Lateral thermoelectric conversion material, lateral thermoelectric conversion element, and thermoelectric conversion module

By replacing cobalt and tin sites in chandite-type sulfides with Group 10 and Group 13 elements to achieve opposite anomalous Nernst coefficients, the transverse thermoelectric conversion material generates enhanced power and simplifies manufacturing, addressing the limitations of current materials and methods.

JP2024136094APending Publication Date: 2024-10-04TOHOKU UNIV +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023047069
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Current transverse thermoelectric conversion materials using the anomalous Nernst effect do not generate sufficient power for practical applications, and existing methods are complex and difficult to scale.

Method used

Develop a transverse thermoelectric conversion material by replacing parts of the cobalt and tin sites in chandite-type sulfides with Group 10 and Group 13 elements, respectively, to achieve opposite signs of anomalous Nernst coefficients, and arrange these materials in a meandering pattern with alternating thermoelectric conversion elements to enhance electromotive force.

Benefits of technology

The proposed solution significantly amplifies the anomalous Nernst effect, allowing for higher power generation and easier manufacturing of transverse thermoelectric conversion elements and modules, with improved durability and reduced manufacturing complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136094000001
    Figure 2024136094000001
  • Figure 2024136094000002
    Figure 2024136094000002
  • Figure 2024136094000003
    Figure 2024136094000003
Patent Text Reader

Abstract

To provide a lateral thermoelectric conversion material, a lateral thermoelectric conversion element, and a thermoelectric conversion module that can obtain a greater anomalous Nernst effect than conventional methods.SOLUTION: A lateral thermoelectric conversion material in which a portion of the cobalt site of a shandite-type sulfide represented by the following formula (1) is substituted with a Group 10 element, or a portion of the tin site of the shandite-type sulfide is substituted with a Group 13 element, the lateral thermoelectric conversion material has an anomalous Nernst coefficient of an opposite sign to that of the shandite-type sulfide. Co3Sn2S2 (1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lateral thermoelectric conversion material, a lateral thermoelectric conversion element, and a thermoelectric conversion module. [Background technology]

[0002] The Seebeck effect is known as a thermoelectric conversion mechanism in which an electromotive force is generated when a temperature gradient is applied to a material. In the Seebeck effect, the electromotive force is proportional to the temperature difference that occurs along the direction of the temperature gradient, so in order to obtain a large electromotive force, a complex three-dimensional structure is required in which p-type and n-type modules are alternately arranged in the vertical direction from the heat source surface. For this reason, it is difficult to deploy such a three-dimensional element over a large area.

[0003] To address such problems, for example, Patent Document 1 proposes a thermoelectric conversion element (lateral thermoelectric conversion element) that utilizes a thermoelectric conversion mechanism in which an electric field is generated in a direction perpendicular to the temperature gradient due to the anomalous Nernst effect. In the anomalous Nernst effect, an electromotive force is generated from an electric field in a lateral direction perpendicular to the temperature gradient (lateral electric field). Therefore, according to the thermoelectric conversion element of Patent Document 1, the element structure can be fabricated in a planar manner so as to follow the surface of the heat source, which is advantageous for making it into a large area and a film. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2020 / 218613 Summary of the Invention [Problem to be solved by the invention]

[0005] Although the anomalous Nernst effect has advantages over the Seebeck effect in terms of large area and film formation, the current amount of power generation achieved by the anomalous Nernst effect using conventional magnetic materials is not satisfactory for full-scale practical use.

[0006] Therefore, an object of the present invention is to provide a lateral thermoelectric conversion material, a lateral thermoelectric conversion element, and a thermoelectric conversion module that can obtain a larger anomalous Nernst effect than conventional ones. [Means for solving the problem]

[0007] The present inventors have found that it is possible to amplify electromotive force by connecting layers with different signs of the anomalous Nernst coefficient (= transverse electric field / temperature gradient). In the examples reported so far, different materials with significantly different optimal fabrication processes and conditions were used as layers with different signs of the anomalous Nernst coefficient. Therefore, the present inventors thought that realizing anomalous Nernst coefficients with different signs in material systems that have a common crystal structure and can be fabricated under similar processes and conditions would enable development into various device applications. Based on this knowledge, they conducted extensive research and completed the present invention.

[0008] That is, the present invention has the following aspects. [1] A transverse thermoelectric conversion material in which a part of the cobalt site of a shandite-type sulfide represented by the following formula (1) is substituted with a Group 10 element or a part of the tin site of the shandite-type sulfide is substituted with a Group 13 element, A transverse thermoelectric conversion material having an anomalous Nernst coefficient of the opposite sign to that of the shandite-type sulfide. Co3Sn2S2...Formula (1) [2] The lateral thermoelectric conversion material according to [1], wherein the Group 13 element is indium, and a portion of the tin sites is substituted with indium. [3] The lateral thermoelectric conversion material according to [1], wherein the Group 10 element is nickel, and a portion of the cobalt site is substituted with nickel. [4] A lateral thermoelectric conversion element in which a first thermoelectric conversion element including a lateral thermoelectric conversion material having a positive anomalous Nernst coefficient and a second thermoelectric conversion element including a lateral thermoelectric conversion material according to any one of [1] to [3] having a negative anomalous Nernst coefficient are alternately arranged and connected in a meandering wiring pattern. [5] A thermoelectric conversion module comprising the lateral thermoelectric conversion element described in [4]. Effect of the Invention

