal directions (X-axis and Y-axis directions). Therefore, in the opening 14a, the element X2 is removed and the compound is decomposed, whereas in the covering portion 14b, the element X1 and the element X2 remain bonded to each other.

[0057] In the wet etching (step S203b), the dry etching residue 13R is dissolved in an etching solution to remove the residue 13R. The etching solution is not particularly limited, but may include, for example, a sulfuric acid / hydrogen peroxide mixture (aqueous solution containing sulfuric acid and hydrogen peroxide) or an ammonia / hydrogen peroxide mixture (aqueous solution containing ammonia and hydrogen peroxide).

[0058] The element X1 is easily dissolved in the etching solution, and the residue 13R can be removed. On the other hand, the element X2 is hardly dissolved in the etching solution, and has excellent durability against the etching solution. Therefore, in the area where the element X1 and the element X2 remain bonded to each other, the wet etching hardly progresses.

[0059] The element X2 promotes etching in the vertical direction (Z-axis direction) in the dry etching (step S203a) and suppresses etching in the horizontal directions (X-axis direction and Y-axis direction) in the wet etching (step S203b). Therefore, by adding X2 to X1, a phase shift film 13 with excellent optical properties and processability can be obtained.

[0060] It is preferable that the phase shift film 13 contains Ag as X1 and at least one element selected from Ta and Ru as X2. Ta and Ru can improve durability against etching solutions by bonding with Ag, and can suppress etching in the lateral direction. It is more preferable that X2 is Ru. That is, it is more preferable that the phase shift film 13 contains Ag as X1 and Ru as X2.

[0061] In the phase shift film 13, the ratio (X1:X2) of the total content (mol%) of X1 to the total content (mol%) of X2 is preferably 20:80 to 80:20. If the ratio value (X1 / X2) is 20 / 80 or more, the optical characteristics are good. If the ratio value (X1 / X2) is 80 / 20 or less, etching in the vertical direction can be promoted in dry etching, and etching in the horizontal direction can be suppressed in wet etching.

[0062] In the phase shift film 13, (X1:X2) is more preferably 20:80 to 50:50, further preferably 25:75 to 50:50, and particularly preferably 25:75 to 40:60. If X2 is greater than X1, etching is more likely to proceed vertically in dry etching, and the phase shift film 13 is more likely to decompose into granular portions in the opening 14a. Therefore, the residue 13R is more likely to be removed in the subsequent wet etching.

[0063] The compound containing X1 and X2 may further contain at least one element selected from O, N, B, and C. The compound containing X1 and X2 can suppress crystallization by further containing O, N, B, or C. In addition, the compound containing X1 and X2 can reduce the refractive index n by further containing N.

[0064] The phase shift film 13 has a full width at half maximum FWHM of 1.0° or more of the highest intensity peak in the 2θ range of 20° to 50° measured by XRD using CuKα radiation. The out of plane method is used as the XRD method. If the full width at half maximum FWHM is 1.0° or more, the crystallinity of the phase shift film 13 is low, and the roughness of the sidewall of the opening pattern 13a can be reduced. The full width at half maximum FWHM is preferably 2.0° or more, more preferably 3.0° or more, and particularly preferably 4.0° or more. The larger the full width at half maximum FWHM, the better, and it is preferable that there is no clear peak.

[0065] The refractive index n of the phase shift film 13 is, for example, 0.920 or less, preferably 0.910 or less, and more preferably 0.900 or less. The smaller the refractive index n, the smaller the film thickness of the phase shift film 13 can be. The refractive index n is preferably 0.870 or more. In this specification, the refractive index is the refractive index for light with a wavelength of 13.5 nm.

[0066] The extinction coefficient k of the phase shift film 13 is, for example, 0.025 or more, preferably 0.028 or more, and more preferably 0.030 or more. The larger the extinction coefficient k, the more the reflectance for EUV light can be reduced. The extinction coefficient k is preferably 0.080 or less. In this specification, the extinction coefficient is the extinction coefficient for light with a wavelength of 13.5 nm.

[0067] The optical properties (refractive index n and extinction coefficient k) of the phase shift film 13 are taken from the database of the Center for X-Ray Optics, Lawrence Berkeley National Laboratory, or values ​​calculated from the "incident angle dependence" of reflectance described below.

