Skin pack mount and skin pack package
A skin pack mount with controlled thickness and Taber stiffness addresses corner lifting issues, enabling effective packaging of heavy items and maintaining printing quality.
Patent Information
- Application Number
- JP2023047665
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 2024136524000003 
Figure 2024136524000004 
Figure 2024136524000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a skin pack liner and a skin pack package. [Background technology]
[0002] In the field of food packaging, skin packs are used to maintain the freshness and extend the shelf life of food, in which the food is placed on a tray and the tray and food are vacuum-packed using a barrier film. Skin packs, especially when used to package meat and other foods, can suppress dripping (water that escapes from food during storage), which can extend the expiration date and reduce food waste, and so they are increasingly being used.
[0003] In light of this, taking into consideration design aspects such as printability and reduced environmental impact, skin packs have been developed in which food is placed on a paper backing and then sealed in film, instead of plastic trays made of polystyrene or polypropylene.
[0004] For example, Patent Document 1 discloses a skin pack package in which a backing sheet has a base material, a release layer, and an adhesive layer, and a skin pack film is adhered to the base material via the adhesive layer, with the aim of providing a skin pack package that allows the packaged item to be easily removed.
[0005] Furthermore, Patent Document 2 discloses a skin pack package that has a base material including a paper layer, a film that covers the contents placed on the base material, and an easy-peel structure that joins the film to the base material so as to seal the contents, with the aim of providing a package that allows the contents to be easily removed. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2014-181075 A [Patent Document 2] International Publication No. 2021 / 039823 Summary of the Invention [Problem to be solved by the invention]
[0007] Skin pack packaging is generally intended for light items weighing up to several hundred grams. This is because when a heavy item is placed on a skin pack mount, the four corners of the mount rise up, which makes it impossible to accurately attach the film that covers the item to the mount, resulting in defective packaging. It is possible to reduce the lifting of the four corners of the mount by increasing its thickness and strength. However, if the mount is thick, it is difficult to apply uniform tension to the mount, and the mount meanders on the production line, so the problem of not being able to accurately attach the film to the mount remains unsolved. In addition, if the mount is thick, various problems arise when printing is performed to enhance the design. For example, printing machines that are widely available in general circulation are limited in the thickness of paper that can be printed, so they cannot print thick paper. In addition, it is difficult to wind thick mounts into a roll, so it is difficult to perform large-lot gravure printing.
[0008] An object of the present disclosure is to provide a backing for skin packs that has good runnability on an operating line and can withstand the packaging of heavy items. [Means for solving the problem]
[0009] As a result of extensive research, the present inventors have found that the above problems can be solved by setting the Taber stiffness and thickness of the mount within specific ranges. In other words, the gist of the present disclosure is as follows.
[0010] [1] A skin pack mount having a paper base layer, The thickness of the skin pack mount is 1.05 mm or less, The Taber stiffness of the skin pack mount in the longitudinal direction is 143 mN·m or more, A skin pack mount having a lateral Taber stiffness of 83 mN·m or more. [2] The tensile modulus of the skin pack mount in the longitudinal direction is 2.65 GPa or more, The skin pack mount according to [1], wherein the tensile modulus of elasticity in the lateral direction of the skin pack mount is 1.65 GPa or more. [3] The basis weight of the skin pack mount is 650 g / m 2 The above-mentioned skin pack mount described in [1] or [2]. [4] The mount for skin packs according to any one of [1] to [3], wherein the paper base layer is a laminate having a paper layer A, an adhesive layer A, and a paper layer B in this order, or a single paper. [5] The skin pack mount according to [4], wherein the adhesive layer A contains a polyolefin resin. [6] The mount for skin packs according to any one of [1] to [5], which has a thermoplastic resin layer on at least one surface of the paper base layer. [7] The skin pack mount according to [6], having an adhesive layer B between the paper base layer and the thermoplastic resin layer. [8] The skin pack mount according to [7], wherein the adhesive layer B contains a water-based adhesive. [9] The skin pack mount according to [8], wherein the water-based adhesive is at least one selected from the group consisting of acrylic adhesives, polyurethane adhesives, and isocyanate adhesives.
[10] A skin pack comprising the mount for a skin pack according to any one of [1] to [9], a storage item, and a resin film, A skin pack packaging body, in which the item to be contained is contained between the skin pack backing and the resin film. Effect of the Invention
[0011] According to the present disclosure, it is possible to provide a skin pack backing that has good runnability on an operating line and can withstand the packaging of heavy items. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic diagram illustrating a method for evaluating the deflection of a skin pack mount. [Diagram 2] FIG. 2 is a schematic diagram illustrating a method for evaluating the running properties of a skin pack mount. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] In this specification, the expressions "X to Y" and "X to Y" representing a numerical range mean a numerical range including the lower and upper limits, which are the endpoints, unless otherwise specified. When the lower limit and the upper limit of a numerical range are stated separately, the numerical range can be a combination of any lower limit and any upper limit.
[0014] <Skin pack mount> The first embodiment of the present invention is a skin pack mount (hereinafter sometimes simply referred to as "mount") having a paper base layer, which has a thickness of 1.05 mm or less, a longitudinal Taber stiffness of 143 mN·m or more, and a transverse Taber stiffness of 83 mN·m or more. The "machine direction" of the skin pack backing paper is the machine direction (MD) of the paper base material, and is the direction of the fibers. The "cross direction" of the skin pack backing paper is the direction perpendicular to the papermaking direction (CD).
[0015] By having the thickness of the skin pack backing paper be equal to or less than the above value, the necessary tension can be applied uniformly to the backing paper, which prevents the backing paper from meandering while running and improves running properties (printing running properties) on the production line. In addition, by setting the thickness of the skin pack mount to the above value or less, deterioration of print running properties can be prevented, and highly accurate printing can be achieved. In addition, printing can be performed using a commonly available printing machine. Furthermore, since both the vertical and horizontal Taber stiffnesses are equal to or greater than the above values, it is possible to suppress the deflection of the mount when an article is placed on the mount, making the mount for skin packs according to this embodiment suitable for packaging heavy articles.
[0016] In this specification, "heavy stored items" refers to items heavier than the stored items of about several hundred grams that are typically packaged in conventional skin packs, for example, items weighing 1 kg or more. In addition, in this specification, "a skin pack backing that can withstand the packaging of heavy stored items" and "a skin pack backing that is suitable for packaging heavy stored items" refer to a skin pack backing that is judged to be at a practical level when a 1 kg weight is placed on the skin pack backing and the deflection is evaluated, as shown in the examples described below.
[0017] (Thickness of skin pack backing paper) The thickness of the skin pack mount is 1.05 mm or less, and from the viewpoint of further improving print running properties, is preferably 1.03 mm or less, more preferably 1.00 mm or less, and even more preferably 0.98 mm or less. The thickness of the skin pack backing paper is not particularly limited, since the smaller the thickness, the better the printing runnability. However, in order to easily produce a backing paper with sufficient Taber stiffness, the thickness is preferably 0.80 mm or more, more preferably 0.85 mm or more, and even more preferably 0.90 mm or more.