[0009] According to the present invention, it is possible to provide a lateral thermoelectric conversion material, a lateral thermoelectric conversion element, and a thermoelectric conversion module that can obtain a larger anomalous Nernst effect than ever before. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a plan view showing an arrangement pattern of a Kagome lattice. [Diagram 2] FIG. 2 is a perspective view showing a schematic configuration of a horizontal thermoelectric conversion element according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a plan view illustrating a method for measuring the anomalous Nernst coefficient of a lateral thermoelectric conversion material constituting the lateral thermoelectric conversion element of the present invention. [Figure 4] 4 is a graph showing the temperature dependence of electrical resistivity of a lateral thermoelectric conversion material according to one embodiment of the present invention. [Diagram 5] 13 is a graph showing the temperature dependence of electrical resistivity of a transverse thermoelectric conversion material according to another embodiment of the present invention. [Figure 6] 4 is a graph showing the temperature dependence of the anomalous Nernst coefficient of a transverse thermoelectric conversion material according to an embodiment of the present invention. [Figure 7] 13 is a graph showing the temperature dependence of the anomalous Nernst coefficient of a transverse thermoelectric conversion material according to another embodiment of the present invention. [Figure 8] 4 is a graph showing the change in the anomalous Nernst coefficient of a transverse thermoelectric conversion material according to an embodiment of the present invention depending on the amount of element substitution. [Figure 9] 13 is a graph showing the change in the anomalous Nernst coefficient of a transverse thermoelectric conversion material according to another embodiment of the present invention depending on the amount of element substitution. [Figure 10] 1 is a photograph showing a plan view of a lateral thermoelectric conversion element used in an example. [Figure 11] 4 is a graph showing the magnetic field dependence of the electromotive force of a lateral thermoelectric conversion element according to an embodiment of the present invention. [Figure 12] 4 is a graph showing the temperature dependence of electromotive force of a lateral thermoelectric conversion element according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In addition, the drawings used in the following description may show characteristic parts in a schematic manner for the sake of convenience in order to make the characteristics easier to understand, and the dimensional ratios of each component may not necessarily be the same as in reality. Furthermore, the materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not necessarily limited to them, and may be appropriately modified and implemented within the scope of the present invention.

[0012] <Lateral thermoelectric conversion material> The transverse thermoelectric conversion material of the present invention has an anomalous Nernst coefficient with an opposite sign to that of the shandite-type sulfide represented by the following formula (1). Co3Sn2S2...Formula (1)

[0013] Shandite-type sulfides are sulfides with the formula T3M2S2. T is a transition metal element such as cobalt (Co) or nickel (Ni), and M is a typical metal element such as tin (Sn) or indium (In). Shandite-type sulfides are characterized by the transition metal element T forming a kagome lattice.

[0014] The kagome lattice is a lattice with a pattern in which atoms are arranged at the vertices of equilateral triangles and regular hexagons, as shown in Figure 1. The kagome lattice is formed by removing one-quarter of the atoms from a triangular lattice in which atoms are arranged at the vertices of equilateral triangles. In the kagome lattice, atoms are arranged in a "basket weave" pattern, with each atom having four neighbors. The kagome lattice is expected to be a stage for the emergence of topologically protected band states and dispersion-free flat bands.

[0015] Anomalous Nernst coefficient S xy is expressed by the following formula (2). S xy =ρ xx α xy +ρ yx α xx ...Equation (2) In equation (2), ρ xx is the electrical resistivity, α xy is the lateral thermal conductivity, ρ yx is the Hall resistivity, α xx represents the Peltier coefficient, where α xy is expressed by the Mott equation, given by the following equation (3). α xy =(π 2 / 3)×{(k B 2 T) / e}(∂σ xy / ∂ε) (3)

[0016] In equation (3), k B is the Boltzmann constant, T is the absolute temperature, e is the elementary charge, σ xy is the Hall conductivity, and ε is the electron energy. Here, ∂σ xy / ∂ε is the value at the Fermi level.

[0017] In the shandite-type sulfide of this embodiment, when no element substitution is performed, the anomalous Nernst coefficient S xy The sign of is positive.

[0018] In this specification, the term "lateral thermoelectric conversion material" refers to a thermoelectric conversion material that generates an electromotive force due to the anomalous Nernst effect.

[0019] The transverse thermoelectric conversion material of this embodiment is a shandite-type sulfide represented by formula (1) in which a portion of the cobalt site is replaced with a Group 10 element, or a portion of the tin site of the shandite-type sulfide is replaced with a Group 13 element. The lateral thermoelectric conversion material of this embodiment is represented by, for example, the composition formula of formula (4) below. Co 3-x X x Sn 2-y Y y S2...Equation (4)

[0020] In formula (4), X is a Group 10 element substituted for a part of the cobalt site, x is a number between 0 and 3 that represents the substance amount ratio (molar ratio), Y is a Group 13 element substituted for a part of the tin site, and y is a number between 0 and 2 that represents the substance amount ratio (molar ratio). However, in formula (4), when x is positive, y=0, and when y is positive, x=0, that is, xy=0 (except when x=0 and y=0).

[0021] Examples of X in the formula (4) include nickel (Ni), palladium (Pd), and platinum (Pt). X in the formula (4) is preferably a transition metal element such as nickel or palladium, and more preferably nickel, because it is easily substituted by the cobalt site.

[0022] In formula (4), x is 0 or more and 3 or less, preferably 0.01 or more and 1.0 or less, and more preferably 0.15 or more and 0.4 or less. When x in formula (4) is within the above numerical range, the anomalous Nernst coefficient S xy The sign of may be inverted. The x in formula (4) can be determined by a composition analysis method such as energy dispersive X-ray spectroscopy, electron probe microanalysis, X-ray photoelectron spectroscopy, or inductively coupled plasma atomic emission spectrometry.

[0023] Examples of Y in the formula (4) include boron (B), aluminum (Al), gallium (Ga), indium (In), and thallium (Tl). As Y in the formula (4), typical metal elements such as aluminum, gallium, and indium are preferred because they are easily substituted at the tin site, and indium is more preferred.

