Reflective mask blank, reflective mask, method for producing reflective mask blank, and method for producing reflective mask

A rhenium-based phase shift film with additional elements addresses the surface roughness issue of Ru, providing enhanced optical properties and stability in EUV lithography.

JP2024135147AInactive Publication Date: 2024-10-04AGC INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023045692
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Ruthenium (Ru) is used in phase shift films for EUV lithography due to its low refractive index, but it has a small extinction coefficient, increasing reflectance and causing surface roughness due to oxidation in the atmosphere.

Method used

A phase shift film containing rhenium (Re) with additional elements such as Ta, Cr, W, Pt, Os, Pd, Rh, Co, Ni, Sn, or Au, and not substantially containing Ru, to enhance stability and reduce surface roughness.

Benefits of technology

The film achieves excellent optical properties and atmospheric stability by increasing the extinction coefficient and reducing surface roughness, while maintaining phase shift functionality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135147000001_ABST
    Figure 2024135147000001_ABST
Patent Text Reader

Abstract

To provide a phase shift film with superior optical properties and superior atmospheric stability.SOLUTION: A reflective mask blank includes a substrate, a multilayer reflection film that reflects EUV light, a protective film that protects the multilayer reflection film, and a phase shift film that shifts the phase of the EUV light, in the stated order. The phase shift film has a layer composed of a Re compound that contains at least one element X selected from Ta, Cr, W, Pt, Os, Pd, Rh, Co, Ni, Sn and Au in addition to Re, while being substantially free of Ru. The Re compound has the elemental ratio of Re to all X (Re:X) is 15:85 and 70:30.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a reflective mask blank, a reflective mask, a method for manufacturing a reflective mask blank, and a method for manufacturing a reflective mask. [Background technology]

[0002] In recent years, with the miniaturization of semiconductor devices, EUV lithography (EUVL), an exposure technology using extreme ultraviolet (EUV) light, has been developed. EUV includes soft X-rays and vacuum ultraviolet light, and specifically refers to light with a wavelength of about 0.2 nm to 100 nm. At present, EUV with a wavelength of about 13.5 nm is mainly being considered.

[0003] In EUVL, a reflective mask is used. The reflective mask has, in this order, a substrate such as a glass substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light. An opening pattern is formed in the phase shift film. In EUVL, the opening pattern in the phase shift film is transferred to a target substrate such as a semiconductor substrate. Transferring includes reducing and transferring.

[0004] Patent Document 1 describes that the phase shift film has a first layer and a second layer, and the second layer is made of a material containing Ru and Re. The element ratio of Ru to Re (Ru:Re) is 40:1 to 9:16. Patent Document 2 also describes that the phase shift film is made of a material containing Ru and Re, just like Patent Document 1. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2019 / 225737 [Patent Document 2] Patent Publication No. 2022-24617 Summary of the Invention [Problem to be solved by the invention]

[0006] Ru has been considered as a material for phase shift films. Ru has a small refractive index, which allows the phase shift film to be made thin while maintaining the phase difference of the film. However, Ru has a small extinction coefficient, which increases the reflectance of the film against EUV light.

[0007] Therefore, it is considered to use Re instead of Ru as the material for the phase shift film. Re has better workability than Rh, Pd, Pt, and Ir, and is non-toxic, unlike Os.

[0008] However, a film made only of Re will develop surface roughness and defects in the atmosphere. This is thought to be because the surface is oxidized by oxygen in the air, and the oxide reacts with water in the air (deliquesces). For example, the deliquescence of Re2O7 produces HReO4.

[0009] One aspect of the present disclosure provides a phase shift film having excellent optical properties and stability in air. [Means for solving the problem]

[0010] A reflective mask blank according to one embodiment of the present disclosure includes, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light. The phase shift film includes a layer formed of a Re compound that contains, in addition to Re, at least one element X selected from Ta, Cr, W, Pt, Os, Pd, Rh, Co, Ni, Sn, and Au, and is substantially free of Ru. The Re compound has an element ratio (Re:X) of Re to all Xs of 15:85 to 70:30. Effect of the Invention