[0018] The thickness of the skin pack mount is measured in accordance with JIS P 8118:2014 ("Paper and cardboard -- Test methods for thickness, density and specific volume", revised on November 20, 2014). If the skin pack mount has layers other than paper, such as an adhesive layer and a thermoplastic resin layer described below, the thickness of each layer is measured from an observation image of the cross section of the skin pack mount under an electron microscope (SEM), and the thickness of the skin pack mount is calculated from the measurement results. In other words, if the skin pack mount has layers other than paper, such as an adhesive layer and a thermoplastic resin layer described below, the thickness of the skin pack mount includes the thickness of those layers.
[0019] (Taber stiffness of skin pack backing paper) The Taber stiffness in the longitudinal direction of the skin pack mount is 143 mN·m or more, and from the viewpoint of further suppressing deflection of the mount, it is preferably 150 mN·m or more, and more preferably 155 mN·m or more. The Taber stiffness in the longitudinal direction of the skin pack mount is not particularly limited, as the greater the stiffness, the more the mount can be prevented from sagging. From the viewpoint of punching processability, however, the upper limit is preferably 210 mN·m or less, more preferably 190 mN·m or less, and even more preferably 170 mN·m or less.
[0020] The Taber stiffness in the lateral direction of the skin pack mount is 83 mN·m or more, preferably 88 mN·m or more, and more preferably 90 mN·m or more, in order to further suppress the deflection of the mount. Above. The higher the lateral Taber stiffness of the skin pack mount, the more the mount can be prevented from sagging; therefore, there is no particular upper limit to the Taber stiffness. From the viewpoint of punching processability, however, the upper limit is preferably 120 mN·m or less, and more preferably 110 mN·m or less.
[0021] The longitudinal Taber stiffness of the skin pack backing paper is measured using a Taber stiffness meter (e.g., Taber stiffness tester, manufactured by Toyo Seiki Seisakusho) in accordance with JIS P 8125-2:2017 ("Paper and cardboard-Bending resistance test methods-Part 2: Taber type tester method", enacted on March 21, 2017).
[0022] The ratio of the longitudinal Taber stiffness to the transverse Taber stiffness of the skin pack mount (hereinafter sometimes referred to as the "T / Y ratio of Taber stiffness") is not particularly limited, but is preferably 1.25 or more and 2.10 or less, more preferably 1.50 or more and 2.00 or less, and even more preferably 1.60 or more and 1.80 or less, in order to effectively suppress deflection of the mount.
[0023] The T / Y ratio of the skin pack backing paper can be adjusted by controlling the jet wire ratio (J / W ratio) during the production of the paper base layer. The J / W ratio is the ratio of the stock ejection speed (J) to the wire running speed (W) when the stock is ejected onto the wire from the inlet of the papermaking machine. If the J / W ratio is 1, the fibers are randomly oriented, and the more the stock ejection speed is increased or decreased from a J / W ratio of 1, the more the fibers are oriented vertically, and the greater the Taber stiffness in the vertical direction.
[0024] A method for adjusting the longitudinal and lateral Taber stiffnesses of the skin pack mount to fall within the above ranges will be described below.
[0025] Generally, the physical properties of paper follow the following formulas (I) to (III). From formula (I), it is effective to increase the tensile modulus of elasticity in order to improve the Taber stiffness without increasing the thickness of the skin pack liner more than necessary. From formula (II), it is effective to increase the tensile modulus of elasticity by increasing the density of the skin pack liner. However, from formula (III), in order to keep the thickness of the skin pack liner at least constant, it is inevitable that the basis weight of the skin pack liner will increase.
[0026] (paper stiffness) ∝ (paper thickness) 3 × (tensile modulus of paper) Formula (I) (Paper tensile modulus) ∝ (Paper density) Equation (II) (Paper density) = (paper basis weight) / (paper thickness) Formula (III)
[0027] Methods for adjusting the tensile modulus of the skin pack backing paper include, for example, a method of incorporating a specific amount of very small fibers into the paper base layer, a method of increasing the press line pressure in the wet press process (a process of compressing and squeezing the water from the wet paper after wire dewatering) during papermaking, a method of adjusting the disintegration freeness of the paper base material, and a method of adjusting the amount of internal additives such as paper strength enhancers. These methods may be used alone or in combination.
[0028] In the method of incorporating a specific amount of ultrafine fibers in the paper base layer, the ultrafine fibers penetrate into the gaps between the fibers of the pulp that constitute the paper base layer (if the paper base layer is an interleaf paper, the paper layer that constitutes the interleaf paper), thereby increasing the basis weight and density of the paper base layer and improving the tensile modulus, and as a result, the basis weight, density, and tensile modulus of the skin pack liner are also improved. The suitable amount of ultrafine fibers to be incorporated in the paper base layer in this method is as described below. In this specification, "ultrafine fibers" refers to fibers having a fiber length of 0.2 mm or less. The fiber length of pulp was measured using a fiber length measuring instrument (manufactured by Valmet Co., Ltd., Model FS-5 with UHD base unit) according to ISO 16065-2:2014 ("Pulp - Automatic Optical Analysis"). Measurements were performed in accordance with "Determination of Fiber Length by Polarization - Part 2: Non-polarized Methods" (issued January 14, 2014) will be done.
[0029] In the method of increasing the press line pressure in the wet press process during papermaking, the application of pressure to the wet paper and the decrease in the moisture content of the wet paper decrease the interfiber distance and strengthen the interfiber bonds, improving the tensile modulus of the finished paper base layer or paper layer, and as a result, the tensile modulus of the skin pack liner is also improved.
[0030] The method of adjusting the disintegration freeness of the paper base material is carried out by beating the pulp that is the raw material of the paper base material (when the paper base material layer is a slip sheet, the paper layer that constitutes the slip sheet). In general, the smaller the freeness value of the pulp, the higher the tensile modulus of the paper made. Note that disintegration freeness refers to the Canadian standard freeness measured in accordance with JIS P 8121-2:2012 ("Pulp - Disintegration methods - Part 1: Disintegration of chemical pulp", established on April 20, 2012) for pulp after papermaking, measured in accordance with JIS P 8121-2:2012 ("Pulp - Freeness test methods - Part 2: Canadian standard freeness method", established on June 20, 2012).
[0031] The specific ranges of the tensile modulus, basis weight, and density suitable for improving the Taber stiffness of the skin pack mount will be described below.
[0032] (Tensile modulus of elasticity of skin pack mount) The tensile modulus of elasticity in the longitudinal direction of the skin pack mount is preferably 2.65 GPa or more, more preferably 3.00 GPa or more, and even more preferably 3.15 GPa or more. The higher the longitudinal tensile modulus of the skin pack mount, the higher the longitudinal Taber stiffness, so there is no particular upper limit; however, from the viewpoint of punching processability, it is preferably 5.30 GPa or less, and more preferably 4.30 GPa or less.