[0024] In the formula (4), y is 0 or more and 2 or less, preferably 0.01 or more and 1.0 or less, and more preferably 0.15 or more and 0.6 or less. When y in the formula (4) is within the above numerical range, the anomalous Nernst coefficient S xy The sign of may be inverted. The value of y in formula (4) can be determined by a composition analysis method such as energy dispersive X-ray spectroscopy, electron probe microanalysis, X-ray photoelectron spectroscopy, or inductively coupled plasma atomic emission spectrometry.

[0025] The shandite-type sulfide represented by formula (1) used in the transverse thermoelectric conversion material of this embodiment can be obtained, for example, by chemical vapor deposition in the case of a bulk sample, and by sputtering or molecular beam epitaxy in the case of a thin film sample.

[0026] The lateral thermoelectric conversion material of this embodiment can have an anomalous Nernst coefficient of the opposite sign to that of the shandite-type sulfide represented by formula (1) depending on the element substitution conditions. Therefore, by creating a thermopile structure in which it is appropriately combined with the shandite-type sulfide represented by formula (1), the value of the electromotive force generated by the temperature gradient can be increased compared to the electromotive force output when each material is used alone. This makes it possible to obtain better lateral thermoelectric conversion performance than before. In addition, since the transverse thermoelectric conversion material of this embodiment and the shandite-type sulfide represented by formula (1) have perpendicular magnetic anisotropy, the magnetization directions of the transverse thermoelectric conversion material of this embodiment and the shandite-type sulfide represented by formula (1) can be aligned by applying a magnetic field larger than the saturation magnetic field of the transverse thermoelectric conversion material of this embodiment and the shandite-type sulfide represented by formula (1) in the direction perpendicular to the sample surface (perpendicular to the thermal gradient). Furthermore, even after the magnetic field is reduced to zero Tesla (T), the magnetization remains in the direction perpendicular to the surface, so the magnetization orientation state can be maintained in the absence of a magnetic field. Therefore, as in the conventional method, in order to control the magnetization orientation directions of multiple constituent materials having the same sign of anomalous Nernst coefficient in opposite directions to accumulate the electromotive force, a complex magnetization process that takes into account the saturation magnetic field of multiple constituent materials and the application of a steady magnetic field to maintain the magnetized state are no longer necessary, making it easier to apply the method to transverse thermoelectric conversion elements and thermoelectric conversion modules.

[0027] In the shandite-type sulfide represented by formula (1), the substitution of a group 10 element at the cobalt site corresponds to an increase in the number of electrons, and the substitution of a group 13 element at the tin site corresponds to a decrease in the total number of electrons. The shandite-type sulfide has a singular point where bands intersect in the band structure, and the energy position of the Fermi level is very sensitive to an increase or decrease in the number of electrons. Therefore, it is considered that the sign and absolute value of the anomalous Nernst coefficient of the transverse thermoelectric conversion material of this embodiment can be modulated by raising or lowering the energy position of the Fermi level in the electronic structure of the substance constituting the transverse thermoelectric conversion material. For these reasons, the sign and absolute value of the anomalous Nernst coefficient of the transverse thermoelectric conversion material of this embodiment can be adjusted by the type and amount of the Group 10 element substituted on the cobalt site, the type and amount of the Group 13 element substituted on the tin site, and a combination of these.

[0028] <Manufacturing method of horizontal thermoelectric conversion material> The transverse thermoelectric conversion material of the present invention can be obtained by substituting a portion of the cobalt site of the shandite-type sulfide represented by formula (1) with a Group 10 element or by substituting a portion of the tin site of the shandite-type sulfide with a Group 13 element. Methods for substituting a part of the cobalt site of the shandite-type sulfide represented by formula (1) with a group 10 element include, for example, a method of mixing a powder of a cobalt raw material with a powder of a group 10 element raw material, a method of separately supplying a cobalt raw material and a raw material of a group 10 element in a vacuum to form a film, and a method of supplying a premix of a cobalt raw material and a raw material of a group 10 element in a vacuum to form a film. Methods for supplying raw materials in a vacuum include vacuum deposition, molecular beam epitaxy, sputtering, and pulsed laser deposition. In order to perform homogeneous substitution, the sample may be heat-treated after film formation. Examples of the cobalt raw material include simple cobalt, cobalt sulfide, cobalt alloys, cobalt-containing complexes, and organic compounds containing cobalt. Examples of raw materials for the Group 10 elements include nickel, nickel sulfide, nickel alloys, nickel complexes, organic compounds containing nickel, palladium, palladium sulfide, palladium alloys, palladium complexes, and organic compounds containing palladium.

[0029] As a method for substituting a part of the cobalt site of the shandite-type sulfide represented by formula (1) with a Group 10 element, a sputtering method is preferred because it is easy to prepare a thin film that shows the anomalous Nernst effect and to prepare an element using the thin film, and it is also suitable for mass production.

[0030] Methods for substituting a part of the tin site of the shandite-type sulfide represented by formula (1) with a Group 13 element include, for example, a method of mixing a powder of a tin raw material with a powder of a Group 13 element raw material, a method of separately supplying a raw material of tin and a raw material of a Group 13 element in a vacuum to form a film, a method of supplying a mixture of a raw material of tin and a raw material of a Group 13 element in advance in a vacuum to form a film, etc. In order to perform the substitution uniformly, the sample may be heat-treated after film formation. Examples of the tin raw material include simple tin, tin sulfide, tin alloys, tin complexes, and organic compounds containing tin. Examples of raw materials for the Group 13 elements include indium alone, indium sulfide, indium alloys, indium complexes, organic compounds containing indium, aluminum alone, aluminum sulfide, aluminum alloys, aluminum complexes, organic compounds containing aluminum, gallium alone, gallium sulfide, gallium alloys, gallium complexes, and organic compounds containing gallium.

