Reflective mask blank, reflective mask, method for producing reflective mask blank, and method for producing reflective mask

A Ru compound-based phase shift film with controlled Cr oxidation and O content addresses the etching rate and optical property issues in EUV lithography masks, improving processability and optical performance.

JP2024135499AActive Publication Date: 2024-10-04AGC INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023046214
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

The addition of chromium (Cr) to ruthenium (Ru) in phase shift films for EUV lithography reduces the etching rate, leading to decreased processability of the phase shift film, while ruthenium alone decreases the extinction coefficient, affecting the optical properties and thickness of the film.

Method used

A phase shift film composed of a Ru compound containing Cr, O, and optionally N, with a controlled Cr oxidation degree to Ru oxidation degree ratio between 0 and 7.5, and an O content of 0 to 50 at%, enhances the optical properties and processability by adjusting the extinction coefficient and etching rate.

Benefits of technology

The solution provides a phase shift film with improved optical properties and processability, maintaining a high extinction coefficient and reducing film thickness while ensuring phase difference, thus enhancing the performance of EUV lithography masks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135499000001_ABST
    Figure 2024135499000001_ABST
Patent Text Reader

Abstract

To provide a phase shift film with superior optical properties and superior processability.SOLUTION: A reflective mask blank includes a substrate, a multilayer reflection film that reflects EUV light, a protective film that protects the multilayer reflection film, and a phase shift film that shifts the phase of the EUV light, in the stated order. The phase shift film has a layer composed of a Ru compound that contains at least Ru, Cr and O. For the Ru compound, the ratio of the Cr oxidation level to the Ru oxidation level (Cr oxidation level / Ru oxidation level), as determined from X-ray photoelectron spectroscopy, is more than 0 and less than 7.5, and the O content is more than 0 at% and less than 50 at%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a reflective mask blank, a reflective mask, a method for manufacturing a reflective mask blank, and a method for manufacturing a reflective mask. [Background technology]

[0002] In recent years, with the miniaturization of semiconductor devices, EUV lithography (EUVL), an exposure technology using extreme ultraviolet (EUV) light, has been developed. EUV includes soft X-rays and vacuum ultraviolet light, and specifically refers to light with a wavelength of about 0.2 nm to 100 nm. At present, EUV with a wavelength of about 13.5 nm is mainly being considered.

[0003] In EUVL, a reflective mask is used. The reflective mask has, in this order, a substrate such as a glass substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light. An opening pattern is formed in the phase shift film. In EUVL, the opening pattern in the phase shift film is transferred to a target substrate such as a semiconductor substrate. Transferring includes reducing and transferring.

[0004] The phase shift film of Example 1 of Patent Document 1 has a RuCrN film as a lower layer and a RuCrO film as an upper layer. The RuCrN film has an element ratio (Ru:Cr:N) of 79.4:13.6:7.0, a refractive index n of 0.900, and an extinction coefficient k of 0.023. The RuCrO film has an element ratio (Ru:Cr:O) of 18.1:29.5:52.4, a refractive index n of 0.931, and an extinction coefficient k of 0.027.

[0005] The phase shift film of Example 1 of Patent Document 2 has a RuCrNO film as a lower layer and a RuCrO film as an upper layer. The RuCrNO film has an unknown element ratio, but has a refractive index n of 0.894 and an extinction coefficient k of 0.019. The RuCrO film has an element ratio (Ru:Cr:O) of 18.1:29.5:52.4, a refractive index n of 0.931, and an extinction coefficient k of 0.027. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 6929340 [Patent Document 2] Patent No. 6929983 Summary of the Invention [Problem to be solved by the invention]

[0007] Ru has been considered as a material for phase shift films. Ru can reduce the refractive index of the phase shift film, and the film can be made thinner while maintaining the phase difference. However, Ru reduces the extinction coefficient of the phase shift film.

[0008] Therefore, it is considered to add Cr to Ru. By adding Cr, the extinction coefficient of the phase shift film can be increased. However, adding Cr decreases the etching rate of the phase shift film. As a result, the ratio (selectivity) of the etching rate of the phase shift film to the etching rate of the protective film decreases, and the processability of the phase shift film decreases.

[0009] One aspect of the present disclosure provides a phase shift film having excellent optical properties and processability. [Means for solving the problem]

[0010] A reflective mask blank according to one embodiment of the present disclosure includes, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light. The phase shift film includes a layer formed of a Ru compound containing at least Ru, Cr, and O. The Ru compound has a ratio of the Cr oxidation degree to the Ru oxidation degree (Cr oxidation degree / Ru oxidation degree) determined from an X-ray photoelectron spectroscopy spectrum that is greater than 0 and less than 7.5, and an O content that is greater than 0 at% and less than 50 at%. Effect of the Invention

[0011] According to one embodiment of the present disclosure, by adjusting the ratio of the Cr oxidation degree to the Ru oxidation degree in the Ru compound (Cr oxidation degree / Ru oxidation degree) to greater than 0 and less than 7.5, and by adjusting the O content in the Ru compound to greater than 0 at% and less than 50 at%, a phase shift film with excellent optical properties and processability can be provided. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a cross-sectional view showing a reflective mask blank according to one embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a reflective mask according to an embodiment. [Diagram 3] FIG. 3 is a cross-sectional view showing an example of EUV light reflected by the reflective mask of FIG. [Figure 4] FIG. 4 is a flowchart showing a method for manufacturing a reflective mask blank according to one embodiment. [Diagram 5] FIG. 5 is a flowchart showing a method for manufacturing a reflective mask according to an embodiment. [Figure 6] FIG. 6 is a diagram showing an example of the refractive index and extinction coefficient of each element. [Figure 7] FIG. 7 is a diagram showing an example of changes in the refractive index and extinction coefficient due to oxidation of Ru and Cr. [Figure 8] FIG. 8 is a diagram showing an example of an XPS spectrum of a Ru compound. [Figure 9]FIG. 9 is a diagram illustrating an example of the reference value and the rate of increase of the extinction coefficient. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In each drawing, the same or corresponding components are denoted by the same reference numerals, and the description may be omitted. In the specification, the symbol "~" indicating a range of values ​​means that the values ​​before and after the symbol are included as the lower and upper limits.