[0011] According to one embodiment of the present disclosure, by using a Re compound containing, in addition to Re, at least one element X selected from Ta, Cr, W, Ir, Pt, Os, Pd, and Rh and substantially not containing Ru as the material of the phase shift film, it is possible to provide a phase shift film having excellent optical properties and stability in the atmosphere. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a cross-sectional view showing a reflective mask blank according to one embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a reflective mask according to an embodiment. [Diagram 3] FIG. 3 is a cross-sectional view showing an example of EUV light reflected by the reflective mask of FIG. [Figure 4] FIG. 4 is a flowchart showing a method for manufacturing a reflective mask blank according to one embodiment. [Diagram 5] FIG. 5 is a flowchart showing a method for manufacturing a reflective mask according to an embodiment. [Figure 6] FIG. 6 is a diagram showing an example of the refractive index and extinction coefficient of each element. [Figure 7] FIG. 7 is a graph showing an example of the change in haze value with time for each Ta content. [Figure 8] FIG. 8 is a graph showing an example of the change in haze value with time for each Cr content. [Figure 9] FIG. 9(A) is an SEM photograph showing the surface of the TaRe film of Example 1, FIG. 9(B) is an SEM photograph showing the surface of the TaRe film of Example 2, FIG. 9(C) is an SEM photograph showing the surface of the CrRe film of Example 3, and FIG. 9(D) is an SEM photograph showing the surface of the CrRe film of Example 4. [Figure 10] FIG. 10(A) is an SEM photograph showing the surface of the CrRe film of Example 5, FIG. 10(B) is an SEM photograph showing the surface of the Re film of Example 6, FIG. 10(C) is an SEM photograph showing the surface of the TaRe film of Example 7, and FIG. 10(D) is an SEM photograph showing the surface of the CrRe film of Example 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In each drawing, the same or corresponding components are denoted by the same reference numerals, and the description may be omitted. In the specification, the symbol "~" indicating a range of values ​​means that the values ​​before and after the symbol are included as the lower and upper limits.

[0014] 1 to 3, the X-axis direction, the Y-axis direction, and the Z-axis direction are perpendicular to each other. The Z-axis direction is perpendicular to the first main surface 10a of the substrate 10. The X-axis direction is perpendicular to the incidence surface of the EUV light (the surface including the incident light beam and the reflected light beam). As shown in FIG. 3, the incident light beam is inclined toward the positive Y-axis direction as it moves toward the negative Z-axis direction, and the reflected light beam is inclined toward the positive Y-axis direction as it moves toward the positive Z-axis direction.

[0015] A reflective mask blank 1 according to one embodiment will be described with reference to Fig. 1. The reflective mask blank 1 has, for example, a substrate 10, a multilayer reflective film 11, a protective film 12, a phase shift film 13, and an etching mask film 14, in this order. The multilayer reflective film 11, the protective film 12, the phase shift film 13, and the etching mask film 14 are formed, in this order, on a first main surface 10a of the substrate 10. It should be noted that the reflective mask blank 1 only needs to have at least the substrate 10, the multilayer reflective film 11, the protective film 12, and the phase shift film 13.

[0016] The reflective mask blank 1 may further have a functional film not shown in FIG. 1. For example, the reflective mask blank 1 may have a conductive film on the opposite side of the multilayer reflective film 11 with respect to the substrate 10. The conductive film is formed on the second main surface 10b of the substrate 10. The second main surface 10b is the surface facing opposite to the first main surface 10a. The conductive film is used, for example, to attach the reflective mask 2 to an electrostatic chuck of an exposure tool. The reflective mask blank 1 may have a diffusion barrier film (not shown) between the multilayer reflective film 11 and the protective film 12. The diffusion barrier film suppresses diffusion of metal elements contained in the protective film 12 into the multilayer reflective film 11.

[0017] Although not shown, the reflective mask blank 1 may have a buffer film between the protective film 12 and the phase shift film 13. The buffer film protects the protective film 12 from an etching gas that forms an opening pattern 13a in the phase shift film 13. The buffer film is etched more slowly than the phase shift film 13. Unlike the protective film 12, the buffer film will ultimately have the same opening pattern as the opening pattern 13a of the phase shift film 13.

[0018] Next, a reflective mask 2 according to one embodiment will be described with reference to Figures 2 and 3. The reflective mask 2 is produced, for example, by using the reflective mask blank 1 shown in Figure 1, and includes an opening pattern 13a in a phase shift film 13. Note that the etching mask film 14 shown in Figure 1 is removed after the opening pattern 13a is formed in the phase shift film 13.

[0019] In EUVL, the opening pattern 13a of the phase shift film 13 is transferred to a target substrate such as a semiconductor substrate. The transfer includes reducing and transferring. The substrate 10, the multilayer reflective film 11, the protective film 12, the phase shift film 13, and the etching mask film 14 will be described below in this order.

[0020] The substrate 10 is, for example, a glass substrate. The material of the substrate 10 is preferably quartz glass containing TiO2. Quartz glass has a smaller linear expansion coefficient and a smaller dimensional change due to temperature change than general soda-lime glass. Quartz glass may contain 80% to 95% by mass of SiO2 and 4% to 17% by mass of TiO2. When the TiO2 content is 4% to 17% by mass, the linear expansion coefficient is approximately zero near room temperature, and there is almost no dimensional change near room temperature. Quartz glass may contain a third component or impurity other than SiO2 and TiO2. The material of the substrate 10 may be crystallized glass in which a β-quartz solid solution is precipitated, silicon, metal, or the like.