[0068] The incident angle θ of the EUV light, the reflectance R for the EUV light, the refractive index n of the phase shift film 13, and the extinction coefficient k of the phase shift film 13 satisfy the following formula (1). R = |(sinθ-((n+ik) 2 -cos 2 θ) 1 / 2 ) / (sinθ+((n+ik) 2 -cos 2 θ) 1 / 2 )|···(1) A number of combinations of the incident angle θ and the reflectance R are measured, and the refractive index n and the extinction coefficient k are calculated by the least squares method so that the error between the multiple measurement data and equation (1) is minimized.

[0069] The etching rate of the phase shift film 13 by sulfuric acid peroxide is 0 nm / min to 0.05 nm / min. Sulfuric acid peroxide is used for removing the resist film described later, cleaning the reflective mask 2, etc. If the etching rate of the phase shift film 13 by sulfuric acid peroxide is 0.05 nm / min or less, damage to the phase shift film 13 during cleaning can be suppressed.

[0070] The film formation method of the phase shift film 13 is, for example, the DC sputtering method, the magnetron sputtering method, or the ion beam sputtering method, etc. The oxygen content of the phase shift film 13 can be controlled by the content of O2 gas in the sputtering gas. Also, the nitrogen content of the phase shift film 13 can be controlled by the content of N2 gas in the sputtering gas.

[0071] When forming a RuAg film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of RuAg film> Target: Ru target and Ag target, Output density of Re target: 1.0 W / cm 2 ~8.5 W / cm 2 、 Output density of Ag target: 0.1 W / cm 2 ~5.0 W / cm 2 、 Sputtering gas: Ar gas, Film formation rate: 0.020 nm / sec to 0.060 nm / sec, Film thickness: 20 nm to 60 nm.

[0072] The etching mask film 14 is formed on the opposite side of the protective film 12 with respect to the phase shift film 13, and is used to form an opening pattern 13a in the phase shift film 13. A resist film (not shown) is provided on the etching mask film 14. In the manufacturing process of the reflective mask 2, a first opening pattern is first formed in the resist film, then a second opening pattern is formed in the etching mask film 14 using the first opening pattern, and then a third opening pattern 13a is formed in the phase shift film 13 using the second opening pattern. The first opening pattern, the second opening pattern, and the third opening pattern 13a have the same dimensions and the same shape in a plan view (Z-axis direction view). The etching mask film 14 enables the resist film to be made thinner.

[0073] The etching mask film 14 preferably contains at least one element selected from Al, Hf, Y, Cr, Nb, Ti, Mo, Ta, and Si. The etching mask film 14 may further contain at least one element selected from O, N, C, and B.

[0074] The thickness of the etching mask film 14 is preferably 2 nm or more and 30 nm or less, more preferably 2 nm or more and 25 nm or less, and further preferably 2 nm or more and 10 nm or less.

[0075] The etching mask film 14 may be formed by, for example, DC sputtering, magnetron sputtering, or ion beam sputtering.

[0076] Next, a method for manufacturing a reflective mask blank 1 according to one embodiment will be described with reference to Fig. 4. The method for manufacturing the reflective mask blank 1 includes, for example, steps S101 to S105 shown in Fig. 4. In step S101, a substrate 10 is prepared. In step S102, a multilayer reflective film 11 is formed on a first main surface 10a of the substrate 10. In step S103, a protective film 12 is formed on the multilayer reflective film 11. In step S104, a phase shift film 13 is formed on the protective film 12. In step S105, an etching mask film 14 is formed on the phase shift film 13.

[0077] The method for manufacturing the reflective mask blank 1 only needs to include at least steps S101 to S104. The method for manufacturing the reflective mask blank 1 may further include a step of forming a functional film not shown in FIG.