[0014] 1 to 3, the X-axis direction, the Y-axis direction, and the Z-axis direction are perpendicular to each other. The Z-axis direction is perpendicular to the first main surface 10a of the substrate 10. The X-axis direction is perpendicular to the incidence surface of the EUV light (the surface including the incident light beam and the reflected light beam). As shown in FIG. 3, the incident light beam is inclined toward the positive Y-axis direction as it moves toward the negative Z-axis direction, and the reflected light beam is inclined toward the positive Y-axis direction as it moves toward the positive Z-axis direction.

[0015] A reflective mask blank 1 according to one embodiment will be described with reference to Fig. 1. The reflective mask blank 1 has, for example, a substrate 10, a multilayer reflective film 11, a protective film 12, a phase shift film 13, and an etching mask film 14, in this order. The multilayer reflective film 11, the protective film 12, the phase shift film 13, and the etching mask film 14 are formed, in this order, on a first main surface 10a of the substrate 10. It should be noted that the reflective mask blank 1 only needs to have at least the substrate 10, the multilayer reflective film 11, the protective film 12, and the phase shift film 13.

[0016] The reflective mask blank 1 may further have a functional film not shown in FIG. 1. For example, the reflective mask blank 1 may have a conductive film on the opposite side of the multilayer reflective film 11 with respect to the substrate 10. The conductive film is formed on the second main surface 10b of the substrate 10. The second main surface 10b is the surface facing opposite to the first main surface 10a. The conductive film is used, for example, to attach the reflective mask 2 to an electrostatic chuck of an exposure tool. The reflective mask blank 1 may have a diffusion barrier film (not shown) between the multilayer reflective film 11 and the protective film 12. The diffusion barrier film suppresses diffusion of metal elements contained in the protective film 12 into the multilayer reflective film 11.

[0017] Although not shown, the reflective mask blank 1 may have a buffer film between the protective film 12 and the phase shift film 13. The buffer film protects the protective film 12 from an etching gas that forms an opening pattern 13a in the phase shift film 13. The buffer film is etched more slowly than the phase shift film 13. Unlike the protective film 12, the buffer film will ultimately have the same opening pattern as the opening pattern 13a of the phase shift film 13.

[0018] Next, a reflective mask 2 according to one embodiment will be described with reference to Figures 2 and 3. The reflective mask 2 is produced, for example, by using the reflective mask blank 1 shown in Figure 1, and includes an opening pattern 13a in a phase shift film 13. Note that the etching mask film 14 shown in Figure 1 is removed after the opening pattern 13a is formed in the phase shift film 13.

[0019] In EUVL, the opening pattern 13a of the phase shift film 13 is transferred to a target substrate such as a semiconductor substrate. The transfer includes reducing and transferring. The substrate 10, the multilayer reflective film 11, the protective film 12, the phase shift film 13, and the etching mask film 14 will be described below in this order.

[0020] The substrate 10 is, for example, a glass substrate. The material of the substrate 10 is preferably quartz glass containing TiO2. Quartz glass has a smaller linear expansion coefficient and a smaller dimensional change due to temperature change than general soda-lime glass. Quartz glass may contain 80% to 95% by mass of SiO2 and 4% to 17% by mass of TiO2. When the TiO2 content is 4% to 17% by mass, the linear expansion coefficient is approximately zero near room temperature, and there is almost no dimensional change near room temperature. Quartz glass may contain a third component or impurity other than SiO2 and TiO2. The material of the substrate 10 may be crystallized glass in which a β-quartz solid solution is precipitated, silicon, metal, or the like.

[0021] The substrate 10 has a first main surface 10a and a second main surface 10b facing opposite to the first main surface 10a. A multilayer reflective film 11 and the like are formed on the first main surface 10a. The size of the substrate 10 in plan view (viewed in the Z-axis direction) is, for example, 152 mm long and 152 mm wide. The vertical and horizontal dimensions may be 152 mm or more. The first main surface 10a and the second main surface 10b each have, for example, a square quality assurance area in the center. The size of the quality assurance area is, for example, 142 mm long and 142 mm wide. The quality assurance area of ​​the first main surface 10a preferably has a root-mean-square roughness (Rq) of 0.15 nm or less and a flatness of 100 nm or less. In addition, it is preferable that the quality assurance area of ​​the first main surface 10a does not have a defect that causes a phase defect.

[0022] The multilayer reflective film 11 reflects EUV light. The multilayer reflective film 11 is, for example, a laminate of high refractive index layers and low refractive index layers alternately. The high refractive index layers are made of, for example, silicon (Si), and the low refractive index layers are made of, for example, molybdenum (Mo), and a Mo / Si multilayer reflective film is used. Note that Ru / Si multilayer reflective film, Mo / Be multilayer reflective film, Mo compound / Si compound multilayer reflective film, Si / Mo / Ru multilayer reflective film, Si / Mo / Ru / Mo multilayer reflective film, Si / Ru / Mo / Ru multilayer reflective film, Si / Ru / Mo multilayer reflective film, and the like can also be used as the multilayer reflective film 11.

[0023] The film thickness of each layer constituting the multilayer reflective film 11 and the number of repeating units of the layer can be appropriately selected according to the material of each layer and the reflectivity with respect to EUV light. When the multilayer reflective film 11 is a Mo / Si multilayer reflective film, in order to achieve a reflectivity of 60% or more with respect to EUV light with an incident angle θ (see Fig. 3) of 6°, a Mo layer with a film thickness of 2.3 ± 0.1 nm and a Si layer with a film thickness of 4.5 ± 0.1 nm may be laminated so that the number of repeating units is 30 or more and 60 or less. The multilayer reflective film 11 preferably has a reflectivity of 60% or more with respect to EUV light with an incident angle θ of 6°. More preferably, the reflectivity is 65% or more.