[0021] The substrate 10 has a first main surface 10a and a second main surface 10b facing opposite to the first main surface 10a. A multilayer reflective film 11 and the like are formed on the first main surface 10a. The size of the substrate 10 in plan view (viewed in the Z-axis direction) is, for example, 152 mm long and 152 mm wide. The vertical and horizontal dimensions may be 152 mm or more. The first main surface 10a and the second main surface 10b each have, for example, a square quality assurance area in the center. The size of the quality assurance area is, for example, 142 mm long and 142 mm wide. The quality assurance area of ​​the first main surface 10a preferably has a root-mean-square roughness (Rq) of 0.15 nm or less and a flatness of 100 nm or less. In addition, it is preferable that the quality assurance area of ​​the first main surface 10a does not have a defect that causes a phase defect.

[0022] The multilayer reflective film 11 reflects EUV light. The multilayer reflective film 11 is, for example, a laminate of high refractive index layers and low refractive index layers alternately. The high refractive index layers are made of, for example, silicon (Si), and the low refractive index layers are made of, for example, molybdenum (Mo), and a Mo / Si multilayer reflective film is used. Note that Ru / Si multilayer reflective film, Mo / Be multilayer reflective film, Mo compound / Si compound multilayer reflective film, Si / Mo / Ru multilayer reflective film, Si / Mo / Ru / Mo multilayer reflective film, Si / Ru / Mo / Ru multilayer reflective film, Si / Ru / Mo multilayer reflective film, and the like can also be used as the multilayer reflective film 11.

[0023] The thickness of each layer constituting the multilayer reflective film 11 and the number of repeating units of the layers can be appropriately selected depending on the material of each layer and the reflectance to EUV light. When the multilayer reflective film 11 is a Mo / Si multilayer reflective film, in order to achieve a reflectance of 60% or more to EUV light with an incident angle θ (see FIG. 3) of 6°, Mo layers with a thickness of 2.3±0.1 nm and Si layers with a thickness of 4.5±0.1 nm may be laminated so that the number of repeating units is 30 or more and 60 or less. The multilayer reflective film 11 preferably has a reflectance of 60% or more to EUV light with an incident angle θ of 6°. The reflectance is more preferably 65% ​​or more.

[0024] The film formation method for each layer constituting the multilayer reflective film 11 is, for example, the DC sputtering method, the magnetron sputtering method, or the ion beam sputtering method, etc. When forming a Mo / Si multilayer reflective film using the ion beam sputtering method, an example of the film formation conditions for each of the Mo layer and the Si layer is as follows. <Film formation conditions for the Si layer> Target: Si target, Sputtering gas: Ar gas, Gas pressure: 1.3×10 -2 Pa~2.7×10 -2 Pa, Ion acceleration voltage: 300V~1500V, Film formation rate: 0.030nm / sec~0.300nm / sec, Thickness of the Si layer: 4.5±0.1nm, <Film formation conditions for the Mo layer> Target: Mo target, Sputtering gas: Ar gas, Gas pressure: 1.3×10 -2 Pa~2.7×10 -2 Pa, Ion acceleration voltage: 300V~1500V, Film formation rate: 0.030nm / sec~0.300nm / sec, Thickness of the Mo layer: 2.3±0.1nm, <Repeating unit of the Si layer and the Mo layer> Number of repeating units: 30~60 (preferably 40~50).

[0025] The protective film 12 is formed between the multilayer reflective film 11 and the phase shift film 13 and protects the multilayer reflective film 11. The protective film 12 protects the multilayer reflective film 11 from the etching gas that forms the opening pattern 13a (see Figure 2) in the phase shift film 13. The protective film 12 remains on the multilayer reflective film 11 without being removed even when exposed to the etching gas.

[0026] The etching gas is, for example, a halogen-based gas, an oxygen-based gas, or a mixed gas thereof. The halogen-based gas includes a chlorine-based gas and a fluorine-based gas. The chlorine-based gas is, for example, Cl2 gas, SiCl4 gas, CHCl3 gas, CCl4 gas, BCl3 gas, or a mixed gas thereof. The fluorine-based gas is, for example, CF4 gas, CHF3 gas, SF6 gas, BF3 gas, XeF2 gas, or a mixed gas thereof. The oxygen-based gas is, for example, O2 gas, O3 gas, or a mixed gas thereof.

[0027] The ratio (ER1 / ER2) of the etching rate ER1 of the phase shift film 13 by the etching gas to the etching rate ER2 of the protective film 12 by the etching gas is also called the selectivity. The higher the selectivity, the better the processability of the phase shift film 13. The selectivity is preferably 10 or more, and more preferably 30 or more. The selectivity is preferably 200 or less, and more preferably 100 or less.

[0028] The protective film 12 contains at least one element selected from, for example, Ru, Rh, and Si. When the protective film 12 contains Rh, the protective film 12 may contain only Rh, or may contain an Rh compound. The Rh compound may contain, in addition to Rh, at least one element Z1 selected from the group consisting of Ru, Nb, Mo, Ta, Ir, Pd, Zr, Y, and Ti.

