Method of forming altered layer of ceramic based material, device of forming altered layer, processing method, and processing device
By heating ceramic materials to 500°C or less and irradiating them with a 10W or less laser, an altered layer with reduced hardness is formed, enhancing machinability and addressing the challenges of processing ceramic matrix composites.
Patent Information
- Application Number
- JP2023046081
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-22
AI Technical Summary
Ceramic matrix composite materials are difficult to machine due to their hardness, and existing laser processing methods may leave residual cracks, necessitating improved machinability and workability.
A method involving heating the ceramic material to 500°C or less and irradiating it with a laser of 10W or less to form an altered layer with reduced hardness, which extends deeper into the material, facilitating easier removal of the deteriorated layer.
The method improves the workability of ceramic materials by forming an altered layer with lower hardness, allowing for more effective machining and reducing the likelihood of residual cracks.
Smart Images

Figure 2024135414000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and apparatus for forming a deteriorated layer on a ceramic material, a processing method and a processing apparatus. [Background technology]
[0002] Conventionally, nickel-based superalloys (e.g., Inconel (registered trademark)) have been used for high-temperature structural components in aircraft engines and the like, but there is a strong demand, particularly in the aerospace industry, for weight reduction of aircraft bodies, improved fuel efficiency, and longer life. Therefore, research and development of composite materials has been conducted, and in particular, further research and development of ceramic matrix composite materials (CMC: Ceramic Matrix Composites) is being conducted. Ceramic matrix composite materials include SiC fiber-reinforced SiC composite materials (SiC / SiC composite materials) and carbon fiber-reinforced carbon composite materials (C / C composites).
[0003] Ceramic matrix composite materials have the advantages of ceramics, such as high heat resistance, high rigidity, and high wear resistance, and are made by combining ceramic matrix with ceramic fibers to improve the low toughness, which is a drawback of ceramics. However, because of their hardness, ceramic matrix composite materials are difficult to machine, and because they are difficult to cut, they have only been processed by surface grinding. Therefore, various research efforts are being conducted to improve the processability of ceramic matrix composite materials.
[0004] Patent Document 1 discloses an example of a method for processing such a ceramic matrix composite material. According to the description in Patent Document 1, the method for processing a ceramic matrix composite material disclosed therein includes a step of scanning and irradiating a laser irradiation portion on the surface of a workpiece, forming a deteriorated layer (embrittled surface layer) on the surface of the workpiece in the irradiated portion, and a step of sequentially removing the deteriorated layer formed in the irradiated portion by an end mill, and the deteriorated layer is formed by heating the irradiated portion to a predetermined temperature by irradiating it with a continuous wave laser and forming cracks by irradiating it with a pulsed wave laser. The predetermined temperature is a temperature at which a thermally altered layer can be formed on the surface of the ceramic matrix composite material, and it is described that, for example, SiC fibers and matrices made of polymer raw materials with low heat resistance start to thermally decompose at about 1300°C to 1400°C or higher, and a thermally altered layer is formed. Thus, the method of Patent Document 1 is directed to a process in which a ceramic matrix composite is heated to a predetermined temperature exceeding 1,300°C by irradiating it with a continuous wave laser, and a deterioration layer is formed by forming cracks on the surface of the ceramic matrix composite by irradiating it with a pulsed wave laser, and the deterioration layer formed in the irradiated area is sequentially removed with an end mill. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2014-172127 A [Non-patent literature]
[0006] [Non-Patent Document 1] Ryo Ando, Yuji Sogabe, Hidemaru Saotome, and Osamu Iimura, Study on softening of SiC surface by laser irradiation, Abstracts of the Annual Meeting of the Ceramic Society of Japan (Web), 2022 [Non-Patent Document 2] Yuji Sogabe, Ryo Ando, Hidemaru Saotome, and Shuji Iimura, Study on the altered layer formed on the surface of SiC by laser irradiation, Proceedings of the Symposium on Basic Science of Ceramics (Web), 2022 Summary of the Invention [Problem to be solved by the invention]
[0007] The method of Patent Document 1 involves irradiating the surface of a ceramic matrix composite with a laser (e.g., laser output of 50 W) to physically generate cracks thereon, and there is a concern that the cracks may remain even after the step of removing the deteriorated layer having the cracks. Therefore, it is desirable to perform a step of removing the deteriorated layer so that such cracks do not remain, and there is still a problem in terms of machinability.