[0031] As a method for substituting a part of the tin site of the shandite-type sulfide represented by formula (1) with a Group 13 element, a sputtering method is preferred because it is easy to prepare a thin film that shows the anomalous Nernst effect and to prepare an element using the thin film, and it is also suitable for mass production.

[0032] In addition, the above-mentioned powder mixing method, vacuum deposition method, molecular beam epitaxy method, sputtering method, and pulse laser deposition method are not particularly limited and can be performed using known methods.

[0033] <Horizontal thermoelectric conversion element> The lateral thermoelectric conversion element of the present invention has first thermoelectric conversion elements and second thermoelectric conversion elements arranged alternately in a meandering wiring pattern on a substrate. The first thermoelectric conversion element includes a transverse thermoelectric conversion material having a temperature region in which the sign of the anomalous Nernst coefficient is positive below the ferromagnetic transition temperature. Examples of transverse thermoelectric conversion materials having a positive anomalous Nernst coefficient include a shandite-type sulfide represented by formula (1), a sulfide in which a portion of the cobalt site of the shandite-type sulfide represented by formula (1) is substituted with a Group 10 element, and a sulfide in which a portion of the tin site of the shandite-type sulfide represented by formula (1) is substituted with a Group 13 element. As a transverse thermoelectric conversion material having a positive anomalous Nernst coefficient, a shandite-type sulfide represented by formula (1) is preferable because it has a large absolute value of the anomalous Nernst coefficient.

[0034] The second thermoelectric conversion element includes the transverse thermoelectric conversion material of this embodiment, which has a temperature region in which the sign of the anomalous Nernst coefficient is negative below the ferromagnetic transition temperature. Examples of transverse thermoelectric conversion materials having a negative anomalous Nernst coefficient include a sulfide in which a part of the cobalt site of the shandite-type sulfide represented by formula (1) is substituted with a Group 10 element, and a sulfide in which a part of the tin site of the shandite-type sulfide represented by formula (1) is substituted with a Group 13 element. The second thermoelectric conversion element is substituted with x or y in formula (4) that is greater than 0 and less than or equal to 3, preferably greater than or equal to 0.01 and less than or equal to 1.0, and more preferably greater than or equal to 0.15 and less than or equal to 0.4. As a transverse thermoelectric conversion material having a negative anomalous Nernst coefficient, a sulfide in which part of the tin site of the shandite-type sulfide represented by formula (1) is substituted with a Group 13 element is preferable because the absolute value of the anomalous Nernst coefficient is large.

[0035] The lateral thermoelectric conversion element of this embodiment will be described with reference to FIG. FIG. 2 is a perspective view that illustrates a schematic configuration of the lateral thermoelectric conversion element 20. As shown in FIG.

[0036] 2, the lateral thermoelectric conversion element 20 of this embodiment includes a substrate 22 and a power generating body 23 arranged on the substrate 22. In the lateral thermoelectric conversion element 20, when a temperature gradient ▽T is applied in the +y direction within the plane of the power generating body 23, a voltage V is generated in the power generating body 23 due to the anomalous Nernst effect.

[0037] The substrate 22 has a first surface 22a on which the power generator 23 is arranged, and a second surface 22b opposite to the first surface 22a. In Fig. 2, the short side direction of the substrate 22 is the x-direction, the long side direction is the y-direction, and the thickness direction is the z-direction.

[0038] The power generating body 23 has a plurality of first thermoelectric conversion elements 24 and a plurality of second thermoelectric conversion elements 25. The first thermoelectric conversion elements 24 may be the same as the first thermoelectric conversion elements described above. The second thermoelectric conversion elements 25 may be the same as the second thermoelectric conversion elements described above.

[0039] A plurality of first thermoelectric conversion elements 24 and a plurality of second thermoelectric conversion elements 25 are arranged alternately on the substrate 22, parallel to each other in their respective longitudinal directions (x direction in this embodiment), and have electrical connection portions, which will be described below, in a direction perpendicular thereto (y direction in this embodiment). The number of first thermoelectric conversion elements 24 and second thermoelectric conversion elements 25 constituting the power generating body 23 is not limited.

[0040] The first thermoelectric conversion element 24 has a first connection portion 24a at one end side (+x side) in the longitudinal direction (x direction) facing one side (+y side) in the other direction (y direction). The second thermoelectric conversion element 25 has a first connection portion 25a protruding from one end side (+x side) in the longitudinal direction (x direction) toward the other side (-y side) in the other direction (y direction). Either the first thermoelectric conversion element 24 or the second thermoelectric conversion element 25 may have the protruding connection portion.

[0041] The first thermoelectric conversion element 24 has a second connection portion 24b at the other end side (-x side) in the longitudinal direction (x direction) facing the other side (-y side) in the other direction (y direction). The second thermoelectric conversion element 25 has a second connection portion 25b protruding from the other end side (-x side) in the longitudinal direction (x direction) toward one side (+y side) in the other direction (y direction). Either the first thermoelectric conversion element 24 or the second thermoelectric conversion element 25 may have the protruding connection portion.

[0042] The first thermoelectric conversion element 24 is electrically connected to a first connection portion 25a of the second thermoelectric conversion element 25 via a first connection portion 24a. The first thermoelectric conversion element 24 is electrically connected to a second connection portion 25b of the second thermoelectric conversion element 25 via a second connection portion 24b. As a result, the plurality of first thermoelectric conversion elements 24 and the plurality of second thermoelectric conversion elements 25 are electrically connected in series in a meandering wiring shape. That is, the power generation body 23 is provided on the first surface 22a of the substrate 22 in a meandering shape (meander wiring shape).

