Laser welding method

The laser welding method addresses the issue of welding defects in stacked metal plates by setting the scanning start point and adjusting energy density to control molten pool expansion, ensuring a smaller keyhole and preventing defects.

JP2024134755AActive Publication Date: 2024-10-04TOYOTA JIDOSHA KK

Patent Information

Application Number
JP2023045104
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

When welding multiple stacked metal plates in an upright position, the molten pool becomes thinner due to gravity, leading to a large keyhole and potential welding defects such as holes.

Method used

A laser welding method that sets the scanning start point of the laser beam between 135 to 315 degrees relative to the vertical axis of the molten pool and adjusts the energy density to suppress the formation of large keyholes by controlling the molten pool expansion.

Benefits of technology

The method effectively prevents welding defects by maintaining a smaller keyhole and constriction in the upper side of the molten pool, thereby enhancing the welding quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134755000001_ABST
    Figure 2024134755000001_ABST
Patent Text Reader

Abstract

To provide a laser welding method that can suppress the occurrence of poor welding, in welding a plurality of laminated metal plates while erecting the plates.SOLUTION: A laser welding method, which welds a plurality of laminated metal plates, by irradiating the plurality of metal plates with laser beams, while erecting the plurality of metal plates, comprises a step of irradiating the plurality of metal plates with laser beams to form circular molten pools and a step of scanning the outer peripheries of the molten pools with laser beams in one circle to enlarge the molten pools. In the step of enlarging the molten pools, a starting point for scanning with a laser beam is set in a range from 135 degrees to 315 degrees in a scanning direction of a laser beam with a portion just above the molten pool in a vertical direction set as zero degree.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to laser welding methods. [Background technology]

[0002] Patent Document 1 discloses welding a plurality of stacked metal plates by irradiating the metal plates with a laser beam while scanning the metal plates in a circular pattern. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-228715 A Summary of the Invention [Problem to be solved by the invention]

[0004] The inventors have found the following problems with a laser welding method in which a laser beam is irradiated onto a plurality of stacked metal plates while being scanned in a circular manner to weld the plurality of metal plates. When welding multiple stacked metal plates in an upright position, if the molten pool becomes large enough and the amount of molten metal increases, the gravity acting on the molten pool will cause the thickness of the molten pool in the plate thickness direction on the vertically upper side to become thinner. As a result, the keyhole formed in the molten pool by the irradiation of the laser beam will become too large, which may result in poor welding such as holes.

[0005] The present disclosure has been made in consideration of the above circumstances, and provides a laser welding method capable of suppressing the occurrence of welding defects when welding a plurality of stacked metal plates in an upright state. [Means for solving the problem]

[0006] A laser welding method according to an aspect of the present disclosure includes: A laser welding method for welding a plurality of stacked metal plates by irradiating the plurality of metal plates with a laser beam in an upright state, comprising the steps of: irradiating the plurality of metal plates with the laser beam to form a circular molten pool; and scanning the laser beam once around the outer periphery of the molten pool to expand the molten pool. In the step of expanding the molten pool, The scanning start point of the laser beam is set to 0 degrees directly above the molten pool in the vertical direction, and is set to a range of 135 degrees to 315 degrees in the scanning direction of the laser beam.

[0007] In a laser welding method according to one embodiment of the present disclosure, in a step of scanning a laser beam once around the outer periphery of the molten pool to expand the molten pool, the starting point of the scanning of the laser beam is set to 0 degrees directly above the vertical direction of the molten pool, and is set in the range of 135 degrees to 315 degrees in the scanning direction of the laser beam. In this configuration, when the laser beam is irradiated to the vertically upper side of the molten pool, the molten pool is not expanded sufficiently, and the amount of molten metal in the molten pool is small. Therefore, the constriction on the vertically upper side of the molten pool is small, and the keyhole formed on the vertically upper side of the molten pool is not too large. Therefore, the occurrence of welding defects such as holes can be suppressed.

[0008] In the step of expanding the molten pool, the scanning start point of the laser beam may be set in a range of 180 degrees to 270 degrees in the scanning direction of the laser beam. With this configuration, the occurrence of welding defects such as holes can be further suppressed.