[0008] Meanwhile, the present inventors have discovered and reported that, aiming to improve the difficulty of post-processing of, for example, SiC / SiC composite materials, monolithic SiC, which is a single SiC ceramic, can be irradiated with a laser at a lower output than in the method of Patent Document 1, and the surface irradiated with the laser can be chemically altered (see Non-Patent Documents 1 and 2). However, although the reported method makes it possible to obtain an altered layer sufficient for finish processing, it is desired to further expand the area that can be altered, for example, for rough processing.
[0009] The object of the present disclosure is to provide a new method and apparatus that allows improving the workability of the surface of ceramic-based materials. [Means for solving the problem]
[0010] A first aspect of the present disclosure is a method for manufacturing a semiconductor device comprising: A method for forming a deteriorated layer on a ceramic material, comprising the steps of: Heating the surface of the ceramic material to a predetermined temperature of 500° C. or less; irradiating the surface of the heated ceramic material with a laser having a predetermined output of 10 W or less; Including, method to provide.
[0011] According to the above-mentioned configuration of the first aspect, an altered layer can be formed on the surface of the ceramic material by a step of heating the surface of the ceramic material to a predetermined temperature of 500° C. or less and a step of irradiating the heated surface of the ceramic material with a laser having a predetermined output of 10 W or less. The altered layer thus formed may have a lower hardness than the previous surface. And, such a reduction in hardness extends to a deeper region of the ceramic material compared to the case of only irradiating the laser as reported in Non-Patent Document 1 or Non-Patent Document 2. Therefore, according to the above-mentioned configuration of the first aspect, the workability of the ceramic material can be improved.
[0012] A second aspect of the present disclosure is A method for processing a ceramic material, comprising the steps of: Heating the surface of the ceramic material to a predetermined temperature of 500° C. or less; irradiating the surface of the heated ceramic material with a laser having a predetermined output of 10 W or less; a step of removing the altered layer on the surface formed by the laser irradiation; Including, method to provide.
[0013] According to the above configuration of the second aspect, first, an altered layer can be formed on the surface of the ceramic material by a step of heating the surface of the ceramic material to a predetermined temperature of 500° C. or less and a step of irradiating the heated surface of the ceramic material with a laser of a predetermined output of 10 W or less. The altered layer thus formed can have a lower hardness than the previous surface. And, as reported in Non-Patent Document 1 or Non-Patent Document 2, such a decrease in hardness extends to a deeper region of the ceramic material compared to the case where only laser irradiation is performed. Therefore, the processability of the ceramic material in the above step of processing to remove the altered layer can be improved.
[0014] A third aspect of the present disclosure is An apparatus for forming a deteriorated layer on a ceramic material, comprising: A heating unit that heats the surface of the ceramic material to a predetermined temperature of 500° C. or less; a laser irradiation unit that irradiates a laser having a predetermined output of 10 W or less onto the surface of the ceramic material heated by the heating unit; Equipped with Deteriorated layer forming device to provide.
[0015] According to the above-mentioned configuration of the third aspect, the heating unit heats the surface of the ceramic material to a predetermined temperature of 500°C or less, and the laser irradiation unit irradiates the heated surface of the ceramic material with a laser of a predetermined output of 10 W or less, thereby forming an altered layer on the surface of the ceramic material. The altered layer thus formed may have a lower hardness than the previous surface. And, such a decrease in hardness extends to a deeper region of the ceramic material compared to the case of only laser irradiation as reported in Non-Patent Document 1 or Non-Patent Document 2. Therefore, according to the above-mentioned configuration of the third aspect, the workability of the ceramic material can be improved.
[0016] A fourth aspect of the present disclosure is A processing device for ceramic materials, comprising: The aforementioned deteriorated layer forming device; a machining device for removing the deteriorated layer formed on the surface by the irradiation of the laser by the deteriorated layer forming device; Equipped with processing equipment to provide.
[0017] According to the above-mentioned configuration of the fourth aspect, an altered layer can be formed on the surface of a ceramic-based material by the altered layer forming device. The altered layer thus formed can have a lower hardness than the previous surface. Such a reduction in hardness extends to a deeper region of the ceramic-based material compared to the case where only laser irradiation is used, as reported in Non-Patent Document 1 or Non-Patent Document 2. Therefore, the processability of the ceramic-based material can be improved in the process of removing the altered layer by the above-mentioned mechanical processing device.