[0043] A magnetic field is applied to the lateral thermoelectric conversion element 20 in a direction (+z direction) from the surface 22b to the first surface 22a of the substrate 22. By applying the magnetic field, the first thermoelectric conversion element 24 is magnetized (magnetization M1) in a direction (+z direction) from the second surface 22b to the first surface 22a of the substrate 22. Moreover, the second thermoelectric conversion element 25 is magnetized in the direction from the second surface 22b to the first surface 22a of the substrate 22 (the +z direction) (magnetization M2). After the first thermoelectric conversion element 24 and the second thermoelectric conversion element 25 are magnetized, the application of the magnetic field to the lateral thermoelectric conversion element 20 may be continued or the application of the magnetic field may be stopped.

[0044] Furthermore, the first thermoelectric conversion elements 24 and the second thermoelectric conversion elements 25 are designed to have anomalous Nernst coefficients of opposite signs to each other at or below the ferromagnetic transition temperature to be used. Therefore, the first thermoelectric conversion elements 24 and the second thermoelectric conversion elements 25 can be arranged so that the direction of magnetization M1 of the first thermoelectric conversion elements 24 (+z direction) and the direction of magnetization M2 of the second thermoelectric conversion elements 25 (+z direction) are the same. As described above, this means that the directions of magnetization M1 and magnetization M2 can be aligned by applying a magnetic field in the z direction that is greater than the saturation magnetic field of the first thermoelectric conversion elements 24 and the second thermoelectric conversion elements 25 to the power generation body 23, and has the effect of making it easier to manufacture the transverse thermoelectric conversion element 20.

[0045] When a temperature difference occurs in the +y direction in the plane of the substrate 22, a temperature gradient ▽T in the +y direction occurs in the plane of the power generation body 23. At this time, in the first thermoelectric conversion element 24, an electromotive force E1 is generated in a direction (+x direction) perpendicular to both the direction of the magnetization M1 (+z direction) and the direction of the temperature gradient ▽T (+y direction). On the other hand, in the second thermoelectric conversion element 25, an electromotive force E2 is generated in a direction (-x direction) perpendicular to both the direction of the magnetization M2 (+z direction) and the direction of the temperature gradient ▽T (+y direction). The reason that the directions of the electromotive forces E1 and E2 are opposite to each other is that the first thermoelectric conversion element 24 and the second thermoelectric conversion element 25 have anomalous Nernst coefficients with opposite signs to each other.

[0046] In the power generation body 23, the alternating first thermoelectric conversion element 24 and the second thermoelectric conversion element 25 are electrically connected in series, so that the transverse electric field generated in the first thermoelectric conversion element 24 and the transverse electric field generated in the second thermoelectric conversion element 25 are integrated, making it possible to increase the output voltage V. In addition, since the easy axes of magnetization M1 and magnetization M2 of the power generating body 23 are in the z direction, by applying a magnetic field in the z direction, the orientation directions of magnetization M1 and magnetization M2 can be aligned, making it easier to manufacture the horizontal thermoelectric conversion element 20.

[0047] In the horizontal thermoelectric conversion element 20 of this embodiment, the temperature gradient, the magnetization direction, and the electric field direction are perpendicular to each other, so that it is possible to use thin sheet-like first thermoelectric conversion element 24 and second thermoelectric conversion element 25.

[0048] Here, if the length of the first thermoelectric conversion element 24 and the second thermoelectric conversion element 25 in the direction perpendicular to the temperature gradient ▽T (longitudinal direction) is L, when the temperature gradient ▽T in the first thermoelectric conversion element 24 and the second thermoelectric conversion element 25 is constant, the voltage V generated by the anomalous Nernst effect is proportional to L. In other words, the longer the first thermoelectric conversion element 24 and the second thermoelectric conversion element 25 are, the larger the obtained voltage V will be.

[0049] Therefore, in the horizontal thermoelectric conversion element 20 of this embodiment, by adopting a power generation body 23 in which the above-mentioned alternatingly adjacent first thermoelectric conversion elements 24 and second thermoelectric conversion elements 25 are electrically connected in series, a further increase in voltage V can be expected.

[0050] In the lateral thermoelectric conversion element 20 of this embodiment, the anomalous Nernst coefficient S xy Therefore, the power generating body 23 having a thermopile structure as shown in Fig. 2 can be made from a single material system. This makes it possible to reduce the contact resistance at the first connecting parts 24a and 25a and the second connecting parts 24b and 25b, and improve the connection state at the interfaces between the alternating adjacent first thermoelectric conversion elements 24 and second thermoelectric conversion elements 25. In addition, in the lateral thermoelectric conversion element 20 of this embodiment, the magnetization directions of the first thermoelectric conversion element 24 and the second thermoelectric conversion element 25 can be made the same. Therefore, the magnetization orientation direction can be aligned by applying a magnetic field in one direction, and the lateral thermoelectric conversion element 20 can be manufactured more easily. In addition, the lateral thermoelectric conversion element 20 of this embodiment can be made of a single material, which simplifies the manufacturing process. In addition, the durability of the power generation body 23 can be improved because there is no difference in the thermal expansion coefficient between the first thermoelectric conversion element 24 and the second thermoelectric conversion element 25 that are alternately adjacent to each other.