[0024] The film formation method of each layer constituting the multilayer reflective film 11 is, for example, a DC sputtering method, a magnetron sputtering method, an ion beam sputtering method, or the like. When forming a Mo / Si multilayer reflective film using the ion beam sputtering method, an example of the film formation conditions for each of the Mo layer and the Si layer is as follows. <Film formation conditions for Si layer> Target: Si target, Sputtering gas: Ar gas, Gas pressure: 1.3×10 -2 Pa~2.7×10 -2 Pa, Ion acceleration voltage: 300V~1500V, Film formation rate: 0.030 nm / sec~0.300 nm / sec, Film thickness of Si layer: 4.5 ± 0.1 nm, <Film formation conditions for Mo layer> Target: Mo target, Sputtering gas: Ar gas, Gas pressure: 1.3×10 -2 Pa~2.7×10 -2 Pa, Ion acceleration voltage: 300V~1500V, Film formation rate: 0.030 nm / sec~0.300 nm / sec, Film thickness of Mo layer: 2.3 ± 0.1 nm, <Repeating unit of Si layer and Mo layer> Number of repeating units: 30~60 (preferably 40~50).

[0025] The protective film 12 is formed between the multilayer reflective film 11 and the phase shift film 13, and protects the multilayer reflective film 11. The protective film 12 protects the multilayer reflective film 11 from an etching gas that forms an opening pattern 13a (see FIG. 2) in the phase shift film 13. The protective film 12 is not removed even when exposed to the etching gas, but remains on the multilayer reflective film 11.

[0026] The etching gas is, for example, a halogen-based gas, an oxygen-based gas, or a mixed gas thereof. The halogen-based gas includes a chlorine-based gas and a fluorine-based gas. The chlorine-based gas is, for example, Cl2 gas, SiCl4 gas, CHCl3 gas, CCl4 gas, BCl3 gas, or a mixed gas thereof. The fluorine-based gas is, for example, CF4 gas, CHF3 gas, SF6 gas, BF3 gas, XeF2 gas, or a mixed gas thereof. The oxygen-based gas is, for example, O2 gas, O3 gas, or a mixed gas thereof.

[0027] The ratio (ER1 / ER2) of the etching rate ER1 of the phase shift film 13 by the etching gas to the etching rate ER2 of the protective film 12 by the etching gas is also called the selectivity. The higher the selectivity, the better the processability of the phase shift film 13. The selectivity is preferably 10 or more, and more preferably 30 or more. The selectivity is preferably 200 or less, and more preferably 100 or less.

[0028] The protective film 12 contains at least one element selected from, for example, Ru, Rh, and Si. When the protective film 12 contains Rh, the protective film 12 may contain only Rh, or may contain an Rh compound. The Rh compound may contain, in addition to Rh, at least one element Z1 selected from the group consisting of Ru, Nb, Mo, Ta, Ir, Pd, Zr, Y, and Ti.

[0029] By adding Ru, Nb, Mo, Zr, Y or Ti to Rh, the extinction coefficient can be reduced while suppressing an increase in the refractive index, and the reflectance to EUV light can be improved. Furthermore, by adding Ta, Ir, Pd or Y to Rh, the durability to etching gas and / or sulfuric acid / hydrogen peroxide can be improved. Sulfuric acid / hydrogen peroxide is used for removing a resist film or cleaning a reflective mask 2, which will be described later.

[0030] The element ratio (Z1:Rh) of Z1 (all Z1) to Rh is preferably 1:99 to 1:1. In this specification, the element ratio means a molar ratio. If the ratio value (Z1 / Rh) is 1 / 99 or more, the reflectance to EUV light is good. If the ratio value (Z1 / Rh) is 1 or less, the durability of the protective film 12 to the etching gas is good. The element ratio (Z1:Rh) of Z1 to Rh is more preferably 3:10 to 1:1.

[0031] When Z1 is Ru, the element ratio of Ru to Rh (Ru / Rh) is preferably greater than 0.0 and less than 1.0 (0.0<(Ru / Rh)<1.0), and more preferably greater than 0.3 and less than 0.5 (0.3<(Ru / Rh)<0.5). When the element ratio (Ru / Rh) is greater than 0.0, the reflectance to EUV light is good. When the element ratio (Ru / Rh) is less than 1.0, the etching resistance is good.

[0032] When Z1 is Pd, the element ratio of Pd to Rh (Pd / Rh) is preferably more than 0.00 and less than 1.0 (0.00<(Pd / Rh)<1.0), and more preferably more than 0.01 and less than 0.1 (0.01<(Pd / Rh)<0.1). When the element ratio (Pd / Rh) is more than 0.00, the etching resistance is good. When the element ratio (Pd / Rh) is less than 1.0, the reflectance to EUV light is good.

[0033] The Rh compound may contain, in addition to Rh, at least one element Z2 selected from the group consisting of N, O, C, and B. The element Z2 reduces the durability of the protective film 12 against etching gas, but improves the smoothness of the protective film 12 by reducing the crystallinity of the protective film 12. The Rh compound containing the element Z2 has an amorphous structure or a microcrystalline structure. When the Rh compound has an amorphous structure or a microcrystalline structure, the X-ray diffraction profile of the Rh compound does not have a clear peak.

[0034] When the Rh compound contains Z2 in addition to Rh, the content of Rh or the total content of Rh and Z1 is preferably 40 at% to 99 at% and the total content of Z2 is preferably 1 at% to 60 at%. When the Rh compound contains Z2 in addition to Rh, the content of Rh or the total content of Rh and Z1 is more preferably 80 at% to 99 at% and the total content of Z2 is more preferably 1 at% to 20 at%.

[0035] The Rh compound contains 90 at % or more of Rh, contains at least one of Z1 and Z2, and has a concentration of 10.0 g / cm 3 ~14.0g / cm 3 The Rh compound has an amorphous or microcrystalline structure when it has a density of 11.0 g / cm. 3 ~13.0g / cm 3 It is.