[0033] The tensile modulus of elasticity in the lateral direction of the skin pack mount is preferably 1.65 GPa or more, and more preferably 2.00 GPa or more. The higher the lateral tensile modulus of the skin pack mount, the higher the lateral Taber stiffness, so there is no particular upper limit; however, from the viewpoint of punching processability, it is preferably 3.30 GPa or less, and more preferably 3.00 GPa or less.
[0034] The longitudinal tensile modulus and transverse tensile modulus of the skin pack backing paper are measured in accordance with JIS P 8113:2006 ("Paper and paperboard -- Test methods for tensile properties -- Part 2: Constant speed extension method", revised on December 20, 2006).
[0035] (Skin pack backing paper basis weight) The basis weight of the skin pack mount is preferably 650 g / m 2 More preferably, 680 g / m 2 More preferably, 710 g / m 2 More preferably, 750 g / m 2 More than 800g / m 2 That's all. The larger the basis weight of the skin pack backing paper, the higher the Taber stiffness in the longitudinal and transverse directions. Therefore, the upper limit of the basis weight is not particularly limited. However, from the viewpoint of punching processability and ease of manufacture, the upper limit is preferably 1,100 g / m 2 More preferably, it is 1,000 g / m 2 More preferably, 950 g / m 2Less than 900 g / m 2 The following is the result.
[0036] The basis weight of the skin pack liner is measured in accordance with JIS P 8124:2011 ("Paper and paperboard -- Determination of basis weight", revised March 22, 2011).
[0037] (Density of skin pack backing paper) The density of the skin pack mount is preferably 0.63 g / cm 3 More preferably, 0.75 g / cm 3 More preferably, 0.80 g / cm 3 That's all. The higher the density of the skin pack backing paper, the higher the Taber stiffness in the longitudinal and transverse directions. Therefore, the upper limit of the density is not particularly limited. From the viewpoints of punching processability and ease of manufacture, the density is preferably 1.05 g / cm 3 More preferably, it is 1.00 g / cm 3 More preferably, 0.95 g / cm 3 The following is the result.
[0038] The density of the skin pack liner is calculated by applying the thickness and basis weight of the skin pack liner measured as described above to formula (III).
[0039] (Paper base layer) The skin pack mount according to the present embodiment is not particularly limited in terms of the material and layer structure of the paper base layer, as long as it satisfies the above-mentioned thickness and Taber stiffness. The paper base layer may be a laminated paper including two or more paper layers, or a single paper including one paper layer.
[0040] When the paper base layer is a slip sheet, the number of paper layers contained in the slip sheet, the lamination method of each paper layer, the physical properties of each paper layer, etc. are not particularly limited, but a preferred slip sheet is one having paper layer A, adhesive layer A, and paper layer B in this order. The slip sheet having paper layer A, adhesive layer A, and paper layer B in this order may be a slip sheet consisting of only paper layer A, adhesive layer A, and paper layer B, or may be a slip sheet in which another paper layer is laminated via an adhesive layer. In this case, the same paper layer as paper layer A may be used as paper layer B. Furthermore, the same paper layer as paper layer A or paper layer B may be used as the other paper layer.
[0041] The basis weight of the paper layer A is preferably 300 g / m 2 More than 1,000g / m 2 Less than 400 g / m 2 More than 1,000g / m 2 More preferably, 450 g / m 2 More than 900g / m 2 Less than 500 g / m 2 More than 800g / m 2 The following is the result.
[0042] The density of the paper layer A is preferably 0.50 g / cm from the viewpoint of moldability. 3 More than 1.20g / cm 3 Less than or equal to 0.70 g / cm 3 More than 1.00g / cm 3 The following is the result.
[0043] The thickness of the paper layer A is preferably 0.30 mm or more and 1.20 mm or less, more preferably 0.40 mm or more and 1.10 mm or less, even more preferably 0.50 mm or more and 1.00 mm or less, and particularly preferably 0.60 mm or more and 0.95 mm or less.
[0044] The paper layer A may have a single layer structure or a multi-layer structure. From the viewpoint of productivity, the paper layer A preferably has a single layer structure. In addition, from the viewpoint of being able to arbitrarily adjust the raw material composition, basis weight, papermaking conditions, etc. of each layer, the paper layer A also preferably has a multi-layer structure. When the paper layer A has a multi-layer structure, the number of layers constituting the paper layer A is usually 2 to 10, preferably 3 to 9, more preferably 4 to 8, and even more preferably 4 to 6.
[0045] The basis weight of the paper layer B is preferably 50 g / m 2 More than 480g / m 2 Less than 60 g / m 2 More than 400g / m 2 More preferably, 100 g / m or less 2 More than 360g / m 2 Less than 120 g / m 2 More than 240g / m 2 The following is the result.
[0046] The density of the paper layer B is preferably 0.50 g / cm from the viewpoint of moldability. 3 More than 1.20g / cm 3 Less than or equal to 0.70 g / cm 3 More than 1.00g / cm 3 More preferably, 0.75 g / cm 3 More than 1.00g / cm 3 The following is the result.
[0047] The thickness of the paper layer B is preferably 0.05 mm or more and 0.70 mm or less, more preferably 0. The thickness is preferably 0.06 mm or more and 0.60 mm or less, and more preferably 0.07 mm or more and 0.50 mm or less.
[0048] The basis weight, density, and thickness of each paper layer are measured in the same manner as the basis weight, density, and thickness of the skin pack liner.
[0049] The paper layer B may be of a single layer construction or a multi-layer construction, but from the viewpoint of productivity, a single layer construction is preferable.
[0050] The paper layer A and the paper layer B are not particularly limited as long as they are commonly used papers, and are preferably papers whose main component is plant-derived pulp, and more preferably papers whose main component is wood pulp. Specific examples of the paper layer A and the paper layer B include kraft paper, fine paper, (white) paperboard, base paper for paper containers, milk carton base paper, cup base paper, liner paper, coated paper, one-sided gloss paper, glassine paper, and graphene paper. Among these, the paper layer A and the paper layer B are preferably selected from the group consisting of kraft paper, fine paper, (white) paperboard, base paper for paper containers, cup base paper, and one-sided gloss paper, and from the viewpoint of rigidity, it is more preferable that the (white) paperboard is selected from the group consisting of high-grade paperboard, special paperboard, cup base paper, and kraft paper. Examples of the kraft paper include bleached kraft paper, unbleached kraft paper, and one-sided gloss bleached kraft paper. Among these, the kraft paper is preferably selected from the group consisting of bleached kraft paper and one-sided gloss bleached kraft paper from the viewpoint of printability and hygiene.