[0009] In the step of expanding the molten pool, a vertical direction may be detected by a sensor, and a scanning start point of the laser beam may be determined based on the vertical direction detected by the sensor. With this configuration, the laser welding system can automatically determine the scanning start point of the laser beam.

[0010] In the step of expanding the molten pool, the irradiation energy density of the laser beam may be smaller on a vertically upper side of the molten pool than on a vertically lower side of the molten pool. With this configuration, occurrence of welding defects such as holes can be further suppressed.

[0011] A laser welding method according to an aspect of the present disclosure includes: A laser welding method for welding a plurality of stacked metal plates by irradiating the plurality of metal plates with a laser beam in an upright state, comprising the steps of: irradiating the plurality of metal plates with the laser beam to form a circular molten pool; and scanning the laser beam once around the outer periphery of the molten pool to expand the molten pool. In the step of expanding the molten pool, The irradiation energy density of the laser beam is made smaller on the vertically upper side of the molten pool than on the vertically lower side.

[0012] In a laser welding method according to one aspect of the present disclosure, in the step of expanding the molten pool, the irradiation energy density of the laser beam is made smaller on a vertically upper side of the molten pool than on a vertically lower side thereof. Therefore, the keyhole formed on the vertically upper side of the molten pool does not become too large, and the occurrence of welding defects such as holes can be suppressed.

[0013] In the step of expanding the molten pool, the irradiation energy density of the laser beam may be gradually decreased from the vertical lower side to the vertical upper side of the molten pool, and gradually increased from the vertical upper side to the vertical lower side of the molten pool. Effect of the Invention

[0014] The present disclosure provides a laser welding method capable of suppressing the occurrence of welding defects when welding a plurality of stacked metal plates in an upright state. [Brief description of the drawings]

[0015] [Figure 1]1 is a block diagram showing a laser welding system according to a first embodiment. [Diagram 2] This is a cross-sectional view along the xz plane showing how the laser beam LB is scanned once around the outer periphery of the circular molten pool MP, thereby expanding the molten pool MP. [Diagram 3] This is a cross-sectional view along the xz plane showing how the laser beam LB is scanned once around the outer periphery of the circular molten pool MP, thereby expanding the molten pool MP. [Figure 4] 1 is a yz plan view showing a schematic diagram of a scanning trajectory when a laser beam LB is scanned once around the outer periphery of a circular molten pool MP to expand the molten pool MP in a laser welding method according to a first embodiment. FIG. [Diagram 5] 1 is a macrophotograph showing a keyhole KH formed directly above in the vertical direction in a molten pool MP in a laser welding method according to an example of the first embodiment. [Figure 6] 11 is a macrophotograph showing a keyhole KH formed directly above in the vertical direction in a molten pool MP in a laser welding method according to a comparative example of the first embodiment. [Figure 7] FIG. 11 is a yz plan view showing a schematic diagram of a scanning trajectory when a laser beam LB is scanned once around the outer periphery of a circular molten pool MP to expand the molten pool MP in a laser welding method according to a second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, specific embodiments of the present disclosure will be described in detail with reference to the drawings. However, the present disclosure is not limited to the following embodiments. In addition, the following description and drawings are appropriately simplified for clarity of explanation.

[0017] (First embodiment) <Laser welding system configuration> First, a laser welding system according to a first embodiment will be described with reference to FIG. Fig. 1 is a block diagram showing a laser welding system according to the first embodiment. As shown in Fig. 1, in the laser welding system according to the present embodiment, a laser beam LB is irradiated onto two stacked metal sheets M1 and M2 in an upright state, forming a molten pool MP penetrating the two metal sheets M1 and M2, and welding the two metal sheets M1 and M2. The laser welding system shown in FIG. 1 is mounted on, for example, a manipulator (robot arm).

[0018] As shown in FIG. 1, the laser welding system according to this embodiment includes a laser oscillator 101, a galvano scanner 102, a gravity sensor 103, and a laser control unit 104. Naturally, the right-handed xyz Cartesian coordinate system shown in Fig. 1 and other drawings is for the convenience of explaining the positional relationship of the components. In Fig. 1 etc., the positive direction of the z axis is vertically upward, and the xy plane is the horizontal plane, which is common to all drawings.