[0036] The protective film 12 contains 100 at % Rh and has a density of 11.0 g / cm 3 ~12.0g / cm 3 When the protective film 12 has a density of 0.1 to 100%, the protective film 12 has an amorphous structure or a microcrystalline structure. The density of the protective film 12 is measured by X-ray reflectance method.

[0037] The protective film 12 may be a film consisting of a single layer, or may be a multi-layer film having a lower layer and an upper layer. The lower layer is a layer formed in contact with the uppermost surface of the multilayer reflective film 11, and the upper layer is in contact with the lowermost surface of the phase shift film 13. By forming the protective film 12 in this manner with a multi-layer structure, materials having excellent predetermined functions can be used for each layer, thereby making it possible to make the protective film 12 as a whole multifunctional.

[0038] The upper layer of the protective film 12 preferably contains Rh, and more preferably contains an Rh compound. The lower layer of the protective film 12 preferably contains at least one element selected from the group consisting of Ru, Nb, Mo, Zr, Y, C, and B, and more preferably contains Ru. In addition, when the protective film 12 is a multilayer film, it is also preferable that the total thickness of the multilayer film is within the following preferred range of the thickness of the protective film 12.

[0039] The thickness of the protective film 12 is preferably 1.0 nm to 4.0 nm, more preferably 2.0 nm to 3.5 nm, and further preferably 2.3 nm to 3.0 nm. If the thickness of the protective film 12 is 1.0 nm or more, the etching resistance is good. If the thickness of the protective film 12 is 4.0 nm or less, the reflectance to EUV light is good.

[0040] The density of the protective film 12 is preferably 10.0 g / cm 3 ~14.0g / cm 3 The density of the protective film 12 is 10.0 g / cm 3 If the density of the protective film 12 is 14.0 g / cm or more, the etching resistance is good. 3 If it is equal to or less than this, a decrease in reflectance for EUV light can be suppressed.

[0041] The upper surface of the protective film 12, that is, the surface on which the phase shift film 13 of the protective film 12 is formed, preferably has a root mean square roughness Rq of 0.20 nm or less, more preferably 0.17 nm or less. If the root mean square roughness Rq is 0.20 nm or less, a phase shift film 13 or the like can be smoothly formed on the protective film 12. In addition, scattering of EUV light can be suppressed, and the reflectivity with respect to EUV light can be improved. The root mean square roughness Rq is preferably 0.05 nm or more.

[0042] Examples of the method for forming the protective film 12 include a DC sputtering method, a magnetron sputtering method, or an ion beam sputtering method. When forming a Rh film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of Rh film> Target: Rh target, Sputtering gas: Ar gas, Gas pressure: 1.0×10 -2 Pa~1.0×10 0 Pa, Output density of target: 1.0 W / cm 2 ~8.5 W / cm 2 , Film formation rate: 0.020 nm / sec~1.000 nm / sec, Film thickness: 1 nm~10 nm.

[0043] When forming a Rh film, N2 gas or a mixed gas of Ar gas and N2 may be used as the sputtering gas. The volume ratio of N2 gas in the sputtering gas (N2 / (Ar + N2)) is 0.05 or more and 1.0 or less.

[0044] When forming a RhO film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of RhO film> Target: Rh target, Sputtering gas: O2 gas or a mixed gas of Ar gas and O2, Volume ratio of O2 gas in the sputtering gas (O2 / (Ar + O2)): 0.05~1.0, Gas pressure: 1.0×10-2 Pa~1.0×10 0 Pa, Output density of the target: 1.0 W / cm 2 ~8.5 W / cm 2 , Film formation rate: 0.020 nm / sec to 1.000 nm / sec, Film thickness: 1 nm to 10 nm.

[0045] When forming an RhRu film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of RhRu film> Target: Rh target and Ru target (or RhRu target), Sputtering gas: Ar gas, Gas pressure: 1.0×10 -2 Pa~1.0×10 0 Pa, Output density of the target: 1.0 W / cm 2 ~8.5 W / cm 2 , Film formation rate: 0.020 nm / sec to 1.000 nm / sec, Film thickness: 1 nm to 10 nm.

[0046] The reflective mask blank 1 may further have a buffer film between the protective film 12 and the phase shift film 13. By having the buffer film in the reflective mask blank 1, the thickness of the phase shift film 13 may be further reduced in some cases.

[0047] The buffer film preferably contains one or more elements selected from the group consisting of Ta and Cr. Further, the buffer film preferably further contains one or more elements selected from the group consisting of B, C, N, and O. As the material constituting the buffer film, for example, a compound containing Ta and one or more elements selected from the group consisting of B, C, N, and O is preferable, and TaBN or TaBO is more preferable. Note that "TaBN" represents a compound containing Ta, B, and N, and "TaBO" represents a compound containing Ta, B, and O.

[0048] When the buffer film contains one or more elements selected from the group consisting of Ta and Cr, the content of the one or more elements selected from the group consisting of Ta and Cr is preferably 50 at% or more, more preferably 70 at% or more. The elements contained in the buffer film and the amounts thereof can be obtained by the same method as that of the phase shift film 13.

[0049] The thickness of the buffer film is preferably 0.5 nm to 25 nm. In particular, the thickness of the buffer film is preferably 10 nm or less in order to further reduce the total thickness of the buffer film and the phase shift film 13. The thickness of the buffer film can be measured by XRR (X-ray reflectometry).

[0050] The refractive index n of the buffer film is preferably 0.930 to 0.970. The extinction coefficient k of the buffer film is preferably 0.0150 to 0.0400. The refractive index n and extinction coefficient k of the buffer film can be measured in the same manner as the refractive index n and extinction coefficient k of the phase shift film 13.

[0051] The buffer film can be formed by a known film formation method, such as a sputtering method, which includes magnetron sputtering and ion beam sputtering.

[0052] The phase shift film 13 is a film in which an opening pattern 13a is to be formed. The opening pattern 13a is not formed in the manufacturing process of the reflective mask blank 1, but is formed in the manufacturing process of the reflective mask 2. The phase shift film 13 shifts the phase of the second EUV light L2 with respect to the first EUV light L1 shown in FIG.