[0051] As described above, the pulp constituting the paper layer A and the paper layer B is preferably wood pulp, and more preferably kraft pulp. Kraft pulp includes hardwood kraft pulp (LKP) and softwood kraft pulp (NKP) based on the difference in raw materials. As hardwood kraft pulp (LKP), hardwood bleached kraft pulp (LBKP) is preferable, and as softwood kraft pulp (NKP), softwood bleached kraft pulp (NBKP) is preferable. In addition, as the difference in processing state, bleached kraft pulp (BKP), unbleached kraft pulp (UKP), and oxygen bleached kraft pulp (OKP) are mentioned, and from the viewpoint of printability, bleached kraft pulp (BKP) is preferable. Among these, the pulp is preferably one or more selected from the group consisting of hardwood kraft pulp (LKP) and softwood kraft pulp (NKP), and more preferably a mixture of hardwood kraft pulp (LKP) and softwood kraft pulp (NKP). In the mixture, the mass ratio of hardwood kraft pulp (LKP) to softwood kraft pulp (NKP) (LKP / NKP) is not particularly limited as long as it is a ratio used in general paper, and is preferably 1 / 99 to 99 / 1, more preferably 30 / 80 to 99 / 1, and even more preferably 40 / 60 to 99 / 1.
[0052] It is preferable that either or both of the pulp constituting the paper layer A and the pulp constituting the paper layer B contain a specific amount of very small fibers having a fiber length of 0.2 mm or less.
[0053] From the standpoint of improving density and basis weight, the amount (number) of ultrafine fibers contained in the pulp constituting each paper layer is preferably 10.0% or more and 27.0% or less, more preferably 13.0% or more and 23.0% or less, and even more preferably 16.0% or more and 20.0% or less.
[0054] The amount of microfibers in each layer is calculated using a fiber length measuring instrument (Valmet, Model FS-5 with UHD base unit). More specifically, the same instrument is used to measure the fiber length according to ISO 16065-2:2014 ("Pulp - Determination of fiber length by automated optical analysis - Part 2: Unbiased analysis"). The photograph was taken within a measurement cell with a depth of field of 0.5 mm in accordance with the "Optical Measurement Method" published on January 14, 2014. By shading the material, each fiber is detected and its length is measured, and the percentage of extremely small fibers with a fiber length of 0.2 mm or less is calculated from the results.
[0055] The Oken smoothness (JIS P 8155:2010) of the paper layer A and the paper layer B is preferably 5 seconds or more, more preferably 10 seconds or more and 1,000 seconds or less. From the viewpoint of printability, the 75° gloss of the paper layer A and the paper layer B is preferably 5% or more, more preferably 10% or more and 70% or less.
[0056] The adhesive layer A that bonds the paper layer A and the paper layer B may be any layer made of a material having adhesive properties, but preferably contains a thermoplastic resin. By using a thermoplastic resin, it is possible to easily obtain an interleaving paper by coating at least one paper layer with a heated and melted resin and then laminating the other paper layer.
[0057] The thermoplastic resin preferably contains one or more resins selected from the group consisting of polyolefin-based resins, polyester-based resins, polylactic acid, styrene-based resins, and acrylic-based resins, and more preferably contains a polyolefin-based resin. Examples of polyolefin resins include polyethylene (low density polyethylene (LDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), linear low density polyethylene (LLDPE), etc.), polypropylene (PP), polymethylpentene, etc. Among these, the polyolefin resin is preferably one or more types selected from the group consisting of polyethylene and polypropylene, and from the viewpoints of extrusion lamination properties and ease of coating on the paper layer, it is more preferably one or more types selected from the group consisting of LDPE and MDPE.
[0058] The adhesive layer A may be formed by laminating the paper layer A and the paper layer B using an adhesive described later. The adhesive is not particularly limited, and may be a water-based adhesive, a solvent-based adhesive, a UV-based adhesive, or the like. Of these, the adhesive used in the adhesive layer A is preferably a water-based adhesive. The water-based adhesive is preferably one or more selected from the group consisting of an acrylic adhesive, a polyurethane adhesive, and an isocyanate adhesive, and is more preferably an acrylic adhesive in terms of ease of control of adhesive strength and excellent heat resistance.
[0059] The amount of the adhesive layer A per unit area is not particularly limited, but is preferably 1.0 g / m 2 More than 50.0g / m 2 Less than 1.0 g / m, more preferably 1.0 g / m 2 More than 20.0g / m 2When forming the adhesive layer A, it is preferable to coat the adhesive on the paper layer A or the paper layer B so that the solid content is in this amount.
[0060] The adhesive layer A may be formed as a single layer of a single resin, or may be formed as a single layer of a mixture of multiple resins, or may be formed as multiple layers made of the same or different types of resins. The thickness of the adhesive layer A is not particularly limited, but from the viewpoint of moldability, it is preferably 0.005 mm or more and 0.100 mm or less, and more preferably 0.010 mm or more and 0.050 mm or less.
[0061] When the paper base layer is a single sheet, the above-mentioned paper layer A is preferably used as the single sheet.
[0062] (thermoplastic resin layer) The skin pack mount according to this embodiment may be composed of only a paper base layer, but may have a thermoplastic resin layer on at least one side of the paper base layer. The thermoplastic resin layer protects the surface of the skin pack mount from stored items such as food, and protects the stored items from external stimuli such as oxygen. In addition, for example, when the stored items are sandwiched between the skin pack mount and a resin film, the thermoplastic resin layer adheres to the resin film. It has a role to play.
[0063] The thermoplastic resin layer may be a single layer of a thermoplastic resin or a laminate containing a thermoplastic resin, but is preferably a laminate containing a barrier layer, and is particularly preferably a laminate having a barrier layer between thermoplastic resin layers, such as "thermoplastic resin layer / barrier layer / thermoplastic resin layer." The thermoplastic resin layer may also be a laminate layer.
[0064] When the thermoplastic resin layer is a laminate having a barrier layer, the barrier layer is not particularly limited as long as it is a layer that can barrier oxygen and / or water vapor, and may have a single layer structure or a multilayer structure of two or more layers.
[0065] Specifically, the resin forming the barrier layer is preferably one or more selected from the group consisting of polyamide resins, polyvinyl alcohol, ethylene-vinyl alcohol copolymers (EVOH), and polyvinylidene chloride resins, and more preferably one or more selected from the group consisting of polyamide resins, polyvinyl alcohol, and ethylene-vinyl alcohol copolymers. The polyamide resin is preferably an aromatic polyamide, and more preferably polyamide MXD6. The barrier layer may further contain one or more other resins such as biomass resins and biodegradable resins. Alternatively, the barrier layer may be a metal layer.
[0066] The thickness of the barrier layer is not particularly limited, but is preferably 0.003 mm or more and 0.100 mm or less, more preferably 0.004 mm or more and 0.050 mm or less, and further preferably 0.005 mm or more and 0.030 mm or less.