[0029] By adding Ru, Nb, Mo, Zr, Y or Ti to Rh, the extinction coefficient can be reduced while suppressing an increase in the refractive index, and the reflectance to EUV light can be improved. Furthermore, by adding Ta, Ir, Pd or Y to Rh, the durability to etching gas and / or sulfuric acid / hydrogen peroxide can be improved. Sulfuric acid / hydrogen peroxide is used for removing a resist film or cleaning a reflective mask 2, which will be described later.

[0030] The element ratio (Z1:Rh) of Z1 (all Z1) to Rh is preferably 1:99 to 1:1. In this specification, the element ratio means a molar ratio. If the ratio value (Z1 / Rh) is 1 / 99 or more, the reflectance to EUV light is good. If the ratio value (Z1 / Rh) is 1 or less, the durability of the protective film 12 to the etching gas is good. The element ratio (Z1:Rh) of Z1 to Rh is more preferably 3:10 to 1:1.

[0031] When Z1 is Ru, the element ratio of Ru to Rh (Ru / Rh) is preferably greater than 0.0 and less than 1.0 (0.0<(Ru / Rh)<1.0), and more preferably greater than 0.3 and less than 0.5 (0.3<(Ru / Rh)<0.5). When the element ratio (Ru / Rh) is greater than 0.0, the reflectance to EUV light is good. When the element ratio (Ru / Rh) is less than 1.0, the etching resistance is good.

[0032] When Z1 is Pd, the element ratio of Pd to Rh (Pd / Rh) is preferably more than 0.00 and less than 1.0 (0.00<(Pd / Rh)<1.0), and more preferably more than 0.01 and less than 0.1 (0.01<(Pd / Rh)<0.1). When the element ratio (Pd / Rh) is more than 0.00, the etching resistance is good. When the element ratio (Pd / Rh) is less than 1.0, the reflectance to EUV light is good.

[0033] The Rh compound may contain, in addition to Rh, at least one element Z2 selected from the group consisting of N, O, C, and B. The element Z2 reduces the durability of the protective film 12 against etching gas, but improves the smoothness of the protective film 12 by reducing the crystallinity of the protective film 12. The Rh compound containing the element Z2 has an amorphous structure or a microcrystalline structure. When the Rh compound has an amorphous structure or a microcrystalline structure, the X-ray diffraction profile of the Rh compound does not have a clear peak.

[0034] When the Rh compound contains Z2 in addition to Rh, the content of Rh or the total content of Rh and Z1 is preferably 40 at% to 99 at% and the total content of Z2 is preferably 1 at% to 60 at%. When the Rh compound contains Z2 in addition to Rh, the content of Rh or the total content of Rh and Z1 is more preferably 80 at% to 99 at% and the total content of Z2 is more preferably 1 at% to 20 at%.

[0035] The Rh compound contains 90 at % or more of Rh, contains at least one of Z1 and Z2, and has a density of 10.0 g / cm 3 ~14.0g / cm 3 The Rh compound has an amorphous or microcrystalline structure when it has a density of 11.0 g / cm. 3 ~13.0g / cm 3 It is.

[0036] The protective film 12 contains 100 at % Rh and has a density of 11.0 g / cm 3 ~12.0g / cm 3 When the protective film 12 has a density of 0.1 to 100%, the protective film 12 has an amorphous structure or a microcrystalline structure. The density of the protective film 12 is measured by X-ray reflectance method.

[0037] The thickness of the protective film 12 is preferably 1.0 nm to 4.0 nm, more preferably 2.0 nm to 3.5 nm, and further preferably 2.5 nm to 3.0 nm. If the thickness of the protective film 12 is 1.0 nm or more, the etching resistance is good. If the thickness of the protective film 12 is 4.0 nm or less, the reflectance to EUV light is good.

[0038] The density of the protective film 12 is preferably 10.0 g / cm 3 ~14.0g / cm 3 The density of the protective film 12 is 10.0 g / cm 3 If the density of the protective film 12 is 14.0 g / cm or more, the etching resistance is good. 3 If it is equal to or less than this, a decrease in reflectance for EUV light can be suppressed.

[0039] The upper surface of the protective film 12, that is, the surface on which the phase shift film 13 of the protective film 12 is formed, preferably has a root mean square roughness Rq of 0.20 nm or less, more preferably 0.17 nm or less. If the root mean square roughness Rq is 0.20 nm or less, a phase shift film 13 or the like can be smoothly formed on the protective film 12. In addition, scattering of EUV light can be suppressed, and the reflectivity with respect to EUV light can be improved. The root mean square roughness Rq is preferably 0.05 nm or more.