[0019] The metal plates M1 and M2 to be welded are not limited to any particular material, but may be, for example, steel plates or aluminum alloy plates that constitute a vehicle. The metal plates M1 and M2 are made of, for example, the same metal, but may be made of different metals. The number of metal plates to be welded may be three or more.

[0020] The laser oscillator 101 oscillates a laser beam LB with a laser output based on a control signal output from a laser control unit 104. The laser beam LB output from the laser oscillator 101 is input to a galvano scanner . The laser oscillator 101 and the galvano scanner 102 constitute a laser irradiation unit that irradiates the metal plates M1 and M2, which are the objects to be welded, with a laser beam LB.

[0021] The galvano scanner 102 irradiates the metal plates M1 and M2, which are the objects to be welded, with a laser beam LB while scanning the metal plates M1 and M2 based on a control signal output from the laser control unit 104. For example, the spot diameter d of the laser beam LB irradiated from the galvano scanner 102 is set based on the control signal output from the laser control unit 104. s , scanning speed v s , trajectory, scanning start point, etc. are determined.

[0022] As shown in FIG. 1, a laser beam LB emitted from a galvano scanner 102 is scanned, for example, in a circular shape on stacked metal sheets M1 and M2, to form a molten pool MP having a circular shape when viewed in the yz plane. Furthermore, the laser beam LB is scanned once around the outer periphery of the circular molten pool MP thus formed, thereby enlarging the molten pool MP.

[0023] The gravity sensor 103 is a sensor that detects the direction of gravity, that is, the vertical direction. Note that the gravity sensor 103 is not essential. The laser control unit 104 controls the irradiation conditions of the laser beam LB. Specifically, the laser control unit 104 controls the output (laser output) P of the laser beam LB oscillated by the laser oscillator 101. The laser control unit 104 also controls the spot diameter d s , scanning speed v s , to control the trajectory.

[0024] Furthermore, the laser control unit 104 determines the scanning start point of the laser beam LB when enlarging the molten pool MP by scanning the laser beam LB once, based on the vertical direction detected by the gravity sensor 103. A method of determining the scanning start point in the laser control unit 104 will be described later in detail.

[0025] Although not shown, the laser control unit 104 includes a calculation unit such as a CPU (Central Processing Unit) and a storage unit such as a RAM (Random Access Memory) or a ROM (Read Only Memory) in which various control programs and data are stored. In other words, the laser control unit 104 has a function as a computer and performs various control processes based on the control programs.

[0026] 1 can be realized in hardware by the above-mentioned CPU, storage unit, other circuits, etc., and in software by various control programs stored in the storage unit, etc. In other words, the laser control unit 104 can be realized in various forms by hardware, software, or a combination of both.

[0027] <Laser welding method> Next, a laser welding method according to the first embodiment will be described with reference to Fig. 2 to Fig. 4. Fig. 2 and Fig. 3 are cross-sectional views in an xz plane showing a state in which a laser beam LB is caused to scan one revolution along the outer periphery of a circular molten pool MP to enlarge the molten pool MP. Fig. 4 is a yz plane view that typically shows a scanning trajectory when a laser beam LB is caused to scan one revolution along the outer periphery of a circular molten pool MP to enlarge the molten pool MP in the laser welding method according to the first embodiment.

[0028] First, as described with reference to Fig. 1, two stacked metal plates M1 and M2 are in an upright state and are irradiated with a laser beam LB emitted from a galvanometer scanner 102. Here, as shown in Fig. 1, the stacked metal plates M1 and M2 are scanned, for example, in a circular shape with the laser beam LB to form a molten pool MP having a circular shape when viewed in the yz plane.

[0029] The state in which the two stacked metal plates M1 and M2 are upright is not limited to a state in which the main surfaces of the metal plates M1 and M2 are parallel to the vertical direction. For example, the state in which the two stacked metal plates M1 and M2 are upright also includes a state in which the main surfaces of the metal plates M1 and M2 are inclined to some extent with respect to the vertical direction.