[0067] When the thermoplastic resin layer is a laminate layer, the laminate layer is not particularly limited, but is preferably a layer that can impart waterproof and stain-resistant properties to the skin pack mount.
[0068] The thermoplastic resin used in the laminate layer is not particularly limited as long as it can be laminated to the paper base layer, and may be appropriately selected from known thermoplastic resins. Specific examples include polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polylactic acid, and polybutylene succinate; polyolefin-based resins such as polyvinyl chloride, polyvinylidene chloride, polybutene, polybutadiene, ethylene-vinyl acetate copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, and polymethylpentene; polycarbonate; polyurethane; polyamide; polyacrylonitrile; and poly(meth)acrylate.
[0069] Among these thermoplastic resins, the thermoplastic resin used in the laminate layer is preferably one or more selected from the group consisting of polyethylene (PE) and polypropylene (PP) because of its excellent extrusion lamination properties and barrier properties. In addition, the PE is preferably one or more selected from the group consisting of low density polyethylene (LDPE) and medium density polyethylene (MDPE) because of its excellent extrusion lamination properties and foaming properties.
[0070] The total thickness of the thermoplastic resin layer is not particularly limited, but is preferably 0.001 mm or more and 0.200 mm or less, more preferably 0.005 mm or more and 0.100 mm or less, still more preferably 0.010 mm or more and 0.080 mm or less, and particularly preferably 0.010 mm or more and 0.050 mm or less.
[0071] (Adhesive layer B) The skin pack mount according to this embodiment has an adhesive layer B between a paper base layer and a thermoplastic resin layer, and the thermoplastic resin layer is laminated on one or both surfaces of the paper base layer via the adhesive layer B. When the surface of the thermoplastic resin layer has adhesiveness, the thermoplastic resin layer may be directly bonded to the surface of the paper base layer, but in order to prevent peeling during transportation and display, it is preferable to have an adhesive layer B between the paper base layer and the thermoplastic resin layer.
[0072] The adhesive used in the adhesive layer B is not particularly limited, but is preferably a resin-based adhesive suitable for dry lamination and wet lamination, and for example, a water-based adhesive, a solvent-based adhesive, a UV-based adhesive, etc. can be used. Among these, the adhesive used in the adhesive layer B is preferably a water-based adhesive. In addition, the water-based adhesive is preferably one or more selected from the group consisting of an acrylic adhesive, a polyurethane adhesive, and an isocyanate adhesive, and an acrylic adhesive is more preferable in terms of ease of control of adhesive strength and excellent heat resistance.
[0073] The amount of adhesive layer B per unit area is not particularly limited, but is preferably 1 g / m2 More than 50g / m 2 Less than 1 g / m, more preferably 2 More than 20g / m 2 The adhesive is preferably applied to the paper substrate layer or the thermoplastic resin layer so that the solid content is in this amount when forming the adhesive layer B. For coating, it is preferable to use a coating liquid containing an adhesive, and it is more preferable to use a mixed coating liquid in which a curing agent is mixed with a coating liquid containing an adhesive.
[0074] The thickness of the adhesive layer B is not particularly limited, but from the viewpoint of moldability, it is preferably 0.005 mm or more and 0.100 mm or less, and more preferably 0.008 mm or more and 0.030 mm or less.
[0075] (other layers) The skin pack mount according to this embodiment may have other layers as long as the effects of the present invention are not impaired. For example, the skin pack mount may have a printed layer made of ink formed by offset printing on one or both sides of a paper base layer. When the skin pack mount has a printed layer, it is preferable to provide a thermoplastic resin layer on the surface of the printed layer via an adhesive layer B.
[0076] <Manufacturing method for skin pack mount> The method for producing the skin pack mount according to the present embodiment is not particularly limited, and any known method can be used. An example of the production method is shown below.
[0077] (Preparation of paper base layer) First, a paper stock containing pulp is made into paper, and the obtained paper is laminated with an adhesive as necessary to produce a paper base layer.
[0078] When a specific amount of very small fibers is to be contained in the pulp, it is preferable to add very small fibers obtained by pulping hardwood kraft pulp such as bleached hardwood kraft pulp with a known pulping device such as a cutter mill when preparing the pulp, since this makes it easier to control the amount of very small fibers in the pulp. In addition, when preparing the pulp, internal additives may be added to the pulp, such as sizing agents, fillers, paper strength agents, retention aids, pH adjusters, drainage improvers, water resistance agents, softeners, antistatic agents, defoamers, slime control agents, dyes, and pigments.
[0079] In the papermaking process, a known wet papermaking machine can be appropriately selected and used, such as a Fourdrinier papermaking machine, a gap former type papermaking machine, a cylinder papermaking machine, and a short wire papermaking machine. In addition, in papermaking, it is preferable to adjust the J / W ratio so as to obtain a skin pack backing paper having a T / Y ratio of the desired Taber stiffness.
[0080] The paper produced by the papermaking machine is preferably transported on a felt and dried in a dryer. A multi-stage cylinder dryer may be used as a pre-dryer before drying in the dryer.
[0081] The paper obtained as described above may be surface-treated with a calendar to make the thickness and profile uniform. For the calendar treatment, a known calendaring machine can be appropriately selected and used.
[0082] The paper obtained as described above is used as the paper base layer when the paper base layer is a single sheet, and is used as a paper layer constituting the interleaf when the paper base layer is an interleaf. When the paper base layer is an interleaf having paper layer A, adhesive layer A, and paper layer B in this order, the interleaf can be obtained by melt-extrusion coating one side of paper layer A with a thermoplastic resin that will become adhesive layer A, and laminating paper layer B to this coated surface.
[0083] (Formation of Thermoplastic Resin Layer) When a thermoplastic resin layer is provided on one or both surfaces of the paper base layer, the thermoplastic resin layer may be directly adhered to the paper base layer, or may be adhered to the paper base layer via an adhesive layer B. In the latter case, it is preferable to apply a coating liquid containing an adhesive onto the surface of the paper base layer, and then laminate the thermoplastic resin layer on the surface of the paper base layer via the adhesive layer B. In this case, a film may be attached to the paper base layer as the thermoplastic resin layer.
[0084] When the thermoplastic resin layer includes a laminate having a barrier layer in the middle of the thermoplastic resin layers, such as "thermoplastic resin layer / barrier layer / thermoplastic resin layer", the thermoplastic resin may be melt-extrusion coated onto the surface of the paper base layer, a laminate film having a barrier layer in the middle of the thermoplastic resin layers is placed thereon, and the surface of the melt-extrusion coated thermoplastic resin and the surface of the thermoplastic resin layer of the laminate film are heated and fused to form the thermoplastic resin layer. By laminating a film to the paper base layer using this method, a skin pack mount having a thermoplastic resin layer can also be produced.