[0053] The first EUV light L1 is light that passes through the opening pattern 13a without passing through the phase shift film 13, is reflected by the multilayer reflective film 11, and passes through the opening pattern 13a without passing through the phase shift film 13 again. The second EUV light L2 is light that passes through the phase shift film 13 while being absorbed by the phase shift film 13, is reflected by the multilayer reflective film 11, and passes through the phase shift film 13 while being absorbed by the phase shift film 13 again.

[0054] The phase difference (≧0) between the first EUV light L1 and the second EUV light L2 is, for example, 170° to 250°. The phase of the first EUV light L1 may be ahead of or behind the phase of the second EUV light L2. The phase shift film 13 improves the contrast of the transferred image by utilizing the interference between the first EUV light L1 and the second EUV light L2. The transferred image is an image obtained by transferring the opening pattern 13a of the phase shift film 13 onto the target substrate.

[0055] In EUVL, a so-called projection effect (shadowing effect) occurs. The shadowing effect refers to a region in which the sidewall of the opening pattern 13a blocks the EUV light due to the incident angle θ of the EUV light being not 0° (for example, 6°), resulting in a positional or dimensional shift of the transferred image. In order to reduce the shadowing effect, it is effective to reduce the height of the sidewall of the opening pattern 13a, and it is also effective to thin the phase shift film 13.

[0056] The thickness of the phase shift film 13 is, for example, 60 nm or less, and preferably 50 nm or less, in order to reduce the shadowing effect. The thickness of the phase shift film 13 is preferably 20 nm or more, and more preferably 30 nm or more, in order to ensure a phase difference between the first EUV light L1 and the second EUV light L2.

[0057] In order to reduce the thickness of the phase shift film 13 to reduce the shadowing effect while ensuring the phase difference between the first EUV light L1 and the second EUV light L2, it is effective to reduce the refractive index n of the phase shift film 13. Therefore, the phase shift film 13 of this embodiment has a layer formed of a Ru compound containing at least Ru, Cr, and O. The Ru compound may further contain N. In this embodiment, the phase shift film 13 is a single layer, but may be a multi-layer film. In any case, it is sufficient that at least one layer constituting the phase shift film 13 is formed of a Ru compound.

[0058] As shown in FIG. 6, Ru can reduce the refractive index n of the phase shift film 13, and the phase shift film 13 can be made thinner while maintaining the phase difference. However, Ru reduces the extinction coefficient k of the phase shift film 13. Therefore, it is considered to add Cr to Ru. By adding Cr, the extinction coefficient k of the phase shift film 13 can be increased. However, adding Cr reduces the etching rate ER1 of the phase shift film 13. As a result, the selectivity (ER1 / ER2) decreases, and the processability of the phase shift film 13 decreases.

[0059] The present inventors have focused on the fact that the extinction coefficient k can be increased by oxidizing Ru, as shown in Fig. 7. O has a small extinction coefficient k by itself (see Fig. 6), but by bonding with Ru, it is possible to increase the extinction coefficient k to a value greater than that of Ru. Therefore, by oxidizing Ru, the Cr content can be reduced, and a phase shift film 13 with excellent optical properties (refractive index n and extinction coefficient k) and processability can be obtained.

[0060] As shown in Fig. 7, Ru oxides (e.g., RuO2) have a larger extinction coefficient k than simple Ru. Cr oxides (e.g., Cr2O3) have a smaller extinction coefficient k than simple Cr. Therefore, when the ratio (Cr / (Ru+Cr)) of the Cr content (at%) to the sum of the Ru content (at%) and the Cr content (at%) is the same, the higher the Ru oxidation degree and the lower the Cr oxidation degree, the larger the extinction coefficient k.

[0061] The Ru oxidation degree and the Cr oxidation degree are obtained from X-ray photoelectron spectroscopy (XPS) spectra. An example of an XPS spectrum of a Ru compound is shown in Figure 8. The XPS spectrum has a peak waveform W0 in the range of 572 eV to 580 eV. This peak waveform W0 can be separated into a first peak waveform W1 derived from simple Cr and a second peak waveform W2 derived from Cr2O3.

[0062] For the measurement of XPS spectrum, for example, an analyzer "PHI 5000 VersaProbe" manufactured by ULVAC-PHI, Inc. is used. The measurement sample is cut out from the reflective mask blank into a size of about 1 cm square, and set in the measurement holder so that the surface of the phase shift film becomes the measurement surface. Then, the surface of the phase shift film is removed with an argon ion beam until the peak observed from the surface of the phase shift film becomes constant. After that, the removed part is irradiated with X-rays (monochromated AlKα rays) to obtain an XPS spectrum. The photoelectron take-off angle (the angle between the surface of the measurement sample and the direction of the detector) is set to 45°. In addition, a neutralization gun is used during the analysis to suppress charge-up. The narrow scan of Cr is performed, for example, with a pass energy of 58.7 eV, an energy step of 0.1 eV, a time / step of 50 ms, and 5 accumulations.

[0063] For example, analysis software "Multipak" made by ULVAC-PHI, Inc. is used to analyze the XPS spectrum. The background W4 of the peak waveform W0 is estimated by the Shirley method, and the peak waveform W0 with the background W4 removed is separated into the first peak waveform W1 and the second peak waveform W2. The first peak waveform W1 is the peak waveform of Cr alone, and the second peak waveform W2 is the peak waveform of Cr2O3.

[0064] The parameters of the first peak waveform W1 are set as follows: Function: Asymmetric Gauss-Lorentzian, Position: 573.75 eV ~ 574.25 eV, FWHM: 1.30 eV, Gauss: 80%, Tell length: 12.8, Tail scale:1.2.

[0065] The parameters of the second peak waveform W2 are set as follows: Function: Asymmetric Gauss-Lorentzian, Position: 576.3eV~576.6eV, FWHM: 3.5 eV, Gauss: 95%, Tell length: 12.0, Tail scale:0.0.