[0051] <Thermoelectric conversion module> The thermoelectric conversion module of the present invention includes the lateral thermoelectric conversion element of the present invention. In this specification, the lateral thermoelectric conversion element refers to a thermoelectric conversion element that generates an electromotive force due to the anomalous Nernst effect. In the lateral thermoelectric conversion element, the temperature gradient, the magnetization direction, and the electric field direction are perpendicular to each other, so that it is possible to fabricate a thin sheet-like thermoelectric conversion element. By including such a lateral thermoelectric conversion element, the thermoelectric conversion module can be used as a power generation module or a heat flow sensor.

[0052] Thermoelectric conversion modules can be used in a variety of applications, particularly as a standalone power source or heat flow sensor for Internet of Things (IoT) sensors in the temperature range from room temperature (e.g., 25°C) to several hundred degrees Celsius.

[0053] For example, by applying the thermoelectric conversion module of this embodiment to a heat flow sensor, it can be used to judge the quality of the thermal insulation performance of a building or to detect dynamic changes in the temperature of a machine operating part. Also, by providing a thermoelectric conversion module in an exhaust system of an automobile or the like, it is possible to generate electricity using the heat (waste heat) of the exhaust gas, and the thermoelectric conversion module can be effectively used as an auxiliary power source. In other words, the thermoelectric conversion module can be used as a power generation module. Moreover, by arranging heat flow sensors in a mesh pattern on the wall surface of a space, it becomes possible to recognize heat flow and heat sources in space. This is expected to be applied, for example, to high-precision temperature control for high-density crop cultivation and livestock breeding, and as a driver detection system for autonomous driving. Furthermore, heat flow sensors can be used in indoor air conditioning management and deep body temperature management in medicine. Moreover, by making the lateral thermoelectric conversion material of this embodiment into a powder or paste, it is expected to be applied to a wide range of fields. EXAMPLES

[0054] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. The measurement methods and evaluations of various measured values ​​shown in this specification were performed as follows.

[0055] In this example, a target serving as the raw material for Co3Sn2S2 was prepared as follows. A SnS target having an outer diameter of 60 mm was prepared by mixing tin sulfide (II) and tin sulfide (IV) (amount ratio of substances: 1:1). 1.5 A cobalt metal chip and a nickel metal chip, or a cobalt metal chip and an indium (III) sulfide chip, were attached to the surface of the sintered disk to form a target. The above target was set in a sputtering device (ES-250, manufactured by Eiko Co., Ltd.), and a thin film in which part of the cobalt site of Co3Sn2S2 was replaced with nickel, or a thin film in which part of the tin site of Co3Sn2S2 was replaced with indium, was formed as a sample on a SrTiO3 (111) single crystal substrate. 1.5 A cobalt metal chip was attached to the surface of the sintered disk to serve as a target, and a sample was prepared by depositing a film using the above-mentioned sputtering device. The substrate temperature during deposition on the SrTiO3 (111) single crystal substrate was 400°C, and after deposition, a heat treatment was performed at 800°C in a vacuum. The composition of the sulfide contained in the obtained thin film (thickness 40 nm) was Co. 3-x X x Sn 2-y Y yS2 (Equation (4)) ((x=0,y=0), (x=0.11,y=0), (x=0.21,y=0), (x=0.44,y=0), (x=0,y=0.08), (x=0,y=0.24), (x=0,y=0.41), (x=0,y=0.60)). The shape of the sample was a rectangle with a length of 10 mm, a width of 5 mm, and a thickness of 300 μm.

[0056] The anomalous Nernst coefficient of the lateral thermoelectric conversion material constituting the lateral thermoelectric conversion element of the present invention was calculated as follows. FIG. 3 shows a schematic diagram of a sample formed to obtain the anomalous Nernst coefficient of a transverse thermoelectric conversion material and the measurement method thereof, as viewed from above. Sample 30 is a sample in which a thin film 33 is formed on the surface of a substrate 32. After the thin film 33 is formed, a pattern is formed by mechanically polishing the lower half of the surface of the substrate 32 using abrasive paper. Thermometers 36A and 36B are attached to the xy surface of the substrate 32 from which the thin film 33 has been removed by mechanical polishing in order to estimate the temperature gradient ▽T occurring in sample 30. Thermometer 36A is a Pt / Ti resistance thermometer. Thermometer 36B is a Pt / Ti resistance thermometer. The Pt / Ti resistance thermometer is formed by sputtering using a photoresist patterned by photolithography. The distance in the x direction between thermometer 36A and thermometer 36B is L. The distance in the other in-plane direction (y direction) of the thin film 33 is W.

[0057] One end of the deposited sample 30 in the x direction was heated by a heater, and the other end was brought into contact with a heat sink, generating a temperature gradient ▽T along the x direction of the sample 30. The temperature difference ΔT between the thermometers 36A and 36B at this time was measured. A magnetic field was applied in the direction (z direction) perpendicular to this temperature gradient ▽T (=ΔT / L), and a potential difference V xy At this time, the anomalous Nernst coefficient S xy is calculated using the following formula (5). S xy =(V xy / ΔT) × (L / W) (5) The electrical resistivity ρxx is the potential difference V in the in-plane direction (x direction) of the thin film 33 xx was obtained from.

[0058] The electrical resistivity (ρ xx ) was calculated and a graph was created. Figure 4 shows the results when x and y are (x=0,y=0), (x=0.11,y=0), (x=0.21,y=0), and (x=0.44,y=0) when X in formula (4) is Ni. Figure 5 shows the results when x and y are (x=0,y=0), (x=0,y=0.08), (x=0,y=0.24), (x=0,y=0.41), and (x=0,y=0.60) when Y in formula (4) is In.

[0059] As shown in Figure 4, when the measurement temperature was 150 K or less, the electrical resistivity (ρ xx ) was found to have an increasing tendency.

[0060] As shown in Figure 5, the electrical resistivity (ρ xx ) was found to have an increasing tendency.