[0085] When the thermoplastic resin layer is a laminate layer, the lamination method of the laminate layer is not particularly limited, and may be appropriately selected from known methods such as melt extrusion, melt casting, and calendaring.
[0086] (processing) The skin pack mount obtained as described above may be cut to an appropriate size, taking into consideration the size and shape of the contents, and suitability for transportation and display. Cutting is preferably performed by punching, from the viewpoint of efficiently obtaining skin pack mounts of the same shape. The punching process is preferably carried out using a high-speed automatic punching machine, a flat-bed punching machine, or a rotary punching machine, and more preferably a high-speed automatic punching machine. By carrying out the punching process using a high-speed automatic punching machine or a flat-bed punching machine, skin pack mounts having shapes such as a rectangle, a rounded rectangle, an ellipse, and the like can be easily and efficiently obtained.
[0087] <Skin pack packaging> A second embodiment of the present invention is a skin pack package having the above-mentioned skin pack mount, a storage item, and a resin film, with the storage item being stored between the skin pack mount and the resin film. The skin pack package according to this embodiment is preferably one that hermetically stores the storage item.
[0088] The resin film can be appropriately selected depending on the type and shape of the stored item. However, since it is necessary to adhere the contained items to the thermoplastic resin layer of the skin pack mount, the resin film preferably has excellent adhesiveness and is also peelable when the contained items are removed. Therefore, the resin film is preferably made of the thermoplastic resin used in the above-mentioned thermoplastic resin layer, and more preferably has a barrier layer when the contents are food or the like. As the barrier layer, the barrier layer used in the above-mentioned thermoplastic resin layer is preferably used.
[0089] There are no restrictions on the items to be stored, and examples include food, daily necessities, etc., but preferably, since the items to be stored can be sealed, it is suitable for storing fresh foods such as vegetables, meat, fresh fish, and other processed foods. EXAMPLES
[0090] The present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.
[0091] <Preparation of paper layer A-1> 75 parts by mass of bleached hardwood kraft pulp (LBKP) beaten to 450 mL Canadian Standard Freeness (CSF), 5 parts by mass of bleached softwood kraft pulp (NBKP) beaten to 600 mL CSF, and 20 parts by mass of ultrafine fibers were mixed and beaten to obtain a pulp slurry. The ultrafine fibers were obtained by mixing and beating a dry sheet of LBKP with a cutter mill (HORAI Corporation, model number: HA8 2542 The pulp was mechanically crushed using a pulp mill (Made by Aikawa Iron Works Co., Ltd., model number: MAX-F700) and a fraction with a pulp fiber length of 0.2 mm or less was separated. 0.35 parts by mass (solid content equivalent) of aluminum sulfate was added to 100 parts by mass of the obtained pulp slurry to prepare 500 mL of CSF stock. Using this stock, paper was made on a five-layer short-wire papermaking machine with the same set basis weight for all five layers (surface layer, undersurface layer, middle layer, underback layer, and back layer). During papermaking, the press line pressure was adjusted to a basis weight of 600 g / m 2 , thickness 0.73mm, density 0.83g / cm 3 Thus, a paper layer A-1 was obtained.
[0092] <Preparation of paper layer A-2> The amount of paper material and press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 620 g / m 2 A paper layer A-2 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.75 mm.
[0093] <Preparation of paper layer A-3> The amount of paper material and press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 660 g / m 2 A paper layer A-3 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.80 mm.
[0094] <Preparation of paper layer A-4> The amount of paper material and the press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 660 g / m 2 A paper layer A-4 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.75 mm.
[0095] <Preparation of paper layer A-5> The amount of paper material and the press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 570 g / m 2 A paper layer A-5 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.75 mm.
[0096] <Preparation of paper layer A-6> The amount of paper material and press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 480 g / m 2A paper layer A-6 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.82 mm.
[0097] <Preparation of paper layer A-7> The amount of paper material and press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 765 g / m 2 A paper layer A-7 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.93 mm.
[0098] <Preparation of paper layer A-8> The amount of paper material and press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 680 g / m 2 A paper layer A-8 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.82 mm.
[0099] <Preparation of paper layer A-9> The amount of paper material and the press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 500 g / m 2 A paper layer A-9 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.60 mm.
[0100] <Preparation of paper layer A-10> The amount of paper material and the press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 380 g / m 2 A paper layer A-10 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.46 mm.
[0101] <Preparation of paper layer A-11> The amount of paper material and the press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 580 g / m 2 A paper layer A-11 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.70 mm.
[0102] <Preparation of paper layer A-12> The J / W ratio during papermaking was adjusted so that the T / Y ratio of the Taber stiffness of the skin pack liner of Comparative Example 2 obtained by laminating with the paper layer B-1 was 2.0, and the amount of paper material and the press line pressure during papermaking were adjusted so that the basis weight of the paper layer was 620 g / m 2 A paper layer A-12 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.75 mm.
[0103] <Preparation of paper layer A-13> The J / W ratio during papermaking was adjusted so that the T / Y ratio of the Taber stiffness of the skin pack liner of Comparative Example 3 obtained by laminating with the paper layer B-1 was 1.2, and the amount of paper material and the press line pressure during papermaking were adjusted to give a basis weight of the paper layer of 620 g / m 2 A paper layer A-13 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.75 mm.
[0104] <Preparation of paper layer A-14> The amount of paper material and the press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 700 g / m 2 A paper layer A-14 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.84 mm.
[0105] <Preparation of paper layer A-15> The amount of paper material and the press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 520 g / m 2 A paper layer A-15 was obtained in the same manner as the paper layer A-1, except that the thickness was 0.75 mm.
[0106] <Preparation of paper layer A-16> The amount of paper material and the press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 460 g / m 2 A paper layer A-16 was obtained in the same manner as paper layer A-1, except that the thickness was 0.82 mm.
[0107] <Preparation of paper layer B-1> 50 parts by mass of hardwood bleached kraft pulp (LBKP) beaten into 520 mL of CSF, and 50 parts by mass of softwood bleached kraft pulp (NBKP) beaten into 570 mL of CSF were mixed and beaten to obtain a pulp slurry. For 100 parts by mass of the obtained pulp slurry, 0.75 parts by mass (solid content equivalent) of cationic starch (Kate F, manufactured by Oji Cornstarch Co., Ltd.), 1.0 part by mass of rosin emulsion (SPN, manufactured by Arakawa Chemical Industries Co., Ltd.), and anion-modified 0.33 parts by mass of polyacrylamide (Polystron, manufactured by Arakawa Chemical Industries, Ltd.) was added to prepare a paper stock. This paper stock was used to make paper on a Fourdrinier paper machine equipped with a Yankee dryer. The paper obtained was smoothed with a calendar to obtain a paper with a basis weight of 120 g / m. 2 , thickness 0.15mm, density 0.80g / cm 3 Thus, a paper layer B-1 was obtained.