[0018] In each of the first to fourth aspects, the ceramic material may be a ceramic-based composite material or a monolithic ceramic material. For example, the ceramic material may be a SiC material. The SiC material may include a SiC fiber-reinforced SiC composite material and a SiC ceramic material. When the ceramic material is a SiC material, the predetermined temperature may be 100° C. or higher, and the predetermined output may be 2 W or higher and 7.5 W or lower. More preferably, when the ceramic material is a SiC material, the predetermined temperature may be 100° C. or higher and 300° C. or lower, the predetermined output may be 2.5 W or higher and 5 W or lower, and the laser may be an infrared pulse laser with a wavelength of 1064 nm, a frequency of 10 kHz, and a scanning speed of 100 mm / s. The step of irradiating the laser may be performed in an oxygen-containing atmosphere. In other words, the laser irradiation unit is preferably provided so as to irradiate the surface of a ceramic material, for example, a SiC material, with a laser in an oxygen-containing atmosphere. Effect of the Invention
[0019] According to each of the first to fourth aspects of the present disclosure, since the above configuration is provided, it is possible to improve the workability of the surface of the ceramic material. [Brief description of the drawings]
[0020] [Figure 1] 1 is a schematic configuration diagram of a processing device according to an embodiment; [Diagram 2] FIG. 2 is a schematic diagram of a portion of the processing apparatus of FIG. [Diagram 3] 2 is a flowchart of a process in the processing device of FIG. 1. [Figure 4] FIG. 1 is a schematic diagram for explaining a test method. [Diagram 5] 13 is a graph showing experimental results. [Figure 6] 13 is a graph showing experimental results. [Figure 7]13 is a graph showing experimental results. [Figure 8] 13 is a graph showing experimental results. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. The same components (or configurations) are denoted by the same reference characters, and have the same names and functions. Therefore, detailed description thereof will not be repeated.
[0022] A processing apparatus 10 according to one embodiment will be described with reference to Fig. 1 and Fig. 2. Fig. 1 shows a schematic configuration diagram of the processing apparatus 10, and Fig. 2 shows a schematic diagram of a part of the processing apparatus 10.
[0023] The processing device 10 is used for processing ceramic materials and is a processing device for ceramic materials. The processing device 10 includes a deteriorated layer forming device 12 and a mechanical processing device 14. The deteriorated layer forming device 12 may be configured as a standalone deteriorated layer forming device independent of the mechanical processing device 14.
[0024] The deteriorated layer forming device 12 is configured to form an deteriorated layer on the workpiece W, which is a ceramic material. The deteriorated layer forming device 12 includes a heating device 16 and a laser irradiation device 18. The heating device 16 is an example of a heating section. The laser irradiation device 18 is an example of a laser irradiation section. The heating device 16 and the laser irradiation device 18 are arranged in sequence from the upstream side in the transport direction D of the workpiece W.
[0025] The processing device 10 has a conveying device 20 which is a conveying means. The conveying device 20 conveys the workpiece W in a conveying direction D. In the conveying direction D, a deteriorated layer forming device 12 and a mechanical processing device 14 are provided in this order from the upstream side, and more specifically, in the conveying direction D, a heating device 16, a laser irradiation device 18, and the mechanical processing device 14 are provided in this order from the upstream side.
[0026] The conveying device 20 includes a moving table 24 that moves in the conveying direction D by the driving force of a motor 22. Here, the table 24 is arranged so as to extend in the horizontal direction, but is not limited thereto. The workpiece W is fixed to the table 24 using a jig 26. Therefore, when the table 24 moves, the workpiece W fixed thereto also moves together. When the degraded layer forming device 12 is configured as a single degraded layer forming device independent of the machining device 14, the conveying device 20 can be provided in the degraded layer forming device 12 so as to convey the workpiece W from the heating device 16 side to the laser irradiation device 18 side in the conveying direction D. Either or both of the conveying of the workpiece W from the heating device 16 to the laser irradiation device 18 in the degraded layer forming device 12 and the conveying of the workpiece W from the laser irradiation device 18 to the machining device 14 in the degraded layer forming device 12 may be performed by manual operation of an operator, for example, without being performed by such a conveying device 20.