[0040] Examples of the method for forming the protective film 12 include a DC sputtering method, a magnetron sputtering method, or an ion beam sputtering method. When forming a Rh film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of Rh film> Target: Rh target, Sputtering gas: Ar gas, Gas pressure: 1.0×10 -2 Pa~1.0×10 0 Pa, Output density of target: 1.0 W / cm 2 ~8.5 W / cm 2 、 Film formation rate: 0.020 nm / sec~1.000 nm / sec, Film thickness: 1 nm~10 nm.

[0041] When forming a Rh film, as the sputtering gas, N2 gas or a mixed gas of Ar gas and N2 may be used. The volume ratio of N2 gas in the sputtering gas (N2 / (Ar + N2)) is 0.05 or more and 1.0 or less.

[0042] When forming a RhO film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of RhO film> Target: Rh target, Sputtering gas: O2 gas or a mixed gas of Ar gas and O2, Volume ratio of O2 gas in the sputtering gas (O2 / (Ar + O2)): 0.05~1.0, Gas pressure: 1.0×10-2 Pa to 1.0×10 0 Pa, Output density of target: 1.0 W / cm 2 to 8.5 W / cm 2 , Film formation rate: 0.020 nm / sec to 1.000 nm / sec, Film thickness: 1 nm to 10 nm.

[0043] When forming a RhRu film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of RhRu film> Target: Rh target and Ru target (or RhRu target), Sputtering gas: Ar gas, Gas pressure: 1.0×10 -2 Pa to 1.0×10 0 Pa, Output density of target: 1.0 W / cm 2 to 8.5 W / cm 2 , Film formation rate: 0.020 nm / sec to 1.000 nm / sec, Film thickness: 1 nm to 10 nm.

[0044] The phase shift film 13 is a film on which an opening pattern 13a is to be formed. The opening pattern 13a is not formed in the manufacturing process of the reflective mask blank 1, but is formed in the manufacturing process of the reflective mask 2. The phase shift film 13 shifts the phase of the second EUV light L2 with respect to the first EUV light L1 shown in FIG. 3.

[0045] The first EUV light L1 passes through the opening pattern 13a without passing through the phase shift film 13, is reflected by the multilayer reflective film 11, and passes through the opening pattern 13a again without passing through the phase shift film 13. The second EUV light L2 passes through the phase shift film 13 while being absorbed by the phase shift film 13, is reflected by the multilayer reflective film 11, and passes through the phase shift film 13 again while being absorbed by the phase shift film 13.

[0046] The phase difference (≧0) between the first EUV light L1 and the second EUV light L2 is, for example, 170° to 250°. The phase of the first EUV light L1 may be ahead of or behind the phase of the second EUV light L2. The phase shift film 13 improves the contrast of the transferred image by utilizing the interference between the first EUV light L1 and the second EUV light L2. The transferred image is an image obtained by transferring the opening pattern 13a of the phase shift film 13 onto the target substrate.

[0047] In EUVL, a so-called projection effect (shadowing effect) occurs. The shadowing effect refers to a region in which the sidewall of the opening pattern 13a blocks the EUV light due to the incident angle θ of the EUV light being not 0° (for example, 6°), resulting in a positional or dimensional shift of the transferred image. In order to reduce the shadowing effect, it is effective to reduce the height of the sidewall of the opening pattern 13a, and it is also effective to thin the phase shift film 13.

[0048] The thickness of the phase shift film 13 is, for example, 60 nm or less, and preferably 50 nm or less, in order to reduce the shadowing effect. The thickness of the phase shift film 13 is preferably 20 nm or more, and more preferably 30 nm or more, in order to ensure a phase difference between the first EUV light L1 and the second EUV light L2.

[0049] In order to reduce the thickness of the phase shift film 13 so as to reduce the shadowing effect while ensuring the phase difference between the first EUV light L1 and the second EUV light L2, it is effective to reduce the refractive index n of the phase shift film 13. Therefore, the phase shift film 13 of this embodiment has a layer formed of a Re compound containing at least Re. In this embodiment, the phase shift film 13 is a single layer, but may be a multi-layer film. In any case, it is sufficient that at least one layer constituting the phase shift film 13 is formed of a Re compound.

[0050] As shown in Figure 6, materials with a small refractive index n include Ru, Rh, Pd, Pt, Ir, Os, and Re. Among these, Re has a larger extinction coefficient k than Ru, a higher selectivity (ER1 / ER2) than Rh, Pd, Pt, and Ir, and is non-toxic, unlike Os. However, a film made only of Re will develop surface roughness in the atmosphere, resulting in defects on the surface. This is thought to be because the surface is oxidized by oxygen in the atmosphere, and the oxide reacts with water in the atmosphere (deliquesces). For example, HReO4 is produced by the deliquescence of Re2O7.

[0051] The Re compound of this embodiment contains at least one element X selected from Ta, Cr, W, Pt, Os, Pd, Rh, Co, Ni, Sn, and Au in addition to Re, and is substantially free of Ru. By being substantially free of Ru, the Re compound can increase the extinction coefficient k and reduce the reflectance for EUV light. "Substantially free of Ru" means that the Ru content is 1 at% or less. By containing X, the Re compound can improve stability in the atmosphere and suppress surface roughness.