[0108] <Preparation of paper layer B-2> The amount of paper material and the press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 60 g / m 2 A paper layer B-2 was obtained in the same manner as the paper layer B-1, except that the thickness was 0.075 mm.
[0109] <Preparation of paper layer B-3> The amount of paper material and the press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 240 g / m 2 A paper layer B-3 was obtained in the same manner as paper layer B-1, except that the thickness was 0.30 mm.
[0110] <Preparation of paper layer B-4> The amount of paper material and the press line pressure during papermaking were adjusted to achieve a paper layer basis weight of 360 g / m 2 A paper layer B-4 was obtained in the same manner as paper layer B-1, except that the thickness was 0.45 mm.
[0111] <Example 1> One side of paper layer A-1 was melt-extrusion coated with MDPE (manufactured by ENEOS NUC Corporation, model number: 8010) to a dry film thickness of 0.02 mm, and paper layer B-1 was attached to the coated surface to obtain a two-layer paper base layer. After that, printing layers were formed on both sides using an offset printing machine. Next, a PE / EVOH / PP three-layer film A (manufactured by Mitsubishi Chemical Corporation, Diamiron YF1966, thickness 0.04 mm) was applied to the PP layer side with a coating amount of 10 g / m2 after heat drying. 2An adhesive layer was formed by applying a coating liquid made by mixing 100 parts by mass of a water-based acrylic adhesive (EM-575, manufactured by Arakawa Paint Co., Ltd.) and 3 parts by mass of a hardener (EM-550K, manufactured by Arakawa Paint Co., Ltd.) so that the adhesive layer and the paper base layer were adjacent to each other by dry lamination to form a skin pack. A mount was prepared.
[0112] <Examples 2 to 6, 8 to 10> A skin pack mount was prepared in the same manner as in Example 1, except that the paper layer, adhesive layer, and thermoplastic resin layer were changed to those shown in Table 1.
[0113] <Example 7> The coating amount after heat drying was 10 g / m on the PP layer side of film A (Mitsubishi Chemical Corporation, Diamiron YF1966, thickness 0.04 mm) with a PE / EVOH / PP three-layer structure. 2 An adhesive layer was formed by applying a coating liquid made by mixing 100 parts by mass of a water-based acrylic adhesive (EM-575, manufactured by Arakawa Paint Co., Ltd.) with 3 parts by mass of a hardener (EM-550K, manufactured by Arakawa Paint Co., Ltd.) so that the adhesive layer was formed as follows: A skin pack mount was produced by dry laminating this adhesive layer and the paper base layer A-7 together.
[0114] <Example 11> A skin pack backing was prepared in the same manner as in Example 1, except that one side of paper layer A-2 was melt-extrusion coated with LDPE (manufactured by Japan Polyethylene Corporation, model number: LC522) to a dry film thickness of 0.02 mm, and paper layer B-1 was laminated to the coated surface to obtain a two-layer paper base layer.
[0115] <Example 12> One side of the paper layer A-2 is melt-extrusion coated with HDPE (manufactured by Japan Polyethylene Co., Ltd., model number: HJ580N) to a dry film thickness of 0.02 mm, and the paper layer is applied to the coated surface. A skin pack mount was produced in the same manner as in Example 1, except that B-1 was laminated to obtain a two-layer paper base layer.
[0116] <Example 13> A skin pack backing was prepared in the same manner as in Example 1, except that one side of paper layer A-2 was melt-extrusion coated with PP (manufactured by Sun Allomer Co., Ltd., model number: PHA03A) to a dry film thickness of 0.02 mm, and paper layer B-1 was laminated to the coated surface to obtain a two-layer paper base layer.
[0117] <Example 14> A skin pack mount was prepared in the same manner as in Example 2, except that the coating liquid applied to the PP layer side of Film A was changed to a polyurethane adhesive (manufactured by Mitsui Chemicals, Inc., model number: Takelac A310).
[0118] <Example 15> A skin pack mount was prepared in the same manner as in Example 2, except that the coating liquid applied to the PP layer side of Film A was changed to a mixture of 100 parts by mass of an isocyanate-based adhesive (manufactured by DIC Corporation, model number: DiCdry LX-500) and 10 parts by mass of DiCdry KW-75.
[0119] <Example 16> One side of the paper layer A-2 was coated with MDPE by melt extrusion coating to a dry thickness of 0.02 mm, and the paper layer B-1 was laminated to the coated side. After that, a printing layer was formed on both sides with an offset printing machine to produce a skin pack backing.
[0120] <Example 17> One side of the paper layer A-2 was coated with MDPE (manufactured by ENEOS NUC Corporation, model number: 8010) by melt extrusion coating to a dry thickness of 0.02 mm, and the paper layer B-1 was attached to the coated surface to obtain a two-layer paper base layer. Then, PP was melt extrusion coated on the paper layer A-2 of the paper base layer to a dry thickness of 0.04 mm to produce a skin pack backing paper.
[0121] <Example 18> One side of paper layer A-2 was coated with MDPE (manufactured by ENEOS NUC Corporation, model number: 8010) by melt extrusion coating to a dry thickness of 0.02 mm, and paper layer B-1 was attached to the coated surface to obtain a two-layer paper base layer. Then, MDPE was melt extrusion coated on top of paper layer A-2 of the paper base layer to a dry thickness of 0.04 mm to produce a skin pack backing.
[0122] <Example 19> One side of the paper layer A-2 was coated with MDPE (manufactured by ENEOS NUC Corporation, model number: 8010) by melt extrusion coating to a dry film thickness of 0.02 mm, and the paper layer B-1 was laminated to the coated surface to obtain a two-layered paper base layer. Next, a three-layered film B (manufactured by Mitsubishi Chemical Corporation, model number: Diamiron F001) of PP / EVOH / PP was coated with 10 g / m2 of MDPE after heat drying. 2 An adhesive layer was formed by applying a coating liquid made by mixing 100 parts by mass of a water-based acrylic adhesive (EM-575, manufactured by Arakawa Paint Co., Ltd.) with 3 parts by mass of a hardener (EM-550K, manufactured by Arakawa Paint Co., Ltd.) so that the adhesive layer and the paper base layer were adjacent to each other by dry lamination to produce a skin pack mount.
[0123] <Comparative Examples 1 to 6> A skin pack mount was prepared in the same manner as in Example 1, except that paper layer A shown in Table 1 was used instead of paper layer A-1.
[0124] The physical properties of the skin pack mounts prepared in the Examples and Comparative Examples were measured and evaluated by the following methods. The results are shown in Tables 1 and 2.
[0125] [Basic weight] The basis weights of the paper layer, the paper base layer, and the skin pack backing paper were measured in accordance with JIS P 8124:2011 ("Paper and paperboard -- Determination of basis weight," revised March 22, 2011).