[0061] At 200K, above the ferromagnetic transition temperature, a magnetic field of 1 tesla (T) or -1 T was applied in the perpendicular direction to the surface of the deposited thin film sample, then it was cooled to 50K and demagnetized to 0 T at 50K (cooling under a magnetic field). Since this thin film sample has perpendicular magnetic anisotropy, by performing this cooling under a magnetic field, it is possible to maintain a state at 0 T in which the magnetization directions are aligned in the thickness direction of the thin film (+z direction and -z direction in Figure 3) below the ferromagnetic transition temperature. In this state, the anomalous Nernst coefficient S xyA graph was created by antisymmetrically processing the data when the magnetization direction was aligned to the +z and -z directions in Figure 3. Figure 6 shows the results when x and y are (x=0,y=0), (x=0.11,y=0), (x=0.21,y=0), and (x=0.44,y=0) when X in formula (4) is Ni. Figure 7 shows the results when x and y are (x=0,y=0), (x=0,y=0.08), (x=0,y=0.24), (x=0,y=0.41), and (x=0,y=0.60) when Y in formula (4) is In.

[0062] As shown in Figure 6, the anomalous Nernst coefficient S xy In the case of no substitution (x=0, y=0), the sign is positive in the region below 140K, whereas when a part of the cobalt site is substituted with a certain amount of nickel (x=0.21), the anomalous Nernst coefficient S xy It was found that the sign of is negative. Anomalous Nernst coefficient S xy tends to decrease with increasing nickel substitution (x = 0.11, x = 0.21). When the nickel substitution is further increased (x = 0.44), the anomalous Nernst coefficient S xy increases again and takes a value close to 0, which is related to the decrease in the temperature region showing the anomalous Nernst effect due to the decrease in the ferromagnetic transition temperature. This result indicates that the nickel substitution modulates the electronic state near the Fermi level, which is involved in the anomalous Nernst effect. In addition, as is clear from FIG. 6, the anomalous Nernst coefficient S xy There are cases where the substitution amount has a positive sign and a negative sign. Therefore, by using the first thermoelectric conversion element 24 and the second thermoelectric conversion element 25 of the horizontal thermoelectric conversion element 20 of the present invention with a substitution amount with a positive sign and a substitution amount with a negative sign, a large anomalous Nernst effect can be obtained.

[0063] As shown in Figure 7, the anomalous Nernst coefficient S xyIn the case of no substitution (x=0, y=0), the sign is positive in the region below 140K, whereas when a part of the tin site is substituted with a certain amount of indium (y=0.08), the anomalous Nernst coefficient S xy It was found that the sign of is negative. Anomalous Nernst coefficient S xy tends to decrease with increasing indium substitution (y=0.24), but when the indium substitution is further increased (y=0.41, y=0.60), the anomalous Nernst coefficient S xy It was found that the anomalous Nernst coefficient S xy It was found that the temperature at which the ferromagnetic transition occurs is systematically decreased, which is considered to correspond to the decrease in the ferromagnetic transition temperature. These results indicate that the indium substitution modulates the electronic state near the Fermi level, which is involved in the anomalous Nernst effect. In addition, as is clear from FIG. 7, the anomalous Nernst coefficient S xy There are cases where the substitution amount has a positive sign and a negative sign. Therefore, by using the first thermoelectric conversion element 24 and the second thermoelectric conversion element 25 of the horizontal thermoelectric conversion element 20 of the present invention with a substitution amount with a positive sign and a substitution amount with a negative sign, a large anomalous Nernst effect can be obtained.

[0064] The above-mentioned magnetic field cooling operation was performed, and the anomalous Nernst coefficient S at a measurement temperature of 100 K was xy The results were calculated and a graph was created. The results are shown in Figure 8.

[0065] As shown in Figure 8, at 100 K, the anomalous Nernst coefficient S xy The sign of is positive when there is no substitution (x=0, y=0). When some of the cobalt sites are substituted with nickel, the anomalous Nernst coefficient S xy The value of x becomes smaller, and at x=0.21, the anomalous Nernst coefficient S xy It was found that the sign of is negative. In addition, when some of the tin sites are replaced with indium, the anomalous Nernst coefficient S xy The value of anomalous Nernst coefficient S becomes smaller at y=0.08, y=0.24, and y=0.41. xy It was found that the sign of is negative. Thus, in an environment of 100K, the anomalous Nernst coefficient S xy The value of changes with the substitution of nickel or indium, and the anomalous Nernst coefficient S xy It was found that the sign of reversed from positive to negative.

[0066] The above-mentioned magnetic field cooling operation was performed, and the anomalous Nernst coefficient S at a measurement temperature of 50 K was xy The results were calculated and plotted in a graph, as shown in Figure 9.

[0067] As shown in Fig. 9, at 50 K, the anomalous Nernst coefficient S xy The sign of is positive when there is no substitution (x=0, y=0). When some of the cobalt sites are substituted with nickel, the anomalous Nernst coefficient S xy The value of x becomes smaller, and at x=0.21, the anomalous Nernst coefficient S xy It was found that the sign of is negative. In addition, when some of the tin sites are replaced with indium, the anomalous Nernst coefficient S xy The value of anomalous Nernst coefficient S becomes smaller at y=0.24, y=0.41, and y=0.60. xy It was found that the sign of is negative. Thus, in a 50K environment, the anomalous Nernst coefficient S xy The value of changes with the substitution of nickel or indium, and the anomalous Nernst coefficient S xy It was found that the sign of reversed from positive to negative.