[0027] Now, the workpiece W is a ceramic material. The ceramic material may include a ceramic-based composite material or a monolithic ceramic material. For example, the ceramic material is a SiC material. The SiC material includes a SiC fiber-reinforced SiC composite material and a SiC ceramic material. The SiC ceramic material is, for example, polytype SiC. Specifically, as an example of a SiC material, monolithic SiC, for example, monolithic SiC itself having a crystal structure corresponding to 6H-SiC, or a SiC fiber-reinforced SiC composite material having monolithic SiC as a matrix can be processed as the workpiece W by the processing device 10, and is subjected to processing by, for example, the altered layer forming device 12. The ceramic material may also include a carbon fiber-reinforced carbon composite material, so-called C / C composite.
[0028] Various processes in the processing device 10, for example, each process in the above-mentioned deteriorated layer forming device 12, which will be described later, are performed in the atmosphere. That is, each process in the deteriorated layer forming device 12 and the mechanical processing device 14 is performed in an oxygen-containing atmosphere, including the atmosphere. In particular, the laser irradiation in the laser irradiation device 18 of the deteriorated layer forming device 12 is preferably performed in an oxygen-containing atmosphere, including the atmosphere. The oxygen-containing atmosphere preferably has an oxygen concentration (about 20 to 21%) similar to that of the atmosphere, but the oxygen concentration is not limited thereto. It is more preferable that the oxygen concentration is a concentration suitable for introducing oxygen into the workpiece W, which will be described later. Thereby, for example, when a SiC-based material is processed in the deteriorated layer forming device 12, oxygen is introduced into the laser irradiated area of the SiC-based material to increase the oxygen concentration. For example, it is known that the Knoop hardness of silicon carbide (SiC) is 2500, and that of quartz (SiO2) is 820. In general, the hardness of silicon oxide (SiO2) is lower than that of silicon carbide (SiC). In the technology disclosed herein, the oxygen concentration of the surface of a SiC-based material is increased by a combination of heating and laser irradiation, thereby lowering the hardness of the surface of the SiC-based material and improving its processability. In order to suitably expand the area of reduced hardness of the surface, the altered layer forming device 12 has a configuration that combines heating and laser irradiation, which has not been conventionally used. The processing device 10, the altered layer forming device 12, etc. will be described in more detail below.
[0029] The heating device 16 of the altered layer forming device 12 has a configuration for heating the workpiece W, for example, the surface WS of the workpiece W. Heating in the heating device 16 is performed so as to heat the workpiece W to a predetermined temperature of 500° C. or less. Here, the heating device 16 is equipped with an infrared heater, and the heating of the infrared heater is controlled so as to heat the workpiece W to a predetermined temperature of 500° C. or less. However, the heating device 16 is not limited to being equipped with an infrared heater, and may be configured to be equipped with, for example, a heating plate (hot plate) that directly contacts and heats the workpiece W. The workpiece W can be more accurately heated to a predetermined temperature by bringing a heating plate of a predetermined temperature, that is, a heated heating plate, into contact with the workpiece W for a predetermined time or more, for example by pressing it against the workpiece W. The heating of the heating plate may be an electric heating type for temperature control, but is not limited to this. For example, high-frequency heating may be used to heat the workpiece W. The heating in the heating device 16 is performed prior to the laser irradiation in the laser irradiation device 18 and may be referred to as preliminary heating (preheating), in which case the heating device 16 may be referred to as a preliminary heating device. The heating temperature of the workpiece W by the heating device 16, that is, the temperature of the heated workpiece W, for example the surface temperature, may be 500° C. or lower, preferably 100° C. or higher, and more preferably 100° C. or higher and 300° C. or lower. This temperature is not limited to this range and may be determined based on experiments depending on the workpiece W.