[0126] [Thickness] The thicknesses of the paper layer, the paper base layer, and the skin pack liner were measured in accordance with JIS P 8118:2014 ("Paper and paperboard -- Test methods for thickness, density and specific volume", revised on November 20, 2014). When the skin pack liner had an adhesive layer and / or a thermoplastic resin layer, the thickness of each layer was measured from the cross-section of the skin pack liner observed under a scanning electron microscope (SEM).
[0127] [Amount of ultrafine fibers] Using a fiber length measuring instrument (Valmet, Model FS-5 with UHD base unit) and photographing within a measurement cell with a depth of field of 0.5 mm in accordance with ISO 16065-2:2014, each fiber was detected and its length was measured, and the percentage of extremely small fibers with a fiber length of 0.2 mm or less in the paper layer was calculated from the results. The content (number) of ultrafine fibers in the pulp constituting the paper layers A-1 to A-16 was 23%. The content (number) of ultrafine fibers in the pulp constituting the paper layers B-1 to B-4 was 15%.
[0128] [Taber stiffness] The Taber stiffness in the longitudinal and transverse directions of the skin pack mounts prepared in the Examples and Comparative Examples was measured using a Taber stiffness meter (a digital Taber stiffness tester manufactured by Toyo Seiki Seisakusho) in accordance with JIS P 8125-2:2017 ("Paper and cardboard -- Bending resistance test methods -- Part 2: Taber type testing machine method", enacted on March 21, 2017).
[0129] [Tensile modulus] The tensile modulus in the longitudinal and transverse directions of the skin pack mounts prepared in the examples and comparative examples was measured in accordance with JIS P 8113:2006 ("Paper and cardboard -- Test methods for tensile properties -- Part 2: Constant speed extension method", revised on December 20, 2006).
[0130] [Deflection evaluation] The skin pack mounts obtained in the Examples and Comparative Examples were punched to obtain rectangular evaluation paper pieces measuring 330 mm in length (MD) × 290 mm in width (CD). The punching was performed using an automatic flat-platen punching machine (Carton Master AP-1300-TSG-8, manufactured by Asahi Machinery Co., Ltd.) at a rate of 6,000 sheets / hour.
[0131] As shown in Fig. 1(a), the evaluation paper piece 11 was placed on four square stands 13 so that the four corners of the evaluation paper piece 11 were placed on each stand by 1 cm x 1 cm. Then, as shown in Fig. 1(b) and (c), two weights 15 of 500 g (cuboids of 200 mm length x 70 mm width x 30 mm thickness) were placed on the center of the evaluation paper piece 11, and the degree of deflection was confirmed. The number of centimeters that the evaluation paper piece 11 sunk in both the vertical and horizontal directions was measured, and the evaluation was made based on the larger deflection according to the following criteria. 3 or more was considered a usable level, and 2 or less was considered a poor evaluation.
[0132] Evaluation criteria 4: Deflection is 2.50 cm or less 3: Deflection is 2.51~3.50cm 2: Deflection is 3.51~4.00cm 1: Deflection is 4.01 cm or more
[0133] [Drivability evaluation] The skin pack mounts prepared in the Examples and Comparative Examples were punched to obtain rectangular evaluation paper pieces measuring 330 mm in length (MD) × 290 mm in width (CD). The punching was performed using an automatic flat-platen punching machine (Carton Master AP-1300-TSG-8, manufactured by Asahi Machinery Co., Ltd.) at a rate of 6,000 sheets / hour.
[0134] Using an offset printer, cross lines (line width: 0.1 mm) were printed as register marks on a piece of cardboard 500 μm thick. The register marks were printed in black, indigo blue, yellow, and red in that order, and the printing conditions of the offset printer were set so that all the register marks overlapped.
[0135] Using an offset printing machine, black, indigo, yellow, and red cross lines (line width: 0.1 mm) were printed as register marks on the evaluation paper pieces under the above printing conditions. For each color of printed register mark, the distance between the intersection of the black cross line and the intersection of the indigo cross line (see Figure 2(b)), the distance between the intersection of the indigo cross line and the yellow cross line (see Figure 2(c)), and the distance between the intersection of the yellow cross line and the red cross line (see Figure 2(d)) were measured by image analysis. The sum of these distances was calculated and evaluated according to the following criteria. 2 or more was considered to be a usable level, and 1 was considered to be poor. In FIG. 2, for ease of explanation, the indigo, yellow, and red register marks are shown with dashed lines, but in reality they are printed with solid lines.
[0136] Evaluation criteria 3: The total value is 0.1 mm or less 2: Total value is over 0.1 mm and 0.4 mm or less 1: Total value is greater than 0.4 mm
[0137] [Table 1]
[0138] [Table 2]
[0139] From the results of the Examples and Comparative Examples, it can be seen that a skin pack liner having a thickness of a specific value or less and a Taber stiffness in the longitudinal and transverse directions of a specific value or more shows good running properties and shows little deflection when a 1 kg article is placed on it. Therefore, such a skin pack liner can be suitably used not only for packaging lightweight articles, but also for packaging heavy articles. [Explanation of symbols]
[0140] 11 Evaluation Sheet 13 units 15 Weight
Claims
1. A skin pack mount having a paper base layer, The thickness of the skin pack mount is 1.05 mm or less, The Taber stiffness of the skin pack mount in the longitudinal direction is 143 mN m or more, The skin pack mount has a Taber stiffness in the lateral direction of 83 mN·m or more.
2. The skin pack mount has a longitudinal tensile modulus of 2.65 GPa or more; 2. The skin pack mount according to claim 1, wherein the skin pack mount has a tensile modulus in the lateral direction of 1.65 GPa or more.
3. The skin pack mount has a basis weight of 650 g / m 2 The mount for skin packs according to claim 1 .
4. The skin pack mount according to claim 1 , wherein the paper base layer is a laminate having a paper layer A, an adhesive layer A, and a paper layer B in this order, or a single paper.
5. The skin pack mount according to claim 4 , wherein the adhesive layer A contains a polyolefin resin.
6. The skin pack mount according to claim 1 , further comprising a thermoplastic resin layer on at least one surface of the paper base layer.
7. The skin pack mount according to claim 6, further comprising an adhesive layer B between the paper base layer and the thermoplastic resin layer.
8. The skin pack mount according to claim 7 , wherein the adhesive layer B contains a water-based adhesive.
9. 9. The skin pack mount according to claim 8, wherein the water-based adhesive is at least one selected from the group consisting of an acrylic adhesive, a polyurethane adhesive, and an isocyanate adhesive.
10. A skin pack comprising the skin pack mount according to any one of claims 1 to 9, a storage item, and a resin film, A skin pack packaging body, in which the item to be contained is contained between the skin pack backing and the resin film.
Citation Information
Patent Citations
Drip absorbing mat board
JP2009227299A
Skin-pack base paper
JP2021191690A
Skin pack package
JP2014181075A
Package
WO2021039823A1
Cited By
Backing paper for skin packs and skin pack packaging
WO2026190924A1