[0030] Next, as shown in FIGS. 2 and 3, the laser beam LB is scanned once around the outer periphery of the circular molten pool MP, thereby expanding the molten pool MP. 2 and 3, the molten pool MP becomes larger, and the thickness of the molten pool MP at the upper vertical side becomes thinner due to gravity acting on the molten pool MP. In other words, a constriction occurs at the upper vertical side of the molten pool MP in the thickness direction. Also, the larger the gap between the metal sheets M1 and M2 becomes, the larger the constriction at the upper vertical side of the molten pool MP becomes.

[0031] 2 and 3, a keyhole KH penetrating the molten pool MP is formed in the molten pool MP by the irradiation of the laser beam LB. As described above, the thickness of the molten pool MP in the plate thickness direction on the vertically upper side becomes thinner. Therefore, if the irradiation energy density of the laser beam LB is constant, the keyhole KH formed on the vertically upper side of the molten pool MP shown in FIG. 3 is larger than the keyhole KH formed on the vertically lower side of the molten pool MP shown in FIG. 2. The irradiation energy density of the laser beam LB will be described in detail in the second embodiment.

[0032] Therefore, as shown in Figure 3, if the molten pool MP is expanded and then the laser beam LB is irradiated to the vertically upward side of the molten pool MP, the keyhole KH becomes too large, which may result in welding defects such as holes.

[0033] Therefore, in the laser welding method according to this embodiment, the laser beam LB is scanned once around the outer periphery of the circular molten pool MP, and when the molten pool MP is expanded, the starting point of the scanning of the laser beam LB is set to a predetermined range as shown in FIG. The radius of the circular scanning locus shown in FIG. 4 is, for example, 1.0 mm or more, and preferably 2.0 mm or more.

[0034] Specifically, as shown by the thin double-headed arrow in Fig. 4, the scanning start point of the laser beam LB is set to 0 degrees directly above the molten pool MP in the vertical direction, and is set to a range of 135 degrees to 315 degrees in the scanning direction of the laser beam LB. Preferably, the scanning start point of the laser beam LB is set to a range of 180 degrees to 270 degrees in the scanning direction of the laser beam LB, as shown by the thick double-headed arrow in Fig. 4.

[0035] In this configuration, when the laser beam LB is irradiated to the vertically upper side of the molten pool MP, the molten pool MP is not expanded sufficiently, and the amount of molten metal in the molten pool MP is small. Therefore, the constriction generated on the vertically upper side of the molten pool MP shown in Figures 2 and 3 is small, and the keyhole KH formed on the vertically upper side of the molten pool MP does not become too large, which suppresses the occurrence of welding defects such as holes.

[0036] Although FIG. 4 is a plan view, the molten pool MP is displayed as a dot to facilitate understanding. In addition, although the laser beam LB scans counterclockwise in FIG. 4, the laser beam LB may scan clockwise.

[0037] Here, Fig. 5 is a macro photograph showing a keyhole KH formed directly above the molten pool MP in the vertical direction in a laser welding method according to an example of the first embodiment, and Fig. 6 is a macro photograph showing a keyhole KH formed directly above the molten pool MP in the vertical direction in a laser welding method according to a comparative example of the first embodiment.

[0038] In the embodiment shown in Fig. 5, the scanning start point of the laser beam LB when expanding the molten pool MP was set to 225 degrees in the scanning direction of the laser beam LB, with 0 degrees being directly above the molten pool MP in the vertical direction. On the other hand, in the comparative example shown in Fig. 6, the scanning start point of the laser beam LB when expanding the molten pool MP was set to 45 degrees in the scanning direction of the laser beam LB, with 0 degrees being directly above the molten pool MP in the vertical direction.

[0039] The keyhole KH in the comparative example shown in FIG. 6 is larger than the keyhole KH in the embodiment shown in FIG. In the comparative example shown in Fig. 6, the laser beam LB scans 315 degrees in one revolution of 360 degrees before reaching the vertically upper part of the molten pool MP (0 degrees in Fig. 4). Therefore, the molten pool MP is sufficiently enlarged, and the amount of molten metal in the molten pool MP increases. Therefore, it is considered that the constriction generated on the vertically upper side of the molten pool MP shown in Figs. 2 and 3 becomes larger, and the keyhole KH becomes larger.