[0030] The laser irradiation device 18 of the deteriorated layer forming device 12 is configured to irradiate a laser of a predetermined output onto the workpiece W, for example, the surface WS of the workpiece W, particularly onto the surface WS heated to a predetermined temperature by the heating device 16. The predetermined output may be 20 W or less, and is 10 W or less here. In this embodiment, the laser irradiation device 18 is configured to generate an infrared laser in a wavelength band in the infrared region (780 nm to 16 μm). For example, the laser irradiation device 18 has an infrared laser source. The laser irradiation device 18 may also adjust the frequency of the laser, that is, the pulse width, and may irradiate a pulsed laser. The irradiation of this pulsed laser is not limited to the laser irradiated to the workpiece W being a pulsed laser, but may be adopted to suppress the thermal effect on the workpiece W to a lower level than when a continuous laser is irradiated. For example, the wavelength of the laser in the laser irradiation device 18 may be 1064 nm. The laser output may be, for example, in the range of 1 W to 10 W, preferably 2 W to 10 W, more preferably 2 W to 7.5 W, and even more preferably 2.5 W to 5 W. The laser frequency may be, for example, from 1 kHz to 100 kHz, specifically 10 kHz to 75 kHz, for example 10 kHz. However, the laser output and frequency may each be determined based on an experiment according to the workpiece W. The laser irradiation device 18 may also have a function of adjusting the laser scanning time.
[0031] The machining device 14 is configured to machine the workpiece W on which the deteriorated layer has been formed in a region including the surface WS by the deteriorated layer forming device 12. The machining device 14 includes a rotating tool 28 that rotates around a rotation axis 28A. The rotating tool 28 is configured so that the rotation axis 28A extends substantially parallel to the horizontal plane, substantially perpendicular to the conveying direction D. The cutter that is the rotating tool 28 here is a side milling cutter whose rotation axis 28A extends substantially parallel to the horizontal plane, substantially perpendicular to the conveying direction D, and has a cutting edge formed in its circumferential direction. However, the rotating tool 28 is not limited to such a tool. The rotating tool 28 may be a tool whose rotation axis 28A extends substantially perpendicular to the conveying direction D and substantially perpendicular to the horizontal plane, for example, a face milling cutter, an end mill, or the like. The machining device 14 may include a rotating tool 28 suitable for any one of surface polishing, surface grinding, and cutting. For example, the rotating tool 28 may be a grinder. The tool used in the machining device 14 is not limited to the rotary tool 28, and various tools such as lathe tools can be used.
[0032] The processing method in the processing device 10 having the above configuration will be described with reference to the flow chart of FIG.
[0033] In the processing device 10, the workpiece W is transported in the transport direction D by the transport device 20. In the deteriorated layer forming device 12 located upstream of the mechanical processing device 14 in the transport direction D, a deteriorated layer forming process step (step S301 in FIG. 3) is first performed. In the deteriorated layer forming process step (step S301), a deteriorated layer forming method is executed, and specifically, a step of heating the workpiece W (step S303 in FIG. 3) and a subsequent step of irradiating the heated workpiece W with a laser (step S305 in FIG. 3) are performed. The irradiated area, i.e., the irradiated portion, of the surface WS of the workpiece W irradiated with the laser preferably includes the surface heated by the heating device 16.
[0034] That is, in the process of forming the altered layer AL, first, a process of heating the workpiece W by the heating device 16 (step S303 in FIG. 3) is performed. As a result, at least the surface WS of the workpiece W is heated to a predetermined temperature of 500° C. or less. In FIG. 2, heat H supplied from the heating device 16 to the workpiece W is shown in schematic form.
[0035] Then, the workpiece W heated by the heating device 16 is further sent in the conveying direction D by the conveying device 20 and reaches the laser irradiation device 18. In the laser irradiation device 18, a step (step S305 in FIG. 3) of irradiating the workpiece W with a laser LB at a predetermined scanning speed using a laser light of a predetermined output and a predetermined frequency is performed. As a result, in the deteriorated layer forming device 12, an deteriorated layer AL can be formed on the surface of the workpiece W as described later. The workpiece W to be irradiated with the laser, particularly the irradiation area of the surface, is preferably maintained at a predetermined temperature. In other words, the heated workpiece W is preferably irradiated with the laser on the surface area, i.e., the irradiation area, in a state where the surface area to be irradiated with the laser is maintained at a substantially predetermined temperature, particularly in a state where the surface area to be irradiated with the laser has a substantially predetermined temperature. The heating of the workpiece W by the heating device 16 is performed so as to heat the surface WS, which can be the irradiation area of the workpiece W, to a predetermined temperature, but this predetermined temperature may have a certain temperature range. For example, the predetermined temperature may have an allowable temperature range of, for example, ±20° C. around the predetermined temperature.
[0036] Furthermore, the workpiece W on which the deteriorated layer AL has been formed is sent in the conveying direction D by the conveying device 20, and reaches the machining device 14. Then, in the machining device 14, a process is performed to remove the deteriorated layer AL on the surface formed by the laser irradiation (step S307 in FIG. 3). More specifically, in this process, the workpiece W is machined to remove the deteriorated layer AL.