[0066] The degree of Cr oxidation is calculated using the following formula (1). (Cr oxidation degree) = (A2 × 3 / 5) / (A1 + A2 × 2 / 5) (1) In the above formula (1), A1 is the area of ​​the region surrounded by the first peak waveform W1 and the background W4, and A2 is the area of ​​the region surrounded by the second peak waveform W2 and the background W4.

[0067] The Ru oxidation degree is calculated using the following formula (2). (Ru oxidation degree) = (B3 - B2 × (Cr oxidation degree)) / B1 (2) In the above formula (2), B1 is the Ru content (at %), B2 is the Cr content (at %), and B3 is the O content (at %).

[0068] In the Ru compound of this embodiment, the Cr oxidation degree / Ru oxidation degree is greater than 0 and less than 7.5. The Cr oxidation degree / Ru oxidation degree is preferably less than 3.0, more preferably less than 2.0, even more preferably less than 1.6, and particularly preferably less than 1.0. The smaller the Cr oxidation degree / Ru oxidation degree, the greater the extinction coefficient k of the Ru compound tends to be.

[0069] The extinction coefficient k of the Ru compound is preferably larger than a reference value k0. The reference value k0 is the extinction coefficient of an O-free RuCr alloy, and is a linear function of Cr / (Ru+Cr) (straight line L shown in FIG. 9). The reference value k0 varies according to Cr / (Ru+Cr). The rate of increase or decrease of k is expressed as the ratio (Δk / k0×100) of Δk (Δk=k−k0) to k0.

[0070] When Cr / (Ru+Cr) is less than 0.10, if the Cr oxidation degree / Ru oxidation degree is less than 7.5, k is greater than k0 and the rate of increase or decrease of k exceeds 0%.

[0071] When Cr / (Ru+Cr) is less than 0.20, if the Cr oxidation degree / Ru oxidation degree is less than 2.5, k is greater than k0 and the rate of increase or decrease of k exceeds 0%.

[0072] When Cr / (Ru+Cr) is 0.30 or less, if the Cr oxidation degree / Ru oxidation degree is less than 1.3, k is greater than k0 and the rate of increase or decrease of k exceeds 0%.

[0073] When Cr / (Ru+Cr) is less than 0.40, if the Cr oxidation degree / Ru oxidation degree is less than 1.0, k is greater than k0 and the rate of increase or decrease of k exceeds 0%.

[0074] When Cr / (Ru+Cr) is less than 0.50, if the Cr oxidation degree / Ru oxidation degree is less than 0.7, k is greater than k0 and the rate of increase or decrease of k exceeds 0%.

[0075] The layer made of the Ru compound is obtained, for example, by reactive sputtering. In reactive sputtering, a Ru target and a Cr target are used as targets. The O content in the Ru compound can be controlled by the content of O2 gas in the sputtering gas. Also, the N content in the Ru compound can be controlled by the content of N2 gas in the sputtering gas.

[0076] In reactive sputtering, it is preferable that the O2 gas supply port in the chamber is closer to the Ru target than to the Cr target. This allows the Cr oxidation degree / Ru oxidation degree to be small. Note that sputtering is not limited to reactive sputtering. The Cr oxidation degree / Ru oxidation degree can also be reduced by using a Ru oxide target and a Cr target.

[0077] The Ru compound preferably has an O content of more than 0 at% and less than 50 at%. If the O content is more than 0 at%, this is preferred from the viewpoint of the extinction coefficient k. If the O content is less than 50 at%, this is preferred from the viewpoint of the refractive index n and hydrogen resistance. The O content is more preferably 2 at% or more, even more preferably 3 at% or more, and particularly preferably 4 at% or more. The O content is more preferably 45 at% or less, even more preferably 35 at% or less, particularly preferably 30 at% or less, and most preferably 25 at% or less.

[0078] The Ru compound preferably has a Ru content of 50 at% or more and 90 at% or less. If the Ru content is 50 at% or more, the refractive index n of the phase shift film 13 is small. If the Ru content is 90 at% or less, the extinction coefficient k of the phase shift film 13 is large. The Ru content is more preferably 60 at% or more and 90 at% or less, and further preferably 60 at% or more and 80 at% or less.

[0079] The Ru compound preferably has a ratio (Cr / (Ru+Cr)) of the Cr content (at%) to the sum of the Ru content (at%) and the Cr content (at%) of 0.03 or more and 0.30 or less. If Cr / (Ru+Cr) is 0.03 or more, the extinction coefficient k of the phase shift film 13 is large. If Cr / (Ru+Cr) is 0.30 or less, the etching rate ER1 of the phase shift film 13 is large. Cr / (Ru+Cr) is more preferably 0.05 or more and 0.30 or less, further preferably 0.05 or more and 0.25 or less, and particularly preferably 0.10 or more and 0.20 or less.

[0080] The Ru compound preferably has a ratio (O / Cr) of the O content (at%) to the Cr content (at%) of 0.01 or more and 3.0 or less. If O / Cr is 0.01 or more, the extinction coefficient k of the phase shift film 13 is large. If O / Cr is 3.0 or less, the hydrogen resistance (stability against hydrogen gas) of the phase shift film 13 is good. O / Cr is more preferably 0.05 or more and 1.5 or less, and further preferably 0.1 or more and 1.0 or less.

[0081] The phase shift film 13 has a full width at half maximum FWHM of 1.0° or more of the highest intensity peak in the 2θ range of 20° to 50° measured by XRD using CuKα radiation. The out of plane method is used as the XRD method. If the full width at half maximum FWHM is 1.0° or more, the crystallinity of the phase shift film 13 is low, and the roughness of the sidewall of the opening pattern 13a can be reduced. The full width at half maximum FWHM is preferably 2.0° or more, more preferably 3.0° or more, and particularly preferably 4.0° or more. The larger the full width at half maximum FWHM, the better, and it is preferable that there is no clear peak.