[0078] Next, referring to FIG. 5, a method for manufacturing a reflective mask 2 according to an embodiment will be described. The method for manufacturing a reflective mask 2 includes steps S201 to S204 shown in FIG. 5. In step S201, a reflective mask blank 1 is prepared. In step S202, the etching mask film 14 is processed. A resist film (not shown) is provided on the etching mask film 14. First, a first opening pattern is formed in the resist film, and then a second opening pattern is formed in the etching mask film 14 using the first opening pattern. Thereafter, the resist film is removed. For example, sulfuric acid / hydrogen peroxide is used to remove the resist film. In step S203, a third opening pattern 13a is formed in the phase shift film 13 using the second opening pattern. In step S203, the phase shift film 13 is etched using an etching gas. In step S204, the etching mask film 14 is removed. For example, an etching gas is used to remove the etching mask film 14. The etching gas used in step S204 (removing the etching mask film 14) may be the same as the etching gas used in step S203 (forming the opening pattern 13a). The manufacturing method of the reflective mask 2 only needs to include at least steps S201 and S203. EXAMPLES

[0079] The experimental data will be described below. In Example 1, a reflective mask blank for EUVL was produced. The reflective mask blank was composed of a substrate, a multilayer reflective film, a protective film, and a phase shift film. Example 1 is an example.

[0080] The substrate was a SiO2-TiO2 glass substrate (6-inch (152 mm) square, 6.3 mm thick). The thermal expansion coefficient of this glass substrate at 20°C was 0.02×10 -7 / °C, Young's modulus is 67 GPa, Poisson's ratio is 0.17, and specific stiffness is 3.07 × 10 7 m 2 / s 2 The quality assurance area of ​​the first main surface of the substrate was polished to a root-mean-square roughness (Rq) of 0.15 nm or less and a flatness of 100 nm or less. A 100 nm-thick Cr film was formed on the second main surface of the substrate by magnetron sputtering. The sheet resistance of the Cr film was 100 Ω / □.

[0081] The multilayer reflective film was a Mo / Si multilayer reflective film. The Mo / Si multilayer reflective film was formed by repeating the deposition of a Si layer (thickness 4.5 nm) and a Mo layer (thickness 2.3 nm) 40 times using the ion beam sputtering method. The total thickness of the Mo / Si multilayer reflective film was 272 nm ((4.5 nm + 2.3 nm) x 40).

[0082] The protective film was a Rh film (thickness: 2.5 nm) formed by ion beam sputtering.

[0083] A RuAg film (thickness 35 nm) was formed as the phase shift film. The RuAg film was formed by using a two-target sputtering method. The film formation conditions for the RuAg film were as follows: Target: Ru target and Ag target, Power density of Ru target: 5.0 W / cm 2 , Power density of Ag target: 0.45W / cm 2 , Sputtering gas: Ar gas.

[0084] The chemical composition of the phase shift film was measured using an X-ray photoelectron spectrometer (PHI 5000 VersaProbe) manufactured by ULVAC-PHI, Inc. The chemical composition of the phase shift film was Ru content 70 at%, Ag content 30 at%, and the element ratio of Ru to Ag (Ru:Ag) was 70:30.

[0085] As an etching mask film, a Ta2O5 film (thickness: 10 nm) was formed by reactive sputtering.

[0086] A reflective mask was produced using the reflective mask blank of the above configuration. First, a resist was applied to the surface of the etching mask film to form a resist film. Next, electron beam lithography (exposure) and development were performed to form an opening pattern in the resist film. The opening pattern was a line and space pattern, and the line width and space (opening) width were each 200 nm.

[0087] Thereafter, processing of the etching mask film (step S202), dry etching of the phase shift film (step S203a), and wet etching of the phase shift film (step S203a) were performed in this order.

[0088] In step S202, plasma etching was performed using an ICP (Inductively Coupled Plasma) etching device under the following conditions: ICP antenna power: 100W, Substrate bias: 40W, Etching time: 30 sec. Etching gas: He gas and CF4 gas mixture, He gas flow rate: 12sccm, CF4 gas flow rate: 12sccm.

[0089] In step S203a, plasma etching was performed using an ICP etching device under the following conditions: ICP antenna power: 200W, Substrate bias: 40W, Etching time: 150 sec. Etching gas: A mixture of Cl2 and O2 gases Cl2 gas flow rate: 10sccm, O2 gas flow rate: 10sccm.

[0090] In step S203b, wet etching was performed by a dipping method under the following conditions: Etching solution: sulfuric acid / hydrogen peroxide (concentrated sulfuric acid 75% by volume, hydrogen peroxide 25% by volume), Concentrated sulfuric acid: 96% sulfuric acid by volume, 4% water by volume, Hydrogen peroxide solution: 30-35% hydrogen peroxide by volume, 65-70% water by volume, Etching solution temperature: 100°C, Soaking time: 20 minutes.