[0052] By adding Ta, Cr, W, Os, or Sn to Re, the etching rate ER1 can be increased, the selectivity (ER1 / ER2) can be increased, and processability can be improved. By adding Pt, Pd, Rh, Os, or Au to Re, the refractive index n can be decreased. By adding Pd, Pt, Os, Au, Co, Ni, or Sn to Re, the extinction coefficient k can be increased. By adding Ta, Cr, Os, Pt, Pd, Rh, or Au to Re, resistance to sulfuric acid / hydrogen peroxide can be improved.

[0053] The Re compound preferably contains at least one of Ta, Cr and Os as X, and more preferably contains Ta.

[0054] The Re compound preferably has an element ratio (Re:X) of Re to all X of 15:85 to 70:30. Re:X means (Re content (at%)):(total content (at%) of X). When the ratio value (Re / X) is 15 / 85 or more, the optical properties are good. When the ratio value (Re / X) is 70 / 30 or less, the stability in the atmosphere can be improved and surface roughness can be suppressed. (Re:X) is more preferably 30:70 to 65:35, and further preferably 40:60 to 60:40.

[0055] In the Re compound, the total content of Re and all of the X is preferably 70 at % or more and 100 at % or less.

[0056] The Re compound preferably contains at least one element selected from O, N, B, and C in addition to Re and X. The Re compound can suppress crystallization by containing O, N, B, or C. Furthermore, the Re compound can reduce the refractive index n by containing N.

[0057] The phase shift film 13 has a full width at half maximum FWHM of 1.0° or more of the highest intensity peak in the 2θ range of 20° to 50° measured by XRD using CuKα radiation. The out of plane method is used as the XRD method. If the full width at half maximum FWHM is 1.0° or more, the crystallinity of the phase shift film 13 is low, and the roughness of the sidewall of the opening pattern 13a can be reduced. The full width at half maximum FWHM is preferably 2.0° or more, more preferably 3.0° or more, and particularly preferably 4.0° or more. The larger the full width at half maximum FWHM, the better, and it is preferable that there is no clear peak.

[0058] The refractive index n of the phase shift film 13 is, for example, 0.945 or less, preferably 0.940 or less, and more preferably 0.935 or less. The smaller the refractive index n, the smaller the film thickness of the phase shift film 13 can be. The refractive index n is preferably 0.910 or more. In this specification, the refractive index is the refractive index for light with a wavelength of 13.5 nm.

[0059] The extinction coefficient k of the phase shift film 13 is, for example, 0.030 or more, preferably 0.033 or more, and more preferably 0.035 or more. The larger the extinction coefficient k, the more the reflectance for EUV light can be reduced. The extinction coefficient k is preferably 0.040 or less. In this specification, the extinction coefficient is the extinction coefficient for light with a wavelength of 13.5 nm.

[0060] The optical properties (refractive index n and extinction coefficient k) of the phase shift film 13 are taken from the database of the Center for X-Ray Optics, Lawrence Berkeley National Laboratory, or values ​​calculated from the "incident angle dependence" of reflectance described below.

[0061] The incident angle θ of the EUV light, the reflectance R for the EUV light, the refractive index n of the phase shift film 13, and the extinction coefficient k of the phase shift film 13 satisfy the following formula (1). R = |(sinθ-((n+ik) 2 -cos 2 θ) 1 / 2 ) / (sinθ+((n+ik) 2 -cos 2 θ) 1 / 2 )|···(1) A number of combinations of the incident angle θ and the reflectance R are measured, and the refractive index n and the extinction coefficient k are calculated by the least squares method so that the error between the multiple measurement data and equation (1) is minimized.

[0062] The etching rate of phase shift film 13 by sulfuric acid / hydrogen peroxide is 0 nm / min to 0.05 nm / min. Sulfuric acid / hydrogen peroxide is used for removing a resist film, which will be described later, or for cleaning reflective mask 2. If the etching rate of phase shift film 13 by sulfuric acid / hydrogen peroxide is 0.05 nm / min or less, damage to phase shift film 13 during cleaning can be suppressed.

[0063] The method for forming the phase shift film 13 is, for example, the DC sputtering method, the magnetron sputtering method, or the ion beam sputtering method. The oxygen content of the phase shift film 13 can be controlled by the content of O2 gas in the sputtering gas. Also, the nitrogen content of the phase shift film 13 can be controlled by the content of N2 gas in the sputtering gas.

[0064] When forming a TaRe film using the DC sputtering method, an example of the film formation conditions is as follows. <Film Formation Conditions of TaRe Film> Targets: Re target and Ta target, Output density of Re target: 1.0 W / cm 2 ~8.5 W / cm 2 , Output density of Ta target: 1.0 W / cm 2 ~8.5 W / cm 2 , Sputtering gas: Ar gas, Film formation rate: 0.020 nm / sec to 0.060 nm / sec, Film thickness: 20 nm to 60 nm.