[0068] A lateral thermoelectric conversion element having a thermopile structure as shown in Figure 10 was fabricated and thermoelectric conversion measurements were performed. In the lateral thermoelectric conversion element in Figure 10, a shandite-type sulfide represented by formula (1) was used as the first thermoelectric conversion element, and a lateral thermoelectric conversion material in which x and y in formula (4) are (x=0, y=0.23) was used as the second thermoelectric conversion element. "1 pair A", "1 pair B", "1 pair C", and "3 pairs" in the figure indicate the positions where the electromotive force was measured. A temperature gradient was generated in the in-plane direction of the horizontal thermoelectric conversion element, and the electromotive force was measured at 140 K when the magnetic field perpendicular to the plane was changed from -3 Tesla to 3 Tesla. The results are shown in Figure 11.

[0069] As shown in FIG. 11, the electromotive force at 140 K when the magnetic field perpendicular to the surface was changed from -3 T to 3 T was similar for pair A, pair B, and pair C. This indicates that the first thermoelectric conversion element and the second thermoelectric conversion element in each pair exhibited performance comparable to that of the first thermoelectric conversion element and the second thermoelectric conversion element in the other pairs, and that the contact resistance between the first thermoelectric conversion element and the second thermoelectric conversion element in each pair was comparable to that between the first thermoelectric conversion element and the second thermoelectric conversion element in the other pairs. In other words, it was found that the first thermoelectric conversion element and the second thermoelectric conversion element in the fabricated lateral thermoelectric conversion element were uniform thin films, and the respective connection parts were well connected. Moreover, because the electromotive force of three pairs was about three times that of one pair, it was found that by increasing the number of pairs, the electromotive force can be increased accordingly. Furthermore, it was found that the sign of the electromotive force of the fabricated transverse thermoelectric conversion element can be changed depending on the direction of magnetization, and that even when the external magnetic field is returned to 0 T after applying an external magnetic field of ±3 T, more than 75% of the thermoelectromotive force component remains.

[0070] The above-mentioned cooling operation under a magnetic field was performed in the direction perpendicular to the surface of the lateral thermoelectric conversion element in Figure 10, and the electromotive force was measured when the temperature was raised from 50 K to 300 K at 0 T. The results are shown in Figure 12.

[0071] As shown in Figure 12, below 150 K, the electromotive force increases as the temperature decreases, reaching a maximum of approximately 130 μV at approximately 70 K, and below 70 K, the electromotive force decreases as the temperature decreases. Thus, it was found that the fabricated transverse thermoelectric conversion element has a thermoelectromotive force even in the absence of an external magnetic field, and that the thermoelectromotive force reaches a maximum value at a certain temperature. In addition, the electromotive force of three pairs was three times that of one pair at all temperatures, indicating that the electromotive force can be increased by increasing the number of pairs.

[0072] From the above results, it was found that by combining a transverse thermoelectric conversion material with a positive anomalous Nernst coefficient and a transverse thermoelectric conversion material with a negative anomalous Nernst coefficient, it is possible to produce an element that operates by magnetizing in a certain direction when a transverse thermoelectric conversion element as shown in Figure 10 is produced. This makes magnetization easier than an element produced by alternately arranging materials with the same anomalous Nernst coefficient and controlling the magnetization direction to be antiparallel, and simplifies the production of the element. It is also possible to provide an element with higher thermoelectric conversion performance per unit area than an element driven by connecting materials with the same anomalous Nernst coefficient with a conductor and magnetizing them in a certain direction. In addition, it is possible to provide an element that is more durable against damage due to thermal expansion and thermal contraction by using materials that show the anomalous Nernst effect of different material systems, compared to the case where materials with anomalous Nernst coefficients with different signs are arranged as shown in Figure 2. This is because the same material system has similar thermal expansion coefficients, so that electrical connection parts are less likely to break due to differences in thermal expansion coefficients. It was also found that when the sign of the anomalous Nernst coefficient is negative, the absolute value of the anomalous Nernst coefficient can be made larger by substituting a portion of the tin site with indium than by substituting a portion of the cobalt site with nickel. It was also confirmed that for each element substitution, there exists a substitution amount of nickel or indium (x=0.21, y=0.24) that can maximize the absolute value of the anomalous Nernst coefficient. [Explanation of symbols]

[0073] 20, 30... lateral thermoelectric conversion element, 22, 32... substrate, 23... power generation body, 24... first thermoelectric conversion element, 25... second thermoelectric conversion element, 33... thin film, 36A, 36B... thermometer

Claims

1. A transverse thermoelectric conversion material in which a part of the cobalt site of a shandite-type sulfide represented by the following formula (1) is substituted with a Group 10 element or a part of the tin site of the shandite-type sulfide is substituted with a Group 13 element, A transverse thermoelectric conversion material having an anomalous Nernst coefficient of the opposite sign to that of the shandite-type sulfide. Co 3 Sn 2 S 2 ... Formula (1)

2. The lateral thermoelectric conversion material according to claim 1 , wherein the Group 13 element is indium, and a portion of the tin sites are substituted with indium.

3. The lateral thermoelectric conversion material according to claim 1 , wherein the Group 10 element is nickel, and a portion of the cobalt sites are substituted with nickel.

4. A lateral thermoelectric conversion element in which a first thermoelectric conversion element including a lateral thermoelectric conversion material having a positive anomalous Nernst coefficient and a second thermoelectric conversion element including the lateral thermoelectric conversion material according to any one of claims 1 to 3 having a negative anomalous Nernst coefficient are alternately arranged and connected in a meandering wiring pattern.

5. A thermoelectric conversion module comprising the lateral thermoelectric conversion element according to claim 4.

Citation Information

Patent Citations

  • Thermoelectric generation device

    JP2014072256A

  • Thermoelectric body

    JP2016103535A

  • Thermoelectric conversion element and thermoelectric conversion device