[0082] The refractive index n of the phase shift film 13 is, for example, 0.925 or less, preferably 0.920 or less, more preferably 0.915 or less, and even more preferably 0.910 or less. The smaller the refractive index n, the smaller the film thickness of the phase shift film 13 can be. The refractive index n is preferably 0.900 or more. In this specification, the refractive index is the refractive index for light with a wavelength of 13.5 nm.

[0083] The extinction coefficient k of the phase shift film 13 is, for example, 0.0195 or more, preferably 0.0200 or more, more preferably 0.0205 or more, and even more preferably 0.0210 or more. The larger the extinction coefficient k, the more the reflectance for EUV light can be reduced. The extinction coefficient k is preferably 0.0275 or less. In this specification, the extinction coefficient is the extinction coefficient for light with a wavelength of 13.5 nm.

[0084] The optical properties (refractive index n and extinction coefficient k) of the phase shift film 13 are taken from the database of the Center for X-Ray Optics, Lawrence Berkeley National Laboratory, or values ​​calculated from the "incident angle dependence" of reflectance described below.

[0085] The incident angle θ of the EUV light, the reflectance R for the EUV light, the refractive index n of the phase shift film 13, and the extinction coefficient k of the phase shift film 13 satisfy the following formula (1). R = |(sinθ-((n+ik) 2-cos 2 θ) 1 / 2 ) / (sinθ + ((n + ik) 2 -cos 2 θ) 1 / 2 )|···(1) Measure a plurality of combinations of the incident angle θ and the reflectance R, and calculate the refractive index n and the attenuation coefficient k by the least squares method so that the error between the plurality of measurement data and the formula (1) is minimized.

[0086] The phase shift film 13 has an etching rate of 0 nm / min to 0.05 nm / min with sulfuric acid peroxide. Sulfuric acid peroxide is used for removing the resist film described later or cleaning the reflective mask 2. If the etching rate of the phase shift film 13 with sulfuric acid peroxide is 0.05 nm / min or less, damage to the phase shift film 13 during cleaning can be suppressed.

[0087] The film formation method of the phase shift film 13 is, for example, a DC sputtering method, a magnetron sputtering method, or an ion beam sputtering method. The oxygen content of the phase shift film 13 can be controlled by the content of O2 gas in the sputtering gas. Also, the nitrogen content of the phase shift film 13 can be controlled by the content of N2 gas in the sputtering gas.

[0088] When forming a RuCrON film using the reactive sputtering method, an example of the film formation conditions is as follows. <Film Formation Conditions of RuCrON Film> Targets: Ru target and Cr target, Output density of Ru target: 1.0 W / cm 2 ~8.5 W / cm 2 , Output density of Cr target: 1.0 W / cm 2 ~8.5 W / cm 2 , Sputtering gas: Mixed gas of Ar gas, O2 gas, and N2 gas, Volume ratio of O2 gas in the sputtering gas (O2 / (Ar + O2 + N2)): 0.01 to 0.25, Volume ratio of N2 gas in the sputtering gas (N2 / (Ar + O2 + N2)): 0.01 to 0.25, Deposition rate: 0.020nm / sec~0.060nm / sec, Film thickness: 20nm~60nm.

[0089] The etching mask film 14 is formed on the opposite side of the protective film 12 with respect to the phase shift film 13, and is used to form an opening pattern 13a in the phase shift film 13. A resist film (not shown) is provided on the etching mask film 14. In the manufacturing process of the reflective mask 2, a first opening pattern is first formed in the resist film, then a second opening pattern is formed in the etching mask film 14 using the first opening pattern, and then a third opening pattern 13a is formed in the phase shift film 13 using the second opening pattern. The first opening pattern, the second opening pattern, and the third opening pattern 13a have the same dimensions and the same shape in a plan view (Z-axis direction view). The etching mask film 14 enables the resist film to be made thinner.

[0090] The etching mask film 14 preferably contains at least one element selected from Al, Hf, Y, Cr, Nb, Ti, Mo, Ta, and Si. The etching mask film 14 may further contain at least one element selected from O, N, and B.

[0091] The thickness of the etching mask film 14 is preferably 2 nm or more and 30 nm or less, more preferably 2 nm or more and 25 nm or less, and further preferably 2 nm or more and 10 nm or less.

[0092] The etching mask film 14 may be formed by, for example, DC sputtering, magnetron sputtering, or ion beam sputtering.

[0093] Next, a method for manufacturing a reflective mask blank 1 according to one embodiment will be described with reference to Fig. 4. The method for manufacturing the reflective mask blank 1 includes, for example, steps S101 to S105 shown in Fig. 4. In step S101, a substrate 10 is prepared. In step S102, a multilayer reflective film 11 is formed on a first main surface 10a of the substrate 10. In step S103, a protective film 12 is formed on the multilayer reflective film 11. In step S104, a phase shift film 13 is formed on the protective film 12. In step S105, an etching mask film 14 is formed on the phase shift film 13.

[0094] The method for manufacturing the reflective mask blank 1 only needs to include at least steps S101 to S104. The method for manufacturing the reflective mask blank 1 may further include a step of forming a functional film not shown in FIG.

[0095] Next, referring to FIG. 5, a method for manufacturing a reflective mask 2 according to an embodiment will be described. The method for manufacturing a reflective mask 2 includes steps S201 to S204 shown in FIG. 5. In step S201, a reflective mask blank 1 is prepared. In step S202, the etching mask film 14 is processed. A resist film (not shown) is provided on the etching mask film 14. First, a first opening pattern is formed in the resist film, and then a second opening pattern is formed in the etching mask film 14 using the first opening pattern. Thereafter, the resist film is removed. For example, sulfuric acid / hydrogen peroxide is used to remove the resist film. In step S203, a third opening pattern 13a is formed in the phase shift film 13 using the second opening pattern. In step S203, the phase shift film 13 is etched using an etching gas. In step S204, the etching mask film 14 is removed. For example, an etching gas is used to remove the etching mask film 14. The etching gas used in step S204 (removing the etching mask film 14) may be the same as the etching gas used in step S203 (forming the opening pattern 13a). The manufacturing method of the reflective mask 2 only needs to include at least steps S201 and S203. EXAMPLES

[0096] The experimental data will be described below. In Examples 1 to 14, EUVL reflective mask blanks were produced under the same conditions except for the type of phase shift film and its deposition conditions. Each reflective mask blank was composed of a substrate, a multilayer reflective film, a protective film, and a phase shift film. Examples 1 to 8 and 14 are working examples, and Examples 9 to 13 are comparative examples.