[0065] When forming a CrRe film using the DC sputtering method, an example of the film formation conditions is as follows. <Film Formation Conditions of CrRe Film> Targets: Re target and Cr target, Output density of Re target: 1.0 W / cm 2 ~8.5 W / cm 2 , Output density of Cr target: 1.0 W / cm 2 ~8.5 W / cm 2 , Sputtering gas: Ar gas, Film formation rate: 0.020 nm / sec to 0.060 nm / sec, Film thickness: 20 nm to 60 nm.

[0066] The etching mask film 14 is formed on the opposite side of the protective film 12 with respect to the phase shift film 13, and is used to form an opening pattern 13a in the phase shift film 13. A resist film (not shown) is provided on the etching mask film 14. In the manufacturing process of the reflective mask 2, a first opening pattern is first formed in the resist film, then a second opening pattern is formed in the etching mask film 14 using the first opening pattern, and then a third opening pattern 13a is formed in the phase shift film 13 using the second opening pattern. The first opening pattern, the second opening pattern, and the third opening pattern 13a have the same dimensions and the same shape in a plan view (Z-axis direction view). The etching mask film 14 enables the resist film to be made thinner.

[0067] The etching mask film 14 preferably contains at least one element selected from Al, Hf, Y, Cr, Nb, Ti, Mo, Ta, and Si. The etching mask film 14 may further contain at least one element selected from O, N, and B.

[0068] The thickness of the etching mask film 14 is preferably 2 nm or more and 30 nm or less, more preferably 2 nm or more and 25 nm or less, and further preferably 2 nm or more and 10 nm or less.

[0069] The etching mask film 14 may be formed by, for example, DC sputtering, magnetron sputtering, or ion beam sputtering.

[0070] Next, a method for manufacturing a reflective mask blank 1 according to one embodiment will be described with reference to Fig. 4. The method for manufacturing the reflective mask blank 1 includes, for example, steps S101 to S105 shown in Fig. 4. In step S101, a substrate 10 is prepared. In step S102, a multilayer reflective film 11 is formed on a first main surface 10a of the substrate 10. In step S103, a protective film 12 is formed on the multilayer reflective film 11. In step S104, a phase shift film 13 is formed on the protective film 12. In step S105, an etching mask film 14 is formed on the phase shift film 13.

[0071] The method for manufacturing the reflective mask blank 1 only needs to include at least steps S101 to S104. The method for manufacturing the reflective mask blank 1 may further include a step of forming a functional film not shown in FIG.

[0072] Next, referring to FIG. 5, a method for manufacturing a reflective mask 2 according to an embodiment will be described. The method for manufacturing a reflective mask 2 includes steps S201 to S204 shown in FIG. 5. In step S201, a reflective mask blank 1 is prepared. In step S202, the etching mask film 14 is processed. A resist film (not shown) is provided on the etching mask film 14. First, a first opening pattern is formed in the resist film, and then a second opening pattern is formed in the etching mask film 14 using the first opening pattern. Thereafter, the resist film is removed. For example, sulfuric acid / hydrogen peroxide is used to remove the resist film. In step S203, a third opening pattern 13a is formed in the phase shift film 13 using the second opening pattern. In step S203, the phase shift film 13 is etched using an etching gas. In step S204, the etching mask film 14 is removed. For example, an etching gas is used to remove the etching mask film 14. The etching gas used in step S204 (removing the etching mask film 14) may be the same as the etching gas used in step S203 (forming the opening pattern 13a). The manufacturing method of the reflective mask 2 only needs to include at least steps S201 and S203. EXAMPLES

[0073] The experimental data will be described below. In Examples 1 to 10, phase shift films having the chemical compositions shown in Table 1 were formed on glass substrates. A SiO2-TiO2-based glass substrate (6-inch (152 mm) square outer shape, 6.3 mm thick) was prepared as the glass substrate. This glass substrate had a thermal expansion coefficient of 0.02×10 at 20°C. -7 / °C, Young's modulus is 67 GPa, Poisson's ratio is 0.17, and specific stiffness is 3.07 × 10 7 m 2 / s2 The phase shift film was formed by DC sputtering. The thickness of the phase shift film was 20 nm. Examples 1 to 5 are working examples, and Examples 6 to 10 are comparative examples.

[0074] The evaluation results of the phase shift films obtained in Examples 1 to 10 are shown in Table 1.

[0075] [Table 1] The chemical composition of the phase shift film was measured using an ULVAC-PHI X-ray photoelectron spectrometer (PHI 5000 VersaProbe). The optical properties (refractive index n and extinction coefficient k) of the phase shift film were measured as described above. The surface roughness of the phase shift film due to exposure to the atmosphere was evaluated by the haze value. The greater the surface roughness, the greater the haze value.