[0037] The results of an experiment on the formation of a deteriorated layer in the deteriorated layer forming apparatus 12 are shown below.
[0038] (Experimental Example 1) A monolithic SiC test piece having a crystal structure equivalent to 6H-SiC was used as the workpiece W. The workpiece W was placed on a hot plate, which is an example of the heating device 16, and the area including the surface WS of the workpiece W was heated to a predetermined temperature. The predetermined temperature was changed to room temperature (23°C in this case), 50°C, 100°C, 200°C, and 300°C. When the predetermined temperature was set to room temperature, heating was not performed with the heating device 16. The surface WS of the workpiece W in the heated state was used as the irradiation area, and the irradiation area was irradiated with a laser using a "laser marker" (MD-X1520, Keyence Corporation) as the laser irradiation device 18. The frequency and scanning speed of the infrared pulse laser with a wavelength of 1064 nm were fixed to 10 kHz and 100 mm / s, respectively, and only the predetermined output was changed to irradiate the test piece, the workpiece W, with the laser. The spot size of the laser was set to 80 μm. The specified output was changed to 1.0 W, 2.5 W, and 5.0 W. For comparison, a test piece was also prepared by irradiating the surface of an unheated workpiece W with a laser under the same conditions.
[0039] As the material properties of the test piece, which is the workpiece W thus prepared, the indentation hardness of the surface WS irradiated with the laser was obtained and the indentation depth was measured using a nanoindentation system TS77 (Bruker). The indenter was a Berkovich type, and the maximum indentation load was 5000 μN. As shown in FIG. 4, the indenter IN was pressed into the surface WS of the workpiece W, which is the test piece, with the indentation load, and the hardness calculated from the load-displacement curve during the process of pulling out the indenter IN was taken as the indentation hardness of the workpiece W, and the depth TD reached by the tip of the indenter IN at the maximum indentation load was measured as the indentation depth. The calculated indentation hardness (unit: MPa) and the contact depth (unit: nm) obtained by subtracting the elastic deformation from the measured indentation depth are shown in FIG. 5 and FIG. 6, respectively. The contact depth was obtained by calculating based on the measured indentation depth using a known arithmetic formula. In FIG. 5, the horizontal axis represents the heating temperature in the heating device 16, the vertical axis represents the indentation hardness, and the indentation hardness is plotted against the heating temperature. In FIG. 6, the horizontal axis represents the heating temperature, the vertical axis represents the contact depth, and the contact depth is plotted against the heating temperature.
[0040] As shown in FIG. 5, when the laser output was 1 W, no substantial change in the indentation hardness was observed at any heating temperature. In contrast, when the laser output was 2.5 W, the indentation hardness did not change at room temperature and 50° C., but as the heating temperature was changed to 100° C., 200° C., and 300° C., the indentation hardness decreased with increasing heating temperature. Similarly, when the laser output was 5.0 W, the indentation hardness did not change at room temperature and 50° C., but as the heating temperature was changed to 100° C., 200° C., and 300° C., the indentation hardness decreased with increasing heating temperature. More specifically, when the laser output was 2.5 W and the heating temperature was room temperature, 50° C., 100° C., 200° C., and 300° C., the indentation hardness was 30.10 MPa, 30.07 MPa, 24.10 MPa, 13.19 MPa, and 7.29 MPa. Similarly, when the laser output was 5.0 W and the heating temperatures were room temperature, 50°C, 100°C, 200°C, and 300°C, the indentation hardness was 17.59 MPa, 19.56 MPa, 16.14 MPa, 7.95 MPa, and 7.93 MPa.
[0041] As shown in FIG. 6, when the laser output was 1 W, no substantial change in contact depth was observed at any heating temperature. In contrast, when the laser output was 2.5 W, the contact depth did not change at room temperature and 50° C., but increased with increasing heating temperature as the heating temperature was changed to 100° C., 200° C., and 300° C. Similarly, when the laser output was 5.0 W, the contact depth did not change at room temperature and 50° C., but increased with increasing heating temperature as the heating temperature was changed to 100° C., 200° C., and 300° C. More specifically, when the laser output was 2.5 W and the heating temperature was room temperature, 50° C., 100° C., 200° C., and 300° C., the contact depths were 2694.2 nm, 2662.7 nm, 2964.0 nm, 3991.1 nm, and 5328.6 nm. Similarly, when the laser output was 5.0 W and the heating temperatures were room temperature, 50°C, 100°C, 200°C, and 300°C, the contact depths were 3436.4 nm, 3282.3 nm, 3641.5 nm, 5117.8 nm, and 5134.0 nm.