[0040] In contrast, in the embodiment shown in Fig. 5, the laser beam LB scans 135 degrees in one revolution of 360 degrees before reaching the vertically upper part of the molten pool MP (0 degrees in Fig. 4). Therefore, the molten pool MP is not sufficiently expanded, and the amount of molten metal in the molten pool MP is small. Therefore, it is considered that the constriction generated on the vertically upper side of the molten pool MP shown in Figs. 2 and 3 is small, and the keyhole KH is also small. In this way, the laser welding method according to the embodiment can suppress the occurrence of welding defects such as holes, compared to the laser welding method according to the comparative example. The details of the examples and comparative examples will be described later.

[0041] As described above, in the laser welding method according to this embodiment, the laser beam LB is caused to scan once around the outer periphery of the circular molten pool MP, and when the molten pool MP is enlarged, the scanning start point of the laser beam LB is set to a predetermined range. Specifically, the scanning start point of the laser beam LB is set to 0 degrees directly above the molten pool MP in the vertical direction, and is set to a range of 135 degrees to 315 degrees in the scanning direction of the laser beam LB.

[0042] In this configuration, when the laser beam LB is irradiated to the vertically upper side of the molten pool MP, the molten pool MP is not expanded sufficiently, and the amount of molten metal in the molten pool MP is small. Therefore, the constriction generated on the vertically upper side of the molten pool MP shown in Figures 2 and 3 is small, and the keyhole KH formed on the vertically upper side of the molten pool MP is not too large. Therefore, the laser welding method according to this embodiment can suppress the occurrence of welding defects such as holes.

[0043] Second Embodiment Next, a laser welding method according to a second embodiment will be described with reference to Fig. 7. Fig. 7 is a yz plan view that shows a schematic diagram of a scanning trajectory when a laser beam LB is caused to scan once around the outer periphery of a circular molten pool MP to expand the molten pool MP in the laser welding method according to the second embodiment.

[0044] Although Fig. 7 is a plan view, the molten pool MP is displayed as a dot for easy understanding, similar to Fig. 4. Also, although the laser beam LB is scanned counterclockwise in Fig. 7, the laser beam LB may be scanned clockwise.

[0045] In the laser welding method according to this embodiment, the laser beam LB is scanned once around the outer periphery of the circular molten pool MP, and when expanding the molten pool MP, the irradiation energy density E of the laser beam LB is made smaller on the vertically upper side of the molten pool MP than on the vertically lower side. In the laser welding method according to this embodiment, the scanning start point of the laser beam LB is arbitrary.

[0046] Here, the irradiation energy density E [J / mm 2 ] is the laser power P [W], the scanning speed v s [mm / s], spot diameter d s Using [mm], it can be expressed by the following formula (1). E = P / (v s ×d s )...Equation (1)

[0047] Therefore, the laser output P should be reduced or the scanning speed v s or the spot diameter d s By increasing the irradiation energy density E, the irradiation energy density E of the laser beam LB on the vertically upper side of the molten pool MP is reduced. As an example, the irradiation energy density E of the laser beam LB on the vertically lower side of the molten pool MP is set to about 50% to 90% of the irradiation energy density E of the laser beam LB on the vertically lower side of the molten pool MP.

[0048] 7, the irradiation energy density of the laser beam LB is set to a maximum value directly below the molten pool MP in the vertical direction (180 degrees in FIG. 7) and a minimum value directly above the molten pool MP in the vertical direction (0 degrees in FIG. 7).Then, the irradiation energy density is gradually decreased from directly below the molten pool MP in the vertical direction toward directly above the molten pool MP, and gradually increased from directly above the molten pool MP in the vertical direction toward directly below the molten pool MP.