[0076] The haze value was measured in accordance with the Japanese Industrial Standard JIS K7136:2000 and was calculated as the percentage of the transmitted light that deviated from the incident light by 2.5° or more due to forward scattering among the light transmitted through the test panel in the thickness direction of the test panel. The light source used for measuring the haze value was the D65 light source described in the Japanese Industrial Standard JIS Z8720:2012.

[0077] The haze value was measured using a haze meter HZ-2 manufactured by Suga Test Co., Ltd., and the average value was calculated from three measurements. Table 1 shows the haze value H(0hr) measured immediately after film formation, the haze value H(24hr) measured after exposure to the atmosphere at room temperature for 24 hours, and the rate of increase (H(24hr) / H(0hr)).

[0078] Figure 7 shows the change in haze value over time for each Ta content (at%). Figure 8 shows the change in haze value over time for each Cr content (at%). In Figures 7 and 8, the horizontal axis shows the time of exposure to the atmosphere at room temperature. Furthermore, Figures 9 and 10 show SEM photographs of the surface of the phase shift film exposed to the atmosphere at room temperature for 24 hours.

[0079] As is clear from Table 1 and Figures 7 to 10, by adding Ta or Cr to Re, surface roughening due to exposure to the atmosphere can be suppressed. In particular, when the element ratio (Re:X) is 15:85 to 70:30, that is, when the Ta content or the Cr content is 30 at% to 85 at%, the haze value hardly increases and the surface roughening hardly occurs even when the phase shift film is exposed to the atmosphere for a long time.

[0080] As shown in Table 1, in Examples 9 and 10, since Ru was added to Re, the extinction coefficient k was low, being less than 0.035.

[0081] The reflective mask blank, the reflective mask, the manufacturing method of the reflective mask blank, and the manufacturing method of the reflective mask according to the present disclosure have been described above, but the present disclosure is not limited to the above-mentioned embodiments. Various changes, modifications, substitutions, additions, deletions, and combinations are possible within the scope of the claims. These naturally fall within the technical scope of the present disclosure. [Explanation of symbols]

[0082] 1 Reflective mask blank 2 Reflective mask 10 Substrate 11 Multilayer reflective film 12 Protective film 13 Phase shift film

Claims

1. A reflective mask blank having, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light, the phase shift film has a layer formed of an Re compound containing at least one element X selected from Ta, Cr, W, Pt, Os, Pd, Rh, Co, Ni, Sn and Au in addition to Re and substantially no Ru; The reflective mask blank, wherein the Re compound has an element ratio of Re to all X (Re:X) of 15:85 to 70:

30.

2. The reflective mask blank according to claim 1 , wherein the Re compound contains at least one element selected from O, N, B and C in addition to Re and X.

3. The reflective mask blank according to claim 1 or 2, wherein the Re compound has a refractive index n of 0.945 or less and an extinction coefficient k of 0.030 or more.

4. The reflective mask blank according to claim 1 , wherein the Re compound contains Ta as X.

5. 3. The reflective mask blank according to claim 1, wherein the phase shift film has a thickness of 20 nm to 60 nm.

6. The reflective mask blank according to claim 1 , wherein the protective film contains at least one element selected from the group consisting of Ru, Rh and Si.

7. an etching mask film is provided on the opposite side of the protective film with respect to the phase shift film; 3. The reflective mask blank according to claim 1, wherein the etching mask film contains at least one element selected from the group consisting of Al, Hf, Y, Cr, Nb, Ti, Mo, Ta and Si.

8. The reflective mask blank according to claim 7 , wherein the etching mask film further contains at least one element selected from the group consisting of O, N and B.

9. A reflective mask blank according to claim 1 or 2, A reflective mask including an opening pattern in the phase shift film.

10. A method for producing a reflective mask blank having, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light, comprising: forming the multilayer reflective film, the protective film, and the phase shift film in this order on the substrate; the phase shift film has a layer formed of an Re compound containing at least one element X selected from Ta, Cr, W, Pt, Os, Pd, Rh, Co, Ni, Sn and Au in addition to Re and substantially no Ru; The method for producing a reflective mask blank, wherein the Re compound has an element ratio of Re to all X (Re:X) of 15:85 to 70:

30.

11. Preparing a reflective mask blank according to claim 1 or 2; forming an opening pattern in the phase shift film; The method for manufacturing a reflective mask includes the steps of:

Citation Information

Patent Citations

  • Reflective mask blanks, reflective mask, and manufacturing method of semiconductor device

    JP2007273678A

  • Reflective photomask blank and reflective photomask

    JP2022107355A

  • Extreme ultraviolet mask absorber materials

    US20210341828A1

  • Reflective mask blank, reflective mask, production method therefor, and semiconductor device production method

    WO2019225736A1

  • Reflection-type mask blank for EUV lithography, reflection-type mask for EUV lithography, and manufacturing methods therefor

    WO2022118762A1