[0042] When neither heating nor laser irradiation was performed, the indentation hardness of the test piece of the same material was 36,403 MPa and the contact depth was 63.6 nm. A test piece of the same material that was only heated at 300°C and not irradiated with a laser also had almost the same indentation hardness and contact depth.
[0043] In this way, when a monolithic SiC test piece was used as the workpiece W, a significant decrease in mechanical properties, especially hardness, and an increase in contact depth were observed by heating the workpiece W at a temperature of 100°C to 300°C and then irradiating it with an infrared pulse laser having an output of 2.5 W to 5 W, a frequency of 10 kHz, a scanning speed of 100 mm / s, and a wavelength of 1064 nm. In other words, by processing under these conditions, the hardness of the workpiece W, which is a type of SiC-based material, was significantly decreased, and the decrease in hardness extended to a deeper region compared to the cases of only heating or only laser irradiation.
[0044] Here, elemental analysis was performed on the surface WS of the workpiece W evaluated as above, which was the laser irradiated region. The elemental analysis was performed by energy dispersive X-ray analysis (EDX) using a tabletop SEM (TM4000Plus, Hitachi High-Technologies Corporation) with an acceleration voltage of 5 kV. The results are shown in Table 1. However, the values shown in Figure 1 may deviate very slightly from 100 at% in total due to the measurement system. In Table 1, the workpiece W with both the laser output and heating temperature of "none" refers to a test piece that was neither heated nor subsequently irradiated with a laser.
[0045] [Table 1]
[0046] From the results shown in Table 1, it can be seen that the oxygen concentration was increased in the workpiece W in which the hardness was significantly decreased, that is, in the workpiece W irradiated with an infrared pulse laser at an output of 2.5 W or 5 W. The elemental analysis result of the workpiece W in which the laser output and heating temperature were both "none" corresponds to that of SiC itself, but the elemental analysis result of the workpiece W in which the hardness was particularly decreased after "heating at 300 degrees and then irradiating with a laser at 5.0 W" was 31.19:5.58:63.23 (at%) in terms of Si:C:O, and the elements of the surface WS were significantly changed, an altered layer AL was formed, oxygen was introduced, and the ratio was roughly equivalent to the atomic concentration ratio of SiO2. Thus, the formation of the altered layer into which oxygen was introduced in the workpiece W corresponds to the decrease in the indentation hardness and the increase in the contact depth. This relationship is shown diagrammatically in FIG. 4.
[0047] In this way, by heating the workpiece W to a predetermined temperature and then irradiating it with a laser, an altered layer AL is formed on the surface of the workpiece W, and not only can the indentation hardness be reduced, but the contact depth can also be increased. Presumably, the altered layer formed in this way is thicker and extends to a deeper area than an altered layer formed by laser irradiation alone. The formation of this altered layer, the reduction in indentation hardness, and the increase in contact depth can contribute to improving the workability of the workpiece.
[0048] (Experimental Example 2) As in Experimental Example 1, a monolithic SiC test piece having a crystal structure equivalent to 6H-SiC was used as the workpiece W. The workpiece W was placed on a hot plate, which is a heating device 16, and the surface WS of the workpiece W was heated to a predetermined temperature. The predetermined temperature was changed to room temperature (23°C in this case) and 200°C. When the predetermined temperature was set to room temperature, heating was not performed with the heating device 16. The surface WS of the workpiece W in the heated state was used as the irradiation area, and the irradiation area was irradiated with a laser using the same "laser marker" (MD-X1520, Keyence Corporation). The frequency and scanning speed of the infrared pulse laser with a wavelength of 1064 nm were fixed at 10 kHz and 100 mm / s, respectively, and only the predetermined output was changed to irradiate the workpiece W with the laser. The predetermined output was changed to 1.0 W, 1.5 W, 2.0 W, 2.5 W, 5.0 W, and 7.5 W. As material properties of the workpiece W thus obtained, the indentation hardness was determined and the indentation depth was measured under the same conditions as in Experimental Example 1 above, and the indentation hardness and the contact depth calculated based on the indentation depth are shown in Figures 7 and 8. However, in Figure 7, the horizontal axis is the laser output and the vertical axis is the indentation hardness, and the indentation hardness is plotted against the laser output at each heating temperature, while in Figure 8, the horizontal axis is the laser output and the vertical axis is the contact depth, and the contact depth is plotted against the laser output at each heating temperature.