[0097] The substrate was a SiO2-TiO2 glass substrate (6-inch (152 mm) square, 6.3 mm thick). The thermal expansion coefficient of this glass substrate at 20°C was 0.02×10 -7 / °C, Young's modulus is 67 GPa, Poisson's ratio is 0.17, and specific stiffness is 3.07 × 10 7 m 2 / s 2 The quality assurance area of ​​the first main surface of the substrate was polished to a root mean square roughness (RMS) of 0.15 nm or less and a flatness of 100 nm or less. A 100 nm-thick Cr film was formed on the second main surface of the substrate by magnetron sputtering. The sheet resistance of the Cr film was 100 Ω / □.

[0098] The multilayer reflective film was a Mo / Si multilayer reflective film. The Mo / Si multilayer reflective film was formed by repeating the deposition of a Si layer (thickness 4.5 nm) and a Mo layer (thickness 2.3 nm) 40 times using the ion beam sputtering method. The total thickness of the Mo / Si multilayer reflective film was 272 nm ((4.5 nm + 2.3 nm) x 40).

[0099] As a protective film, a Rh film (thickness: 2.5 nm) was formed by using a DC sputtering method.

[0100] The phase shift films formed had the chemical compositions shown in Table 1. In Examples 1 to 8 and 12 to 14, RuCrON films or RuCrN films were formed using reactive sputtering. In Examples 9 to 11, RuCr films were formed using DC sputtering. The film types and properties of the phase shift films obtained in Examples 1 to 20 are shown in Table 1.

[0101] [Table 1]

[0102] The chemical composition of the phase shift film was measured using an X-ray photoelectron spectrometer (PHI 5000 VersaProbe) manufactured by ULVAC-PHI, Inc. The optical properties (refractive index n and extinction coefficient k) of the phase shift film were measured as described above.

[0103] As shown in Table 1, in Examples 1 to 8 and 14, the Ru compound had a Cr oxidation degree / Ru oxidation degree of more than 0 and less than 7.5, and an O content of more than 0 at% and less than 50 at%. Therefore, in Examples 1 to 8 and 14, phase shift films excellent in optical properties (refractive index n and extinction coefficient k) and processability were obtained.

[0104] The reflective mask blank, the reflective mask, the manufacturing method of the reflective mask blank, and the manufacturing method of the reflective mask according to the present disclosure have been described above, but the present disclosure is not limited to the above-mentioned embodiments. Various changes, modifications, substitutions, additions, deletions, and combinations are possible within the scope of the claims. These naturally fall within the technical scope of the present disclosure. [Explanation of symbols]

[0105] 1 Reflective mask blank 2 Reflective mask 10 Substrate 11 Multilayer reflective film 12 Protective film 13 Phase shift film

Claims

1. A reflective mask blank having, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light, the phase shift film has a layer formed of a Ru compound containing at least Ru, Cr and O; The Ru compound has a ratio of a Cr oxidation degree to a Ru oxidation degree (Cr oxidation degree / Ru oxidation degree) determined from an X-ray photoelectron spectroscopy spectrum that is greater than 0 and less than 7.5, and an O content that is greater than 0 at% and less than 50 at%.

2. The Ru compound has a Ru content of 50 at % or more and 90 at % or less, The ratio (Cr / (Ru+Cr)) of the Cr content (at%) to the sum of the Ru content (at%) and the Cr content (at%) is 0.03 or more and 0.30 or less, 2. The reflective mask blank according to claim 1, wherein the ratio (O / Cr) of the O content (at %) to the Cr content (at %) is 0.01 or more and 3.0 or less.

3. The reflective mask blank according to claim 1 or 2, wherein the Ru compound has a refractive index n of 0.925 or less and an extinction coefficient k of 0.0195 or more.

4. 3. The reflective mask blank according to claim 1, wherein the phase shift film has a thickness of 20 nm to 60 nm.

5. The reflective mask blank according to claim 1 , wherein the protective film contains at least one element selected from the group consisting of Ru, Rh and Si.

6. an etching mask film is provided on the opposite side of the protective film with respect to the phase shift film; 3. The reflective mask blank according to claim 1, wherein the etching mask film contains at least one element selected from the group consisting of Al, Hf, Y, Cr, Nb, Ti, Mo, Ta and Si.

7. The reflective mask blank according to claim 6 , wherein the etching mask film further contains at least one element selected from the group consisting of O, N and B.

8. A reflective mask blank according to claim 1 or 2, A reflective mask including an opening pattern in the phase shift film.

9. A method for producing a reflective mask blank having, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and a phase shift film that shifts the phase of the EUV light, comprising: forming the multilayer reflective film, the protective film, and the phase shift film in this order on the substrate; the phase shift film has a layer formed of a Ru compound containing at least Ru, Cr and O; The Ru compound has a ratio of a Cr oxidation degree to a Ru oxidation degree (Cr oxidation degree / Ru oxidation degree) determined from an X-ray photoelectron spectroscopy spectrum that is greater than 0 and less than 7.5, and an O content that is greater than 0 at% and less than 50 at%.

10. Preparing a reflective mask blank according to claim 1 or 2; forming an opening pattern in the phase shift film; The method for manufacturing a reflective mask includes the steps of:

Citation Information

Patent Citations

  • Reflective mask blank for EUV lithography, reflective mask for EUV lithography and their manufacturing method

    JP2022024617A

  • Reflective mask blank, reflective mask, and method for manufacturing semiconductor device

    WO2022065421A1

  • Reflective mask blank, reflective mask, and method for manufacturing semiconductor device

    JP6929340B2

  • Reflective mask blank, reflective mask, and method for manufacturing semiconductor device