[0049] The irradiation energy density of the laser beam LB may be constant at a maximum value in a predetermined range including the area directly below the molten pool MP in the vertical direction (e.g., from 135 degrees to 225 degrees in FIG. 7). Also, the irradiation energy density of the laser beam LB may be constant at a minimum value in a predetermined range including the area directly above the molten pool MP in the vertical direction (e.g., from 0 degrees to 45 degrees and from 315 degrees to 360 degrees in FIG. 7).

[0050] As described above, in the laser welding method according to this embodiment, the laser beam LB is scanned once around the outer periphery of the circular molten pool MP, and when the molten pool MP is expanded, the irradiation energy density of the laser beam LB is made smaller on the vertically upper side of the molten pool MP than on the vertically lower side of the molten pool MP. Therefore, regardless of the scanning start point of the laser beam LB, the keyhole KH formed on the vertically upper side of the molten pool MP does not become too large, and the occurrence of welding defects such as holes can be suppressed.

[0051] The other configuration is similar to that of the first embodiment, and therefore the description will be omitted. This embodiment can be combined with the first embodiment. That is, when expanding the molten pool MP, the scanning start point of the laser beam LB may be set in the range of 135 degrees to 315 degrees in the scanning direction of the laser beam LB, and the irradiation energy density of the laser beam LB may be made smaller on the vertical upper side of the molten pool MP than on the vertical lower side. EXAMPLES

[0052] The laser welding method according to the first embodiment will be described in detail below with reference to examples and comparative examples. However, the laser welding method according to the first embodiment is not limited to the following examples.

[0053] <Test conditions> First, test conditions for the laser welding methods according to the examples and comparative examples will be described. The stacked three-piece steel plate set (upper plate, middle plate, and lower plate) was welded by irradiating the laser beam LB from the upper plate side while standing. Hot-dip galvanized steel plate SCGA440 was used for the upper plate, middle plate, and lower plate. The thickness of the upper plate was 1.4 mm, the thickness of the middle plate was 2.0 mm, and the thickness of the lower plate was 1.8 mm.

[0054] The gap between the upper plate and the middle plate was set equal to the gap between the middle plate and the lower plate. In each of the examples and the comparative examples, a three-piece steel plate set was used in which both gaps were changed to three levels: 0.1 mm, 0.3 mm, and 0.6 mm. Welding was performed at 1,000 locations for each of the three types of three-piece steel plate sets in the examples and the comparative examples.

[0055] A 20 kW ring laser oscillator manufactured by IPG was used as the laser oscillator 101. Furthermore, a 3D galvano head unit YD-3000ML (optical magnification 7.4 times) manufactured by Yaskawa Electric Corporation was used as the galvano scanner 102.

[0056] The irradiation conditions of the laser beam LB are: laser power P = 15 kW, scanning speed v s = 108 mm / s, spot diameter d s First, a circular molten pool MP with a radius of about 1.5 mm was formed, and then the laser beam LB was scanned along the outer periphery of the molten pool MP in a circular shape with a radius of 2.5 mm. In addition, compressed air with a flow rate of 3.0 m / s was supplied to the area irradiated with the laser beam LB, that is, the welded area.

[0057] 5 and 6, the scanning start point of the laser beam LB when expanding the molten pool MP (when the laser beam LB is scanned once around the circumference of the circular molten pool MP) was changed between the example and the comparative example. In the example, as shown in Fig. 5, the scanning start point of the laser beam LB was set to 225 degrees in the scanning direction of the laser beam LB, with 0 degrees being directly above the vertical direction of the molten pool MP. On the other hand, in the comparative example, as shown in Fig. 6, the scanning start point of the laser beam LB when expanding the molten pool MP was set to 45 degrees in the scanning direction of the laser beam LB, with 0 degrees being directly above the vertical direction of the molten pool MP.

[0058] <Test Results> In the laser welding method according to the embodiment, no welding defects occurred even when the gap between the three steel plates was 0.1 mm, 0.3 mm, or 0.6 mm. In the laser welding method according to the comparative example, no welding defects occurred when the gap between the three steel plates was 0.1 mm and 0.3 mm. On the other hand, in the laser welding method according to the comparative example, when the gap between the three steel plates was 0.6 mm, 12% of welding defects occurred.