[0049] As is clear from Figures 7 and 8, when the heating temperature was 200°C, by setting the laser output to 2 W or more, particularly 2.5 W or more, the hardness was significantly reduced and the contact depth was increased compared to when only the laser was irradiated.
[0050] Although the embodiment and its modified examples according to the present invention have been described above, the present invention is not limited thereto. Various substitutions and modifications are possible without departing from the spirit and scope of the present invention as defined by the claims of this application. [Explanation of symbols]
[0051] 10 Processing equipment 12. Deterioration layer forming device 14 Machining equipment 16 Heating device (heating section) 18 Laser irradiation device (laser irradiation section) 20. Conveyor
Claims
1. A method for forming a deteriorated layer on a ceramic material, comprising the steps of: Heating the surface of the ceramic material to a predetermined temperature of 500° C. or less; irradiating the surface of the heated ceramic material with a laser having a predetermined output of 10 W or less; Including, method.
2. The ceramic material is a ceramic matrix composite material or a monolithic ceramic material; The method of claim 1.
3. The ceramic-based material is a SiC-based material including a SiC fiber-reinforced SiC composite material and a SiC ceramic material; The method of claim 1.
4. the ceramic material is a SiC material, The predetermined temperature is a temperature of 100° C. or higher, The predetermined output is an output of 2 W or more and 7.5 W or less. The method of claim 1.
5. The predetermined temperature is a temperature of 100° C. or more and 300° C. or less, The predetermined output is an output of 2.5 W or more and 5 W or less, The laser is an infrared pulse laser having a wavelength of 1064 nm, a frequency of 10 kHz, and a scanning speed of 100 mm / s. The method according to claim 4.
6. The step of irradiating the laser is carried out in an oxygen-containing atmosphere.
6. The method according to any one of claims 1 to 5.
7. A method for processing a ceramic material, comprising the steps of: Heating the surface of the ceramic material to a predetermined temperature of 500° C. or less; irradiating the surface of the heated ceramic material with a laser having a predetermined output of 10 W or less; a step of removing the altered layer on the surface formed by the laser irradiation; Including, method.
8. An apparatus for forming a deteriorated layer on a ceramic material, comprising: A heating unit that heats the surface of the ceramic material to a predetermined temperature of 500° C. or less; a laser irradiation unit that irradiates a laser having a predetermined output of 10 W or less onto the surface of the ceramic material heated by the heating unit; Equipped with Degenerated layer forming device.
9. The ceramic material is a ceramic matrix composite material or a monolithic ceramic material; The altered layer forming apparatus according to claim 8 .
10. The ceramic-based material is a SiC-based material including a SiC fiber-reinforced SiC composite material and a SiC ceramic material; The altered layer forming apparatus according to claim 8 .
11. the ceramic material is a SiC material, The predetermined temperature is a temperature of 100° C. or higher, The predetermined output is an output of 2 W or more and 7.5 W or less. The altered layer forming apparatus according to claim 8 .
12. The predetermined temperature is a temperature of 100° C. or more and 300° C. or less, The predetermined output is an output of 2.5 W or more and 5 W or less, The laser is an infrared pulse laser having a wavelength of 1064 nm, a frequency of 10 kHz, and a scanning speed of 100 mm / s. The altered layer forming apparatus according to claim 11 .
13. The laser irradiation unit is configured to irradiate the surface with a laser in an oxygen-containing atmosphere. The altered layer forming apparatus according to claim 8 .
14. A processing device for ceramic materials, comprising: The deteriorated layer forming apparatus according to any one of claims 8 to 13, a machining device for removing the deteriorated layer formed on the surface by the irradiation of the laser by the deteriorated layer forming device; Equipped with Processing equipment.
Citation Information
Patent Citations
Laser working device
JP1984035890A
Composite machining method and composite machining apparatus
JP2014117767A
Method of processing ceramic matrix composite material
JP2014172127A