[0091] SEM photographs taken immediately after step S202, immediately after step S203a, and immediately after step S203b are shown in Fig. 9. As is clear from Fig. 9, an opening pattern identical to the opening pattern in the resist film was formed in the phase shift film.

[0092] In addition, when a reflective mask blank prepared under the same conditions as in Example 1 was immersed in sulfuric acid / hydrogen peroxide at 100°C for 20 minutes without forming a resist film, no change was observed in the film thickness of the phase shift film (RuAg film) before and after immersion.

[0093] The reflective mask blank, the reflective mask, the manufacturing method of the reflective mask blank, and the manufacturing method of the reflective mask according to the present disclosure have been described above, but the present disclosure is not limited to the above-mentioned embodiments. Various changes, modifications, substitutions, additions, deletions, and combinations are possible within the scope of the claims. These naturally fall within the technical scope of the present disclosure. [Explanation of symbols]

[0094] 1 Reflective mask blank 2 Reflective mask 10 Substrate 11 Multilayer reflective film 12 Protective film 13 Phase shift film

Claims

1. A reflective mask blank having, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light, The phase shift film has a layer made of a compound, and the compound contains at least one element X1 selected from Ag, Pd, In, Co, Ni, Pt, Cu, and Au, and at least one element X2 selected from Ru, Ta, Os, Si, and Cr.

2. 2. The reflective mask blank according to claim 1, wherein the phase shift film has a ratio (X1:X2) of the total content (mol %) of X1 to the total content (mol %) of X2 of 20:80 to 80:

20.

3. 3. The reflective mask blank according to claim 1, wherein the phase shift film contains Ag as X1 and at least one element selected from Ta and Ru as X2.

4. The reflective mask blank according to claim 3 , wherein the phase shift film contains Ag as X1 and Ru as X2.

5. 3. The reflective mask blank according to claim 1, wherein the phase shift film has a thickness of 20 nm to 60 nm.

6. The reflective mask blank according to claim 1 , wherein the protective film contains at least one element selected from the group consisting of Ru, Rh and Si.

7. an etching mask film is provided on the opposite side of the protective film with respect to the phase shift film; 3. The reflective mask blank according to claim 1, wherein the etching mask film contains at least one element selected from the group consisting of Al, Hf, Y, Cr, Nb, Ti, Mo, Ta and Si.

8. The reflective mask blank according to claim 7 , wherein the etching mask film further contains at least one element selected from the group consisting of O, N, C and B.

9. A reflective mask blank according to claim 1 or 2, A reflective mask including an opening pattern in the phase shift film.

10. A method for producing a reflective mask blank having, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light, comprising: forming the multilayer reflective film, the protective film, and the phase shift film in this order on the substrate; The phase shift film has a layer made of a compound, and the compound contains at least one element X1 selected from Ag, Pd, In, Co, Ni, Pt, Cu, and Au, and at least one element X2 selected from Ru, Ta, Os, Si, and Cr.

11. Preparing a reflective mask blank according to claim 1 or 2; forming an opening pattern in the phase shift film; having A method for manufacturing a reflective mask, wherein the formation of the opening pattern comprises dry etching and wet etching in this order.

12. The etching gas used in the dry etching is chlorine gas (Cl 2 gas) and oxygen gas (O 2 The method for producing a reflective mask according to claim 11 , further comprising the step of:

13. 12. The method for producing a reflective mask according to claim 11, wherein an etching solution used in the wet etching contains one of sulfuric acid / hydrogen peroxide (aqueous solution containing sulfuric acid and hydrogen peroxide) and ammonia / hydrogen peroxide (aqueous solution containing ammonia and hydrogen peroxide).

Citation Information

Patent Citations

  • Reflective mask blank, reflective mask and method of manufacturing the same, and method of manufacturing semiconductor device

    JP2016072438A

  • Reflection type photomask blank, and reflection type photomask

    JP2022108203A

  • Reflective photomask blank and reflective photomask

    JP2024091002A

  • Patterning device

    US20200096875A1

  • Reflective mask blank, reflective mask, production method therefor, and semiconductor device production method

    WO2019225736A1