[0059] The keyhole KH in the comparative example shown in FIG. 6 is larger than the keyhole KH in the embodiment shown in FIG. In the comparative example shown in Fig. 6, the laser beam LB scans 315 degrees in one revolution of 360 degrees before reaching the vertically upper part of the molten pool MP (0 degrees in Fig. 4). Therefore, the molten pool MP is sufficiently enlarged, and the amount of molten metal in the molten pool MP increases. Therefore, it is considered that the constriction generated on the vertically upper side of the molten pool MP shown in Figs. 2 and 3 becomes larger, and the keyhole KH becomes larger.

[0060] In contrast, in the embodiment shown in Fig. 5, the laser beam LB scans 135 degrees in one revolution of 360 degrees before reaching the vertically upper part of the molten pool MP (0 degrees in Fig. 4). Therefore, the molten pool MP is not sufficiently enlarged, and the amount of molten metal in the molten pool MP is small. Therefore, it is considered that the constriction generated on the vertically upper side of the molten pool MP shown in Figs. 2 and 3 is small, and the keyhole KH is also small.

[0061] In this way, the laser welding method according to the example was able to suppress the occurrence of welding defects such as holes, compared to the laser welding method according to the comparative example. That is, it was found that the laser welding method according to the first embodiment can suppress the occurrence of welding defects such as holes. It was also found that the laser welding method according to the first embodiment can more effectively suppress the occurrence of welding defects as the gap between the metal plates becomes larger.

[0062] The present disclosure is not limited to the above-described embodiment, and can be modified as appropriate without departing from the spirit and scope of the present disclosure. [Explanation of symbols]

[0063] 101 Laser Oscillator 102 Galvanometer Scanner 103 Gravity Sensor 104 Laser control unit KH Keyhole LB Laser Beam M1, M2 metal plate MP molten pool

Claims

1. A laser welding method for welding a plurality of stacked metal plates by irradiating the plurality of metal plates with a laser beam in an upright state, comprising the steps of: irradiating the plurality of metal plates with the laser beam to form a circular molten pool; and scanning the laser beam once around the outer periphery of the molten pool to expand the molten pool. In the step of expanding the molten pool, The scanning start point of the laser beam is set to 0 degrees directly above the molten pool in the vertical direction, and the scanning direction of the laser beam is set to a range of 135 degrees to 315 degrees. Laser welding method.

2. In the step of expanding the molten pool, The scanning start point of the laser beam is set in a range of 180 degrees to 270 degrees in the scanning direction of the laser beam. The laser welding method according to claim 1 .

3. In the step of expanding the molten pool, The sensor detects the vertical direction. determining a scanning start point of the laser beam based on the vertical direction detected by the sensor; The laser welding method according to claim 1 or 2.

4. In the step of expanding the molten pool, The irradiation energy density of the laser beam is made smaller on a vertically upper side of the molten pool than on a vertically lower side of the molten pool. The laser welding method according to claim 1 or 2.

5. A laser welding method for welding a plurality of stacked metal plates by irradiating the plurality of metal plates with a laser beam in an upright state, comprising the steps of: irradiating the plurality of metal plates with the laser beam to form a circular molten pool; and scanning the laser beam once around the outer periphery of the molten pool to expand the molten pool. In the step of expanding the molten pool, The irradiation energy density of the laser beam is made smaller on a vertically upper side of the molten pool than on a vertically lower side of the molten pool. Laser welding method.

6. In the step of expanding the molten pool, The irradiation energy density of the laser beam is gradually decreased from the vertical lower side to the vertical upper side of the molten pool, and is gradually increased from the vertical upper side to the vertical lower side of the molten pool. The laser welding method according to claim 5.

Citation Information

Patent Citations

  • Spot welding by laser beam

    JP1985021190A

  • Manufacture of thin semiconductor film

    JP1992062834A

  • Vessel made of ferritic stainless steel sheet having excellent weld zone low temperature strength and welding method therefor

    JP2007119808A

  • Laser welding apparatus and laser welding method

    JP2012228715A

  • Welding method and weld structure

    JP2015205323A

Cited By

  • Laser welding method and laser welding device

    CN123149564A